Airbag storage cover
A thermoplastic elastomer composition with propylene, ethylene, and partially hydrogenated styrene-conjugated diene block copolymers addresses the issue of insufficient low-temperature and heat resistance in airbag storage covers, ensuring effective performance under demanding conditions.
Patent Information
- Application Number
- JP2021005063
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-15
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-01-15
AI Technical Summary
Conventional thermoplastic elastomer compositions used in airbag storage covers exhibit insufficient low-temperature impact resistance and heat resistance after a heat resistance test, limiting their effectiveness in larger airbags that require higher deployment forces.
A thermoplastic elastomer composition comprising propylene polymer, ethylene copolymer, and partially hydrogenated styrene-conjugated diene block copolymer, in specific ratios, to enhance both low-temperature impact resistance and heat resistance.
The composition achieves excellent low-temperature impact resistance and maintains this performance even after a heat resistance test, making it suitable for airbag storage covers that require high deployment forces.
Smart Images

Figure 0007571559000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic elastomer composition having excellent low-temperature impact resistance and heat resistance, a molded article made of said thermoplastic elastomer composition, and an airbag storage cover made of said thermoplastic elastomer composition. [Background technology]
[0002] An automobile airbag system protects the driver and passengers in the event of a collision, and is made up of a device that detects the impact of the collision and an airbag device. The airbag device is installed in the steering wheel, the instrument panel in front of the passenger seat, the driver's and passenger's seats, the front and side pillars, etc.
[0003] Regarding the airbag storage cover of an airbag device, various proposals have been made regarding the structure and material thereof so that the cover will tear as designed when the airbag inflates.
[0004] For example, Patent Document 1 proposes a thermoplastic elastomer for airbag storage covers that has excellent high-temperature strength, low-temperature impact resistance, mold releasability, injection moldability, etc., and that is made of a styrene-conjugated diene block copolymer such as a styrene-butadiene-styrene block copolymer, a propylene-based resin, and an ethylene-α-olefin copolymer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-38925 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, airbags have become larger from the viewpoint of safety, while airbag devices are required to be smaller from the viewpoint of aesthetics. Therefore, the relative force acting on the airbag storage cover when the airbag is deployed is increasing, and better low-temperature impact resistance is required. The thermoplastic elastomer composition described in Patent Document 1 has excellent low-temperature impact resistance, but in order to evaluate the low-temperature impact resistance after a heat resistance test, the composition was subjected to a heat resistance test in which the composition was heated at 110°C for 1000 hours, and then the IZOD impact strength was measured at a temperature of -45°C. As shown in Comparative Example 2 below, the heat resistance was insufficient, and there was room for improvement in this respect.
[0007] An object of the present invention is to solve the above-mentioned problems associated with conventional products and to provide a thermoplastic elastomer composition having excellent low-temperature impact resistance and heat resistance, and an airbag storage cover made of the same. [Means for solving the problem]
[0008] Means for Solving the Problems The present inventors have conducted intensive studies to solve the above problems, and have found that a thermoplastic elastomer composition containing a specific amount of a propylene-based polymer, an ethylene-based copolymer, preferably an ethylene-based copolymer containing a polymer block consisting of ethylene and an ethylene-α-olefin copolymer block, and a partially hydrogenated styrene-conjugated diene block copolymer has excellent low-temperature impact resistance and heat resistance and can be suitably used for an airbag storage cover, thereby completing the present invention.
[0009] That is, the gist of the present invention lies in the following [1] to [7].
[0010] [1] A thermoplastic elastomer composition comprising the following components (A) to (C), in a ratio of 11 to 68 parts by mass of component (B) and 1 to 58 parts by mass of component (C) per 100 parts by mass of component (A): Component (A): Propylene-based polymer Component (B): Ethylene-based copolymer Component (C): Partially hydrogenated styrene-conjugated diene block copolymer
[0011] [2] The thermoplastic elastomer composition according to [1], wherein the component (A) is a propylene-based block copolymer.
[0012] [3] The thermoplastic elastomer composition according to [1] or [2], wherein the content of the component (C) is lower than the content of the component (B).
[0013] [4] A thermoplastic elastomer composition comprising the following components (A) to (C), wherein a notched IZOD impact strength test piece made from the thermoplastic elastomer composition is heated at 110°C for 1000 hours in a heat resistance test in accordance with ISO 180, and the IZOD impact value measured in an atmosphere at -45°C is 50 kJ / m 2 The above is a thermoplastic elastomer composition. Component (A): Propylene-based polymer Component (B): Ethylene-based copolymer Component (C): Partially hydrogenated styrene-conjugated diene block copolymer
[0014] [5] The thermoplastic elastomer composition according to any one of [1] to [4], wherein the component (B) has a crystalline melting peak at 110 to 125°C and a crystalline melting heat of 20 to 60 J / g.
[0015] [6] The thermoplastic elastomer composition according to any one of [1] to [5], wherein the melt flow rate of the component (A) measured in accordance with ISO 1133 under conditions of a measuring temperature of 230°C and a measuring load of 21.18 N is 20 to 150 g / 10 min.
[0016] [7] A molded article made of the thermoplastic elastomer composition according to any one of [1] to [6].
