Laminates consisting of metal and a polymer interlayer made of thermoplastic polyurethane
The laminate with a thermoplastic polyurethane polymer composition addresses the issues of tensile strength and moisture absorption in existing laminates, ensuring stability and improved mechanical properties in humid environments.
Patent Information
- Application Number
- JP2021514376
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-14
- Filing Date
- 2019-09-11
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2039-09-11
AI Technical Summary
Existing laminates for aircraft, automobile, and ship construction exhibit poor tensile strength and varying moisture absorption properties, leading to inconsistent binding and mechanical instability, especially in humid environments.
A laminate comprising at least one metal layer and a polymer composition made of thermoplastic polyurethane (TPU), which includes polyether polyol, polyisocyanate, and C2-C20 polyol, providing improved elastic modulus and release properties.
The laminate demonstrates enhanced tensile strength and stability, maintaining mechanical properties even in humid conditions, with a preferred elastic modulus range of 800 to 1400 MPa.
Smart Images

Figure 0007572354000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate comprising at least one first layer of at least one first metal and at least one further layer of a polymer composition (PC), as well as to a method for producing the laminate of the invention. [Background technology]
[0002] A problem frequently encountered these days is to provide new materials, especially for aircraft construction, automobile manufacturing and ship construction, which are lighter than the materials used up to now. At the same time, these new materials will have the same mechanical properties, especially strength, stiffness and stability, as known materials, or even improve these mechanical properties. The new materials will be formable by known methods, such as deep drawing, rolling, bending, punching or seaming.
[0003] WO2005 / 014278 describes a laminate comprising an adhesive polymer layer between two metal outer layers. The polymer layer comprises nylon-6, nylon-6,6, nylon-11, nylon-12, nylon-4,6, nylon-6,10 or nylon-6,12, and copolymers of ethylene and unsaturated carboxylic acids and / or carboxylic acid derivatives, and reactive copolymers. The copolymers of ethylene and unsaturated carboxylic acids and / or carboxylic acid derivatives may be grafted with polar groups.
[0004] A particular disadvantage of the laminates described in WO2005 / 014278 is that they have poor tensile strength after storage in a humid environment. Furthermore, the polymer layers often have variable moisture absorption, resulting in variable bonding properties.
[0005] US 2011 / 0200816 describes a laminate that includes two metal layers and a polymer layer sandwiched between them. The polymer layer includes, for example, nylon-6 / 6,6 copolymer. Also described are a variety of other thermoplastic polymers, such as polyolefins and polyimides. The laminate described in US 2011 / 0200816 also exhibits poor tensile strength, especially after storage in humid environments, or can even be destroyed by atmospheric humidity to the point of being unusable.
[0006] DE 10 2011 084519 describes a sealing layer for solar cells, which comprises a first outer layer, an intermediate layer and a second outer layer. These layers may comprise polyamide, for example nylon-6 or nylon-6,6. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] WO2005 / 014278 [Patent Document 2] US Patent Application Publication No. 2011 / 0200816 [Patent Document 3] German Patent No. 10 2011 084519 Summary of the Invention [Problem to be solved by the invention]
[0008] It is therefore an object of the present invention to provide a laminate, and a method for its production, which has to a reduced extent, if at all, the disadvantages of the laminates described in the prior art. [Means for solving the problem]
[0009] The object is to provide a laminate comprising at least one first layer of at least one first metal and at least one further layer of a polymer composition (PC) comprising at least one thermoplastic polyurethane (TPU), the at least one TPU comprising at least the following components: (A) at least one polyether polyol; (B) at least one polyisocyanate; (C) at least one of C2 to C 20 Polyol and This was achieved by lamination, which can be obtained by polymerizing the above.
[0010] Surprisingly, the laminates of the present invention have been found to have particularly good modulus, and good release properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The invention is described in more detail below.
[0012] laminate According to the invention, the laminate comprises at least one first layer of at least one first metal and at least one further layer of a polymer composition (PC).
[0013] By "at least one first layer" in the context of the present invention is meant either exactly one first layer, or two or more first layers.
[0014] By "at least one first metal" in the context of the present invention is meant either exactly one first metal, or a mixture of two or more first metals.
[0015] By "at least one further layer" in the context of the present invention is meant either exactly one further layer or two or more further layers.
[0016] The laminate preferably additionally comprises at least one second layer of at least one second metal, with at least one first layer of at least one first metal being bonded to at least one second layer of at least one second metal via at least one further layer of polymer composition (PC).In such a laminate, the at least one first layer is thus continued to at least one further layer, which in turn is continued to at least one second layer.
[0017] Such laminates comprising at least one first layer, at least one further layer and at least one second layer are also known as "sandwich materials."
[0018] Thus, the present invention also provides a laminate further comprising at least one second layer of at least one second metal, wherein the at least one first layer is bonded to the at least one second layer via at least one further layer.
[0019] The at least one first metal of the at least one first layer may be the same as or different from the at least one second metal of the at least one second layer, and the at least one first metal of the at least one first layer is preferably the same as the at least one second metal of the at least one second layer.
[0020] The laminate comprises at least one first layer of at least one first metal, in other words, the laminate comprises at least one first layer made of at least one first metal.
[0021] The at least one first layer of the at least one first metal has, for example, a thickness in the range of 0.1 to 0.6 mm, preferably in the range of 0.15 to 0.4 mm, particularly preferably in the range of 0.18 to 0.3 mm.
[0022] Thus, the invention also provides a laminate, wherein at least one first layer has a thickness in the range of 0.1 to 0.6 mm.
