Silicone rubber composition
A blend of non-fluorinated and fluorinated polydiorganosiloxane polymers addresses the challenge of managing electrical stresses in DC power transmission by ensuring uniform electrical properties and preventing dielectric breakdown in high voltage DC systems.
Patent Information
- Application Number
- JP2021513870
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-11
- Filing Date
- 2019-09-19
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2039-09-19
AI Technical Summary
Insulating materials used in AC power transmission systems fail to effectively manage the higher electrical stresses in DC power transmission systems, leading to dielectric breakdown due to increased localized electrical loads, and the introduction of conductive fillers to address this issue complicates uniform electrical properties and physical properties.
A blend of non-fluorinated and fluorinated polydiorganosiloxane polymers is used in a curable silicone elastomer composition, minimizing the need for conductive or semiconductive fillers, with a hydrosilylation or peroxide catalyst to achieve suitable insulation for high voltage direct current applications.
The composition provides effective distribution of localized DC loads, maintaining uniform electrical properties and physical integrity, thus preventing dielectric breakdown in high voltage DC applications.
Smart Images

Figure 0007572946000001 
Figure 0007572946000002 
Figure 0007572946000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to the use of silicone-based compositions comprising blends of non-fluorinated and fluorinated polydiorganosiloxane polymers in the manufacture of insulation for high voltage direct current (HVDC) applications and accessories, such as cable joints, cable terminal applications, and connectors.
[0002] While in most cases Alternating Current (AC) is preferred for power supply to end users, long distance transmission, e.g. >1000km, can be performed using High Voltage Direct Current (HVDC) systems, as it has less electrical losses and is therefore cheaper. Long distance HVDC transmission is generally done in three ways: overhead (e.g. via pylons); through underground systems and, if necessary, through "subsea" systems such as subsea transport. It is fair to say that underground systems are much more aesthetically pleasing to the public than pylons, while the latter may be perceived as practical but unsightly. However, underground HVDC transmission is generally the most challenging for suppliers, due to the use of cable joints every 1-2km compared to overhead and subsea systems. Thus, many cable joints are required for any kind of HVDC transmission, but for underground systems this requirement is particularly acute.
[0003] However, insulating materials utilized with respect to AC current transmission systems typically cannot be transferred to DC transmission systems, since electrical stresses are significantly different between AC and DC conditions, and in particular insulating materials are subject to higher continuous electrical stresses under DC conditions, which may result in dielectric breakdown of the material. Addressing such issues is particularly important today, given that the industry's HVDC voltage requirements for new cables and cable accessories continue to increase, and may now be >500 kV and even >800 kV. Apart from EPDM, liquid silicone rubber (LSR) compositions, which are generally the preferred insulating material for the manufacture of HVDC cable joints and other accessories, are excellent electrical insulators when cured into the final product, typically with a dielectric strength of ≥ 10 kV. 15 It has a resistivity of ohm-cm.
[0004] However, they can be "too good" insulators, in that the electric field cannot be distributed within them.
[0005] Therefore, HVDC places much greater electrical stress on silicone-based insulating materials due to increased localized loading compared to AC insulation. Generally, the industry introduces conductive fillers (e.g., carbon black or carbon nanotubes), thermally conductive fillers or semiconductive fillers into the compositions to make them sufficiently conductive and to provide a 10 10 ~10 15 This problem is solved by allowing localized DC load distribution through a slightly conductive silicone elastomer article made from a conductive LSR composition that provides bulk resistivity in the ohm-cm range.
[0006] However, although this solution can solve the dispersion problem, the introduction of such fillers can cause further problems, in particular the inability to control and / or obtain uniform electrical properties within the silicone elastomer, especially for the use of conductive fillers, and deterioration of physical properties, as well as reduced dielectric strength, when relying on said conductive, thermally conductive or semi-conductive fillers.
[0007] It has now been found that the need to incorporate the above-mentioned conductive and / or semiconductive fillers can be avoided by using blends of non-fluorinated and fluorinated polydiorganosiloxane polymers in compositions for producing insulators for high voltage direct current applications.
[0008] There is provided a use of a curable silicone elastomer composition, the curable silicone elastomer composition comprising: (A)(i) is a non-fluorinated polydiorganosiloxane in an amount of 50 to 99.5% by weight of component A; (A)(ii) a combination of (A)(A)(i) and (A)(ii), which is a fluorinated polydiorganosiloxane polymer in an amount of 0.5 to 50 weight percent of component A; (B) at least one reinforcing filler; (C) is at least one organohydrogenpolysiloxane (C)(i), at least one hydrosilylation catalyst (C)(ii), and optionally at least one cure inhibitor (C)(iii); or (D) at least one of (C) or (D), which is at least one peroxide catalyst; The composition contains ≦0.1% by weight of the composition of a conductive or semiconductive filler or mixture thereof in or as the high voltage DC insulation.
[0009] In one embodiment, the composition contains 0 (zero) weight percent conductive filler. (C) When a hydrosilylation cure package is present in the composition, at least the non-fluorinated polydiorganosiloxane (A)(i) and optionally the fluorinated polydiorganosiloxane (A)(ii) must contain at least one, and alternatively at least two, alkenyl or alkynyl groups per molecule.
[0010] Also provided is a curable silicone elastomer composition, (A)(i) is a non-fluorinated polydiorganosiloxane in an amount of 50 to 99.5% by weight of component A; (A)(ii) a blend of (A)(i) and (A)(ii), which is a fluorinated polydiorganosiloxane polymer in an amount of 0.5 to 50 weight percent of component A; (B) at least one reinforcing filler; (C) is at least one organohydrogenpolysiloxane (C)(i), at least one hydrosilylation catalyst (C)(ii), and optionally at least one cure inhibitor (C)(iii); or (D) at least one of (C) or (D), which is at least one peroxide catalyst; The composition contains ≦0.1% by weight of the composition of a conductive filler or semiconductive filler or mixtures thereof.
[0011] In one embodiment, the composition contains 0 (zero) weight percent conductive filler. (C) When a hydrosilylation cure package is present in the composition, at least the non-fluorinated polydiorganosiloxane (A)(i) and optionally the fluorinated polydiorganosiloxane (A)(ii) must contain at least one, and alternatively at least two, alkenyl or alkynyl groups per molecule.
[0012] Also provided is a high voltage DC insulator comprising an elastomeric article of a curable silicone elastomer composition, the curable silicone elastomer composition comprising: (A)(i) is a non-fluorinated polydiorganosiloxane polymer in an amount of 50 to 99.5% by weight of component A; (A)(ii) a combination of (A)(A)(i) and (A)(ii), which is a fluorinated polydiorganosiloxane polymer in an amount of 0.5 to 50 weight percent of component A; (B) at least one reinforcing filler; (C) is at least one organohydrogenpolysiloxane (C)(i), at least one hydrosilylation catalyst (C)(ii), and optionally at least one cure inhibitor (C)(iii); or (D) at least one of (C) or (D), which is at least one peroxide catalyst; The composition contains ≦0.1% by weight of the composition of a conductive filler or semiconductive filler or mixtures thereof.
[0013] In one embodiment, the compositions herein contain 0 (zero) weight percent conductive filler. (C) When a hydrosilylation cure package is present in the composition, at least the non-fluorinated polydiorganosiloxane (A)(i) and optionally the fluorinated polydiorganosiloxane (A)(ii) must contain at least one, and alternatively at least two, alkenyl or alkynyl groups per molecule.
[0014] In yet a further embodiment, there is provided a high voltage DC insulator comprising an elastomeric article obtained by curing a silicone elastomer composition comprising: (A)(i) is a non-fluorinated polydiorganosiloxane in an amount of 50 to 99.5% by weight of component A; (A)(ii) a blend of (A)(i) and (A)(ii), which is a fluorinated polydiorganosiloxane siloxane polymer in an amount of 0.5 to 50 weight percent of component A; (B) at least one reinforcing filler; (C) is at least one organohydrogenpolysiloxane (C)(i), at least one hydrosilylation catalyst (C)(ii), and optionally at least one cure inhibitor (C)(iii); or (D) at least one of (C) or (D), which is at least one peroxide catalyst; The composition contains ≦0.1% by weight of the composition of a conductive filler or semiconductive filler or mixtures thereof.
