Electrophotographic photoreceptor, its manufacturing method and electrophotographic device

By using zinc oxide particles treated with N-acylated amino acids in the undercoat layer, the photoreceptor addresses transfer ghosts and maintains electrical stability under high transfer voltages, enhancing imaging quality.

JP7567538B2Active Publication Date: 2024-10-16FUJI ELECTRIC CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021022110
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-15
Publication Date
2024-10-16
Estimated Expiration
2041-02-15

AI Technical Summary

Technical Problem

Electrophotographic photoreceptors experience transfer ghosts due to high transfer voltages in high-speed or cleanerless processes, which are not adequately addressed by existing technologies.

Method used

Incorporating zinc oxide particles surface-treated with N-acylated amino acids or their salts, either alone or in combination with other metal oxides, into the undercoat layer of the photoreceptor, enhances the undercoat layer's properties to reduce transfer ghosts and improve electrical stability.

Benefits of technology

The solution results in a photoreceptor that effectively reduces transfer ghosts and maintains electrical stability even under high transfer voltages, ensuring high-quality imaging without defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567538000014
    Figure 0007567538000014
  • Figure 0007567538000015
    Figure 0007567538000015
  • Figure 0007567538000016
    Figure 0007567538000016
Patent Text Reader

Abstract

To provide an electrophotographic photoreceptor which is less susceptible to transfer ghosts even when installed in an electrophotographic device with transfer voltage set to a high level for high-speed processing or cleanerless processing, a manufacturing method therefor, and an electrophotographic device.SOLUTION: An electrophotographic photoreceptor comprises a conductive base body 1, and an undercoat layer 2 and a photosensitive layer sequentially provided on the conductive base body 1. The undercoat layer 2 comprises a binder resin and a first filler containing zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrophotographic photoreceptor (hereinafter also simply referred to as "photoreceptor"), a method for producing the same, and an electrophotographic apparatus equipped with the photoreceptor. [Background technology]

[0002] In addition to office copiers, printers, plotters, and digital image multifunction machines that combine the functions of these, in recent years, electrophotographic image forming methods have been widely applied to electrophotographic devices such as small personal printers and fax machines. Organic photoconductors (OPCs), which use organic materials, have become common as photoconductors for these various electrophotographic devices.

[0003] As organic photoreceptors, functionally separated photoreceptors and single-layered photoreceptors are known. The functionally separated photoreceptor is formed by sequentially laminating an undercoat layer made of an anodized film or a resin film on a conductive substrate such as aluminum, a charge generation layer in which an organic pigment having photoconductivity such as phthalocyanines or azo pigments is dispersed in a resin, a charge transport layer in which a molecule having a partial structure involved in charge hopping conduction such as amine or hydrazone bonded to a π-electron conjugated system is dissolved in a resin, and a protective layer as required. The single-layered photoreceptor is formed by, instead of the charge generation layer and the charge transport layer, providing a single photosensitive layer having both functions of charge generation and charge transport on the undercoat layer as required.

[0004] The electrophotographic process includes charging, exposing, developing and transferring. In the charging process, the photoconductor is charged to several hundred volts, in the exposing process, a latent image is formed on the surface of the photoconductor, in the developing process, the latent image is developed with toner, and finally, in the transferring process, the toner is transferred to the medium, and an image is obtained on the medium.

[0005] In recent years, so-called digital machines have become the mainstream of electrophotographic devices, and in the exposure and development process, information such as images and characters is digitized and converted into optical signals using a monochromatic light source such as an argon laser, helium-neon laser, semiconductor laser, or light-emitting diode as the exposure light source. A charged photoconductor is then irradiated with light to form an electrostatic latent image on the surface of the photoconductor, which is then visualized using toner.

[0006] Methods for charging a photoconductor include a non-contact charging method in which a charging member such as a scorotron does not come into contact with the photoconductor, and a contact charging method in which a charging member using a semiconductive rubber roller or brush comes into contact with the photoconductor. The contact charging method has the advantage that corona discharge occurs in the close vicinity of the photoconductor compared to the non-contact charging method, so less ozone is generated and a lower applied voltage is sufficient. Therefore, the contact charging method is mainstream, especially in medium to small devices, because it can realize electrophotographic devices that are more compact, lower cost, and less environmentally polluting.

[0007] In an electrophotographic apparatus equipped with a contact charging type charging device, a high electric field is locally applied to defective portions of a photoconductor during contact charging, which can cause electrical pinholes and result in image quality defects.

[0008] As a photoreceptor capable of preventing the above-mentioned image quality defects, an electrophotographic photoreceptor provided with an undercoat layer having a uniform thickness and capable of covering the irregularities on the surface of a conductive substrate is known.

[0009] Examples of the undercoat layer include anodized aluminum films, boehmite films, and resin films such as polyvinyl alcohol, casein, polyvinylpyrrolidone, polyacrylic acid, gelatin, polyurethane, and polyamide.

[0010] These resin films can also contain particles of metal oxides such as titanium oxide and zinc oxide as a filler for the purposes of preventing image defects caused by interference fringes by suppressing excessive reflection of exposure light from the conductive substrate and for the purposes of appropriately adjusting the resistance value of the undercoat layer.

[0011] As an example of a photoreceptor having an undercoat layer containing zinc oxide particles as a filler, Patent Document 1 discloses a photoreceptor containing in an undercoat layer metal oxide particles that have been surface-treated with an organometallic compound having a hydrolyzable functional group.

[0012] Patent Document 2 discloses a photoreceptor having an undercoat layer containing titanium oxide and zinc oxide particles hydrophobized with a reactive organosilicon compound. Patent Document 3 discloses an electrophotographic photoreceptor having an undercoat layer containing zinc oxide particles treated with a specific amount of an aminosilane compound and a urethane resin. Patent Document 4 discloses an electrophotographic photoreceptor having an undercoat layer containing zinc oxide particles surface-treated with an organometallic compound or an organosilicon compound, and titanium oxide particles surface-treated with an organometallic compound or an organosilicon compound.

[0013] However, in electrophotographic photoreceptors having an undercoat layer containing metal oxide particles, when the transfer voltage is high and the transfer history is strong due to the recent increase in device speed, or when the transfer voltage is set high to accommodate a cleanerless process, space charges of the opposite polarity are accumulated in the photosensitive layer, affecting the charging property during the next rotation process and causing image failure (transfer ghost), which is a problem. In contrast, none of Patent Documents 1 to 4 suggests a method for sufficiently suppressing transfer ghost under conditions where the transfer history is strong. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2004-20727 A [Patent Document 2] JP 2008-299020 A [Patent Document 3] JP 2013-137527 A [Patent Document 4] JP 2016-110127 A Summary of the Invention [Problem to be solved by the invention]

[0015] An object of the present invention is to provide an electrophotographic photoreceptor which is less likely to produce transfer ghosts even when mounted in an electrophotographic apparatus in which a transfer voltage is set high for a high-speed process or a cleanerless process, a manufacturing method thereof, and an electrophotographic apparatus. [Means for solving the problem]

[0016] As a result of extensive research, the inventors have found that the above problems can be solved by using zinc oxide particles that have been surface-treated with an N-acylated amino acid or a salt thereof, either alone or in combination with other metal oxides in a specific ratio, as a filler for the undercoat layer of a photoreceptor, and have thus completed the present invention.

[0017] That is, a first aspect of the present invention is an electrophotographic photoreceptor comprising a conductive substrate, and an undercoat layer and a photosensitive layer provided in that order on the conductive substrate, wherein the undercoat layer contains a resin binder and a first filler, and the first filler contains zinc oxide particles that have been surface-treated with an N-acylated amino acid or a salt of an N-acylated amino acid.

[0018] Furthermore, it is preferable that the undercoat layer contains a second filler, and the second filler contains at least one type of metal oxide particles different from the zinc oxide particles surface-treated with the N-acylated amino acid or a salt of the N-acylated amino acid. The metal oxide particles may be made of one or more metal oxides selected from the group consisting of zinc oxide, titanium oxide, tin oxide, zirconium oxide, silicon oxide, copper oxide, magnesium oxide, antimony oxide, vanadium oxide, yttrium oxide, and niobium oxide. Furthermore, it is preferable that the second filler contains titanium oxide particles surface-treated with an aminosilane compound.

[0020] Furthermore, the average primary particle size of the zinc oxide particles is preferably from 1 nm to 350 nm.

[0021] Furthermore, it is preferable that the resin binder contains two or more types selected from the group consisting of acrylic resins, melamine resins, and polyvinylphenol resins.

[0022] Furthermore, it is preferable that the photosensitive layer contains a charge generating material, and that the charge generating material contains at least one material selected from the group consisting of titanyl phthalocyanine and metal-free phthalocyanine.

[0023] Furthermore, the photosensitive layer may be a laminated type photosensitive layer including a charge generating layer and a charge transporting layer, or may be a single-layer type photosensitive layer consisting of a single layer containing a charge generating material and a charge transporting material.

[0024] A second aspect of the present invention is a method for producing the above-mentioned electrophotographic photoreceptor, comprising the steps of: preparing an undercoat layer coating liquid containing zinc oxide particles surface-treated with the N-acylated amino acid or a salt thereof; and forming the undercoat layer on the conductive substrate using the undercoat layer coating liquid.

[0025] A third aspect of the present invention is an electrophotographic apparatus equipped with the above electrophotographic photoreceptor. Effect of the Invention

[0026] According to the present invention, by adopting the above-mentioned configuration, it has been possible to provide an electrophotographic photosensitive member, a manufacturing method thereof, and an electrophotographic device which are less likely to produce transfer ghosts, even when the electrophotographic photosensitive member is mounted in an electrophotographic device in which a high transfer voltage is set for a high speed process or a cleanerless process. [Brief description of the drawings]

[0027] [Figure 1A] 1 is a schematic cross-sectional view showing a negatively-charged function-separated laminated type electrophotographic photoreceptor according to one configuration example of the electrophotographic photoreceptor of the present invention. [Figure 1B] FIG. 2 is a schematic cross-sectional view showing a positively charged single-layer type electrophotographic photoreceptor according to another example of the configuration of the electrophotographic photoreceptor of the present invention. [Figure 1C] FIG. 2 is a schematic cross-sectional view showing a positive-charging function-separated laminated type electrophotographic photoreceptor according to still another configuration example of the electrophotographic photoreceptor of the present invention. [Diagram 2] 1 is a schematic diagram showing an example of the configuration of an electrophotographic apparatus of the present invention; [Diagram 3] FIG. 2 is an explanatory diagram illustrating a configuration of an electrophotographic apparatus used in evaluation of a charging potential difference in the examples. [Figure 4] FIG. 4 is a diagram illustrating a method for evaluating a transfer ghost in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the accompanying drawings. The present invention is not limited to the following description.

