Polarizing plate and image display device
The polarizing plate design with specific hole shapes and boron content in the polyvinyl alcohol resin layer addresses cracking issues in high-temperature environments, maintaining structural integrity during thermal shock tests.
Patent Information
- Application Number
- JP2021049689
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-03-24
AI Technical Summary
Polarizing plates used in in-vehicle image display devices with high temperature durability tend to crack in the hole portions during thermal shock tests due to their high shrinkage force.
A polarizing plate design with specific hole shapes, including straight and curved parts parallel to the transmission and absorption axes, and a boron content of 4.0% to 8.0% by mass in the polyvinyl alcohol resin layer, to reduce cracking during thermal shock tests.
The proposed polarizing plate design effectively minimizes cracking in holes even when subjected to high temperature durability tests, ensuring structural integrity.
Smart Images

Figure 0007570957000002 
Figure 0007570957000003 
Figure 0007570957000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing plate, and further to an image display device including a polarizing plate. [Background technology]
[0002] Liquid crystal display devices (LCDs) are widely used not only in liquid crystal televisions, but also in personal computers, mobile devices such as mobile phones, and in-vehicle applications such as car navigation systems. Typically, liquid crystal display devices have liquid crystal panels in which polarizing plates are attached to both sides of a liquid crystal cell via an adhesive layer, and display is performed by controlling light from a backlight member with the liquid crystal panel. In addition, organic electroluminescence (EL) display devices have also been widely used in recent years in mobile devices such as televisions and mobile phones, and in-vehicle applications such as car navigation systems, similar to liquid crystal display devices. In organic EL display devices, a circular polarizing plate (a laminate including a polarizing element and a λ / 4 plate) may be placed on the viewing side surface of the image display panel to prevent external light from being reflected by a metal electrode (cathode) and being viewed as a mirror surface.
[0003] As described above, polarizing plates are increasingly being installed in vehicles as components of liquid crystal display devices and organic electroluminescence display devices. Polarizing plates used in vehicle-mounted image display devices are more often exposed to high-temperature environments than other mobile applications such as televisions and mobile phones, and are therefore required to have smaller changes in properties at high temperatures (high-temperature durability), and a polarizing element aimed at ensuring such durability has been proposed (Patent Document 1). The polarizing element described in Patent Document 1 can ensure high-temperature durability, but has a high boron content and tends to have a high shrinkage force at high temperatures. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2019 / 188779 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, holes are increasingly being provided in polarizing plates. For example, polarizing plates used in in-vehicle image display devices and the like may have holes for passing the needles of meter panels, and polarizing plates used in smartphones may have holes for camera holes. However, when a polarizing element having high high-temperature durability (shrinkage force) as described above is used in a polarizing plate having such holes, cracks tend to easily occur in the absorption axis direction of the polarizing element in a thermal shock test (also called a heat shock test).
[0006] An object of the present invention is to provide a polarizing plate in which cracks are unlikely to occur in holes during a thermal shock test, even when a polarizing element having high high-temperature durability is used. [Means for solving the problem]
[0007] The present invention provides the following polarizing plate and image display device. [1] A polarizing element having a dichroic dye adsorbed and oriented in a polyvinyl alcohol-based resin layer; A transparent protective film; A polarizing plate having The polyvinyl alcohol-based resin layer has a boron adsorption rate of 5.70% by mass or more, The polarizing element has a boron content of 4.0% by mass or more and 8.0% by mass or less, At least one hole is provided within a plane in a plan view, The shape of the hole satisfies both of the following conditions (1a) and (1b): (1a) The shape of the hole has two straight line portions that are approximately parallel to the transmission axis of the polarizing element, and the length of the straight line portions that are approximately parallel to the transmission axis of the polarizing element is 10 mm or less. (1b) The shape of the hole has at least two curved portions, and the radius of curvature of the curved portions is 0.5 mm or more and less than 11 mm. [2] The polarizing plate according to [1], wherein the shape of the hole further satisfies the following condition (1c): (1c) The polarizing element further has two linear portions approximately parallel to the absorption axis. [3] The polarizing plate according to [1] or [2], wherein the polarizing plate has a rectangular shape in a plan view and a diagonal length of 6 inches or more. [4] An image display device comprising the polarizing plate according to any one of [1] to [3]. Effect of the Invention
[0008] According to the present invention, it is possible to provide a polarizing plate in which cracks are unlikely to occur in holes during a thermal shock test, even when a polarizing element having high high-temperature durability is used. [Brief description of the drawings]
[0009] [Figure 1] 5A to 5C are schematic plan views showing examples of the shape of a hole portion. [Diagram 2] FIG. 2 is a schematic plan view illustrating an example of a polarizing plate. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing an example of a layer structure of a polarizing plate. [Figure 4] (A) is a plan view showing an example of how the cutting tool moves in a spiral shape relative to the laminate film in the first cutting step. (B) is a plan view showing how the cutting tool moves relative to the laminate film as a comparative example. The line with the arrow in the figure indicates the route along which the cutting tool moves relative to the laminate film when viewed from a direction perpendicular to the main surface of the laminate film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings, but the present invention is not limited to the following embodiment. In all of the drawings, the scale of each component is appropriately adjusted to make it easier to understand, and the scale of each component shown in the drawings does not necessarily match the scale of the actual component.
[0011] <Polarizing plate> A polarizing plate according to one embodiment of the present invention has a polarizing element formed by adsorbing and aligning a dichroic dye in a polyvinyl alcohol-based resin layer, and a transparent protective film, in which the polyvinyl alcohol-based resin layer has a boron adsorption rate of 5.70 mass% or more, the polarizing element has a boron content of 4.0 mass% or more and 8.0 mass% or less, and has at least one hole within a plane when viewed in a plan view, and the shape of the hole satisfies both of the following conditions (1a) and (1b): (1a) The shape of the hole has two straight line portions that are approximately parallel to the transmission axis of the polarizing element, and the length of the straight line portions that are approximately parallel to the transmission axis of the polarizing element is 10 mm or less. (1b) The shape of the hole has at least two curved portions, and the radius of curvature of the curved portions is 0.5 mm or more and less than 11 mm. In this specification, the term "planar view" refers to a view from the thickness direction (stacking direction) of the polarizing plate.
[0012] The holes in the polarizing plate penetrate in a direction perpendicular to the main surface of the polarizing plate. The shape of the holes can be, for example, a rectangular shape with curved corners (hereinafter, also referred to as a rounded rectangular shape). As shown in FIG. 1, examples of the rounded rectangular shape include a shape having four curved parts and four straight parts [FIGS. 1(a), (b), and (c)], a shape having two curved parts and two straight parts [FIGS. 1(d) and (e)], and a shape having two curved parts and five straight parts [FIG. 1(f)]. The main surface of the polarizing plate refers to the surface in a plan view.
[0013] [Condition (1a)] The shape of the hole has two straight line parts that are approximately parallel to the transmission axis of the polarizing element. In this specification, one straight line part refers to a part of the shape of the hole that consists of only one straight line. For example, in the shape of FIG. 1(f), the number of straight line parts is two in both the part where two parallel straight lines f1 and f2 are formed separately on the same line and the part where two non-parallel straight lines f3 and f4 are connected. In this specification, approximately parallel to the transmission axis is not limited to being strictly parallel, and for example, the angle between the transmission axis of the polarizing element and the straight line part is preferably 5° or less, more preferably 3° or less, even more preferably 1° or less, and most preferably 0°. When the shape of the hole has four straight line parts as shown in FIG. 1(a), (b), and (c), a pair of opposing straight line parts is approximately parallel to the transmission axis of the polarizing element. For example, in the polarizing plate 1 shown in FIG. 2, the straight line parts 2a and 2c that constitute the shape of the hole part 2 can be approximately parallel to the transmission axis direction. The length of the straight line portion approximately parallel to the transmission axis of the polarizing element is preferably 9 mm or less, more preferably 0.2 mm to 8 mm, and even more preferably 0.5 mm to 7 mm. The polarizing plate tends to be less susceptible to cracks in a thermal shock test when the hole has two straight line portions approximately parallel to the transmission axis of the polarizing element. The shape of the hole may have two or more straight line portions approximately parallel to the transmission axis of the polarizing element.
[0014] [Condition (1b)] The shape of the hole has at least two curved parts. The curved parts refer to the parts of the shape of the hole that are made of continuous curves. For example, in Fig. 1(a), (b) and (c), the number of curved parts is four, and in Fig. 1(d) and (e), the number of curved parts is two. Also, as shown in Fig. 1(a), (b), (d) and (f), the radii of curvature of the curved parts may all be the same, and as shown in Fig. 1(c) and (e), all of the radii of curvature of the curved parts may not be the same. The radii of curvature of the curved parts are preferably 1 mm or more and 10 mm or less, more preferably 1.5 mm or more and 9 mm or less. When the hole has at least two of the above-mentioned curved parts, the polarizing plate tends to be less likely to crack in a thermal shock test. The shape of the hole preferably has four curved parts all of which have the same radii of curvature.
[0015] The shape of the holes in the polarizing plate can further satisfy the following condition (1c). (1c) The polarizing element further has two linear portions approximately parallel to the absorption axis. In this specification, "approximately parallel to the absorption axis" is not limited to being strictly parallel, and for example, the angle between the absorption axis of the polarizing element and the straight line portion is preferably 5° or less, more preferably 3° or less, even more preferably 1° or less, and most preferably 0°. When the shape of the hole has four straight lines as shown in Figures 1(a), (b) and (c), a pair of opposing straight lines can be approximately parallel to the absorption axis of the polarizing element. For example, in the polarizing plate 1 shown in Figure 2, the straight lines 2b and 2d constituting the shape of the hole 2 can be approximately parallel to the absorption axis direction. The length of the straight line portion approximately parallel to the absorption axis of the polarizing element may be, for example, less than 11 mm, preferably 0.5 mm or more and 10.5 mm or less, more preferably 1 mm or more and 10 mm or less.
[0016] The shape of the polarizing plate may be rectangular in a plan view, for example, a square, a rectangle, a square with rounded corners, or a rectangle with rounded corners.