[0017] [8] An airbag storage cover comprising the thermoplastic elastomer composition according to any one of [1] to [6]. Effect of the Invention
[0018] According to the present invention, it is possible to provide a thermoplastic elastomer composition having excellent low-temperature impact resistance and heat resistance.
[0019] Therefore, the thermoplastic elastomer composition of the present invention or a molded article made of the thermoplastic elastomer composition of the present invention can be suitably used as an airbag storage cover. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will be described in detail below. The following description is an example of an embodiment of the present invention, and the present invention is not limited to the contents of the following description as long as it does not exceed the gist of the present invention. The present invention can be modified in any way as long as it does not deviate from the gist of the present invention.
[0021] In the present invention, when "~" is used to express a numerical value or a physical property value, the values before and after the "~" are included.
[0022] [Thermoplastic elastomer composition] The thermoplastic elastomer composition of the present invention is a thermoplastic elastomer composition containing the following components (A) to (C) in a ratio of 11 to 68 parts by mass of component (B) and 1 to 58 parts by mass of component (C) per 100 parts by mass of component (A). Component (A): Propylene-based polymer Component (B): Ethylene-based copolymer Component (C): Partially hydrogenated styrene-conjugated diene block copolymer
[0023] Another embodiment of the thermoplastic elastomer composition of the present invention is a thermoplastic elastomer composition containing the following components (A) to (C), and the composition has an IZOD impact value of 50 kJ / m when measured in an atmosphere at -45°C using a test piece prepared from the thermoplastic elastomer composition and subjected to a heat resistance test in which the test piece was heated at 110°C for 1000 hours in accordance with ISO 180. 2 The above is the thermoplastic elastomer composition. Component (A): Propylene-based polymer Component (B): Ethylene-based copolymer Component (C): Partially hydrogenated styrene-conjugated diene block copolymer
[0024] [mechanism] The thermoplastic elastomer composition of the present invention exhibits the effect of being able to obtain a molded article having excellent low-temperature impact resistance and heat resistance. Although the details of why the thermoplastic elastomer composition of the present invention exhibits such effects are not clear, it is presumed as follows. In the thermoplastic elastomer composition of the present invention, heat resistance is obtained by component (A), and low-temperature impact resistance is obtained by components (B) and (C). At this time, it is important to use 11 to 68 parts by mass of component (B) and 1 to 58 parts by mass of component (C) per 100 parts by mass of component (A). As is clear from the results of Examples 1 to 4 and Comparative Examples 1 and 4 described later, it is believed that excellent low-temperature impact resistance and heat resistance are obtained in this specific blending composition due to the interaction between components (B) and (C).
[0025] [Component (A): Propylene-based polymer] The propylene polymer of component (A) is a polymer having a propylene unit content of more than 50% by mass relative to all monomer units, i.e., component (A) is a polypropylene resin having a propylene unit content of more than 50% by mass and not more than 100% by mass.
[0026] The type of the propylene-based polymer of component (A) is not particularly limited, and may be a propylene homopolymer or a propylene-based copolymer containing, in addition to propylene units, α-olefin units other than propylene (however, "α-olefin" as used herein includes ethylene) or monomer units other than α-olefins. The propylene-based copolymer may be any of a propylene-based random copolymer, a propylene-based block copolymer, etc. In component (A), the propylene polymer component contributes to rigidity and heat resistance.
[0027] Examples of the α-olefin units other than propylene contained in the propylene-based copolymer include ethylene and α-olefin units having 4 to 20 carbon atoms. Examples of the α-olefins having 4 to 20 carbon atoms include 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 2-ethyl-1-hexene, and 2,2,4-trimethyl-1-pentene. The α-olefin other than propylene is preferably ethylene or an α-olefin having 4 to 10 carbon atoms, and more preferably ethylene, 1-butene, 1-hexene, or 1-octene.
[0028] Examples of the propylene polymer of component (A) include propylene homopolymer, propylene-ethylene copolymer, propylene-1-butene copolymer, propylene-1-hexene copolymer, propylene-1-octene copolymer, propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, propylene-ethylene-1-octene copolymer, etc. Preferred are propylene homopolymer, and copolymers of propylene and at least one monomer selected from ethylene and α-olefins having 4 to 10 carbon atoms.
[0029] From the viewpoints of low-temperature impact resistance and high-temperature strength, a particularly preferred component (A) is a polypropylene block copolymer obtained by polymerizing a propylene homopolymer in the first step and then polymerizing an ethylene-propylene copolymer in the second step.
[0030] The content of propylene units in component (A) is more than 50% by mass and not more than 100% by mass, preferably 70-100% by mass, and more preferably 90-100% by mass, based on the total mass of component (A). When the content of propylene units in component (A) is equal to or more than the lower limit, heat resistance and rigidity tend to be good. The content of propylene units and α-olefin units such as ethylene in component (A) can be determined by infrared spectroscopy.
[0031] From the viewpoint of the appearance of the obtained molded article, the melt flow rate of component (A) is preferably 1 g / 10 min or more, more preferably 5 g / 10 min or more, even more preferably 10 g / 10 min or more, and particularly preferably 20 g / 10 min or more. The melt flow rate of component (A) is usually 150 g / 10 min or less, and from the viewpoint of tensile strength, it is preferably 130 g / 10 min or less, more preferably 100 g / 10 min or less. The melt flow rate (MFR) of component (A) is measured according to ISO 1133 under the conditions of a measurement temperature of 230° C. and a measurement load of 21.18 N.
