Method for producing fluorescent ceramic and fluorescent ceramic

By applying an electric field during the heating process of zirconia ceramics within a specific temperature range, the method achieves fluorescent zirconia sintered bodies with uniform fluorescence and maintained translucency, addressing the visibility issues of conventional zirconia dental prostheses under UV light.

JP7568421B2Active Publication Date: 2024-10-16KURARAY NORITAKE DENTAL
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020081588
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-12
Filing Date
2020-05-01
Publication Date
2024-10-16
Estimated Expiration
2040-05-01

AI Technical Summary

Technical Problem

Conventional ceramic sintering methods at high temperatures result in zirconia dental prostheses lacking fluorescence, leading to visibility issues under UV light, and adding fluorescent agents reduces translucency.

Method used

A method involving the application of a predetermined electric field during the heating process of a zirconia-based ceramic sample in a specific temperature range to induce fluorescence without adding fluorescent substances, utilizing zirconia, yttria, and hafnia, with controlled electric field parameters to maintain translucency.

Benefits of technology

Produces a fluorescent zirconia sintered body that exhibits uniform fluorescence without compromising translucency, suitable for dental applications, by employing a flash sintering technique at lower temperatures and controlled electric field parameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568421000002
    Figure 0007568421000002
  • Figure 0007568421000003
    Figure 0007568421000003
  • Figure 0007568421000004
    Figure 0007568421000004
Patent Text Reader

Abstract

To provide ceramics having new properties.SOLUTION: A method for producing fluorescent ceramics, which is characterized in that a material that consists mainly of zirconium oxide and is in the form of a pressed powder, temporarily sintered body or sintered body is subjected to predetermined electric field while being heated in a predetermined temperature range to produce ceramics with fluorescent properties. Fluorescent ceramics obtained by the method are also disclosed.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to fluorescent ceramics. [Background technology]

[0002] Generally, ceramic sintered bodies are produced by compressing and molding raw material powders, and then heat-treating the molded body at high temperatures. The heat treatment temperature (called the sintering temperature) is 1200°C to 1500°C, depending on the type of ceramic, and the sintering time is about several hours. In order to improve the density of the sintered body, various methods have been devised, such as methods of applying pressure from the outside (hot pressing method, HIP method, etc.), in addition to the general sintering methods mentioned above.

[0003] Recently, a flash sintering method has been developed that can complete sintering at a lower temperature and in a shorter time than before by applying an electric field to a ceramic powder compact (see Non-Patent Document 1). This sintering method is characterized in that when the ceramic powder compact is heated while an electric field is applied, the sample current increases sharply at a certain temperature (hereinafter, this phenomenon may be referred to as the "flash phenomenon"), and the sintering process ends instantly. It has also been revealed that increasing the electric field strength lowers the temperature at which the sintered compact begins to shrink, and the shrinkage behavior changes more sharply.

[0004] On the other hand, zirconia, a type of ceramic, is used as a dental material such as dental prostheses due to its high translucency and strength. In addition, human natural teeth have fluorescence. Therefore, if the dental prosthesis does not have fluorescence, there is a problem that only the dental prosthesis does not fluoresce under ultraviolet light irradiation environment such as an amusement facility with black light, and the teeth look missing. In order to solve this problem, it is possible to include a fluorescent agent in the dental prosthesis. For example, the zirconia sintered body containing a fluorescent agent is known to be described in Patent Document 1. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Marco Cologna et al, “Flash Sintering of Nanograin Zirconia in <5 s at 850℃”, Rapid Communications of the American Ceramic Society, 2010, Vol. 93, No. 11, p. 3556-3559 [Patent documents]

[0006] [Patent Document 1] Special Publication No. 2016-540772 Summary of the Invention [Problem to be solved by the invention]

[0007] In the above-mentioned situation, the present inventors have conducted extensive research and found that ceramics having new properties can be obtained by producing ceramics using a method different from the conventional method of heat treatment at high temperatures. In addition, in the process of considering the inclusion of a fluorescent agent in a zirconia sintered body, the present inventors found that simply including a fluorescent agent in a zirconia sintered body causes problems such as a decrease in translucency. Therefore, the present invention aims to provide a fluorescent zirconia sintered body that has fluorescence despite not substantially including any fluorescent material other than zirconia, yttria, and hafnia, and a method for producing the fluorescent zirconia sintered body.

[0008] The present invention has been made in view of the above circumstances, and one of the exemplary objects of the present invention is to provide a technique for obtaining ceramics having new properties. [Means for solving the problem]

[0009] As a result of intensive research into solving the above problems, the inventors discovered that in a manufacturing method of a fluorescent ceramic according to one embodiment of the present invention, the above problems can be solved by applying a predetermined electric field to a sample which is a compressed powder body, a pre-sintered body or a sintered body mainly composed of zirconium oxide during the process of heating the sample within a predetermined temperature range. Based on this finding, the inventors carried out further research and completed the present invention.

[0010] The present invention includes the following inventions. [1] A fluorescent ceramic containing zirconium oxide as a main component and not containing more than 0.0001 wt% of compounds of Pr, Sm, Eu, Ga, Gd, Tm, Nd, Dy, Tb, Er, and Bi; [2] The fluorescent ceramic according to claim 1, wherein the fluorescent wavelength of the fluorescence spectrum at an excitation wavelength of 366 nm is in the range of 430 to 500 nm and the maximum intensity within the range is 45 or more; [3] At a thickness of 1.2 mm, ΔL * The fluorescent ceramic according to [1] or [2], wherein (WB) is 5 or more; [4] The fluorescent ceramic according to any one of claims 1 to 3, wherein, on a line extending in a first direction from one end to the other end, a first point A in a section from the one end to 25% of the total length has a fluorescence wavelength in the range of 430 to 500 nm, and when the maximum intensity within the range is defined as 100%, a second point D in a section from the other end to 25% of the total length has a fluorescence wavelength in the range of 430 to 500 nm, and the maximum intensity of the second point D within the range is in the range of 70% to 130% of the maximum intensity of the first point A; [5] The fluorescent ceramic according to any one of [1] to [4], further comprising yttria, the yttria content being 2 to 8 mol%; [6] A fluorescent ceramic whose main component is zirconium oxide and whose fluorescence spectrum peak wavelength is in the range of 430-460 nm at an excitation wavelength of 245 nm; [7] A method for producing a fluorescent ceramic, comprising the step of applying a predetermined electric field to a sample containing zirconium oxide as a main component during heating of the sample within a predetermined temperature range, the sample being a green compact, a provisionally sintered body or a sintered body; [8] The method for producing a fluorescent ceramic according to [7], wherein the predetermined electric field is in the range of 3 V / cm to 100 V / cm; [9] The heating process is a temperature-raising process for raising the temperature of the sample to a predetermined temperature, the predetermined temperature is a temperature at which a flash phenomenon occurs in which a current flowing through the sample increases suddenly when the sample is heated while an electric field is applied to the sample, The method for producing a fluorescent ceramic according to [7] or [8], wherein the predetermined electric field is an electric field in a range in which a phenomenon occurs in which a current flowing through the sample increases rapidly when the sample is heated while an electric field is applied to the sample;

[10] The method for producing a fluorescent ceramic according to any one of [7] to [9], wherein the predetermined electric field is an AC electric field in a frequency range of 1 Hz to 10,000 Hz;