[0015] In one embodiment, the compositions herein contain 0 (zero) weight percent conductive filler. (C) When a hydrosilylation cure package is present in the composition, at least the non-fluorinated polydiorganosiloxane (A)(i) and optionally the fluorinated polydiorganosiloxane (A)(ii) must contain at least one, and alternatively at least two, alkenyl or alkynyl groups per molecule.
[0016] For the purposes of this application, "substituted" means that one or more hydrogen atoms in a hydrocarbon group are replaced with another substituent. Examples of such substituents include, but are not limited to, halogen atoms such as chlorine, bromine, and iodine; halogen atom-containing groups (other than fluoro) such as chloromethyl; oxygen atoms; oxygen atom-containing groups such as (meth)acrylic groups and carboxyl groups; nitrogen atoms; nitrogen atom-containing groups such as amino, amide, and cyano functional groups; sulfur atoms; and sulfur atom-containing groups such as mercapto groups.
[0017] The siloxane polymer (A) used in the above composition is a combination of (A)(i) and (A)(ii) which, when taken together in the relative amounts indicated, have been found to function as an insulator suitable for use in high voltage direct current applications when cured with the other components of the composition. (A)(i) a non-fluorinated polydiorganosiloxane in an amount of 50 to 99.5 weight percent of component (A); (A)(ii) a fluorinated polydiorganosiloxane in an amount of 0.5 to 50 weight percent of component (A).
[0018] When a (C) hydrosilylation cure package is present in the composition, at least the non-fluorinated polydiorganosiloxane (A)(i) and optionally the fluorinated polydiorganosiloxane (A)(ii) should contain at least one, or alternatively at least two, alkenyl or alkynyl groups per molecule. However, when component (D) is the sole means of catalysis of the cure process, it is preferred, but not required, that at least one alkenyl or alkynyl group per molecule, or at least two alkenyl or alkynyl groups per molecule, be present in (A)(i) and (A)(ii).
[0019] Thus, preferably, component (A)(i) should contain at least one, or at least two, alkenyl or alkynyl groups per molecule, and component (A)(ii) may optionally contain at least one, or at least two, alkenyl or alkynyl groups per molecule, but may alternatively contain no unsaturated groups, such as alkenyl and / or alkynyl groups, per molecule. Alternatively, in one embodiment, both components (A)(i) and (A)(ii) should contain at least one, or at least two, alkenyl or alkynyl groups per molecule.
[0020] The non-fluorinated polydiorganosiloxane polymer (A)(i) is present in an amount of 50 to 99.5% of component (A) and has the formula (I): R a SiO (4-a) / 2 (I) wherein each R is independently selected from an aliphatic hydrocarbyl group, an aromatic hydrocarbyl group, or an organyl group (i.e., any organic substituent having one free valence at a carbon atom, regardless of the type of functional group). Examples of saturated aliphatic hydrocarbyl include, but are not limited to, alkyl groups such as methyl, ethyl, propyl, pentyl, octyl, undecyl, and octadecyl, and cycloalkyl groups such as cyclohexyl. Examples of unsaturated aliphatic hydrocarbyl include, but are not limited to, alkenyl groups such as vinyl, allyl, butenyl, pentenyl, cyclohexenyl, and hexenyl, and alkynyl groups. Examples of aromatic hydrocarbon groups include, but are not limited to, phenyl, tolyl, xylyl, benzyl, styryl, and 2-phenylethyl. Examples of organyl groups include, but are not limited to, halogenated alkyl groups (except fluoro-containing groups), such as chloromethyl and 3-chloropropyl; nitrogen-containing groups, such as amino, amido, imino, and imido groups; oxygen-containing groups, such as polyoxyalkylene, carbonyl, alkoxy, and hydroxyl groups. Further organyl groups include sulfur-, phosphorus-, and boron-containing groups. The subscript "a" is 0, 1, 2, or 3.
[0021] Siloxy units may be described by the contractions (abbreviations) "M", "D", "T", and "Q" when R is a methyl group (further teachings on silicone nomenclature can be found in Walter Noll, Chemistry and Technology of Silicones, dated 1962, Chapter I, pages 1-9). M units are siloxy units where a=3, i.e., RSiO 1 / 2 and D units are siloxy units where a=2, i.e., RSiO 2 / 2 where T units are siloxy units where a=1, i.e., RSiO 3 / 2 and Q units are siloxy units where a=0, i.e., SiO 4 / 2 is equivalent to.
[0022] Examples of typical groups on the non-fluorinated polydiorganosiloxane polymer (A)(i) include primarily alkenyl, alkyl, and / or aryl groups. The groups may be pendant (on D or T siloxy units) or terminal (on M siloxy units). As previously mentioned, alkenyl and / or alkynyl groups are essential when component (C) participates in the curing process, but are optional when the sole catalyst of the curing process is component (D). Thus, when present, suitable alkenyl groups in component (A)(i) typically contain from 2 to 10 carbon atoms, with preferred examples being vinyl, isopropenyl, allyl, and 5-hexenyl.
[0023] Typically, the silicon-bonded organic groups bonded to component (A)(i) other than the alkenyl groups are selected from monovalent saturated hydrocarbon groups, typically containing 1 to 10 carbon atoms, and monovalent aromatic hydrocarbon groups, typically containing 6 to 12 carbon atoms. These hydrocarbon groups are either unsubstituted or substituted with groups that do not interfere with the curing of the compositions of the present invention, such as halogen atoms. Preferred species of silicon-bonded organic groups are, for example, alkyl groups, such as methyl, ethyl, and propyl, and aryl groups, such as phenyl.
[0024] The non-fluorinated polydiorganosiloxane polymer may be selected from, for example, polydimethylsiloxane, alkylmethylpolysiloxane, alkylarylpolysiloxane, or copolymers thereof, containing alkenyl and / or alkynyl groups (alkyl means an alkyl group having two or more carbons), and may have any suitable end group, for example, trialkyl-terminated, alkenyldialkyl-terminated, or terminated with any other suitable combination of end groups, provided that each polymer contains at least two alkenyl groups in one molecule. Thus, the non-fluorinated polydiorganosiloxane polymer may be, by way of example, dimethylvinyl-terminated polydimethylsiloxane, dimethylvinylsiloxy-terminated dimethylmethylphenylsiloxane, trialkyl-terminated dimethylmethylvinylpolysiloxane, or dialkylvinyl-terminated dimethylmethylvinylpolysiloxane copolymer.
[0025] The molecular structure of component (A)(i) is typically linear, although some branching may be present resulting from the presence of T units (as described above) within the molecule. To achieve useful levels of physical properties in the elastomers prepared by curing the compositions as described above, the molecular weight of component (A)(i) should be sufficient to achieve a viscosity of at least 1000 mPa.s at 25° C. using the most appropriate spindle in the Brookfield® RV or LV range for the viscosity range, according to ASTM D 1084 Method B cup / spindle method. The upper molecular weight of component (A)(i) is not particularly limited, but is typically limited only by the processability of the LSR compositions of the present invention.
[0026] However, (A)(i) may also be a gum. Polydiorganosiloxane gums typically have a viscosity of at least 1,000,000 mPa·s at 25°C. However, due to the difficulty in measuring viscosities above these values, gums tend to be described in terms of their Williams plasticity values according to ASTM D-926-08 rather than their viscosity. Thus, polydiorganosiloxane gum A(i) has a viscosity that results in a Williams plasticity of at least 30 mm / 100 measured according to ASTM D-926-08, alternatively at least 50 mm / 100 measured according to ASTM D-926-08, alternatively at least 100 mm / 100 measured according to ASTM D-926-08, alternatively between 100 mm / 100 and 300 mm / 100 measured according to ASTM D-926-08.
[0027] An example of component (A)(i) is a polydiorganosiloxane containing two terminal alkenyl groups and can be represented by the general formula (II): R'R''R'''SiO-(R''R''SiO) m -SiR'''R''R'' (II)
[0028] In formula (II), each R' is an alkenyl group, typically containing from 2 to 10 carbon atoms, such as vinyl, allyl, and 5-hexenyl.
