Golf club shaft and manufacturing method thereof

The golf club shaft design addresses anisotropy by controlling the outermost layer's contribution to bending rigidity and shaft shape, enhancing swing consistency and reducing manufacturing complexity.

JP7570801B2Active Publication Date: 2024-10-22MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2018165584
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-09-05
Publication Date
2024-10-22
Estimated Expiration
2038-09-05

AI Technical Summary

Technical Problem

Existing methods for reducing anisotropy in golf club shafts using special materials and complex manufacturing processes are limited and result in anisotropy issues due to overlapping ends during winding and polishing.

Method used

A golf club shaft design with a controlled outermost fiber-reinforced resin layer contributing 0.5% to 15% of bending rigidity, combined with precise control of the shaft's cross-sectional shape and orientation of reinforcing fibers, minimizes anisotropy without requiring special materials.

Benefits of technology

The shaft exhibits reduced anisotropy, improved swing consistency, and decreased defects, allowing for a smoother and more predictable swing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570801000012
    Figure 0007570801000012
  • Figure 0007570801000013
    Figure 0007570801000013
  • Figure 0007570801000014
    Figure 0007570801000014
Patent Text Reader

Abstract

To provide a shaft with little anisotropy, and a manufacturing method thereof.SOLUTION: The golf club shaft is so configured that a contribution ratio of a fiber-reinforced resin layer as an outermost layer to bending rigidity of the golf club shaft is not less than 0.5% and not more than 15%. The manufacturing method of the golf club shaft includes the following steps of (1) to (3): (1) a step of disposing a prepreg whose contribution ratio to the bending rigidity is 0.5-15%, as the outermost layer; (2) a step of heating and cooling the prepreg; and (3) a step of polishing, while controlling the external shape.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a golf club shaft and a method for manufacturing the same. [Background technology]

[0002] A fiber-reinforced resin golf club shaft (shaft) is obtained by winding a plurality of prepregs, which are obtained by impregnating widened carbon fiber bundles with uncured thermosetting resin such as epoxy resin, around a rod-shaped mandrel to form a laminate, which is then heated and cured, and the surface is smoothed through a polishing process to obtain a blank tube, which is then decorated. The shape of the prepreg sheet is designed taking into consideration the outer diameter of the mandrel so that the start and end of the winding do not overlap as much as possible when the prepreg is wound around the mandrel. In the polishing process, the physical properties of the shaft, such as the natural frequency, required for the golf club shaft are adjusted.

[0003] The prepreg wound around the mandrel is designed so that the ends do not overlap as much as possible when wound, but some overlapping may occur due to manufacturing reasons. The usual polishing method is to polish by applying pressure along the outer shape of the shaft. Therefore, when a laminate having a convex part due to overlapping ends is heated and cured when winding the prepreg, the cross-sectional shape does not change significantly because the polishing is performed along the outer shape. As a result, the rigidity of the convex part increases, resulting in anisotropy.

[0004] Known methods for reducing anisotropy include making the stiffness distribution uniform in the circumferential direction of the shaft and discretizing the winding positions of the laminations.

[0005] Patent Document 1 discloses a shaft in which a vibration-damping layer made of metal fibers is braided to eliminate overlapping around the circumference of the shaft, making the distribution of the metal amount uniform and reducing the anisotropy of the stiffness distribution when metal is used.

[0006] Patent Document 2 discloses a tubular body in which reinforcing fiber bundles impregnated with synthetic resin are oriented at a predetermined interval to form a fiber bundle group, and a fiber bundle reinforced resin layer (polymerized fiber sheet) having the fiber bundle group is formed. The fiber bundle group is oriented at an angle to the axial direction of the shaft and the circumferential direction perpendicular to the axial direction of the shaft, thereby preventing the occurrence of anisotropy with respect to bending of the tubular body. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2009-261473 A [Patent Document 2] JP 2012-179134 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, these methods require the use of special materials, such as using a braided layer of metal fibers to reduce anisotropy, or manufacturing and incorporating a special fiber bundle reinforced resin layer using narrow resin-impregnated reinforced fiber tape, and require design to utilize the materials effectively, making manufacturing complicated and limiting their use to shafts with special specifications.

[0009] An object of the present invention is to provide a shaft with little anisotropy without using special materials, and to provide a method for manufacturing the same. [Means for solving the problem]

[0010] As a result of intensive research, the inventors have found that the above-mentioned problems can be solved by setting the contribution rate of the outermost fiber-reinforced resin layer of the raw tube of the shaft to the bending rigidity within a specific range and by controlling the outer diameter of the raw tube, and have thus completed the present invention. That is, the gist of the present invention is as follows: [1] to [8].

[0011] [1] A golf club shaft including a mother tube having a plurality of fiber-reinforced resin layers, wherein the contribution rate of the outermost fiber-reinforced resin layer of the mother tube to the bending rigidity of the golf club shaft is 0.5% or more and 15% or less. [2] A shaft for a golf club according to [1], wherein the horizontal displacement evaluated by the following evaluation method is less than 20 mm. [Method of evaluating horizontal displacement] The mother tube is held approximately horizontally so that the thin-diameter end side can vibrate from 180 mm from the thick-diameter end of the mother tube. Two supports are installed on each side of the mother tube in the horizontal direction, 314.5 mm from the thin-diameter end. Next, with a weight of 196 g attached to the small diameter end of the mother tube, a load was applied in the direction of gravity so that the small diameter end was displaced 60 mm, and then the load was removed to vibrate the mother tube. The positions of the two supports were adjusted independently, and the distance from the axis of the mother tube to the supports when the vibrating mother tube came into contact with each of the two supports was taken as the horizontal displacement. The distance between the right support and the mother tube axis when looking at the mother tube from the small diameter end was taken as the horizontal displacement (right), and similarly the distance between the left support and the mother tube axis was taken as the horizontal displacement (left). [3] A shaft for a golf club according to [1] or [2], wherein the circularity obtained by the evaluation method described below is 0.5 or less. [Roundness evaluation method] A jig is inserted into the inside of the small diameter end side and the large diameter end side of the mother tube to fix the mother tube approximately horizontally. One of the two lines formed by a plane passing through the axis of the mother tube and the outermost surface of the mother tube is defined as the 0° line. Using the 0° line as a reference, lines at 45°, 90°, and 135° are similarly defined in the counterclockwise circumferential direction of the mother tube as viewed from the small diameter end side. The outer diameter is measured using a laser type CCD length measuring sensor at any m points (m is a natural number of 5 or more) along the entire length of the shaft. At each measurement point, the outer diameter is measured including the lines of 0°, 45°, 90°, and 135°, obtaining data for a total of 4 m points. Based on the measurement results at each measurement point, the ratio of the difference between the maximum and minimum outer diameter values ​​to the average outer diameter is calculated. That is, Circularity = 100 × (D x,max -Dx,min ) / D x,ave ...Equation (1) (In formula (1), x:Position [mm] D x,max : Maximum outer diameter of shaft at position x [mm] D x,min :Minimum outer diameter of shaft at position x [mm] D x,ave :Average shaft outer diameter at position x [mm] is) and calculate it. [4] A shaft for a golf club according to any one of [1] to [3], wherein the reinforcing fibers contained in the outermost fiber-reinforced resin layer have a tensile modulus of elasticity of 5 GPa or more but less than 200 GPa, and the absolute value of the orientation direction of the reinforcing fibers in the outermost layer is 5° or less with respect to the axial direction of the mother tube. [5] The tensile modulus of the reinforcing fibers contained in the outermost fiber-reinforced resin layer is 200 GPa or more and 500 GPa or less, and the absolute value of the orientation direction of the reinforcing fibers in the outermost layer is 20° or more and 95° or less with respect to the axial direction of the mother tube. The shaft for a golf club according to any one of [1] to [3]. [6] A shaft for a golf club described in any of [1] to [3], wherein the tensile modulus of the reinforcing fibers contained in the outermost fiber-reinforced resin layer is 50 GPa or more and less than 100 GPa, the outermost layer is a fiber-reinforced resin layer in which a fabric of reinforcing fibers is impregnated with resin, and the warp threads of the fabric have a fiber orientation angle of 0° to the axial direction of the mother tube of -5° to 5° relative to the axial direction of the mother tube. [7] A golf club comprising the golf club shaft according to any one of [1] to [6]. [8] A method for manufacturing a golf club shaft, comprising the following steps (1) to (3): (1) A process of arranging a prepreg having a contribution rate to bending rigidity of 0.5 to 15% as the outermost layer of a blank tube. (2) Heating and then cooling the prepreg (3) Polishing process to control the outer shape Effect of the Invention