[11] The method for producing a fluorescent ceramic according to

[10] , wherein the AC electric field is in the range of 3 V / cm or more and 50 V / cm or less;

[12] The method for producing a fluorescent ceramic according to

[10] , wherein the AC electric field is in the range of 3 V / cm to 40 V / cm;

[13] The heating step is a step of heating the sample at a predetermined temperature after the sample has been heated to the predetermined temperature; The predetermined temperature is a temperature higher than a flash sintering temperature at which a current flowing through the sample increases rapidly when the sample is heated while an electric field is applied to the sample, The method for producing a fluorescent ceramic according to [7] or [8], wherein the predetermined electric field is an electric field in a range in which a phenomenon occurs in which a current flowing through the sample increases rapidly when the sample is heated while an electric field is applied to the sample;

[14] The method for producing a fluorescent ceramic according to

[13] , wherein the predetermined temperature is at least 200° C. higher than the flash sintering temperature;

[15] The method for producing a fluorescent ceramic according to

[13] , wherein the predetermined temperature is in the range of 1000°C to 1200°C;

[16] The method for producing a fluorescent ceramic according to any one of

[13] to

[15] , wherein the predetermined electric field is 30 V / cm or more;

[17] The method for producing a fluorescent ceramic according to any one of [7] to

[16] , wherein the predetermined electric field is applied for one minute or more;

[18] The method for producing a fluorescent ceramic according to any one of [7] to

[17] , wherein the sample is a green compact, and a raw material powder for the green compact is a solid solution of Y2O3 dispersed in ZrO2;

[19] The method for producing a fluorescent ceramic according to any one of [7] to

[18] , wherein in the step of applying a predetermined electric field to the sample, application of the electric field to the sample is maintained for a predetermined time after a current flowing through the sample reaches a predetermined limiting current value;

[20] The method for producing a fluorescent ceramic according to any one of claims 7 to 19, wherein in the step of applying a predetermined electric field to the sample, a time period during which the application of the electric field to the sample is maintained after a current flowing through the sample reaches a predetermined limiting current value is controlled to thereby control the fluorescence intensity of the fluorescent ceramic;

[21] The method for producing a fluorescent ceramic according to any one of claims 7 to 20, wherein in the step of applying a predetermined electric field to the sample, the intensity of the electric field applied to the sample is controlled to thereby control the fluorescence intensity of the fluorescent ceramic;

[22] The heating step is a step of heating the sample at a predetermined temperature after the sample has been heated to the predetermined temperature; By controlling the level of the predetermined temperature, the fluorescent intensity of the fluorescent ceramic is controlled; 9. The method for producing a fluorescent ceramic according to claim 7, wherein the predetermined temperature is higher than a flash sintering temperature at which a current flowing through the sample increases rapidly when the sample is heated while an electric field is applied to the sample. Effect of the Invention

[0011] According to the present invention, it is possible to realize ceramics having new properties. Also, according to the present invention, it is possible to provide a fluorescent zirconia sintered body that has fluorescence without a decrease in translucency despite being substantially free of fluorescent substances other than zirconia, yttria, and hafnia, and a method for producing the fluorescent zirconia sintered body. Furthermore, according to the present invention, it is possible to provide a fluorescent zirconia sintered body that has uniform fluorescence despite being substantially free of fluorescent substances other than zirconia, yttria, and hafnia, and a method for producing the fluorescent zirconia sintered body. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 shows the relationship between the sample current flowing through a powder compact of zirconium oxide as a starting sample and the applied electric field (V / cm) when the sample was heated while a constant electric field was applied. [Diagram 2] FIG. 2 is a diagram showing photographs of the fluorescent state of samples prepared under the conditions of the applied electric field shown in FIG. 1. [Diagram 3] This figure shows the relationship between the furnace temperature and the sample current when an AC electric field of 100 V / cm and 100 Hz is applied at the point when the sample temperature reaches a predetermined temperature (1000°C, 1100°C, 1200°C). [Figure 4] FIG. 4 is a diagram showing photographs of the fluorescent states of samples prepared under the temperature conditions shown in FIG. 3. [Diagram 5] FIG. 13 is a diagram showing photographs of the fluorescence state of samples prepared at each retention time. [Figure 6] FIG. 13 is a photograph showing the fluorescent state of a sample prepared by applying an AC electric field (left side) and a sample prepared by applying a DC electric field (right side). [Figure 7] FIG. 13 is a diagram showing photographs of the fluorescent state of a sample that was produced as a sintered body at a firing temperature of 1400° C. (firing time of 2 to 3 hours) and then further subjected to various treatments. [Figure 8] FIG. 2 is a diagram showing an example of a fluorescence spectrum of the fluorescent ceramic according to the embodiment. [Figure 9]FIG. 1 is a photograph showing the fluorescent state of a fluorescent ceramic containing zirconium oxide as a main component and not including yttria. [Figure 10] FIG. 2 is a schematic diagram showing evaluation positions of the fluorescence intensity of the fluorescent ceramic according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] An embodiment of the present invention relates to a method for producing a fluorescent ceramic, in which a sample mainly composed of zirconium oxide is heated within a predetermined temperature range, and a predetermined electric field is applied to the sample, and the sample is a green compact, a pre-sintered body, or a sintered body. In the present invention, the "green compact" is also called a "molded body" or a "press molded body." In addition, in the present invention, the "main component" means the component with the largest content. The content of zirconium oxide in the green compact, the pre-sintered body, or the sintered body is preferably 80 mass% or more, more preferably 85 mass% or more, and even more preferably 90 mass% or more, and may be 92 mass% or more, or may be 95 mass% or more.

[0014] According to this embodiment, a fluorescent ceramic having fluorescent properties that are not exhibited by a conventional ceramic sintered body mainly composed of zirconium oxide sintered at high temperatures can be obtained.

[0015] The predetermined electric field is preferably in the range of 3 V / cm to 100 V / cm. By setting it to 3 V / cm or more, the sintering temperature can be lowered, and by setting it to 100 V / cm or less, high fluorescence intensity can be obtained. In a preferred embodiment, the predetermined electric field is preferably in the range of 3 V / cm to 40 V / cm, more preferably in the range of 3.5 V / cm to 35 V / cm, and even more preferably in the range of 4 V / cm to 30 V / cm, from the viewpoint of industrial advantages such as not undergoing a flash phenomenon, not needing to control the limiting source current caused by the flash phenomenon, and not needing a control device.