[0029] R" does not contain ethylenic unsaturation and each R" may be the same or different and is independently selected from monovalent saturated hydrocarbon radicals typically containing 1 to 10 carbon atoms and monovalent aromatic hydrocarbon radicals typically containing 6 to 12 carbon atoms. R" may be unsubstituted or substituted with one or more groups which do not interfere with the cure of the compositions of the present invention, such as halogen (except fluorine) atoms. R'" is R' or R". For the avoidance of doubt, the R'", R' or R" groups in component (A)(i) polymer cannot contain fluoro groups or any fluorine-containing groups. As stated above, when the polymer is designed to be used as part of an LSR composition, the letter m represents the degree of polymerization suitable for component (A)(i) to have a viscosity of 1,000 mPa.s to 100,000 mPa.s at 25°C using the ASTM D 1084 Method B cup / spindle method using the most appropriate spindle in the Brookfield® RV or LV range for the viscosity range. However, when (A)(i) is in the form of a gum, whose viscosity is often >1,000,000 mPa.s at 25° C., the value of m will be significantly larger and the Williams plasticity measurement will be measured instead of viscosity.
[0030] The fluorinated polydiorganosiloxane polymer (A)(ii) has the formula: (R 2 Z) d (R 3 ) e SiO (4-d-e) / 2 [In the formula, Each R 2 may be the same or different and represent a branched or linear fluoroalkyl group having 1 to 8 carbon atoms, Each Z may be the same or different and represents a divalent alkylene group, hydrocarbon ether, or hydrocarbon thioether containing at least two carbon atoms. 2 The group is linked to the silicon atom via the Z group, Each R 3are the same or different and represent an optionally substituted saturated or unsaturated silicon-bonded monovalent hydrocarbon radical, or R 3 If is on a terminal group, then one or more R 3 can be -OH. The value of d+e is up to 4, but is 3 for M-type groups and 2 for D-type groups, typically d=0-2, e=0-2, and when d is 0, at least one R 3 It will be understood that the group includes one or more carbon-fluorine bonds.
[0031] Preferred saturation R 3 Exemplary groups include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, hexyl, 2-ethylhexyl, octyl, isooctyl, and decyl. Preferably, when e is >0, at least 90 percent, more preferably all R groups in the fluorosilicone polymer, except for alkenyl groups, are substituted with 1, 2, or 3. 3 The group is a methyl group. Preferably, when d is 0, there is an average of at least one R 3 contains at least one carbon-fluorine bond, or when e is 0, at least one R 2 is CF3-.
[0032] Preferably, R 2 R represents a fluoroalkyl group having at least one carbon atom, alternatively having 1 to 8 carbon atoms, over the full range of 5 to 100 mole percent fluorinated siloxane units. Each fluoroalkyl group present has at least one -CF bond. 2 The groups may be the same or different and may have a standard or branched structure. Preferably, at least some, most preferably at least 50%, of the fluoroalkyl groups are perfluoroalkyl groups. Examples include CF3-, C2F5-, C3F7-, such as CF3CF2CF2- or (CF3)2CF-, C4F9-, such as CF3CF2CF2CF2-, (CF3)2CFCF2-, (CF3)3C- and CF3CF2(CF3)CF-; C5F11 , e.g. CF3CF2CF2CF2CF2-, C6F 13 -, e.g. CF3(CF2)4CF2-;C7F 14 -, for example CF3(CF2CF2)3-; and C8F 17 -- are some examples.
[0033] Each perfluoroalkyl group is attached to a silicon atom by Z, a divalent spacing group containing carbon, hydrogen, and optionally oxygen and / or sulfur atoms present as ether and thioether linkages, respectively. The sulfur and oxygen atoms, if present, must be attached to carbon atoms only.
[0034] Each Z radical can have any structure containing the recited elements, but is preferably an alkylene radical (i.e., an acyclic, branched, or unbranched saturated divalent hydrocarbon group). Examples of suitable alkylene radicals include -CH2CH2-, -CH2CH2CH2-, -CH(CH3)CH2-, (CH2CH2)2-, and -CH(CH3)CH2CH2-. In one embodiment, each fluorinated radical R 2 Z is preferably of the formula R 2 CH 2 CH 2 -, i.e., Z is an ethylene group.
[0035] As stated above, alkenyl and / or alkynyl groups are optional, but are preferred in component (A)(ii) when component (C) is involved in the curing process, however, they are optional when it is the sole catalyst for the curing process in component (D). Thus, when present, suitable alkenyl groups in component (A)(i) typically contain from 2 to 10 carbon atoms, with preferred examples being vinyl, isopropenyl, allyl, and 5-hexenyl. These may be present as terminal groups or pendant on the polymer chain.
[0036] The fluorinated polydiorganosiloxane polymer (A)(ii) may further comprise up to about 90%, alternatively up to about 80%, of the total number of units in one molecule of non-fluorinated siloxane units having the formula: (R 4 ) c SiO (4-c) / 2 In the formula, R 4 represents an optionally substituted saturated or unsaturated silicon-bonded monovalent hydrocarbon radical, where c=0 to 3, preferably with an average value of about 2. 4 does not contain fluorine (hence, R 4 may not contain any of the previously specified fluoro-containing substituents.
[0037] As mentioned above, R 4 represents an optionally substituted saturated or unsaturated silicon-bonded monovalent hydrocarbon radical. 4 may be the same or different, C1 to C 10 Alkyl groups, such as vinyl or allyl groups, and / or aryl groups, such as phenyl, tolyl, benzyl, β-phenylethyl, and styryl. Preferably, at least two R 4 The substituents are alkenyl or alkynyl groups. If present, each alkenyl group has from 2 to 8 carbon atoms, alternatively each alkenyl group is a vinyl group.
[0038] Examples of component (A)(ii) include copolymers of dimethylsiloxy and (3,3,3-trifluoropropyl)methylsiloxy units, copolymers of dimethylsiloxy, (3,3,3-trifluoropropyl)methylsiloxy, and vinylmethylsiloxy units, copolymers of (3,3,3-trifluoropropyl)methylsiloxy and vinylmethylsiloxy units, and poly(3,3,3-trifluoropropyl)methylsiloxane. Component (A)(ii) is trialkyl or trimethyl-terminated, vinyldimethyl-terminated, dimethylhydroxy-terminated, and / or (3,3,3-trifluoropropyl)methylhydroxy-terminated.
[0039] The molecular structure of component (A)(ii) is typically linear, although some branching may be present due to the presence of T units (defined above) within the molecule. In order to achieve useful levels of physical properties in the elastomers prepared by curing the compositions as described above, the molecular weight of component (A)(ii) should be sufficient to achieve a viscosity of at least 1000 mPa.s at 25°C using the most appropriate spindle in the Brookfield® RV or LV range for the viscosity range, according to ASTM D 1084 Method B cup / spindle method. The upper limit of the molecular weight of component (A)(ii) is also not particularly limited. If the composition is designed to make a liquid fluorosilicone rubber (F-LSR) composition, the final composition is typically limited only by the processability of the F-LSR composition of the present invention.
[0040] However, (A)(ii) may also be a gum. As mentioned above, gums typically have a viscosity of at least 1,000,000 mPa.s at 25°C. Because it is difficult to measure viscosities above these values, they tend to be described by their Williams plasticity values according to ASTM D-926-08 rather than viscosity. When component (A)(ii) is a gum, it preferably has a viscosity that results in a Williams plasticity of at least 30 mm / 100 measured according to ASTM D-926-08, alternatively at least 50 mm / 100 measured according to ASTM D-926-08, alternatively at least 100 mm / 100 measured according to ASTM D-926-08, alternatively between 100 mm / 100 and 400 mm / 100 measured according to ASTM D-926-08.
[0041] (B) Reinforcing filler To obtain the high level of physical properties that characterize some types of cured elastomers that can be prepared using the compositions herein, it may be desirable to include a reinforcing filler (B), such as finely divided silica. Often, silica and other reinforcing fillers are surface treated with one or more known filler treating agents to prevent a phenomenon called "creping" or "crepe hardening" during processing of the curable composition.