[0012] In the golf club shaft of the present invention, the contribution rate of the outermost layer to the bending rigidity is small, so that anisotropy is unlikely to occur. Also, in the golf club shaft of the present invention, the shape of the cross section perpendicular to the shaft axial direction is controlled to be a perfect circle, so that anisotropy caused by the shape of the cross section is small. Furthermore, according to the manufacturing method of the golf club shaft of the present invention, the rate of defective products caused by anisotropy due to conventional polishing methods can be reduced. Additionally, the shaft of the present invention can be manufactured without using special materials.

[0013] In this specification, anisotropy refers to non-uniformity in the bending stiffness of the shaft. The bending stiffness will be described in detail later. Non-uniformity refers to the presence of points with unequal bending stiffness values ​​at any circumferential position on the outer circumference of a cross section perpendicular to the axial direction of the shaft. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is an explanatory diagram showing a cut shape of a prepreg and a winding sequence showing one embodiment of a golf club shaft of the present invention. [Diagram 2] 10 is an explanatory diagram showing a cut shape of a prepreg and a winding order showing another embodiment of a golf club shaft of the present invention. FIG. [Diagram 3] FIG. 11 is an explanatory diagram showing a cut shape of a prepreg and a winding order in yet another embodiment of a golf club shaft of the present invention. [Figure 4] FIG. 2 is an explanatory view showing a cut shape of a prepreg and a winding sequence, illustrating an example of the configuration of Comparative Example 1. [Diagram 5] FIG. 2 is a schematic diagram of a mandrel used in the examples. [Figure 6] FIG. 4 is a schematic diagram for explaining a method for measuring a natural frequency in one embodiment of the present invention. [Figure 7] FIG. 4 is a schematic diagram for explaining a balance point in one embodiment of the present invention. [Figure 8]FIG. 4 is a schematic diagram for explaining a kick point in one embodiment of the present invention. [Figure 9] FIG. 2 is a schematic diagram for explaining a method for evaluating bending rigidity in one embodiment of the present invention. [Figure 10] FIG. 2 is a schematic diagram (side view) for explaining a method for evaluating anisotropy in one embodiment of the present invention. [Figure 11] FIG. 2 is a schematic diagram (as viewed from the chip end side) for explaining a method for evaluating anisotropy in one embodiment of the present invention. [Figure 12] FIG. 2 is a schematic diagram for explaining lines of 0°, 45°, 90°, and 135° in one embodiment of the present invention. [Figure 13] 1A to 1C are schematic diagrams for explaining a method for evaluating roundness in one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, specific examples of embodiments of the present invention will be described. In the following description, a golf club shaft will be referred to as a shaft, a larger diameter end of the shaft as a butt end, and a smaller diameter end as a tip end. In the present embodiment, the term "golf club shaft" refers to both the shaft (golf club part) before being assembled into a golf club, and the shaft part of the golf club when each part of the golf club is assembled into a golf club. Note that the shaft part of the golf club is more effective in demonstrating the effects of the present invention. The present invention is not limited to this embodiment.

[0016] (Golf club shafts) The golf club shaft of the present invention includes a blank tube having a plurality of fiber-reinforced resin layers, and, if necessary, a design-imparting layer for decoration.

[0017] (Plain tube) The physical properties of the blank tube substantially determine the physical properties of the golf club shaft. The blank tube has a plurality of fiber reinforced resin layers, and the number of fiber reinforced resin layers is preferably two or more since the functions of the golf club shaft are shared among the layers as described below. In addition to the fiber reinforced resin layer, the base tube may include a resin layer, a weight adjustment layer which is a resin layer containing metal powder such as tungsten, a resin layer containing a filler other than metal or reinforcing fiber, resin powder, etc.

[0018] (Fiber reinforced resin layer) The fiber reinforced resin layer is made of a fiber reinforced resin containing reinforcing fibers and a resin composition. The reinforcing fibers and the resin composition will be described below.

[0019] (Reinforced Fiber) (Type of reinforcing fiber) The fibers constituting the fiber-reinforced resin of the present invention may be inorganic fibers such as metal fibers, boron fibers, carbon fibers, glass fibers, and ceramic fibers, aramid fibers, and other high-strength synthetic fibers. Inorganic fibers are preferably used because they are lightweight and strong. Among these, carbon fibers are most preferable because they have excellent specific strength and specific rigidity. These fibers may be used alone or in combination of two or more types.

[0020] (reinforcement fiber length) Furthermore, fibers of any length may be used, such as long fibers, short fibers, and mixtures thereof, and two or more types of fibers may be used in combination. From the viewpoint of strength, it is preferable to use long fibers.

