Manufacturing method for RTB sintered magnets
The method integrates RH introduction into the sintering process to enhance R-T-B sintered magnets' magnetic properties, eliminating the need for a separate diffusion step and simplifying mass production.
Patent Information
- Application Number
- JP2021032885
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-02
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-03-02
AI Technical Summary
Existing methods for producing R-T-B sintered magnets with high residual magnetic flux density (B r ) and coercive force (H cJ ) require additional diffusion processes, complicating mass production.
A manufacturing method involving the preparation of R-T-B alloy powder, molding, adhesion of RH-containing alloy powder to the molded object, and sintering at specific temperatures and times to introduce RH into the outer shell of main phase crystal grains without entering the center, eliminating the need for a separate diffusion process.
Achieves high B r and H cJ in R-T-B sintered magnets without complicating the mass production process by integrating RH introduction into the sintering step.
Smart Images

Figure 0007567558000007 
Figure 0007567558000008 
Figure 0007567558000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an RTB based sintered magnet. [Background technology]
[0002] In recent years, there has been high demand for rare earth sintered magnets, and among them, RTB sintered magnets (R is at least one rare earth element and contains at least one of Nd and Pr. T is mainly Fe, and B is boron) are known as the highest performance magnets, and are used in a variety of motors such as voice coil motors (VCM) for hard disk drives, motors for electric vehicles (EV, HV, PHV, etc.), motors for industrial equipment, and home appliances.
[0003] RTB sintered magnets are mainly R2T 14 It is composed of a main phase made of B compounds and a grain boundary phase located at the grain boundary of this main phase. 14 B compounds are ferromagnetic materials with high saturation magnetization and anisotropic magnetic field, and form the basis of the properties of RTB sintered magnets.
[0004] At high temperatures, the coercive force H of RTB sintered magnets cJ (Hereafter, simply "H cJ This causes irreversible thermal demagnetization. Therefore, the RTB sintered magnets used in electric vehicle motors, in particular, have a high H cJ It is required that the applicant have:
[0005] In RTB sintered magnets, R2T 14 When a part of the light rare earth element RL (e.g., Nd or Pr) contained in R in the B compound is replaced with a heavy rare earth element RH (e.g., Tb or Dy), H cJ It is known that the H cJ However, R2T 14 When RL in the B compound is replaced by RH, the H of the RTB sintered magnet cJ While the residual magnetic flux density Br (Hereinafter, simply "B r ") decreases. In recent years, the RH concentration in the outer periphery of the main phase crystal grains has been increased by diffusing RH from the surface of the RTB sintered magnet (after sintering) to the inside. r While suppressing the decline of cJ A method has been proposed to obtain
[0006] In Patent Document 1, a powder containing Rh such as Dy and Tb is placed on the surface of a sintered body, and the surface is heated at a temperature lower than the sintering temperature, whereby Dy, Tb, etc. are diffused from the powder into the sintered body to form H cJ A method for improving the
[0007] In Patent Document 2, RM alloy powder containing RH is present on the surface of an RTB sintered magnet, and heat treatment is performed to diffuse the RM alloy powder into the sintered magnet. cJ A method for improving the
[0008] In Patent Document 3, an adhesive is applied to the surface of an RTB sintered magnet, and powder of an RL-RH-M alloy or compound is attached to the surface, and the powder is then heat-treated to diffuse into the sintered magnet, producing H cJ A method for improving the [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2008-147634 A [Patent Document 2] JP 2008-263179 A [Patent Document 3] International Publication No. 2018 / 030187 Summary of the Invention [Problem to be solved by the invention]
[0010] By the methods described in Patent Documents 1 to 3, high B r and high HcJ However, since an additional diffusion step is required, the mass production process becomes complicated.