[0042] Finely divided forms of silica are the preferred reinforcing fillers (B), such as fumed silica, precipitated silica and / or colloidal silica. They are typically at least 50 ml 2 This is particularly preferred because it has a relatively large surface area of 100 to 600 m / g as measured according to the BET method. 2 / g, or 100-500m 2 / g (using the BET method according to ISO9277:2010), or 200-400m 2 Fillers with a surface area of 0.1 g / g (using the BET method according to ISO 9277:2010) are typically used.
[0043] The amount of finely divided silica or other reinforcing filler used in the compositions described herein is typically from about 1 to 40% by weight of the composition, alternatively from 5 to 35% by weight of the composition, alternatively from 10 to 35% by weight of the composition, alternatively from 15 to 35% by weight of the composition.
[0044] When the filler is naturally hydrophilic (e.g., untreated silica filler), it is typically surface-treated with a treating agent. This treatment is carried out either before introduction into the composition or in situ (i.e., by blending together, in the presence of at least some of the other components of the composition of the present invention, until the surface treatment of the filler is complete and uniformly dispersed into a homogenous material). Typically, the untreated filler (B) is treated in situ with a treating agent in the presence of at least one of (A)(i) and (A)(ii).
[0045] Typically, the filler (B) is surface-treated, for example, with an organosilane, polydiorganosiloxane, or organosilazane, hexaalkyldisilazane, short-chain siloxanediol, fatty acid or fatty acid ester such as stearic acid, to render the filler hydrophobic, making it easier to handle and to obtain a homogeneous mixture with other components. Specific examples include, but are not limited to, liquid hydroxyl-terminated polydiorganosiloxanes containing an average of 2 to 20 repeating units of diorganosiloxane in each molecule, which may optionally contain fluoro groups and / or fluoro-containing groups, and, if necessary, hexaorganodisiloxane, hexaorganodisilazane, and the like. A small amount of water may be added as a processing aid, along with the silica treatment agent. The surface treatment of the filler makes it easier to wet with the polymer of component (A). These surface-modified fillers do not agglomerate and can be homogeneously incorporated into component (A), resulting in improved room temperature mechanical properties of the uncured composition.
[0046] Typically, the filler treating agent may be any low molecular weight organosilicon compound disclosed in the art that can be applied to prevent creping of organosiloxane compositions during processing.
[0047] The composition is cured using a cure package of components (C)(i), (C)(ii), and optionally (C)(iii), or using component (D), or if deemed necessary, using a mixture of the two.
[0048] (C)(i) Organohydrogenpolysiloxane Component (C)(i) is an organohydrogenpolysiloxane that acts as a crosslinker to cure component (A) by addition reaction of silicon-bonded hydrogen atoms of component (C)(i) with alkenyl groups of component (A) under the catalytic activity of component (C)(ii). Typically, component (C)(i) contains three or more silicon-bonded hydrogen atoms such that the hydrogen atoms of component (C)(i) can react sufficiently with the alkenyl groups of component (A) to form a network structure, thereby curing the composition. When component (A) has >2 alkenyl or alkynyl groups per molecule, or alkenyl groups per molecule, some or all of component (C)(i) may instead have two silicon-bonded hydrogen atoms per molecule.
[0049] The molecular structure of component (C)(i) is not particularly limited and may be linear, branched linear, or cyclic. The molecular weight of this component is not particularly limited, but the viscosity is typically 0.001 to 50 Pa.s at 25° C. using the most appropriate spindle in the Brookfield® RV or LV range for the viscosity range, according to ASTM D 1084 Method B cup / spindle method, to obtain good miscibility with component (A).
[0050] Component (C)(i) may typically be added in an amount such that the molar ratio of the total number of silicon-bonded hydrogen atoms in component (C)(i) to the total number of alkenyl and alkynyl groups, or alkenyls, in component (A) is 0.5:1 to 20:1. If this ratio is less than 0.5:1, a sufficiently cured composition is not obtained. If this ratio is greater than 20:1, the hardness of the cured composition tends to increase when heated.
[0051] Examples of component (C)(i) include: (i) trimethylsiloxy-terminated methylhydrogenpolysiloxane, (ii) trimethylsiloxy-terminated polydimethylsiloxane-methylhydrogensiloxane; (iii) dimethylhydrogensiloxy-terminated dimethylsiloxane-methylhydrogensiloxane copolymers; (iv) dimethylsiloxane-methylhydrogensiloxane cyclic copolymers; (v)(CH3)2HSiO 1 / 2 Units and SiO 4 / 2 A copolymer consisting of units, (vi)(CH3)3SiO 1 / 2 Unit: (CH3)2HSiO 1 / 2 Units, and SiO 4 / 2 Copolymers consisting of units, and (vii) the above (CH3)2HSiO 1 / 2 Units and (R 2 Z) d (R 3 ) e SiO (4-d-e) / 2 Examples of copolymers that can be used include, but are not limited to, copolymers containing:
[0052] (C)(ii) Hydrosilylation Catalyst When present, the hydrosilylation catalyst (C)(ii) is one of the platinum metals (platinum, ruthenium, osmium, rhodium, iridium, and palladium) or a compound of one or more of such metals. Platinum and platinum compounds are preferred due to the high activity levels of these catalysts in hydrosilylation reactions.
[0053] Examples of preferred hydrosilylation catalysts (C)(ii) include, but are not limited to, platinum black, platinum on various solid supports, chloroplatinic acid, alcoholic solutions of chloroplatinic acid, and complexes of chloroplatinic acid with ethylenically unsaturated compounds such as olefins and organosiloxanes containing ethylenically unsaturated silicon-bonded hydrocarbon groups. Catalyst (C)(ii) is platinum metal, platinum metal deposited on a support such as silica gel or powdered charcoal, or a compound or complex of a platinum group metal.
[0054] Examples of suitable platinum-based catalysts include: (i) complexes of chloroplatinic acid with organosiloxanes containing ethylenically unsaturated hydrocarbon groups, as described in U.S. Pat. No. 3,419,593; (ii) Chloroplatinic acid in either the hexahydrate or anhydrous form; (iii) platinum-containing catalysts obtained by a process comprising reacting chloroplatinic acid with an aliphatically unsaturated organosilicon compound, such as divinyltetramethyldisiloxane; (iv) alkene-platinum-silyl complexes as described in U.S. Pat. No. 6,605,734, such as (COD)Pt(SiMeCl2)2, where "COD" is 1,5-cyclooctadiene; and / or (v) Karstedt's catalysts, which are platinum divinyltetramethyldisiloxane complexes typically containing about 1% by weight of platinum in a solvent such as toluene, as described in U.S. Patents 3,715,334 and 3,814,730.
[0055] When present, the hydrosilylation catalyst (C)(ii) is present throughout the composition in a catalytic amount, i.e., an amount or quantity sufficient to promote its reaction or cure under the desired conditions. Varying levels of the hydrosilylation catalyst (C)(ii) can be used to adjust the reaction rate and cure reaction rate. The catalytic amount of the hydrosilylation catalyst (C)(ii) is generally from 0.01 parts per million (ppm) to 10,000 parts by weight of platinum group metal per million parts (ppm) based on the total weight of the compositional components (a) and (b); alternatively from 0.01 to 5000 ppm; alternatively from 0.01 to 3,000 ppm, alternatively from 0.01 to 1,000 ppm. In specific embodiments, the catalytic amount of the catalyst can range from 0.01 to 1,000 ppm, alternatively from 0.01 to 750 ppm, alternatively from 0.01 to 500 ppm, alternatively from 0.01 to 100 ppm of metal based on the weight of the composition. The ranges may relate to just the metal content in the catalyst, or to the entire catalyst (including its ligands), as specified, but typically these ranges relate to just the metal content in the catalyst. The catalyst may be added as a single species or as a mixture of two or more different species. Typically, depending on the form / concentration in which the catalyst package is provided, the amount of catalyst present is in the range of 0.001-3.0% by weight of the composition.