[0016] In an embodiment, the electric field application step may be performed by applying a predetermined electric field to the sample while heating the sample to a predetermined temperature. The heating rate is not particularly limited, but is preferably 80° C. / h or more, and more preferably 150° C. / h or more from the viewpoint of being able to perform firing in a short time, and is preferably 200° C. / h or more, and may be 250° C. / h or more. The heating rate is also not particularly limited, and may be 20000° C. / h or less, 10000° C. / h or less, or 4000° C. / h or less. In an embodiment (X-1) in which a predetermined electric field is applied to the sample while heating the sample to a predetermined temperature, the predetermined temperature, which is the target temperature for heating, is preferably a flash sintering temperature (temperature at which a flash phenomenon occurs) at which the current flowing through the sample increases rapidly when the sample is heated while an electric field is applied to the sample. In an embodiment (X-1), it is preferable to stop heating at the time when the flash phenomenon occurs, that is, at the temperature at which the flash phenomenon occurs, from the viewpoint of protecting the device. In the embodiment (X-1), the predetermined electric field is preferably an electric field in a range where a phenomenon occurs in which the current flowing through the sample increases abruptly when the sample is heated while an electric field is applied to the sample. In another embodiment (X-2) in which a predetermined electric field is applied to the sample while the sample is heated to a predetermined temperature, the predetermined temperature, which is the target temperature for heating, is preferably a temperature lower than the flash sintering temperature at which the current flowing through the sample increases abruptly when the sample is heated while an electric field is applied to the sample. The predetermined electric field is preferably an electric field in a range where a phenomenon does not occur in which the current flowing through the sample increases abruptly when the sample is heated while an electric field is applied to the sample. In another embodiment, the electric field application step may include applying a predetermined electric field after heating the sample to a predetermined temperature. The predetermined temperature may be a temperature higher than the flash sintering temperature at which the current flowing through the sample increases abruptly when the sample is heated while an electric field is applied to the sample. The predetermined electric field may be an electric field in a range where a phenomenon occurs in which the current flowing through the sample increases abruptly when the sample is heated while an electric field is applied to the sample. This allows sintering at a temperature higher than the flash sintering temperature that is uniquely determined when the sample is heated while an electric field is applied. Moreover, by setting the predetermined temperature higher than the flash sintering temperature, the intensity of the fluorescent light can be increased.

[0017] In any embodiment of the present invention (e.g., an embodiment in which the sample is heated to a predetermined temperature and then an electric field is applied), the predetermined temperature may be 200° C. or more higher than the flash sintering temperature. The predetermined temperature may be in the range of 1000° C. to 1200° C., or in the range of 1100° C. to 1200° C. This allows sintering in a temperature range where the fluorescent ceramic is likely to have a high fluorescence intensity.

[0018] In any embodiment of the present invention (e.g., an embodiment in which an electric field is applied after the sample is heated to a predetermined temperature), the predetermined electric field may be 30 V / cm or more, 35 V / cm or more, or more than 40 V / cm. For example, in another embodiment, the predetermined electric field is preferably in the range of more than 40 V / cm and not more than 100 V / cm. This allows flash sintering at a lower temperature than the firing temperature of general zirconium oxide.

[0019] In some embodiments of the present invention (e.g., embodiment (Y)), the electric field may be applied for 1 minute or longer, which can enhance the fluorescence intensity of the fluorescent ceramic.

[0020] After sintering by applying an electric field, a heating and firing step may be added in a normal atmosphere without applying an electric field. The addition of the heating and firing step in the normal atmosphere does not cause the loss of fluorescence. The heating temperature in the heating and firing step may be 1300 to 1700°C. This firing step increases the density of the resulting fluorescent ceramic, and can improve the light transmittance, bending strength, and fluorescent intensity.

[0021] The raw powder of the green compact may be one in which Y2O3 is dispersed and solid-solved in ZrO2. Y2O3 may be contained in an amount of 2 to 10 mol% or 2 to 8 mol% relative to the raw powder. The content of Y2O3 in the raw powder means the ratio of the number of moles of yttria to the total number of moles of zirconia and yttria contained in the raw powder. In a preferred embodiment, the content of Y2O3 is 2 to 4.5 mol% relative to the raw powder. In another preferred embodiment, it is 5.5 to 8 mol%. The method of dispersing and solid-solving Y2O3 in ZrO2 is not particularly limited, but may include a method in which a precursor of ZrO2 (e.g., zirconium oxychloride (ZrOCl2) and its octahydrate, etc.) and a precursor of Y2O3 (e.g., yttrium chloride (YCl3) and its hexahydrate, etc.) are mixed in the presence of a solvent as necessary, and the resulting mixture or mixed liquid is subjected to a reaction process to produce an oxide. Examples of the reaction process to produce an oxide include a sol-gel method and a coprecipitation method. This improves durability in a variety of applications, such as high-hardness materials, use at high temperatures, conductive ceramics, solid electrolytes, and translucent materials.

[0022] Another embodiment of the present invention is also a method for producing a fluorescent ceramic, which comprises applying a predetermined electric field to a sample, which is a green compact, a pre-sintered compact or a sintered compact mainly composed of zirconium oxide, during the heating process within a predetermined temperature range, and maintaining the sample for a predetermined time after the current flowing through the sample reaches a predetermined limiting current value, thereby producing a fluorescent ceramic.

[0023] According to this embodiment, by maintaining the application of an electric field to the sample for a predetermined period of time after the current flowing through the sample reaches a predetermined limiting current value, a fluorescent ceramic having fluorescent properties that are not exhibited in conventional ceramic sintered bodies mainly composed of zirconium oxide sintered at high temperatures can be obtained.

[0024] Yet another embodiment of the present invention is a method for producing a fluorescent ceramic, which comprises applying a predetermined electric field to a sample, which is a green compact, a pre-sintered compact or a sintered compact mainly composed of zirconium oxide, during the heating process within a predetermined temperature range to produce a ceramic having fluorescent properties, and controlling the fluorescence intensity of the resulting fluorescent ceramic by controlling the time during which the application of the electric field to the sample is maintained after the current flowing through the sample reaches a predetermined limiting current value.

[0025] According to this embodiment, the fluorescence intensity of the resulting fluorescent ceramic can be adjusted by a relatively simple method of controlling the duration of current application.

[0026] Yet another embodiment of the present invention is also a method for producing a fluorescent ceramic, which produces a ceramic having fluorescent properties by applying a predetermined electric field during the process of heating a sample, which is a green compact, a pre-sintered compact or a sintered compact mainly composed of zirconium oxide, within a predetermined temperature range, and by controlling the magnitude of the electric field applied to the sample, the fluorescence intensity of the resulting fluorescent ceramic is controlled.

[0027] According to this embodiment, the fluorescence intensity of the resulting fluorescent ceramic can be adjusted by a relatively simple method of controlling the magnitude of the electric field applied to the sample.

[0028] Yet another embodiment of the present invention is also a method for producing a fluorescent ceramic, which comprises heating a sample, which is a green compact, a pre-sintered compact or a sintered compact mainly composed of zirconium oxide, to a predetermined temperature and then applying a predetermined electric field to produce a ceramic having fluorescent properties, and controlling the level of the predetermined temperature to control the fluorescence intensity of the resulting fluorescent ceramic. The predetermined temperature is a temperature higher than the flash sintering temperature at which the current flowing through the sample increases rapidly when the sample is heated while an electric field is applied to the sample.

[0029] According to this embodiment, the fluorescence intensity of the resulting fluorescent ceramic can be adjusted by controlling the height of the predetermined temperature that is higher than the flash sintering temperature.

[0030] Another embodiment of the present invention is a fluorescent ceramic, which contains zirconium oxide as a main component and has a peak wavelength of a fluorescence spectrum in the range of 430 to 460 nm when excited at a wavelength of 245 nm.

[0031] The fluorescent zirconia sintered body (fluorescent ceramic) of the present invention does not substantially contain any fluorescent material other than zirconia, yttria, and hafnia. Specifically, the content of Pr, Sm, Eu, Ga, Gd, Tm, Nd, Dy, Tb, Er, and Bi compounds is less than 0.0001 wt%. These contents may be 0 wt%. If the fluorescent material other than zirconia, yttria, and hafnia is contained in an amount of 0.0001 wt% or more, the light transmittance of the sintered body decreases.