[0023] The laminate preferably further comprises at least one second layer of at least one second metal, in other words, the laminate preferably further comprises at least one second layer made of at least one second metal.
[0024] The at least one second layer of the at least one second metal has, for example, a thickness in the range of 0.1 to 0.6 mm, preferably in the range of 0.15 to 0.4 mm, particularly preferably in the range of 0.18 to 0.3 mm.
[0025] Thus, the present invention also provides a laminate further comprising at least one second layer of at least one second metal, wherein the at least one second layer has a thickness in the range of 0.1 to 0.6 mm.
[0026] The thickness of the at least one second layer may be the same as or different from the thickness of the at least one first layer, and the thickness of the at least one second layer is preferably the same as the thickness of the at least one first layer.
[0027] Suitable as the at least one first metal of the at least one first layer are any metals and metal alloys known to those skilled in the art that are solid at the manufacturing and use temperatures of the laminate. The at least one first metal of the at least one first layer is preferably selected from the group consisting of iron, aluminum, copper, nickel and magnesium, as well as alloys thereof. The at least one first metal is more preferably an alloy of iron, and the at least one first metal is particularly preferably steel.
[0028] Thus, the present invention also provides a laminate, wherein the at least one first metal of the at least one first layer is selected from the group consisting of iron, aluminum, copper, nickel and magnesium, as well as alloys thereof.
[0029] Thus, the present invention also provides a laminate, wherein the at least one first metal is selected from the group consisting of iron, aluminum, copper, nickel and magnesium, as well as alloys thereof.
[0030] Steel is known to the person skilled in the art. In the context of the present invention, "steel" is understood to mean an alloy containing iron as the main constituent. This corresponds to the definition of steel according to DIN EN 10020:2000-07.
[0031] The at least one first metal may be coated or uncoated. The at least one first metal is preferably coated. Suitable coatings for the at least one first metal are known per se to those skilled in the art, for example adhesion promoter layers, anticorrosive layers, paints, or zinc or magnesium coatings.
[0032] The at least one first metal is preferably zinc-coated. By "zinc-coated" is meant that the at least one first metal is coated with a further metal, in particular with zinc or a zinc alloy.
[0033] It is therefore particularly preferred that the at least one first metal is steel coated with zinc.
[0034] The zinc coating of the at least one first metal can be carried out by methods known to those skilled in the art, for example by hot dip zinc coating or by galvanic zinc coating.
[0035] If the at least one first metal is zinc coated, it may further comprise further coatings, such as adhesion promoter layers and / or paints, as known to those skilled in the art.
[0036] The coating of the at least one first metal may be carried out in any manner known to those skilled in the art, for example the coating may be carried out from an aqueous solution or dispersion.
[0037] The explanations and preferences given above for the at least one first metal of the at least one first layer apply correspondingly to the at least one second metal of the at least one second layer.
[0038] Thus, the present invention also provides a laminate further comprising at least one second layer of at least one second metal, wherein the at least one second metal of the at least one second layer is selected from the group consisting of iron, aluminum, copper, nickel and magnesium, as well as alloys thereof.
[0039] The laminate comprises at least one further layer of a polymer composition (PC), which means, in other words, that at least one further layer consists of a polymer composition (PC).
[0040] The at least one further layer of polymer composition (PC) has for example a thickness in the range from 0.02 to 1.5 mm, preferably in the range from 0.05 to 1 mm, particularly preferably in the range from 0.1 to 0.5 mm.
[0041] The invention therefore also provides a laminate, wherein at least one further layer has a thickness in the range of 0.02 to 1.5 mm.
[0042] The invention further provides a laminate, wherein at least one first layer has a thickness in the range of 0.1 mm to 0.6 mm and / or at least one further layer has a thickness in the range of 0.02 mm to 1.5 mm.
[0043] Polymer Composition (PC) According to the invention, the polymer composition (PC) comprises at least one thermoplastic polyurethane (TPU).
[0044] By "at least one thermoplastic polyurethane (TPU)" in the context of the present invention is meant either exactly one thermoplastic polyurethane (TPU) or a mixture (blend) of two or more thermoplastic polyurethanes (TPUs).
[0045] In addition, the polymer composition (PC) may further comprise at least one further polymer.
[0046] By "at least one further polymer" in the context of the present invention is meant either exactly one further polymer or a mixture (blend) of two or more further polymers.
[0047] Suitable polymers for the at least one further polymer include any further polymer known to a person skilled in the art, provided that the at least one further polymer is different from the at least one thermoplastic polyurethane (TPU).
[0048] The at least one further polymer is preferably selected from the group consisting of polyethylene and copolymers of at least two monomers selected from the group consisting of ethylene, acrylic acid, maleic anhydride, isobutylene, butene, propylene, octene, alkyl acrylates and alkyl methacrylates.
[0049] The present invention therefore also provides a laminate, in which the polymer composition (PC) additionally comprises at least one further polymer selected from the group consisting of polyethylene and copolymers of at least two monomers selected from the group consisting of ethylene, isobutylene, butene, propylene, octene, alkyl acrylates, alkyl methacrylates, acrylic acid and maleic anhydride.
[0050] Alkyl acrylates are known to those skilled in the art and are also referred to as "alkyl acrylate esters". Alkyl acrylates are formed in the reaction of acrylic acid with alkyl alcohols. Preferred according to the invention as alkyl acrylate is n-butyl acrylate.