[0056] Inhibitor (C)(iii) The mixture of components (A), (C)(i), and (C)(ii) above can begin to cure at ambient temperature. When (C)(i) and (C)(ii) are present, a suitable inhibitor (C)(iii) can be used to retard or inhibit the activity of the catalyst to obtain a longer working time or working pot life of the hydrosilylation curing composition. Inhibitors of hydrosilylation catalysts, generally platinum metal-based catalysts, are known in the art. Hydrosilylation or addition reaction inhibitors include hydrazines, triazoles, phosphines, mercaptans, organic nitrogen compounds, acetylenic alcohols, silylated acetylenic alcohols, maleates, fumarates, ethylenically or aromatically unsaturated amides, ethylenically unsaturated isocyanates, olefinic siloxanes, unsaturated hydrocarbon monoesters and diesters, conjugated eneines, hydroperoxides, nitriles, and diaziridines.
[0057] One group of known inhibitors for platinum catalysts includes the acetylenic compounds disclosed in U.S. Patent No. 3,445,420. Acetylenic alcohols such as 2-methyl-3-butyn-2-ol constitute a preferred class of inhibitors that inhibit the activity of platinum-containing catalysts at 25° C. Typically, compositions containing these inhibitors must be heated to temperatures of 70° C. or higher in order to cure at a practical rate.
[0058] Examples of acetylenic alcohols and their derivatives include 1-ethynyl-1-cyclohexanol (ETCH), 2-methyl-3-butyn-2-ol, 3-butyn-1-ol, 3-butyn-2-ol, propargyl alcohol, 2-phenyl-2-propyn-1-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclopentanol, 1-phenyl-2-propynol, 3-methyl-1-penten-4-yn-3-ol, and mixtures thereof.
[0059] If present, in some cases, inhibitor concentrations as low as 1 mole of inhibitor per mole of metal in catalyst (C)(ii) provide sufficient storage stability and cure speed. In other cases, inhibitor concentrations of up to 500 moles of inhibitor per mole of metal in catalyst (C)(ii) are necessary. The optimum concentration for a given inhibitor in a given composition can be readily determined by routine experimentation. Depending on the concentration and form in which the selected inhibitor is commercially provided / available, if present in the composition, the inhibitor is typically present in an amount of 0.0125-10% by weight of the composition.
[0060] (D) Peroxide catalyst The compositions described herein may alternatively or additionally be cured with a peroxide catalyst (D) or a mixture of different types of peroxide catalysts.
[0061] The peroxide catalyst may be any of the well-known commercially available peroxides used to cure fluorosilicone elastomer compositions. The amount of organic peroxide used will depend on the nature of the cure process, the organic peroxide used, and the composition used. Typically, the amount of peroxide catalyst used in the compositions described herein is 0.2 to 3 wt.%, alternatively 0.2 to 2 wt.%, in each case based on the weight of the composition.
[0062] Suitable organic peroxides are substituted or unsubstituted dialkyl-, alkylaroyl-, diaroyl-peroxides, such as benzoyl peroxide and 2,4-dichlorobenzoyl peroxide, ditertiary butyl peroxide, dicumyl peroxide, t-butyl cumyl peroxide, bis(t-butylperoxyisopropyl)benzene bis(t-butylperoxy)-2,5-dimethylhexyne 2,4-dimethyl-2,5-di(t-butylperoxy)hexane, di-t-butyl peroxide and 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane.Mixtures of the above may also be used.
[0063] When component C is relied upon to cure the composition, the composition is typically stored in two parts, often referred to as Parts A and B, for the purposes of separating components (C)(i) and (C)(ii) prior to curing. Typically, component (C)(iii), if present, is in the same part as the hydrosilylation catalyst (C)(ii). Such two-part compositions are configured for easy mixing immediately prior to use, typically having a weight ratio of Part A:Part B of 15:1 to 1:1.
[0064] Additional Optional Ingredients Additional optional ingredients may be present in the silicone rubber composition depending on its intended use. Examples of such optional ingredients include compatibilizers, thermally conductive fillers, non-conductive fillers, pot life extenders, flame retardants, lubricants, non-reinforcing fillers, compression set additives, pigment colorants, adhesion promoters, chain extenders, silicone polyethers, and mixtures thereof.
[0065] Further examples of additives include mold release agents, diluents, solvents, UV light stabilizers, germicides, wetting agents, heat stabilizers, compression set additives, plasticizers, and mixtures thereof.
[0066] A compatibilizer may be introduced into the composition as deemed appropriate to help avoid phase separation between polymers (A)(i) and (A)(ii). Any suitable agent may be utilized, such as a block, graft or random copolymer containing dimethyl silicone and methyl trifluoropropyl silicone repeat units different from (A)(ii), such as those described in U.S. Pat. No. 5,824,736.
[0067] A pot life extender, such as a triazole, may be used but is not considered essential within the scope of the present invention, and thus the liquid curable silicone rubber composition may be free of a pot life extender.
[0068] Examples of flame retardants include aluminum trihydrate, chlorinated paraffins, hexabromocyclododecalane, triphenyl phosphate, dimethylmethylphosphonate, tris(2,3-dibromopropyl)phosphate (brominated tris), and mixtures or derivatives thereof.
[0069] Examples of lubricants include tetrafluoroethylene, resin powder, graphite, fluorinated graphite, talc, boron nitride, molybdenum disulfide, and mixtures or derivatives thereof.
[0070] Further additives include silicone fluids such as trimethyl- or dimethylhydroxy-terminated siloxanes, which typically have a viscosity of less than 150 mPa.s at 25° C. using the ASTM D1084 Method B cup / spindle method, using the most appropriate spindle in the Brookfield® RV or LV range for the viscosity range. When present, such silicone fluids may be present in the liquid curable silicone rubber composition in an amount ranging from 0.1 to 5 weight percent (wt %), based on the total weight of the composition.
[0071] Examples of pigments include titanium dioxide, chromium oxide, bismuth vanadium oxide, iron oxide, and mixtures thereof.
[0072] Examples of adhesion promoters include alkoxysilanes containing methacryl or acryl groups, such as methacryloxymethyl-trimethoxysilane, 3-methacryloxypropyl-trimethoxysilane, 3-methacryloxypropyl-methyldimethoxysilane, 3-methacryloxypropyl-dimethylmethoxysilane, 3-methacryloxypropyl-triethoxysilane, 3-methacryloxypropyl-methyldiethoxysilane, 3-methacryloxyisobutyl-trimethoxysilane, or similar methacryloxy-substituted alkoxysilanes; 3-acryloxypropyl-trimethoxysilane, 3-acryloxypropyl-methyldimethoxysilane, 3-acryloxypropyl-dimethyl-methoxysilane, 3-acryloxypropyl-triethoxysilane, or similar acryloxy-substituted alkyl-containing alkoxysilanes; zirconium chelate compounds, such as zirconium(IV) tetraacetylacetonate, zirconium(IV) hexafluoroacetate, zirconium(IV) tetrafluoroethylene ... bis(ethyl acetonate), zirconium(IV) trifluoroacetylacetonate, tetrakis(ethyl trifluoroacetylacetonate)zirconium, tetrakis(2,2,6,6-tetramethyl-heptane ethynate)zirconium, zirconium(IV) dibutoxybis(ethyl acetonate), diisopropoxybis(2,2,6,6-tetramethyl-heptane ethynate)zirconium, or β-diketones (including their alkyl- and fluorine-substituted forms). and epoxy-containing alkoxysilanes such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 4-glycidoxybutyltrimethoxysilane, 5,6-epoxyhexyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, or 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.
[0073] Examples of chain extenders include disiloxanes or low molecular weight polyorganosiloxanes containing two silicon-bonded hydrogen atoms at the terminal positions. Chain extenders typically link two or more molecules of component (A) by reacting with the alkenyl groups of component (A), increasing the effective molecular weight and the distance between potential crosslinking sites.
[0074] Disiloxanes are typically represented by the general formula (HR a 2Si)2O. When the chain extender is a polyorganosiloxane, it has the general formula HR a 2SiO 1 / 2 and the terminal units of formula R b 2SiO. In these formulas, R a and R b independently represent an unsubstituted or substituted monovalent hydrocarbon group having no ethylenic unsaturation and no fluorine content, including, but not limited to, alkyl groups containing 1 to 10 carbon atoms, substituted alkyl groups containing 1 to 10 carbon atoms (such as chloromethyl), cycloalkyl groups containing 3 to 10 carbon atoms, aryl groups containing 6 to 10 carbon atoms, alkaryl groups containing 7 to 10 carbon atoms (such as tolyl and xylyl), and aralkyl groups containing 7 to 10 carbon atoms (such as benzyl).