[0029] The electrophotographic photoreceptor comprises a conductive substrate, and an undercoat layer and a photosensitive layer sequentially provided on the conductive substrate. The electrophotographic photoreceptor is roughly classified into a so-called negatively charged laminated photoreceptor and a positively charged laminated photoreceptor as a laminated (function-separated) photoreceptor, and a single-layered photoreceptor mainly used as a positively charged type. Figures 1A to 1C are schematic cross-sectional views showing an example of the configuration of the electrophotographic photoreceptor of the present invention, in which Figure 1A shows a negatively charged laminated electrophotographic photoreceptor, Figure 1B shows a positively charged single-layered electrophotographic photoreceptor, and Figure 1C shows a positively charged laminated electrophotographic photoreceptor, respectively.

[0030] As shown in the figure, in the negatively charged laminated photoreceptor, an undercoat layer 2 and a laminated photosensitive layer having a charge generating layer 4 with a charge generating function and a charge transport layer 5 with a charge transport function are sequentially laminated on a conductive substrate 1. In the positively charged single-layered photoreceptor, an undercoat layer 2 and a single-layered photosensitive layer 3 consisting of a single layer having both functions of charge generation and charge transport are sequentially laminated on a conductive substrate 1. In the positively charged laminated photoreceptor, an undercoat layer 2 and a laminated photosensitive layer having a charge transport layer 5 with a charge transport function and a charge generating layer 4 with both functions of charge generation and charge transport are sequentially laminated on a conductive substrate 1. Here, the "photosensitive layer" includes both a laminated photosensitive layer in which a charge generating layer and a charge transport layer are laminated, and a single-layered photosensitive layer. In addition, for example, for the purpose of improving printing durability, a protective layer (not shown) may be provided on the photosensitive layer as necessary.

[0031] In the photoreceptor according to the embodiment of the present invention, regardless of whether the photoreceptor has any of the above types of photosensitive layers, the undercoat layer 2 contains a resin binder and a first filler, and the first filler includes zinc oxide particles that have been surface-treated with an N-acylated amino acid or a salt of an N-acylated amino acid.

[0032] By adopting the above-mentioned configuration, an electrophotographic photoreceptor that is less likely to cause transfer ghosts can be obtained even when it is mounted on an electrophotographic device in which a transfer voltage is set high for a high-speed process or a cleanerless process. This is presumably because the hole transport ability of the undercoat layer 2 is improved by using the above-mentioned undercoat layer 2, and the amount of holes trapped by the undercoat layer 2 is reduced even when the transfer voltage is high, making it possible to reduce the amount of decrease in the surface charge potential in the next process. In addition, by using the above-mentioned undercoat layer 2, the dispersion stability of the undercoat layer coating liquid is improved, and the occurrence of secondary aggregates caused by dispersing metal oxides in the undercoat layer 2 is suppressed, thereby realizing a photoreceptor that does not cause image defects caused by these secondary aggregates, such as black spots on white paper and background fogging. Furthermore, it is also possible to sufficiently suppress the increase in the surface residual potential while maintaining the stability of the potential retention rate of the photoreceptor surface before and after repeated printing.

[0033] Therefore, by mounting this electrophotographic photoreceptor in an electrophotographic device, it is possible to sufficiently suppress an increase in the surface residual potential while maintaining the stability of the potential retention rate of the photoreceptor surface before and after repeated printing without causing transfer ghosts, even in devices with high transfer currents.

[0034] The undercoat layer 2 may contain a second filler in addition to the first filler, and the second filler may include at least one type of metal oxide particles other than zinc oxide particles that have been surface-treated with an N-acylated amino acid or a salt of an N-acylated amino acid.

[0035] (Zinc oxide particles surface-treated with N-acylated amino acid or its salt) The N-acylated amino acid used in the surface treatment of the zinc oxide particles is composed of an amino acid portion and a fatty acid portion. Examples of the amino acid in the amino acid portion include glycine, α-alanine, valine, leucine, isoleucine, serine, threonine, lysine, arginine, aspartic acid, glutamic acid, asparagine, glutamine, cysteine, cystine, methionine, phenylalanine, tyrosine, proline, hydroxyproline, tryptophan, histidine, β-alanine, ε-aminocaproic acid, sarcosine, and DL-pyroglutamic acid. The fatty acid in the fatty acid portion may be either saturated or unsaturated fatty acid, and among them, fatty acids having 8 to 20 carbon atoms are preferred, such as lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, and coconut oil fatty acid.

[0036] Examples of N-acylated amino acids include lauroyl glutamic acid, myristoyl glutamic acid, coconut oil fatty acid glutamic acid (also called cocoyl glutamic acid), stearoyl glutamic acid, lauroyl aspartic acid, lauroyl sarcosine, myristoyl sarcosine, coconut oil fatty acid sarcosine, N-lauryl-N-methyl-β-alanine, cocoyl alanine, N-myristoyl-N-methyl-β-alanine, N-coconut oil fatty acid-N-methyl-β-alanine, cocoyl glycine, etc. Among these, cocoyl glutamic acid is preferred.

[0037] In addition, the salt of N-acylated amino acid is not particularly limited, but metal salt, ammonium salt, organic amine salt are preferable. Metal atoms constituting metal salts include, for example, monovalent metals such as sodium, lithium, potassium, rubidium, cesium, etc.; divalent metals such as zinc, magnesium, calcium, strontium, barium, etc.; trivalent metals such as aluminum, etc.; other metals such as iron, titanium, etc.; and the like. Organic amine groups constituting organic amine salts include, for example, alkanolamine groups such as monoethanolamine group, diethanolamine group, triethanolamine group, etc.; alkylamine groups such as monoethylamine group, diethylamine group, triethylamine group, etc.; polyamine groups such as ethylenediamine group, triethylenediamine group, etc.; and the like. Among the above salts, more preferable are ammonium salt, sodium salt, potassium salt, and even more preferable are sodium salt. Therefore, as the salt of N-acylated amino acid, sodium cocoyl glutamate is particularly preferable.

[0038] Specific examples of N-acylated amino acids or salts thereof include AminoSurfact (registered trademark) ACDS-L (aqueous solution of sodium cocoyl glutamate), ACDP-L (aqueous solution of potassium / sodium cocoyl glutamate), ACMT-L (aqueous solution of triethanolamine cocoyl glutamate), ALMS-P1 (sodium lauroyl glutamate), AMMS-P1 (sodium myristoyl glutamate), Aminoformer (registered trademark) FLDS-L (aqueous solution of sodium lauroyl aspartate), FCMT-L (aqueous solution of triethanolamine acylaspartate), and FLMS-P, all of which are manufactured by Asahi Kasei Finechem Corporation. Examples of the usable surfactants include Amisoft® HS-11P (sodium stearoyl glutamate), Amisoft® HA-P (stearoyl glutamic acid), Amisoft® MK-11 (potassium myristoyl glutamine), Amisoft® CA (cocoyl glutamic acid), Amisoft® CS-11 (sodium cocoyl glutamate), Amisoft® CS-22 (disodium cocoyl glutamate / sodium salt aqueous solution), and Amirite® ACS-12 (sodium cocoyl alanine aqueous solution).

[0039] The surface treatment of zinc oxide particles with the N-acylated amino acid or its salt refers to attaching the N-acylated amino acid or its salt as a surface treatment agent to the surface of the zinc oxide particles by chemical or physical adsorption, and the method can be any conventionally used surface treatment method, and is not particularly limited.Specific examples of the method include a method of directly mixing the N-acylated amino acid or its salt with particles (dry treatment method, mechanochemical method), a method of dispersing the N-acylated amino acid or its salt in a dispersion medium and then mixing it with particles (semi-dry method), and a method of dispersing the particles in a dispersion medium to prepare a slurry and then mixing it with the N-acylated amino acid or its salt (wet method).

[0040] The dry treatment method is a method for surface treating particles by using mechanochemical treatment such as utilizing the impact force of an air jet containing a surface treatment agent, or utilizing the shear force of a ball mill or the like that mixes a dispersion medium such as a medium, to adsorb and bond the surface treatment agent to the particle surface.

[0041] The dispersion medium used in the semi-dry method or the wet method is not particularly limited, and may be, for example, water, an organic solvent, or a mixture thereof. Examples of the organic solvent include alcohol, acetone, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, dioxane, etc., and examples of the alcohol include water-soluble monohydric alcohols such as methanol, ethanol, and propanol, and water-soluble dihydric or higher alcohols such as ethylene glycol and glycerin. The dispersion medium is preferably water, and more preferably ion-exchanged water.

[0042] In the semi-dry method and the wet method, the particles and the surface treatment agent are dispersed in a solvent to perform surface treatment. The dispersion method may be any known method and is not particularly limited. Dispersion can be performed, for example, by stirring in a tank, but is preferably performed using a dispersing machine that can be used to disperse particles in liquid, such as a dispersing mixer, a homogenizing mixer, an in-line mixer, a media grinder, a three-roll mill, an attritor, a colloid mill, or an ultrasonic dispersing machine.

[0043] In the surface treatment, it is preferable to thoroughly stir the particles and the surface treatment agent so that they are uniformly mixed. When a mixer is used in the dry method and the semi-dry method, specifically, for example, Powder Lab (volume 130 ml) and FM mixer (volume 9 L) manufactured by Nippon Coke & Engineering Co., Ltd. can be used as the mixer, and it is preferable to stir by increasing the rotation speed. The stirring time may be any time as long as the particles are uniformly mixed and the surface treatment proceeds, but it is preferably 10 minutes or more, and from the viewpoint of productivity, it is preferably within 10 hours. The rotation speed of the stirring is preferably 1000 rpm or more, and more preferably 2000 rpm or more. If the rotation speed is 500 rpm or less, the surface treatment may not be sufficient. The temperature during the surface treatment is not particularly limited, but from the viewpoint of workability, it is preferably performed at 5 to 150 ° C, and more preferably 60 to 150 ° C.

[0044] The amounts of particles, surface treatment agent, solvent and dispersion medium in each surface treatment are not particularly limited as long as the desired surface treatment can be performed. Specifically, since loss of the surface treatment agent may occur during or after the treatment, for example, it is preferable to use 0.1 to 15 parts by mass of N-acylated amino acid or a salt thereof relative to 100 parts by mass of zinc oxide particles. The amount of N-acylated amino acid or a salt thereof relative to 100 parts by mass of zinc oxide particles is more preferably 0.2 to 12 parts by mass, and even more preferably 0.5 to 10 parts by mass.