[0011] Therefore, this disclosure aims to achieve a high B r and high H cJ The present invention provides a production method for an RTB sintered magnet having the above properties. [Means for solving the problem]
[0012] In an exemplary embodiment, a method for producing an RTB based sintered magnet according to the present disclosure includes the steps of: preparing an RTB based (R is at least one rare earth element and includes at least one of Nd and Pr; T is at least one transition metal element and includes Fe; and B is boron) alloy powder; forming the RTB based alloy powder to obtain a compact; adhering an alloy powder including RH (RH is at least one selected from the group consisting of Tb, Dy, and Ho) to at least a portion of a surface of the compact; and sintering the compact after the adhering step at a temperature in the range of 900° C. or higher and lower than 1000° C. for a time in the range of 10 hours or higher and lower than 100 hours, wherein the sintering step reduces the median diameter of the alloy powder to d 50 (μm), the heating temperature in the sintering step is T (℃), the sintering time is t (h), and the amount of rare earth in the obtained sintered body, obtained by subtracting the amount of rare earth consumed as oxides, nitrides, and carbides from the total amount of rare earth, is the effective rare earth amount R eff (mass%), 40×d 50 -10×R eff -0.65×t+1155≦T≦40×d 50 -10×R eff The relationship -0.65×t+1175 holds.
[0013] In one embodiment, in the sintering step, the compact after the adhesion step is heated at a temperature in the range of 950° C. to 990° C. for a time in the range of 50 hours to 80 hours. Effect of the Invention
[0014] According to the embodiment of the present disclosure, it is possible to achieve a high B r and high H cJ It is possible to provide a production method for obtaining an RTB based sintered magnet having the above properties. [Brief description of the drawings]
[0015] [Figure 1A] FIG. 2 is an enlarged schematic cross-sectional view of a portion of an RTB based sintered magnet. [Figure 1B] 1B is a cross-sectional view showing a further enlarged schematic view of the dashed rectangular region in FIG. 1A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] First, the basic structure of the RTB based sintered magnet according to the present disclosure will be described. The RTB based sintered magnet has a structure in which powder particles of raw alloys are bonded together by sintering, and is mainly 14 It is composed of a main phase made of B compound particles and a grain boundary phase located at the grain boundaries of this main phase.
[0017] FIG. 1A is a cross-sectional view showing an enlarged schematic view of a portion of an RTB sintered magnet, and FIG. 1B is a cross-sectional view showing an enlarged schematic view of the dashed rectangular region in FIG. 1A. In FIG. 1A, an arrow of 5 μm in length is shown as an example for reference, showing the reference length of the size. As shown in FIG. 1A and FIG. 1B, an RTB sintered magnet is mainly 14 The grain boundary phase 14 is composed of a main phase 12 made of a B compound and a grain boundary phase 14 located at the grain boundary portion of the main phase 12. As shown in FIG. 1B, the grain boundary phase 14 is composed of two R2T 14 The two-particle grain boundary phase 14a in which B compound grains are adjacent, and the three R2T 14 The B compound grains include adjacent grain boundary triple junctions 14b. The typical main phase crystal grain size is 3 μm or more and 10 μm or less in terms of the average circle equivalent diameter of the magnet cross section. 14B compounds are ferromagnetic materials with high saturation magnetization and anisotropic magnetic field. Therefore, in RTB sintered magnets, the R2T 14 By increasing the proportion of B compounds, r It can improve R2T 14 In order to increase the ratio of B compounds, the amounts of R, T, and B in the raw alloy should be adjusted to R2T 14 It is sufficient to approach the stoichiometric ratio of the B compound (amount of R:amount of T:amount of B = 2:14:1). In addition, the main phase R2T 14 It is known that by substituting a part of R in B compounds with heavy rare earth elements such as Dy, Tb, and Ho, the saturation magnetization can be reduced while the anisotropic magnetic field of the main phase can be increased. In particular, the outer shell of the main phase that contacts the two-particle grain boundary phase is likely to be the starting point of magnetization reversal. Therefore, heavy rare earth diffusion technology that can preferentially substitute heavy rare earth elements in the outer shell of the main phase can efficiently achieve high H while suppressing the decrease in saturation magnetization. cJ is obtained.