[0032] When component (A) is a blend of propylene-based polymers having different MFRs, the MFR of component (A) can be calculated by the following formula (I). log(MFR blend) = w1log(MFR1) + w2log(MFR2) + … …+wilog(MFRi)+…+wnlog(MFRn)…(I)
[0033] In formula (I), wi is the mass fraction of component i, MFRi is the MFR of component i, and n is the total number of components in the blend. w1+w2+...+wi+...wn=1.
[0034] The propylene polymer of component (A) can be produced by a known polymerization method using a known olefin polymerization catalyst. For example, a multi-stage polymerization method using a Ziegler-Natta catalyst can be used. The multi-stage polymerization method can be a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, or the like, and two or more of these methods can be used in combination.
[0035] In addition, the component (A) used in the thermoplastic elastomer composition of the present invention may be a commercially available product. The propylene-based polymer in the component (A) may be procured from the manufacturers listed below and may be appropriately selected. Available commercial products include PrimePolypro® from Prime Polymer, Sumitomo Noblen® from Sumitomo Chemical, polypropylene block copolymer from SunAllomer, Novatec® PP from Japan Polypropylene, Moplen® and HifaxX® from LyondellBasell, ExxonMobil PP from ExxonMobil, Formolene® from Formosa Plastics, Borealis PP from Borealis, SEETEC PP from LG Chemical, ASIPOLYPROPYLENE from A. Schulman, INEOS PP from INEOS Olefins & Polymers, Braskem PP from Braskem, Samsung Total from SAMSUNG TOTAL PETROCHEMICALS, Sabic® PP from Sabic, TOTAL PETROCHEMICALS Polypropylene from TOTAL PETROCHEMICALS, and YUPLENE® from SK.
[0036] The thermoplastic elastomer composition of the present invention may contain only one type of component (A), or may contain two or more types having different monomer unit compositions, physical properties, and the like.
[0037] [Component (B): Ethylene-based copolymer] The thermoplastic elastomer composition of the present invention contains an ethylene-based copolymer as component (B). The ethylene-based copolymer of component (B) may be one having an ethylene unit content of 50% by mass or more relative to the total monomer units, and is not particularly limited. Among them, an ethylene-α-olefin copolymer is preferred. The ethylene-α-olefin copolymer is preferably one having an ethylene unit content of 50-80% by mass and an α-olefin unit content of 20-50% by mass, when the total content of ethylene units and α-olefin units is taken as 100% by mass. When the ethylene unit content is within the above range, the affinity with other components is good, and the fine dispersibility of the thermoplastic elastomer composition tends to be improved.
[0038] The α-olefin constituting the ethylene-α-olefin copolymer is not limited, but specific examples include propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, and 1-decene. Only one type of these α-olefin units may be contained in component (B), or two or more types may be contained. Among these, α-olefins having 4 to 8 carbon atoms are preferred, and 1-octene is more preferred. When the ethylene-α-olefin copolymer contains 1-octene units as the α-olefin units, the tensile strength is improved.
[0039] Examples of the ethylene-α-olefin copolymer include ethylene-α-olefin random copolymers and ethylene-α-olefin block copolymers. Among these, ethylene-α-olefin block copolymers, particularly ethylene-α-olefin block copolymers containing a polymer block composed of ethylene and an ethylene-α-olefin copolymer block, are preferred.
[0040] The ethylene copolymer of component (B) used in the present invention preferably has a crystalline melting peak at 110 to 125°C and a crystalline melting heat of 20 to 60 J / g. Here, the fact that component (B) has a crystalline melting peak at 110 to 125°C and a crystalline melting heat of 20 to 60 J / g is an indicator that component (B) has a polymer block made of crystalline ethylene. From the viewpoint of high-temperature strength, the crystalline melting heat of component (B) is preferably 20 J / g or more, more preferably 30 J / g or more. Also, from the viewpoint of low-temperature impact resistance, the crystalline melting heat of component (B) is preferably 60 J / g or less, more preferably 50 J / g or less.
[0041] In addition to having a polymer block made of crystalline ethylene, component (B) preferably has amorphous properties due to the ethylene-α-olefin copolymer block. This amorphous property can be expressed by the glass transition temperature, and the glass transition temperature of component (B) measured by the DSC method is preferably -80°C or higher, more preferably -75°C or higher, and is preferably -50°C or lower, more preferably -60°C or lower. When component (B) has such a structure, the thermoplastic elastomer composition of the present invention is provided with the effects of high temperature strength and low temperature impact resistance.
[0042] The values of the crystalline melting peak, crystalline melting heat, and glass transition temperature of component (B) are obtained by differential scanning calorimetry (DSC). The crystalline melting peak is the top temperature of the melting peak obtained by a differential scanning calorimeter. The crystalline melting heat can be determined from the area of the melting peak obtained by a differential scanning calorimeter. The glass transition temperature is the intersection point of the tangent line at the inflection point and the baseline obtained by a differential scanning calorimeter. The specific measurement conditions for determining these values are as follows: That is, a 10 mg sample is taken and melted using a DSC at a heating rate of 100°C / min from 25°C to 200°C, held at 200°C for 1 minute, crystallized at a heating rate of 10°C / min to -130°C, held at -130°C for 10 minutes, and then measured at a heating rate of 10°C / min up to 200°C.