[0017] When the polarizing plate has a rectangular shape in a plan view, the diagonal length may be, for example, 6 inches (152.4 mm) or more, and preferably 6 inches (152.4 mm) or more and 30 inches (767 mm) or less.
[0018] The relationship between the shape of the polarizing plate and the direction of the absorption axis of the polarizing element is not particularly limited, but for example, when the polarizing plate is rectangular in plan view, the absorption axis may be parallel to the long side direction, or parallel to the short side direction, or may be at an angle of 45±5° with respect to the long side direction (or short side direction), preferably 45±2°. The absorption axis of the polarizing element may be the extension axis of the polarizing element.
[0019] The thickness of the polarizing plate can usually be set to 5 μm or more and 200 μm or less, and may be 150 μm or less, or may be 120 μm or less.
[0020] Fig. 3 shows an example of the layer structure of a polarizing plate. The polarizing plate 10 shown in Fig. 3 has a polarizing element 11 and a transparent protective film 12. The polarizing element 11 and the transparent protective film 12 may be laminated via an adhesive layer described later. The polarizing plate may further have an optically functional layer, an attachment layer, and a protective film described later.
[0021] [Polarizing element] A well-known polarizing element can be used as the polarizing element formed by adsorbing and orienting a dichroic dye in a polyvinyl alcohol (hereinafter also referred to as "PVA")-based resin layer (also referred to as a "PVA-based resin layer" in this specification). Examples of such polarizing elements include those formed by using a PVA-based resin film, dyeing this PVA-based resin film with a dichroic dye, and uniaxially stretching it, and those formed by using a laminated film obtained by applying a coating liquid containing a PVA-based resin onto a base film, dyeing the PVA-based resin layer, which is the coating layer of this laminated film, with a dichroic dye, and uniaxially stretching the laminated film.
[0022] The polarizing element is made of a PVA resin obtained by saponifying a polyvinyl acetate resin. Examples of polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, and copolymers of vinyl acetate and other monomers that can be copolymerized with it. Examples of other monomers that can be copolymerized include unsaturated carboxylic acids, olefins such as ethylene, vinyl ethers, and unsaturated sulfonic acids.
[0023] In the present invention, the PVA-based resin layer is formed from a PVA-based resin having a boron adsorption rate of 5.70% by mass or more. That is, the boron adsorption rate of the PVA-based resin in the raw material stage before dyeing or stretching is 5.70% by mass or more. By using such a PVA-based resin, the transmittance is unlikely to decrease even when exposed to a high-temperature environment of, for example, 105°C. A polarizing element is produced using a PVA-based resin having a boron adsorption rate of more preferably 5.72% by mass or more, further preferably 5.75% by mass, and most preferably 5.80% by mass or more. In addition, the boron adsorption rate of the PVA-based resin is preferably 10% by mass or less. By producing a polarizing element using such a PVA-based resin, the boric acid concentration in the boric acid treatment bath does not need to be high, and the treatment time by boric acid treatment can be shortened, making it easier to obtain a desired polarizing element and increasing the productivity of the polarizing element. When the boron adsorption rate of the PVA-based resin is 10% by mass or less, an appropriate amount of boron is incorporated into the PVA-based resin layer, and the shrinkage force of the polarizing element is easily reduced. As a result, when the PVA-based resin is incorporated into an image display device, problems such as peeling between the polarizing plate and other members such as a front plate are unlikely to occur. In addition, when the boron adsorption rate of the PVA-based resin is less than 5.70%, the transmittance is likely to decrease even when exposed to a high-temperature environment of, for example, 105°C, and the productivity may also decrease as described above. The boron adsorption rate of the PVA-based resin can be measured by the method described in the examples below.
[0024] The boron adsorption rate of PVA-based resin is a characteristic of PVA-based resin that reflects the spacing between molecular chains and the crystal structure in the PVA-based resin. It is considered that PVA-based resin with a boron adsorption rate of 5.70% by mass or more has a wider spacing between molecular chains and fewer crystals of the PVA-based resin compared to PVA-based resin with a boron adsorption rate of less than 5.70% by mass. It is therefore assumed that boron can easily penetrate into the PVA-based resin layer, making it easier to prevent polyenization in a high-temperature environment.
[0025] The boron adsorption rate of the PVA-based resin can be adjusted, for example, by subjecting the PVA-based resin to a pretreatment such as hot water treatment, acid solution treatment, ultrasonic irradiation treatment, or radiation irradiation treatment before the production of a polarizing element. These treatments can increase the distance between molecular chains in the PVA-based resin or destroy the crystal structure. The hot water treatment can be, for example, a treatment of immersing the resin in pure water at 30°C to 100°C for 1 to 90 seconds and drying it. The acid solution treatment can be, for example, a treatment of immersing the resin in an aqueous boric acid solution with a concentration of 10% to 20% for 1 to 90 seconds and drying it. The ultrasonic treatment can be, for example, a treatment of irradiating ultrasonic waves with a frequency of 20 to 29 kc at an output of 200 W to 500 W for 30 seconds to 10 minutes. The ultrasonic treatment can be carried out in a solvent such as water.
[0026] The saponification degree of the PVA resin is preferably about 85 mol% or more, more preferably about 90 mol% or more, and further preferably about 99 mol% to 100 mol%. The polymerization degree of the PVA resin is 1000 to 10000, preferably 1500 to 5000. The PVA resin may be modified, and may be, for example, polyvinyl formal, polyvinyl acetal, polyvinyl butyral, etc., modified with aldehydes.
[0027] The thickness of the polarizing element of this embodiment is preferably 5 to 50 μm, more preferably 8 to 28 μm, even more preferably 12 to 22 μm, and most preferably 12 to 15 μm. When the thickness of the polarizing element is 50 μm or less, the effect of polyenation of the PVA resin on the deterioration of optical properties in a high-temperature environment can be suppressed, and when the thickness of the polarizing element is 5 μm or more, it is easy to achieve a configuration that achieves desired optical properties.
[0028] The polarizing element has a boron content of preferably 4.0% by mass to 8.0% by mass, more preferably 4.2% by mass to 7.0% by mass, and even more preferably 4.4% by mass to 6.0% by mass. If the boron content of the polarizing element exceeds 8.0% by mass, the contraction force of the polarizing element increases, and problems such as peeling between the polarizing element and other members such as a front plate to which the polarizing element is bonded when the polarizing element is incorporated into an image display device may occur. If the boron content is less than 2.4% by mass, the desired optical characteristics may not be achieved. The boron content of the polarizing element can be calculated as the mass fraction (mass%) of boron relative to the mass of the polarizing element by, for example, inductively coupled plasma (ICP) emission spectroscopy. Boron is considered to exist in the polarizing element in the form of boric acid or a crosslinked structure formed between the boric acid and a component of a polyvinyl alcohol resin, but the boron content here is a value in terms of boron atoms (B).
[0029] By setting the boron content at 4.0% by mass or more and 8.0% by mass or less, the decrease in transmittance of the polarizing element is suppressed even when it is exposed to a high-temperature environment as a component of an image display device with an interlayer filling structure. This is presumably because, when the boron content of the polarizing element is 4.0% by mass or more and 8.0% by mass or less, polyenization is unlikely to occur even in a high-temperature environment, and the decrease in transmittance is suppressed.
[0030] From the viewpoint of suppressing deterioration of the optical properties of the polarizing element in a high-temperature environment, the potassium content in the polarizing element is preferably 0.28 mass% or more, more preferably 0.32 mass% or more, and even more preferably 0.34 mass% or more, and from the viewpoint of suppressing a change in hue in a high-temperature environment, the potassium content is preferably 0.60 mass% or less, more preferably 0.55 mass% or less, and even more preferably 0.50 mass% or less.
[0031] The zinc content in the polarizing element is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.05% by mass or more, and is preferably 2.00% by mass or less, more preferably 1.00% by mass or less, and even more preferably 0.50% by mass or less, from the viewpoint of suppressing the deterioration of the optical properties of the polarizing element and the change in hue in a high-temperature environment. The zinc content in the polarizing element can be measured, for example, as follows. Nitric acid is added to a precisely weighed polarizer, and the solution obtained by acid decomposition using a microwave sample preparation device (ETHOS D) manufactured by Milestone General is used as the measurement solution. The zinc concentration is determined by quantifying the zinc concentration in the measurement solution using an ICP optical emission spectrometer (5110 ICP-OES) manufactured by Agilent Technologies, and calculating it from the mass of zinc relative to the mass of the polarizing element.
[0032] Although the detailed mechanism is unknown, it is presumed that polyenation can be suppressed because the polarizing element contains more boron and less potassium than conventional polarizing elements, and therefore the hydroxyl groups of the polyvinyl alcohol in the polarizing element are protected (stabilized) by boric acid crosslinking, and the appropriate potassium content stabilizes the iodine ions that serve as counter ions in the polarizing element.
[0033] The luminosity-corrected single transmittance of the polarizing plate is preferably 38.8% to 44.8%, more preferably 40.4% to 43.2%, and further preferably 40.7% to 43.0%. If the luminosity-corrected single transmittance exceeds 44.8%, the optical properties may deteriorate significantly, such as red discoloration in a high-temperature environment, whereas if the luminosity-corrected single transmittance is less than 38.8%, polyenization may easily proceed in a high-temperature environment, resulting in significant deterioration of the optical properties.
[0034] The luminosity-corrected single transmittance can be determined by measuring the luminosity-corrected Y value using a 2-degree visual field (C light source) as specified in JIS Z8701-1982.
[0035] The luminosity-corrected polarization degree of the polarizing plate may be, for example, 99.00% or more, preferably 99.90% or more, and is usually 100% or less, for example, less than 100%.
[0036] The polarizing plate may have an absolute value of difference in luminous efficiency corrected single transmittance before and after a high-temperature durability test of, for example, 6% or less, preferably 4% or less, and more preferably 2% or less. The polarizing plate may have an absolute value of the difference in luminosity-corrected polarization degree before and after a high-temperature durability test that is, for example, less than 0.5%, preferably 0.4% or less, and more preferably 0.2% or less. The polarizing plate may have an absolute value of the amount of change in hue (color difference: NBS unit) before and after a high-temperature durability test of, for example, 15 NBS or less, preferably 10 NMB or less, and more preferably 7 NBS or less. The high temperature durability test can be carried out according to the method described in the Examples section below.