[0032] The fluorescent zirconia sintered body of the present invention has a fluorescence spectrum of 430 to 500 nm at an excitation wavelength of 366 nm. The lower limit of the maximum peak intensity of the fluorescence spectrum in the range of 430 to 500 nm is 45 or more, preferably 50 or more, more preferably 55 or more, and particularly preferably 60 or more, when measured with a spectrofluorometer F-7100 manufactured by Hitachi High-Tech Science Co., Ltd. If the maximum peak intensity of the fluorescence spectrum in the range of 430 to 500 nm is less than 45, the fluorescence is insufficient for human teeth. Rhodamine B can be used to correct the spectrum between models. The upper limit of the maximum peak intensity of the fluorescence spectrum in the range of 430 to 500 nm is 2000 or less, preferably 1900 or less, more preferably 1800 or less, and particularly preferably 1700 or less, when measured with a spectrofluorometer F-7100 manufactured by Hitachi High-Tech Science Co., Ltd. If the maximum peak intensity of the fluorescence spectrum in the range of 430 to 500 nm is 2000 or less, the fluorescence is not too strong and looks natural as a human tooth.

[0033] According to this embodiment, a ceramic material that has a bluish color in addition to the base color of the fluorescent ceramic can be realized.

[0034] In one embodiment of the present invention, ΔL *Fluorescent ceramics with a WB of 5 or more are also included. * (WB) is the brightness on a white background (L * ) and lightness on a black background (L * ) on a white background. * value (JIS Z 8781-4:2013 Colorimetry-Part 4:CIE 1976 L*a*b* color space) and L on a black background * The white background refers to the white part of the hiding ratio test paper described in JIS K 5600-4-1:1999 Part 4, Section 1, and the black background refers to the black part of the hiding ratio test paper. ΔL at a thickness of 1.2 mm * (WB) can be measured using a spectrophotometer, for example, a spectrophotometer (manufactured by Konica Minolta Japan, Inc., "CM-3610A", geometric conditions c (di: 8°, de: 8°), diffuse illumination: 8° light reception, measurement mode SCI, measurement diameter / illumination diameter = φ8mm / φ11mm) and can be calculated using color management software "SpectraMagic NX ver.2.5" manufactured by Konica Minolta, Inc. In this measurement, the light source can be determined by using F11.

[0035] In another embodiment of the present invention, the presintered body or sintered body mainly composed of zirconium oxide may be one in which Y2O3 is dispersed and dissolved in ZrO2, similar to the compacted powder mainly composed of zirconium oxide. The method for producing the presintered body or sintered body in which Y2O3 is dispersed and dissolved in ZrO2 is not particularly limited, and includes a method of firing the compacted powder in which Y2O3 is dispersed and dissolved in ZrO2 at a temperature range depending on whether the presintered body or sintered body is to be obtained. For example, the presintered body can be obtained by firing the compacted powder in which Y2O3 is dispersed and dissolved in ZrO2 at a temperature range of 800°C to 1200°C. In the case of a sintered body, the compacted powder in which Y2O3 is dispersed and dissolved in ZrO2 may be fired at a temperature range of more than 1200°C to 1700°C. The content of Y2O3 in the presintered body or sintered body may be 2 to 10 mol%, or 2 to 8 mol%. In a preferred embodiment, the content of Y2O3 in the pre-sintered body or sintered body is 2-4.5 mol%. In another preferred embodiment, the content of Y2O3 in the pre-sintered body or sintered body is 5.5-8 mol%. The content of Y2O3 in the pre-sintered body or sintered body means the ratio of the number of moles of yttria to the total number of moles of zirconia and yttria. This can improve durability in various applications such as high hardness materials, use at high temperatures, conductive ceramics, solid electrolytes, translucent materials, etc.

[0036] In another embodiment of the fluorescent ceramic of the present invention, as shown in FIG. 10 , on a straight line extending in a first direction Y from one end P to the other end Q, the fluorescence wavelength of the fluorescence spectrum of an excitation wavelength of 366 nm at a first point A in a section from the one end P to 25% of the total length is in the range of 430 to 500 nm, and the maximum intensity within this range is defined as 100%, the fluorescence wavelength of the fluorescence spectrum of an excitation wavelength of 366 nm at a second point D in a section from the other end Q to 25% of the total length is in the range of 430 to 500 nm, and the maximum intensity of the second point D within this range is preferably in the range of 70% to 130% of the maximum intensity of the first point A, more preferably in the range of 75% to 125% of the maximum intensity of the first point A, even more preferably in the range of 80% to 120%, and particularly preferably in the range of 90% to 110%. By having the maximum intensity of the second point D within the above range, it is possible to suppress the difference in appearance of the teeth depending on the part of the tooth from being noticed by others when visually inspected under an ultraviolet irradiation environment such as a black light. A commercially available product (such as a spectrofluorophotometer F-7100 manufactured by Hitachi High-Tech Science Corporation) can be used to measure the fluorescence intensity. Rhodamine B can be used to correct the spectrum between models. The fluorescence intensity can be measured separately and site-specifically by masking the sample. In addition, for example, when a part with strong fluorescence and a part with weak fluorescence are measured by visual inspection, the difference exceeds 30% (for example, when the maximum intensity of the second point D is less than 70% or more than 130% of the maximum intensity of the first point A), resulting in non-uniform fluorescence emission.

[0037] 10, a point between the first point A and the second point D on a line connecting one end P and the other end Q is defined as the third point B. If the fluorescence wavelength of the fluorescence spectrum at the excitation wavelength of 366 nm at the third point B is in the range of 430 to 500 nm and the maximum intensity within that range at the first point A is defined as 100%, then the maximum intensity at the third point B is preferably in the range of 70% to 130% of the maximum intensity at the first point A, more preferably in the range of 75% to 125%, even more preferably in the range of 80% to 120%, and particularly preferably in the range of 90% to 110%. In addition, in relation to the second point D, when the maximum intensity of the second point D is defined as 100%, the maximum intensity of the third point B is preferably in the range of 70% to 130% of the maximum intensity of the second point D, more preferably in the range of 75% to 125%, even more preferably in the range of 80% to 120%, and particularly preferably in the range of 90% to 110%. By having the maximum intensity of the third point B in the above range, it is possible to suppress the difference in appearance depending on the part of the tooth from being perceived by others when visually inspected under an ultraviolet irradiation environment such as a black light.

[0038] Furthermore, the point between the third point B and the second point D is the fourth point C. When the fluorescence wavelength of the fluorescence spectrum of the fourth point C at an excitation wavelength of 366 nm is in the range of 430 to 500 nm, and the maximum intensity within the range of the first point A is defined as 100%, the maximum intensity of the fourth point C is preferably in the range of 70% to 130% of the maximum intensity of the first point A, more preferably in the range of 75% to 125%, even more preferably in the range of 80% to 120%, and particularly preferably in the range of 90% to 110%. In addition, in terms of the relationship with the second point D, when the maximum intensity of the second point D is defined as 100%, the maximum intensity of the fourth point C is preferably in the range of 70% to 130% of the maximum intensity of the second point D, more preferably in the range of 75% to 125%, even more preferably in the range of 80% to 120%, and particularly preferably in the range of 90% to 110%. In relation to the third point B, when the maximum intensity of the third point B is defined as 100%, the maximum intensity of the fourth point C is preferably in the range of 70% to 130% of the maximum intensity of the third point B, more preferably in the range of 75% to 125%, even more preferably in the range of 80% to 120%, and particularly preferably in the range of 90% to 110%. By having the maximum intensity of the fourth point C in the above range, it is possible to suppress the difference in appearance depending on the part of the tooth when visually observed under an ultraviolet irradiation environment such as a black light.

