Ferromagnetic Josephson junction and its manufacturing method

The use of an iron alloy in the ferromagnetic layer for ferromagnetic Josephson junctions addresses instability issues by controlling saturation magnetization and exchange energy, ensuring stable critical current values.

JP7567830B2Active Publication Date: 2024-10-16KK TOYOTA CHUO KENKYUSHO
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022024367
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-02-21
Publication Date
2024-10-16
Estimated Expiration
2042-02-21

AI Technical Summary

Technical Problem

Existing ferromagnetic Josephson junctions face challenges in stabilizing critical current values and junction characteristics due to the thickness and magnetic exchange energy of the ferromagnetic layer, leading to instability and defects.

Method used

A ferromagnetic Josephson junction using an iron alloy for the ferromagnetic layer, allowing control of saturation magnetization and exchange energy through alloy composition, ensuring a suitable thickness for stable operation.

Benefits of technology

The iron alloy-based ferromagnetic layer stabilizes critical current values and reduces exchange energy, enabling consistent and reliable performance of the junction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567830000003
    Figure 0007567830000003
  • Figure 0007567830000004
    Figure 0007567830000004
  • Figure 0007567830000005
    Figure 0007567830000005
Patent Text Reader

Abstract

To provide a ferromagnetic Josephson junction body capable of realizing a high performance superconducting device.SOLUTION: The present invention discloses a ferromagnetic Josephson junction body in which a first superconducting layer, a ferromagnetic layer, and a second superconducting layer are sequentially laminated. The ferromagnetic layer comprises iron alloy. The iron alloy contains, for example, 20 to 90 atomic% of Fe with the total as 100 atomic%. One example of the iron alloy is an Fe-Mo alloy. The ferromagnetic layer comprising the iron alloy has lower saturation magnetism than a ferromagnetic layer comprising pure iron, and has smaller magnetic exchange energy. Further, it is preferable that the first superconducting layer, the ferromagnetic layer, and the second superconducting layer are epitaxially grown and are oriented in the same direction. In such a ferromagnetic Josephson junction body can exhibit a high critical electric current value etc. while having a thickness of the ferromagnetic layer being a proper value ( for instance, 0.5 to 30 nm).SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate in which two superconducting layers are coupled via a (ferro)magnetic layer (referred to as a "(ferro)magnetic Josephson junction") and the like. [Background technology]

[0002] Josephson junction elements are used in superconducting devices such as SFQ (Single Flux Quantum) logic circuits that can process at high speed with low power consumption, and SQUIDs (superconducting quantum interference devices) that can detect extremely small magnetizations (magnetism). A Josephson junction is made up of two superconductors (layers) connected via a thin insulator (layer), and exhibits the phenomenon (Josephson effect) of quantum tunneling of superconducting electron pairs (Cooper pairs) through the insulator.

[0003] Recently, ferromagnetic Josephson junctions, in which conventional insulators are replaced with ferromagnetic materials (layers), have been attracting attention as a promising candidate for quantum bits (basic elements of quantum computing). In ferromagnetic Josephson junctions, the phase of the superconducting current (Josephson current) can be shifted by π (π junction) relative to the Josephson junction (0 junction). For example, the following literature provides information related to such ferromagnetic Josephson junctions: [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-251768 [Patent Document 2] JP 2018-174015 A [Non-patent literature]

[0005] [Non-Patent Document 1] VV Ryazanov et al., Phys. Rev. Lett. 86, 2427, (2001).

Non-licensed Document 2

Non-licensed Document 4

Non-licensed Document 5

Non-licensed Document 6

Non-licensed Document 7

Non-licensed literature 9

Non-licensed literature 10

Non-licensed Document 11

Non-licensed Document 12

[0006] Patent documents 1 and 2 and non-patent documents 1 to 13 are still at the initial stage of confirming the emergence of a π state in a ferromagnetic Josephson junction or the operation of a bit formed by a junction.

