Machinery Parts

A cobalt-based alloy with specific compositions and additive manufacturing addresses the hardness-toughness trade-off in mechanical parts, achieving superior hardness and toughness, especially in cutting edges, with improved wear resistance and manufacturing efficiency.

JP7571965B2Active Publication Date: 2024-10-23TOHOKU UNIV +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020155229
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-16
Publication Date
2024-10-23
Estimated Expiration
2040-09-16

AI Technical Summary

Technical Problem

Conventional mechanical parts made from materials like die steel, high-speed tool steel, and cemented carbide face a trade-off between hardness and toughness, with lower toughness as they become harder, and there is a need for a material with superior hardness and toughness.

Method used

A cobalt-based alloy with specific compositions of C, Cr, Mo, W, and inevitable impurities, formed using additive manufacturing, with carbides uniformly dispersed at 10 μm or less, achieving both high hardness and toughness.

Benefits of technology

The cobalt-based alloy achieves hardness comparable to cemented carbide and toughness superior to existing materials, with improved wear resistance and strength, particularly in cutting edges, and can be manufactured efficiently through additive manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571965000002
    Figure 0007571965000002
  • Figure 0007571965000003
    Figure 0007571965000003
  • Figure 0007571965000004
    Figure 0007571965000004
Patent Text Reader

Abstract

To provide a mechanical component that is composed of a cobalt-base alloy and has both of hardness comparable to that of cemented carbide and improved toughness.SOLUTION: A mechanical component is made up of Co-base alloy powder containing C: 2.5-5.0 mass%, Cr: 26-35 mass%, Mo: 10 mass% or less, W: 8-18 mass%, and unavoidable impurities with the balance being Co and is formed by additive manufacturing, wherein the Co-base alloy includes uniformly dispersed carbides of 10 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a machine part. [Background technology]

[0002] Materials conventionally used as machine parts include die steel (SKD material), high-speed tool steel (HSS), ceramics, cemented carbide, etc. As machine parts using these materials, for example, blades have been developed that are manufactured by using high-speed tool steel, die steel, or alloy tool steel powder material to create a compact by hot isostatic pressing, cutting this compact to desired dimensions, and processing it into a final shape (for example, see Patent Document 1).

[0003] However, when powdered high speed steel is used as the material for this machine part, the Charpy impact value is about 30 to 42 J / cm 2 and cemented carbide (approx. 3 J / cm 2 ), but its hardness is HRC (Rockwell hardness) 62-64, which is slightly lower than that of cemented carbide (HRC>70). Even when die steel is used, the Charpy impact value is about 18-20 J / cm 2 Although its toughness is superior to that of cemented carbide, its hardness is HRC62, which is slightly lower than that of cemented carbide. Thus, with conventional machine parts, the harder they become, the lower their toughness (Charpy impact value: dynamic toughness) tends to be, and there was a problem in that there were no materials in the high hardness range close to that of cemented carbide that had the same toughness as steel materials such as die steel and high-speed tool steel.

[0004] In order to solve this problem, the present inventors are developing a machine part made of a cobalt-based alloy that has both excellent hardness and toughness by using an additive manufacturing method. That is, the inventors are developing a machine part with a hardness of HRC63 that is formed by using an additive manufacturing method using a Co-based alloy powder containing 0.5-5.0 mass% C, 26-35 mass% Cr, 5.0-7.0 mass% Mo, unavoidable impurities, and the balance Co (see, for example, Patent Document 2).

[0005] In order to further improve hardness and toughness, they have developed a Co-based alloy powder containing 2.5 to 5.0 mass% C, 26 to 35 mass% Cr, 14 to 20 mass% Mo, unavoidable impurities, and the balance being Co, a Co-based alloy powder containing 2.5 to 5.0 mass% C, 26 to 35 mass% Cr, 20 to 26 mass% W, unavoidable impurities, and the balance being Co, and a Co-based alloy powder containing 2.5 to 5.0 mass% C, 26 to 35 mass% Cr, 10 to 15 mass% Mo, 5 to 7 mass% W, unavoidable impurities, and the balance being Co, and a machine part in which carbides of 10 μm or less are uniformly dispersed, which is formed using an additive manufacturing method (for example, see Patent Document 3). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 11-106801 [Patent Document 2] JP 2015-190004 A [Patent Document 3] JP 2019-014921 A Summary of the Invention [Problem to be solved by the invention]

[0007] The mechanical part described in Patent Document 3 has a hardness of HRC70.1 to 70.4 and a Charpy impact value of 8 to 12 J / cm 2 It has a hardness comparable to that of cemented carbide and a toughness that is about 3 to 4 times that of cemented carbide, approaching that of steel. However, there are hopes for the development of machine parts with even greater hardness and toughness.

[0008] The present invention has been made in view of the above-mentioned problems, and has an object to provide a machine part made of a cobalt-based alloy that has both hardness comparable to that of cemented carbide and superior toughness. [Means for solving the problem]

[0009] In order to achieve the above object, the inventors have investigated whether it is possible to further improve toughness by changing the content of components, etc., and as a result of extensive research and trial and error, they have arrived at the present invention.