[0039] Any combination of the above components and any conversion of the present invention into a method, device, system, or the like are also effective as embodiments of the present invention.

[0040] Hereinafter, the embodiment of the present invention will be described in detail with reference to the drawings. In the description of the drawings, the same elements are given the same reference numerals, and duplicated descriptions are omitted as appropriate. In addition, the configurations described below are examples, and do not limit the scope of the present invention in any way.

[0041] (Method of manufacturing fluorescent ceramics) The fluorescent ceramic according to this embodiment is a sample that is a green compact, a pre-sintered body, or a sintered body mainly composed of zirconium oxide, and is given the property of emitting fluorescence under excitation light by passing electricity (applying a pre-determined electric field) during the process of heating the sample within a pre-determined temperature range. Here, the sintered body is a body that has been sintered in advance at a pre-determined sintering temperature. Also, the pre-sintered body (semi-sintered body) is a body that has been oxidized by removing impurities and the like contained in the raw material at a temperature lower than the sintering temperature in order to sinter the raw material.

[0042] The inventors of the present application have conducted extensive research into the conditions under which a specific electric field should be applied during the production of ceramics in order to obtain fluorescent ceramics having fluorescent properties. First, a method for producing samples will be described.

[0043] The raw powder of the green compact is, for example, ZrO2 dispersed and solid-solved with Y2O3 (2-8 mol%), which can improve durability in various applications such as high-hardness materials, use at high temperatures, conductive ceramics, solid electrolytes, and translucent materials.

[0044] For example, in the manufacturing method of fluorescent ceramic according to this embodiment, zirconia (ZrO2) powder (TZ-3Y: manufactured by Tosoh Corporation, hereinafter sometimes referred to as "3YSZ") in which 3 mol% of yttria (Y2O3) is uniformly dispersed and solid-solved is used as the raw ceramic powder. This raw powder is compressed, and a rectangular parallelepiped sample (ceramic powder compact) with a length of 15 mm and a cross-sectional shape of 3.5 mm x 3.5 mm is produced by uniaxial and isostatic pressing. After the sample molding, platinum (Pt) foil is fixed as an electrode to both longitudinal end faces of the sample with Pt paste. The raw ceramic powder is ZrO2 with (2 to 8 mol%, preferably 2 to 4.5 mol%) of Y2O3. をIt is preferable that the zirconia sintered body is dispersed and solid-solved. According to the manufacturing method of the present invention, it is possible to provide a fluorescent zirconia sintered body that has fluorescence even though it does not substantially contain any fluorescent material other than zirconia, yttria, and hafnia. Therefore, it is preferable that the ceramic raw material powder does not contain any fluorescent material such as a compound of Pr, Sm, Eu, Ga, Gd, Tm, Nd, Dy, Tb, Er, or Bi, which causes a decrease in translucency.

[0045] Next, the sample with the electrodes fixed was placed in a differential thermal dilatometer (Thermo plus EVO2 TMA8301: manufactured by Rigaku Corporation) that had been modified to allow connection to DC and AC power sources. A specified electric field was applied to the sample while or after the sample was heated to a specified temperature. After that, the heating of the electric furnace was stopped when the limiting current value was reached, and the sample was held at that temperature for a specified time, after which the voltage application was stopped and the sample was allowed to cool naturally.

[0046] Next, the relationship between the applied electric field and the fluorescence intensity will be described. Figure 1 shows the relationship between the sample current flowing through a compact of zirconium oxide as the starting sample and the applied electric field (V / cm) when the sample is heated while a constant electric field is applied. The electric fields applied are 30, 40, 50, 60, 80, and 100 V / cm, AC 100 Hz, and a limited current value of 1000 mA. The heating rate of the furnace for heating the sample is 300°C / h, and the holding time for holding the application of the electric field to the sample is 5 minutes after the sample current reaches its maximum value. The holding temperature is the temperature at which the sample current reaches the limited current value.

[0047] FIG. 2 shows photographs of the fluorescent state of samples produced under the conditions of the applied electric field shown in FIG. 1. The samples in the photographs shown in FIG. 2 are fluorescent ceramics produced by applying electric fields of 100 V / cm, 80 V / cm, 60 V / cm, 50 V / cm, 40 V / cm, and 30 V / cm from left to right. The fluorescent state was observed by illuminating the samples with a black light and taking a photograph. In addition, the whiter the sample in the photograph, the higher the fluorescent intensity. Therefore, it can be seen that, among the samples shown in FIG. 2, the sample (at the far right of the photograph) with an applied electric field of 30 V / cm has the highest fluorescent intensity.

[0048] In the process of heating the sample in a predetermined temperature range, it is confirmed that the fluorescent characteristics are expressed by applying an electric field to the sample and performing a current treatment, as shown in FIG. 2. In addition, it is confirmed that the fluorescence intensity depends on the applied electric field, and at first glance, the smaller the applied electric field, the higher the fluorescence intensity, and that the fluorescence is uniformly emitted even inside the sample. In other words, the fluorescence intensity of the fluorescent ceramic obtained can be adjusted by a relatively simple method of controlling the magnitude of the electric field applied to the sample. When the fluorescent ceramic of the present invention is used for dental purposes such as dental prostheses, it is preferable that the fluorescent ceramic has high fluorescence intensity and emits fluorescence uniformly, because human natural teeth (e.g., enamel) emit fluorescence uniformly under an ultraviolet ray irradiation environment such as a black light, and therefore the artificial tooth using the dental prosthesis does not look like a missing tooth or a partially missing tooth (hole, tip missing, etc.) even under an ultraviolet ray irradiation environment.

[0049] In this way, the manufacturing method according to the present embodiment can produce a fluorescent ceramic mainly composed of zirconium oxide, which has a fluorescent property not exhibited by a conventional ceramic sintered body fired at a high temperature. It can also be seen that if the applied electric field is in the range of 30 V / cm to 100 V / cm, a fluorescent ceramic having a certain degree of fluorescent intensity can be produced at a temperature lower than the firing temperature of general zirconium oxide.

[0050] However, looking at the dependence of the sample current on the applied electric field shown in Figure 1, it becomes clear that this tendency is merely apparent. In other words, when the temperature is raised while an electric field is applied, the sample current increases slightly. This is due to the negative temperature dependence of the electrical resistance that many oxide ceramics have. However, as the applied electric field increases, the tendency for the sample current to increase gradually becomes more pronounced, and finally it shows a steep increase. The characteristic of a gradual increase is commonly referred to as FAST (Field Assisted Sintering Technique), and the characteristic of a steep increase is commonly referred to as FLASH.

[0051] For each sample shown in Figure 1, samples to which an electric field of 30 V / cm was applied are classified as FAST, and other samples to which an electric field of 40 V / cm or more was applied are classified as FLASH, which rises almost linearly. However, it is not necessary to strictly classify FAST and FLASH. The important point here is that as the applied electric field increases, the temperature at which the sample current begins to increase, or the temperature at which the sample current increases linearly, decreases.

