Method for producing rubber composition and method for producing tire

The method for producing a rubber composition in an intermeshing type closed kneader with controlled ram positioning and PID-controlled rotor speed addresses the inefficiencies of intermeshing kneaders, achieving improved silica dispersion and wet road braking performance by maintaining high fill factor and controlled temperature conditions.

JP7572232B2Active Publication Date: 2024-10-23TOYO TIRE CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020211132
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-21
Publication Date
2024-10-23
Estimated Expiration
2040-12-21

AI Technical Summary

Technical Problem

Intermeshing type closed kneaders have inferior biting properties and efficiency in incorporating ingredients compared to tangential type closed kneaders, leading to reduced productivity and silica dispersion efficiency, while lowering the fill factor to improve uptake efficiency results in decreased productivity.

Method used

A method for producing a rubber composition using an intermeshing type closed kneader with controlled ram positioning and PID-controlled rotor speed to maintain a high fill factor, applying shear and elongation deformations, and controlling kneading temperature to suppress coupling reactions, ensuring efficient silica dispersion.

Benefits of technology

Improves silica dispersion and wet road braking performance by maintaining high fill factor and controlled temperature conditions, reducing Black Incorporation Time (BIT) and enhancing kneading efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572232000002
    Figure 0007572232000002
  • Figure 0007572232000001
    Figure 0007572232000001
Patent Text Reader

Abstract

To provide a method for producing rubber composition in which, when using a meshing type closed kneader, it is possible to knead with a high fill factor (for example, a fill factor substantially the same level as the fill factor adopted in tangential type closed kneader).SOLUTION: The method for producing rubber composition of the present invention includes a process of kneading at least rubber, silica and silane coupling agent with a meshing type closed kneader 1, and, at the early part of the process, a first stage of performing the kneading with an increase in kneading temperature is included, and, in the first stage, kneading is performed while the ram 7 is maintained at a first position above the lowest position of the movable range of the ram 7, and, in the first stage, the effective volume when the ram 7 is in the first position is 105% to 120% for the effective volume of 100% when the ram 7 is in the lowest position.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a rubber composition and a method for producing a tire. [Background technology]

[0002] It is known that in order to prepare a rubber composition in which silica is dispersed, silica, a silane coupling agent, rubber, etc. are kneaded in a tangential internal mixer or an intermeshing internal mixer. A tangential internal mixer is designed so that the rotation circles of the two rotors do not overlap, and a shearing action occurs between the rotors and the wall of the casing. On the other hand, an intermeshing internal mixer is designed so that the rotation circles of the two rotors overlap, and a shearing action occurs not only between the rotors and the wall of the casing, but also between the rotors.

[0003] During kneading, the temperature of the dough, i.e., the kneading temperature, rises due to the shearing action. If the temperature becomes too high, for example, gel may form, so it is necessary to knead the dough so that the temperature does not become too high (see, for example, Patent Document 1).

[0004] An intermeshing internal mixer used for mixing generally has better cooling performance than a tangential internal mixer, and can effectively suppress temperature rise.

[0005] However, the intermeshing internal mixer generally has inferior intermeshing properties compared to the tangential internal mixer, i.e., the intermeshing internal mixer generally has poor efficiency in taking in the compounding ingredients. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2020-100116 A Summary of the Invention [Problem to be solved by the invention]

[0007] If the fill factor were lowered to increase the intake efficiency, the amount of materials (i.e. compounding agents and rubber) input would decrease, which would decrease productivity. Also, if the fill factor was not lowered, the amount of compounding agents and rubber placed on the ram would increase, which would result in a decrease in the intake efficiency of the compounding agents.

[0008] An object of the present invention is to provide a method for producing a rubber composition that can be kneaded with a high fill factor (e.g., a fill factor substantially the same as the fill factor employed in a tangential internal kneader) when using an intermeshing internal kneader. [Means for solving the problem]

[0009] In order to solve this problem, the method for producing a rubber composition of the present invention includes the steps of: The method includes a step of kneading at least rubber, silica, and a silane coupling agent in an intermeshing internal mixer including a casing, at least two rotors capable of rotating within the casing, a neck portion located above the rotors, and a ram capable of moving up and down in a space within the neck portion, At an early stage of the process, the process includes a first stage of kneading accompanied by an increase in kneading temperature, In the first stage, kneading is performed while the ram is maintained at a first position that is higher than the lowest position within the movable range of the ram, When the volume of the space enclosed by the ram and the casing when the ram is in the lowest position is defined as a first effective volume, and when the volume of the space enclosed by the ram and the casing when the ram is in the first position is defined as a second effective volume, in the first stage, the second effective volume is 105% to 120% of the first effective volume (100%).

[0010] According to the present invention, by kneading with an intermeshing internal mixer, it is possible to impart shear deformation and elongation deformation to the kneaded dough between the rotors.

[0011] Moreover, in the present invention, by performing kneading while maintaining the ram in the first position (i.e., a position higher than the lowest position) in the first stage of the initial stage (i.e., the stage in which kneading is accompanied by an increase in kneading temperature), it is possible to prevent the materials (i.e., compounding ingredients and rubber) from landing on the ram, and therefore it is possible to knead with a high fill factor (for example, a fill factor that is substantially the same as or higher than the fill factor employed in a tangential internal kneader).