[0021] (Mold of reinforcing fibers) These fibers may be used as unidirectional materials (fibers aligned in one direction) or as cloth materials made by weaving reinforcing fibers into fabric. Unidirectional materials can fully utilize physical properties such as strength and elastic modulus in the fiber axis direction, and also have excellent drapeability in the direction perpendicular to the reinforcing fibers, so that when a blank tube is manufactured by the sheet wrap method, it is easy to wrap around a mandrel and has good handleability. Cloth materials are mainly used to impart design to the outermost surface of a blank tube. The weaving method of the cloth material may be any weaving structure such as unidirectional fabrics such as cord weave, bidirectional fabrics such as plain weave, satin weave, and twill weave, triaxial fabrics, and non-crimp fabrics, but bidirectional fabrics and triaxial fabrics are preferred from the viewpoint of design. Triaxial fabrics are preferred from the viewpoint of durability.

[0022] (Reinforcing fiber content) The fiber volume content of the fiber reinforced resin layer is preferably 60% or more, more preferably 65% ​​or more, because the rigidity of the blank tube can be increased, and is preferably 75% or less, more preferably 70% or less, because a certain amount of resin is necessary to sufficiently bond the matrix resin and the reinforcing fibers. The fiber weight of the fiber reinforced resin layer is not particularly limited, but can be appropriately selected based on the thickness and winding diameter required for each layer.

[0023] (Resin composition) The resin composition constituting the fiber reinforced resin of the present invention contains a matrix resin and, if necessary, a curing agent, an antifoaming agent, a defoaming agent, a colorant, and other components. Thermoplastic resins and thermosetting resins can be used as the matrix resin contained in the resin composition, but thermosetting resins are preferably used because they have high physical properties after curing.

[0024] Thermoplastic resins become liquid with high viscosity when heated, and can be freely deformed by external forces. When cooled and the external forces are removed, the resins retain their shape in a solid state. This process can be repeated. There are no particular limitations on the thermoplastic resins, and they can be appropriately selected within a range that does not significantly reduce the mechanical properties of the molded product. Examples of the thermoplastic resins that can be used include polyamide resins, polyacrylate resins, polystyrene resins, polyethylene resins, and mixed resins thereof.

[0025] Thermosetting resins are reactive polymers that undergo a curing reaction by intermolecular crosslinking under the action of heat or a catalyst, and have an insoluble and infusible three-dimensional network structure. There is no particular restriction on the thermosetting resin, and it can be appropriately selected within a range that does not significantly reduce the mechanical properties of the molded product. As the thermosetting resin, for example, epoxy resins, unsaturated polyester resins, phenol resins, urea resins, melamine resins, diallyl phthalate resins, urethane resins, polyimide resins, and mixed resins thereof can be used. Among them, epoxy resins are most preferably used because they have a low cure shrinkage rate and high strength, rigidity, and toughness values.

[0026] Examples of epoxy resins that can be used include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, glycidylamine type epoxy resins, isocyanate modified epoxy resins, and alicyclic epoxy resins. These epoxy resins can be used in liquid or solid form. Furthermore, a single type of epoxy resin or a blend of two or more types of epoxy resins can be used. In addition, epoxy resins are often used with a curing agent added.

[0027] The curing agent for the thermosetting resin is not particularly limited as long as it can promote the curing reaction of the thermosetting resin, but an amine-based curing agent is preferred because it has high physical properties after curing.

[0028] (Orientation angle of reinforcing fibers in fiber-reinforced resin layer) Examples of fiber-reinforced resin layers constituting the mother pipe of this embodiment include straight layers in which the reinforcing fibers of unidirectional materials are oriented at an angle of -5° to +5° with respect to the longitudinal direction of the mother pipe, hoop layers in which the reinforcing fibers of unidirectional materials are oriented at an angle of 85° to 95° with respect to the longitudinal direction of the mother pipe, and angle layers in which the reinforcing fibers of unidirectional materials are oriented at an angle of +20° to +70° or -20° to -70° with respect to the longitudinal direction of the mother pipe. Note that two angle layers, one with a positive orientation angle of the reinforcing fibers with respect to the axial direction of the mother pipe and the other with a negative orientation angle of the reinforcing fibers, are used as a set as bias layers.

[0029] The resin composition and reinforcing fibers constituting the straight layer, the hoop layer, and the bias layer are as described above for the fiber-reinforced resin.

[0030] (Straight layer) The straight layer is a fiber-reinforced resin layer and contains reinforcing fibers oriented approximately parallel to the longitudinal axis of the mother tube. The reinforcing fibers are oriented approximately parallel to the longitudinal axis of the mother tube, which can increase bending rigidity and bending strength. The approximately parallel range is between -5° and +5° with respect to the longitudinal axis of the mother tube.

[0031] The tensile modulus of the reinforcing fiber forming the straight layer is preferably 50 GPa or more and 400 GPa or less. If the tensile modulus of the reinforcing fiber is 50 GPa or more, the bending rigidity is sufficient and the swing rhythm is improved. On the other hand, if the tensile modulus of the reinforcing fiber is 400 GPa or less, the bending rigidity and bending strength are in an appropriate range.

[0032] The thickness of one straight layer is preferably 0.050 mm or more and 0.500 mm or less, and more preferably 0.075 mm or more and 0.150 mm or less. If the thickness of the straight layer is above the lower limit, the number of layers to be laminated is not too large, and productivity is high. In addition, since the handleability is improved, defects such as wrinkles are less likely to occur, and moldability is good. On the other hand, if the thickness of the straight layer is below the upper limit, the outer diameter and bending rigidity can be made uniform, and quality is good.

[0033] (Hoop layer) The hoop layer mainly has the effect of increasing the crushing rigidity and crushing strength. If the orientation angle of the reinforcing fibers of the unidirectional material used in the hoop layer is +85 to +95° or -85 to -95° with respect to the longitudinal axis direction of the bare pipe, that is, the absolute value of the orientation angle is 85° or more and 95° or less, both the crushing rigidity and the crushing strength of the bare pipe are sufficient. The tensile modulus of the reinforcing fibers forming the hoop layer is preferably 240 GPa or more and 400 GPa or less. If the tensile modulus of the reinforcing fibers is 240 GPa or more, the crushing rigidity is sufficiently ensured, and the swing rhythm is less likely to be disturbed due to crushing deformation. On the other hand, if the tensile modulus of the reinforcing fibers is 400 GPa or less, the crushing rigidity and the crushing strength can be sufficiently ensured.

[0034] The thickness of one hoop layer is preferably 0.020 mm or more and 0.100 mm or less. If the thickness of the hoop layer is 0.020 mm or more, sufficient crushing rigidity is obtained. On the other hand, if the thickness of the hoop layer is 0.100 mm or less, the handling property is improved, the occurrence of wrinkles is suppressed, and the moldability is improved.