[0018] As a result of intensive research, the inventors of the present invention have found that by adhering an alloy powder containing RH (RH being at least one selected from the group consisting of Tb, Dy and Ho) to the surface of a compact of RTB alloy powder and then carrying out a sintering process under predetermined conditions, it is possible to obtain a high B while eliminating the need for a separate diffusion process. r and high H cJ It has been found that an RTB-based sintered magnet having the above-mentioned properties can be obtained. This is believed to be because, while sintering, it is possible to simultaneously introduce RH in the RH-containing alloy powder into the outer periphery of the main phase crystal grains 12 with almost no introduction of RH into the central portion of the main phase crystal grains 12.
[0019] (RTB sintered magnet) The RTB based sintered magnet of the present disclosure has, for example, the following composition. R: 27-35 mass%, B: 0.80 to 1.20 mass%, Ga: 0 to 1.0 mass%, Cu: 0 to 0.5 mass%, T: Contains 60 mass% or more.
[0020] (R: 27-35 mass%) R is at least one rare earth element, including at least one of Nd and Pr. If R is less than 27 mass%, the liquid phase is not sufficiently generated during the sintering process, and it may be difficult to sufficiently densify the sintered body. On the other hand, if R exceeds 35 mass%, grain growth occurs during sintering, and H cJ The content of R is preferably 29.5 to 33.0 mass%. If the content of R is within this range, a higher B r can be obtained.
[0021] (B: 0.80~1.20mass%) When B is less than 0.80 mass%, B r On the other hand, if B exceeds 1.20 mass%, H cJ The B content is preferably 0.88 to 0.90 mass%. If the B content is within this range, a higher H cJ is obtained.
[0022] (Ga: 0 to 1.0 mass%) The Ga content is preferably 0 to 1.0 mass%, and more preferably 0.2 to 0.7 mass%. When the Ga content is in this range, the higher H cJ is obtained.
[0023] (Cu: 0-0.50 mass%) The Cu content is preferably 0 to 0.50 mass%, more preferably 0.05 to 0.30 mass%. When the Cu content is within this range, a higher H cJ is obtained.
[0024] (T:60mass% or more) T is at least one transition metal element and necessarily includes Fe. The content of T in the sintered magnet is preferably 61.5 to 69.5% by mass. Furthermore, when the total amount of T is taken as 100% by mass, up to 10% by mass of this can be substituted with Co. For example, 90% by mass of the total amount of T can be Fe and 10% by mass of Co. Furthermore, the total amount of T (100% by mass) may be Fe. The inclusion of Co can improve corrosion resistance, but if the amount of Co substituted exceeds 10% by mass of Fe, high B content will result. r may not be obtained. The sintered magnet of the present invention may further contain any other elements.
[0025] The method for producing an RTB based sintered magnet will now be described. (1) Preparation of RTB alloy powder Metals or alloys of each element are prepared to obtain a target composition, and flake-shaped alloys are produced using a strip casting method or the like. The RTB alloy powder may contain RH, but the RH concentration in the RTB alloy powder is preferably lower than the RH concentration in the RH-containing alloy powder to be attached to the compact. By setting the RH concentration in the RTB alloy powder lower than the RH concentration in the RH-containing alloy powder, the RH in the RH-containing alloy can be introduced more into the compact. The obtained flake-shaped alloy is subjected to hydrogen pulverization to obtain a coarsely pulverized powder having a size of, for example, 1.0 mm or less. Next, the coarsely pulverized powder is finely pulverized by a jet mill or the like to obtain a fine powder having a median diameter d 50 A finely pulverized powder (alloy powder) having a d50 of 2.5 μm≦d50≦4.5 μm (a value obtained by laser diffraction method using an airflow dispersion method) is obtained. A known lubricant may be used as an auxiliary agent in the coarsely pulverized powder before the jet mill pulverization, and in the alloy powder during and after the jet mill pulverization. d50 can be measured by an airflow dispersion laser diffraction method (in accordance with JIS Z 8825: 2013 revised edition). That is, in the present disclosure, d50 means a particle size (median diameter) at which the cumulative particle size distribution (volume basis) from the small particle size side is 50%. In this disclosure, d50 is measured using a particle size distribution analyzer "HELOS&RODOS" manufactured by Sympatec. Dispersion pressure: 4bar Measurement range: R2 Calculation mode: HRLD The d50 measured under the above conditions is shown.