[0051] Alkyl methacrylates are likewise known to those skilled in the art and are also referred to as "methacrylic acid alkyl esters". Alkyl methacrylates can be obtained, for example, by reaction of methacrylic acid with alkyl alcohols. Alkyl methacrylates can also be substituted, for example. An example of a substituted alkyl methacrylate is 2,3-epoxypropyl methacrylate. 2,3-epoxypropyl methacrylate is also known as "glycidyl methacrylate". Preferably, according to the invention, the alkyl methacrylate is selected from the group consisting of methyl methacrylate and 2,3-epoxypropyl methacrylate.
[0052] In addition, the polymer composition (PC) may additionally comprise at least one filler.
[0053] By "at least one filler" in the context of the present invention is meant either exactly one filler or a mixture of two or more fillers.
[0054] Suitable fillers include all fillers known to those skilled in the art and which may be mixed with components (A), (B) and (C) and optionally with at least one further polymer in the polymer composition (PC).
[0055] Preferably, the at least one filler is selected from the group consisting of inorganic fillers, organic fillers and natural fillers.
[0056] The at least one filler is typically particulate. For example, the at least one filler may be, for example, a fibrous material or may take the form of a sphere. The at least one filler has, for example, an aspect ratio in the range of 1 to 15, preferably in the range of 1 to 10, particularly preferably in the range of 1 to 5. What is meant by "aspect ratio" in the context of the present invention is the ratio of the maximum dimension of the particle of the at least one filler to the minimum dimension of the particle of the at least one filler.
[0057] In the context of the present invention, "fibrous material" is understood to mean all materials which contain fibres, such as individual fibres, fibre bundles (rovings), nonwovens, laid scrims, woven or knitted fabrics.
[0058] Thus, for example, the at least one filler is selected from the group consisting of wollastonite, talc, boron fibrous material, glass fibrous material, carbon fibrous material, silica fibrous material, ceramic fibrous material, basalt fibrous material, metal fibrous material, aramid fibrous material, poly(p-phenylene-2,6-benzobisoxazole) fibrous material, polyester fibrous material, nylon fibrous material, polyethylene fibrous material, wood fibrous material, flax fibrous material, hemp fibrous material, coconut fibrous material and sisal fibrous material.
[0059] It is particularly preferred that the at least one filler is selected from the group consisting of glass fiber materials, carbon fiber materials, aramid fiber materials, poly(p-phenylene-2,6-benzobisoxazole) fiber materials, boron fiber materials, metal fiber materials and potassium titanate fiber materials. It is particularly preferred that the at least one filler is a glass fiber material.
[0060] The polymer composition (PC) preferably does not contain any fillers.
[0061] The polymer composition (PC) comprises, for example, at least one further polymer in a range from 0% to 50% by weight, preferably in the range from 5% to 50% by weight, particularly preferably in the range from 10% to 30% by weight, based on the sum of the mass percentages in each case of the at least one thermoplastic polyurethane (TPU), of the at least one further polymer and optionally of the at least one filler, based on the total mass of the polymer composition (PC).
[0062] The polymer composition (PC) comprises, for example, in the range of 0.1% to 70% by weight of at least one filler, preferably in the range of 0.5% to 60%, particularly preferably in the range of 1% to 50% by weight of at least one filler, based in each case on the sum of the mass percentages of the at least one thermoplastic polyurethane (TPU), of the at least one filler and of any at least one further polymer, based on the total mass of the polymer composition (PC).
[0063] The sum of the weight percentages of the thermoplastic polyurethane (TPU), of any at least one further polymer and any at least one filler, is typically 100 weight %.
[0064] In addition, the polymer composition (PC) may contain additives known to those skilled in the art. The additives that may be present in the polymer composition (PC) are, for example, selected from the group consisting of stabilizers, dyes, antistatic agents, filler oils, surface improvers, drying agents, release aids, release agents, antioxidants, light stabilizers, PVC stabilizers, lubricants, flame retardants, foaming agents, impact modifiers, adhesion promoters, coupling agents and nucleation aids.
[0065] The present invention therefore also provides a laminate, wherein the polymer composition (PC) additionally comprises at least one additive selected from the group consisting of stabilizers, dyes, antistatic agents, filler oils, surface modifiers, drying agents, release aids, release agents, antioxidants, light stabilizers, PVC stabilizers, lubricants, flame retardants, blowing agents, impact modifiers, adhesion promoters, coupling agents and nucleation aids.
[0066] These additives are known per se to those skilled in the art. Coupling agents are also known as "crosslinking agents". In the context of the present invention, "adhesion promoter" is understood to mean an additive that further improves the adhesion of at least one further layer of polymer composition (PC) to at least one first layer and optionally to at least one second layer.
[0067] When the polymer composition (PC) additionally comprises additives, the sum of the mass percentages of the at least one further polymer and of the at least one filler, of the additives, of the thermoplastic polyurethane (TPU) is typically 100% by mass.
[0068] The polymer composition (PC) typically has a modulus of elasticity, determined according to ISO 527-1:2012, in the range of 800 to 1400 MPa, preferably in the range of 900 to 1350 MPa, particularly preferably in the range of 1000 to 1300 MPa.
[0069] Thermoplastic Polyurethane (TPU) According to the invention, the polymer composition (PC) comprises at least the following components: (A) at least one polyether polyol; (B) at least one polyisocyanate; (C) at least one of C2 to C 20 Polyol and The thermoplastic polyurethane may be obtained by polymerizing at least one thermoplastic polyurethane.