[0037] The luminous efficiency corrected single transmittance, luminous efficiency polarization degree, and hue can be easily measured using, for example, a spectrophotometer manufactured by JASCO Corporation (model number: V7100).
[0038] The method for producing the polarizing element is not particularly limited, but typical examples include a method in which a polyvinyl alcohol-based resin film that has been previously wound into a roll is sent out and stretched, dyed, crosslinked, etc. (hereinafter referred to as "production method 1"), and a method including a step of applying a coating liquid containing a polyvinyl alcohol-based resin onto a substrate film to form a polyvinyl alcohol-based resin layer as a coating layer, and stretching the resulting laminate (hereinafter referred to as "production method 2").
[0039] Manufacturing method 1 can be achieved through a process of uniaxially stretching a polyvinyl alcohol-based resin film, a process of dyeing the polyvinyl alcohol-based resin film with a dichroic dye such as iodine to adsorb the dichroic dye, a process of treating the polyvinyl alcohol-based resin film with the adsorbed dichroic dye with an aqueous boric acid solution, and a process of washing with water after the treatment with the aqueous boric acid solution.
[0040] The boron content and potassium content in the polarizing element can be controlled by the concentration of boron component donating substances such as boron compounds such as boric acid, borate, borax, etc., and the concentration of potassium component donating substances such as potassium halide such as potassium iodide, etc., contained in any of the treatment baths in the swelling step, dyeing step, crosslinking step, stretching step, and water washing step, and the treatment temperature and treatment time in each of the above treatment baths. In particular, the crosslinking step and stretching step are easy to adjust the boron content to a desired range depending on treatment conditions such as the concentration of the boron component donating substance. In addition, the water washing step is easy to adjust the boron content and potassium content to a desired range, taking into consideration treatment conditions such as the amount of the boron component donating substance and potassium component donating substance used in the dyeing step, crosslinking step, stretching step, etc., from the viewpoint of being able to dissolve components such as boron and potassium from the polyvinyl alcohol-based resin film or adsorb them to the polyvinyl alcohol-based resin film.
[0041] The swelling step is a treatment step of immersing the polyvinyl alcohol-based resin film in a swelling bath, which can remove dirt and blocking agents on the surface of the polyvinyl alcohol-based resin film, and can suppress uneven dyeing by swelling the polyvinyl alcohol-based resin film. The swelling bath is usually a medium mainly composed of water, such as distilled water or pure water. The swelling bath may contain surfactants, alcohol, etc., as appropriate, according to a conventional method. In addition, potassium iodide may be used in the swelling bath from the viewpoint of controlling the potassium content of the polarizing element. In this case, the concentration of potassium iodide in the swelling bath is preferably 1.5% by weight or less, more preferably 1.0% by weight or less, and even more preferably 0.5% by weight or less.
[0042] The temperature of the swelling bath is preferably about 10 to 60° C., more preferably about 15 to 45° C., and even more preferably about 18 to 30° C. The immersion time in the swelling bath cannot be determined in general because the degree of swelling of the polyvinyl alcohol-based resin film is affected by the temperature of the swelling bath, but is preferably about 5 to 300 seconds, more preferably about 10 to 200 seconds, and even more preferably about 20 to 100 seconds. The swelling step may be carried out only once, or may be carried out multiple times as necessary.
[0043] The dyeing process is a treatment process in which the polyvinyl alcohol-based resin film is immersed in a dye bath (iodine solution), and iodine or a dichroic substance such as a dichroic dye can be adsorbed and oriented in the polyvinyl alcohol-based resin film. The iodine solution is usually preferably an aqueous iodine solution, and contains iodine and an iodide as a dissolving aid. Examples of iodides include potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, and titanium iodide. Among these, potassium iodide is preferred from the viewpoint of controlling the potassium content in the polarizing element.
[0044] In the dye bath, the iodine concentration is preferably about 0.01 to 1% by weight, more preferably about 0.02 to 0.5% by weight, and the iodide concentration is preferably about 0.01 to 10% by weight, more preferably about 0.05 to 5% by weight, and even more preferably about 0.1 to 3% by weight.
[0045] The temperature of the dye bath is preferably about 10 to 50° C., more preferably about 15 to 45° C., and even more preferably about 18 to 30° C. The immersion time in the dye bath cannot be determined in general because the degree of dyeing of the polyvinyl alcohol-based resin film is affected by the temperature of the dye bath, but is preferably about 10 to 300 seconds, and more preferably about 20 to 240 seconds. The dyeing process may be carried out only once, or may be carried out multiple times as necessary.
[0046] The crosslinking step is a treatment step in which the polyvinyl alcohol-based resin film dyed in the dyeing step is immersed in a treatment bath (crosslinking bath) containing a boron compound, and the polyvinyl alcohol-based resin film is crosslinked by the boron compound, so that iodine molecules or dye molecules can be adsorbed to the crosslinked structure. Examples of the boron compound include boric acid, borate salts, and borax. The crosslinking bath is generally an aqueous solution, but may also be, for example, a mixed solution of water and an organic solvent miscible with water. In addition, the crosslinking bath preferably contains potassium iodide from the viewpoint of controlling the content of potassium in the polarizing element.
[0047] In the crosslinking bath, the concentration of the boron compound is preferably about 1 to 15% by weight, more preferably about 1.5 to 10% by weight, and more preferably about 2 to 5% by weight. In addition, when potassium iodide is used in the crosslinking bath, the concentration of potassium iodide in the crosslinking bath is preferably about 1 to 15% by weight, more preferably about 1.5 to 10% by weight, and more preferably about 2 to 5% by weight.
[0048] The temperature of the crosslinking bath is preferably about 20 to 70° C., more preferably about 30 to 60° C. The immersion time in the crosslinking bath cannot be determined in general because the degree of crosslinking of the polyvinyl alcohol resin film is affected by the temperature of the crosslinking bath, but is preferably about 5 to 300 seconds, more preferably about 10 to 200 seconds. The crosslinking step may be carried out only once, or may be carried out multiple times as necessary.
[0049] The stretching process is a process for stretching a polyvinyl alcohol-based resin film at least in one direction to a predetermined magnification. In general, the polyvinyl alcohol-based resin film is uniaxially stretched in the conveying direction (longitudinal direction). There are no particular limitations on the stretching method, and either a wet stretching method or a dry stretching method can be used. The stretching process may be carried out only once, or may be carried out multiple times as necessary. The stretching process may be carried out at any stage in the production of a polarizing element.
[0050] The treatment bath (stretching bath) in the wet stretching method can usually use a solvent such as water or a mixed solution of water and an organic solvent miscible with water. The stretching bath preferably contains potassium iodide from the viewpoint of controlling the potassium content in the polarizing element. When potassium iodide is used in the stretching bath, the concentration of potassium iodide in the stretching bath is preferably about 1 to 15% by weight, more preferably about 2 to 10% by weight, and more preferably about 3 to 6% by weight. In addition, the treatment bath (stretching bath) can contain a boron compound from the viewpoint of suppressing film breakage during stretching, and in this case, the concentration of the boron compound in the stretching bath is preferably about 1 to 15% by weight, more preferably about 1.5 to 10% by weight, and more preferably about 2 to 5% by weight.
[0051] The temperature of the stretching bath is preferably about 25 to 80° C., more preferably about 40 to 75° C., and even more preferably about 50 to 70° C. The immersion time in the stretching bath cannot be determined in general because the degree of stretching of the polyvinyl alcohol-based resin film is affected by the temperature of the stretching bath, but is preferably about 10 to 800 seconds, and more preferably about 30 to 500 seconds. The stretching treatment in the wet stretching method may be performed together with one or more treatment steps of a swelling step, a dyeing step, a crosslinking step, and a washing step.
[0052] Examples of the dry stretching method include a roll-to-roll stretching method, a heated roll stretching method, a compression stretching method, etc. The dry stretching method may be carried out together with a drying step.
[0053] The total stretching ratio (cumulative stretching ratio) applied to the polyvinyl alcohol-based resin film can be appropriately set depending on the purpose, but is preferably about 2 to 7 times, more preferably about 3 to 6.8 times, and even more preferably about 3.5 to 6.5 times.
[0054] The cleaning step is a treatment step in which the polyvinyl alcohol-based resin film is immersed in a cleaning bath, and foreign matter remaining on the surface of the polyvinyl alcohol-based resin film can be removed. A medium containing water as a main component, such as water, distilled water, or pure water, is usually used as the cleaning bath. From the viewpoint of controlling the potassium content in the polarizing element, it is preferable to use potassium iodide in the cleaning bath. In this case, the concentration of potassium iodide in the cleaning bath is preferably about 1 to 10% by weight, more preferably about 1.5 to 4% by weight, and even more preferably about 1.8 to 3.8% by weight.
[0055] The temperature of the cleaning bath is preferably about 5 to 50° C., more preferably about 10 to 40° C., and even more preferably about 15 to 30° C. The immersion time in the cleaning bath cannot be determined in general because the degree of cleaning of the polyvinyl alcohol-based resin film is affected by the temperature of the cleaning bath, but is preferably about 1 to 100 seconds, more preferably about 2 to 50 seconds, and even more preferably about 3 to 20 seconds. The cleaning step may be carried out only once, or may be carried out multiple times as necessary.
[0056] Furthermore, among the above steps, or as a step separate from the above steps, a metal ion treatment step may be included. The metal ion treatment step is carried out by immersing the polyvinyl alcohol-based resin film in an aqueous solution containing a metal salt of a metal ion. The metal ion treatment step causes the polyvinyl alcohol-based resin film to contain metal ions.
[0057] The metal ion is not limited as long as it is a metal ion other than potassium ion, and is preferably an ion of a metal other than an alkali metal, and in particular, from the viewpoint of color tone adjustment and durability, it is preferable to include at least one metal ion of a transition metal such as cobalt, nickel, zinc, chromium, aluminum, copper, manganese, and iron. Among these metal ions, zinc ion is preferable from the viewpoint of color tone adjustment and heat resistance. Examples of zinc salts include zinc halides such as zinc chloride and zinc iodide, zinc sulfate, and zinc acetate.