[0012] Moreover, in the present invention, since the materials (i.e., compounding agents and rubber) can be prevented from getting on the ram, the incorporation efficiency of the compounding agents can be improved. In other words, the Black Incorporation Time (hereinafter sometimes referred to as "BIT") can be shortened. As a result, the kneading time for dispersing silica can be secured, and the silica dispersion can be improved. Therefore, the low heat generation property and the braking performance on wet road surfaces (hereinafter referred to as "wet road braking performance") can be improved.

[0013] Moreover, in the present invention, the second effective volume (i.e., the volume of the space surrounded by the ram and the casing when the ram is in the first position) is 105% or more of the first effective volume (i.e., the volume of the space surrounded by the ram and the casing when the ram is in the lowest position), which is 100%, so that the material (i.e., the compounding agent and rubber) can be effectively prevented from getting on the ram, and the intake efficiency of the compounding agent can be further improved. In other words, the BIT can be further shortened.

[0014] Furthermore, in the present invention, since the second effective volume (i.e., the volume of the space when the ram is in the first position) is 120% or less of the first effective volume (i.e., the volume of the space when the ram is in the lowest position), which is 100%, shear can be effectively applied to the kneaded dough, and therefore the kneading temperature can be increased without any problems in the first stage (i.e., the stage in which kneading is performed accompanied by an increase in the kneading temperature).

[0015] The method for producing a rubber composition of the present invention preferably has the following features. The process includes, after the first stage, a second stage in which kneading is performed while controlling the kneading temperature so as to suppress a coupling reaction between the silica and the silane coupling agent, and in the second stage, the rotation speed of the rotor is controlled by PID control to set the kneading temperature to a target temperature; In the second stage, mixing is performed while maintaining the ram at the first position, In the second stage, the second effective volume is also 105% to 120% with respect to the first effective volume being 100%.

[0016] According to this configuration, the mixing temperature is controlled to suppress the coupling reaction, so that the silica can be effectively dispersed before the coupling reaction actively proceeds. As a result, the low heat generation and the braking performance on wet roads (wet road braking performance) can be further improved.

[0017] Moreover, since the second effective volume (i.e., the volume of the space when the ram is in the first position) in the second stage is 105% or more of the first effective volume (i.e., the volume of the space when the ram is in the lowest position) which is 100%, the kneading temperature can be easily maintained. This will be explained. If the ram were in the lowest position in the second stage, the temperature would easily rise due to large shear heat generation. In contrast, in the present invention, since the second effective volume (i.e., the volume of the space when the ram is in the first position) is 105% or more of the first effective volume (i.e., the volume of the space when the ram is in the lowest position) which is 100%, that is, since the ram is appropriately positioned, it is possible to prevent the shear heat from becoming excessively large, and the kneading temperature can be easily maintained at the target temperature.

[0018] Moreover, the kneading temperature can be maintained without problems because the second effective volume (i.e., the volume of the space when the ram is in the first position) in the second stage is 120% or less of the first effective volume (i.e., the volume of the space when the ram is in the lowest position) of 100%. This will be explained. If the ram is located too high in the second stage, the shear heat generation will be excessively small. In contrast, in the present invention, the second effective volume (i.e., the volume of the space when the ram is in the first position) is 120% or less of the first effective volume (i.e., the volume of the space when the ram is in the lowest position) of 100%, that is, the ram is located appropriately, so that it is possible to prevent the shear heat generation from being excessively small, and therefore the kneading temperature can be maintained at the target temperature without problems.

[0019] The method for producing a tire of the present invention includes a step of producing a rubber composition by the method for producing a rubber composition of the present invention, and a step of producing an unvulcanized tire using the rubber composition. [Brief description of the drawings]

[0020] [Figure 1]FIG. 2 is a conceptual diagram showing the configuration of an intermeshing internal mixer that can be used in the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, an embodiment of the present invention will be described.

[0022] In this specification, all concepts such as "first" and "second" are described only for the purpose of distinguishing one thing from another, and do not indicate or suggest a relative order or technique.

[0023] <1. Intermeshing type internal mixer> First, an internal intermeshing mixer that can be used in this embodiment will be described.

[0024] As shown in FIG. 1, the intermeshing-type closed-type kneader 1 comprises a casing 2, two rotors 3 capable of rotating within the casing 2, a neck portion 5 located above the rotors 3, an inlet 6 provided in the neck portion 5, a ram 7 capable of moving up and down in the space within the neck portion 5, and a drop door 9 capable of closing a discharge outlet provided in the casing 2.

[0025] An opening 2a is provided in the center of the top surface of the casing 2. A neck portion 5 having a cylindrical space therein is provided above the opening 2a. An inlet 6 through which rubber and compounding ingredients can be added is provided on the side of the neck portion 5. Two or more inlets 6 may be provided. The rubber and compounding ingredients added from the inlet 6 pass through the cylindrical space of the neck portion 5 and are added into the casing 2 from the opening 2a of the casing 2.

[0026] The ram 7 is shaped so as to be able to close the opening 2a of the casing 2. The ram 7 can move up and down in the cylindrical space of the neck portion 5 by means of a shaft 8 connected to the upper end of the ram 7. The ram 7 can press and apply pressure to the dough present in the casing 2 by means of its own weight or the pressing force from the shaft 8.

[0027] The drop door 9 can be opened and closed. During kneading, the drop door 9 is closed. That is, during kneading, the drop door 9 blocks the discharge port provided in the casing 2. After kneading is completed, the drop door 9 is opened.