[0043] The polymer block of ethylene in component (B) is mainly composed of ethylene units, but may have other monomer units in addition to ethylene units. Here, "mainly composed" means that it accounts for 50% by mass or more, particularly 60 to 100% by mass of the whole. Examples of other monomers include α-olefins such as 1-propylene, 1-butene, 2-methylpropylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene. Preferred are 1-propylene, 1-butene, 1-hexene, and 1-octene. When the polymer block of ethylene in component (B) contains α-olefin units having 3 to 8 carbon atoms and a carbon-carbon double bond at the terminal carbon atom, only one type of α-olefin may be copolymerized with ethylene, or two or more types may be copolymerized with ethylene.
[0044] Examples of the α-olefin in the ethylene-α-olefin copolymer block in component (B) include 1-propylene, 1-butene, 2-methylpropylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 1-octene, etc. Preferred are 1-propylene, 1-butene, 1-hexene, and 1-octene. The ethylene-α-olefin copolymer block in component (B) may have other monomer units such as monomer units based on non-conjugated dienes (non-conjugated diene units) in addition to ethylene units and α-olefin units. Examples of the non-conjugated dienes include linear non-conjugated dienes such as 1,4-hexadiene, 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, and 7-methyl-1,6-octadiene; and cyclic non-conjugated dienes such as cyclohexadiene, dicyclopentadiene, methyltetrahydroindene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, and 6-chloromethyl-5-isopropenyl-2-norbornene. Preferred are 5-ethylidene-2-norbornene and dicyclopentadiene.
[0045] The content of the ethylene unit in component (B) is preferably 50 to 80% by mass based on the total amount of component (B). The content of the ethylene unit in component (B) is preferably high in order to prevent fusion due to blocking of component (B), and is preferably low in terms of low-temperature impact resistance when the thermoplastic elastomer composition of the present invention is molded. The lower limit of the content of the ethylene unit in component (B) is more preferably 55% by mass or more, and even more preferably 60% by mass or more. On the other hand, the upper limit of the content of the ethylene unit in component (B) is more preferably 75% by mass or less. The content of the ethylene unit and the content of the α-olefin unit in component (B) can each be determined by infrared spectroscopy.
[0046] In addition, when component (B) has other monomer units such as non-conjugated diene units, the content thereof is usually 10 mass% or less, preferably 5 mass% or less, based on the total of component (B). The content of non-conjugated diene units can also be determined by infrared spectroscopy.
[0047] Specific examples of component (B) used in the thermoplastic elastomer composition of the present invention include ethylene-based block copolymers containing a polymer block made of ethylene and an ethylene / α-olefin copolymer block, such as an ethylene / 1-butene copolymer, an ethylene / 1-hexene copolymer, an ethylene / 1-octene copolymer, an ethylene / propylene / 1-butene copolymer, an ethylene / propylene / 1-hexene copolymer, or an ethylene / propylene / 1-octene copolymer. In component (B), these ethylene-α-olefin copolymer blocks may be used alone or in combination of two or more kinds. Among these, component (B) is most preferably an ethylene-based block copolymer containing a polymer block composed of ethylene and an ethylene-1-octene copolymer block.
[0048] The melt flow rate of component (B) is not limited, but is usually 10 g / 10 min or less, and from the viewpoint of strength, it is preferably 8.0 g / 10 min or less, more preferably 5.0 g / 10 min or less, and even more preferably 3.0 g / 10 min or less. The melt flow rate of component (B) is usually 0.01 g / 10 min or more, and from the viewpoint of fluidity, it is preferably 0.05 g / 10 min or more, more preferably 0.10 g / 10 min or more. The melt flow rate (MFR) of component (B) is measured according to ASTM D1238 under the conditions of a measurement temperature of 190 ° C. and a measurement load of 21.18 N.
[0049] From the viewpoint of low-temperature impact resistance, the density of component (B) is preferably 0.880 g / cm 3 More preferably, it is 0.875 g / cm or less. 3 On the other hand, the lower limit is not particularly limited, but is usually 0.850 g / cm 3 The density of component (B) is measured at a measurement temperature of 23°C according to ISO 1183-A method.
[0050] Component (B) can be synthesized according to the methods disclosed in JP-A-2007-529617, JP-A-2008-537563, and JP-A-2008-543978. For example, it can be produced by preparing a composition containing a mixture or reaction product obtained by combining a first olefin polymerization catalyst, a second olefin polymerization catalyst capable of preparing a polymer having different chemical or physical properties from a polymer prepared by the first olefin polymerization catalyst under the same polymerization conditions, and a chain shuttling agent, and contacting the composition with the ethylene and α-olefin under addition polymerization conditions.
[0051] The polymerization of component (B) is preferably carried out by a continuous solution polymerization method. In the continuous solution polymerization method, the catalyst components, the chain shuttling agent, the monomers, and optionally the solvent, the auxiliary, the scavenger and the polymerization aid are continuously fed into a reaction zone, and the polymer product is continuously taken out therefrom. The length of the block can be changed by controlling the ratio and type of the catalyst, the ratio and type of the chain shuttling agent, the polymerization temperature, etc.