[0045] In addition, the temperature during the treatment is not particularly limited as long as the desired surface treatment is performed, but in the wet method, after the slurry is prepared, it is preferable to age the slurry at 60°C or higher. The aging temperature is more preferably 80°C or higher, and even more preferably 90°C or higher. The upper limit of the aging temperature is preferably 200°C or lower in order to suppress decomposition of amino acids. The upper limit of the aging temperature is more preferably 150°C or lower, and even more preferably 130°C or lower. It is preferable to age the slurry while stirring it.

[0046] The maturation time is not particularly limited, but is preferably 1 minute or more, more preferably 5 minutes or more, and even more preferably 10 minutes or more. The upper limit of the maturation time is not particularly limited, but is preferably 10 hours or less, for example, from the viewpoint of improving production efficiency. The upper limit of the maturation time is more preferably 5 hours or less, and even more preferably 2 hours or less.

[0047] In the wet method, it is preferable to remove the dispersion medium after aging the slurry. If necessary, other steps such as neutralization, washing, pulverization, and other steps that are usually performed for surface treatment of particles may be further performed.

[0048] After removing the dispersion medium, it is also preferable to carry out drying. Drying can be performed by vacuum drying, heat drying, or the like. When heat drying is performed, it is preferable to carry out the drying at a temperature of 35° C. to 200° C. for 5 minutes to 72 hours. By carrying out drying, it is expected that the dispersibility of the zinc oxide particles surface-treated with the N-acylated amino acid or a salt thereof is further improved.

[0049] In the surface treatment with N-acylated amino acid or a salt thereof, it is preferable that the surface treatment is performed so that the content of the surface treatment agent is 0.1 to 15 mass % when the treated zinc oxide particles are taken as 100 parts by mass. By making the content of the surface treatment agent 0.1 mass % or more, it is possible to ensure good liquid stability and suppress the occurrence of aggregation and precipitation over time. Furthermore, by making the content of the surface treatment agent 15 mass % or less, it is possible to ensure good electrical properties of the photoreceptor and suppress the occurrence of image defects. The content of the surface treatment agent is more preferably 0.2 to 9 mass %, and even more preferably 0.5 to 8 mass %.

[0050] The average primary particle diameter of the zinc oxide particles is preferably in the range of 1 to 800 nm, more preferably 1 to 350 nm, and even more preferably 10 to 300 nm. When the average primary particle diameter of the zinc oxide particles is 800 nm or less, the coating solution stability of the undercoat layer coating solution is further improved, which is preferable. As a method for producing zinc oxide particles, a production method by various conventionally known production processes can be used. For example, zinc oxide particles produced by the French method or the American method may be used. The French method is a production method in which metallic zinc is heated to produce zinc vapor, which is oxidized and then cooled. The American method is a production method in which a reducing agent is added to zinc ore, which is heated, reduced and volatilized, and the resulting metal vapor is oxidized with air. Alternatively, zinc oxide particles obtained by a wet method in which zinc hydroxide or basic zinc carbonate obtained by precipitating through a reaction between soluble zincs (zinc chloride, zinc sulfate, etc.) and an alkaline solution (sodium hydroxide aqueous solution, etc.) is roasted may be used. Specifically, for example, FINEX-25, FINEX-30, FINEX-50, XZ-100F-LP, XZ-300F-LP manufactured by Sakai Chemical Industry Co., Ltd., MZ-300, MZ-500 manufactured by Teika Corporation, FZO-50 manufactured by Ishihara Sangyo Kaisha, Ltd., etc. can be used.

[0051] (metal oxide particles) Metal oxide particles other than zinc oxide particles surface-treated with N-acylated amino acid or a salt thereof, which may be further mixed as a second filler in the undercoat layer 2, are preferably particles made of one or more metal oxides selected from the group consisting of zinc oxide, titanium oxide, tin oxide, zirconium oxide, silicon oxide, copper oxide, magnesium oxide, antimony oxide, vanadium oxide, yttrium oxide, and niobium oxide. Among them, titanium oxide particles are preferred, and titanium oxide particles surface-treated with a silane coupling agent are particularly preferred. The average primary particle size of the titanium oxide particles is preferably 10 nm to 500 nm, more preferably 20 nm to 300 nm.

[0052] As the silane coupling agent, preferably, an aminosilane compound can be mentioned, for example, N-β (aminoethyl) γ-aminopropyl trimethoxysilane, γ-aminopropyl triethoxysilane, N-phenyl-γ-aminopropyl trimethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl trimethoxysilane, 3-aminopropyl trimethoxysilane, 3-aminopropyl methyl trimethoxysilane, 3-aminopropyl methyl triethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene) propylamine, aminopropyl methyl trimethoxysilane, N-phenyl-3-aminopropyl trimethoxysilane, and other aminosilane compounds can be mentioned. Specifically, silane coupling agents such as KBM-603 (N-β(aminoethyl)γ-aminopropyltrimethoxysilane), KBE-903 (γ-aminopropyltriethoxysilane), KBM-573 (N-phenyl-γ-aminopropyltrimethoxysilane), KBM-602 (N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane), KBM-903 (3-aminopropyltrimethoxysilane), and KBE-9103P (3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine) manufactured by Shin-Etsu Chemical Co., Ltd. can be used.

[0053] Among these, it is preferable to use titanium oxide particles whose surface has been treated with an aminosilane compound as the metal oxide particles, and transfer ghosts can be more effectively suppressed.

[0054] As a method of surface treatment of titanium oxide particles with a silane coupling agent, preferably, the titanium oxide particles are surface-treated mechanochemically with a silane coupling agent by gas phase method to bond. Specifically, the titanium oxide particles and the silane coupling agent are mixed in a blender such as a ball mill or a Henschel mixer, and then surface-treated while being pulverized in a jet-type air pulverizer such as a jet mill. The titanium oxide surface-treated with the obtained silane coupling agent can be used as it is, or it can be washed with pure water before use. The crystal type of titanium oxide can be any of anatase type, rutile type, brookite type, and mixed crystals thereof.

[0055] The undercoat layer 2 may contain at least a first filler, and the first filler may contain zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof. When the undercoat layer 2 contains a second filler in addition to the zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof, and the second filler is used in combination with at least one metal oxide particle different from the zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof, it is preferable that the zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof are contained in the first filler and the second filler in an amount of 2% by mass or more. From the viewpoint of suppressing transfer ghost, it is more preferable that the zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof are contained in an amount of 20% by mass or more, and even more preferable that the zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof are contained in an amount of 40% by mass or more of the total amount of the filler. When the undercoat layer 2 does not contain zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof as a filler, the effect of improving the transfer ghost cannot be obtained.

[0056] In the photoreceptor according to the embodiment of the present invention, the undercoat layer 2 is not particularly limited as long as it satisfies the above-mentioned conditions for the filler, and other configurations can be appropriately selected according to the usual method. The configurations of each layer of the photoreceptor are described below.

[0057] (Conductive substrate) The conductive substrate 1 may be a cylinder made of various metals, such as aluminum alloys of JIS 3003, JIS 5000, or JIS 6000, or a film made of conductive plastic. The conductive substrate 1 may also be a molded body or sheet material of glass, acrylic, polyamide, or polyethylene terephthalate to which electrodes are attached. The conductive substrate 1 is finished into a substrate with a predetermined dimensional accuracy by extrusion or drawing if it is made of an aluminum alloy, or by injection molding if it is made of resin. The surface of the conductive substrate 1 is processed to an appropriate surface roughness by cutting with a diamond bit, as necessary, and then degreased and washed with an aqueous detergent such as a weak alkaline detergent to clean it.

[0058] (Undercoat layer) The undercoat layer 2 contains a filler and a resin binder, and as described above, the filler must satisfy the above conditions.

[0059] The resin binder for the undercoat layer 2 may be a resin such as polyethylene, polypropylene, polystyrene, acrylic resin, vinyl chloride resin, vinyl acetate resin, polyurethane, epoxy resin, polyester, melamine resin, silicone resin, polyvinyl butyral, polyamide, casein, gelatin, polyvinyl alcohol, phenol resin, polyvinyl phenol resin, and ethyl cellulose, which may be used alone or in combination of two or more. In particular, it is preferable that the resin binder for the undercoat layer 2 contains two or more selected from the group consisting of acrylic resin, melamine resin, and polyvinyl phenol resin.

[0060] In the undercoat layer 2, the mass ratio [filler / resin binder] of the filler including the first filler or the filler including the first filler and the second filler to the resin binder is preferably 50 / 50 to 90 / 10. By making the filler ratio in the undercoat layer 2 50 / 50 or more, the ratio of the resin binder can be kept low, and it is possible to suppress the occurrence of low-density image defects due to the volume resistance of the undercoat layer 2 being too high in a low-temperature, low-humidity environment, which causes the potential of the exposed area to not decrease sufficiently. In addition, by making the filler ratio 90 / 10 or less, it is possible to increase the stability of the undercoat layer coating solution and suppress the occurrence of aggregation and sedimentation over time.

[0061] The undercoat layer 2 is mainly composed of a filler and a resin, but may further contain known additives. Examples of such additives include known materials such as metal powders such as aluminum, conductive materials such as carbon black, electron transport materials such as electron transport pigments, polycyclic condensation compounds, metal chelate compounds, and organometallic compounds. Examples of preferred electron transport materials include benzophenone compounds having a hydroxyl group and anthraquinone compounds having a hydroxyl group.

[0062] The undercoat layer coating liquid used to form the undercoat layer 2 is prepared by dispersing the filler in a resin solution obtained by dissolving a resin binder in a solvent. The solvent may be appropriately selected in consideration of the dispersibility of the filler, the solubility in the resin binder, storage stability, volatility, safety, and the like. Specific examples of the solvent that can be used include alcohols such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butanol, t-butanol, sec-butanol, and benzyl alcohol, toluene, cyclohexanone, tetrahydrofuran, and methylene chloride. A general-purpose device such as a vibration mill, a paint shaker, or a sand grinder can be used to disperse the filler, and it is preferable to use zirconia as the dispersion medium because it can disperse the filler more uniformly.

[0063] The thickness of the undercoat layer 2 is preferably in the range of 0.1 to 10 μm, more preferably 0.3 to 5 μm, and even more preferably 0.5 to 3 μm. By making the thickness of the undercoat layer 2 0.1 μm or more, it is possible to appropriately suppress the injection of charges and suppress the occurrence of black spot defects on the image. In addition, by making the thickness of the undercoat layer 2 10 μm or less, it is possible to suppress an increase in resistance and suppress the occurrence of image defects due to low concentration.

[0064] The undercoat layer 2 may be a single layer, or may be a laminate of two or more layers of different types. In this case, it is not necessary that all layers contain zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof, and may be, for example, a structure in which an undercoat layer 2 made of only a thermoplastic resin such as alcohol-soluble nylon is laminated on an undercoat layer 2 containing zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof, or a structure in which an undercoat layer 2 containing zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof is laminated on an undercoat layer 2 made of an anodized aluminum film.