[0028] The rotation speed of a motor (not shown) that rotates the rotor 3 is adjusted based on a control signal from the control unit 11. The control unit 11 controls the rotation speed of the motor based on temperature information (specifically, the measured temperature Tp) in the kneading chamber 4 sent from the temperature sensor 13. The rotation speed of the motor can be freely changed by the control unit 11. The motor can be, for example, an inverter motor.

[0029] In order to determine the rotation speed of the motor, the PID calculation processor provided inside the control unit 11 performs proportional (P), integral (I) and differential (D) calculations based on the deviation between the actual temperature Tp in the kneading chamber 4 detected by the temperature sensor 13 and the target temperature Ts. Specifically, the PID calculation processor determines the rotation speed of the motor based on the sum of the control amounts obtained by the proportional (P) operation that calculates a control amount proportional to the difference (deviation e) between the actual temperature Tp and the target temperature Ts, the integral (I) operation that calculates a control amount from an integral value obtained by integrating the deviation e in the time axis direction, and the differential (D) operation that calculates a control amount from the gradient of the change in the deviation e, i.e., the differential value. Note that PID is an abbreviation for Proportional Integral Differential.

[0030] The intermeshing internal mixer 1 is designed so that the two rotors 3 are intermeshed with each other. In other words, the rotation circles of the two rotors 3, more precisely, the rotation circles drawn by the outermost parts of the two rotors 3, are designed so as to overlap. Here, the outermost part is the part farthest from the rotation axis of the rotor 3. Therefore, in the intermeshing internal mixer 1, not only is a shear action applied between the rotor 3 and the wall surface of the casing 2, but also a shear action applies between the rotors 3. In other words, not only can the kneaded dough be subjected to shear deformation or elongation deformation between the rotor 3 and the wall surface of the casing 2, but also the kneaded dough can be subjected to shear deformation or elongation deformation between the rotors 3.

[0031] <2. Each step in the method for producing rubber composition> Next, some of the steps included in the method for producing the rubber composition in this embodiment will be described.

[0032] The method for producing a rubber composition in this embodiment includes a step of kneading at least rubber, silica, and a silane coupling agent in an intermeshing internal mixer 1 to prepare a rubber mixture (hereinafter referred to as "step S1"), and a step of kneading at least a rubber mixture and vulcanization compounding agents to obtain a rubber composition (hereinafter referred to as "step S2"). According to this embodiment, by kneading with the intermeshing internal mixer 1 in step S1, the kneaded dough can be subjected to shear deformation and elongation deformation between the rotors 3. Therefore, as described later, kneading can be performed in a state in which the ram 7 is maintained at a first position above the lowest position of the movable range of the ram 7 (if kneading is performed using a tangential internal mixer with the ram maintained at a position above the lowest position of the ram, the kneaded dough will remain on the rotor, and it is difficult to knead in such a state). In addition, the kneaded dough can also be effectively cooled.

[0033] <2.1. Step S1 (step of preparing rubber mixture)> Step S1 includes a stage of kneading accompanied by an increase in the kneading temperature (hereinafter referred to as the "first stage"), a stage of kneading while controlling the kneading temperature so as to suppress the coupling reaction of the silica and the silane coupling agent (hereinafter referred to as the "second stage"), a stage of kneading accompanied by a further increase in the kneading temperature (hereinafter referred to as the "third stage"), and a stage of kneading while controlling the kneading temperature so as to promote the coupling reaction (hereinafter referred to as the "fourth stage").

[0034] The first to fourth stages constitute one kneading stage. The kneading stage is a cycle from the input of materials to the interlocking internal mixer 1 to the discharge of materials. Therefore, when moving from the first stage to the second stage, materials such as rubber, silica, and silane coupling agent are not discharged from the interlocking internal mixer 1, and when moving from the second stage to the third stage, and when moving from the third stage to the fourth stage, materials are not discharged.

[0035] In step S1, the fill factor is preferably 68% or more, and more preferably 70% or more. According to this embodiment, as described below, since it is possible to prevent the materials (i.e., compounding agents and rubber) from landing on the ram 7, kneading can be performed with a fill factor of 68% or more. The fill factor in step S1 is preferably 80% or less, and more preferably 78% or less. If it is 80% or less, silica can be easily dispersed.

[0036] The fill factor is calculated using the following formula: Fill factor = (volume of rubber mixture / first effective volume) x 100 In this formula, the volume of the rubber mixture is the volume of the rubber mixture discharged from the intermeshing internal mixer 1. The first effective volume, as described below, is the volume of the space surrounded by the ram 7 and the casing 2 when the ram 7 is at the lowest position. In this formula, both the volume of the rubber mixture and the first effective volume can be expressed in liters (L).

[0037] In step S1, the ram 7 may be moved up and down at any timing for cleaning (for example, to remove compounding agents or rubber on the ram 7). For example, the ram 7 may be moved up and down when moving from the first stage to the second stage, the ram 7 may be moved up and down when moving from the second stage to the third stage, or the ram 7 may be moved up and down when moving from the third stage to the fourth stage. The ram 7 may be moved up and down at any timing in any stage (for example, the first stage).

[0038] <2.1.1. First stage (stage in which kneading is performed with an increase in kneading temperature)> In the first stage, at least rubber, silica, and a silane coupling agent are charged into the intermeshing internal mixer 1 and mixed. The mixing in the first stage is accompanied by an increase in the mixing temperature due to shear heat.