[0052] Other conditions for the synthesis of the olefin block copolymer of component (B) are disclosed in JP-A-2007-529617, JP-A-2008-537563, and JP-A-2008-543978.
[0053] Also, a commercially available product can be used as component (B), such as the Engage (registered trademark)-XLT series or INFUSE (registered trademark) series manufactured by Dow Chemical Co. Among the components (B), those having an ethylene-octene copolymer block were not available as products until Dow Chemical Co. began to commercially produce the INFUSE (registered trademark) series in 2007 and the Engage (registered trademark)-XLT series in 2011.
[0054] The thermoplastic elastomer composition of the present invention may contain only one type of component (B), or may contain two or more types having different monomer unit compositions, physical properties, and the like.
[0055] [Component (C): Partially hydrogenated styrene-conjugated diene block copolymer] A suitable conjugated diene in the partially hydrogenated styrene-conjugated diene block copolymer of component (C) is butadiene, isoprene or a mixture thereof. An example of the partially hydrogenated styrene-conjugated diene block copolymer of component (C) is styrene-butadiene-butylene-styrene block copolymer (hereinafter sometimes abbreviated as "SBBS").
[0056] The styrene unit content of the partially hydrogenated styrene-conjugated diene block copolymer is not particularly limited, but from the viewpoints of strength and heat resistance, it is preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more. Also, from the viewpoints of flexibility and impact resistance, the styrene unit content is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less.
[0057] The conjugated diene of the partially hydrogenated styrene-conjugated diene block copolymer of component (C) may be isoprene alone, butadiene alone, or a mixture of isoprene and butadiene.
[0058] The hydrogenation rate of the double bonds derived from 1,4-bonds in the conjugated diene block of component (C) is 20-80%, preferably 30-70%. If the hydrogenation rate of the double bonds derived from 1,4-bonds is 20% or more, the weather resistance and heat resistance of the thermoplastic elastomer composition of the present invention tend to be good, and if the hydrogenation rate is 80% or less, the low-temperature impact resistance tends to be sufficiently improved. In addition, the hydrogenation rate of the double bonds derived from 1,2-bonds and 3,4-bonds in the conjugated diene block is 85% or more, preferably 90% or more. If the hydrogenation rate of the double bonds derived from 1,2-bonds and 3,4-bonds is 85% or more, the weather resistance and heat resistance of the thermoplastic elastomer composition of the present invention tend to be good.
[0059] The weight average molecular weight (Mw) of the partially hydrogenated styrene-conjugated diene block copolymer of component (C) is preferably 50,000 or more, more preferably 80,000 or more, and even more preferably 90,000 or more, from the viewpoint of releasability. Also, from the viewpoint of flowability, Mw is preferably 500,000 or less, more preferably 450,000 or less, even more preferably 400,000 or less, and particularly preferably 350,000 or less.
[0060] The Mw of component (C) is measured by gel permeation chromatography (GPC), and can be measured, for example, under the following conditions. Equipment: Tosoh Corporation "HLC-8220GPC(R)" Column: Tosoh Corporation "TSKgel Super HM-M (6.0 mm I.D. x 15 cm x 2+G)" Detector: Differential refractive index detector (RI / built-in) Solvent: Chloroform Temperature: 40℃ Flow rate: 0.25mL / min Injection volume: 0.1 mass% x 20 μL Calibration sample: monodisperse polystyrene Calibration method: Polystyrene equivalent Calibration curve approximation: cubic (hyperbola) Exclusion limit setting time: 12 minutes
[0061] From the viewpoint of moldability, the density of component (C) is preferably 1.00 g / cm 3 More preferably, it is 0.95 g / cm or less. 3 On the other hand, the lower limit is not particularly limited, but is usually 0.85 g / cm 3 The density of component (C) is measured at a measurement temperature of 23° C. in accordance with ASTM D792.
[0062] The styrene-conjugated diene block copolymer of component (C) can be produced in an inert solvent using a lithium catalyst, for example, by the method described in JP-B-40-23798. Also, a partially hydrogenated product of the styrene-conjugated diene block copolymer can be produced by hydrogenating the styrene-conjugated diene block copolymer thus produced in an inert solvent in the presence of a hydrogenation catalyst, for example, by the methods described in JP-B-42-8704, JP-B-43-6636, JP-A-59-133203, and JP-A-60-79005.
[0063] An example of a commercially available partially hydrogenated styrene-conjugated diene block copolymer of component (C) is "Tuftec (registered trademark) P" manufactured by Asahi Kasei Corporation.
[0064] The thermoplastic elastomer composition of the present invention may contain only one type of component (C), or may contain two or more types having different monomer unit compositions, physical properties, and the like.
[0065] [Content ratio] In the thermoplastic elastomer composition of the present invention, the content of component (B) is usually 11 parts by mass or more, preferably 15 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 25 parts by mass or more, and particularly preferably 30 parts by mass or more, per 100 parts by mass of component (A), from the viewpoint of the low-temperature characteristics and heat resistance of the obtained molded article. Also, the content of component (B) is usually 68 parts by mass or less, preferably 65 parts by mass or less, more preferably 60 parts by mass or less, even more preferably 55 parts by mass or less, and particularly preferably 50 parts by mass or less, per 100 parts by mass of component (A), from the viewpoint of the heat resistance of the obtained molded article.