[0010] That is, the mechanical component according to the present invention is composed of C: 2.5 to 5.0 mass %, Cr: 26 to 35 mass %, and Mo: 3~ 10 mass %and , W: 13 The material is a Co-based alloy powder containing up to 18% by mass of Co and unavoidable impurities, with the remainder being Co, Using an electron beam It is characterized by being made of a Co-based alloy in which carbides of 10 μm or less are uniformly dispersed, formed using additive manufacturing techniques.

[0011] The mechanical part according to the present invention has high hardness, HRC≧72, and has high hardness comparable to that of cemented carbide, and has excellent wear resistance, because carbides of 10 μm or less are uniformly dispersed. Therefore, the strength of thinly formed parts such as cutting edges can be increased. By forming the mechanical part using an additive manufacturing method, precipitates such as carbides can be easily refined to 10 μm or less, and hardness can be increased. In addition, by mixing each composition in the respective ratios, a relatively high toughness close to that of die steel or high-speed tool steel can be obtained. Thus, the mechanical part according to the present invention is an additive manufacturing body made of a cobalt-based alloy, and has hardness comparable to that of cemented carbide and better toughness.

[0012] In the machine component according to the present invention, when C is less than 2.5 mass%, Cr is less than 26 mass%, and W is less than 8 mass%, the hardness is lower than HRC72. When C is more than 5.0 mass%, Cr is more than 35 mass%, Mo is more than 10 mass%, and W is more than 18 mass%, the toughness is significantly reduced and the component becomes brittle and cannot be used. In the machine component according to the present invention, the inevitable impurities are Si, Mn, N, Ni, Ti, Fe, Nb, V, Ta, etc.

[0013] Mechanical parts according to the present invention And, Mo is added to obtain excellent hardness and toughness. 、5 It is more preferable that the content is 8% by mass or less, and more preferably 8% by mass or less. stomach.

[0014] The mechanical part according to the present invention can be easily manufactured by utilizing the additive manufacturing method, even if a Co-based alloy powder containing carbon and having high hardness is used as a material. In addition, the mechanical part according to the present invention is preferably formed by irradiating the Co-based alloy powder with an electron beam or a laser beam, sintering and melting the powder, forming the powder into a near-net shape, and then finishing the molded product. In this case, complicated manufacturing processes such as mechanical processing such as forging and rolling, cutting from raw materials, raw processing (inner diameter hole processing), and quenching and tempering are not required, and the mechanical part can be manufactured more easily and inexpensively. In addition, various shapes and types of products can be manufactured, and a wide variety of small-scale production can be performed.

[0015] In the mechanical component according to the present invention, the Co-based alloy preferably has the carbides three-dimensionally connected in a network shape, thereby obtaining better hardness and toughness.

[0016] The machine part according to the present invention may be a part for any purpose. It is particularly preferable that the machine part according to the present invention is made of a blade, since it has excellent hardness and toughness, and is also highly resistant to corrosion and wear. In this case, the strength of the blade edge is high, and the blade edge is not easily cracked or chipped. Effect of the Invention

[0017] According to the present invention, it is possible to provide a machine part made of a cobalt-based alloy that has both hardness comparable to that of cemented carbide and superior toughness. [Brief description of the drawings]

[0018] [Figure 1]4A and 4B are electron microscope photographs of a horizontal section and a vertical section, respectively, of a test sample corresponding to a mechanical part according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view showing an image of carbides connected three-dimensionally in a network shape in the test sample shown in FIG. 1 excluding the Co matrix portion. [Diagram 3] 2 is an electron microscope photograph of a cross section of a cast material having the same components as the test sample shown in FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, the embodiment of the present invention will be described with reference to examples. A mechanical component according to an embodiment of the present invention is formed by using an additive manufacturing method using a Co-based alloy powder containing 2.5 to 5.0 mass% C, 26 to 35 mass% Cr, 10 mass% or less Mo, 8 to 18 mass% W, unavoidable impurities, and the balance being Co. The mechanical component according to an embodiment of the present invention is an additive manufacturing body, and is made of a Co-based alloy in which carbides of 10 μm or less are uniformly dispersed. EXAMPLES

[0020] As a powder sample corresponding to the mechanical part of the embodiment of the present invention, a Co-based alloy composition containing 27 mass% Cr, 6 mass% Mo, 16 mass% W, and the remainder Co, to which 3 mass% carbon was added, was vacuum melted and gas atomized in nitrogen gas to prepare a Co-based alloy powder. The average particle size of these powders was adjusted to 1 μm to 200 μm by adjusting the atomization conditions and the mesh sieve.

[0021] Using the powder sample as material, an additive manufacturing method was used to create an additive manufacturing test sample. In the additive manufacturing method, Co-based alloy powder was irradiated with an electron beam in a vacuum chamber and sintered and melted to form a near-net shape. At this time, the electron beam was alternately scanned in directions perpendicular to the X-axis and Y-axis of the stage for each layer thickness of 70 μm, and sintering and melting were performed. After forming into a near-net shape, it was cooled in a He gas atmosphere and further finished to create a cubic test sample with one side measuring 10 mm.