[0070] For example, at least one thermoplastic polyurethane (TPU) can be obtained by polymerizing component (A) in the range of 5% to 50% by weight, component (B) in the range of 20% to 80% by weight, and component (C) in the range of 5% to 40% by weight, in each case relative to the sum of the mass percentages of components (A), (B) and (C).
[0071] At least one thermoplastic polyurethane (TPU) is preferably obtainable by polymerizing component (A) in the range of 10% to 40% by weight, component (B) in the range of 40% to 70% by weight, and component (C) in the range of 8% to 30% by weight, relative to the sum of the mass percentages of components (A), (B) and (C) in each case.
[0072] The at least one thermoplastic polyurethane (TPU) is more preferably obtained by polymerizing component (A) in the range of 14% to 35% by weight, component (B) in the range of 50% to 65% by weight, and component (C) in the range of 13% to 24% by weight, based in each case on the total mass percentages of components (A), (B) and (C).
[0073] The present invention therefore also provides a laminate, in which a thermoplastic polyurethane (TPU) is obtainable by polymerizing component (A) in the range of 5% to 50% by weight, component (B) in the range of 20% to 80% by weight and component (C) in the range of 5% to 40% by weight, in each case relative to the sum of the mass percentages of components (A), (B) and (C).
[0074] It will be clear that the mass percentages of components (A), (B) and (C) relate to the mass percentages of components (A), (B) and (C) before polymerization. During polymerization, the mass percentages may possibly change. This is known per se to the person skilled in the art.
[0075] Components (A), (B) and (C) are described in further detail below.
[0076] By "at least one thermoplastic polyurethane (TPU)" in the context of the present invention is meant either exactly one thermoplastic polyurethane (TPU) or a mixture (blend) of two or more thermoplastic polyurethanes (TPUs).
[0077] When the polymer composition (PC) comprises two or more thermoplastic polyurethanes (TPUs), the mixture of two or more thermoplastic polyurethanes (TPUs) satisfies the properties described hereinafter for at least one of the thermoplastic polyurethanes (TPUs).
[0078] In other words, in this case, a blend of two or more thermoplastic polyurethanes (TPUs) has the properties described hereafter, which means that in this case, the individual thermoplastic polyurethanes (TPUs) present in the blend may also have properties that differ from those described below, if the blend has these properties.
[0079] According to the present invention, at least one thermoplastic polyurethane (TPU) can be obtained by polymerizing components (A), (B) and (C). Component (A) is at least one polyether polyol. Therefore, the at least one thermoplastic polyurethane (TPU) is also called polyether-based thermoplastic polyurethane (TPU).
[0080] Thus, the present invention also provides a laminate, wherein the at least one thermoplastic polyurethane (TPU) is at least one polyether-based thermoplastic polyurethane (TPU).
[0081] It is preferred that no polyesters are used as components for the preparation of the at least one thermoplastic polyurethane (TPU). It is particularly preferred that no components which form ester bonds in the polymerization are used.
[0082] Thus, the present invention also provides a laminate, wherein no component that forms an ester bond in the polymerization is used in the polymerization of components (A), (B) and (C).
[0083] Thermoplastic polyurethanes (TPUs) prepared using polyesters and / or components that form ester bonds in the polymerization are also referred to as polyester-based thermoplastic polyurethanes (TPUs). The at least one thermoplastic polyurethane (TPU) is preferably not a polyester-based thermoplastic polyurethane (TPU).
[0084] Thus, the present invention also provides a laminate, wherein the at least one thermoplastic polyurethane (TPU) is not a polyester-based thermoplastic polyurethane (TPU).
[0085] In the polymerization of components (A), (B) and (C) for the preparation of at least one thermoplastic polyurethane (TPU), it is additionally possible to use at least one further component selected from the group consisting of chain transfer agents (D), catalysts (E) and additives (F).
[0086] The present invention therefore also provides a laminate, in which at least one thermoplastic polyurethane (TPU) is obtainable by polymerization of components (A), (B) and (C) with at least one further component selected from the group consisting of chain transfer agents (D), catalysts (E) and additives (F).
[0087] Suitable chain transfer agents (D) are known per se to those skilled in the art.
[0088] "Chain transfer agent" in the context of the present invention is understood to mean a compound that has exactly one group that is reactive towards isocyanates. Such chain transfer agents are monofunctional alcohols, polyfunctional amines and monofunctional polyols. A preferred chain transfer agent is methylamine.
[0089] For example, the chain transfer agent (D) has a molecular weight in the range of 30 g / mol to 500 g / mol.
[0090] The chain transfer agent (D) is preferably used in an amount within the range of 0% by mass to 5% by mass, preferably within the range of 0.1% by mass to 1% by mass, based on the total mass percentage of components (A), (C) and (D).
[0091] Suitable catalysts (E) are compounds known to those skilled in the art that catalyze the reaction between the isocyanate groups (NCO groups) of component (B) and the hydroxyl groups of components (A) and (C). For example, catalyst (E) is selected from the group consisting of tertiary amines and organometallic compounds.
[0092] Suitable tertiary amines are known to those skilled in the art and are, for example, selected from the group consisting of triethylamine, dimethylcyclohexylamine, N-methylmorpholine, N,N-dimethylpiperazine, 2-(dimethylaminoethyl)ethanol and diazabicyclo[2.2.2]octane.
[0093] Suitable organometallic compounds are, for example, selected from the group consisting of titanates, iron(III) acetylacetonate, tin diacetate, tin dioctanoate, tin dilaurate, dibutyltin diacetate and dibutyltin dilaurate.