[0026] (2) Molding process The obtained alloy powder is subjected to compaction in a magnetic field to obtain a compact. The compaction in a magnetic field may be performed by any known method including a dry compaction method in which dried alloy powder is inserted into a cavity of a die and compacted while a magnetic field is applied, and a wet compaction method in which a slurry in which the alloy powder is dispersed is poured into a cavity of a die and compacted while the dispersion medium of the slurry is discharged.
[0027] (3) Attachment process As an alloy powder containing RH, for example, RL-RH-M (M includes 0 mol%) alloy powder is prepared. Here, RL is at least one of light rare earth elements, and includes at least one of Nd and Pr. RH is at least one selected from the group consisting of Tb, Dy, and Ho. RL includes at least one of Nd and Pr, but may include at least one of La and Ce, for example. M preferably includes Cu. As other M elements, for example, one or more selected from Ga, Al, Zn, Fe, Co, and Ni may be included. The total content of RL and RH is 25 mol% or more and 100 mol% or less of the entire RL-RH-M alloy powder, and preferably 50 mol% or more and 100 mol% or less of the entire RL-RH-M alloy powder. The method for producing the RL-RH-M alloy powder is not particularly limited, and may be produced by crushing an ingot produced by a casting method, or by a known atomization method. In addition, as the alloy powder containing RH, a fluoride, oxide, or oxyfluoride containing RH may be used. The shape of the alloy powder containing RH is not particularly limited and may be any shape. The RH compound may take the shape of a film, foil, powder, block, particle, or the like. In addition, the size of the alloy powder containing RH is preferably 1 mm or less. By making the size 1 mm or less, it becomes easier to introduce RH into the inside of the molded body.
[0028] The alloy powder containing RH can be attached to at least a part of the surface of the compact by any method. For example, the alloy powder containing RH may be attached by scattering it on the surface of the compact, or the alloy powder containing RH may be dispersed in a solvent and the resulting slurry applied to the compact. The amount of the attached alloy powder is such that the mass ratio of the alloy powder containing RH to the entire compact to which the alloy powder containing RH is attached is 0.1 mass% or more and 5.0 mass% or less. By adjusting the amount of the attached alloy powder to this range, a high B r and high H cJ It is possible to obtain an RTB based sintered magnet having the above properties.
[0029] (4) Sintering process. In the sintering process, the RH in the alloy powder containing RH is introduced into the compact while sintering the compact. This eliminates the need for an additional diffusion process, making the mass production process less cumbersome. Conventionally, RTB sintered magnets are sintered at around 1100°C, depending on the composition, so that sufficient sintering is performed to obtain the desired magnetic properties. However, if the RH in the alloy powder containing RH is introduced into the compact at this temperature, the RH is introduced into the center of the main phase crystal grains, resulting in a high B r and high H cJ In order to suppress the introduction of RH into the inside of the main phase crystal grains, it is necessary to heat the RH-containing alloy powder at a temperature lower than 1000°C. However, as described above, since sintering requires heating at about 1100°C, sufficient sintering cannot be achieved at temperatures lower than 1000°C, resulting in a decrease in magnetic properties. For this reason, it has been considered difficult to simultaneously perform sintering and effectively introduce RH into the inside of the compact. In response to this, the inventors of the present invention have found that, by heating the compact after the adhesion step at a temperature in the range of 900°C to 1000°C for a time in the range of 10 hours to 100 hours, and performing a sintering step that satisfies the following detailed formula 1, it is possible to simultaneously perform sintering and introduce RH in the RH-containing alloy powder into the outer shell of the main phase crystal grains without introducing it into the center of the main phase crystal grains. This makes it possible to obtain a high B while eliminating the need for a diffusion step. r and high H cJIf the sintering temperature is less than 900°C, the sintering will be insufficient and the magnet will have a low molecular weight. r and H cJ On the other hand, if the sintering temperature is 1000°C or higher, the RH in the alloy powder containing RH is introduced into the center of the main phase crystal grains, resulting in a high B r and high H cJ If the sintering time is less than 10 hours, the introduction of RH into the compact from the alloy powder containing RH may be insufficient, and the resulting RTB sintered magnet may not have a high H content. cJ On the other hand, if the sintering time is more than 100 hours, the mass productivity may be deteriorated due to the excessively long sintering time. r and high H cJ To obtain an RTB sintered magnet having the above properties, the green body after the adhesion step is preferably heated at a temperature in the range of 950° C. to 990° C. for a time in the range of 50 hours to 80 hours.