[0007] Non-Patent Documents 14 and 15 propose a ferromagnetic Josephson junction in which a Nb layer (superconducting layer) with a bcc structure and a PdNi layer (magnetic layer) with an fcc structure are stacked.

[0008] Non-Patent Document 16 proposes a ferromagnetic Josephson junction in which an NbN layer (superconducting layer) with a bcc structure and a CuNi layer (magnetic layer) with an fcc structure are stacked.

[0009] Non-Patent Document 17 proposes a Josephson junction in which a NbN layer (superconducting layer) having a bcc structure and a hexagonal AlN layer (nonmagnetic insulating layer) are stacked, instead of a ferromagnetic Josephson junction.

[0010] The present invention has been made in view of the above circumstances, and has as its object to provide a new ferromagnetic Josephson junction and the like which are different from conventional ones. [Means for solving the problem]

[0011] As a result of intensive research, the inventors came up with the idea of ​​a ferromagnetic Josephson junction using an iron alloy for the ferromagnetic layer, and embodied this idea. By further developing this result, the inventors have completed the present invention, which will be described below.

[0012] Ferromagnetic Josephson junctions (1) The ferromagnetic Josephson junction of the present invention is a ferromagnetic Josephson junction comprising a first superconducting layer, a ferromagnetic layer and a second superconducting layer laminated in this order, the ferromagnetic layer being made of an iron alloy.

[0013] (2) According to the present invention, it is possible to provide a ferromagnetic Josephson junction (also simply called a "junction" or a "laminate") capable of stably exhibiting desired characteristics. The reason for this is believed to be as follows.

[0014] Important characteristics of ferromagnetic Josephson junctions include the critical current value (Ic: maximum Josephson current value) or critical current density (Jc), and the junction characteristic parameter IcRn product (Rn: junction resistance), and there is a demand for improving and stabilizing these (reducing variation).

[0015] A typical critical current value (Ic) is affected by the thickness of the ferromagnetic layer (simply called "film thickness") and the magnetic exchange energy (see formula (1)). The thinner the ferromagnetic layer, the higher the Ic tends to be, but short defects between the superconducting layers become more likely to occur. For this reason, in order to stably obtain a sufficient Ic, it is necessary to reduce the exchange energy while ensuring an appropriate film thickness for the ferromagnetic layer.

[0016] The exchange energy of a ferromagnetic layer is correlated (positively correlated) with its magnetization (see formula (2)). Fe (pure iron) has a very large saturation magnetization, but the saturation magnetization of a ferromagnetic iron alloy can change depending on its chemical composition. In other words, the saturation magnetization and, in turn, the exchange energy of the ferromagnetic layer can be controlled by the component composition of the iron alloy. Thus, it is believed that the joint of the present invention, in which the ferromagnetic layer is made of an iron alloy, can stably exhibit the desired characteristics (Ic, etc.).

[0017] <Method of manufacturing a ferromagnetic Josephson junction> The present invention can also be understood as a method for manufacturing such a junction. For example, the present invention may be a method for manufacturing a ferromagnetic Josephson junction, comprising a lamination step of laminating a first superconducting layer, a ferromagnetic layer made of an iron alloy, and a second superconducting layer in this order.

[0018] "others" Unless otherwise specified, "x to y" in this specification includes a lower limit value x and an upper limit value y. Any numerical value included in the various numerical values ​​or numerical ranges described in this specification may be used as a new lower limit or upper limit value to create a new range such as "a to b". Furthermore, "x to ynm" in this specification means xnm to ynm. Other unit systems (emu / cm 3 The same applies to (etc.). [Brief description of the drawings]

[0019] [Figure 1A] FIG. 1 is a schematic diagram of a fabricated sample (laminate). [Figure 1B] X-ray diffraction spectra (XRD) of each sample. [Diagram 2] 4 is a scatter diagram showing the relationship between the Fe composition ratio of the ferromagnetic layer and the Nb lattice constant of the superconducting layer. [Diagram 3] FIG. 2 is a scatter diagram showing the relationship between the Fe composition ratio and the saturation magnetization. [Figure 4] This is a TEM image of a cross section of a sample (ferromagnetic layer: pure iron). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The contents described in this specification may apply not only to the bonded body but also to the manufacturing method thereof. One or more components arbitrarily selected from this specification may be added as components of the present invention. The components related to the manufacturing method may also be components related to the product. Which embodiment is best depends on the target, required performance, etc.