[0094] The catalyst (E) is typically used in an amount of 0.0001% to 0.1% by weight, based on 100% by weight of components (A) and (C).
[0095] Suitable additives (F) are, for example, hydrolysis stabilizers and flame retardants.
[0096] The at least one thermoplastic polyurethane (TPU) can be prepared by any method known to those skilled in the art. For example, the at least one thermoplastic polyurethane (TPU) is prepared by a continuous method such as the reactive extrusion method, the belt method, the "one-shot" method or the prepolymer method. These methods are known per se to those skilled in the art.
[0097] At least one thermoplastic polyurethane (TPU) is typically M(TPU)) at least one thermoplastic polyurethane (TPU) has a melting temperature (T M(TPU) ) is determined according to ISO11357-3:2014 and is, for example, within the range of 140 to 240°C, preferably within the range of 150 to 230°C, and particularly preferably within the range of 170 to 220°C.
[0098] Therefore, the present invention also provides a method for producing a thermoplastic polyurethane (TPU) having a melting temperature (T M(TPU) Also provided is a laminate having a
[0099] Melting temperature according to ISO11357-3:2014 (T M(TPU) For the determination of the particle size, the at least one thermoplastic polyurethane (TPU) is typically used in pelletized form. The pellets of the at least one thermoplastic polyurethane (TPU) in that case typically have a size in the range of 1 mm to 10 mm.
[0100] At least one thermoplastic polyurethane (TPU) typically has a glass transition temperature (T G(TPU) ) has a glass transition temperature (T G(TPU) ) is determined according to ISO11357-3:2014 and is, for example, within the range of -150 to 20°C, preferably within the range of -80 to 0°C, and particularly preferably within the range of -60 to -20°C.
[0101] Therefore, the present invention also provides a thermoplastic polyurethane (TPU) having a glass transition temperature (T G(TPU) Also provided is a laminate having a
[0102] In the context of the present invention, the glass transition temperature (T G(TPU) ) is the glass transition temperature (T) of at least one thermoplastic polyurethane (TPU) in dry form according to ISO 11357-2:2014. G(TPU) )
[0103] In the context of the present invention, "dry" means that the at least one thermoplastic polyurethane (TPU) contains less than 1% by weight, preferably less than 0.5% by weight, particularly preferably less than 0.1% by weight of water, based on the total weight of the at least one thermoplastic polyurethane (TPU). More preferably, "dry" means that the at least one thermoplastic polyurethane (TPU) does not contain any water, and most preferably that the at least one thermoplastic polyurethane (TPU) does not contain any solvent.
[0104] The at least one thermoplastic polyurethane (TPU) has, for example, a modulus of elasticity, determined according to DIN EN ISO 527-1:2012, in the range of 800 to 1400 MPa, preferably in the range of 900 to 1350 MPa, more preferably in the range of 1000 to 1300 MPa.
[0105] Thus, the present invention also provides a laminate, wherein the at least one thermoplastic polyurethane (TPU) has a modulus of elasticity in the range of 800 to 1400 MPa.
[0106] Component (A) According to the present invention, component (A) is at least one polyether polyol.
[0107] In the context of the present invention, the terms "component (A)" and "at least one polyether polyol" are used synonymously and therefore have the same meaning.
[0108] By "at least one polyether polyol" in the context of the present invention is meant either exactly one polyether polyol or a mixture of two or more polyether polyols.
[0109] "Polyether polyol" in the context of the present invention is understood to mean a polyether having two or more alcohol groups (hydroxyl groups, OH groups). Preferred polyether polyols are polyether diols. "Polyether diol" is understood to mean a polyether having exactly two alcohol groups (OH groups, hydroxyl groups). Polyether polyols are known per se to those skilled in the art.
[0110] Preferred polyether polyols can be obtained, for example, by anionic polymerization of alkylene oxides with alkali metal hydroxides, such as sodium or potassium hydroxide, or alkali metal alkoxides, such as sodium methoxide, sodium or potassium ethoxide or potassium isopropoxide, with the addition of at least one starter molecule as catalyst, the starter molecule containing 2 to 3, preferably 2, reactive hydrogen atoms.In addition, polyether polyols can be obtained by catalytic polymerization of alkylene oxides having 2 to 4 carbon atoms in the alkyl group and using Lewis acids as catalysts.
[0111] Preferred alkylene oxides are, for example, selected from the group consisting of tetrahydrofuran, 1,3-propylene oxide, ethylene oxide and 1,2-propylene oxide. Particularly preferred are tetrahydrofuran, ethylene oxide and 1,2-propylene oxide. Most preferred is tetrahydrofuran.
[0112] Thus, preferably according to the invention, component (A) is selected from the group consisting of polytetrahydrofuran, polyethylene oxide and poly-1,2-propylene oxide. Preferably according to the invention, component (A) is polytetrahydrofuran.
[0113] Preferred starter molecules are known per se to those skilled in the art, for example, the starter molecules are selected from the group consisting of water, ethanediol, propane-1,2-diol, butane-1,4-diol, diethylene glycol, hexane-1,6-diol and 2-methylpentane-1,5-diol.
[0114] Component (A) is preferably linear and has, for example, a number average molecular weight (Mw) in the range of 100 to 8000 g / mol, preferably in the range of 200 to 7000 g / mol, and more preferably in the range of 600 to 6000 g / mol.
[0115] Thus, the present invention also provides a laminate, wherein component (A) has a number average molecular weight (Mn) within the range of 100 to 8000 g / mol.