[0066] In the thermoplastic elastomer composition of the present invention, the content of component (C) is usually 1 part by mass or more, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 15 parts by mass or more, and particularly preferably 20 parts by mass or more, per 100 parts by mass of component (A), from the viewpoint of the low-temperature impact resistance and heat resistance of the resulting molded article. Also, the content of component (C) is usually 58 parts by mass or less, preferably 50 parts by mass or less, more preferably 45 parts by mass or less, even more preferably 40 parts by mass or less, and particularly preferably 35 parts by mass or less, per 100 parts by mass of component (A), from the viewpoint of the low-temperature impact resistance and heat resistance of the resulting molded article.
[0067] From the viewpoint of heat resistance, it is preferable that the components (C) and (B) are blended such that the content of component (C) is lower than the content of component (B). Specifically, the content of component (B) relative to 100 parts by mass of component (A) is W B The content of component (C) in parts by mass is W C If it is parts by weight, W B -W C (parts by mass) is preferably 1 part by mass or more, particularly 15 parts by mass or more. On the other hand, from the viewpoint of ensuring the content of component (B), W B -W C (Parts by mass) is preferably 60 parts by mass or less, particularly preferably 40 parts by mass or less.
[0068] [Other ingredients] In addition to the above-mentioned components, the thermoplastic elastomer composition of the present invention may contain optional components such as the following additives, inorganic fillers, organic fillers, and resins other than components (A) to (C) (hereinafter referred to as "other resins") depending on various purposes, within the range that does not significantly impair the effects of the present invention.
[0069] Examples of additives include various additives such as colorants, antioxidants, weathering aids, heat stabilizers, light stabilizers, ultraviolet absorbers, neutralizing agents, lubricants, antifogging agents, antiblocking agents, slip agents, flame retardants, dispersants, antistatic agents, conductivity imparting agents, metal deactivators, molecular weight regulators, antibacterial agents, fluorescent whitening agents, etc. These additives can usually be used in an amount of 0.01 to 2 parts by mass per 100 parts by mass of the total of components (A) to (C).
[0070] Examples of other resins that may be contained in the thermoplastic elastomer composition of the present invention include polyester elastomers, urethane elastomers, polyester resins, polyamide resins, polyurethane resins, styrene resins (excluding those corresponding to component (C)), acrylic resins, polycarbonate resins, polyvinyl chloride resins, polypropylene resins and other polyolefin resins (excluding those corresponding to components (A) and (B)), various elastomers other than those mentioned above, etc. The above-mentioned other resins may be contained alone or in combination of two or more kinds.
[0071] [Method of producing thermoplastic elastomer composition] The thermoplastic elastomer composition of the present invention can be produced by kneading the components (A) to (C) and other components in a conventional manner using a conventional extruder, Banbury mixer, roll, Brabender Plastograph, Kneader Brabender, etc. Among these production methods, it is preferable to use an extruder, particularly a twin-screw extruder. When the thermoplastic elastomer composition of the present invention is produced by kneading it using an extruder or the like, it can be produced by melt kneading it in a heated state usually at 160 to 240°C, preferably 180 to 220°C. Furthermore, the thermoplastic elastomer composition of the present invention may be partially crosslinked by blending the following crosslinking agent or crosslinking aid and dynamically heat treating it.
[0072] As a crosslinking agent for partially crosslinking the thermoplastic elastomer composition of the present invention, it is preferable to use an organic peroxide, and examples of such a crosslinking agent include 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, 1,3-bis(t-butylperoxyisopropyl)benzene, 1,1-di(t-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(peroxybenzoyl)-3-hexyne, and dicumyl peroxide.
[0073] Examples of crosslinking aids used in partial crosslinking with these organic peroxides include compounds having a radically polymerizable carbon-carbon double bond, such as N,N'-m-phenylene bismaleimide, toluylene bismaleimide, P-quinone dioxime, p-dinitrosobenzene, 1,3-diphenyl guanidine, trimethylolpropane triacrylate, divinylbenzene, ethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, and allyl methacrylate, and compounds having a functional group that reacts with the straight carbon chain portion of component (B).
[0074] [Low temperature impact resistance of thermoplastic elastomer composition] In the present invention, the notched IZOD impact strength at −45° C. measured according to ISO 180 (2013) is taken as an index of low-temperature impact resistance. Details of the method for measuring this notched IZOD impact strength are as described in the Examples section below. The notched IZOD impact strength at -45°C measured for the thermoplastic elastomer composition of the present invention is 50 kJ / m 2 It is preferable that the concentration is 55 kJ / m or more. 2 More preferably, it is 60 kJ / m or more. 2 More preferably, it is 70 kJ / m or more. 2 On the other hand, the upper limit of the notched IZOD impact strength of the thermoplastic elastomer composition of the present invention is not particularly limited, but is usually 150 kJ / m 2 The following is the result.
[0075] [Heat resistance of thermoplastic elastomer composition] In the present invention, the notched IZOD impact strength measured in the same manner as in the above-mentioned evaluation of low-temperature impact resistance after a heat resistance test in which the sample is heated for 1000 hours under heating conditions of 110° C. is used as an index of heat resistance. Details of this heat resistance test method and the subsequent method of measuring the notched IZOD impact strength are as described in the Examples section below. The thermoplastic elastomer composition of the present invention has a notched IZOD impact strength of 50 kJ / m at -45°C after heat resistance testing. 2 It is preferable that the concentration is 52 kJ / m or more. 2 More preferably, it is 57 kJ / m or more. 2 More preferably, it is 60 kJ / m or more. 2 On the other hand, the upper limit of the notched IZOD impact strength of the thermoplastic elastomer composition of the present invention after the heat resistance test is not particularly limited, but is usually 150 kJ / m 2 The following is the result.