[0039] Examples of rubber include natural rubber, polyisoprene rubber, styrene butadiene rubber (SBR), polybutadiene rubber (BR), nitrile rubber, and chloroprene rubber. Any one or any combination of these may be selected and used. The rubber is preferably a diene rubber.

[0040] Modified rubber may be used as the rubber. Examples of modified rubber include modified SBR and modified BR. The modified rubber may have a functional group containing a heteroatom. The functional group may be introduced to the end of the polymer chain or may be introduced into the polymer chain, but is preferably introduced to the end. Examples of the functional group include amino groups, alkoxyl groups, hydroxyl groups, carboxyl groups, epoxy groups, cyano groups, and halogen groups. Among these, amino groups, alkoxyl groups, hydroxyl groups, and carboxyl groups are preferred. The modified rubber may have at least one of the exemplified functional groups. Examples of the amino group include primary amino groups, secondary amino groups, and tertiary amino groups. Examples of the alkoxyl group include methoxy groups, ethoxy groups, propoxy groups, and butoxy groups. The exemplified functional groups interact with the silanol groups (Si-OH) of silica. Here, the interaction means, for example, chemical bonding or hydrogen bonding by chemical reaction with the silanol groups of silica. The amount of the modified rubber in 100% by mass of the rubber used in the first stage may be 10% by mass or more, 20% by mass or more, or 30% by mass or more. The amount of the modified rubber in 100% by mass of the rubber used in the first stage may be 90% by mass or less, 80% by mass or less, or 70% by mass or less.

[0041] Examples of silica include wet silica and dry silica. Of these, wet silica is preferred. Examples of wet silica include precipitated silica. The specific surface area of ​​silica measured by the nitrogen adsorption method is, for example, 80 m 2 / g or more, 2 / g or more, 2 / g or more, 2 The specific surface area of ​​silica may be, for example, 300 m 2 / g or less, and 2 / g or less, and 2 / g or less, and 2 / g or less. Here, the specific surface area of ​​silica is measured in accordance with the multipoint nitrogen adsorption method (BET method) described in JIS K-6430.

[0042] In the first stage, the amount of silica is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, even more preferably 50 parts by mass or more, even more preferably 70 parts by mass or more, and even more preferably 80 parts by mass or more, based on 100 parts by mass of rubber. The amount of silica is preferably 150 parts by mass or less, more preferably 140 parts by mass or less, even more preferably 130 parts by mass or less, and even more preferably 120 parts by mass or less, based on 100 parts by mass of rubber.

[0043] Examples of the silane coupling agent include sulfide silanes such as bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, and bis(2-trimethoxysilylethyl)disulfide; mercaptosilanes such as γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, mercaptopropylmethyldimethoxysilane, mercaptopropyldimethylmethoxysilane, and mercaptoethyltriethoxysilane; and protected mercaptosilanes such as 3-octanoylthio-1-propyltriethoxysilane and 3-propionylthiopropyltrimethoxysilane. One or any combination of these may be selected and used.

[0044] In the first stage, the amount of the silane coupling agent is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the amount of the silane coupling agent is, for example, 20 parts by mass or 15 parts by mass, based on 100 parts by mass of silica.

[0045] In the first stage, rubber, silica, and a silane coupling agent can be kneaded with carbon black, an antioxidant, stearic acid, wax, zinc oxide, oil, etc. Any one or any combination of these can be selected and used.

[0046] As the carbon black, for example, furnace black such as SAF, ISAF, HAF, FEF, GPF, etc., as well as conductive carbon black such as acetylene black and ketjen black, etc., can be used. The carbon black may be granulated carbon black, which is granulated in consideration of its handling properties, or may be ungranulated carbon black. One or more of these may be used.

[0047] Examples of the antiaging agent include aromatic amine-based antiaging agents, amine-ketone-based antiaging agents, monophenol-based antiaging agents, bisphenol-based antiaging agents, polyphenol-based antiaging agents, dithiocarbamate-based antiaging agents, thiourea-based antiaging agents, etc. The antiaging agent may be used alone or in any combination selected from these.

[0048] In the first stage, mixing is performed with the ram 7 maintained at a first position above the lowest position within the movable range of the ram 7. This makes it possible to prevent the materials (i.e., compounding agents and rubber) from landing on the ram 7, and therefore allows mixing with a high fill factor (e.g., a fill factor substantially equal to or higher than the fill factor employed in a tangential closed-type mixer). Moreover, since the materials (i.e., compounding agents and rubber) are prevented from landing on the ram 7, the intake efficiency of the compounding agents can be improved. In other words, the BIT can be shortened. As a result, mixing time for silica dispersion can be secured, and therefore silica dispersion can be improved. Therefore, low heat generation and wet road braking performance can be improved.

[0049] When the volume of the space surrounded by the ram 7 and the casing 2 when the ram 7 is at the lowest position is defined as the first effective volume, and when the volume of the space surrounded by the ram 7 and the casing 2 when the ram 7 is at the first position is defined as the second effective volume, in the first stage, the second effective volume is 105% or more, preferably 108% or more, more preferably 110% or more, even more preferably 112% or more, and even more preferably 114% or more, with respect to the first effective volume being 100%. By being 105% or more, it is possible to effectively prevent the material (i.e., the compounding agent and rubber) from getting on top of the ram 7, so that the efficiency of taking in the compounding agent can be further improved. In other words, the BIT can be further shortened.