[0058] In the metal ion treatment step, a metal salt solution is used. Hereinafter, a treatment of immersion in a zinc-containing solution will be described as a representative example of a metal ion treatment step in which an aqueous zinc salt solution is used.
[0059] The zinc ion concentration in the zinc salt aqueous solution is about 0.1 to 10% by mass, preferably in the range of 0.3 to 7% by mass. In addition, it is preferable to use an aqueous solution of the zinc salt containing potassium ions and iodine ions by potassium iodide or the like, since this makes it easier to impregnate the zinc ions. The potassium iodide concentration in the zinc salt solution is about 0.1 to 10% by mass, preferably 0.2 to 5% by mass.
[0060] In the immersion treatment in the zinc-containing solution, the temperature of the zinc salt solution is usually about 15 to 85°C, preferably 25 to 70°C. The immersion time is usually about 1 to 120 seconds, preferably 3 to 90 seconds. In the immersion treatment in the zinc-containing solution, the zinc content in the polyvinyl alcohol-based resin film is adjusted to be within the above range by adjusting the conditions such as the concentration of the zinc salt solution, the immersion temperature of the polyvinyl alcohol-based resin film in the zinc salt solution, and the immersion time. There is no particular restriction on when the immersion treatment in the zinc-containing solution is performed. The immersion treatment in the zinc-containing solution may be performed alone, or may be performed simultaneously with at least one of the dyeing step, the crosslinking step, and the stretching step by making the zinc salt coexist in the dyeing bath, the crosslinking bath, and the stretching bath.
[0061] The drying step is a step of drying the polyvinyl alcohol-based resin film washed in the washing step to obtain a polarizing element. The drying can be performed by any appropriate method, for example, natural drying, air drying, or heat drying.
[0062] The manufacturing method 2 can be produced through the steps of applying a coating solution containing the polyvinyl alcohol resin onto a substrate film, uniaxially stretching the obtained laminated film, dyeing the polyvinyl alcohol resin layer of the uniaxially stretched laminated film with a dichroic dye to adsorb the dichroic dye to form a polarizing element, treating the film with the adsorbed dichroic dye with an aqueous boric acid solution, and washing with water after the treatment with the aqueous boric acid solution. The substrate film used to form the polarizing element may be used as a protective layer for the polarizing element. If necessary, the substrate film may be peeled off and removed from the polarizing element.
[0063] [Transparent protective film] The transparent protective film used in this embodiment (hereinafter also simply referred to as "protective film") is attached to at least one surface of the polarizing element via an adhesive layer. This transparent protective film is attached to one or both surfaces of the polarizing element, but it is more preferable that it is attached to both surfaces.
[0064] The protective film may have other optical functions at the same time, and may be formed into a laminated structure in which a plurality of layers are laminated. The thickness of the protective film is preferably thin from the viewpoint of optical properties, but if it is too thin, the strength decreases and the processability becomes poor. The appropriate thickness is 5 to 100 μm, preferably 10 to 80 μm, and more preferably 15 to 70 μm.
[0065] The protective film may be a cellulose acylate film, a film made of a polycarbonate resin, a film made of a cycloolefin resin such as norbornene, a (meth)acrylic polymer film, a polyester resin film such as polyethylene terephthalate, etc. In a configuration in which protective films are provided on both sides of a polarizing element, when bonding is performed using a water-based adhesive such as a PVA adhesive, it is preferable that the protective film on at least one side is either a cellulose acylate film or a (meth)acrylic polymer film in terms of moisture permeability, and among these, a cellulose acylate film is preferable.
[0066] At least one of the protective films may have a retardation function for the purpose of compensating for viewing angle, etc. In that case, the film itself may have a retardation function, may have a separate retardation layer, or may be a combination of both. In the above description, the film having phase difference function is directly attached to the polarizing element via an adhesive. However, the film may be attached to the polarizing element via a pressure-sensitive adhesive or adhesive via another protective film attached to the polarizing element.
[0067] [Adhesive layer] The adhesive constituting the adhesive layer for bonding the protective film to the polarizing element can be any suitable adhesive. The adhesive can be a water-based adhesive, a solvent-based adhesive, an active energy ray curable adhesive, or the like, but is preferably a water-based adhesive. From the viewpoint of improving heat resistance, the adhesive layer preferably contains at least one urea-based compound selected from urea, urea derivatives, thiourea, and thiourea derivatives.
[0068] The thickness of the adhesive when applied can be set to any suitable value. For example, it is set so that an adhesive layer having a desired thickness is obtained after curing or heating (drying). The thickness of the adhesive layer is preferably 0.01 μm or more and 7 μm or less, more preferably 0.01 μm or more and 5 μm or less, even more preferably 0.01 μm or more and 2 μm or less, and most preferably 0.01 μm or more and 1 μm or less.
[0069] (Water-based adhesive) Any suitable aqueous adhesive may be used as the aqueous adhesive. Among them, an aqueous adhesive containing a PVA resin (PVA adhesive) is preferably used. The average polymerization degree of the PVA resin contained in the aqueous adhesive is preferably about 100 to 5500, more preferably 1000 to 4500, from the viewpoint of adhesiveness. The average saponification degree is preferably about 85 mol% to 100 mol%, more preferably 90 mol% to 100 mol%, from the viewpoint of adhesiveness.
[0070] The PVA resin contained in the water-based adhesive preferably contains an acetoacetyl group, because it has excellent adhesion between the PVA resin layer and the protective film and excellent durability. The acetoacetyl group-containing PVA resin can be obtained, for example, by reacting a PVA resin with diketene by any method. The acetoacetyl group modification degree of the acetoacetyl group-containing PVA resin is typically 0.1 mol% or more, and preferably about 0.1 mol% to 20 mol%. The resin concentration of the above-mentioned water-based adhesive is preferably 0.1% by mass to 15% by mass, and more preferably 0.5% by mass to 10% by mass.
[0071] The water-based adhesive may contain a crosslinking agent. Any known crosslinking agent may be used as the crosslinking agent. Examples of such crosslinking agents include water-soluble epoxy compounds, dialdehydes, and isocyanates.
[0072] When the PVA-based resin is an acetoacetyl group-containing PVA-based resin, the crosslinking agent is preferably any one of glyoxal, glyoxylate, and methylolmelamine, more preferably any one of glyoxal and glyoxylate, and particularly preferably glyoxal.
[0073] The water-based adhesive may also contain an organic solvent. The organic solvent is preferably an alcohol in that it is miscible with water, and among alcohols, methanol or ethanol is more preferable. Some urea compounds have low solubility in water, but some have sufficient solubility in alcohol. In this case, one of the preferred embodiments is to dissolve the urea compound in alcohol to prepare an alcohol solution of the urea compound, and then add the alcohol solution of the urea compound to the aqueous PVA solution to prepare the adhesive.
[0074] The methanol concentration of the water-based adhesive is preferably 10% by mass or more and 70% by mass or less, more preferably 15% by mass or more and 60% by mass or less, and even more preferably 20% by mass or more and 60% by mass or less. By making the methanol concentration 10% by mass or more, it becomes easier to suppress polyenation in a high-temperature environment. In addition, by making the methanol content 70% by mass or less, it is possible to suppress deterioration of the hue.
[0075] (Active energy ray curing adhesive) The active energy ray curable adhesive is an adhesive that is cured by irradiation with active energy rays such as ultraviolet rays, and examples thereof include an adhesive containing a polymerizable compound and a photopolymerization initiator, an adhesive containing a photoreactive resin, and an adhesive containing a binder resin and a photoreactive crosslinking agent. Examples of the polymerizable compound include photopolymerizable monomers such as photocurable epoxy monomers, photocurable acrylic monomers, and photocurable urethane monomers, and oligomers derived from these monomers. Examples of the photopolymerization initiator include a compound containing a substance that generates active species such as neutral radicals, anion radicals, and cation radicals when irradiated with active energy rays such as ultraviolet rays.
[0076] (Urea-based compounds) When the adhesive layer contains a urea-based compound, the urea-based compound is at least one selected from urea, urea derivatives, thiourea, and thiourea derivatives. As a method for incorporating a urea-based compound into the adhesive layer, it is preferable to incorporate a urea-based compound into the above-mentioned adhesive. In addition, in the process of forming the adhesive layer through a drying process from the adhesive, a part of the urea-based compound may move from the adhesive layer to the polarizing element, etc. That is, the polarizing element may contain a urea-based compound. There are water-soluble and poorly water-soluble urea-based compounds, and both urea-based compounds can be used in the adhesive of this embodiment. When a poorly water-soluble urea-based compound is used in a water-based adhesive, it is preferable to devise a dispersion method so that haze increase does not occur after the adhesive layer is formed.
[0077] When the adhesive is an aqueous adhesive containing a PVA resin, the amount of the urea compound added is preferably 0.1 to 400 parts by mass, more preferably 1 to 200 parts by mass, and even more preferably 3 to 100 parts by mass, per 100 parts by mass of the PVA resin.
[0078] (urea derivative) A urea derivative is a compound in which at least one of the four hydrogen atoms of a urea molecule is substituted with a substituent. In this case, the substituent is not particularly limited, but is preferably a substituent consisting of a carbon atom, a hydrogen atom, and an oxygen atom.
[0079] Specific examples of urea derivatives include mono-substituted ureas such as methylurea, ethylurea, propylurea, butylurea, isobutylurea, N-octadecylurea, 2-hydroxyethylurea, hydroxyurea, acetylurea, allylurea, 2-propynylurea, cyclohexylurea, phenylurea, 3-hydroxyphenylurea, (4-methoxyphenyl)urea, benzylurea, benzoylurea, o-tolylurea, and p-tolylurea. Disubstituted ureas include 1,1-dimethylurea, 1,3-dimethylurea, 1,1-diethylurea, 1,3-diethylurea, 1,3-bis(hydroxymethyl)urea, 1,3-tert-butylurea, 1,3-dicyclohexylurea, 1,3-diphenylurea, 1,3-bis(4-methoxyphenyl)urea, 1-acetyl-3-methylurea, 2-imidazolidinone (ethylene urea), and tetrahydro-2-pyrimidinone (propylene urea). Examples of 4-substituted ureas include tetramethylurea, 1,1,3,3-tetraethylurea, 1,1,3,3-tetrabutylurea, 1,3-dimethoxy-1,3-dimethylurea, 1,3-dimethyl-2-imidazolidinone, and 1,3-dimethyl-3,4,5,6-tetrahydro-2(1H)-pyrimidinone.