[0035] (Bias layer) The bias layer mainly has the effect of increasing the torsional rigidity and torsional strength. The bias layer is a fiber-reinforced resin layer, and includes an angle layer (+α layer) containing reinforcing fibers oriented at a positive orientation angle of +α° with respect to the longitudinal axis direction of the bare tube, and an angle layer (-α layer) containing reinforcing fibers oriented at a negative orientation angle of -α° with respect to the longitudinal axis direction of the bare tube. Here, α° is 20° to 70°, preferably 30° to 60°, and more preferably 35° to 55°. Usually, the absolute values ​​of the positive orientation angle and the negative orientation angle are designed to be the same, although there is an unavoidable error in manufacturing. By setting α° within the above range, the torsional rigidity, bending rigidity, and crushing rigidity of the blank tube become sufficient.

[0036] It is desirable to laminate the +α layer and -α layer that make up the bias layer with a shift of substantially half a circumference. If the +α layer and -α layer are laminated with a shift, the unevenness of the wound end is not large, so that anisotropy can be reduced and problems such as poor appearance and reduced strength are less likely to occur.

[0037] The tensile modulus of the reinforcing fiber forming the bias layer is preferably 240 GPa or more and 550 GPa or less. If the tensile modulus of the reinforcing fiber is 240 GPa or more, the torsional rigidity is sufficient, and the return of the face surface of the head at the time of impact with the ball is not delayed, so that the directionality is good. On the other hand, if the tensile modulus of the reinforcing fiber is 550 GPa or less, the torsional strength can be sufficiently secured.

[0038] The thickness of one bias layer is preferably 0.020 mm or more and 0.150 mm or less, more preferably 0.050 mm or more and 0.125 mm or less. If the thickness of one bias layer is equal to or more than the lower limit, the number of layers is not too large, so that the occurrence of wrinkles and the like is suppressed and the moldability is good. On the other hand, if the thickness of one bias layer is equal to or less than the upper limit, the outer diameter and bending rigidity can be made uniform.

[0039] (outermost layer) The outermost layer of the fiber reinforced resin layers constituting the mother pipe of this embodiment is the last fiber reinforced resin layer to be wound around the mandrel and is located on the outermost surface of the mother pipe. The number of times the fiber reinforced resin layer is wound around the mandrel in the circumferential direction may be one turn or two or more turns. When the outermost layer is an angle layer, a bias layer consisting of two layers, including an angle layer located one layer inward from the outermost layer, is defined as the outermost layer.

[0040] The length of the outermost layer in the axial direction of the raw tube is preferably 50% or more of the total length of the raw tube in order to protect the area near the kick point, which is greatly affected by the deflection during a swing. It is more preferably 60% or more, and even more preferably 70% or more. The length of the outermost layer in the axial direction of the raw tube is preferably 100% or less of the total length of the raw tube. It is more preferably 95% or more, and even more preferably 90% or more, in order to maintain the function of the outermost layer while reducing the amount of prepreg used.

[0041] The outermost layer is preferably positioned close to the tip end in order to protect the area that is most susceptible to the narrowing of the outer diameter due to polishing in the polishing process of the mother tube and to facilitate positioning.

[0042] The outermost layer may be used as a single layer, or may be divided into two or more layers in the axial direction of the mother tube. The use of one piece is preferred because positioning is easy. When two or more pieces are divided in the axial direction of the blank tube, it is preferred to arrange the ends of each piece without overlapping each other, in order to avoid overload during polishing due to convex parts generated by overlapping parts and defects caused by unevenness of the outer shape due to insufficient polishing. When the base tube is divided into two or more pieces in the axial direction, the pieces are preferably arranged so as to cover the tip end, which is significantly affected by the reduction in rigidity caused by the thinning of the tube wall due to polishing, and the kick point position, which is significantly affected by the deflection of the shaft during a swing.

[0043] (Contribution rate to bending stiffness of the outermost layer) The bending stiffness (EI) is the ratio of the elastic modulus E (unit: Pa) and the moment of inertia I (unit: m 4 When the cross section is a hollow concentric circle, the second moment of area is given by the following formula (2): I=π(D 4 -d 4 ) / 64...Equation (2) D: Outer diameter (m) d: Inner diameter (m) When considering the bending stiffness of a shaft, the elastic modulus of a material does not refer to the elastic modulus of the material itself, but to the elastic modulus exhibited in the longitudinal direction of the shaft. In particular, when the fibers are not oriented in the longitudinal direction of the shaft, the calculation is performed taking into account the orientation angle of the fibers.

[0044] The contribution rate of the outermost layer to the flexural rigidity indicates the ratio of the flexural rigidity of the outermost layer to the flexural rigidity of the shaft at any position in the longitudinal direction of the shaft, and is calculated by the following method. [Method for measuring the contribution rate of the outermost layer to bending rigidity] One blank tube for the shaft of the present invention and one blank tube for the shaft of the present invention that does not include the outermost layer are prepared, and the displacements of these shafts in a cantilever bending test are measured. When the displacement in the cantilever bending test of the blank tube for the shaft of the present invention is a (mm) and the displacement of the blank tube for the shaft of the present invention that does not include the outermost layer is b (mm), the contribution rate C (%) of the bending rigidity is calculated according to the following formula (3). C=100×(1-a / b)…Equation (3) <Cantilever bending test method> As shown in Figure 9, the shaft is supported from below at a position 920 mm from the small diameter end, and supported from above at a position 150 mm further in the direction of the large diameter (1070 mm from the small diameter end), and a load of 3.0 kgf is applied at a position 10 mm from the small diameter end. The vertical displacement of the small diameter end at this time is the "displacement in the cantilever bending test" in this invention, and is expressed in mm. However, if the total length of the shaft is less than 1,070 mm, the shaft shall be supported from below at a position 760 mm from the thin end, and then supported from above at a position 150 mm further in the direction of the thicker diameter (910 mm from the thin end).

[0045] With reference to formula (2) above, it can be seen that, since the outer diameter of the outermost layer is the largest when comparing the laminated layers, the stiffness of the outermost layer has the greatest effect on the bending stiffness of the shaft among the layers constituting the shaft. In other words, if a material with a high elastic modulus in the longitudinal direction of the shaft is arranged in the outermost layer, significant anisotropy in bending stiffness will occur if winding irregularities occur. Therefore, the contribution rate of the outermost fiber-reinforced resin layer to the bending rigidity is preferably 0.5% to 15%, more preferably 0.5% to 10%, even more preferably 0.5% to 5%, and particularly preferably 0.5% to 1.5%. By setting the contribution rate within the above range, the influence of anisotropy due to the material can be minimized. Furthermore, even if the outermost fiber-reinforced resin layer is a sacrificial layer that is partially or entirely scraped off in the polishing process of the mother tube, or a layer that is scraped off only on the surface and remains over the entire length and circumference, the outermost layer has a small contribution rate to the bending rigidity, so that the influence on the expression of anisotropy is small, and the anisotropy of the produced mother tube is small.