[0021] 《Zygote》 (1)Ferromagnetic layer The ferromagnetic layer is made of an iron alloy. The iron alloy exhibits ferromagnetism, and the composition of the components may be adjusted within a range that does not impair the properties of the joined body. For example, the iron alloy contains 20 to 90 at %, or even 35 to 80 at %, of Fe (balance), with the whole being 100 at %.

[0022] The iron alloy is preferably suitable for lattice matching (especially epitaxial growth) between the ferromagnetic layer and the superconducting layer. For example, when the crystal structure of the material (superconducting material) constituting the first superconducting layer and the second superconducting layer is a body-centered cubic lattice (bcc), the ferromagnetic layer is preferably made of an iron alloy whose crystal structure is also a body-centered cubic lattice. Examples of such alloying elements (elements other than Fe contained in the iron alloy) include Mo, Ti, Zr, Nb, Ta, W, and Cr. Note that the iron alloy is not limited to a binary system, and may be a ternary or higher system (two or more alloying elements).

[0023] The thickness of the ferromagnetic layer made of such an iron alloy can be set within a suitable range, for example, 0.5 to 30 nm, 1 to 20 nm, or even 1.5 to 10 nm.

[0024] (2) Superconducting layer The superconducting layer is made of a superconducting material capable of exhibiting superconductivity. Examples of the superconducting material include Nb simple substance, compounds (NbN, NbTi, NbZr, Nb3Sn, Nb3Al, Nb3Ge, Nb3Ga, etc.), and alloys (MgB2, TiN, etc.). In particular, it is preferable to select a superconducting material whose crystal structure is a body-centered cubic lattice.

[0025] The first and second superconducting layers may be different in material and thickness. Of course, both layers may be made of the same material and / or have the same thickness. The thickness of the superconducting layer is, for example, about 3 to 300 nm, 10 to 100 nm, or 25 to 75 nm. The thickness of each layer in this specification is the arithmetic mean value of the maximum thickness and the minimum thickness measured in a region with a stable thickness based on an image (photograph) of the cross section observed with an electron microscope (TEM, etc.).

[0026] (3) Other layers In addition to the ferromagnetic layer and both superconducting layers, the joint may also include a substrate and / or intermediate layers (buffer layer and / or insert layer) as appropriate.

[0027] The substrate should preferably have a single crystal surface on which a layer (film) is formed. The single crystal surface may be the surface of the substrate itself, which is a single crystal, or a layer (film) formed separately on the substrate. Examples of single crystals (or the substrate itself) include MgO, Si, sapphire, SrTiO3, and SiC.

[0028] The buffer layer serves as an underlayer for the first superconducting layer, and is provided, for example, between the single crystal surface of the substrate and the first superconducting layer. The buffer layer is preferably made of a material having the same crystal structure as the first superconducting layer. Furthermore, the material preferably has a lattice constant that reduces the lattice mismatch between the single crystal surface and the first superconducting layer. Such materials include, for example, simple substances, alloys, or compounds having one or more of Mo, W, and V as a base material (50 atomic % or more of the entire material). The thickness of the buffer layer is, for example, about 1 to 50 nm, 5 to 40 nm, or 10 to 30 nm.

[0029] The insert layer is provided between the ferromagnetic layer and the second superconducting layer. The insert layer can reduce the influence of the ferromagnetic layer on the second superconducting layer, improving its orientation (e.g., c-plane orientation) and flatness. The insert layer may be provided between two or more different layers. Like the buffer layer, the insert layer is made of a simple substance, alloy, or compound based on one or more of Mo, W, and V. The thickness of the insert layer is, for example, about 0.1 to 50 nm, 0.3 to 30 nm, 0.8 to 15 nm, or 1.5 to 5 nm.