[0080] (Thiourea derivatives) A thiourea derivative is a compound in which at least one of the four hydrogen atoms of a thiourea molecule is substituted with a substituent. In this case, the substituent is not particularly limited, but is preferably a substituent consisting of a carbon atom, a hydrogen atom, and an oxygen atom.
[0081] Specific examples of thiourea derivatives include mono-substituted thioureas such as N-methylthiourea, ethylthiourea, propylthiourea, isopropylthiourea, 1-butylthiourea, cyclohexylthiourea, N-acetylthiourea, N-allylthiourea, (2-methoxyethyl)thiourea, N-phenylthiourea, (4-methoxyphenyl)thiourea, N-(2-methoxyphenyl)thiourea, N-(1-naphthyl)thiourea, (2-pyridyl)thiourea, o-tolylthiourea, and p-tolylthiourea. Examples of the disubstituted thiourea include 1,1-dimethylthiourea, 1,3-dimethylthiourea, 1,1-diethylthiourea, 1,3-diethylthiourea, 1,3-dibutylthiourea, 1,3-diisopropylthiourea, 1,3-dicyclohexylthiourea, N,N-diphenylthiourea, N,N'-diphenylthiourea, 1,3-di(o-tolyl)thiourea, 1,3-di(p-tolyl)thiourea, 1-benzyl-3-phenylthiourea, 1-methyl-3-phenylthiourea, N-allyl-N'-(2-hydroxyethyl)thiourea, and ethylenethiourea. An example of the 3-substituted thiourea is trimethylthiourea, and an example of the 4-substituted thiourea is tetramethylthiourea or 1,1,3,3-tetraethylthiourea.
[0082] Among the urea-based compounds, urea derivatives or thiourea derivatives are preferred, and urea derivatives are more preferred, in that they can further suppress the decrease in transmittance in a high-temperature environment when used in an image display device with an interlayer filling configuration. Among the urea derivatives, mono- or di-substituted ureas are preferred, and mono-substituted ureas are more preferred. Di-substituted ureas include 1,1-substituted ureas and 1,3-substituted ureas, and 1,3-substituted ureas are more preferred.
[0083] [Other layers] The polarizing plate may further have other layers, such as an optically functional layer, a pressure-sensitive adhesive layer, and a protective film.
[0084] [Optical functional layer] The optical functional layer can be, for example, a retardation layer. Examples of the retardation layer include a layer that imparts a retardation of λ / 2, a layer that imparts a retardation of λ / 4 (positive A plate), and a positive C plate. The optical functional layer may include an alignment layer and a substrate, or may have two or more liquid crystal layers, alignment layers, and substrates. When the polarizing plate has a polarizing element and a film that imparts a retardation of λ / 4, the polarizing plate can be a circular polarizing plate. The transparent protective film may also function as a retardation layer, but a retardation layer may also be laminated separately from these films. In the latter case, the retardation layer may be laminated on the polarizing plate via a pressure-sensitive adhesive layer or an adhesive layer.
[0085] Examples of the retardation layer include a birefringent film made of a stretched film of a thermoplastic resin having light transmission, and the above-mentioned liquid crystal layer formed on a substrate film. The substrate film is usually a film made of a thermoplastic resin, and an example of the thermoplastic resin is a cellulose ester resin such as triacetyl cellulose.
[0086] Examples of other optical functional layers include a light collecting plate, a brightness enhancing film, a reflective layer (reflective film), a semi-transmissive reflective layer (semi-transmissive reflective film), a light diffusing layer (light diffusing film), and an anti-reflection film.
[0087] [Adhesive layer] The pressure-sensitive adhesive layer can have a function of bonding the polarizing plate to an image display element, an optical member, etc. The pressure-sensitive adhesive layer can be disposed on one of the outermost surfaces of the polarizing plate. Hereinafter, a polarizing plate having a pressure-sensitive adhesive layer is also referred to as a polarizing plate with a pressure-sensitive adhesive layer.
[0088] The adhesive layer can be applied to the polarizing plate by a suitable method, for example, a method of preparing an adhesive solution of about 10 to 40 mass % by dissolving or dispersing a base polymer or its composition in a solvent consisting of a single or mixture of suitable solvents such as toluene and ethyl acetate, and directly applying the solution to the polarizing plate by a suitable spreading method such as a casting method or a coating method, or a method of forming an adhesive layer on a separator and transferring the layer to the polarizing plate.
[0089] As the (meth)acrylic resin (base polymer) used in the pressure-sensitive adhesive composition, a polymer or copolymer containing one or more monomers of (meth)acrylic acid esters such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc. is preferably used. A polar monomer is preferably copolymerized in the base polymer. Examples of the polar monomer include monomers having a carboxyl group, a hydroxyl group, an amide group, an amino group, an epoxy group, etc., such as a (meth)acrylic acid compound, a 2-hydroxypropyl (meth)acrylate compound, a hydroxyethyl (meth)acrylate compound, a (meth)acrylamide compound, an N,N-dimethylaminoethyl (meth)acrylate compound, and a glycidyl (meth)acrylate compound.
[0090] The adhesive composition may contain only the base polymer, but usually further contains a crosslinking agent. Examples of the crosslinking agent include a divalent or higher metal ion that forms a carboxylate metal salt with a carboxyl group, a polyamine compound that forms an amide bond with a carboxyl group, a polyepoxy compound or polyol that forms an ester bond with a carboxyl group, and a polyisocyanate compound that forms an amide bond with a carboxyl group. Among them, a polyisocyanate compound is preferred.
[0091] The active energy ray curable adhesive composition has a property of being cured by irradiation with active energy rays such as ultraviolet rays and electron beams, and has a property of being able to adhere to an adherend such as a film even before irradiation with active energy rays, and is able to adjust the adhesive strength by being cured by irradiation with active energy rays. The active energy ray curable adhesive composition is preferably an ultraviolet ray curable type. The active energy ray curable adhesive composition further contains an active energy ray polymerizable compound in addition to a base polymer and a crosslinking agent. If necessary, a photopolymerization initiator, a photosensitizer, etc. may be contained.
[0092] The pressure-sensitive adhesive composition can contain additives such as microparticles for imparting light scattering properties, beads (resin beads, glass beads, etc.), glass fibers, resins other than the base polymer, tackifiers, fillers (metal powders and other inorganic powders, etc.), antioxidants, UV absorbers, dyes, pigments, colorants, defoamers, corrosion inhibitors, and photopolymerization initiators.
[0093] The adhesive layer can be formed by applying the organic solvent dilution of the adhesive composition on the surface of a substrate film or a polarizing plate and drying it.The substrate film is generally a thermoplastic resin film, and a typical example thereof can be a separate film that has been subjected to a release treatment.The separate film can be, for example, a film made of a resin such as polyethylene terephthalate, polybutylene terephthalate, polycarbonate, or polyarene, and the surface on which the adhesive layer is formed is subjected to a release treatment such as silicone treatment.
[0094] For example, a pressure-sensitive adhesive composition may be directly applied to the release-treated surface of a separate film to form a pressure-sensitive adhesive layer, and this pressure-sensitive adhesive layer with a separate film may be laminated on the surface of a polarizing plate. A pressure-sensitive adhesive composition may be directly applied to the surface of a polarizing plate to form a pressure-sensitive adhesive layer, and a separate film may be laminated on the outer surface of the pressure-sensitive adhesive layer. When providing the pressure-sensitive adhesive layer on the surface of the polarizing plate, it is preferable to subject the bonding surface of the polarizing plate and / or the bonding surface of the pressure-sensitive adhesive layer to a surface activation treatment such as a plasma treatment or corona treatment, and it is more preferable to subject the layer to a corona treatment. Alternatively, a pressure-sensitive adhesive composition may be applied onto a second separate film to form a pressure-sensitive adhesive layer, a separate film may be laminated onto the formed pressure-sensitive adhesive layer to prepare a pressure-sensitive adhesive sheet, and the pressure-sensitive adhesive layer with the separate film after peeling the second separate film from the pressure-sensitive adhesive sheet may be laminated onto a polarizing plate. The second separate film used has a weaker adhesion to the pressure-sensitive adhesive layer than the separate film and is therefore easier to peel off.
[0095] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is, for example, preferably from 1 μm to 100 μm, more preferably from 3 μm to 50 μm, and may be 20 μm or more.
[0096] [Protection film] The polarizing plate may include a protective film for protecting its surface (typically, the surface of a protective film of the polarizing plate). After the polarizing plate is attached to, for example, an image display element or other optical members, the protective film is peeled off and removed together with the pressure-sensitive adhesive layer that the polarizing plate has.
[0097] The protective film is composed of, for example, a base film and an adhesive layer laminated thereon. The adhesive layer is as described above. The resin constituting the base film may be, for example, a thermoplastic resin such as a polyethylene-based resin, such as polyethylene, a polypropylene-based resin, such as polypropylene, a polyester-based resin, such as polyethylene terephthalate or polyethylene naphthalate, or a polycarbonate-based resin. A polyester-based resin, such as polyethylene terephthalate, is preferred.
[0098] The thickness of the protective film is not particularly limited, but is preferably in the range of 20 μm to 200 μm. When the thickness of the substrate is 20 μm or more, the polarizing plate tends to be easily provided with strength.
[0099] [Method of manufacturing polarizing plate] The method for producing a polarizing plate according to the present embodiment includes a lamination step of laminating a polarizing element and a transparent protective film to obtain a laminated film, and a cutting step of cutting the laminated film. The cutting step includes a first cutting step of cutting the laminated film by moving a cutting tool in a spiral shape relative to the main surface of the laminated film obtained by laminating the polarizing element and the transparent protective film in a perpendicular direction.