[0030] The sintering process of the present disclosure is The sintering step is performed by setting the median diameter of the alloy powder to d 50 (μm), The heating temperature in the sintering step is T (℃), the sintering time is t (h), The amount of rare earth in the obtained sintered body, obtained by subtracting the amount of rare earth consumed as oxides, nitrides, and carbides from the total amount of rare earth, is called the effective amount of rare earth R. eff When expressed as (mass%), 40×d 50 -10×R eff -0.65×t+1155≦T≦40×d 50 -10×R eff -0.65×t+1175 (formula 1) The following relationship holds. The effective rare earth content of the sintered body is correlated with the alloy composition, manufacturing conditions, properties of the finely pulverized powder, etc. Therefore, the effective rare earth content of the sintered body can be controlled to satisfy formula 1 by using a value predicted based on past data from the alloy composition and manufacturing process. It is also possible to use a value obtained by previously preparing a sample under the same conditions and analyzing it.
[0031] As a result of the study, the inventors found that it is important to consider the particle size of the alloy powder and the amount of rare earth in the sintered body when determining the optimal heating temperature and sintering time for simultaneously introducing RH in the alloy powder containing RH into the outer periphery of the main phase crystal grains without introducing it into the center of the main phase crystal grains. Also, since the amount of rare earth in the sintered body is consumed by combining with oxygen, nitrogen, and carbon during the manufacturing process, the amount of rare earth as a metal that effectively acts during sintering changes during the manufacturing process. Therefore, the effective rare earth amount R, calculated by subtracting 6α+10β+8γ from the total rare earth amount in the sintered body (hereinafter sometimes referred to as "TRE"), where α is the amount of oxygen (mass%) in the sintered body, β is the amount of nitrogen (mass%), and γ is the amount of carbon (mass%) in the sintered body, is calculated as follows: eff In other words, it is effective to use the effective rare earth amount R eff (mass%) is the value calculated by the formula TRE-(6α+10β+8γ), where α (mass%) is the amount of oxygen contained in the sintered body, β (mass%) is the amount of nitrogen, and γ (mass%) is the amount of carbon. As a result of further investigations based on these findings, the inventors have found that by satisfying the above formula (1), RH in the alloy powder containing RH can be introduced into the outer periphery of the main phase crystal grains while sintering, with almost no introduction of RH into the center of the main phase crystal grains. This makes it unnecessary to carry out a new diffusion process, and avoids the complication of the mass production process while achieving a high B r and high H cJ Thus, an RTB based sintered magnet having the above properties can be obtained.