[0022] The electron beam additive manufacturing (EBM) device used was an Arcam EBM A2X system (Arcam AB, Molndal, Sweden). The additive manufacturing conditions were an acceleration voltage of 60 kV and a preheating temperature range of 750 to 850 °C. In addition to the main components, the test samples may contain unavoidable impurities such as Si, Mn, N, Ni, Ti, Fe, Nb, V, and Ta. Although an electron beam was used for additive manufacturing here, samples can also be prepared using a laser beam. Table 1 shows the composition of the test samples prepared.

[0023] [Table 1]

[0024] The test samples were subjected to measurements of Charpy impact value and Rockwell hardness (HRC). The measurement results are shown in Table 1. Table 1 also shows the compositions, Charpy impact values ​​and Rockwell hardness (HRC) of test samples 1 to 3 described in Patent Document 3, which were produced by the present inventors as comparative samples 1 to 3. As shown in Table 1, it was confirmed that the test sample had a hardness of HRC72, which is harder than comparative samples 1 to 3 and is comparable in hardness to that of cemented carbide. The test sample also had a Charpy impact value of 15 J / cm 2 It was confirmed that the toughness of the samples was approximately five times that of the cemented carbide and was greater than those of the comparative samples 1 to 3, and was closer to that of steel materials.

[0025] Next, the structure of the test sample was observed using electron microscope photographs of a horizontal cross section along the layering surface during additive manufacturing, and a vertical cross section along the layering direction. The horizontal and vertical cross sections were each taken as cross sections passing through the center of the test sample, which had a cubic shape with sides of 10 mm. The electron microscope photographs of the horizontal and vertical cross sections of the test sample are shown in Figures 1(a) and (b), respectively.

[0026] As shown in Figure 1, it was confirmed that fine carbides were precipitated in the structure of the test sample (white and grey areas in the figure). It was also confirmed that these carbides were 10μm or less in diameter and size, and were dispersed almost uniformly in the structure. These carbides were mainly Cr, Mo and W carbides. The black areas in the figure are the Co matrix.

[0027] In addition, since the precipitated carbides are finely dispersed in a mesh pattern of 10 μm or less in both the horizontal and vertical cross sections in Fig. 1, it is believed that the carbides are strongly connected in a three-dimensional mesh pattern as shown in Fig. 2. In this way, by forming the test sample using the additive manufacturing method, the precipitates such as carbides are refined to 10 μm or less, and the carbides are connected in a three-dimensional mesh pattern, so it is believed that the test sample has very good hardness and toughness as shown in Table 1.

[0028] From the results of hardness and Charpy impact value shown in Table 1 and the results of the structure observation in the figure, it can be said that the mechanical parts according to the embodiment of the present invention can improve the wear resistance and strength (toughness) of thin parts such as cutting edges. Therefore, even when used for sliding parts (bearings, guide rails, etc.) or blades, they have a long life and are less likely to crack or chip.

[0029] For comparison, raw materials with the same composition as the test samples were vacuum melted and the molten metal was cast into a metal mold to create an ingot (hereafter referred to as the "cast material"), which was then subjected to measurement of the Charpy impact value and Rockwell hardness (HRC) and structural observation using an electron microscope photograph. The composition, Charpy impact value, and Rockwell hardness (HRC) of the cast material are shown in Table 1, and an electron microscope photograph of the cross section of the cast material is shown in Figure 3.

[0030] As shown in Table 1, the hardness of the cast material was HRC72, which was the same as the hardness of the test sample of the additive manufacturing body. In addition, as shown in Figure 3, the precipitated carbides in the cast material are not uniformly dispersed in the structure and are not strongly bonded to each other three-dimensionally. For this reason, it is brittle and easily crumbles, and cannot be used as a structure, so as shown in Table 1, it was not possible to measure the Charpy impact value. Thus, even if the components are the same, the cast material does not have the toughness and cannot be used as a mechanical part.

Claims

1. A mechanical part made of a Co-based alloy powder containing 2.5 to 5.0 mass% C, 26 to 35 mass% Cr, 3 to 10 mass% Mo, 13 to 18 mass% W, unavoidable impurities, and the balance being Co, and formed using an additive manufacturing method using an electron beam, the Co-based alloy having carbides of 10 μm or less uniformly dispersed therein.

2. 2. The mechanical component according to claim 1, wherein the carbides of the Co-based alloy are three-dimensionally connected in a network shape.

3. The mechanical part according to claim 1 or 2, characterized in that the Co-based alloy powder is irradiated with an electron beam and sintered and melted to be molded into a near-net shape by the additive manufacturing method, and then finished to be formed.

4. 4. The machine part according to claim 1, characterized in that it is made of a blade.

Citation Information

Patent Citations

  • Production of cutlery and cutlery obtained by the same

    JP1999106801A

  • Machine component

    JP2015190004A

  • Metal powder for molding

    JP2016102229A

  • Co-BASED ALLOY POWDER FOR ELECTRON BEAM LAMINATION MOLDING

    JP2019014920A

  • Mechanical component

    JP2019014921A