[0116] Ingredient (B) According to the present invention, component (B) is at least one polyisocyanate.
[0117] In the context of the present invention, the terms "component (B)" and "at least one polyisocyanate" are used synonymously and therefore have the same meaning.
[0118] By "at least one polyisocyanate" in the context of the present invention is meant either exactly one polyisocyanate or a mixture of two or more polyisocyanates.
[0119] In the context of the present invention, "polyisocyanate" is understood to mean a compound containing two or more isocyanate groups. The at least one polyisocyanate is preferably an organic polyisocyanate. More preferably, the at least one polyisocyanate is at least one diisocyanate.
[0120] Component (B) is therefore preferably at least one organic diisocyanate. In the context of the present invention, "organic diisocyanate" is understood to mean aliphatic, cycloaliphatic, araliphatic and / or aromatic diisocyanates.
[0121] For example, component (B) may be trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, heptamethylene diisocyanate, octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethylbutylene 1,4-diisocyanate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane 2,4-diisocyanate, 1-methylcyclohexane 2,6-diisocyanate, dicyclohexylmethane 4,4'-diisocyanate, dicyclohexylmethane 2,4'-diisocyanate, dicyclohexylmethane 2,2'-diisocyanate, diphenylmethane 2,2'-diisocyanate (2,2'-MDI), diphenylmethane 2,4'-diisocyanate (2,4'-MDI), diphenylmethane 4,4'-diisocyanate (4,4'-MDI), naphthylene 1,5-diisocyanate (NDI), tolylene 2,4-diisocyanate (2,4-TDI), tolylene 2,6-diisocyanate (2,6TDI), 3,3'-dimethyldiphenyl diisocyanate, diphenylethane 1,2-diisocyanate and phenylene diisocyanate.
[0122] More preferably, component (B) is selected from the group consisting of diphenylmethylene 4,4'-diisocyanate, diphenylmethane 2,4'-diisocyanate and diphenylmethane 2,2'-diisocyanate.
[0123] Thus, the present invention also provides a laminate, in which component (B) is selected from the group consisting of diphenylmethane 4,4'-diisocyanate, diphenylmethane 2,4'-diisocyanate and diphenylmethane 2,2'-diisocyanate.
[0124] Ingredients (C) Component (C) is at least one of C2 to C 20 It is a polyol.
[0125] In the context of the present invention, the terms “component (C)” and “at least one C2-C 20 "Polyol" are used interchangeably and therefore have the same meaning.
[0126] In the context of the present invention, "at least one of C2 to C 20 By "polyol" is meant exactly one C2-C 20 Polyol or two or more C2-C 20 A mixture of polyols.
[0127] In relation to the present invention, "C2-C 20 "Polyol" is understood to mean a compound having 2 to 20 carbon atoms and at least two alcohol groups (hydroxyl groups, OH groups). Component (C) may be an aliphatic, araliphatic, aromatic and / or cycloaliphatic compound having 2 to 20 carbon atoms and two or more alcohol groups (OH groups, hydroxyl groups). Component (C) preferably has exactly two hydroxyl groups.
[0128] For example, component (C) is selected from the group consisting of ethylene glycol, propane-1,2-diol, propane-1,3-diol, butane-1,4-diol, hexane-1,6-diol, dialkylene glycols having 3 to 8 carbon atoms, trialkylene glycols having 3 to 8 carbon atoms, and tetraalkylene glycols having 3 to 8 carbon atoms.
[0129] More preferably, component (C) is selected from the group consisting of ethylene glycol, propane-1,2-diol, propane-1,3-diol and butane-1,4-diol.
[0130] Thus, the present invention also provides a laminate in which component (C) is selected from the group consisting of ethylene glycol, propane-1,2-diol, propane-1,3-diol and butane-1,4-diol.
[0131] manufacturing The laminates of the present invention can be made by any method known to those skilled in the art. It is preferred that the laminates be made in a continuous process.
[0132] The laminate of the present invention preferably comprises: a) producing a film of a polymer composition (PC) comprising at least one thermoplastic polyurethane (TPU), the at least one thermoplastic polyurethane (TPU) comprising at least the following components: (A) at least one polyether polyol; (B) at least one polyisocyanate; (C) at least one of C2 to C 20 Polyol and and b) heating a first sheet of at least one first metal; c) pressing the heated first sheet from step b) with the film produced in step a) to obtain a laminate; The method comprises the steps of:
[0133] The present invention therefore also provides a method for producing a laminate of the present invention, comprising the steps of: a) producing a film of a polymer composition (PC) comprising at least one thermoplastic polyurethane (TPU), the at least one thermoplastic polyurethane (TPU) comprising at least the following components: (A) at least one polyether polyol; (B) at least one polyisocyanate; (C) at least one of C2 to C 20 Polyol and and b) heating a first sheet of at least one first metal; c) pressing the heated first sheet from step b) with the film produced in step a) to obtain a laminate; A method is also provided, including:
[0134] The explanations and preferences given above for the polymer composition (PC) of the laminate of the invention apply correspondingly to the polymer composition (PC) in the method of the invention.
[0135] The comments and preferences for the at least one thermoplastic polyurethane (TPU) of the laminate apply correspondingly to the at least one thermoplastic polyurethane (TPU) of the method.
[0136] Step a) comprises producing a film of the polymer composition (PC). The film produced in step a) consists of the polymer composition (PC). Methods of producing a film of the polymer composition (PC) are known per se to those skilled in the art. Step a) preferably comprises producing the film by an extrusion method.