[0032] (5) Heat treatment process The sintered magnet obtained according to the embodiment of the present disclosure may be subjected to a heat treatment for the purpose of further improving the magnetic properties. For example, a first-stage heat treatment may be performed at a temperature (400°C or more and 600°C or less) lower than the sintering temperature. Alternatively, a first heat treatment may be performed at a relatively high temperature (700°C or more and sintering temperature or less), followed by a second heat treatment at a relatively low temperature (400°C or more and 600°C or less) (two-stage heat treatment). A specific example of the two-stage heat treatment may include a first heat treatment at a temperature of 750°C or more and 850°C or less for about 5 minutes to 500 minutes, and a second heat treatment at a temperature of 440°C or more and 550°C or less for about 5 minutes to 500 minutes. Between the first and second heat treatments, the magnet may be cooled to room temperature or to a temperature of 440°C or more and 550°C or less. Both the sintering and heat treatment are preferably carried out in a vacuum atmosphere or in an inert gas atmosphere (such as helium or argon). EXAMPLES
[0033] The present disclosure will be explained in more detail with reference to examples, but is not limited thereto.
[0034] Example 1 Each element was weighed to obtain the composition shown in No. A to L in Table 1, and the alloy was cast by strip casting to obtain a flake-shaped alloy. The obtained flake-shaped alloy was subjected to hydrogen embrittlement in a pressurized hydrogen atmosphere, and then subjected to a dehydrogenation treatment in which the alloy was heated to 550°C in a vacuum and cooled, to obtain a coarsely pulverized powder. The obtained coarsely pulverized powder was then finely pulverized using an airflow pulverizer (jet mill device) to obtain a median diameter d 50The RTB alloy powders obtained had a diameter (μm) of 3.1 μm for No. A to F and 3.6 μm for No. G to L. The results of the component analysis of the obtained RTB alloy powders are shown in Table 1, No. A to L. The components in Table 1 were measured using inductively coupled plasma optical emission spectroscopy (ICP-OES). The compositions of the alloy powders containing RH and the RTB sintered magnets were measured in the same manner. The obtained RTB alloy powders were mixed with 0.05 mass% zinc stearate as a lubricant based on 100 mass% of the finely pulverized powder, and then molded in a magnetic field to obtain a green body. The molding device used was a so-called rectangular magnetic field molding device (horizontal magnetic field molding device), in which the magnetic field application direction and the pressure direction are perpendicular to each other.
[0035] [Table 1]
[0036] Alloy powders containing RH with the composition shown in Table 2 were prepared. Specifically, Tb oxide powder with a size of 32 μm or less was prepared as No. a, Tb fluoride powder with a size of 32 μm or less was prepared as No. b. Tb metal chips with a size of 1 mm or less were prepared as No. c. Additionally, alloy powders containing Tb with a size of 106 μm or less were produced by atomization as No. d and No. e.
[0037] [Table 2]
[0038] Next, the alloy powder containing RH was adhered to the molded body by scattering it under the conditions shown in Tables 3 and 4 (adhering step). Note that for Nos. 1 to 12 in Table 3, the alloy powder containing RH was not adhered to the molded body. For No. 13 in Table 3, a molded body was produced using the RTB alloy powder No. A, and 1.0 mass% of the alloy powder No. a was adhered to the surface of the molded body. The amount of adhesion is the mass ratio of the alloy powder containing RH to the entire molded body to which the alloy powder containing RH was adhered. Nos. 14 to 60 in Tables 3 and 4 are also described in the same manner.
[0039] The molded body after the adhesion step was sintered at the temperature (sintering temperature) and time (sintering time) shown in Tables 5 and 6. The sintering temperature and sintering time were measured by attaching a thermocouple to the molded body. Tables 5 and 6 also show that the sintering step was performed at 40×d 50 -10×R eff -0.65×t+1155≦T≦40×d 50 -10×R eff -0.65×t+1175 (Formula 1)) was satisfied, and marked with ◯ when it was not satisfied. The RTB sintered magnet after sintering was subjected to a heat treatment in which it was held in a vacuum at 900°C for 2 hours, cooled to room temperature, and then held in a vacuum at 500°C for 2 hours, and then cooled to room temperature to obtain RTB sintered magnets (Nos. 1 to 60). The components of the obtained RTB sintered magnets are shown in Tables 5 and 6. Comparative examples were also prepared in which an alloy powder containing RH was attached to the sintered body after sintering and a diffusion treatment was performed (Nos. 61 and 62). Specifically, as shown in Nos. 61 and 62 in Tables 4 and 6, the RTB alloy powders of Nos. E and F were molded, respectively, and the obtained molded body was sintered at 1020°C for 4 hours to obtain a sintered body. The alloy containing RH of No. c was attached to the surface of the obtained sintered body. Then, a diffusion treatment was performed at 950°C for 10 hours. The RTB sintered magnet after the diffusion treatment was further subjected to the above-mentioned heat treatment. The compositions of the obtained RTB sintered magnets are shown in Table 6 as Nos. 61 and 62. Nos. 61 and 62 have almost the same compositions as Nos. 41 and 42. The heat-treated sintered magnets (Nos. 1 to 62) were machined to produce samples with a length of 7 mm, width of 7 mm and thickness of 7 mm. The properties of each sample (B r and H cJ The measurement results are shown in Tables 5 and 6.