[0030] (4) Orientation The first superconducting layer, the ferromagnetic layer, and the second superconducting layer may each be made of crystals oriented in the same direction (e.g., c-plane orientation). The orientation is determined, for example, by comparing peak intensities obtained from X-ray diffraction. Specifically, for the superconducting layer, the ratio (I / I0) of the peak intensity (I) of the (110) plane to the peak intensity (I0) of the (002) plane obtained from X-ray diffraction may be 2 or less, 1.5 or less, 1 or less, or even 0.5 or less.

[0031] (5) Flatness The flatter each layer is, the better the properties of the joint are. Flatness is judged, for example, by the change in thickness measured by observing the cross section with an electron microscope. Specifically, it is preferable that the change in thickness of each layer is within 10%, 8%, or even 5% of its maximum thickness (t0). In particular, it is preferable that the thickness of the superconducting layer and the ferromagnetic layer (especially the ferromagnetic layer that is thinner than the other layers) is approximately constant. As an example, if the Nb layer is oriented in (002) (i.e., c-plane) rather than in its preferred orientation plane (110), a superconducting layer with surface roughness (irregularities) of 1 / 2 or less can be realized.

[0032] (6) Pseudo single crystal Each layer is not limited to being single crystal, but may be in a pseudo-single crystal state. A pseudo-single crystal is a state in which the crystal orientations are aligned not only in the stacking direction (e.g., the direction perpendicular to the substrate surface, the c-axis direction) but also in the surface direction perpendicular to the stacking direction (e.g., the direction parallel to the substrate surface, the a- and b-axis directions). The difference between a single crystal and a pseudo-single crystal is the presence or absence of a grain boundary. A pseudo-single crystal layer (film) is, for example, a layer (film) in which crystal grains with a size (maximum length) of about several hundred nm are gathered together. Even a bonded body including a pseudo-single crystal layer can exhibit sufficiently high properties.

[0033] 《Manufacturing method》 (1)Lamination process The lamination process is performed by a known thin film method such as physical vapor deposition (PVD) or chemical vapor deposition (CVD). In particular, by using various vacuum deposition methods (sputtering, vacuum heating deposition, pulsed laser deposition, etc.), which are a type of PVD, it becomes easy to form layers with different component compositions (target materials). -5 ~10 -9 Pa and 10 -6 ~10 -8 The process is performed under a high vacuum of about Pa. The substrate temperature at this time is, for example, near room temperature (60° C. or less, or even 40° C. or less).

[0034] (2) Heat treatment process During the lamination process, a heat treatment process may be performed after at least one specific layer is laminated. Heating can improve the flatness of the laminated layer (film). The heating temperature is, for example, 450 to 750°C, or further 500 to 700°C. The heating time is, for example, 1 to 120 minutes, 10 to 60 minutes, or further 15 to 45 minutes.

[0035] The heating source may be electric heat, radiant heat, laser, etc. The heating atmosphere may be, for example, the high vacuum described above. However, when stacking the next layer after the heat treatment process, it is preferable to cool the stacking surface (substrate) to the above-mentioned temperature range before stacking.

[0036] "Exchange energy and saturation magnetization" The mechanism by which the ferromagnetic layer made of an iron alloy can achieve both the thickness of the ferromagnetic layer necessary for stable production of the joint and the properties desired for the joint (such as the critical current value) at a high level is thought to be as follows.