[0075] Further examples of chain extenders include tetramethyldihydrogendisiloxane or dimethylhydrogen terminated polydimethylsiloxane.
[0076] The chain extender may be added in an amount of 1 to 10 parts by weight based on the weight of component (A), typically 1 to 10 parts per 100 parts of component (A).
[0077] Examples of heat stabilizers include metal compounds such as red iron oxide, yellow iron oxide, ferric hydroxide, cerium oxide, cerium hydroxide, lanthanum oxide, copper phthocyanine, aluminum hydroxide, fumed titanium dioxide, iron naphthenate, cerium naphthenate, cerium dimethylpolysilanolate, and acetylacetone salts of metals selected from copper, zinc, aluminum, iron, cerium, zirconium, titanium, etc. The amount of heat stabilizer present in the composition may range from 0.01% to 1.0% by weight of the total composition.
[0078] Thus, the present invention provides Component (A) in an amount of 40 to 95% by weight of the composition; and component (B) in an amount of 1 to 40% by weight of the composition.
[0079] When the composition is cured by hydrosilylation, the composition is The composition may comprise 0.5-10% by weight of component (C)(i), 0.01-1% by weight of component (C)(ii), and 0-1% by weight of component (C)(iii). In such cases, the composition is stored in two parts, part A and part B, prior to use. Typically, part A contains a portion of component (A), component (B) and a portion of component (C)(ii), and part B contains the remainder of components (A) and (B), along with components (C)(i) and (C)(iii), if present. The two-part composition may be designed to be mixed together in any suitable ratio, but typically is mixed in a 1:1 ratio of part A:part B.
[0080] A method for producing high voltage DC insulation is also provided, comprising the steps of preparing a composition as described herein, mixing the composition together and curing. The mixing step can be (a) mixing all the individual components together, (b) if the composition is in two parts, mixing the two parts together, and (c) if the composition is in four parts, mixing the four parts together, in each case immediately prior to curing. If the composition is in more than two parts, the parts are mixed together in a multi-part mix system prior to curing.
[0081] Alternatively, when component (C) is present, the composition may preferably be stored prior to use in four parts: a first part A containing components (A)(i), (B) and (C)(ii); a second part A containing components (A)(ii), (B) and optionally (C)(ii); a first part B containing components (A)(i), (B) and (C)(i) and (C)(iii); and a second part B containing components (A)(ii), (B) and optionally (C)(i) and (C)(iii).
[0082] Alternatively, when component (C) is present in component (A)(ii), the fluorinated polydiorganosiloxane can be kept separate from the components of the cure package (C), i.e., the (C)(ii) catalyst is stored in the non-fluorinated polymer (A)(i) in part A, and the components (C)(i) organohydrogenpolysiloxane and C(iii) inhibitor (if present) are stored in the polymer A(i) composition in part B. This allows the component A(ii) fluorinated polydiorganosiloxane to be introduced into the part A and part B compositions as the polymer alone or in the form of a base with filler (B). Thus, the fluorinated polydiorganosiloxane polymer (A)(ii) is not mixed with the crosslinker (C)(i) prior to blending with the non-fluorinated polydiorganosiloxane (A)(i) in Part B, and / or the fluorinated polydiorganosiloxane polymer (A)(ii) is not mixed with the catalyst (C)(ii) prior to blending with the non-fluorinated polydiorganosiloxane (A)(i) in Part A. That is, the crosslinker (C)(i) may be maintained only in the mixture with the non-fluorinated polydiorganosiloxane (A)(i) prior to blending the non-fluorinated polydiorganosiloxane (A)(i) with the fluorinated polydiorganosiloxane polymer (A)(ii) and / or the catalyst (C)(ii) may be maintained only in the mixture with the non-fluorinated polydiorganosiloxane (A)(i) prior to blending the non-fluorinated polydiorganosiloxane (A)(i) with the fluorinated polydiorganosiloxane polymer (A)(ii). Furthermore, the fluorinated polydiorganosiloxane polymer (A)(ii) may be introduced into parts A and / or B either as a polymer or in the form of a base with filler B.
[0083] The composition of the present invention can be prepared by mixing all of the components at ambient or elevated temperature as needed. Any mixing technique and equipment disclosed in the prior art can be used for this purpose. The specific equipment used is determined by the viscosity of the components and the final curable coating composition. Suitable mixers include, but are not limited to, paddle-type mixers or kneader-type mixers. It may be desirable to avoid premature curing of the composition by cooling the components during mixing.
[0084] The order for mixing the components is not critical to the present invention. Components (A)(i) and (A)(ii), if present, may be mixed together before introducing other components (e.g., component D peroxide catalyst). Alternatively, a part A composition containing (A)(i), a part A composition containing (A)(ii), a part B composition containing (A)(i), and optionally a part B composition containing (A)(ii) may all be prepared. Alternatively, as described above, part A containing fluorinated polydiorganosiloxane polymer (A)(ii) and / or part B containing (A)(ii) may be optional or may consist of polymer (A)(ii) alone or a mixture of polymer (A)(ii) and reinforcing filler (B). Component B reinforcing filler may be present in any or all of these parts, if desired. All four parts can then be mixed together in any order in the ratios required for the blend, or the two A parts can be mixed together and the two B parts can be mixed together and then the part A and B mixtures mixed together. In an alternative process, the various parts can be mixed together in the desired ratios prior to injection molding using a four component mixing system.
[0085] When the compositions herein are designed to be LSR compositions, the viscosity of the compositions is in any case 10 to 200 nm using a cone and plate rheometer at 25° C. -1(A) is a gum, and the viscosity of the gum is in the range of 10 to 1,000 Pa.s, alternatively 10 to 500 Pa.s, alternatively 100 to 500 Pa.s, measured in milliseconds, or measured by the Williams plasticity test of the most viscous material in which (A)(i) and / or (ii) is a gum.
[0086] Alternatively, the silicone rubber composition may be further processed by injection molding, encapsulation molding, press molding, dispenser molding, extrusion molding, transfer molding, press vulcanization, centrifugal casting, calendar molding, bead coating, or blow molding.
[0087] Curing of the curable silicone rubber composition may be carried out as necessary depending on the type of silicone rubber used. Typical curing temperatures may range from 80 to 200°C, or alternatively from 100 to 170°C. Curing times vary depending on the curing temperature and method selected, but are typically about 5 minutes to 1 hour. Furthermore, the resulting cured elastomer may be post-cured as necessary. Any suitable post-curing may be carried out if desired. For example, the cured elastomer may be post-cured in an oven at a temperature of 150 to 250°C, or alternatively from 170°C to 230°C, for a predetermined period of time, for example, 2 to 10 hours, as required.
[0088] Curing can be carried out, for example, in a mold to form a molded silicone article. The composition can be, for example, injection molded to form an article, or such composition can be overmolded by injection molding around an article or onto a substrate.
[0089] Also provided herein is a high voltage DC insulator comprising an elastomeric product of the curable silicone elastomer composition described herein and / or an elastomeric product obtained by curing the silicone elastomer composition described herein.Typically, the composition contains 0 (zero) weight percent conductive filler.
[0090] The cured compositions may be used as insulation adapted to reduce electrical stress in high voltage direct current (HVDC) applications, i.e., power cable systems and the like. As previously mentioned, high voltage DC insulation is provided that includes an elastomeric article of the silicone elastomer composition described herein. The high voltage DC insulation may be used alone or may form part of an article or assembly, e.g., a composite part of an assembly, such as a cable accessory, as a cable joint or cable termination material, boot, sleeve and / or other fitting, in high voltage DC applications, in field grading assemblies as a suitable insulating layer, and in other suitable cable accessories and connectors.
[0091] In a further embodiment, there is provided a method for manufacturing an insulator or a field grading assembly including the insulator for high voltage direct current (HVDC) applications, the method comprising the steps of i) molding a suitable amount of a silicone composition as described above by a suitable means, for example by extrusion or using a mold, and ii) curing the molded composition to form a molded insulator or a field grading assembly including the insulator.