[0137] Therefore, the present invention also provides a method, wherein the film is produced in step a) by an extrusion process.
[0138] Suitable extrusion methods for producing films of the polymer composition (PC) are known to those skilled in the art and include, for example, the casting method, the calendaring method, the blowing method or the multi-blow method.
[0139] The film of the polymer composition produced in step a) may have any desired thickness. The film of the polymer composition (PC) produced in step a) typically has a thickness in the range of 1% to 20% greater than the at least one further layer of the laminate to be produced, preferably in the range of 2% to 15% greater than the at least one further layer of the laminate to be produced, particularly preferably in the range of 4% to 10% greater than the at least one further layer of the laminate to be produced.
[0140] Step b) comprises heating a first sheet of at least one first metal. The first sheet is made of at least one first metal. The details and preferences described above for the at least one first metal present in the laminate apply correspondingly to the at least one first metal. Heating of the first sheet can be carried out by any method known to the skilled person. Step b) preferably comprises heating the first sheet by induction means.
[0141] Therefore, the present invention also provides a method, wherein the first sheet is heated in step b) by induction means.
[0142] Step b) may include heating the first sheet to any desired temperature. Step b) preferably includes heating the first sheet to a temperature above the melting temperature (T M(PC) Step b) preferably includes heating the first sheet to a temperature in the range of 150 to 350°C, more preferably in the range of 180 to 280°C, and particularly preferably in the range of 200 to 220°C.
[0143] Therefore, the present invention also provides a method, wherein step b) comprises heating the first sheet to a temperature in the range of 150°C to 350°C.
[0144] Step c) involves pressing the heated first sheet from step b) with the film produced in step a) to obtain a laminate. Step c) bonds the film to the first sheet. Step c) can reduce the thickness of the film.
[0145] The method of pressing the heated first sheet from step b) with the film produced in step a) in step c) is known per se to the person skilled in the art.
[0146] Steps b) and c) may be performed simultaneously or sequentially. It is preferred that steps b) and c) are performed simultaneously. In that case, the first sheet is heated while being pressed with the film produced in step a).
[0147] The laminate obtained in step c) is typically cooled. Cooling can be carried out by any method known to those skilled in the art, for example by blowing compressed air onto the laminate. The laminate is preferably cooled while maintaining the pressing pressure.
[0148] In the resulting laminate, the heated first sheet is at least one first layer of at least one first metal and the film is at least one further layer of a polymer composition (PC).
[0149] If the laminate is to comprise at least one second layer, an additional step b1) is carried out, which comprises heating a second sheet of at least one second metal. The explanations and preferences given above for the heating of the first sheet in step b) apply correspondingly to the heating of the second sheet in step b1).
[0150] Step c) then involves pressing the heated first sheet together with the heated second sheet from step b1) while the film produced in step a) is disposed between the two sheets.
[0151] The method of making the laminate of the present invention then typically comprises: a) producing a film of a polymer composition (PC) comprising at least one thermoplastic polyurethane (TPU), the at least one thermoplastic polyurethane (TPU) comprising at least the following components: (A) at least one polyether polyol; (B) at least one polyisocyanate; (C) at least one of C2 to C 20 Polyol and and b) heating a first sheet of at least one first metal; b1) heating a second sheet of at least one second metal; c) placing the film produced in step a) between the first sheet heated in step b) and the second sheet heated in step b1) and pressing the first sheet heated in step b) and the second sheet heated in step b1) together with the film produced in step a) to obtain a laminate; Includes.
[0152] The invention therefore also relates to a method for producing a laminate according to the invention, which additionally comprises at least one second layer of at least one second metal, the at least one first layer being joined to the at least one second layer via at least one further layer, the method comprising the steps of: a) producing a film of a polymer composition (PC) comprising at least one thermoplastic polyurethane (TPU), the at least one thermoplastic polyurethane (TPU) comprising at least the following components: (A) at least one polyether polyol; (B) at least one polyisocyanate; (C) at least one of C2 to C 20 Polyol and and b) heating a first sheet of at least one first metal; b1) heating a second sheet of at least one second metal; c) placing the film produced in step a) between the first sheet heated in step b) and the second sheet heated in step b1) and pressing the first sheet heated in step b) and the second sheet heated in step b1) together with the film produced in step a) to obtain a laminate; A method is also provided, including:
[0153] The explanations and preferences set out above for any at least one second metal of at least one second layer present in the laminate apply correspondingly to the at least one second metal of the second sheet in the method of the present invention.
[0154] The explanations and preferences set forth above for the first sheet and the heating of the first sheet apply correspondingly to the second sheet and the heating of the second sheet.
[0155] The explanations and preferences given above for step c) apply correspondingly as well to step c) in which a second sheet is additionally positioned.
[0156] The invention will now be explained in more detail with reference to examples, without being limited thereto. EXAMPLES
[0157] The following ingredients were used: Thermoplastic Polyurethane TPU1: Elastollan 1174 D (thermoplastic polyurethane, manufactured by BASF SE, MDI / polyetherol copolymer) TPU2: Elastollan 1283 D11 (thermoplastic polyurethane, manufactured by BASF SE, MDI / polyetherol copolymer) TPU3: Elastollan C74 D (thermoplastic polyurethane, manufactured by BASF SE, MDI / polyesterol copolymer) First and second metals: steel
[0158] Laminate manufacturing The polymers specified in Table 1 in the amounts specified in Table 1 were compounded at 230°C using a Haake PolyLab QC equipped with a CTW100 extruder to obtain a polymer composition and extruded through a 100 mm wide slot film die. The resulting strand was processed by means of a 20 cm wide water-cooled roll to form a film at least 5 mm wide and 420 μm thick and rolled up. All amounts specified in Table 1 are mass percentages.