[0076] [Molded body / airbag storage cover] The thermoplastic elastomer composition of the present invention can be molded into a molded article by using a normal injection molding method or, if necessary, various molding methods such as gas injection molding, injection compression molding, short shot foam molding, etc., to produce the airbag storage cover of the present invention. In particular, the airbag storage cover of the present invention is preferably produced by injection molding, and the molding conditions for injection molding are as follows. The molding temperature when injection molding the airbag storage cover is generally 150 to 300° C., and preferably 160 to 280° C. The injection pressure is generally 5 to 100 MPa, and preferably 10 to 80 MPa. The mold temperature is generally 0 to 80° C., and preferably 20 to 60° C.
[0077] The airbag storage cover obtained in this manner is suitable for use as an airbag storage cover for an airbag system that activates and inflates when it senses the impact or deformation of a high-speed moving object such as an automobile in a collision accident. The airbag storage cover of the present invention can be suitably used as a driver's airbag storage cover, a passenger's airbag storage cover, a pedestrian airbag storage cover, a knee airbag storage cover, a side airbag storage cover, a curtain airbag storage cover, etc. EXAMPLES
[0078] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the invention. The values of various production conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values of the examples.
[0079] <Raw materials> [Component (A)] (A-1): Propylene block copolymer (obtained by polymerizing propylene homopolymer in the first step, followed by polymerizing ethylene-propylene copolymer in the second step) MFR(ISO 1133):65g / 10min (Measurement conditions: 230℃, load 21.18N (2.16kgf)) Propylene polymer component content: 92% by mass Ethylene-propylene copolymer component content: 8% by mass Ethylene unit content in ethylene-propylene copolymer component: 43% by mass (A-2): HifaxX (registered trademark) 1956A manufactured by LyondellBasell (obtained by polymerizing propylene homopolymer in the first step, followed by polymerizing ethylene-propylene copolymer in the second step) MFR(ISO 1133):1.1g / 10min (Measurement conditions: 230℃, load 21.18N (2.16kgf)) Propylene polymer component content: 70% by mass Ethylene-propylene copolymer component content: 30% by mass, Ethylene unit content in ethylene-propylene copolymer component: 65% by mass
[0080] [Component (B)] (B-1): Engage (registered trademark) XLT8677 manufactured by Dow Chemical Company (an ethylene-based block copolymer having a polymer block composed of ethylene and an ethylene-1-octene copolymer block) Crystal melting peak temperature: 119℃ Heat of crystal fusion: 37J / g Glass transition temperature (DSC method): -67℃ MFR(ASTM D1238): 0.5g / 10min (Measurement conditions: 190℃, load 21.18N (2.16kgf)) (catalog value) Density (ISO 1183-A method): 0.872g / cm 3 (Measurement temperature: 23℃)
[0081] [Component (C)] (C-1): Asahi Kasei Tuftec (registered trademark) P1083 (styrene-butadiene-butylene-styrene block copolymer) Styrene unit content: 20% by mass (catalog value) Butadiene / butylene content: 80% by mass (catalog value) Amount of 1,4-bonds in butadiene-butylene polymer: 63% Hydrogenation rate of 1,4-bonded polymer: 65% Hydrogenation rate of 1,2-bond polymer: 97% Weight average molecular weight (Mw): 95,000 Density (ISO 1183): 0.89g / cm 3 (catalog value)
[0082] [Comparative ingredients] (C'-1): Globalprene (registered trademark) 3411 (styrene-butadiene-styrene block copolymer) manufactured by LCY Styrene unit content: 30% by mass (catalog value) Conjugated diene unit content: 70% by mass (catalog value) Weight average molecular weight (Mw): 240,000 Density (ASTM D792): 0.94g / cm 3 (catalog value)
[0083] <Evaluation method> 1) Low temperature impact resistance (notched IZOD impact strength) The obtained thermoplastic elastomer composition was used to mold a test piece for measuring IZOD impact strength into a thickness of 4 mm, width of 10 mm, and length of 80 mm using an in-line screw type injection molding machine (Sumitomo Wiring Systems, Ltd., "SE180") at an injection pressure of 100 MPa, an injection speed of 27 mm / s, a cylinder temperature setting of 220°C, and a mold temperature of 40°C. Then, a notch was made in the dumbbell (the notch dimensions and evaluation method were in accordance with ISO 180 (2013)), and the IZOD impact strength was measured at a temperature of -45°C. The higher the IZOD impact value, the better the low-temperature impact resistance was evaluated to be.
[0084] 2) Heat resistance (heat resistance test) The notched test piece obtained in 1) above was placed in an oven (Perfect Oven, manufactured by Espec Corp.) and left to stand at 110°C for 1000 hours. The test piece was then taken out and left to stand in a room temperature environment to be used as a test piece for a heat resistance test, and the IZOD impact strength was measured at a temperature of -45°C in the same manner as in 1) above. The larger the IZOD impact value after the heat resistance test, the more excellent the heat resistance is evaluated to be.