[0092] The high voltage DC insulators described above may be part of a cable accessory for high voltage DC applications such as a cable joint, cable termination or cable connector, for example to seal the end of a cable having a thermoplastic or rubber cable insulation.
[0093] The present invention further provides a method for sealing and / or insulating a connected or closed cable end by using a cable joint as described above, the method comprising the steps of: (i) preparing an insulated wire having a DC insulation and a suitable thermoplastic or elastomeric multi-layer sheath for the bare wire or connector; and (ii) encapsulating the bare wire or connector by placing it on the surface of the insulating sheath in the bore of a previously molded and cured tubular cable joint as described above (i) such that under mechanical extension of the joint, the overlap to the wire insulation between the molded silicone cable joint and the sheath exceeds about 0.5 cm, whereby the silicone cable joint seals the sheath insulation of the insulated wire by the mechanical pressure of the relaxed joint and forms an encapsulating insulation on the bare wire and connector as well.
[0094] The compositions described herein can be used to manufacture a cable joint intended to seal the cable ends of one or more cables having a thermoplastic polyolefin or rubber cable insulation, the cable joint sealing the cable ends of one or more cables having a thermoplastic polyolefin or rubber cable insulation.
[0095] The composition as described above can be used in the manufacture of cable accessories as cable joints or cable termination materials in high voltage direct current applications, such as high voltage direct current power cable applications. The cured silicone composition according to the present invention can be used in the construction of any kind of field grading assemblies, such as geometric, capacitive, refractive, resistive, or nonlinear field grading assemblies for high voltage direct current (HVDC) applications. The cured silicone composition can also be used in field grading assemblies for high voltage direct current (HVDC) applications, where in addition to the field grading material, it acts essentially or exclusively in the insulating layer as an insulator that further contributes to reducing electrical stress. In certain cases, it can act as a field grading material, especially in resistive field grading assemblies cable joints, cable terminal applications, cable accessories, and connectors. EXAMPLES
[0096] Separate compositions using non-fluorinated polydiorganosiloxane polymers were prepared and identified as LSR1, LSR2, LSR3, and HCR1. LSR1, 2, and 3 compositions are prepared in two parts since they are hydrosilylation cured. The composition of LSR is shown in Table 1a, and the composition of HCR1 is shown in Table 1b below. All viscosities are given at 25°C unless otherwise noted. The vinyl content and Si-H content of the polymers were measured by quantitative IR according to ASTM E168. [Table 1] [Table 2]
[0097] HCR1 was cured using a peroxide catalyst, hereafter referred to as Peroxide 1, which is a 45% paste of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane in silicone, which is commercially available under various trade names such as DHBP-45-PSI (United Initiators). Peroxide 1 was added to the composition in an amount of 1 part per 100 parts of HCR1.
[0098] Separate compositions using fluorinated polydiorganosiloxane polymers were prepared and identified as F-LSR1, F-LSR2, and FSR1. F-LSR1 was prepared in two parts since it was hydrosilylation cured. The compositions of F-LSR1 and F-LSR2 are shown in Table 2a, the compositions of F-LSR3 and F-LSR4 in Table 2b, and the composition of FSR-1 in Table 2c. [Table 3] [Table 4] [Table 5]
[0099] Hardening Sheet Cured sheets were prepared at 0.5 mm or 1 mm thickness using a compression mold and hydraulic press set at 300 psi (2.068 MPa) and a temperature of 170° C. The sheets were cured for 10 minutes. If necessary, the cured sheets were hung in a ventilated oven and post-cured at 200° C. for up to 4 hours.
[0100] Example 1-F - Blends of LSR1 and LSR1 were prepared using the parts by weight indicated, cured sheets were prepared as above, and the volume resistivity of each cured sheet was measured. In this case, the sheets were not post-cured.
[0101] All necessary part A materials were mixed together first, and all necessary part B materials were similarly mixed together, and the resulting intermediate mixtures were then combined to obtain the final overall formulation. The blends used are shown in Table 3a, and the volume resistivity results obtained are shown in Table 3b below. [Table 6]
[0102] In accordance with ASTM D257-14: Standard Test Methods for DC Resistance or Conductance of Insulating Materials, the volume resistivity of the volume resistivity (VR) test was measured on cured sheets with thickness ranging from 0.5 to 2 mm using a Keithley® 8009 test cell in combination with a Keithley® 5 1 / 2 digit Model 6517B electrometer / high resistance meter, controlled by Model 6524 high resistance measurement software.
[0103] Within the Model 6524 High Resistance Measurement Software, alternating polarity testing was implemented as a "Hi-R" test to minimize the effects of background currents, as described in detail in the Keithley White Paper "Improving the Repeatability of Ultra-High Resistance and Resistivity Measurements" by Adam Daire.
[0104] To minimize the effects of background currents, the Hi-R AC polarity test was used, a method designed to improve high resistance / resistivity measurements that are prone to large errors due to background currents.
[0105] An alternating polarity stimulation voltage was used to separate the stimulation current from background currents. When using the alternating polarity method, the voltage source output of the electrometer alternates between two voltages: offset voltage + AC V and offset voltage - AC V at regular intervals (measurement time).
[0106] A current measurement (Imeas) is taken at the end of each switch. After four Imeas values are collected, a current reading is calculated (Icalc). Icalc is the binomial weighted average of the last four current measurements (Imeas1 through Imeas4). Icalc=(1 * Imeas1-3 * Imeas2+3 * Imeas3-1 * Imeas4) / 8 The symbols used for the four terms are the polarity of the AC portion of the voltage that produces the respective current. This calculation of the stimulation current is not affected by background current levels, gradients, or curvatures, effectively isolating the stimulation current from the background current. The result is a reproducible value of the stimulation current and resistance or resistivity calculated therefrom. The time dependence of the stimulation current is a material property; i.e., different results are obtained when using different measurement times due to the properties of the material.
[0107] A measurement time of 60 seconds was used, typically with three voltage cycles of +1000 V then -1000 V. From the six measured currents obtained, the software obtained three Icalc values, the first of these was rejected and then the next two values were used to calculate VR=(V max -V min VR is calculated from: VR x Area / (2 x Icalc x Sample Thickness). The two resulting VR values were averaged to obtain the final value. For the polymer blends shown in the examples, the weighted average VR is: Calculated based on: Calculated Blend VR = (% mass component A x VR component A) + (% mass component B x VR component B). [Table 7]
[0108] It is clear that in all examples the achieved change in VR is much larger than would be predicted from the calculated blended VR.
[0109] For Examples 1-2 and 1-3, the number of duplicates was measured and the results were statistically analyzed using Student's t-test. This clearly showed that the measured differences between the means were not zero at a 99% confidence level, and therefore the volume resistivity could be well controlled within the desired range. These results are shown in Table 3c below. [Table 8]
[0110] Example 2 - Blends of F-LSR1 and LSR2 were prepared using the parts by weight as shown in Table 4a below. [Table 9]
[0111] Cured sheets of the blends were prepared as described above and the VR was measured for each sheet using the method and apparatus previously described. [Table 10]
[0112] The physical properties of Example 2-1 were also determined and compared to those of the Comparative Examples, which can be found in Table 4c below. [Table 11]
[0113] Elasticity 100means the modulus value at 100% elongation. Example 2-1 shows that it is not necessary to add F-LSR equally to both parts of the formulation to achieve the desired VR modification. Example 2-1 also shows that it is possible to maintain good mechanical properties while achieving the desired VR modification. Example 2-2 shows that further modification of VR can be achieved depending on the formulation.
[0114] Example 3 - Blends of F-LSR2 and LSR2 were prepared using the parts by weight as shown in Table 5a below. [Table 12]
[0115] Cured sheets of the blends were prepared as described above and the VR was measured for each sheet using the method and apparatus previously described. [Table 13]
[0116] It is clear that in all examples, the change achieved in VR is much greater than would be predicted from the calculated blend VR. For Examples 3-1 through 3-3, the measured VR is significantly lower than for Example 3-4, with the lowest VR unexpectedly observed for Example 3-1, which has the lowest level of F-LSR2. Mechanical properties were also measured for Example 3-3 and Comparative Example 3, as shown in Table 5c below. [Table 14]
[0117] EB means elongation at break. Example 3-3 shows good physical properties with actually improved tear strength and dielectric strength over Comparative Example 3.