[0052] The fluorescence characteristics shown in Figure 2 show that the smaller the applied electric field, the stronger the fluorescence, but this is not directly related to the magnitude of the applied electric field itself, but rather is thought to be related to the fact that the sample current increases at higher temperatures when the applied electric field is smaller. In other words, it is necessary to consider the magnitude of the applied electric field and the heating temperature separately.

[0053] Therefore, in order to study the fluorescence characteristics by clearly separating the temperature and the electric field strength during current application, current was applied to the sample when the sample reached the target temperature. Figure 3 shows the relationship between the furnace temperature and the sample current when an AC electric field of 100 V / cm and 100 Hz was applied when the sample temperature reached the specified temperature (1000°C, 1100°C, 1200°C).

[0054] Figure 3 is a schematic diagram for explaining the relationship between the temperature of a sample and the sample current. Line L1 in Figure 3 shows the relationship between the temperature and the current flowing through the sample in the conventional flash sintering method, in which a voltage is applied before the temperature is raised. As shown by line L1 in Figure 3, in the conventional flash sintering method, when the temperature is raised while an electric field of a certain strength (100 V / cm, 100 Hz, limited current 1000 mA) is applied to the sample, the current flowing through the sample increases rapidly as it approaches the flash sintering temperature T0 (≒770°C), and sintering is completed.

[0055] In contrast, in the method for producing a fluorescent ceramic according to the present embodiment, as shown by lines L2 to L4 in FIG. 3, the sample is heated to a predetermined temperature T1 (1000°C, 1100°C, 1200°C in FIG. 3) higher than the flash sintering temperature T0 without applying an electric field (or applying a low electric field that does not cause a flash phenomenon) and then a predetermined electric field (100V / cm, 100Hz, limited current 1000mA) in the range in which a flash phenomenon occurs is applied. The time for which the current is applied to the sample is 5 minutes. As a result, in the method for producing a fluorescent ceramic according to the present embodiment, sintering is performed at a temperature T1 that is higher than the flash sintering temperature T0 by ΔT. Hereinafter, such a method is referred to as HAFS (Heat assisted flash sintering).

[0056] In this way, the method for producing a fluorescent ceramic according to this embodiment can sinter at a temperature T1 higher than the conventional flash sintering temperature T0 that is uniquely determined when the temperature is raised while applying an electric field. In addition, by setting the predetermined temperature higher than the flash sintering temperature, the density of the sintered body can be improved. When the raw material powder is 3YSZ, the predetermined temperature T1 is preferably in the range of about 950 to 1300°C, more preferably in the range of 1000°C to 1200°C. In addition, the predetermined temperature T1 is sufficiently lower than the general temperature of 1500°C when sintering 3YSZ, which improves productivity and simplifies the device configuration.

[0057] When the raw material powder is 3YSZ, the predetermined electric field is greater than 30 V / cm, preferably in the range of 30 to 120 V / cm, and more preferably in the range of 30 to 100 V / cm. This allows the flash phenomenon to occur at a temperature lower than the firing temperature of general zirconium oxide, and allows sintering to be completed in a relatively short time. Also, fluorescent properties can be imparted to the ceramic.

[0058] The predetermined temperature T1 is preferably 50° C. or higher, more preferably 100° C. or higher, and even more preferably 200° C. or higher than the flash sintering temperature T0. This allows sintering in a temperature range that is easy to improve the density of the sintered body. Also, sintering in a temperature range that is easy to increase the fluorescence intensity of the fluorescent ceramic.

[0059] Figure 4 shows photographs of the fluorescent states of the samples produced under the temperature conditions shown in Figure 3. From left to right, the samples in the photographs shown in Figure 4 are ceramics produced by normal FLASH, HAFS at 1000°C, HAFS at 1100°C, and HAFS at 1200°C.

[0060] As shown in Figure 4, the ceramics produced by HAFS, where the heating temperature is higher than the flash sintering temperature, have a much higher fluorescence intensity than the ceramics produced by normal FLASH. Also, the higher the heating temperature in HAFS, the higher the fluorescence intensity. Thus, the fluorescence intensity of the resulting fluorescent ceramic can be adjusted by controlling the magnitude of the predetermined temperature higher than the flash sintering temperature T0.

[0061] Next, we will explain the effect on the fluorescence properties of the time that the electric field applied to the sample during ceramic manufacturing is maintained. The electric field was applied under the FLASH conditions, in which the temperature was raised while a constant electric field was applied, as in Figure 1. The electric field applied was an AC field of 100 V / cm and 100 Hz, with a limiting current value of 1000 mA. For each sample, from the point at which the limiting current value was reached, the temperature was maintained for 0 minutes, 5 minutes, and 3 hours.

[0062] FIG. 5 is a diagram showing photographs of the fluorescent state of samples produced at each retention time. The samples in the photographs shown in FIG. 5 are ceramics produced under conditions of retention times of 0 minutes, 5 minutes, and 3 hours, from left to right. As shown in FIG. 5, it can be seen that the longer the retention time, the higher the fluorescence intensity. The retention time for applying a predetermined electric field is preferably 1 minute or more, more preferably 3 minutes or more. In this way, by holding the current flowing through the sample for a predetermined time after it reaches a predetermined limiting current value, it is possible to produce ceramics having fluorescent properties that are not expressed in conventional ceramic sintered bodies of zirconium oxide. In addition, the fluorescence intensity of the fluorescent ceramic obtained can be adjusted by a relatively simple method of controlling the retention time of the current.

[0063] Next, we will explain the influence on the fluorescent properties of the electric field applied to the sample when manufacturing ceramics, whether it is AC or DC. The conditions of the applied AC electric field are HAFS treatment of 100V / cm, 100Hz, limited current value of 1000mA, holding time of 5 minutes, and holding temperature of 1200°C. The conditions of the applied DC electric field are 100V / cm, limited current value of 1000mA, holding time of 5 minutes, and holding temperature of 1200°C. Figure 6 shows photographs of the fluorescent states of a sample (left) produced by applying an AC electric field and a sample (right) produced by applying a DC electric field. As can be seen from Figure 5, the sample to which an AC electric field was applied exhibits higher fluorescent intensity, and the entire sample exhibits fluorescent properties uniformly. In the method for producing a fluorescent ceramic of the present invention, the predetermined electric field may be an AC electric field in the frequency range of 1 Hz to 10,000 Hz, preferably 10 Hz to 8,000 Hz, more preferably 50 Hz to 5,000 Hz, and even more preferably 100 Hz to 3,000 Hz. In a preferred embodiment, the AC electric field is preferably in the range of 3 V / cm to 50 V / cm, more preferably 3 V / cm to 40 V / cm, in the frequency range. In a preferred embodiment, for example, the predetermined electric field is preferably in the range of 3 V / cm to 50 V / cm, more preferably 3 V / cm to 40 V / cm, at 100 Hz.

[0064] Next, the effect on the fluorescent properties when an electric field is applied to a sample that has been sintered in advance will be described. FIG. 7 is a diagram showing photographs of the fluorescent states of samples that have been produced as sintered bodies at a firing temperature of 1400°C (firing time of 2 to 3 hours) and then further treated in various ways. The samples in the photographs shown in FIG. 7 are, from left to right, a normal sintered body sample, a sample in which a normal sintered body has been subjected to a FLASH treatment again (applied electric field of 100V / cm, 100Hz, limited current value of 1000mA, holding time of 5 minutes), a sample in which a normal sintered body has been subjected to a HAFS treatment again (heating temperature of 1200°C, applied electric field of 100V / cm, 100Hz, limited current value of 1000mA, holding time of 5 minutes), and a sample in which a normal sintered body has been subjected to a HAFS treatment again (heating temperature of 1200°C, applied electric field of 100V / cm, 100Hz, limited current value of 1000mA, holding time of 1 hour).