[0037] (1) The critical current (Ic) in a ferromagnetic Josephson junction is described by the following equation (1) (AA Bannykh et. al., Physical Review B 79, 054501, (2009). ) The variables in the equation are as follows: d F : thickness of the ferromagnetic layer, d F dead: the thickness of the magnetic dead layer of the ferromagnetic layer, h': Dirac constant, E ex : magnetic exchange energy, v F : Fermi velocity

[0038]

number

[0039] As can be seen from formula (1), the thinner the ferromagnetic layer, the larger the critical current value can be. However, when the ferromagnetic layer is made of Fe (pure iron), which has a large exchange energy, the ferromagnetic layer (Fe layer) must be thinned to a thickness of less than 1 nm to obtain the critical current value (several hundred μA) required for practical applications. It is not easy to stably deposit an excessively thin ferromagnetic layer with a uniform thickness.

[0040] As can be seen from formula (1), the critical current value can be increased even if the exchange energy is reduced. Although it is difficult to measure the exchange energy directly, the exchange energy (H) generated by the interaction of the electron orbits of magnetic atoms is generally expressed by the following formula (2). In this formula, Si (Sj) is the operator related to the spin of electron i (electron j), and J is the exchange integral.

[0041]

number

[0042] The exchange integral J is inversely proportional to the distance between electrons, so extending the distance between electrons in a magnetic atom (in other words, relaxing the overlap of electron orbitals) can reduce the exchange energy.

[0043] (2) Saturation magnetization indicates the magnetic moment per unit volume. A decrease in saturation magnetization means that the electron density that contributes to the expression of magnetic properties, including exchange energy, has decreased per unit volume. The increase in the distance between electrons in the magnetic atoms mentioned above also means a decrease in the electron density per unit volume. Thus, a positive correlation can be established between a decrease in saturation magnetization and a decrease in exchange energy.

[0044] (3) The alloying atoms in iron alloys increase the atomic spacing of the ferromagnetic atoms, Fe. For example, in an alloy of bcc Fe (lattice constant: 0.287 nm) and bcc Mo (lattice constant: 0.315 nm), the lattice constant of the iron alloy increases almost monotonically with the amount of Mo.

[0045] Even though it is not possible to directly measure or analyze the lattice constant or exchange energy of a ferromagnetic layer with a thickness of a few nanometers, it is certain that a decrease in the iron concentration in an iron alloy increases the lattice distance between iron atoms, resulting in a ferromagnetic layer with reduced saturation magnetization and exchange energy. Thus, it can be said that an increase in the amount of alloying elements in an iron alloy results in a ferromagnetic layer made of that iron alloy with reduced saturation magnetization and therefore reduced exchange energy.

[0046] The saturation magnetization of iron alloys is, for example, 10 to 800 emu / cm 3 , 30~480emu / cm 3 Furthermore, 60~240 emu / cm 3 The saturation magnetization of Fe (pure iron) is about 1600 emu / cm 3 (1600×10 3 Wb / m 2 ) and the saturation magnetization of Ni is about 480 emu / cm 3 (1600×10 3 Wb / m 2 ) degree.

[0047] 《Application》 The junction of the present invention can be used in various superconducting devices (elements), such as a half flux quantum circuit, a single flux quantum circuit (SFQ circuit), a superconducting phase memory, a quantum bit, a spin valve, a spin filter, a superconducting quantum interference device (SQUID), a quantum sensor, etc. Some specific examples are described below.

[0048] The junction of the present invention can realize a half flux quantum circuit (T. Kamiya, M. Tanaka, K. Sano, and A. Fujimaki, IEICE Transactions on Electronics E101.C, 385 (2018)). Half flux quantum circuits require about 1 / 100 the energy required for state transition compared to SFQ circuits, and the DC bias current required for switching can be significantly reduced. Furthermore, half flux quantum circuits can improve the operating margin and reduce the cell size compared to SFQ circuits.

[0049] The junction of the present invention may also realize a superconducting transfer memory. The superconducting transfer memory may be realized, for example, by making the voltage state of the junction correspond to 0 or 1, by making the half flux quantum correspond to 0 or 1, or by controlling the magnetization of the ferromagnetic layer to make the magnitude of the critical current value correspond to 0 or 1. In addition, a memory made of a half flux quantum circuit has a transition energy between two states that is reduced to about 1 / 100 of that of a memory made of a conventional single flux quantum circuit, enabling low power consumption and high speed operation (B. Baek, WH Rippard, SP Benz, SE Russek, and PD Dresselhaus, Nat. Commun. 5 (2014)).