[0100] [Lamination process] The lamination step can be a step of bonding the polarizing element and the transparent protective film via the adhesive layer.
[0101] [Cutting process] The cutting tool used in the cutting process is not particularly limited as long as it can cut the laminated film, but examples thereof include a cutting tool having a rotatable handle and an outer peripheral blade, the outer peripheral blade being integrated with the handle. A cutting tool having a rotatable handle, an outer peripheral blade, and a bottom blade, the outer peripheral blade and the bottom blade being integrated with the handle, may also be used. The outer peripheral blade and the bottom blade may be integrated. Examples of such cutting tools include end mills.
[0102] The number of peripheral cutting edges and bottom cutting edges of the cutting tool is not particularly limited, but may be, for example, 1 to 6, and may be 2, 3, or 4. If the number of edges is small, shavings tend to be discharged more easily, but the rigidity of the cutting tool tends to decrease.
[0103] The rake angle of the peripheral cutting edge and the bottom cutting edge of the cutting tool is usually 0° or more and less than 20°, and may be 3° or more and less than 15°. If the rake angle is too large, the cutting edge tends to chip easily.
[0104] The clearance angle of the peripheral cutting edge and the bottom cutting edge of the cutting tool is, for example, greater than 0° and less than 20°, and may be between 3° and 15°. If the clearance angle is 0°, the laminated film and the blade will rub against each other, and if the clearance angle is too large, the blade will tend to chip easily.
[0105] The peripheral cutting edge may be twisted along the handle. The twist angle of the peripheral cutting edge of the cutting tool may be from -75° to 75°, or from -65° to 65°. If the twist angle is too large, it tends to be difficult to discharge shavings.
[0106] The peripheral cutting edge of the cutting tool preferably constitutes the maximum diameter of the rotating part of the cutting tool. The diameter of the peripheral cutting edge of the cutting tool (the maximum diameter in the direction perpendicular to the handle) is, for example, 1.0 mm to 10 mm, and preferably 1.5 mm to 8 mm. If the diameter is too small, the end mill tends to break easily, and if it is too large, fine cutting becomes difficult.
[0107] The feed speed of the cutting tool is usually 50 mm / min or more and 30,000 mm / min or less, may be 100 mm / min or more, and is preferably 200 mm / min or more and 20,000 mm / min or less.
[0108] The rotation speed of the peripheral blade and bottom blade of the end mill may be 5000 rpm or more and 100000 rpm or less, 10000 rpm or more and 80000 rpm or less, or 30000 rpm or more and 60000 rpm or less. If the rotation speed is too slow, delamination of the laminated film tends to occur easily, and if the rotation speed is too fast, heat may be generated, damaging the laminated film.
[0109] [1st cutting process] In the first cutting step, for example, as shown in FIG. 4(A), a cutting tool is moved relatively in a spiral shape when viewed from a direction perpendicular to the main surface of the laminate film, thereby cutting the laminate film.
[0110] A spiral refers to a curve that rotates while moving away from the outside. Examples of the spiral include a spiral with equal intervals between the spirals, i.e., a spiral pitch (Archimedes' spiral, etc.), a spiral with a wider spiral pitch toward the outside (logarithmic spiral, etc.), and a spiral with a narrower spiral pitch toward the outside (parabolic spiral, etc.). A spiral with equal intervals between the spirals may be a spiral whose radius increases at regular intervals (e.g., half a revolution, 1 / 4 revolution, etc.) less than one revolution. In a part of one revolution of the spiral, the spiral pitch may be zero, that is, there may be a part that is not cut from the part that has already been cut. The operation of moving the cutting tool relatively in a spiral shape is an operation of moving the cutting tool relatively outside by the spiral pitch width in at least a part of the cut part that has already been cut. As a result, the laminated film on the outside is cut by the spiral pitch width in at least a part of the cut part that has already been cut.
[0111] The spiral in the first cutting step may be one or more revolutions, and preferably, when cutting the laminated film, at least the outermost periphery is cut by a spiral relative movement.
[0112] When the laminate film is cut by moving the cutting tool in a spiral motion when viewed perpendicular to the main surface of the laminate film, delamination of the laminate film can be suppressed compared to cutting by relative movement that combines linear and circular motion (such as (B) in Figure 4). Furthermore, cutting by moving the tool in a spiral motion can shorten the time it takes to form a cut portion of the desired size.
[0113] The shape of the cut portion formed by the first cutting step has curved and straight portions. For example, when cutting the laminated film into the shape shown in Fig. 1(a), the cutting tool can be moved relatively to form curved and straight portions continuously while changing the spiral pitch in one revolution, and the cutting tool can be moved relatively to form a spiral shape while increasing the radius from the center. In Fig. 2, the direction of relative movement of the cutting tool when forming straight portions 2a and 2c, which are straight portions substantially parallel to the transmission axis of the polarizing element, can be substantially parallel to the transmission axis of the polarizing element.
[0114] In the first cutting step, the laminate film is cut by contacting the peripheral blade of the cutting tool with the laminate film. When the cutting tool has a rotatable handle, the rotatable handle may be perpendicular or inclined to the main surface of the laminate film, but the cutting tool is preferably moved relative to the main surface of the laminate film in a perpendicular state. As a result, the cut surface is perpendicular to the main surface of the laminate film.
[0115] In the first cutting step, the operation of moving the cutting tool relative to the laminate film is usually performed in a direction parallel to the main surface of the laminate film. This operation may further include movement perpendicular to the main surface of the laminate film. When movement perpendicular to the main surface of the laminate film is involved, for example, an operation of moving the cutting tool relative to the laminate film in a spiral shape may be mentioned. The cutting performed by moving the cutting tool relative to the laminate film in a spiral shape may also serve as the formation of a through hole, which will be described later.
[0116] In the first cutting step, the spiral pitch is, for example, 0.01 mm or more and 0.5 mm or less, preferably 0.02 mm or more and 0.3 mm or less, and more preferably 0.03 mm or more and 0.2 mm or less. When the spiral pitch is within the above range, the laminate film can be cut to the desired size without excessive time. However, if the spiral pitch is too large, the cut laminate film tends to be more likely to have defects.
[0117] In the first cutting step, the laminate film may be cut one by one, or a laminate of multiple laminate films may be cut. In the first cutting step, when multiple laminate films are cut, each laminate film constituting the laminate can be cut by moving a cutting tool relatively in a spiral shape when viewed from a direction perpendicular to the main surface of the laminate. The number of laminate films constituting the laminate may be, for example, 10 to 500. The thickness of the laminate may be, for example, 1 mm to 50 mm in the stacking direction of the laminate films.
[0118] [Through hole formation process] The manufacturing method of the present invention preferably further includes a through hole forming step of forming a through hole that penetrates the laminated film in a direction perpendicular to the main surface. The through hole forming step and the below-mentioned arrangement step are usually performed before the first cutting step. The size of the through hole is equal to or larger than the maximum diameter perpendicular to the handle of the cutting tool so that the cutting tool can be arranged in the through hole.
[0119] The through hole is preferably formed by moving the cutting tool relative to the main surface of the laminate film in a direction perpendicular to the main surface of the laminate film. For example, when the cutting tool has a rotatable handle and a bottom blade integrated therewith, the cutting tool is moved relative to the main surface of the laminate film in a direction perpendicular to the main surface of the laminate film, so that the bottom blade cuts the laminate film and a through hole having the same diameter as the maximum diameter perpendicular to the handle of the cutting tool can be formed. In the through hole forming step, the operation of moving the cutting tool relative to the main surface of the laminate film in a direction parallel to the main surface of the laminate film may be performed simultaneously or independently with the relative movement in a direction perpendicular to the main surface of the laminate film. This operation can form a through hole larger than the maximum diameter perpendicular to the handle of the cutting tool. The operation of moving the cutting tool relative to the main surface of the laminate film in a direction parallel to the main surface of the laminate film includes an operation of moving the cutting tool in a circular motion, an operation of moving the cutting tool linearly, etc., when viewed from a direction perpendicular to the main surface of the laminate film.
[0120] A plurality of laminate films may be stacked to form a laminate, and the through hole forming step may be performed. In the through hole forming step, a cutting tool is moved relative to the main surface of the laminate in a direction perpendicular to the laminate, thereby forming a through hole in each laminate film constituting the laminate. When the through hole forming step is performed using the laminate film as the laminate, the subsequent arrangement step and first cutting step may be performed on the laminate in which the through hole is formed.
[0121] The through-holes can also be formed by known methods such as punching, laser, etc. The through-holes formed by the above methods are preferably larger than the maximum diameter perpendicular to the shank of the cutting tool.
[0122] [Placement process] The manufacturing method of the present invention preferably further includes a step of arranging a cutting tool so as to penetrate the through hole. The cutting tool may be arranged so as to penetrate the through hole and have a peripheral cutting edge contacting the inside of the through hole. Specifically, after the through hole is formed, the cutting tool may be arranged so as to penetrate the through hole.
[0123] When the through hole is formed by using a cutting tool, the cutting tool can be positioned so as to penetrate the through hole by not removing the cutting tool that has been moved relative to the main surface of the laminated film in a direction perpendicular to the main surface of the laminated film. After the through hole is formed by moving the cutting tool relative to the main surface of the laminated film in a direction perpendicular to the main surface of the laminated film, the cutting tool may be removed from the through hole in a perpendicular direction to remove grinding debris, and the cutting tool may be placed again in the through hole.
[0124] A plurality of laminate films may be stacked to form a laminate, and the arrangement step may be performed. At this time, a cutting tool is placed so as to penetrate the through holes formed in each laminate film constituting the laminate. When the arrangement step is performed on the laminate, the first cutting step may be performed on the laminate as it is.
[0125] [Polishing process] It is preferable that the manufacturing method of the present invention further includes a polishing step of polishing the cut portion formed in the first cutting step or the second cutting step described below.
[0126] A plurality of laminate films may be stacked to form a laminate, and the polishing step may be carried out. In the polishing step, the laminate is polished to polish the cut portions of each laminate film constituting the laminate. After the first cutting step or the second cutting step is carried out on the laminate, the laminate may be polished as it is.