[0065] (Negatively charged laminated photoconductor) As described above, in the negatively charged laminated photoreceptor, the photosensitive layer is formed by laminating the charge generating layer 4 and the charge transport layer 5 in this order on the undercoat layer 2.

[0066] The charge generating layer 4 can be formed by using various organic pigments as charge generating materials together with a resin binder. As charge generating materials, metal-free phthalocyanines having various crystal forms, various phthalocyanines having copper, aluminum, indium, vanadium, titanium, etc. as central metals, various bisazo pigments, trisazo pigments, etc. are particularly suitable. As charge generating materials, titanyl phthalocyanine and metal-free phthalocyanine are more preferable, and one of these can be used alone or two or more can be mixed and used. These organic pigments are adjusted to a particle diameter of 50 to 800 nm, preferably 150 to 500 nm, and are used in a state of being dispersed in a resin binder.

[0067] The performance of the charge generating layer 4 is also affected by the resin binder. There are no particular limitations on the resin binder, and an appropriate one can be selected from various polyvinyl chlorides, polyvinyl butyrals, polyvinyl acetals, polyesters, polycarbonates, acrylic resins, phenoxy resins, etc. The thickness of the charge generating layer 4 can be 0.1 to 5 μm, and is preferably 0.2 to 0.5 μm.

[0068] In order to obtain a good dispersion state and form a uniform charge generation layer 4, the selection of the solvent for the charge generation layer coating liquid is also important. As the solvent, for example, aliphatic halogenated hydrocarbons such as methylene chloride and 1,2-dichloroethane, ether-based hydrocarbons such as tetrahydrofuran, ketones such as acetone, methyl ethyl ketone, and cyclohexanone, esters such as ethyl acetate and ethyl cellosolve, etc. can be used. It is desirable to adjust the ratio of the charge generation material and the resin binder in the coating liquid so that the ratio of the resin binder in the charge generation layer 4 after coating and drying is 20 to 80 parts by mass. A particularly preferred composition of the charge generation layer 4 is 40 to 60 parts by mass of the resin binder and 60 to 40 parts by mass of the charge generation material.

[0069] When forming the charge generating layer 4 by coating, the above-mentioned materials are appropriately mixed to prepare a charge generating layer coating liquid, which is then processed using a dispersion processing device such as a sand mill or a paint shaker to adjust the particle diameter of the organic pigment particles to the desired size, and then the charge generating layer coating liquid can be used for coating.

[0070] The charge transport layer 5 can be formed by preparing a charge transport layer coating solution by dissolving the charge transport material alone or together with a resin binder in an appropriate solvent, applying the solution to the charge generation layer 4 by immersion or an applicator method, and drying the solution. As the charge transport material, an appropriate one can be selected from known substances having hole transport properties (for example, those exemplified in "Borsenberger, PM and Weiss DSed "Organic Photoreceptors for Imaging Systems" Marcel Dekker Inc. 1993"). Specific examples of such hole transport materials include various hydrazones, styryls, diamines, butadienes, enamines, indole compounds, and mixtures thereof.

[0071] As the resin binder that forms the charge transport layer 5 together with the charge transport material, polycarbonate-based polymers are widely used from the viewpoint of film strength and abrasion resistance. These polycarbonate-based polymers include bisphenol A type, C type, Z type, etc., and copolymers containing monomer units that constitute these may also be used. The optimal molecular weight range of such polycarbonate polymers is 10,000 to 100,000. In addition, polyethylene, polyphenylene ether, acrylic, polyester, polyamide, polyurethane, epoxy, polyvinyl acetal, polyvinyl butyral, phenoxy resin, silicone resin, polyvinyl chloride, polyvinylidene chloride, polyvinyl acetate, cellulose resin, and copolymers thereof may also be used.

[0072] The charge transport layer 5 is preferably formed to have a thickness in the range of 3 to 50 μm, taking into consideration the charging characteristics and abrasion resistance of the photoreceptor, etc. Silicone oil may be appropriately added to the charge transport layer 5 to obtain surface smoothness.

[0073] (Positively charged single-layer photoconductor) As described above, in the positively charged single-layer type photoreceptor, the photosensitive layer 3 is formed on the undercoat layer 2 and is a single layer containing a charge generating material and a charge transporting material.

[0074] The single-layer type photosensitive layer 3 mainly consists of a charge generating material, a hole transport material, an electron transport material (acceptor compound), and a resin binder. As the charge generating material, various organic pigments can be used similar to those in the case of the laminated type. As the charge generating material, particularly preferred are metal-free phthalocyanines having various crystal forms, various phthalocyanines having copper, aluminum, indium, vanadium, titanium, etc. as the central metal, various bisazo and trisazo pigments, etc., among which titanyl phthalocyanine and metal-free phthalocyanine are more preferred, and one of these can be used alone or two or more can be mixed and used.

[0075] Examples of hole transport materials include various hydrazone, styryl, diamine, butadiene, and indole compounds, and mixtures of these. Examples of electron transport materials include various benzoquinone derivatives, phenanthrenequinone derivatives, stilbenequinone derivatives, and azoquinone derivatives. Any of these can be used alone or in combination of two or more.

[0076] As the resin binder, polycarbonate resin can be used alone, or a suitable combination of resins such as polyester resin, polyvinyl acetal resin, polyvinyl butyral resin, polyvinyl alcohol resin, vinyl chloride resin, vinyl acetate resin, polyethylene, polypropylene, polystyrene, acrylic resin, polyurethane resin, epoxy resin, melamine resin, silicon resin, silicone resin, polyamide resin, polystyrene resin, polyacetal resin, polyarylate resin, polysulfone resin, methacrylic acid ester polymer, and copolymers thereof can be used. Also, resins of the same type but with different molecular weights can be mixed and used.

[0077] The thickness of the single-layer photosensitive layer 3 is preferably in the range of 3 to 100 μm, more preferably 10 to 50 μm, in order to maintain a practically effective surface potential. Silicone oil may be appropriately added to the single-layer photosensitive layer 3 in order to obtain surface smoothness.

[0078] (Positively charged laminated photoconductor) As described above, in the positively charged laminated photoreceptor, the photosensitive layer is composed of the charge transport layer 5 and the charge generating layer 4 laminated in this order on the undercoat layer 2 .

[0079] In the positively charged laminated photoreceptor, the charge transport layer 5 is mainly composed of a hole transport material and a resin binder. As the hole transport material and the resin binder in the charge transport layer 5, the same materials as those listed for the single-layer type photosensitive layer 3 can be used.

[0080] The content of the hole transport material in the charge transport layer 5 is preferably 10 to 80 mass %, and more preferably 20 to 70 mass %, based on the solid content of the charge transport layer 5. The content of the resin binder in the charge transport layer 5 is preferably 20 to 90 mass %, and more preferably 30 to 80 mass %, based on the solid content of the charge transport layer 5.

[0081] The thickness of the charge transport layer 5 is preferably in the range of 3 to 50 μm, more preferably in the range of 15 to 40 μm, in order to maintain a practically effective surface potential.

[0082] In the positively charged laminated photoreceptor, the charge generation layer 4 is mainly composed of a charge generation material, a hole transport material, an electron transport material, and a resin binder. The charge generation material, hole transport material, electron transport material, and resin binder in the charge generation layer 4 may be the same materials as those listed for the single-layer photosensitive layer 3.

[0083] The content of the charge generating material in the charge generating layer 4 is preferably 0.1 to 5 mass %, more preferably 0.5 to 3 mass %, based on the solid content of the charge generating layer 4. The content of the hole transport material in the charge generating layer 4 is preferably 1 to 30 mass %, more preferably 5 to 20 mass %, based on the solid content of the charge generating layer 4. The content of the electron transport material in the charge generating layer 4 is preferably 5 to 60 mass %, more preferably 10 to 40 mass %, based on the solid content of the charge generating layer 4. The content of the resin binder in the charge generating layer 4 is preferably 20 to 80 mass %, more preferably 30 to 70 mass %, based on the solid content of the charge generating layer 4.

[0084] The thickness of the charge generating layer 4 can be the same as that of the single-layer type photosensitive layer 3 of the single-layer type photoreceptor.

[0085] In the photoreceptor according to the embodiment of the present invention, a leveling agent such as silicone oil or fluorine-based oil can be contained in either the laminated type or single-layer type photosensitive layer in order to improve the leveling property of the formed film or to impart lubricity. In addition, a plurality of inorganic oxides can be contained in order to adjust the film hardness, reduce the friction coefficient, impart lubricity, etc. Metal oxides such as silica, titanium oxide, zinc oxide, calcium oxide, alumina, and zirconium oxide, metal sulfates such as barium sulfate and calcium sulfate, fine particles of metal nitrides such as silicon nitride and aluminum nitride, fluorine-based resin particles such as tetrafluoroethylene resin, and fluorine-based comb-type graft polymerized resin particles can be contained. Furthermore, other known additives can be contained as long as they do not significantly impair the electrophotographic properties, if necessary.

[0086] In addition, the photosensitive layer may contain a deterioration inhibitor such as an antioxidant or a light stabilizer for the purpose of improving the environmental resistance and stability against harmful light. Examples of compounds used for such purposes include chromanol derivatives such as tocopherol and esterified compounds, polyarylalkane compounds, hydroquinone derivatives, etherified compounds, dietherified compounds, benzophenone derivatives, benzotriazole derivatives, thioether compounds, phenylenediamine derivatives, phosphonic acid esters, phosphorous acid esters, phenol compounds, hindered phenol compounds, linear amine compounds, cyclic amine compounds, and hindered amine compounds.

[0087] The electrophotographic photoreceptor according to the embodiment of the present invention can obtain the desired effect by applying it to various machine processes. Specifically, sufficient effects can be obtained in charging processes such as a contact charging method using a charging member such as a roller or a brush, a non-contact charging method using a charging member such as a corotron or a scorotron, and in development processes such as a contact development and non-contact development method using a developer such as a non-magnetic one-component, a magnetic one-component, or a two-component developer.

[0088] (Manufacturing Method of Electrophotographic Photoreceptor) The method for producing an electrophotographic photoreceptor according to an embodiment of the present invention includes the steps of preparing an undercoat layer coating liquid containing zinc oxide particles surface-treated with an N-acylated amino acid or a salt thereof, and forming an undercoat layer 2 on a conductive substrate 1 using the undercoat layer coating liquid when producing the electrophotographic photoreceptor.