[0050] The junction of the present invention can also be used to realize quantum bits. One such type is the flux qubit. For example, there is a flux qubit with three 0 junctions, and another with one of the three 0 junctions being a π junction. The latter flux qubit with a 0 junction and a π junction utilizes the superposition of clockwise and counterclockwise currents flowing through a superconducting ring.

[0051] A flux qubit consisting of only 0 junctions requires an external magnetic field: B=Φ / 2S (S: area of ​​SQUID) to obtain the optimum operating point of the superposition. On the other hand, a flux qubit consisting of 0 junctions and π junctions can obtain the optimum operating point without the application of such external magnetization. In this way, flux qubits including π junctions do not require bias lines for applying a magnetic field adjacent to the qubit, making it easy to increase the number of bits. Depending on the control method, it may also be possible to completely eliminate the external magnetic field, reducing low-frequency noise and enabling integration (T. Yamashita, K. Tanikawa, S. Takahashi, and S. Maekawa, Phys. Rev. Lett. 95 (2005).)

[0052] The junction of the present invention can also be used to realize spin valves and spin filters. A spin valve uses an external magnetic field to change the magnetization of the ferromagnetic layer, modulating the critical current (Ic) that flows between the ferromagnetic Josephson junctions. A spin filter intentionally extracts any spin state by adjusting the material and magnetization of the ferromagnetic layer (S. Hikino and S. Yunoki, Phys. Rev. Lett. 110 (2013)). EXAMPLES

[0053] A number of samples (ferromagnetic Josephson junctions) were fabricated with different component compositions of the ferromagnetic layer, and their characteristics were evaluated. The present invention will be described more specifically based on these samples.

[0054] <Sample Preparation> (1) Overview The sample shown in Figure 1A was fabricated by stacking each layer using the thin-film method. Specifically, the process is as follows. First, a substrate made of MgO single crystal was prepared. This substrate was processed (polished) to make the single crystal surface (100) the film formation surface.

[0055] The deposition was performed using an ultra-high vacuum multi-target sputtering device (MPS-2000-C8, manufactured by ULVAC, Inc.) on the deposition surface of the substrate that had been heat-cleaned (600°C) under vacuum and then cooled to 50°C or less. The ultimate vacuum before deposition was 1×10 -7 The deposition pressure was set to 1 Pa. The deposition rate was set to 0.1 nm / sec or less. A pure metal appropriate for each layer was used as the target (raw material). Note that a binary alloy of Fe and Mo prepared in advance may be used as the target for the ferromagnetic layer.

[0056] (2) Film formation (lamination) On the substrate (MgO single crystal surface), a buffer layer (first Mo layer) made of Mo, a first superconducting layer (first Nb layer) made of Nb, a ferromagnetic layer made of Fe and / or Mo, an insert layer (second Mo layer) made of Mo, and a second superconducting layer (second Nb layer) made of Nb were laminated in this order. The Fe composition ratio (target value) of the ferromagnetic layer was set to 100% (pure Fe), 85%, 80%, 70%, 60%, 50% or 40% with respect to the total of 100 atomic % (simply referred to as "%).

[0057] The film thickness (target value) of each layer was 20 nm for the buffer layer, 50 nm for each superconducting layer, 2 nm for the ferromagnetic layer, and 1 nm for the insert layer. The film thickness was calculated from the product of the film formation speed and the film formation time. Although no heat treatment was performed in this example, annealing or the like may be performed during film formation (for example, after deposition of the first Mo layer or the first Nb layer) or after completion of film formation.

[0058] 《Measurement / Analysis》 (1) Orientation The crystal structure of each sample was analyzed from the top side using an X-ray diffractometer (Rigaku Corporation RINT-TTR II / X-rays used: Cu-Kα rays, 2θ: 30 to 90 °C). The obtained X-ray diffraction spectrum (XRD) of each sample is shown in Figure 1B.