[0085] <Examples / Comparative Examples> [Example 1] (A-1) 75 parts by mass, (A-2) 25 parts by mass, (B-1) 61 parts by mass, (C-1) 8 parts by mass, (A-1), (B-1), (C-1) 100 parts by mass in total, 0.2 parts by mass of antioxidant (breakdown: 0.1 parts by mass of (Irganox (registered trademark) 1010, manufactured by BASF Japan) and 0.1 parts by mass of (Irgafos (registered trademark) 168, manufactured by BASF Japan)), weathering aid (product name of BASF Japan) 0.2 parts by mass of Tinuvin (registered trademark) XT855FF) and 1.5 parts by mass of a colorant (black pigment, carbon concentration 40% by mass) were blended in a Henschel mixer for 1 minute, and fed into a unidirectional twin-screw extruder (Kobe Steel "TEX30α", L / D=45, number of cylinder blocks: 13) at a rate of 20 kg / hr, heated to a range of 180 to 210°C, melt-kneaded, and pellets of a thermoplastic elastomer composition were produced. The pellets of the thermoplastic elastomer composition obtained were evaluated in the above 1) to 2). The evaluation results are shown in Table 1.
[0086] [Examples 2 to 4 and Comparative Examples 1 to 4] Pellets of a thermoplastic elastomer composition were obtained in the same manner as in Example 1, except that the blending amounts of the antioxidant, weathering aid, and colorant were omitted in Table 1. The obtained pellets of the thermoplastic elastomer composition were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.
[0087] [Table 1]
[0088] [Discussion of evaluation results] As shown in Table 1, the thermoplastic elastomer compositions of Examples 1 to 4, which correspond to the thermoplastic elastomer compositions of the present invention, have an IZOD impact strength value of 50 kJ / m at -45°C. 2 This shows that the film has excellent low-temperature impact resistance. In addition, even after the heat resistance test, the IZOD impact strength value at -45°C was 50 kJ / m 2 From these findings, it is clear that the thermoplastic elastomer compositions of Examples 1 to 4 are excellent in low-temperature impact resistance and heat resistance.
[0089] Comparative Example 1 is an example in which component (C) was not used, and the heat resistance was poor. Comparative Example 2 is an example in which 25 parts by mass of non-hydrogenated component (C'-1) was blended in place of component (C), and the heat resistance was poor. Comparative Examples 3 and 4 are examples in which the blending amount of component (C-1) exceeds 58 parts by mass, and the low-temperature impact resistance and heat resistance are poor. [Industrial Applicability]
[0090] The thermoplastic elastomer composition of the present invention has excellent low-temperature impact resistance and heat resistance, and can be suitably used in various applications. For example, the thermoplastic elastomer composition of the present invention is useful as automobile interior parts such as airbag storage covers, instrument panels, center panels, center console boxes, door trims, pillars, assist grips, and handles, automobile exterior parts such as mudguards and chromets, home appliance parts, building materials, furniture, etc. Among these, the thermoplastic elastomer composition of the present invention is particularly useful as an airbag storage cover, and among these airbag storage covers, the thermoplastic elastomer composition of the present invention is suitable as an airbag storage cover for an airbag system that operates by detecting the impact or deformation of a high-speed moving object such as an automobile in a collision accident, and protects the occupant by inflating and deploying.
Claims
1. The thermoplastic elastomer composition comprises the following components (A) to (C), in a ratio of 11 to 68 parts by mass of component (B) and 1 to 58 parts by mass of component (C) relative to 100 parts by mass of component (A): the thermoplastic elastomer composition has an IZOD impact value of 50 kJ / m 2 or more and 150 kJ / m 2 or less, as measured in an atmosphere at -45°C using a test piece for measuring notched IZOD impact strength prepared from the thermoplastic elastomer composition and subjected to a heat resistance test in which the test piece was heated at a heating condition of 110°C for 1000 hours in accordance with ISO 180: Component (A): Propylene-based polymer Component (B): Ethylene-based copolymer Component (C): A partially hydrogenated styrene-conjugated diene block copolymer in which the hydrogenation rate of the double bonds derived from the 1,4-bonds in the conjugated diene block is 20 to 80%.
2. 2. The airbag storage cover according to claim 1, wherein the component (A) is a propylene-based block copolymer.
3. An airbag storage cover as described in claim 1 or 2, wherein the content of component (C) in the thermoplastic elastomer composition is less than the content of component (B).
4. 4. The airbag storage cover according to claim 1, wherein the component (B) has a crystalline melting peak at 110 to 125° C. and a crystalline melting heat of 20 to 60 J / g.
5. The component (A) has a melt flow rate of 20 to 150 g / 10 min, measured according to ISO 1133 at a measurement temperature of 230° C. and a measurement load of 21.18 N. The airbag storage cover according to any one of claims 1 to 4.
Citation Information
Patent Citations
Thermoplastic elastomer composition for air bag cover and air bag
JP1997202202A
Air bag cover for vehicle
JP2001206183A
Thermoplastic elastomer composition
JP2005133021A
Thermoplastic resin composition
JP2007056145A
Thermoplastic elastomer composition, molded article and air bag housing cover
JP2015193821A