[0050] In the first stage, the second effective volume is 120% or less, preferably 119% or less, and more preferably 118% or less, relative to 100% of the first effective volume. By being 120% or less, shear can be effectively applied to the kneaded dough, so that the kneading temperature can be increased without any problems in the first stage (i.e., the stage in which kneading is performed with an increase in the kneading temperature).

[0051] Here, the first and second “effective volumes” are the volumes of the spaces enclosed by the ram 7 and the casing 2. These effective volumes are not values ​​obtained by subtracting the volume of the rotor 3 from the volume of the spaces enclosed by the ram 7 and the casing 2.

[0052] The description of the fill factor in the first stage is omitted because it overlaps with the description of the fill factor in the step S1 described above. Therefore, the description of the fill factor in the step S1 can also be used as the description of the fill factor in the first stage.

[0053] <2.1.2. Second step (a step of kneading so as to suppress the coupling reaction)> In the second stage, the mixing temperature is controlled to suppress the coupling reaction (the reaction between silica and the silane coupling agent). This allows the silica to be effectively dispersed before the coupling reaction actively progresses. As a result, the low heat generation and braking performance on wet roads can be further improved.

[0054] In the second stage, the kneading temperature is kept constant. "Kneading temperature is kept constant" includes keeping the kneading temperature within a certain range. In the second stage, specifically, kneading is performed so that the measured temperature Tp is kept at the target temperature Ts. At this time, the measured temperature Tp can be kept within ±5°C of the target temperature Ts. The target temperature Ts may be less than 140°C, 138°C or less, 135°C or less, 132°C or less, or 130°C or less. The target temperature Ts is preferably 100°C or more, more preferably 110°C or more, even more preferably 115°C or more, and even more preferably 120°C or more. If it is too low, it tends to take a long time to disperse the silica. The target temperature Ts can be appropriately set in consideration of the formulation, particularly the type of silane coupling agent.

[0055] In the second stage, the mixture is kneaded for 10 seconds or more so that the kneading temperature is maintained within a certain range. This is preferably 20 seconds or more, more preferably 30 seconds or more, even more preferably 40 seconds or more, and even more preferably 50 seconds or more. This may be 1000 seconds or less, 800 seconds or less, 600 seconds or less, 400 seconds or less, 200 seconds or less, or 100 seconds or less.

[0056] The kneading temperature is maintained by adjusting the rotation speed of the rotor 3. Specifically, the kneading temperature is maintained by adjusting the rotation speed of the rotor 3 by PID control. Here, the rotation speed of the rotor 3 is adjusted by PID control so as to set the actual temperature Tp to the target temperature Ts. The PID control may be started from the beginning of kneading, or may be started when the actual temperature Tp reaches a predetermined temperature.

[0057] In the second stage, kneading is also performed while the ram 7 is maintained at the first position, which is higher than the lowest position within the movable range of the ram 7.

[0058] In the second stage, the second effective volume (i.e., the volume of the space surrounded by the ram 7 and the casing 2 when the ram 7 is in the first position) is preferably 105% or more, more preferably 108% or more, even more preferably 110% or more, even more preferably 112% or more, and even more preferably 114% or more, relative to 100% of the first effective volume (i.e., the volume of the space surrounded by the ram 7 and the casing 2 when the ram 7 is in the lowest position). By being 105% or more, the kneading temperature can be easily maintained. This will be explained. If the ram 7 is in the lowest position in the second stage, the shear heat is large, which easily leads to a temperature rise. In contrast, in this embodiment, by the second effective volume being 105% or more relative to 100% of the first effective volume, that is, by the ram 7 being appropriately positioned, it is possible to prevent the shear heat from becoming excessively large, and therefore the kneading temperature can be easily maintained at the target temperature Ts.

[0059] In the second stage, the second effective volume is preferably 120% or less, more preferably 119% or less, and even more preferably 118% or less, relative to 100% of the first effective volume. By being 120% or less, the kneading temperature can be maintained without any problems. This will be explained. If the ram 7 is located excessively high in the second stage, the shear heat generation will be excessively small. In contrast, in this embodiment, the second effective volume is 120% or less, relative to 100% of the first effective volume, that is, the ram 7 is appropriately positioned, so that the shear heat generation can be prevented from being excessively small, and the kneading temperature can be maintained at the target temperature Ts without any problems.

[0060] It should be noted that the second effective volume of the second stage does not have to be the same as the second effective volume of the first stage, i.e., the second effective volume of the second stage may be the same as the second effective volume of the first stage or may be different.

[0061] <2.1.3. Third stage (stage in which kneading is performed with further increase in kneading temperature)> In the third stage, kneading is performed with a further increase in the kneading temperature. In the third stage, the kneading temperature is increased to a temperature (e.g., 140°C or higher) at which the coupling reaction actively proceeds. Specifically, the kneading temperature is increased to the target temperature Ts for the fourth stage.

[0062] In the third stage, kneading may be performed while maintaining ram 7 at the lowest position within the range of movement of ram 7, or kneading may be performed while maintaining ram 7 at a first position above the lowest position of ram 7.

[0063] <2.1.4. Fourth step (mixing step to promote the coupling reaction)> In the fourth stage, the mixing temperature is controlled to promote the coupling reaction (the reaction between silica and the silane coupling agent). This allows the coupling reaction to proceed actively, increasing the efficiency of the coupling reaction, and as a result, effectively reducing the cohesive force of the silica. This effectively increases the dispersion of the silica, improving the low heat generation and wet road braking of the tire.