[0089] The undercoat layer 2 can be formed by applying the undercoat layer coating liquid prepared as described above to the surface of the conductive substrate 1 and drying it according to a conventional method. As a method for applying the coating liquid, a known method such as a dip coating method, a doctor blade method, a bar coater, a roll transfer method, a spray method, etc., is used, but when applying to a cylindrical conductive substrate, it is preferable to use a dip coating method. A method for drying the coating film of the undercoat layer coating liquid can be appropriately selected depending on the type of solvent and the film thickness to be formed, but heat drying is particularly preferable. The drying conditions can be, for example, 50 to 200°C and 1 to 120 minutes.

[0090] Specifically, in the case of a negatively charged laminated photoreceptor, first, the undercoat layer coating liquid containing the specific filler prepared as described above is applied to the surface of the conductive substrate 1 and dried according to a conventional method to form the undercoat layer 2. Next, the charge generation layer 4 is formed by a method including a step of preparing and preparing a charge generation layer coating liquid by dissolving and dispersing an arbitrary charge generation material and a resin binder in a solvent, and a step of coating and drying the charge generation layer coating liquid on the surface of the undercoat layer 2 to form the charge generation layer 4. Next, the charge transport layer 5 is formed by a method including a step of preparing and preparing a charge transport layer coating liquid by dissolving an arbitrary hole transport material and a resin binder in a solvent, and a step of coating and drying the charge transport layer coating liquid on the surface of the charge transport layer 5 to form the charge transport layer. By such a manufacturing method, the negatively charged laminated photoreceptor according to the embodiment of the present invention can be manufactured.

[0091] Furthermore, in the case of a positively charged single-layer type photoreceptor, the photoreceptor can be produced by a method including the steps of applying an undercoat layer coating liquid containing the specific filler prepared as described above to the surface of a conductive substrate 1 in a conventional manner, followed by drying to form an undercoat layer 2, dissolving and dispersing an optional charge generating material, a hole transport material, an electron transport material and a resin binder in a solvent to prepare a single-layer type photosensitive layer coating liquid, and applying the obtained single-layer type photosensitive layer coating liquid to the surface of the undercoat layer 2, followed by drying to form a single-layer type photosensitive layer 3.

[0092] Furthermore, in the case of a positively charged laminated photoreceptor, first, the undercoat layer coating liquid containing the specific filler prepared as described above is applied to the surface of the conductive substrate 1 and dried according to a conventional method to form the undercoat layer 2. Next, the charge transport layer 5 is formed by a method including a step of preparing and preparing a charge transport layer coating liquid by dissolving an arbitrary hole transport material and a resin binder in a solvent, and a step of applying and drying the charge transport layer coating liquid on the surface of the undercoat layer 2 to form a charge transport layer. Next, the charge generation layer 4 is formed by a method including a step of preparing and preparing a charge generation layer coating liquid by dissolving and dispersing an arbitrary charge generation material, a hole transport material, an electron transport material, and a resin binder in a solvent, and a step of applying and drying the charge generation layer coating liquid on the surface of the charge transport layer 5 to form the charge generation layer 4. By such a manufacturing method, the positively charged laminated photoreceptor according to the embodiment of the present invention can be manufactured.

[0093] (Electrophotographic device) The electrophotographic apparatus according to the embodiment of the present invention is equipped with the electrophotographic photoreceptor described above, and as a result, even if a high transfer voltage is set for a high-speed process or a cleanerless process, the electrophotographic apparatus is less likely to produce a transfer ghost.

[0094] FIG. 2 shows a schematic diagram of an example of the configuration of the electrophotographic apparatus of the present invention. The electrophotographic apparatus 60 shown in the figure is equipped with a photoreceptor 7 according to an embodiment of the present invention, which includes a conductive substrate 1, an undercoat layer 2 coated on the outer peripheral surface thereof, and a photosensitive layer 300. The electrophotographic apparatus 60 is composed of a charging member 21 arranged on the outer peripheral edge of the photoreceptor 7, a high-voltage power source 22 for supplying a voltage to the charging member 21, an image exposure member 23, a developing device 24, a paper feed member 25, and a transfer charger 26. The charging member 21 may be roller-shaped, the developing device 24 may include a developing roller 241, and the paper feed member 25 may include a paper feed roller 251 and a paper feed guide 252. The transfer charger 26 may be of a direct charging type. The electrophotographic apparatus 60 may further include a cleaning device 27 equipped with a cleaning blade 271, and a charge removing member 28. The electrophotographic apparatus 60 may be a color printer. The image forming method in the electrophotographic apparatus 60 may be a reversal development process in which toner is attached to a portion (latent image) whose surface potential has been reduced by exposure, and developed. A negative voltage may be applied to the negatively charged photoconductor 7 by the charging member 21, the image may be developed using negatively charged toner in the developing device 24, and a positive voltage may be applied by the transfer charger 26. A positive voltage may be applied to the positively charged photoconductor 7 by the charging member 21, the image may be developed using positively charged toner in the developing device 24, and a negative voltage may be applied by the transfer charger 26. EXAMPLES

[0095] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples.

[0096] <Method for producing surface-treated zinc oxide particles> (Production Example 1: Zinc oxide particles (20 nm) surface-treated with amino acid salt A) 100 g of zinc oxide particles that were not surface-treated (FINEX-50, manufactured by Sakai Chemical Industry Co., Ltd., average primary particle diameter 20 nm) were placed in a mixer (Powder Lab, manufactured by Nippon Coke & Engineering Co., Ltd., tank capacity 130 ml), and 50 g of an aqueous solution in which 6 g of sodium cocoyl glutamate (Amisoft CS-11, manufactured by Ajinomoto Co., Inc.) (hereinafter referred to as "amino acid salt A") was dissolved as a surface treatment agent was added, and the mixture was mixed at 2000 rpm for 10 minutes. After that, the rotation speed was changed to a predetermined 2500 rpm, and the temperature inside the tank was raised to a predetermined temperature of 100°C while stirring. Further, negative pressure was applied with a vacuum pump to remove volatile matters such as water, and a powder of zinc oxide particles (20 nm) surface-treated with amino acid salt A was obtained.

[0097] (Production Example 2: Zinc oxide particles (20 nm) surface-treated with amino acid salt A) A powder of zinc oxide particles (20 nm) surface-treated with amino acid salt A was obtained in the same manner as in Production Example 1, except that the amount of the surface treatment agent in Production Example 1 was changed to 0.5 g.

[0098] (Production Example 3: Zinc oxide particles (20 nm) surface-treated with amino acid salt A) A powder of zinc oxide particles (20 nm) surface-treated with amino acid salt A was obtained in the same manner as in Production Example 1, except that the amount of the surface treatment agent in Production Example 1 was changed to 10 g.

[0099] (Production Example 4: Zinc oxide particles (35 nm) surface-treated with amino acid salt A) A powder of zinc oxide particles (35 nm) surface-treated with amino acid salt A was obtained in the same manner as in Production Example 1, except that non-surface-treated zinc oxide particles (manufactured by Sakai Chemical Industry Co., Ltd., FINEX-50, average primary particle diameter 20 nm) were changed to non-surface-treated zinc oxide particles (manufactured by Sakai Chemical Industry Co., Ltd., FINEX-30, average primary particle diameter 35 nm).

[0100] (Production Example 5: Zinc oxide particles (20 nm) surface-treated with amino acid salt B) A powder of zinc oxide particles (20 nm) surface-treated with amino acid salt B was obtained in the same manner as in Production Example 1, except that the surface treatment agent was changed to sodium lauroyl glutamate (Asahi Kasei Finechem, Aminoformer ALMS-P1) (hereinafter referred to as "amino acid salt B").

[0101] (Production Example 6: Zinc oxide particles (20 nm) surface-treated with amino acid C) A powder of zinc oxide particles (20 nm) surface-treated with amino acid treatment C was obtained in the same manner as in Production Example 1, except that the surface treatment agent was changed to stearoyl glutamic acid (Amisoft HA-P, manufactured by Ajinomoto Co., Ltd.) (hereinafter referred to as "amino acid C").

[0102] (Production Example 7: Zinc oxide particles (20 nm) surface-treated with amino acid salt D) A powder of zinc oxide particles (20 nm) surface-treated with amino acid salt D was obtained in the same manner as in Production Example 1, except that the surface treatment agent was changed to myristoyl glutamine potassium salt (Ajinomoto Co., Amisoft MK-11) (hereinafter referred to as "amino acid salt D").

[0103] (Production Example 8: Zinc oxide particles (20 nm) surface-treated with vinylsilane) A powder of zinc oxide particles (20 nm) surface-treated with vinylsilane was obtained in the same manner as in Production Example 1, except that the surface treatment agent was changed to vinyltriethoxysilane (KBE-1003, manufactured by Shin-Etsu Chemical Co., Ltd.) (hereinafter referred to as "vinylsilane").

[0104] (Production Example 9: Zinc oxide particles (20 nm) surface-treated with acrylic silane) A powder of zinc oxide particles (20 nm) surface-treated with acrylic silane was obtained in the same manner as in Production Example 1, except that the surface treatment agent was changed to 3-acryloxypropyltrimethoxysilane (KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.) (hereinafter referred to as "acrylic silane").

[0105] (Production Example 10: Zinc oxide particles (350 nm) surface-treated with amino acid salt A) A powder of zinc oxide particles (350 nm) surface-treated with amino acid salt A was obtained in the same manner as in Production Example 1, except that non-surface-treated zinc oxide particles (manufactured by Sakai Chemical Industry Co., Ltd., FINEX-50, average primary particle diameter 20 nm) were changed to non-surface-treated zinc oxide particles (manufactured by Hakusui Tech, ultrafine zinc oxide for heat dissipation, average primary particle diameter 350 nm).

[0106] (Production Example 11: Titanium oxide particles (21 nm) surface-treated with aminosilane) The surfaces of 100 parts by mass of untreated titanium oxide particles (P25, manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 21 nm) were mechanochemically treated and bonded with 5 parts by mass of γ-aminopropyltriethoxysilane (KBE-903, manufactured by Shin-Etsu Chemical Co., Ltd.) (hereinafter referred to as "aminosilane") as a surface treatment agent by a gas phase method, and the resulting particles were washed with pure water and thoroughly dried to obtain a powder of titanium oxide particles (21 nm) surface-treated with aminosilane.