[0059] As is clear from Fig. 1B, Nb(002) was observed in all samples regardless of the Fe composition ratio, and Nb(110) was not observed. This confirmed that the multilayer film (laminate) from the first Mo layer to the second Nb layer was entirely c-plane oriented due to epitaxial growth.

[0060] (2) Lattice constant The lattice constants of Nb for each sample determined based on XRD are summarized in Figure 2. The lattice constants were determined using data from a JCPDS (Joint Committee on Powder Diffraction Standards) card and software (KaleidaGraph, manufactured by Hulinks Corporation).

[0061] As is clear from Figure 2, the lattice constant of Nb was almost constant in all samples, regardless of the Fe composition ratio. This shows that the ferromagnetic layer can be formed of an Fe-Mo alloy of the desired composition without adversely affecting the superconducting layer (Nb layer).

[0062] (3) Saturation magnetization The saturation magnetization of each sample was measured using a vibrating sample magnetometer (VSM) manufactured by Tamagawa Seisakusho Co., Ltd. The relationship between the saturation magnetization and the Fe composition ratio is summarized in Figure 3.

[0063] As is clear from FIG. 3, the saturation magnetization of a ferromagnetic layer made of an iron alloy (Fe≦95% or even Fe≦90%) drops sharply to about 1 / 10 to 1 / 5 compared to a ferromagnetic layer made of pure iron (Fe: 100%).

[0064] "observation" The cross section of the sample (ferromagnetic layer: pure iron) was observed with a transmission electron microscope (TEM). The TEM image is shown in Figure 4.

[0065] As is clear from FIG. 4, the thickness variation of each layer was very small, and flatness or smoothness was ensured up to the surface of the second Nb layer.

[0066] From the above, it has been confirmed that it is possible to provide a ferromagnetic Josephson junction in which the saturation magnetization and, in turn, the exchange energy can be reduced while ensuring the thickness of the ferromagnetic layer.

[0067] It was also found that epitaxial growth can produce flat stacks with crystal orientation aligned in a specific direction (e.g., c-plane orientation). Such stacks are expected to be used as ferromagnetic Josephson junctions for integrated circuits that stably exhibit excellent electrical properties.

Claims

1. a first superconducting layer, a ferromagnetic layer, and a second superconducting layer stacked in this order; the first superconducting layer, the ferromagnetic layer and the second superconducting layer are composed of a body-centered cubic lattice; The ferromagnetic layer is a ferromagnetic Josephson junction made of an iron alloy.

2. 2. The ferromagnetic Josephson junction according to claim 1, wherein said iron alloy contains 20 to 90 atomic % of Fe, with the whole being taken as 100 atomic %.

3. 3. The ferromagnetic Josephson junction according to claim 1, wherein the iron alloy contains Mo.

4. 4. A ferromagnetic Josephson junction according to claim 1, wherein the ferromagnetic layer has a thickness of 0.5 to 30 nm.

5. 5. A ferromagnetic Josephson junction according to claim 1, wherein said first superconducting layer, said ferromagnetic layer and said second superconducting layer are each made of crystals oriented in the same direction.

6. 6. The ferromagnetic Josephson junction according to claim 1, wherein the first superconducting layer and the second superconducting layer are made of any one of an elemental Nb, a compound, and an alloy of Nb.

7. The method includes a lamination step of laminating a first superconducting layer, a ferromagnetic layer, and a second superconducting layer in this order, A manufacturing method for obtaining a ferromagnetic Josephson junction according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Josephson junction structure, memory cell, memory cell array and preparation method

    CN108364951A

  • superconducting tunnel junction

    JP1993251768A

  • Phase hysteresis magnetic josephson junction memory cell

    JP2018174015A

  • Milliohm resistors for RQL circuits

    JP2022502841A

  • Superconducting Devices with Ferromagnetic Barrier Junctions

    US20120184445A1