[0064] In the fourth stage, kneading may be performed while maintaining ram 7 at the lowest position within the range of movement of ram 7, or kneading may be performed while maintaining ram 7 at a first position above the lowest position of ram 7.

[0065] In the fourth stage, the kneading is performed so that the kneading temperature is kept constant. "Kneading temperature is kept constant" includes keeping the kneading temperature within a certain range. In the fourth stage, specifically, kneading is performed so that the measured temperature Tp is kept at the target temperature Ts. At this time, the measured temperature Tp can be kept within ±5°C of the target temperature Ts. The target temperature Ts may be 140°C or higher, 142°C or higher, 145°C or higher, 148°C or higher, or 150°C or higher. If this is too low, it tends to take too much time to proceed with the coupling reaction. The target temperature Ts is preferably 170°C or lower, more preferably 165°C or lower, even more preferably 160°C or lower, even more preferably 155°C or lower, and even more preferably 153°C or lower. If this is too high, gel may be generated.

[0066] In the fourth stage, the mixture is kneaded for 20 seconds or more so that the kneading temperature is kept within a certain range. This is preferably 40 seconds or more, more preferably 60 seconds or more, even more preferably 80 seconds or more, and even more preferably 100 seconds or more. This may be 2000 seconds or less, 1500 seconds or less, 1000 seconds or less, 500 seconds or less, 300 seconds or less, or 200 seconds or less.

[0067] The kneading temperature is maintained by adjusting the rotation speed of the rotor 3, in the same manner as in the second stage.

[0068] Thereafter, if necessary, mixing is continued until the temperature reaches a predetermined discharge temperature, and then the drop door 9 is opened to discharge the rubber mixture.

[0069] <2.1.5.Other> If necessary, the rubber mixture can be further kneaded, i.e., re-kneaded, to improve the dispersibility of the silica and / or reduce the Mooney viscosity.

[0070] By the above procedure, a rubber mixture can be obtained.

[0071] <2.2. Step S2 (Step of kneading the rubber mixture and the vulcanization compounding ingredients to obtain a rubber composition)> In step S2, at least the rubber mixture and the vulcanization compounding agents are kneaded to obtain a rubber composition. Examples of the vulcanization compounding agents include sulfur, organic peroxides and other vulcanizing agents, vulcanization accelerators, vulcanization accelerator assistants, and vulcanization retarders. The vulcanization compounding agents can be selected from these, or any combination thereof. Examples of sulfur include powdered sulfur, precipitated sulfur, insoluble sulfur, and highly dispersible sulfur. The sulfur can be selected from these, or any combination thereof. Examples of the vulcanization accelerator include sulfenamide-based vulcanization accelerators, thiuram-based vulcanization accelerators, thiazole-based vulcanization accelerators, thiourea-based vulcanization accelerators, guanidine-based vulcanization accelerators, and dithiocarbamate-based vulcanization accelerators. The vulcanization accelerator can be selected from these, or any combination thereof. The kneading can be performed with a kneading machine. Examples of the kneading machine include an internal kneading machine and an open roll. Examples of the internal mixer include an intermeshing internal mixer and a tangential internal mixer.

[0072] In the rubber composition, the amount of silica is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, even more preferably 50 parts by mass or more, even more preferably 70 parts by mass or more, and even more preferably 80 parts by mass or more, based on 100 parts by mass of rubber. The amount of silica is preferably 150 parts by mass or less, more preferably 140 parts by mass or less, even more preferably 130 parts by mass or less, and even more preferably 120 parts by mass or less, based on 100 parts by mass of rubber.

[0073] In the rubber composition, the amount of the silane coupling agent is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and further preferably 5 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the amount of the silane coupling agent is, for example, 20 parts by mass or 15 parts by mass based on 100 parts by mass of silica.

[0074] The rubber composition may further include carbon black, antioxidants, stearic acid, wax, zinc oxide, oil, sulfur, vulcanization accelerators, etc. The rubber composition may include one or any combination of these. The amount of sulfur is preferably 0.5 to 5 parts by mass in terms of sulfur content per 100 parts by mass of rubber. The amount of vulcanization accelerator is preferably 0.1 to 5 parts by mass per 100 parts by mass of rubber.

[0075] The rubber composition can be used to manufacture tires. Specifically, the rubber composition can be used to manufacture tire components that constitute tires. For example, the rubber composition can be used to manufacture tread rubber, sidewall rubber, chafer rubber, bead filler rubber, etc. The rubber composition can be used to manufacture one or any combination of these tire components.

[0076] <3. Each step in tire manufacturing process> Next, some of the steps included in the tire manufacturing method of the present embodiment will be described. Among these steps, the step of preparing the rubber composition has already been described.

[0077] The tire manufacturing method in this embodiment includes a step of producing an unvulcanized tire using the rubber composition. This step includes producing a tire component including the rubber composition, and producing an unvulcanized tire including the tire component. Examples of the tire component include tread rubber, sidewall rubber, chafer rubber, and bead filler rubber. Among them, tread rubber is preferable.

[0078] The tire manufacturing method of the present embodiment may further include a step of vulcanizing and molding the unvulcanized tire. The tire obtained by the method of the present embodiment may be a pneumatic tire.