[0107] (Manufacturing of negatively charged laminated photoreceptors) Example 1 48.0 parts by mass of polyvinylphenol resin (product name Maruka Rincar MH-2: Maruzen Petrochemicals) as a resin binder for the undercoat layer, 42.0 parts by mass of melamine resin (product name Yuban 2021: Mitsui Chemicals, solid content ratio 75%), and 239.0 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid salt A obtained in Production Example 1 as a filler for the undercoat layer, were added to a mixed solvent of 1500.0 parts by mass of methanol and 300.0 parts by mass of butanol as a solvent to prepare a slurry. The mass ratio (F / B) of the filler and the resin binder in this slurry was 75 / 25. 5 L of the obtained slurry was processed for 20 passes at a processing liquid flow rate of 300 ml and a disk peripheral speed of 4 m / s using a disk-type bead mill filled with zirconia beads having a bead diameter of 0.3 mm at a bulk filling rate of 80 v / v% relative to the vessel capacity, to prepare an undercoat layer coating liquid.

[0108] The prepared undercoat layer coating solution was used to form an undercoat layer 2 on a cylindrical aluminum substrate 1 as a conductive substrate by dip coating. The undercoat layer 2 obtained by drying at a drying temperature of 135° C. for a drying time of 20 minutes had a post-drying thickness of 1.5 μm.

[0109] Next, 1 part by mass of polyvinyl butyral resin (S-LEC BM-1, manufactured by Sekisui Chemical Co., Ltd.) as a resin binder for the charge generation layer was dissolved in 98 parts by mass of dichloromethane. 2 parts by mass of α-type titanyl phthalocyanine described in U.S. Patent No. 8,053,570 as a charge generation material was added to this to prepare a slurry. 5 L of the prepared slurry was processed for 10 passes at a processing solution flow rate of 300 mL and a disk peripheral speed of 3 m / s using a disk-type bead mill filled with zirconia beads having a bead diameter of 0.4 mm at a bulk filling rate of 85 v / v% relative to the vessel capacity, to prepare a charge generation layer coating solution.

[0110] Using the obtained charge generating layer coating liquid, a charge generating layer 4 was formed by dip coating on the conductive substrate 1 coated with the above-mentioned undercoat layer 2. The charge generating layer 4 obtained by drying under conditions of a drying temperature of 80° C. and a drying time of 30 minutes had a post-drying thickness of 0.3 μm.

[0111] Next, 5 parts by mass of a compound represented by the following structural formula (3) and 5 parts by mass of a compound represented by the following structural formula (4) as a charge transport material (CTM) of the charge transport layer, and 10 parts by mass of a polycarbonate resin (Iupizeta PCZ-500 manufactured by Mitsubishi Gas Chemical Co., Ltd.) as a resin binder of the charge transport layer were dissolved in 80 parts by mass of dichloromethane. After dissolution, 0.1 parts by mass of silicone oil (KP-340 manufactured by Shin-Etsu Polymer Co., Ltd.) were added to prepare a charge transport layer coating liquid. Using the prepared charge transport layer coating liquid, a charge transport layer 5 was formed on the charge generation layer 4 by dip coating. The film thickness of the charge transport layer 5 obtained by drying at a temperature of 90° C. for 60 minutes after drying was 25 μm. In this way, an electrophotographic photoreceptor was prepared.

[0112] TIFF0007567538000001.tif52153

[0113] Example 2 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the amount of solvent in the undercoat layer coating solution used in Example 1 was adjusted and the dried thickness of the undercoat layer was changed to 0.1 μm.

[0114] Example 3 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the amount of solvent in the undercoat layer coating solution used in Example 1 was adjusted and the dried thickness of the undercoat layer was changed to 10.0 μm.

[0115] Example 4 118.1 parts by mass of polyvinylphenol resin (trade name: Marukancar MH-2: manufactured by Maruzen Petrochemical Co., Ltd.) as a resin binder for the undercoat layer, 104.9 parts by mass of melamine resin (trade name: Yuban 2021: manufactured by Mitsui Chemicals, Inc., solid content ratio 75%), and 106.0 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid salt A obtained in Production Example 1 as a filler were added to a mixed solvent of 1500.0 parts by mass of methanol and 300.0 parts by mass of butanol to prepare a slurry. The mass ratio (F / B) of the filler and the resin binder in this slurry was 35 / 65. This slurry was used in the same manner as in Example 1 to prepare an undercoat layer coating liquid, and an electrophotographic photoreceptor was prepared in the same manner as in Example 1.

[0116] Example 5 7.0 parts by mass of polyvinylphenol resin (trade name: Marukalinker MH-2: manufactured by Maruzen Petrochemical Co., Ltd.) as a resin binder for the undercoat layer, 6.1 parts by mass of melamine resin (trade name: Yuban 2021: manufactured by Mitsui Chemicals, Inc., solid content ratio 75%), and 315.8 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid salt A obtained in Production Example 1 as a filler were added to a mixed solvent of 1500.0 parts by mass of methanol and 300.0 parts by mass of butanol to prepare a slurry. The mass ratio (F / B) of the filler and the resin binder in this slurry was 90 / 10. This slurry was used in the same manner as in Example 1 to prepare an undercoat layer coating liquid, and an electrophotographic photoreceptor was prepared in the same manner as in Example 1.

[0117] Example 6 As the resin binder of the undercoat layer, 80.0 parts by mass of melamine resin (AMIDIR G-821-60 manufactured by DIC Corporation, solid content 60%), 70.0 parts by mass of acrylic resin (ACRYDIC 54-172-60 manufactured by DIC Corporation, solid content 45%), and 239.0 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid salt A obtained in Production Example 1 as the filler were added to a mixed solvent of 1500.0 parts by mass of methanol and 300.0 parts by mass of butanol to prepare a slurry. The mass ratio (F / B) of the filler to the resin binder in this slurry was 75 / 25. This slurry was used in the same manner as in Example 1 to prepare an undercoat layer coating liquid, and an electrophotographic photoreceptor was prepared in the same manner as in Example 1.

[0118] Example 7 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to zinc oxide particles (20 nm) that had been surface-treated with amino acid salt A obtained in Production Example 2.

[0119] Example 8 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to zinc oxide particles (20 nm) that had been surface-treated with amino acid salt A obtained in Production Example 3.

[0120] Example 9 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to zinc oxide particles (35 nm) that had been surface-treated with amino acid salt A obtained in Production Example 4.

[0121] Example 10 An electrophotographic photoreceptor was prepared in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to zinc oxide particles (350 nm) that had been surface-treated with amino acid salt A obtained in Production Example 10.

[0122] Example 11 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to zinc oxide particles (20 nm) that had been surface-treated with amino acid salt B obtained in Production Example 5.

[0123] Example 12 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to zinc oxide particles (20 nm) that had been surface-treated with amino acid C obtained in Production Example 6.

[0124] (Example 13) An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to zinc oxide particles (20 nm) that had been surface-treated with amino acid salt D obtained in Production Example 7.

[0125] Comparative Example 1 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to zinc oxide particles that had not been surface-treated (manufactured by Sakai Chemical Industry Co., Ltd., FINEX-50, average primary particle diameter 20 nm).

[0126] Comparative Example 2 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to the zinc oxide particles (20 nm) that had been surface-treated with vinylsilane obtained in Production Example 8.

[0127] Comparative Example 3 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to the zinc oxide particles (20 nm) treated with acrylic silane obtained in Production Example 9.

[0128] Comparative Example 4 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to the aminosilane-surface-treated titanium oxide particles (21 nm) obtained in Production Example 11.

[0129] Example 14 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler of the undercoat layer in Example 1 was changed to 47.8 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid salt A obtained in Production Example 1 as a first filler (F1), and 191.2 parts by mass of titanium oxide particles (21 nm) surface-treated with aminosilane obtained in Production Example 11 as a second filler (F2) (F1 / F2=20 / 80).

[0130] Example 15 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler in the undercoat layer in Example 1 was changed to 119.5 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid salt A obtained in Production Example 1 as a first filler (F1), and 119.5 parts by mass of titanium oxide particles (21 nm) surface-treated with aminosilane obtained in Production Example 11 as a second filler (F2) (F1 / F2=50 / 50).

[0131] (Example 16) An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler of the undercoat layer in Example 1 was changed to 191.2 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid salt A obtained in Production Example 1 as a first filler (F1), and 47.8 parts by mass of titanium oxide particles (21 nm) surface-treated with aminosilane obtained in Production Example 11 as a second filler (F2) (F1 / F2=80 / 20).

[0132] (Example 17) An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler of the undercoat layer in Example 1 was changed to 234.2 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid salt A obtained in Production Example 1 as a first filler (F1), and 4.8 parts by mass of titanium oxide particles (21 nm) surface-treated with aminosilane obtained in Production Example 11 as a second filler (F2) (F1 / F2=98 / 2).

[0133] (Example 18) An electrophotographic photoreceptor was prepared in the same manner as in Example 15, except that the charge transport material used in Example 15 was changed to 10 parts by mass of a compound represented by the following structural formula (5).

[0134] TIFF0007567538000002.tif57153

[0135] (Example 19) An electrophotographic photoreceptor was produced in the same manner as in Example 15, except that the first filler (F1) used in Example 15 was changed to zinc oxide particles (20 nm) that had been surface-treated with the amino acid salt B obtained in Production Example 5.

[0136] (Example 20) An electrophotographic photoreceptor was prepared in the same manner as in Example 15, except that the second filler (F2) used in Example 15 was changed to non-surface-treated titanium oxide particles (P25, average primary particle diameter 21 nm, manufactured by Nippon Aerosil Co., Ltd.).

[0137] Example 21 An electrophotographic photoreceptor was produced in the same manner as in Example 15, except that the second filler (F2) used in Example 15 was changed to titanium oxide particles (MT-01, manufactured by Teika Corporation, average primary particle diameter 10 nm) and aminosilane treatment was carried out in the same manner as in Production Example 11.

[0138] Example 22 An electrophotographic photoreceptor was produced in the same manner as in Example 15, except that the second filler (F2) used in Example 15 was changed to titanium oxide particles (manufactured by Teika Corporation, JR, average primary particle diameter 270 nm) and aminosilane treatment was carried out in the same manner as in Production Example 11.

[0139] Example 23 An electrophotographic photoreceptor was produced in the same manner as in Example 15, except that the second filler (F2) used in Example 15 was changed to zinc oxide particles that had not been surface-treated (manufactured by Sakai Chemical Industry Co., Ltd., FINEX-50, average primary particle diameter 20 nm).

[0140] Example 24 An electrophotographic photoreceptor was produced in the same manner as in Example 15, except that the second filler (F2) used in Example 15 was changed to zinc oxide particles (35 nm) that had been surface-treated with the amino acid salt A obtained in Production Example 4.

[0141] (Example 25) An electrophotographic photoreceptor was produced in the same manner as in Example 15, except that the second filler (F2) used in Example 15 was changed to zinc oxide particles (20 nm) that had been surface-treated with the amino acid salt D obtained in Production Example 7.