[0127] The polishing method is not particularly limited as long as it can smooth the cut surface, and examples thereof include polishing methods using abrasive paper (sandpaper), abrasive cloth, fine abrasive, grindstone, etc., electric polishing methods, and chemical polishing methods using solvents. The cut surface may be polished using a cutting tool such as an end mill used in the first cutting step by slowing down the feed rate, reducing the amount of polishing, or both. In addition, polishing can also remove dirt, dust, etc. that has been present in previous steps.
[0128] [Second cutting process] The manufacturing method of the present invention may further include a second cutting step in which the laminate film obtained in the first cutting step is further cut by relatively moving a cutting tool in a direction parallel to the main surface of the laminate film.
[0129] A plurality of laminate films may be stacked to form a laminate, and the second cutting step may be performed. In the second cutting step, the laminate films constituting the laminate are further cut by moving a cutting tool relatively in a direction parallel to the main surface of the laminate. The first cutting step may be performed on the laminate, and then the second cutting step may be performed on the laminate as is.
[0130] By continuing the second cutting step from the cut portion formed in the first cutting step, a polarizing plate cut into a desired shape can be obtained.
[0131] <Image display device> The polarizing plate of the present embodiment is used in various image display devices such as liquid crystal display devices and organic EL display devices. An example of the image display device is a configuration having an image display cell, a first adhesive layer laminated on the viewing side surface of the image display cell, and a polarizing plate laminated on the viewing side surface of the first adhesive layer. Such an image display device may further have a second adhesive layer laminated on the viewing side surface of the polarizing plate and a transparent member laminated on the surface of the second adhesive layer. In particular, the polarizing plate of the present embodiment is suitably used in an image display device having an interlayer filling configuration in which a transparent member is arranged on the viewing side of the image display device, the polarizing plate and the image display cell are bonded together by the first adhesive layer, and the polarizing plate and the transparent member are bonded together by the second adhesive layer. In this specification, either one or both of the first adhesive layer and the second adhesive layer may be simply referred to as an "adhesive layer". Note that the member used to bond the polarizing plate and the image display cell and the member used to bond the polarizing plate and the transparent member are not limited to an adhesive layer and may be an adhesive layer.
[0132] [Image display cell] Examples of the image display cell include a liquid crystal cell and an organic EL cell. The liquid crystal cell may be a reflective liquid crystal cell that uses external light, a transmissive liquid crystal cell that uses light from a light source such as a backlight, or a semi-transmissive semi-reflective liquid crystal cell that uses both external light and light from a light source. When the liquid crystal cell uses light from a light source, the image display device (liquid crystal display device) has a polarizing plate disposed on the opposite side to the viewing side of the image display cell (liquid crystal cell), and further has a light source disposed thereon. The polarizing plate on the light source side and the liquid crystal cell are preferably bonded together via an appropriate adhesive layer. The driving method of the liquid crystal cell may be any type, such as VA mode, IPS mode, TN mode, STN mode, or bend orientation (π type).
[0133] As the organic EL cell, a light-emitting body (organic electroluminescence light-emitting body) is preferably formed by sequentially laminating a transparent electrode, an organic light-emitting layer, and a metal electrode on a transparent substrate. The organic light-emitting layer is a laminate of various organic thin films, and various layer configurations can be adopted, such as a laminate of a hole injection layer made of a triphenylamine derivative or the like and a light-emitting layer made of a fluorescent organic solid such as anthracene, a laminate of these light-emitting layers and an electron injection layer made of a perylene derivative or the like, or a laminate of a hole injection layer, a light-emitting layer, and an electron injection layer.
[0134] [Laminating the image display cell and polarizing plate] A pressure-sensitive adhesive layer (pressure-sensitive adhesive sheet) is preferably used for bonding the image display cell and the polarizing plate. Among them, a method of bonding the above-mentioned polarizing plate with the pressure-sensitive adhesive layer to the image display cell is preferred from the viewpoint of workability, etc. A pressure-sensitive adhesive layer can also be formed by applying a diluted solution of the above-mentioned pressure-sensitive adhesive composition to the image display cell in an organic solvent, and then the pressure-sensitive adhesive layer can be bonded to the polarizing plate.
[0135] [Transparent material] Examples of the transparent member arranged on the viewing side of the image display device include a front plate (window layer) and a touch panel. The front plate has appropriate mechanical strength and thickness. Examples of such a front plate include transparent resin plates such as polyimide resin, acrylic resin, and polycarbonate resin, and glass plates. A functional layer such as an anti-reflection layer may be laminated on the viewing side of the front plate. In addition, when the front plate is a transparent resin plate, a hard coat layer may be laminated to increase physical strength, or a low moisture permeable layer may be laminated to reduce moisture permeability. As the touch panel, various touch panels such as resistive, capacitive, optical, and ultrasonic touch panels, as well as glass or transparent resin panels having a touch sensor function are used. When a capacitive touch panel is used as the transparent member, it is preferable that a front panel made of glass or transparent resin plate is provided on the viewing side further than the touch panel.
[0136] [Bonding a polarizing plate and a transparent material] A pressure sensitive adhesive or an active energy ray curable adhesive is preferably used for bonding the polarizing plate and the transparent member. When a pressure sensitive adhesive is used, the pressure sensitive adhesive can be applied by an appropriate method. As a specific application method, for example, the application method of the pressure sensitive adhesive layer used for bonding the image display cell and the polarizing plate described above can be mentioned.
[0137] When an active energy ray curable adhesive is used, a method is preferably used in which a dam material is provided around the periphery of the image display panel in order to prevent the adhesive solution from spreading before curing, a transparent member is placed on the dam material, and the adhesive solution is then poured in. After the adhesive solution is poured, alignment and degassing are performed as necessary, and then the adhesive solution is irradiated with active energy rays to cause curing. EXAMPLES
[0138] The present invention will be specifically described below based on examples. The materials, reagents, amounts of substances and their ratios, operations, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the present invention is not limited to the following examples.
[0139] (1) Measurement of the thickness of the polarizing element: The measurements were made using a digital micrometer "MH-15M" manufactured by Nikon Corporation.
[0140] (2) Measurement of boron content: 0.2 g of the polarizing element was dissolved in 200 g of a 1.9% by mass aqueous mannitol solution. The resulting aqueous solution was then titrated with a 1 mol / L aqueous sodium hydroxide solution, and the boron content of the polarizing element was calculated by comparing the amount of the aqueous sodium hydroxide solution required for neutralization with a calibration curve.
[0141] (3) Measurement of boron adsorption rate of PVA resin film: A PVA-based resin film cut into a 100 mm square was immersed in pure water at 30°C for 60 seconds, and then immersed in an aqueous solution containing 5 parts of boric acid at 60°C for 120 seconds. The PVA-based resin film removed from the aqueous solution of boric acid was dried in an oven at 80°C for 11 minutes. 23°C 55%%RH The film was then conditioned for 24 hours in an environment at 100° C. to obtain a boron-containing PVA film. 0.2 g of the boron-containing PVA resin film thus obtained was dissolved in 200 g of a 1.9% by mass aqueous solution of mannitol. The aqueous solution thus obtained was then titrated with a 1 mol / L aqueous solution of sodium hydroxide, and the boron content of the PVA resin film was calculated by comparing the amount of the aqueous sodium hydroxide solution required for neutralization with a calibration curve. The boron content of the PVA resin film thus obtained was used as the boron adsorption rate of the PVA resin film.
[0142] (4) Measurement of luminosity-corrected single transmittance, luminosity-corrected polarization degree and hue of a polarizing plate: Measurements were made using a spectrophotometer with an integrating sphere ("V7100" manufactured by JASCO Corporation, 2-degree field of view; C light source).
[0143] (Preparation of Polarizing Element 1) A 30 μm thick polyvinyl alcohol resin film with a boron adsorption rate of 5.71% by mass was immersed in pure water at 21.5° C. for 79 seconds (swelling treatment), and then immersed in an aqueous solution containing 1.0 mM iodine and having a mass ratio of potassium iodide / boric acid / water of 2 / 2 / 100 at 23° C. for 151 seconds (dyeing process). Thereafter, the film was immersed in an aqueous solution containing 1.0 mM iodine and having a mass ratio of potassium iodide / boric acid / water of 2.5 / 4 / 100 at 62.8° C. for 76 seconds (first crosslinking process). Subsequently, the film was immersed in an aqueous solution containing 1.0 mM iodine and having a mass ratio of potassium iodide / boric acid / zinc chloride / water of 3 / 5.5 / 0.6 / 100 at 45° C. for 11 seconds (second crosslinking process, metal ion treatment process). The film was then immersed in a cleaning bath for cleaning (cleaning step) and dried at 38°C (drying step) to obtain a 12μm thick polarizing element in which iodine was adsorbed and aligned in the polyvinyl alcohol. Stretching was mainly performed in the dyeing step and the first crosslinking step, and the total stretching ratio was 5.85 times. The zinc ion content of the obtained polarizing element was 0.07% by mass, and the boron content was 4.48% by mass.
[0144] (Preparation of Polarizing Element 2) A 30 μm thick polyvinyl alcohol resin film with a boron adsorption rate of 5.71% by mass was immersed in pure water at 21.5° C. for 79 seconds (swelling treatment), and then immersed in an aqueous solution containing 1.0 mM iodine and having a mass ratio of potassium iodide / boric acid / water of 2 / 2 / 100 at 23° C. for 151 seconds (dyeing process). Thereafter, the film was immersed in an aqueous solution containing 1.0 mM iodine and having a mass ratio of potassium iodide / boric acid / water of 2.5 / 4 / 100 at 62.8° C. for 76 seconds (first crosslinking process). Subsequently, the film was immersed in an aqueous solution containing 1.0 mM iodine and having a mass ratio of potassium iodide / boric acid / zinc chloride / water of 3 / 3.5 / 0.6 / 100 at 45° C. for 11 seconds (second crosslinking process, metal ion treatment process). The film was then immersed in a cleaning bath for cleaning (cleaning step) and dried at 38°C (drying step) to obtain a 12μm thick polarizing element in which iodine was adsorbed and aligned in the polyvinyl alcohol. Stretching was mainly performed in the dyeing step and the first crosslinking step, and the total stretching ratio was 5.85 times. The zinc ion content of the obtained polarizing element was 0.14% by mass, and the boron content was 3.91% by mass.