[0079] <Various modifications can be made to the above-described embodiment> The above-described embodiment may be modified in various ways. For example, the above-described embodiment may be modified by selecting one or more of the following modifications.

[0080] In the above embodiment, the entire amount of silica is added in the kneading stages including the first stage to the fourth stage. However, the above embodiment is not limited to this configuration. For example, silica may be added in a plurality of kneading stages.

[0081] In the above embodiment, the kneading temperature is controlled in the second stage (i.e., the stage in which kneading is performed so as to suppress the coupling reaction). However, the above embodiment is not limited to this configuration. For example, the kneading temperature does not have to be controlled in the second stage.

[0082] In the above embodiment, a configuration has been described in which kneading is performed while the ram 7 is maintained at the first position (i.e., a position above the lowest position within the movable range of the ram 7) not only in the first stage but also in the second stage (i.e., a stage in which kneading is performed so as to suppress the coupling reaction). However, the above embodiment is not limited to this configuration.

[0083] In the above embodiment, the kneading temperature is controlled in the fourth stage (i.e., the stage where kneading is performed so as to promote the coupling reaction). However, the above embodiment is not limited to this configuration. For example, the kneading temperature does not have to be controlled in the fourth stage.

[0084] In the above embodiment, the rubber mixture and the vulcanization compounding agent are kneaded to obtain the rubber composition. However, the above embodiment is not limited to this configuration. For example, the rubber mixture may be regarded as the rubber composition. EXAMPLES

[0085] The following describes an embodiment of the present invention.

[0086] The raw materials and chemicals used in the examples are as follows. SBR1 "SBR1502" manufactured by JSR SBR2 “SBR1723” (oil content 37.5% by mass) manufactured by JSR NR RSS#3 Carbon black "Seat KH" manufactured by Tokai Carbon Co., Ltd. Silica "VN3" (BET=180m 2 / g) Evonik Oil "Process NC-140" manufactured by JX Nippon Oil & Energy Corporation Silane coupling agent "Si75" manufactured by Degussa Zinc oxide "Zinc oxide type 2" manufactured by Mitsui Mining & Smelting Co., Ltd. Wax "OZOACE0355" manufactured by Nippon Seiro Co., Ltd. Stearic acid "Industrial stearic acid" manufactured by Kao Corporation Sulfur "5% oil-treated powdered sulfur" manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator "Noccela NS-P" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. In Table 1, the parts by mass of SBR2 are shown based on the net rubber amount. That is, when the amount of SBR2 is 30 parts by mass in Table 1, the amount of oil is not included in the 30 parts by mass. In addition, Si75 is a silane coupling agent that hardly reacts with silica at 130°C, but reacts with silica at 150°C.

[0087] Preparation of Unvulcanized Rubber in Comparative Example 1 According to Table 1, rubber and compounding ingredients were put into a tangential internal mixer, mixed without PID control, and the mixture was discharged at 160°C. During this mixing, the ram was kept at the lowest position except for the up and down movement of the ram for cleaning. The mixture was mixed with sulfur and a vulcanization accelerator to obtain unvulcanized rubber.

[0088] Preparation of Unvulcanized Rubber in Comparative Example 2 According to Table 1, rubber and compounding ingredients were put into an intermeshing internal mixer, mixed without PID control, and the mixture was discharged at 160°C. During this mixing, the ram was kept at the lowest position except for the up and down movement of the ram for cleaning. The mixture was mixed with sulfur and a vulcanization accelerator to obtain unvulcanized rubber.

[0089] Preparation of Unvulcanized Rubber in Comparative Example 3 According to Table 1, rubber and compounding ingredients were put into an intermeshing internal mixer, mixed with two-stage PID control, and the mixture was discharged at 160°C. That is, in the first stage, mixing was performed at a target temperature of 130°C for 60 seconds, and in the second stage, mixing was performed at a target temperature of 150°C for 120 seconds, and the mixture was discharged at 160°C. During this mixing, the ram was kept at the lowest position, except for the up and down movement of the ram for cleaning. The mixture was mixed with sulfur and a vulcanization accelerator to obtain unvulcanized rubber.

[0090] Preparation of Unvulcanized Rubber in Examples 1 and 2 According to Table 1, the rubber and compounding ingredients were put into an intermeshing internal mixer, mixed by two-stage PID control, and the mixture was discharged at 160°C. That is, in the first stage, the mixture was mixed at a target temperature of 130°C for 60 seconds, and in the second stage, the mixture was mixed at a target temperature of 150°C for 120 seconds, and the mixture was discharged at 160°C. During this mixing, the ram was maintained at a position above the lowest position, except for the up and down movement of the ram for cleaning. In other words, the ram-up state was maintained during this mixing. The mixture was mixed with sulfur and a vulcanization accelerator to obtain unvulcanized rubber.

[0091] Preparation of unvulcanized rubber in Example 3 According to Table 1, the rubber and compounding ingredients were put into an intermeshing internal mixer, mixed by two-stage PID control, and the mixture was discharged at 165°C. That is, in the first stage, the mixture was mixed at a target temperature of 120°C for 80 seconds, and in the second stage, the mixture was mixed at a target temperature of 150°C for 120 seconds, and the mixture was discharged at 165°C. During this mixing, the ram was maintained at a position above the lowest position, except for the up and down movement of the ram for cleaning. In other words, the ram-up state was maintained during this mixing. The mixture was mixed with sulfur and a vulcanization accelerator to obtain unvulcanized rubber.