[0159] The film of polymer composition and the first and second sheets of steel were dried at 80° C. and a pressure of <5 mbar for 7 days before producing the laminate.
[0160] A first sheet of steel and a second sheet of steel were inserted into the device to produce a laminate. A film of the polymer composition was placed between the first and second sheets. The sheets were pressed using a hydraulic press at 250° C. and 30 bar for 60 seconds.
[0161] For cooling, the laminates were removed from the press while still hot and covered with a steel sheet (40x40 mm, 5 mm thick). After cooling, the laminates were stored under air at a relative humidity of <1%. The specimens were measured in a Zwick testing machine (Zwicki BT1-FR5.0TN with pneumatic clamping jaws) according to DIN EN ISO11339 at a measuring speed of 200 mm / min and a specimen thickness of 0.85-0.9 mm. The tensile forces in Newtons (N), ascertained from a measuring distance of 100 mm, were used to form an average over the entire measurement and were calculated and corrected to a width of 40 mm. The results (T-peel) for the various laminates can likewise be seen in Table 1.
[0162] The elastic modulus of the laminate was determined according to ISO 527-1:2012. The results can also be seen in Table 1.
[0163] [Table 1]
[0164] The laminates of the present invention have particularly good release properties and good modulus.
Claims
1. A laminate comprising at least one first layer of at least one first metal and at least one further layer of a polymer composition (PC) comprising at least one thermoplastic polyurethane (TPU), said at least one TPU comprising at least the following components: (A) at least one polyether polyol; (B) at least one polyisocyanate; (C) at least one C 2 ~C 20 Polyol and can be obtained by polymerizing the at least one first metal is steel; A laminate, wherein the polymer composition (PC) has an elastic modulus according to ISO 527-1:2012 of 800 to 1400 MPa.
2. 10. The laminate of claim 1, additionally comprising at least one second layer of at least one second metal, said at least one first layer being bonded to said at least one second layer via at least one additional layer.
3. The at least one thermoplastic polyurethane (TPU) has a glass transition temperature (T G(TPU) 3. The laminate of claim 1 or 2, comprising:
4. 4. The laminate according to claim 1, wherein the thermoplastic polyurethane (TPU) is obtainable by polymerization of component (A) in the range of 5% to 50% by weight, component (B) in the range of 20% to 80% by weight, and component (C) in the range of 5% to 40% by weight, relative in each case to the sum of the mass percentages of components (A), (B) and (C).
5. The laminate of any one of claims 1 to 4, wherein component (B) is selected from the group consisting of diphenylmethane 4,4'-diisocyanate, diphenylmethane 2,4'-diisocyanate and diphenylmethane 2,2'-diisocyanate.
6. The laminate of any one of claims 1 to 5, wherein component (C) is selected from the group consisting of ethylene glycol, propane-1,2-diol, propane-1,3-diol and butane-1,4-diol.
7. A laminate according to any one of claims 1 to 6, wherein said at least one thermoplastic polyurethane (TPU) has a modulus of elasticity in the range of 800 to 1400 MPa.
8. A laminate according to any one of claims 1 to 7, wherein component (A) has a number average molecular weight (Mn) in the range of 100 to 8000 g / mol.
9. 9. A laminate according to any one of claims 1 to 8 which is not a film-laminated flat conductor.
10. 10. A laminate according to any one of the preceding claims, wherein the at least one first layer has a thickness in the range of 0.1 mm to 0.6 mm and / or the at least one further layer has a thickness in the range of 0.02 mm to 1.5 mm.
11. 11. A laminate according to any one of claims 1 to 10, wherein said polymer composition (PC) further comprises at least one additive selected from the group consisting of stabilizers, dyes, antistatic agents, filler oils, surface modifiers, drying agents, release aids, release agents, antioxidants, light stabilizers, PVC stabilizers, lubricants, flame retardants, foaming agents, impact modifiers, adhesion promoters, coupling agents and nucleating agents.
12. A method for producing a laminate according to any one of claims 1 to 11, comprising the steps of: a) producing a film of a polymer composition (PC) comprising at least one thermoplastic polyurethane (TPU), the at least one thermoplastic polyurethane (TPU) comprising at least the following components: (A) at least one polyether polyol; (B) at least one polyisocyanate; (C) at least one C 2 ~C 20 Polyol and and b) heating a first sheet of at least one first metal; c) pressing the heated first sheet from step b) with the film produced in step a) to obtain a laminate; A method comprising:
13. The method of claim 12, wherein step b) comprises heating the first sheet to a temperature in the range of 150°C to 350°C.
14. 14. The method according to claim 12 or 13, wherein the heating of the first sheet in step b) is carried out by induction means.
15. 15. The method of any one of claims 12 to 14, wherein step a) comprises producing a film by an extrusion process.
Citation Information
Patent Citations
Use of a multilayer film for the production of photovoltaic modules
DE102011084519A1
Aqueous polyurethane dispersion from polypropylene glycol and production of composite film formed therefrom
JP1999012458A
Composites containing dense polyisocyanate polyaddition products
JP2002517338A
Composite material containing polyisocyanate polyaddition products
JP2002540982A
Film-laminated flat conductor containing thermoplastic polyurethane
JP2005533133A