[0145] (Preparation of PVA solution for adhesive) 50 g of modified PVA resin containing acetoacetyl groups (Mitsubishi Chemical Corporation: Gohsenex Z-410) was dissolved in 950 g of pure water, heated at 90° C. for 2 hours, and then cooled to room temperature to obtain a PVA solution for adhesive.
[0146] (Preparation of Polarizing Plate Adhesive 1) The prepared PVA solution for adhesive, pure water, and methanol were mixed so that the PVA concentration was 3.0%, the methanol concentration was 35%, and the urea concentration was 0.5%, to obtain an adhesive 1 for polarizing plates.
[0147] (Saponification of Cellulose Acylate Film) A commercially available cellulose acylate film TJ40UL (manufactured by Fujifilm Corporation: film thickness 40 μm) was immersed in a 1.5 mol / L NaOH aqueous solution (saponification solution) kept at 55° C. for 2 minutes, and then the film was washed with water. Thereafter, the film was immersed in a 0.05 mol / L sulfuric acid aqueous solution at 25° C. for 30 seconds, and then passed through a water washing bath under running water for 30 seconds to neutralize the film. Then, the film was repeatedly drained three times with an air knife, and after removing the water, it was allowed to stay in a drying zone at 70° C. for 15 seconds and dried to produce a saponified film.
[0148] (Preparation of Laminated Film 1) The saponified cellulose acylate film prepared above was attached to both sides of the polarizing element 1 via the polarizing plate adhesive 1, and the thickness of the adhesive layer after drying was adjusted to 100 nm on both sides, and the films were laminated using a roll laminator and then dried at 80° C. for 3 minutes to obtain a polarizing plate 1 with cellulose acylate films on both sides. A surface protective film (a peelable film having an adhesive layer formed on one side of a polyethylene terephthalate film: thickness 57 μm) was laminated to one side of the polarizing plate 1 thus prepared.
[0149] Next, an acrylic adhesive (manufacturer: Lintec Corporation) was applied onto a release film (a release-treated polyethylene terephthalate film: thickness 38 μm) to form an adhesive layer. An adhesive layer was laminated on the surface opposite to the surface protective film of the polarizing plate 1 prepared above, to prepare a laminate film 1 provided with peelable protective films on both sides.
[0150] Except for changing the polarizing element 1 of the laminated film 1 to a polarizing element 2, a laminated film 2 having peelable protective films on both sides was prepared in the same manner.
[0151] Example 1 The laminate film 1 was cut into a rectangle of 296.2 mm×114 mm [diagonal length: approximately 317.4 mm (approximately 12.5 inches)] with the long side parallel to the absorption axis of the polarizing element.
[0152] Thirty sheets of the cut laminated film 1 were laminated to form a laminate. An end mill with a diameter of 2 mm and two blades was used for cutting. First, the end mill was moved in a direction perpendicular to the surface of the laminate, a through hole was formed with the bottom blade of the end mill, and the end mill was positioned so as to penetrate the through hole. Then, the laminated film was cut to form a hole with a straight line portion of 0.5 mm and a curvature radius of 1 mm at the four corners. The shape of the hole was composed of four straight lines with a length of 0.5 mm and four curved lines with a curvature radius of 1 mm, and one pair of opposing straight lines among the four straight lines was parallel to the transmission axis of the polarizing element, and the other pair of opposing straight lines was parallel to the absorption axis of the polarizing element. At this time, cutting was performed while performing an operation in which the rotatable handle of the end mill was perpendicular to the main surface of the laminated film and the end mill was relatively moved in a direction parallel to the main surface of the laminated film. The feed speed of the end mill was 15,000 mm / min and the rotation speed was 30,000 rpm. The center position of the hole was formed at a position 47.96 mm from the long side end and 56.92 mm from the short side end.
[0153] (Examples 2 to 4, Comparative Examples 1 to 11) Holes were drilled (cutting) in the same manner as in Example 1, except that the type of laminated film and the shape of the holes were changed as shown in Table 1. In Comparative Examples 1 to 3 and 8 to 10, the shape of the holes was circular without any straight line portions, and the radius of curvature of the circles is shown in the column for the radius of curvature of the four corners of the hole in Table 1. The results are shown in Table 1.
[0154] (Heat shock test) The polarizing plate with holes was attached to a non-alkali glass plate via an adhesive layer. The polarizing plate was then subjected to a heat shock test of 300 cycles, with one cycle consisting of 30 minutes at a low temperature of -40°C and 30 minutes at a high temperature of 85°C. After the test, the polarizing plate was removed and the size of the cracks around the holes was measured under a microscope. In the table, a crack size of 0.0 mm means that no cracks were observed after the test.
[0155] (Preparation of Laminated Film 3) The surface protective film of the laminated film 1 was peeled off. An acrylic adhesive (manufacturer: Lintec Corporation) was applied onto a release film (a release-treated polyethylene terephthalate film: thickness 38 μm) to form an adhesive layer. The adhesive layer was attached to the surface exposed by peeling off the surface protective film, to produce laminated film 3.
[0156] (Preparation of Laminated Film 4) Laminated film 4 was produced in the same manner as laminated film 3, except that polarizing element 1 was changed to polarizing element 2.
[0157] (High temperature durability test (105℃)) The laminated films 3 and 4 prepared above were each cut to a size of 40 mm x 40 mm. The release films on both sides were peeled off, and the surfaces of the adhesive layers were attached to alkali-free glass (trade name "EAGLE XG", Corning Incorporated) to prepare evaluation samples. When preparing these samples, the optical laminate was stored for 72 hours in an environment of a temperature of 20°C and a relative humidity of 40% in order to adjust the moisture content of the polarizing element before laminating the glass plate. For all samples, the mass was measured after 66 hours, 69 hours, and 72 hours of storage, and since there was no change, it was considered that each layer including the polarizing element had reached an equilibrium moisture content at a temperature of 20°C and a relative humidity of 40%.
[0158] This evaluation sample was subjected to a temperature of 50°C and a pressure of 5kgf / cm 2 (490.3 kPa) for 1 hour, and then left in an environment with a temperature of 23°C and a relative humidity of 55% for 24 hours. The initial values of the luminous-corrected polarization degree, luminous-corrected single transmittance, and hue of the polarizing plate were measured, and then the plate was stored in a high-temperature environment at a temperature of 115°C for 48 hours. After storage, the luminous-corrected polarization degree, luminous-corrected single transmittance, and hue of the polarizing plate were measured, and the amount of change from the initial value for each was calculated.
[0159] The change in luminosity-corrected single transmittance of laminate film 3 was −1.3%, the change in luminosity-corrected polarization degree was −0.18%, and the change in hue was 6.4 NBS.
[0160] The change in luminosity-corrected single transmittance of laminate film 4 was −6.8%, the change in luminosity-corrected polarization degree was −0.50%, and the change in hue was 15.4 NBS.
[0161] [Table 1]
[0162] As shown in Table 1, the polarizing plates obtained in Examples 1 to 4 did not crack in the hole in the thermal shock test, even though the polarizing element 1 having high high-temperature durability was used. On the other hand, the polarizing element 2 used in the polarizing plates obtained in Comparative Examples 1 to 3 had low high-temperature durability, and cracks were observed in the hole in the thermal shock test. The polarizing plates obtained in Comparative Examples 4 to 7 did not crack in the hole in the thermal shock test, but the polarizing element 2 used had low high-temperature durability. Furthermore, the polarizing plates obtained in Comparative Examples 8 to 11 used the polarizing element 1 having high high-temperature durability, but cracks were observed in the hole in the thermal shock test. It is understood that according to the present invention, a polarizing plate in which cracks are not generated in the hole in the thermal shock test can be obtained even when a polarizing element having high high-temperature durability is used. [Explanation of symbols]
[0163] 1 polarizing plate, 2 hole portion, 2a, 2b, 2c, 2d straight portion, 10 polarizing plate, 11 polarizing element, 12 transparent protective film, f1, f2, f3, f4 straight line
Claims
1. a polarizing element having a dichroic dye adsorbed and oriented in a polyvinyl alcohol-based resin layer; A transparent protective film; A process of bonding the above-mentioned through an adhesive layer. A method for producing a polarizing plate comprising the steps of: the polyvinyl alcohol-based resin layer is formed from a polyvinyl alcohol resin having a boron adsorption rate of 5.70% by mass or more; The polarizing element has a boron content of 4.0% by mass or more and 8.0% by mass or less, the polarizing plate has at least one hole in a plane in a plan view, The shape of the hole satisfies both of the following conditions (1a) and (1b): (1a) The shape of the hole has two straight line portions that are approximately parallel to the transmission axis of the polarizing element, and the length of the straight line portions that are approximately parallel to the transmission axis of the polarizing element is 10 mm or less. (1b) The shape of the hole has at least two curved portions, and the radius of curvature of the curved portions is 0.5 mm or more and less than 11 mm.
2. The method for producing a polarizing plate according to claim 1 , wherein the shape of the hole further satisfies the following condition (1c): (1c) The polarizing element further has two linear portions approximately parallel to the absorption axis.
3. The method for producing a polarizing plate according to claim 1 , wherein the polarizing plate has a rectangular shape in a plan view and a diagonal length of 6 inches or more.
4. A method for manufacturing an image display device having a polarizing plate, comprising: A method for producing an image display device, comprising the steps of: producing the polarizing plate by the method for producing a polarizing plate according to any one of claims 1 to 3.
Citation Information
Patent Citations
Polarizer, polarizing plate and production method of the polarizer
JP2016206641A
Polarizing film and polarizing plate including the same
JP2017003954A
Polarizing film, polarizing film with adhesive layer, and image display device
JP2019219527A
Polarizing film, polarizing film with adhesive layer, and image display device
JP2019219528A
Polarizing plate
JP2020101574A