[0040] [Table 3]
[0041] [Table 4]
[0042] [Table 5]
[0043] [Table 6]
[0044] As shown in Table 6 for Nos. 41 and 42 (examples of the present invention) and Nos. 61 and 62 (comparative examples), Nos. 41 and 42, which were subjected to the sintering process of the present disclosure, had almost the same B as Nos. 61 and 62, which were subjected to the diffusion process. r and H cJ This makes the diffusion process unnecessary while still achieving a high B r and high H cJ In addition, the magnets Nos. 13 to 18, which do not satisfy the formula 1 of the present disclosure, have a high B r and high H cJ No significant difference was obtained, and compared with Nos. 1 to 6, which did not have alloy powder containing RH attached, B r and H cJ In contrast, the RTB sintered magnets of the present invention all had H values lower than those of the RTB sintered magnets (Nos. 1 to 12) before RH was introduced into the compact from the alloy powder containing RH. cJ This improves the efficiency of the process, eliminating the need for a diffusion process and achieving a high B r and high H cJ Thus, an RTB-based sintered magnet having the above properties has been obtained. [Explanation of symbols]
[0045] 12 R2T 14 Main phase consisting of B compounds 14 Grain boundary phase 14a Two-grain grain boundary phase 14b Grain boundary triple point
Claims
1. preparing an R-T-B system alloy powder (R is at least one rare earth element, including at least one of Nd and Pr; T is at least one transition metal element, including Fe; and B is boron); a molding step of molding the R-T-B based alloy powder to obtain a compact; an adhesion step of adhering an alloy powder containing RH (RH being at least one selected from the group consisting of Tb, Dy and Ho) to at least a part of a surface of the compact; A sintering step of heating the compact after the adhesion step at a temperature in the range of 900° C. or more and less than 1000° C. for a time in the range of 10 hours or more and less than 100 hours, The sintering step is performed by setting the median diameter of the alloy powder to d 50 (μm), The heating temperature in the sintering step is T (° C.), the sintering time is t (h), The amount of rare earth in the obtained sintered body, obtained by subtracting the amount of rare earth consumed as oxides, nitrides and carbides from the total amount of rare earth, is called the effective amount of rare earth R. eff When (mass%) is 40×d 50 -10xR eff −0.65×t+1155≦T≦40×d 50 -10xR eff The relationship of -0.65×t+1175 holds. A method for producing an RTB based sintered magnet.
2. 2. The method for producing a sintered R-T-B based magnet according to claim 1, wherein in the sintering step, the compact after the adhering step is heated at a temperature in the range of 950° C. or higher and 990° C. or lower for a time in the range of 50 hours or higher and 80 hours or lower.
Citation Information
Patent Citations
Manufacturing method of rare earth permanent magnet
JP2008147634A
Rare earth permanent magnet and method of manufacturing the same
JP2008263179A
Rare earth sintered magnet and method for manufacturing the same
JP2012043968A
Sintered magnet, rotary machine provided with sintered magnet, and manufacturing method of sintered magnet
JP2012044203A
Rare earth magnet and method of producing the same
JP2012169464A