[0065] As shown in Figure 7, no fluorescence is observed in the normal sintered body sample. In addition, the sample in which the normal sintered body was subjected to the FLASH process again shows almost no fluorescence. On the other hand, the sample in which the normal sintered body was subjected to the HAFS process again exhibits fluorescent properties.

[0066] Fig. 8 is a diagram showing an example of the fluorescence spectrum of the fluorescent ceramic according to this embodiment. The fluorescence spectrum in Fig. 8 is that of light excited by ultraviolet light with an excitation wavelength peak of 245 nm. The fluorescent ceramic mainly composed of zirconium oxide according to this embodiment emits a fluorescence spectrum with a peak wavelength in the range of 430 to 460 nm, as shown in Fig. 8. Therefore, the fluorescent ceramic according to this embodiment can realize a ceramic material in which a bluish color is added to the base color (white or gray).

[0067] The above-mentioned samples contain yttria (Y2O3) as a raw material to maintain the sample shape, but yttria is not essential for the fluorescent properties to be exhibited. Figure 9 shows a photograph of the fluorescent state of a fluorescent ceramic that does not contain yttria and is mainly composed of zirconium oxide. The fluorescent ceramic shown in Figure 9 is a brittle sample and is unable to maintain its shape overall, but it exhibits the same fluorescent properties as the fluorescent ceramics mentioned above.

[0068] The present invention has been described above based on an embodiment. This embodiment is merely an example, and it will be understood by those skilled in the art that various modifications are possible in the combination of each component and each treatment process, and that such modifications are also within the scope of the present invention. EXAMPLES

[0069] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples, etc. The methods for measuring each physical property are as follows.

[0070] (Examples 1 to 4) As the raw material powder of the ceramic, a commercially available partially stabilized zirconia powder, TZ-3Y (tetragonal system, yttria content: 3 mol%, average primary particle size: 30 nm) manufactured by Tosoh Corporation was used. This raw material powder was press molded at 3 MPa to obtain a rectangular parallelepiped of 5 × 5 × 15 mm, and a press molded body was obtained. Next, the obtained press molded body was further subjected to CIP treatment at 100 MPa to produce a zirconia molded body. After the sample molding of the zirconia molded body, platinum (Pt) foil was fixed as an electrode to both end faces of the longitudinal direction of the sample with Pt paste. Next, the sample with the fixed electrodes was placed on a differential thermal expansion meter (Thermo plus EVO2 TMA8301: manufactured by Rigaku Corporation) that was modified so that DC and AC power sources could be connected. Then, while the sample was heated to a predetermined temperature, a predetermined electric field described later was applied to the sample. Thereafter, in each example, the heating of the electric furnace was stopped when the limiting current value was reached if the limiting current value was reached, or when the limiting current value was reached at 1300°C if the limiting current value was not reached, and the sample was then held at that temperature for a specified time described below, after which the voltage application was stopped and the sample was allowed to cool naturally. Samples that did not reach the limiting current value were additionally fired at 1500°C under normal pressure for 2 hours.

[0071] Example 1 In Example 1, the test was performed with an applied electric field of 30 V / cm, AC of 1000 Hz, and a limiting current value of 1200 mA. The heating rate of the furnace for heating the sample was 300°C / h, and the application of the electric field to the sample was maintained for 15 minutes after the sample current reached its maximum value. The holding temperature was 1250°C, which was the temperature at which the sample current reached the limiting current value. When the obtained sintered body was observed under 366 nm UV light, it showed pale blue fluorescence.

[0072] Example 2 In Example 2, the sintered body was produced in the same manner as in Example 1, except that the applied electric field was 20 V / cm. The limiting current value was not reached even when the holding temperature reached 1300° C. When the obtained sintered body was observed under 366 nm UV light, it showed pale blue fluorescence.

[0073] Example 3 In Example 3, the sintered body was produced in the same manner as in Example 1, except that the applied electric field was 10 V / cm. The limiting current value was not reached even when the holding temperature reached 1300° C. When the obtained sintered body was observed under 366 nm UV light, it showed pale blue fluorescence.

[0074] Example 4 In Example 4, the sintered body was produced in the same manner as in Example 1, except that the applied electric field was 5 V / cm. The limiting current value was not reached even when the holding temperature reached 1300° C. When the obtained sintered body was observed under 366 nm UV light, it showed pale blue fluorescence.

[0075] Comparative Example 1 A zirconia molded body was produced in the same manner as in Example 1. The obtained zirconia molded body was sintered for 2 hours at 1500° C. under normal pressure. The obtained sintered body was observed under 366 nm UV light and did not show pale fluorescence.

[0076] Comparative Example 2 Bismuth oxide (Bi2O3) was added to TZ-3Y manufactured by Tosoh Corporation so that the content was 0.02 mass%, and mixed thoroughly to obtain zirconia powder. A zirconia molded body and a zirconia sintered body were obtained from the obtained zirconia powder in the same manner as in Example 1. When the obtained sintered body was observed under 366 nm UV light, it showed pale blue fluorescence.

[0077] (Fluorescence intensity measurement) Using the sintered bodies obtained in Examples 1 to 4 and Comparative Examples 1 and 2, rectangular parallelepiped samples of approximately 4 x 4 x 12 mm were obtained. The fluorescence intensity of the samples was measured. The fluorescence intensity was measured by using a spectrofluorometer F-7100 manufactured by Hitachi High-Tech Science Corporation, and the fluorescence spectrum was measured in fluorescence mode with an excitation wavelength of 366 nm (n=3). Rhodamine B was used to correct the spectrum between models. The fluorescence wavelength that showed the highest intensity in the fluorescence wavelength range of 430 to 500 nm in the obtained spectrum was taken as the maximum wavelength, and the intensity of the maximum wavelength was taken as the maximum intensity. The results are shown in Table 1.

[0078] (Translucency measurement) The sintered bodies obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were polished with #600 waterproof abrasive paper to a thickness of 1.2 mm. The polished zirconia sintered bodies were used to measure translucency (n=3). The translucency was measured using a color difference meter CE100 (manufactured by Olympus Corporation) and analysis software Crystal Eye (manufactured by Olympus Corporation) as the L*a*b* color system (JIS Z 8781-4:2013) chromaticity (color space). * The L* value was measured with the background of the sintered body set to white, and the first L * Value (L * (W)) and the first L * The L value was measured for the same sample with a black background. * Value (L * (B)) to the second L * value, the first L * Value to second L * The value after subtracting the value (△L *The value of nD (WB) was used as a numerical value indicating the light transmittance. A contact liquid with a refractive index nD of 1.60 was applied to the measurement surface of the sample. The white background means the white part of the hiding ratio test paper described in JIS K 5600-4-1:1999 Part 4, Section 1, and the black background means the black part of the hiding ratio test paper. The results are shown in Table 1.