[0118] Example 4 - Blends of HCR1 and FSR1 were prepared using the parts by weight as shown in Table 6a below. Peroxide 1 was used as the curing catalyst and 0.5 mm thick cured sheets were prepared and post-cured at 200° C. for 1 hour. The volume resistivity of the resulting sheets was then measured and the results are also shown in Table 6a below. [Table 15]
[0119] The physical properties of the product of Example 4 were also determined as shown in Table 6b below. [Table 16]
[0120] It is clear that in all examples the change achieved in VR is much greater than would be predicted from the calculated blend VR. The examples also demonstrate that it is possible to achieve the desired reduction in volume resistivity while maintaining good mechanical properties.
[0121] Example 5 Blends of F-LSR3 or F-LSR4 and LSR3 were prepared using the parts by weight shown in Table 7a below. All necessary part A blend ingredients were first mixed together and all necessary part B blend ingredients were also mixed together. Example formulations were then prepared by mixing the part A and part B blends in a 1:1 ratio. [Table 17]
[0122] Cured sheets of the blends were prepared as described above and the sheets were post-cured as described above for 4 hours at 200° C. The VR of each sheet was measured using the method and equipment described above. [Table 18]
[0123] It is clear that all materials experience some increase in volume resistivity after post-cure, but the degree of increase is significantly reduced when F-LSR is used without a cure package. For Example 5-2, the change in volume resistivity after post-cure is particularly small. Mechanical properties were also measured for the examples after 4 post-curing at 200°C, as shown in Table 7c below. [Table 19]
[0124] Example 5-1 shows good mechanical properties when the F-LSR includes a cure package. The results of Examples 5-2 to 5-4 show that the mechanical properties are not significantly degraded when the F-LSR is used without a cure package.
Claims
1. 1. A curable silicone elastomer composition for use in high voltage DC insulation comprising: (A)(i) is a non-fluorinated polydiorganosiloxane in an amount of 50 to 99.5 weight percent of component A; (A)(ii) a combination of (A)(A)(i) and (A)(ii), which is a fluorinated polydiorganosiloxane polymer in an amount of 0.5 to 50 weight percent of component A; (B) at least one reinforcing filler; (C) is at least one organohydrogenpolysiloxane (C)(i), at least one hydrosilylation catalyst (C)(ii), and optionally at least one cure inhibitor (C)(iii); or (D) at least one of (C) or (D), which is at least one peroxide catalyst; The composition is a curable silicone elastomer composition containing ≦0.1% by weight of the composition of a conductive or semi-conductive filler or mixtures thereof.
2. 1. A high voltage DC insulator comprising an elastomeric product of a curable silicone elastomer composition or obtained by curing a silicone elastomer composition, said silicone elastomer composition comprising: (A)(i) is a non-fluorinated polydiorganosiloxane having at least two alkenyl groups per molecule in an amount of 50 to 99.5% by weight of component A; (A)(ii) a blend of (A)(i) and (A)(ii), which is a fluorinated polydiorganosiloxane polymer having at least two alkenyl groups per molecule, in an amount of 0.5 to 50 weight percent of component A; (B) at least one reinforcing filler; (C) is at least one organohydrogenpolysiloxane (C)(i), at least one hydrosilylation catalyst (C)(ii), and optionally at least one cure inhibitor (C)(iii); or (D) at least one of (C) or (D), which is at least one peroxide catalyst; The composition is a high voltage DC insulator containing ≦0.1% by weight of the composition of a conductive or semiconductive filler or mixtures thereof.
3. 1. A high voltage DC insulator comprising an elastomeric product of a curable silicone elastomer composition or obtained by curing a silicone elastomer composition, said silicone elastomer composition comprising: (A)(i) is a non-fluorinated polydiorganosiloxane having at least two alkenyl groups per molecule in an amount of 50 to 99.5% by weight of component A; (A)(ii) a blend of (A)(i) and (A)(ii), which is a fluorinated polydiorganosiloxane polymer having no alkenyl groups, in an amount of 0.5 to 50 weight percent of component A; (B) at least one reinforcing filler; (C) is at least one organohydrogenpolysiloxane (C)(i), at least one hydrosilylation catalyst (C)(ii), and optionally at least one cure inhibitor (C)(iii); or (D) at least one of (C) or (D), which is at least one peroxide catalyst; The composition is a high voltage DC insulator containing ≦0.1% by weight of the composition of a conductive or semiconductive filler or mixtures thereof.
4. 4. The high voltage DC insulator of claim 2 or 3, characterized in that the composition contains 0 (zero) weight percent conductive filler.
5. A high voltage DC insulator as described in any one of claims 2 to 4, characterized in that when component (C) is present, (A)(i) must have at least two alkenyl groups per molecule and (A)(ii) either does not contain at least two alkenyl groups per molecule.
6. The curable silicone elastomer composition of claim 1, wherein the presence of at least two alkenyl groups per molecule in (A)(i) and (A)(ii) is optional when the hydrosilylation catalyst of component (C) is not present and component (D) is the sole catalyst.
7. A high voltage DC insulator comprising an elastomeric product of the curable silicone elastomer composition of claim 6, or comprising an elastomeric product obtained by curing the curable silicone elastomer composition of claim 6.
8. 8. The high voltage direct current insulator of any one of claims 2 to 5 and 7 used as an insulator adapted to reduce electrical stress in high voltage direct current (HVDC) applications, used alone or as part of an article or assembly.
9. 10. The high voltage DC insulator of claim 8, wherein the article or assembly is a cable accessory, a cable joint or cable termination material, a boot, a sleeve, and / or other fittings in a high voltage DC application.
10. A cable accessory comprising the high voltage DC insulator according to any one of claims 2 to 5 and 7.
11. 11. The cable accessory of claim 10, selected from the group consisting of a cable joint, a cable termination, and a cable connector, each for high voltage direct current applications.
12. 13. A method for making high voltage direct current insulation comprising the steps of: preparing a composition according to claim 1 or 6; and mixing and curing said composition together, said mixing step being able to be: (a) mixing all individual components together; (b) if the composition is in two parts, mixing the two parts together; and (c) if the composition is in four parts, mixing the four parts together, in each case immediately prior to curing.
13. The method for producing a high voltage DC insulator as described in claim 12, wherein the curable silicone elastomer composition may alternatively be further processed by injection molding, encapsulation molding, press molding, dispenser molding, extrusion molding, transfer molding, press vulcanization, centrifugal casting, calendar molding, bead coating or blow molding.
14. 14. A method for manufacturing high voltage direct current insulation as claimed in claim 12 or 13, wherein the composition is either introduced into a mould before curing to form a moulded silicone article, or the composition is either injection moulded to form an article or over moulded by injection moulding around an article, used alone or as part of an article or assembly.
15. Use of a curable silicone elastomer composition, comprising: (A)(i) is a non-fluorinated polydiorganosiloxane in an amount of 50 to 99.5 weight percent of component A; (A)(ii) a combination of (A)(A)(i) and (A)(ii), which is a fluorinated polydiorganosiloxane polymer in an amount of 0.5 to 50 weight percent of component A; (B) at least one reinforcing filler; (C) is at least one organohydrogenpolysiloxane (C)(i), at least one hydrosilylation catalyst (C)(ii), and optionally at least one cure inhibitor (C)(iii); or (D) at least one of (C) or (D), which is at least one peroxide catalyst; 2. Use of the composition in or as a high voltage DC insulator, said composition containing ≦0.1% by weight of said composition of a conductive or semi-conductive filler or mixtures thereof.
16. 10. Use of the curable silicone elastomer composition according to claim 1 or 6 for the reduction of electrical stress in high voltage direct current (HVDC) applications or as an insulator for high voltage direct current (HVDC) applications.
Citation Information
Patent Citations
Silicone rubber composition
JP2000248183A
Curable resin composition, cured product of the same and optical semiconductor device
JP2014221880A
Use of silicone rubber composition for the manufacture of insulators for high-voltage DC applications