[0046] (Shape, orientation angle and type of reinforcing fiber in the outermost layer) When the outermost fiber-reinforced resin layer is a straight layer, the tensile modulus of the reinforcing fibers is preferably 5 GPa or more and less than 200 GPa, more preferably 10 GPa or more and less than 150 GPa, and even more preferably 15 GPa or more and less than 100 GPa. By keeping it within the above range, the anisotropy of the shaft can be reduced.

[0047] When the outermost fiber-reinforced resin layer is a straight layer, it is preferable that the absolute value of the orientation direction of the reinforcing fibers is 5° or less with respect to the axial direction of the shaft.

[0048] When the outermost fiber reinforced resin layer is a bias layer or a hoop layer, the reinforcing fibers contained in the outermost fiber reinforced resin layer preferably have a tensile modulus of elasticity of 200 GPa or more and 500 GPa or less.

[0049] When the outermost fiber-reinforced resin layer is a bias layer, it is preferable that the absolute value of the orientation direction of the reinforcing fibers in the outermost layer is 20° or more and 70° or less with respect to the axial direction of the shaft. When the outermost fiber-reinforced resin layer is a hoop layer, it is preferable that the absolute value of the orientation direction of the reinforcing fibers in the outermost layer is 85° or more and 95° or less with respect to the axial direction of the shaft.

[0050] When a cloth prepreg in which a woven fabric (cloth material) made of reinforcing fibers is impregnated with a resin composition is used for the outermost layer, the tensile modulus of the reinforcing fibers contained in the fiber-reinforced resin layer of the outermost layer is preferably 50 GPa or more and less than 100 GPa, more preferably 60 GPa or more and 90 GPa, and even more preferably 70 GPa or more and 90 GPa or less. By keeping it within the above range, anisotropy can be reduced regardless of the orientation angle of the reinforcing fibers with respect to the axial direction of the shaft.

[0051] As the cloth material used for the cloth prepreg, any of the weave structures described above can be used.

[0052] By setting the orientation angle of the warp yarns of the cloth material to be between -5° and 5° with respect to the axial direction of the shaft, it becomes easier to wind the cut cloth prepreg around a mandrel when manufacturing the shaft by the sheet wrap method. The warp yarns refer to reinforcing fiber bundles that are approximately parallel to the weaving direction of the cloth material.

[0053] When a cross prepreg is used for the outermost layer, it is preferable to use a cross prepreg in which the reinforcing fiber is glass fiber from the viewpoint of cost. The thickness of the cross prepreg is preferably 0.050 mm or more and 0.500 mm or less, and more preferably 0.080 mm or more and 0.200 mm or less.

[0054] (Horizontal Displacement) The horizontal displacement of the blank tube of the present invention is preferably less than 20 mm, more preferably less than 10 mm. By keeping it within this range, the anisotropy is small, so the bending of the shaft during the swing becomes smooth, and the player can swing as imagined. In other words, the bending of the shaft during the swing becomes closer to the theoretical value, and an ideal swing can be performed.

[0055] The horizontal displacement of the shaft of the present invention is measured by the following evaluation method. The "horizontal direction" in the horizontal displacement refers to a direction perpendicular to the direction of gravity and perpendicular to the axial direction of the blank tube. [Method of evaluating horizontal displacement] The mother tube is held approximately horizontally so that the thin-diameter end side can vibrate from 180 mm from the thick-diameter end of the mother tube. Two supports are installed on each side of the mother tube in the horizontal direction, 314.5 mm from the thin-diameter end. Next, with a weight of 196 g attached to the small diameter end of the mother tube, a load was applied in the direction of gravity so that the small diameter end was displaced 60 mm, and then the load was removed to vibrate the mother tube. The positions of the two supports were adjusted independently, and the distance from the axis of the mother tube to the supports when the vibrating mother tube came into contact with each of the two supports was taken as the horizontal displacement. The distance between the right support and the mother tube axis when looking at the mother tube from the small diameter end was taken as the horizontal displacement (right), and similarly the distance between the left support and the mother tube axis was taken as the horizontal displacement (left).

[0056] (anisotropy) The anisotropy evaluation value is preferably 8 mm or less, more preferably 7 mm or less, and even more preferably 5 mm or less. The smaller the anisotropy evaluation value, the higher the uniformity of the physical properties in the circumferential direction of the shaft. Therefore, the way the shaft bends or twists does not change depending on the circumferential setting angle of the shaft when assembling the club, making it easier to swing as imagined. The horizontal displacement of the shaft of the present invention is measured by the following evaluation method.

[0057] [Anisotropy evaluation method] One of the two lines formed by an arbitrary plane including the axis of the mother tube and the outermost surface of the mother tube is defined as the 0° line. Using the 0° line as a reference, lines of 45°, 90°, and 135° are defined counterclockwise around the mother tube as viewed from the small diameter end side. The horizontal displacement is measured by holding the mother tube so that the 0°, 45°, 90°, and 135° lines are on top, and the horizontal displacement is measured on both the left and right sides as viewed from the small diameter end side, obtaining a total of eight data points. The difference between the maximum and minimum values ​​of the eight data points is the evaluation value of anisotropy.

[0058] In the above-mentioned anisotropy evaluation method, if there is no anisotropy in bending rigidity, the small-diameter end of the blank tube moves vertically in a straight line after a load applied in the vertical direction is removed. However, if there is anisotropy in bending rigidity, the small-diameter end of the blank tube moves in an elliptical or circular motion. In other words, the smaller the anisotropy, the smaller the horizontal displacement. Also, a smaller evaluation value of the anisotropy indicates that there is no extreme anisotropy.

[0059] (Circularity) The roundness of the raw tube of the shaft of the present invention, measured by the following evaluation method, is 0.5 or less. It is more preferable that it is 0.4 or less, and even more preferable that it is 0.35 or less. Although the roundness is ideally 0, taking into consideration the error that is unavoidable in manufacturing, it is preferable that it is 0.01 or more. As described above, the outermost layer of the multiple fiber-reinforced resin layers has the greatest effect on bending rigidity. If there is a part of the shaft outer diameter that is convex, the rigidity of that part will be locally high, resulting in anisotropy. By keeping the roundness within the above range, the effect of anisotropy due to the shape of the cross section perpendicular to the shaft axis can be reduced.