[0142] (Example 26) An electrophotographic photoreceptor was produced in the same manner as in Example 15, except that the second filler (F2) used in Example 15 was changed to zinc oxide particles (20 nm) that had been surface-treated with the amino acid salt B obtained in Production Example 5.

[0143] Example 27 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the filler of the undercoat layer in Example 1 was changed to 95.7 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid salt A obtained in Production Example 1 as a first filler (F1), 95.7 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid salt B obtained in Production Example 5 as a second filler (F2), and 47.8 parts by mass of zinc oxide particles (20 nm) surface-treated with amino acid C obtained in Production Example 6 as a third filler (F3) (F1 / F2 / F3=40 / 40 / 20).

[0144] (Example 28) An electrophotographic photoreceptor was produced in the same manner as in Example 27, except that the third filler (F3) used in Example 27 was changed to zinc oxide particles that had not been surface-treated (manufactured by Sakai Chemical Industry Co., Ltd., FINEX-50, average primary particle diameter 20 nm).

[0145] (Example 29) An electrophotographic photoreceptor was produced in the same manner as in Example 27, except that the third filler (F3) used in Example 27 was changed to the aminosilane-surface-treated titanium oxide particles (21 nm) obtained in Production Example 11.

[0146] Comparative Example 5 An electrophotographic photoreceptor was produced in the same manner as in Example 15, except that the first filler (F1) used in Example 15 was changed to zinc oxide particles that had not been surface-treated (manufactured by Sakai Chemical Industry Co., Ltd., FINEX-50, average primary particle diameter 20 nm).

[0147] <Changes in undercoat layer coating solution over time> The undercoat layer coating solution was transferred to a glass bottle and stored at room temperature and humidity. Over time, the bottle was visually observed and evaluated for the presence or absence of filler settling based on the following criteria. ◎: No settling after 14 days. ◯: No settling was observed after 7 days, and slight settling was observed after 14 days. △: No settling was observed after 2 days, and slight settling was observed after 7 days. ×: Sedimentation was observed after 2 days.

[0148] As the performance of the photoreceptor with respect to transfer, the occurrence of ghosts due to transfer and the change in charging potential were evaluated.

[0149] <Transcription Ghost> Each of the electrophotographic photoreceptors obtained in Examples 1 to 29 and Comparative Examples 1 to 5 was mounted on a commercially available printer (Samsung Electronics Co., Ltd., MultiXpress X7600LX) and the printed images were evaluated. Fig. 4 is a diagram that illustrates the evaluation method. In the printer, as shown in FIG. 4(a), a sheet of paper 29 and a sheet of paper 30 are successively inserted between the photoconductor 7 and the transfer charger 26, and a halftone image is printed on the second sheet of paper 30. When the image on the second sheet is halftone, as shown in FIG. 4(b), the difference in density that appears in the halftone image due to the transfer voltage between the first sheet of paper 29 and the second sheet of paper 30 is regarded as a ghost due to transfer (transfer ghost). The transfer ghost appears, for example, as a band having a light and dark density at a distance W of one rotation of the photoconductor from the edge of the paper 29. The width of the band corresponds to the distance (paper distance g) between the paper 29 and the paper 30. FIG. 4(c) shows an example in which the transfer ghost does not appear. Using this procedure, the transfer ghost was judged based on the following criteria. : No transfer ghosting was observed, and the result was at a very good level. ○: A very slight transfer ghost that does not cause any problems in practical use. △: There is slight transfer ghosting that is problematic in practical use. ×: A level where transfer ghosts are clearly visible.

[0150] <Charge potential difference> Using a photoconductor drum electrical characteristic measuring system CYNTHIA 93 manufactured by Gentec, each photoconductor was arranged according to the arrangement in the explanatory diagram of the electrophotographic device shown in Figure 3. In the figure, the reference numerals 7 indicate the photoconductor, 8 the charging roller, 9 the electrometer, and 10 the transfer roller. The photoconductor 7 charged to -600V was rotated in the direction of the arrow in Figure 3 at a peripheral speed of 100 mm / s, and the transfer voltage was set to 0 kV for three rotations, then the transfer voltage was increased to 0.2 kV for three rotations, and the transfer voltage was then increased by 0.2 kV every three rotations until it reached 6.0 kV. The difference (ΔV0) between the charge potential of the photoconductor when the transfer voltage was 0 kV and the charge potential of the cycle immediately after the transfer voltage of 6.0 kV was applied was measured to measure the degree of transfer influence. By applying a transfer voltage (6.0 kV) higher than that of the printer and measuring ΔV0, it is possible to evaluate the tendency of slight ghosting that cannot be detected by evaluation using the printer. When the charging potential difference ΔV0 is small, there is a tendency for transfer ghosts in the image to be less likely to occur, so the degree of the effect can be evaluated depending on the magnitude of ΔV0.

[0151] <Electrical characteristics> Each of the electrophotographic photoreceptors obtained in Examples 1 to 29 and Comparative Examples 1 to 5 was mounted in a black drum cartridge of a commercially available color printer (Samsung Electronics Co., Ltd., MultiXpress X7600LX), and a test pattern with a print rate of 1.1% was printed on 10,000 sheets of A3 paper using black toner, and the electrical characteristics of the electrophotographic photoreceptor were measured before and after printing.

[0152] In an environment with a temperature of 22°C and a humidity of 50%, the surface of the photoreceptor was charged to -650V by corona discharge in a dark place, and the surface potential V0 immediately after charging was measured. Then, after leaving it in a dark place for 5 seconds, the surface potential V5 was measured, and the potential retention rate Vk5 (%) 5 seconds after charging was calculated according to the following calculation formula (1). Vk5 = V5 / V0 × 100 (1)

[0153] Next, a halogen lamp was used as the light source, and a filter was used to split the light into 1.0 μW / cm at 780 nm. 2The exposure light required for the surface potential to attenuate to -300 V when the photoconductor is irradiated with the exposure light of E1 / 2 (μJ / cm) for 5 seconds from the point when the surface potential becomes -600 V is 2 ), and the residual potential on the surface of the photoconductor 5 seconds after exposure was determined as VL (V). The retention rate decrease amount ΔVk5 and the residual potential increase amount ΔVL were evaluated according to the following formula. Retention rate reduction amount ΔVk5 = Vk5 before printing - Vk5 after printing 10000 sheets Residual potential rise ΔVL = VL after printing 10,000 sheets - VL before printing

[0154] ΔVk5 indicates the degree of decrease in charge retention rate before and after printing. If this value is large, the decrease in charge retention rate after printing is large and fogging on white paper is likely to occur. ΔVL indicates the degree of increase in residual potential before and after printing. If this value is large, the print density is likely to decrease.

[0155] The results are shown in Tables 3 and 4 below.

[0156] [Table 1]

[0157] *1) Resin A: Polyvinylphenol resin, Marukalinker (registered trademark) MH-2 (manufactured by Maruzen Petrochemical Co., Ltd.), Resin B: Melamine resin U-BAN (registered trademark) 2021 (Mitsui Chemicals, Inc.), Resin C: Melamine resin AMIDIR (registered trademark) G-821-60 (manufactured by DIC Corporation), Resin D: Acrylic resin ACRYDIC (registered trademark) 54-172-60 (manufactured by DIC Corporation)

[0158] [Table 2]

[0159] [Table 3]

[0160] [Table 4]

[0161] From the results of Tables 1 to 4 above, it was confirmed that a photoreceptor that is less likely to generate transfer ghosts can be obtained by using zinc oxide particles surface-treated with N-acylated amino acid or its salt as a filler in the undercoat layer. Furthermore, a photoreceptor excellent in transfer performance and electrical properties was obtained by using zinc oxide particles surface-treated with N-acylated amino acid or its salt mixed with other metal oxide particles as a filler in the undercoat layer. In particular, from the results of Examples 14 to 19, 21, 22, and 29, it can be seen that a photoreceptor that is less likely to generate ghosts and has a better effect of suppressing transferred ghost images can be obtained by using zinc oxide particles surface-treated with N-acylated amino acid or its salt in combination with titanium oxide particles surface-treated with an aminosilane compound as a filler.

[0162] In addition, the undercoat layer coating solution according to each Example has good coating solution stability, and can provide a photoreceptor that is stable in production and requires little production processing such as redispersion or filtration to break up sediments. It was confirmed that in each Example, a photoreceptor was obtained that had excellent stability in the potential retention rate of the photoreceptor surface before and after repeated printing and in which an increase in the residual potential of the photoreceptor surface was sufficiently suppressed.

[0163] In contrast, the photoreceptors of the comparative examples use metal oxide particles other than zinc oxide particles surface-treated with an N-acylated amino acid or its salt as a filler, and therefore the suppression of transfer ghosts is insufficient, and the coating liquid stability, transfer performance, and electrical properties are also insufficient.

[0164] (Manufacturing of positively charged single-layer photoreceptors) (Example 30) The undercoat layer coating solution prepared in the same manner as in Example 1 was dip-coated onto the outer periphery of an aluminum cylinder having an outer diameter of 24 mm as the conductive substrate 1, and dried under conditions of a drying temperature of 135°C and a drying time of 20 minutes to form an undercoat layer with a thickness of 0.5 μm.

[0165] On the undercoat layer, a charge generating material having the following formula: 1.5 parts by mass of metal-free phthalocyanine represented by the formula (TIFF0007567538000007.tif44153) and a charge transport material represented by the formula (I): 45 parts by mass of a stilbene compound represented by the formula (TIFF0007567538000008.tif41153) and a compound represented by the formula (I) below as an electron transport material: A photosensitive layer coating liquid was prepared by dissolving and dispersing 35 parts by mass of the compound represented by TIFF0007567538000009.tif46153 and 130 parts by mass of a polycarbonate resin (Iupizeta PCZ-500, manufactured by Mitsubishi Gas Chemical Company, Inc.) as a resin binder in 850 parts by mass of tetrahydrofuran, which was then dip-coated and dried at a temperature of 100° C. for 60 minutes to form a photosensitive layer with a thickness of 25 μm, thereby producing a single-layer type electrophotographic photoreceptor.

[0166] (Example 31) A single-layer type electrophotographic photoreceptor was prepared in the same manner as in Example 30, except that the undercoat layer was changed to the same as in Example 11.

[0167] Example 32 A single-layer type electrophotographic photoreceptor was prepared in the same manner as in Example 30, except that the undercoat layer was changed to the same as in Example 12.

[0168] (Example 33) A single-layer type electrophotographic photoreceptor was prepared in the same manner as in Example 30, except that the undercoat layer was changed to the same as in Example 13.

[0169] (Example 34) A single-layer type electrophotographic photoreceptor was prepared in the same manner as in Example 30, except that the undercoat layer was changed to the same as in Example 26.