[0079] [Table 1]

[0080] The results showed that the maximum intensity and the translucency were both high in Examples 1 to 4. In Comparative Example 1, the translucency was high but no bluish white fluorescence was observed and the maximum intensity was low. In Comparative Example 2, the maximum intensity was 45 or more, but the translucency was low. [Industrial Applicability]

[0081] The method for producing a fluorescent ceramic of the present invention can be used to produce industrial abrasives and grinding materials, ceramic materials for dental use, solid electrolyte membrane materials that utilize electrical conductivity, and ceramic materials for sensors. [Explanation of symbols]

[0082] 10 Fluorescent ceramic A 1st point B 3rd point C 4th point D 2nd point P one end Q Other end L total length Y 1st direction

Claims

1. The composition contains zirconium oxide as a main component and further contains yttria, the content of yttria being 2 mol% or more and less than 8 mol%, It does not contain any fluorescent material other than zirconia, yttria, or hafnia, and does not contain 0.0001 wt % or more of compounds of Pr, Sm, Eu, Ga, Gd, Tm, Nd, Dy, Tb, Er, or Bi; The fluorescence wavelength of the fluorescence spectrum at an excitation wavelength of 366 nm is in the range of 430 to 500 nm, and the maximum intensity within the range is 45 or more; On a straight line extending in a first direction from one end to the other end, a fluorescence spectrum of an excitation wavelength of 366 nm at a first point A in a section from the one end to 25% of the total length is in a range of 430 to 500 nm, and the maximum intensity in the range of 430 to 500 nm is defined as 100%, the fluorescence wavelength of the fluorescence spectrum at an excitation wavelength of 366 nm at the second point D in the section from the other end to 25% of the total length is in the range of 430 to 500 nm, and the maximum intensity of the second point D in the range is in the range of 70% to 130% of the maximum intensity of the first point A, The peak wavelength of the fluorescence spectrum at an excitation wavelength of 245 nm is in the range of 430 to 460 nm; An AC electric field having a frequency range of 1 Hz to 10,000 Hz is applied. Fluorescent ceramic.

2. 2. The fluorescent ceramic according to claim 1, wherein the fluorescent wavelength of the fluorescence spectrum at an excitation wavelength of 366 nm is in the range of 430 to 500 nm, and the maximum intensity within the range is 60 or more.

3. At a thickness of 1.2 mm, ΔL * 3. The fluorescent ceramic according to claim 1, wherein (W−B) is 5 or more.

4. 4. The fluorescent ceramic according to claim 1, wherein the content of yttria is 3 mol % or more and less than 8 mol %.

5. The method includes a step of applying a predetermined electric field to a sample containing zirconium oxide as a main component and further containing yttria in a process of heating the sample within a predetermined temperature range, the sample being a green compact, a provisionally sintered body or a sintered body; The content of the yttria is 2 mol% or more and less than 8 mol%, The predetermined electric field is an AC electric field in a frequency range of 1 Hz to 10,000 Hz, The AC electric field is in the range of 3 V / cm to 40 V / cm, (i) the heating step is a temperature-raising step of raising the temperature of the sample to a predetermined temperature higher than 970° C., the predetermined temperature is a temperature at which a flash phenomenon occurs when the sample is heated while an electric field is applied to the sample, and the predetermined electric field is an electric field in a range at which a flash phenomenon occurs when the sample is heated while an electric field is applied to the sample, or (ii) the heating step is a step of heating the sample to a temperature higher than 970° C., and the predetermined electric field is an electric field in a range in which a flash phenomenon does not occur when the sample is heated while an electric field is applied to the sample; In the step of applying a predetermined electric field to the sample, the magnitude of the electric field applied to the sample is controlled so that the fluorescent wavelength of the fluorescent ceramic in the fluorescence spectrum at an excitation wavelength of 366 nm is in the range of 430 to 500 nm, and the maximum peak intensity within the range is controlled to 45 or more. How fluorescent ceramics are made.

6. The method for producing a fluorescent ceramic according to claim 5, wherein the AC electric field is in the range of 3 V / cm to 30 V / cm.

7. The method includes a step of heating a sample containing zirconium oxide as a main component and further containing yttria to a predetermined temperature, heating the sample at the predetermined temperature, and applying a predetermined electric field to the sample, The content of the yttria is 2 mol% or more and less than 8 mol%, The predetermined temperature is a temperature higher than a flash sintering temperature at which a flash phenomenon occurs when the sample is heated while an electric field is applied to the sample, the predetermined electric field is an electric field in a range in which a flash phenomenon occurs when the sample is heated while an electric field is being applied to the sample, the sample is a green compact, a pre-sintered compact, or a sintered compact, In the step of applying a predetermined electric field to the sample, the magnitude of the electric field applied to the sample is controlled so that the fluorescent wavelength of the fluorescent ceramic in the fluorescence spectrum at an excitation wavelength of 366 nm is in the range of 430 to 500 nm, and the maximum peak intensity within the range is controlled to 45 or more. How fluorescent ceramics are made.

8. The method for producing a fluorescent ceramic according to claim 7 , wherein the predetermined temperature is at least 200° C. higher than the flash sintering temperature.

9. The method for producing a fluorescent ceramic according to claim 7, wherein the predetermined temperature is in the range of 1000°C to 1200°C.

10. The method for producing a fluorescent ceramic according to any one of claims 7 to 9, wherein the predetermined electric field is 30 V / cm or more.

11. The method for producing a fluorescent ceramic according to any one of claims 7 to 10, wherein the predetermined electric field is an AC electric field having a frequency range of 1 Hz to 10,000 Hz.

12. The method for producing a fluorescent ceramic according to any one of claims 5 to 11, wherein the predetermined electric field is applied for one minute or more.

13. The sample is a powder compact, and the raw material powder of the powder compact is ZrO 2 To Y 2 O 3 The method for producing a fluorescent ceramic according to any one of claims 5 to 12, wherein the above is dispersed and solid-solved.

14. 14. The method for producing a fluorescent ceramic according to claim 5, wherein in the step of applying a predetermined electric field to the sample, application of the electric field to the sample is maintained for a predetermined time after a current flowing through the sample reaches a set maximum value of the current.

15. 15. The method for producing a fluorescent ceramic according to claim 5, wherein in the step of applying a predetermined electric field to the sample, a time period during which application of the electric field to the sample is maintained after a current flowing through the sample reaches a set maximum value of the current is controlled, thereby controlling the fluorescent wavelength of a fluorescent spectrum of the fluorescent ceramic at an excitation wavelength of 366 nm to be in the range of 430 to 500 nm, and controlling the maximum peak intensity within said range to be 45 or more.

16. the heating step is a step of heating the sample at a predetermined temperature after the sample has been heated to the predetermined temperature, By controlling the level of the predetermined temperature, the fluorescent wavelength of the fluorescent spectrum of the fluorescent ceramic at an excitation wavelength of 366 nm is controlled to be in the range of 430 to 500 nm, and the maximum peak intensity within the range is controlled to be 45 or more; The method for producing a fluorescent ceramic according to any one of claims 7 to 14, wherein the predetermined temperature is a temperature higher than a flash sintering temperature when the sample is heated while an electric field is applied to the sample.

Citation Information

Patent Citations

  • Method for rapidly sintering fully stabilized zirconia powder under low temperature and normal pressure

    CN105503178A

  • Zirconia composition, zirconia calcinated body, zirconia sintered body and manufacturing zirconia sintered body and dental product

    JP2016117618A

  • Dental mill blank, method of manufacture and use thereof

    JP2016540772A

  • Methods of flash sintering

    US20130085055A1