[0060] [Roundness evaluation method] A jig is inserted into the inside of the small diameter end side and the large diameter end side of the mother tube to fix the mother tube approximately horizontally. One of the two lines formed by a plane passing through the axis of the mother tube and the outermost surface of the mother tube is defined as the 0° line. Using the 0° line as a reference, lines at 45°, 90°, and 135° are similarly defined in the counterclockwise circumferential direction of the mother tube as viewed from the small diameter end side. The outer diameter is measured using a laser type CCD length measuring sensor at any m points (m is a natural number of 5 or more) along the entire length of the shaft. At each measurement point, the outer diameter is measured including the lines of 0°, 45°, 90°, and 135°, obtaining data for a total of 4 m points. Based on the measurement results at each measurement point, the ratio of the difference between the maximum and minimum outer diameter values ​​to the average outer diameter is calculated. That is, Circularity = 100 × (D x,max -D x,min ) / D x,ave ...Equation (1) (In formula (1), x:Position [mm] D x,max : Maximum outer diameter of shaft at position x [mm] D x,min :Minimum outer diameter of shaft at position x [mm] D x,ave :Average shaft outer diameter at position x [mm] is) and calculate it.

[0061] The contribution rate of the outermost layer to bending rigidity, the horizontal displacement, the anisotropy, and the circularity can be measured by removing the design-imparting layer from the shaft by polishing to obtain a blank tube.

[0062] (Design-imparting layer) The design-imparting layer is applied to the outer surface of the blank tube and serves to decorate the tube by displaying a pattern, brand name, etc. Usually, a method is used in which an undercoat layer, an intermediate coat layer, etc. are applied first, followed by decoration with a decorative layer, and then an overcoat layer made of a transparent or translucent paint is formed on the surface, or decoration is performed with a colored spray coat. In this specification, the design-imparting layer refers to all layers applied to the outer surface of the blank tube other than the fiber-reinforced resin layer. The material for the decorative layer in the design-imparting layer may be any material that can improve the aesthetic appearance, such as metal foil, ink, spray, etc. The material for the overcoat layer, undercoat layer, and intermediate coat layer applied after decoration may be any material that has high adhesion to adjacent layers, such as the decorated portion and the base pipe, and can be used for protective coating purposes. The design-imparting layer may be provided over the entire length of the mother tube, or may be provided only to a part of the mother tube. The method of decorating with a decorative layer may be any method capable of decorating the outer surface of the tubular body, such as applying a pattern or the like by painting or printing directly onto the component body or via a metal layer, adhering an adhesive sheet having a base sheet with an adhesive layer on the back surface and decorated by screen printing or the like to the component body, or a spray coating method.

[0063] (Shaft properties) (weight)

[0064] The weight of the shaft of this embodiment varies with the overall shaft length Ls, making it difficult to define the weight clearly. Therefore, in this specification, the shaft weight is defined when the overall shaft length Ls is converted to 1,168 mm using the following formula (4). Converted shaft weight M C =M×(Ls / 1168)...Equation (4) M = shaft weight Ls = total shaft length If the shaft of the present invention is a driver, it is preferable that 1168≦Ls≦1219; if it is a fairway wood, it is preferable that 1067≦Ls≦1092; if it is a utility, it is preferable that 1016≦Ls≦1067; if it is an iron, it is preferable that 902≦Ls≦1016; and if it is a putter, it is preferable that 864≦Ls≦915. As mentioned above, the shaft of the present invention may be any type of shaft, but when the shaft of the present invention is a driver, 32.5≦M C ≦89.5 is preferable, and in the case of a fairway wood, 38.3≦M C ≦83.2 is preferable, and for utilities, 32.4≦M C ≦100.0, and in the case of iron, 29.7≦M C ≦99.6 is preferable, and in the case of a putter, 96.2≦M C It is preferred that it is ≦108.1.

[0065] (Shaft manufacturing method) The method for manufacturing the base tube of the shaft of the present invention is not particularly limited as long as it can produce the base tube of the present invention, and any known manufacturing method can be used. One example is a sheet wrapping method in which a fiber-reinforced resin layer (prepreg) made by impregnating a resin composition with sheet-like reinforcing fibers formed by aligning fibers in one direction is wrapped around a mandrel in multiple sheets, heated and cooled, and the mandrel is removed to form the shaft. When the matrix resin contained in the resin composition is a thermosetting resin, the prepreg refers to the matrix resin in an uncured state, and is considered to have been completely cured after heating. Furthermore, in the case where the matrix resin contained in the resin composition is a thermosetting resin, the fiber reinforced resin layer constituting the shaft of the present invention indicates one in which curing has been completed.

[0066] In the sheet wrapping method, a plurality of prepregs with different areas and orientation angles of the reinforcing fibers are prepared and wound one by one around a mandrel to produce a multi-layered shaft. The number of prepregs is generally about 8 to 14.

[0067] The shaft of the present invention can be manufactured by adjusting the area of ​​each prepreg, the orientation angle of the reinforcing fibers contained in each prepreg, the tensile modulus of the reinforcing fibers contained in each prepreg, the winding position of each prepreg, changing the number of prepreg layers, changing the shape of the mandrel, etc. In this case, the shape of the shaft, such as the taper degree and outer diameter of the shaft, and the physical properties of the shaft can be appropriately adjusted.

[0068] An embodiment of the method for manufacturing a shaft of the present invention will be described below, but the present invention is not limited to the following description. The method for producing a shaft of the present invention includes the steps of (1) arranging a prepreg having a contribution rate to bending rigidity of 0.5 to 15% as the outermost layer, (2) heating and then cooling the prepreg, and (3) polishing while controlling the outer shape.

[0069] As the prepreg, one using a thermosetting resin as the matrix resin is preferable because it has high physical properties after curing. The prepreg is heated at a temperature and for a time sufficient to complete curing if the matrix resin contained in the prepreg is a thermosetting resin, and at a temperature and for a time sufficient to soften and mold the prepreg if the matrix resin is a thermoplastic resin.

[0070] A preferred method for controlling the outer shape of the polished product is numerically controlled polishing. Numerical control polishing is a method for controlling the outer shape of the polished product according to CAD data of the outer shape of the molded product after polishing. By performing numerical control polishing, the anisotropy of the shaft caused by the outer shape can be reduced.

[0071] Furthermore, in addition to the bias layer and the straight layer, a partial bias layer, a partial straight reinforcement layer, and an outer diameter adjustment layer may be present. By providing a partial reinforcement layer, the torsional rigidity and bending rigidity can be partially controlled. The tensile modulus and thickness of the fiber are preferably within the above-mentioned ranges. The thickness of the outer diameter adjustment layer is preferably 0.050 mm or more and 0.500 mm or less.

[0072] (Shaft type) The shaft of this embodiment may be a shaft for any type of golf club, such as a driver, a fairway wood, a utility, an iron, or a putter.

[0073] (Golf clubs) Golf clubs are usually assembled by attaching a head to the tip end of a shaft and a grip to the butt end. Wooden golf clubs are usually assembled by cutting both ends of the shaft to make the total length 1100mm to 1130mm, so that the club has a normal length of 45 inches to 46 inches.