[0170] Example 35 A single-layer type electrophotographic photoreceptor was prepared in the same manner as in Example 30, except that the undercoat layer was changed to the same as in Example 15.

[0171] Comparative Example 6 A single-layer type electrophotographic photoreceptor was produced in the same manner as in Example 30, except that the undercoat layer was changed to the same as in Comparative Example 1.

[0172] Comparative Example 7 A single-layer type electrophotographic photoreceptor was produced in the same manner as in Example 30, except that the undercoat layer was changed to the same as in Comparative Example 2.

[0173] Comparative Example 8 A single-layer type electrophotographic photoreceptor was produced in the same manner as in Example 30, except that the undercoat layer was changed to the same as in Comparative Example 3.

[0174] Comparative Example 9 A single-layer type electrophotographic photoreceptor was produced in the same manner as in Example 30, except that the undercoat layer was changed to the same as in Comparative Example 4.

[0175] Comparative Example 10 A single-layer type electrophotographic photoreceptor was produced in the same manner as in Example 30, except that the undercoat layer was changed to the same as in Comparative Example 5.

[0176] <Charge potential difference> Using a photoconductor drum electrical characteristic measuring system CYNTHIA 93 manufactured by Gentec, each photoconductor was arranged according to the arrangement in the explanatory diagram of the electrophotographic device shown in FIG. 3. In the figure, the reference numerals 7 indicate the photoconductor, 8 the charging roller, 9 the electrometer, and 10 the transfer roller. The photoconductor 7 charged to +600V was rotated in the direction of the arrow in FIG. 3 at a peripheral speed of 100 mm / s, and the transfer voltage was set to 0 kV for three rotations, then the transfer voltage was lowered to -0.2 kV for three rotations, and thereafter the transfer voltage was lowered by -0.2 kV for every three rotations until it reached -6.0 kV. The difference between the charge potential of the photoconductor when the transfer voltage was 0 kV and the charge potential of the cycle immediately after the transfer voltage of -6.0 kV was measured to measure the degree of transfer influence. The larger this charge potential difference (absolute value), the more likely it is that transfer ghosts in the image are visually confirmed.

[0177] The results are shown in Table 6 below.

[0178] [Table 5]

[0179] [Table 6]

[0180] From the results of Tables 5 to 6 above, it was confirmed that, even for a positively charged photoreceptor, by using zinc oxide particles surface-treated with an N-acylated amino acid or its salt as a filler in the undercoat layer, either alone or in combination with other metal oxide particles, a photoreceptor that is considered to be less susceptible to the influence of the transfer voltage and less likely to cause transfer ghosts can be obtained. In particular, from the results of Example 35, it is found that by using zinc oxide particles surface-treated with an N-acylated amino acid or its salt in combination with titanium oxide particles surface-treated with an aminosilane compound as a filler, a better photoreceptor that is less susceptible to the influence of the transfer voltage can be obtained.

[0181] (Manufacturing of positively charged laminated photoreceptors) (Example 36) The undercoat layer coating solution prepared in the same manner as in Example 1 was dip-coated onto the outer periphery of an aluminum cylinder having an outer diameter of 24 mm as the conductive substrate 1, and dried under conditions of a drying temperature of 135° C. and a drying time of 20 minutes to form an undercoat layer with a thickness of 0.5 μm.

[0182] A charge transport layer coating liquid was prepared by dissolving 5 parts by mass of a polycarbonate resin (manufactured by Mitsubishi Gas Chemical Company, Inc., Iupizeta PCZ-500) as a resin binder and 5 parts by mass of the charge transport material used in Example 30 in 80 parts by mass of tetrahydrofuran. This charge transport layer coating liquid was dip-coated on the outer periphery of a conductive substrate on which an undercoat layer had been formed by coating, and dried at a temperature of 120° C. for 60 minutes to form a charge transport layer with a thickness of 15 μm.

[0183] 0.1 parts by mass of Y-type titanyl phthalocyanine as a charge generating material, 2 parts by mass of the charge transporting material used in Example 30 as a hole transporting material, 5 parts by mass of the compound used in Example 30 as an electron transporting material, and 13 parts by mass of polycarbonate resin (manufactured by Mitsubishi Gas Chemical Company, Inc., Iupizeta PCZ-500) as a resin binder were dissolved and dispersed in 120 parts by mass of 1,2-dichloroethane to prepare a charge generating layer coating liquid. This charge generating layer coating liquid was applied by dip coating onto the charge transporting layer and dried at a temperature of 100° C. for 60 minutes to form a charge generating layer with a film thickness of 15 μm, thereby preparing a positively charged laminated electrophotographic photoreceptor.

[0184] (Example 37) A positively charged multi-layer electrophotographic photoreceptor was prepared in the same manner as in Example 36, except that the undercoat layer was changed to the same as in Example 15.

[0185] Comparative Example 11 A positively charged multi-layer electrophotographic photoreceptor was prepared in the same manner as in Example 36, except that the undercoat layer was changed to the same as in Comparative Example 1.

[0186] Comparative Example 12 A positively charged multi-layer electrophotographic photoreceptor was prepared in the same manner as in Example 36, except that the undercoat layer was changed to the same as in Comparative Example 4.

[0187] Comparative Example 13 A positively charged multi-layer electrophotographic photoreceptor was prepared in the same manner as in Example 36, except that the undercoat layer was changed to the same as in Comparative Example 5.

[0188] <Charge potential difference> Using a photoconductor drum electrical characteristic measuring system CYNTHIA 93 manufactured by Gentec, each photoconductor was arranged according to the arrangement in the explanatory diagram of the electrophotographic device shown in FIG. 3. In the figure, the reference numerals 7 indicate the photoconductor, 8 the charging roller, 9 the electrometer, and 10 the transfer roller. The photoconductor 7 charged to +600V was rotated in the direction of the arrow in FIG. 3 at a peripheral speed of 100 mm / s, and the transfer voltage was set to 0 kV for three rotations, then the transfer voltage was lowered to -0.2 kV for three rotations, and thereafter the transfer voltage was lowered by -0.2 kV for every three rotations until it reached -6.0 kV. The difference between the charge potential of the photoconductor when the transfer voltage was 0 kV and the charge potential of the cycle immediately after the transfer voltage of -6.0 kV was measured to measure the degree of transfer influence. The larger this charge potential difference (absolute value), the more likely it is that transfer ghosts in the image are visually confirmed.

[0189] The results are shown in Table 8 below.

[0190] [Table 7]

[0191] [Table 8]

[0192] From the results of Tables 7 to 8 above, it was confirmed that a photoreceptor that is considered to be less susceptible to the transfer voltage and less likely to cause transfer ghosts can be obtained by using zinc oxide particles surface-treated with N-acylated amino acid or its salt as a filler in the undercoat layer, either alone or in a mixture with other metal oxide particles. In particular, from the results of Example 37, it can be seen that a better photoreceptor that is less susceptible to the transfer voltage can be obtained by using zinc oxide particles surface-treated with N-acylated amino acid or its salt and titanium oxide particles surface-treated with an aminosilane compound in combination as a filler.

[0193] In this way, it can be seen that by using zinc oxide particles that have been surface-treated with an N-acylated amino acid or its salt as a filler in the undercoat layer of a photoreceptor, either alone or in combination with other metal oxides, a photoreceptor that does not cause transfer ghosts and has excellent transfer performance and electrical performance can be obtained. [Explanation of symbols]

[0194] 1. Conductive substrate 2 Undercoat layer 3. Single-layer photosensitive layer 4. Charge generation layer 5 Charge transport layer 7 Photoreceptor 8. Charging roller 9 Electrometer 10 Transfer roller 21 Electrostatic materials 22 High voltage power supply 23 Image exposure member (exposure light source) 24 Developer 241 Developing roller 25 Paper feed member 251 Paper feed roller 252 Paper feed guide 26 Transfer charger (direct charging type) 27 Cleaning Equipment 271 Cleaning Blade 28 Antistatic material 29 Paper (1st print) 30 Paper (2nd print) 60 Electrophotographic device 300 Photosensitive layer

Claims

1. A conductive substrate; An electrophotographic photoreceptor comprising an undercoat layer and a photosensitive layer provided in this order on the conductive substrate, The electrophotographic photoreceptor wherein the undercoat layer contains a resin binder and a first filler, and the first filler comprises zinc oxide particles that have been surface-treated with an N-acylated amino acid or a salt of an N-acylated amino acid.

2. The electrophotographic photoreceptor according to claim 1, further comprising a second filler, the second filler including at least one kind of metal oxide particles different from the zinc oxide particles surface-treated with the N-acylated amino acid or the salt of the N-acylated amino acid.

3. 3. The electrophotographic photoreceptor according to claim 2, wherein the metal oxide particles are made of one or more metal oxides selected from the group consisting of zinc oxide, titanium oxide, tin oxide, zirconium oxide, silicon oxide, copper oxide, magnesium oxide, antimony oxide, vanadium oxide, yttrium oxide and niobium oxide.

4. 3. The electrophotographic photoreceptor according to claim 2, wherein the second filler comprises titanium oxide particles which have been surface-treated with an aminosilane compound.

5. 5. The electrophotographic photoreceptor according to claim 1, wherein the zinc oxide particles have an average primary particle size of 1 nm to 350 nm.

6. 6. The electrophotographic photoreceptor according to claim 1, wherein the resin binder comprises two or more resins selected from the group consisting of acrylic resins, melamine resins and polyvinylphenol resins.

7. 7. The electrophotographic photoreceptor according to claim 1, wherein the photosensitive layer contains a charge generating material, and the charge generating material contains at least one material selected from the group consisting of titanyl phthalocyanine and metal-free phthalocyanine.

8. 8. The electrophotographic photoreceptor according to claim 1, wherein the photosensitive layer is a laminated type photosensitive layer including a charge generating layer and a charge transporting layer.

9. 8. The electrophotographic photoreceptor according to claim 1, wherein the photosensitive layer is a single-layer type photosensitive layer comprising a single layer containing a charge generating material and a charge transporting material.

10. In producing the electrophotographic photoreceptor according to any one of claims 1 to 9, preparing an undercoat layer coating solution containing zinc oxide particles surface-treated with the N-acylated amino acid or a salt thereof; forming the undercoat layer on the conductive substrate using the undercoat layer coating liquid; A method for producing an electrophotographic photoreceptor comprising the steps of:

11. 10. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to claim 1.

Citation Information

Patent Citations

  • Electrophotographic sensitive body

    JP1989178970A

  • Printing plate for electrophotographic plate making

    JP1989185668A

  • Production of electrophotographic photoreceptor

    JP1995261411A

  • Electrophotography photoreceptor

    JP1996272114A

  • Electrophotographic photoreceptor

    JP1997304958A