[0092] Preparation of vulcanized rubber The unvulcanized rubber was vulcanized at 150°C for 30 minutes to obtain a vulcanized rubber.

[0093] Black Incorporation Time (BIT) The BIT was determined based on the mixing time and torque.

[0094] Temperature stability in the first stage of control (i.e. primary control) In the first stage of control (i.e., first control), if the actual temperature Tp was maintained within plus or minus 3°C of the target temperature Ts, it was judged as ◎, if it was maintained between plus or minus 3°C and 5°C, it was judged as ◯, and if it was maintained between plus or minus 5°C and 10°C, it was judged as ×.

[0095] Unvulcanized rubber sheet Unvulcanized rubber was formed into a sheet using a roll, and the condition was observed. When there were no breaks in the sheet or air bubbles on the surface of the sheet, it was judged as ◯, when there were no breaks in the sheet but air bubbles on the surface of the sheet, it was judged as △, and when there were both breaks in the sheet and air bubbles on the surface of the sheet, it was judged as ×. The more "◯" it is, the better the dispersibility of silica in the unvulcanized rubber.

[0096] Productivity Productivity is an index related to the amount of waste. The amount of waste in each example is shown in the productivity column of Table 1, with the amount of waste in Comparative Example 1 being set as 100. The larger the index, the more waste there is. In other words, the productivity is superior.

[0097] Low fuel consumption The tan δ of the vulcanized rubber was measured in accordance with JIS K-6394 using a viscoelasticity tester manufactured by Toyo Seiki Seisakusho. The tan δ was measured under the conditions of a frequency of 10 Hz, a dynamic strain of 1.0%, a temperature of 60°C, and a static strain (initial strain) of 10%. The tan δ of each example is shown in Table 1 as an index, with the tan δ of Comparative Example 1 taken as 100. The smaller the index, the lower the tan δ and the better the fuel economy.

[0098] Wet road braking performance The rebound resilience (%) was measured at 23° C. in accordance with JIS K6255 using a Lübke rebound resilience tester. The reciprocal of the rebound resilience in Comparative Example 1 is set as an index of 100, and the reciprocal of each example (the reciprocal of the rebound resilience) is shown in Table 1. The higher the index, the better the wet road braking performance.

[0099] [Table 1]

[0100] In Table 1, the two-stage PID control means that the PID control is started when the measured temperature reaches the target temperature. In this PID control, the rotation speed of the rotor is controlled.

[0101] By adopting a fill factor smaller than that used in the tangential internal mixer as the fill factor when kneading with the intermeshing internal mixer, the BIT when kneading with the intermeshing internal mixer became roughly the same as that of the tangential internal mixer (see Comparative Examples 1 and 2).

[0102] When kneading was performed with a fill factor substantially equivalent to that employed in a tangential closed-type kneader, the BIT could be shortened by kneading in the ram-up state (see Comparative Example 3 and Examples 1 to 3). In addition, the state of the unvulcanized rubber sheet could be improved by kneading in the ram-up state (see Comparative Example 3 and Examples 1 to 3). In other words, the dispersibility of silica could be improved. Furthermore, the low heat generation and wet road braking properties could be improved by kneading in the ram-up state (see Comparative Example 3 and Examples 1 to 3). [Explanation of symbols]

[0103] Reference Signs List 1: Intermeshing internal mixer, 2: Casing, 2a: Opening, 3: Rotor, 4: Mixing chamber, 5: Neck, 6: Feeding port, 7: Ram, 8: Shaft, 9: Drop door, 11: Control unit, 13: Temperature sensor

Claims

1. The method includes a step of kneading at least rubber, carbon black, silica, and a silane coupling agent in an intermeshing internal mixer including a casing, at least two rotors capable of rotating within the casing, a neck portion located above the rotors, and a ram capable of moving up and down in a space within the neck portion, Prior to the Black Incorporation Time, the process includes a first stage of compounding with an increased compounding temperature; In the first stage, kneading is performed while maintaining the ram at a first position that is higher than the lowest position within the movable range of the ram, When the volume of the space surrounded by the ram and the casing when the ram is at the lowest position is defined as a first effective volume, and when the volume of the space surrounded by the ram and the casing when the ram is at the first position is defined as a second effective volume, in the first stage, the second effective volume is 105% to 120% with respect to the first effective volume being 100%. A method for producing a rubber composition.

2. The process includes, after the first stage, a second stage in which kneading is performed while controlling the kneading temperature so as to suppress a coupling reaction between the silica and the silane coupling agent, and in the second stage, the rotation speed of the rotor is controlled by PID control to set the kneading temperature to a target temperature; In the second stage, mixing is performed while maintaining the ram at the first position, In the second stage, the second effective volume is 105% to 120% of the first effective volume (100%). A method for producing the rubber composition according to claim 1.

3. A step of preparing a rubber composition by the method for producing a rubber composition according to claim 1 or 2; and producing an unvulcanized tire using the rubber composition. A method for manufacturing tires.

Citation Information

Patent Citations

  • Method and device for kneading rubber material

    JP2018034472A

  • Method of producing rubber composition for tire

    JP2018123193A

  • Rubber composition with improved hysteresis loss, vulcanizate and manufacturing method of rubber composition

    JP2018123225A

  • Method and apparatus for kneading rubber material

    JP2019093585A

  • Rubber kneading method

    JP2019112525A