[0074] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. The technical scope of the present invention also includes embodiments obtained by appropriately combining the technical means disclosed in the different embodiments. Furthermore, new technical features can be formed by combining the technical means disclosed in the respective embodiments. EXAMPLES

[0075] The present invention will now be described in further detail with reference to examples. The present invention is not limited to the above-mentioned embodiment. For example, the bias layer may be one layer or two or more layers. The straight layer may be three layers, two layers, or four or more layers.

[0076] <Evaluation method for raw pipe> (Method of measuring natural frequency) The natural frequency of the blank tube was measured using the method shown in Figure 6. A Fujikura Rubber Golf Club Timing Harmonizer was used, and a weight 4 with a mass of 196 g simulating a head was attached to the tip end of shaft 1. The natural frequency of the shaft was measured with the distance from the butt end to fixture 5A set to 180 mm.

[0077] (How to measure the balance point) A schematic diagram of the balance point of the blank tube is shown in Fig. 7. The distance L from the tip end of the shaft to the center of gravity of the shaft G The total length of the blank tube L S The ratio of the Balance point(%)=(L G / L S )×100...(Formula 5) It can be calculated as follows. (How to measure kick point) The kick point was measured using a Fourteen shaft kick point gauge "FG-105RM" according to the method shown in FIG. Both ends of the shaft are fixed by rotatable fixing jigs 5B and 5C, and by moving one of the jigs, the fixing jigs are brought closer to each other, compressing the shaft and shortening the distance between the two ends to curve it. At this time, the distance L between the most protruding point in the circumferential direction of the shaft and the tip end is K The distance between both ends of the shaft when bent is L B And the above L K and L B The ratio of these two loads was determined as the kick point value. The compression load P applied from both ends varies depending on the flexural rigidity of the shaft, but should be applied so that the linear distance between both ends is 98.5 to 99.5% of the shaft length before compression. That is, Kick point(%)=(L K / L B )×100...(Formula 6) L K The distance between the tip end of the shaft and the intersection point of a perpendicular line drawn from the apex of the bend to a line connecting the two ends of the shaft when a compressive load is applied to the two ends of the shaft to bend the shaft such that the linear distance between the two ends of the shaft is 98.5 to 99.5% of the shaft length. L B The linear distance between both ends of the shaft when the shaft is bent by applying a compressive load to both ends of the shaft so that the linear distance between the two ends of the shaft is 98.5 to 99.5% of the shaft length. was calculated.

[0078] (Measurement of the contribution rate of the outermost layer to the bending stiffness) The evaluation was performed using the method described in the section [Method of measuring the contribution rate of the outermost layer to the bending rigidity]. The blank tube of the shaft of the present invention was designed and manufactured so that the outside diameter of the tip end was 8.5 mm and the outside diameter of the butt end was 15.2 mm.

[0079] (Roundness evaluation) The evaluation was performed based on the method described in [Method of evaluating roundness]. The outer diameter of the blank tube was measured using a laser type CCD length measuring sensor ZX-TG manufactured by Omron Corporation. The measurement positions x (mm) were 100 mm, 200 mm, 300 mm, 400 mm, 500 mm, 600 mm, 700 mm, 800 mm, 900 mm, and 1000 mm from the tip end side. The outer diameter was measured at each position at angles of 0°, 45°, 90°, and 135°, and a total of 40 pieces of data were obtained. This was repeated for three blank tubes, and a total of 120 pieces of data were obtained. For each blank tube, the ratio of the difference between the maximum and minimum values ​​of the outer diameter to the average value of the outer diameter at each position x (mm) was calculated.

[0080] (Evaluation of anisotropy) The evaluation was performed using the method described in the section "Method of evaluating anisotropy." When viewed from the tip end, the right side was taken as the right displacement, and the left side was taken as the left displacement.

[0081] Example 1 An iron mandrel was prepared with the shape shown in Figure 5. The outer diameter, length, and taper of each part of this mandrel were as follows: The outer diameter of P1 is 4.15 mm, the outer diameter of P2 is 5.9 mm, the outer diameter of P3 is 7.65 mm, the outer diameter of P4 and P5 is 13.8 mm, and the distance between P1 and P2 (L 1 )=200mm, distance between P2 and P3 (L 2 )=100mm, distance between P1 and P4 (L 3 )=700mm, distance between P1 and P5 (L 4 )=500mm, taper degree from P1 to P2=8.750 / 1000, taper degree from P2 to P3=17.5 / 1000, taper degree from P3 to P4=8.786 / 1000

[0082] The position on the mandrel where the prepregs were wound was from 80 mm to 1270 mm from the small diameter end. Next, one prepreg containing reinforcing fibers with an orientation angle of +45° to the axis of the bare tube and one prepreg containing reinforcing fibers with an orientation angle of -45° were prepared, and on the left side of pattern 2 in Fig. 1 (small diameter end), the two prepregs were overlapped so that the winding start ends (upper left end in the figure of the prepregs) were shifted by 9 mm, and on the right side of Fig. 2 (large diameter side), the two prepregs were overlapped so that the winding start ends (upper right end in the figure of the prepregs) were shifted by 22 mm, and they were bonded together at 180°C using an iron to obtain a laminated prepreg for forming a bias layer (pattern 2). Next, the prepregs (Patterns 1 to 7) cut to the shapes shown in Fig. 1 were wound around a mandrel in order to form a laminate, and a polypropylene shrink tape 20 mm wide and 0.03 mm thick was wound on top of it with a pitch of 1.5 mm to fix the uncured laminate. Details of the physical properties of the prepregs used in each pattern are shown in Table 1, and the sizes are shown in Table 5. Note that a glass cloth prepreg was used for pattern 7. In pattern 2, one sheet each of reinforcing fibers was arranged so that the orientation angle of the reinforcing fibers was +45° and -45° to form a bias layer. In patterns 4 and 5, reinforcing fibers were arranged so that the orientation angle of the reinforcing fibers was 0° to the axial direction of the mandrel to form a straight layer. In patterns 1, 3, and 6, reinforcing fibers were arranged so that the orientation angle of the reinforcing fibers was 0° to the axial direction of the mandrel to form a partially straight layer. In pattern 7, plain woven glass cloth prepregs were arranged so that the warp yarns were 0° to the axial direction of the mandrel.

[0083] The tube was then placed in a curing oven heated to 145°C for 2 hours to cure, then removed from the oven and allowed to cool to room temperature, the shrink tape was peeled off, and the narrow end was cut off by 10 mm and the wide end by 10 mm to give a total length of 1170 mm. The surface was then numerically controlled polished to the target outer diameter shown in Table 6, yielding a blank tube with a weight of 56.84 g, a natural frequency of 245 cpm, a balance point of 51.7%, and a kick point of 44.0%.

[0084] The total length, weight, natural frequency, balance point, and kick point of the obtained blank tube are shown in Table 7, the contribution rate of the outermost layer to the bending rigidity is shown in Table 8, the evaluation values ​​of horizontal displacement and anisotropy are shown in Table 9, and the roundness value is shown in Table 10.

[0085] Example 2 Shafts were manufactured in the same manner as in Example 1, except that the types of prepregs used were changed as shown in Table 2, the sizes were changed as shown in Table 5, and the prepregs (patterns 1 to 8) cut into the shapes shown in Fig. 2 were used. The results are shown in Tables 7 to 10.

[0086] Example 3 Shafts were manufactured in the same manner as in Example 1, except that the types of prepregs used were changed as shown in Table 3, the sizes as shown in Table 5, and the prepregs (patterns 1 to 7) cut into the shapes shown in Fig. 3 were used. The results are shown in Tables 7 to 9 and 11.

[0087] Comparative Example 1 Shafts were manufactured in the same manner as in Example 1, except that the types of prepregs used were changed as shown in Table 4, the sizes as shown in Table 5, and the prepregs (Patterns 1 to 6) cut into the shapes shown in Fig. 4 were used. The results are shown in Tables 7 to 9 and 11.

[0088] [Table 1]

[0089] [Table 2]

[0090] [Table 3]

[0091] [Table 4]

[0092]

Table 5

[0093]

Table 6

[0094]

Table 7

[0095]

Table 8

[0096]

Table 9

[0097] [Table 10]

[0098] [Table 11]

[0099] As is clear from Tables 7 to 11, the shafts of Examples 1 to 3 had small contributions of the outermost layer to the bending rigidity, and therefore small evaluation values ​​indicating anisotropy. On the other hand, the shaft of Comparative Example 1 had a large contribution of the outermost layer to the bending rigidity, and therefore had a large evaluation value indicating anisotropy, and thus had high anisotropy. [Industrial Applicability]

[0100] According to the present invention, a shaft can be provided that has low anisotropy and allows the golfer to achieve the swing he or she envisions. [Explanation of symbols]

[0101] 1 Shaft 1C Compressed and curved shaft 11 Tip end 12 Butt end 13 Shaft axis 2. Shaft center of gravity 3 Kick point position of the shaft 4. A weight of 196g simulating the head 5A, 5B, 5C, 5D, 5E, 5F, 5G, 5H, 5I fixing jig 6 pillars 7 Floodlight 8 Receiver 9 Sensor slide fixture L S Overall shaft length L G , L K , L B , L D , L H length x length P load

Claims

1. A golf club shaft including a blank tube having a plurality of fiber reinforced resin layers, a contribution rate of an outermost fiber reinforced resin layer of the raw tube to a bending rigidity of the golf club shaft is 0.5% or more and 5% or less, and the outermost fiber reinforced resin layer contains a cloth material, The cloth material is a glass cloth, and the orientation angle of the warp threads of the cloth material is −5° or more and +5° or less with respect to the axial direction of the golf club shaft.

2. 2. The shaft for a golf club according to claim 1, wherein the reinforcing fibers contained in the outermost fiber-reinforced resin layer have a tensile modulus of elasticity of 5 GPa or more and less than 100 GPa.

3. A golf club shaft including a blank tube having a plurality of fiber reinforced resin layers, A golf club shaft, wherein the contribution rate of the outermost fiber reinforced resin layer of the blank tube to the bending rigidity of the golf club shaft is 0.5% or more and 5% or less, the outermost fiber reinforced resin layer contains a unidirectional material, and an orientation angle of reinforcing fibers of the unidirectional material is +20° or more and +70° or less, or -70° or more and -20° or less.

4. 4. The shaft for a golf club according to claim 3, wherein the reinforcing fibers contained in the outermost fiber-reinforced resin layer have a tensile modulus of elasticity of 200 GPa or more and less than 500 GPa.

5. 5. The shaft for golf clubs according to claim 1, wherein the horizontal displacement evaluated by the following evaluation method is less than 18 mm. [Method for evaluating horizontal displacement] The mother tube is held approximately horizontally so that the thin-diameter end side can vibrate from 180 mm from the thick-diameter end of the mother tube. Two supports are installed on each side of the mother tube in the horizontal direction, 314.5 mm from the thin-diameter end. Next, with a weight of 196 g attached to the small diameter end of the mother tube, a load was applied in the direction of gravity so that the small diameter end was displaced 60 mm, and then the load was removed to vibrate the mother tube. The positions of the two supports were adjusted independently, and the distance from the mother tube axis to the supports when the vibrating mother tube came into contact with each of the two supports was taken as the horizontal displacement. The distance between the right support and the mother tube axis when looking at the mother tube from the small diameter end was taken as the horizontal displacement (right), and similarly the distance between the left support and the mother tube axis was taken as the horizontal displacement (left).

6. 6. The shaft for golf clubs according to claim 1, wherein the circularity obtained by the following evaluation method is 0.00 to 0.

39. [Method of evaluating roundness] A jig is inserted into the inside of the small diameter end side and the large diameter end side of the mother tube to fix the mother tube approximately horizontally. One of the two lines formed by a plane passing through the axis of the mother tube and the outermost surface of the mother tube is defined as the 0° line. Similarly, using the 0° line as a reference, lines at 45°, 90°, and 135° are defined counterclockwise around the mother tube as viewed from the small diameter end side. The outer diameter is measured at any m locations (m is a natural number of 5 or more) along the entire length of the shaft using a laser type CCD length measuring sensor. At each measurement point, the outer diameter including lines at 0°, 45°, 90°, and 135° is measured, obtaining data for a total of 4 m points. Based on the measurement results for each measurement point, the ratio of the difference between the maximum and minimum outer diameters to the average outer diameter is calculated. That is, Circularity = 100 x (D x,max -D x,min ) / D x,ave ...Formula (1) (In formula (1), x: position [mm] D x,max : Maximum outer diameter of shaft at position x [mm] D x,min : Minimum outer diameter of shaft at position x [mm] D x,ave : the average value of the outer diameter of the shaft at the position x [mm]) and calculate it.

7. A golf club comprising the golf club shaft according to any one of claims 1 to 6.

8. A method for manufacturing the golf club shaft according to any one of claims 1 to 7, comprising the following steps (1) to (3): (1) A step of disposing a prepreg having a contribution rate to bending rigidity of 0.5 to 15% as the outermost layer of a raw tube. (2) A step of heating and then cooling the prepreg (3) A process of polishing while controlling the outer shape

Citation Information

Patent Citations

  • Liquid drop charger

    JP1981062164A

  • Golf shaft made of fiber-reinforced plastic

    JP2000288139A

  • Golf club shaft

    JP2003024489A

  • Golf club shaft

    JP2009261473A

  • Golf club shaft and golf club

    JP2010284343A