All-solid-state secondary battery, its manufacturing method, its use method and its charging method

By optimizing the charge capacity ratio and using amorphous carbon with specific surface area and oil absorption in the negative electrode layer, the battery addresses dendritic growth issues, enhancing both cycle and discharge rate characteristics in all-solid-state secondary batteries.

JP7573370B2Active Publication Date: 2024-10-25SAMSUNG ELECTRONICS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020013978
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-01-30
Publication Date
2024-10-25
Estimated Expiration
2040-01-30

AI Technical Summary

Technical Problem

Existing all-solid-state secondary batteries using lithium as a negative electrode material face issues with dendritic growth of metallic lithium, leading to short circuits and decreased charging capacity due to insufficient improvement in battery characteristics.

Method used

The ratio of the initial charge capacity of the positive electrode active material layer to the negative electrode active material layer is set within a predetermined range, with the negative electrode active material layer composed of amorphous carbon having a large structure, ensuring a specific surface area and oil absorption, thereby reducing the number of interfaces and enhancing lithium diffusion.

Benefits of technology

This configuration results in an all-solid-state secondary battery with improved cycle characteristics and discharge rate characteristics by suppressing dendritic growth and maintaining lithium distribution within the negative electrode layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573370000004
    Figure 0007573370000004
  • Figure 0007573370000005
    Figure 0007573370000005
  • Figure 0007573370000006
    Figure 0007573370000006
Patent Text Reader

Abstract

To provide an all-solid type secondary battery superior in battery characteristics, especially cycle characteristic and discharge-rate characteristic, and a charging method thereof.SOLUTION: An all-solid type secondary battery comprises a positive electrode active material layer, a solid electrolyte layer, and a layer of a negative electrode active material which forms an alloy or compound in combination with lithium in this order, wherein the negative electrode active material layer contains amorphous carbon of 33 mass% or more, to a total mass of the negative electrode active material, which satisfies at least one of the requirements, (a) a nitrogen adsorption specific surface area of over 0 m2 / g and 100 m2 / g or less and (b) the DBP oil absorption of 150 ml / 100 g or more; and the ratio of an initial charging capacity of the positive electrode active material layer and an initial charging capacity of the negative electrode active material layer satisfies a condition given by the following expression (1): 0.01<b / a<0.5 (1) (where "a" is an initial charging capacity (mAh) of the positive electrode active material layer and "b" is an initial charging capacity (mAh) of the negative electrode active material layer).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an all-solid-state secondary battery, a method for producing the same, a method for using the same, and a method for charging the same. [Background technology]

[0002] In recent years, all-solid-state secondary batteries using solid electrolytes as electrolytes have been attracting attention. In order to increase the energy density of such all-solid-state secondary batteries, it has been proposed to use lithium as the negative electrode active material. The capacity density (capacity per unit mass) of lithium is about 10 times that of graphite, which is commonly used as a negative electrode active material. Therefore, by using lithium as the negative electrode active material, it is possible to increase the output of the all-solid-state secondary battery while making it thinner.

[0003] As an all-solid-state secondary battery using lithium as the negative electrode active material, there has been proposed a battery that does not have a negative electrode active material layer, but deposits metallic lithium at the interface between the negative electrode current collector and the solid electrolyte by charging, and uses the deposited metallic lithium as the negative electrode active material. However, in this type of all-solid-state secondary battery, when the battery is repeatedly charged and discharged, the deposited metallic lithium grows in a dendritic shape (dendrite shape) so as to weave through the gaps in the solid electrolyte. The metallic lithium that grows in a dendritic shape not only can cause a short circuit in the secondary battery, but can also cause a decrease in the charging capacity.

[0004] In order to solve such problems, Patent Document 1 discloses that a metal layer made of lithium or a metal that forms an alloy with lithium is used as the negative electrode active material layer, and an interface layer made of amorphous carbon is provided on the negative electrode active material layer, whereby lithium ions are dispersed in the interface layer, thereby suppressing the deposition and growth of metallic lithium. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2011-086554 A [Non-Patent Document 1] Naoki Suzuki et al., "Synthesis and Electrochemical Properties of I4--type Li1+2xZn1-xPS4 Solid Electrolyte", Chemistry of Materials, March 9, 2018, No. 30, 2236-2244 (2018) Summary of the Invention [Problem to be solved by the invention]

[0006] However, the all-solid-state secondary battery described in the above-mentioned Patent Document 1 still fails to sufficiently improve various battery characteristics, and is considered to be insufficient to meet recent demands.

[0007] Therefore, a main object of the present invention is to provide an all-solid-state secondary battery having excellent battery characteristics, particularly excellent cycle characteristics and discharge rate characteristics, and a charging method thereof. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that an all-solid-state secondary battery excellent in both cycle characteristics and discharge rate characteristics can be obtained by setting the ratio of the initial charge capacity of each of the positive electrode active material layer and the negative electrode active material layer within a predetermined range and by containing a predetermined amount or more of amorphous carbon having a large structure or amorphous carbon having a large particle size as the negative electrode active material. That is, by containing a predetermined amount or more of amorphous carbon having such characteristics in the negative electrode active material layer, the number of interfaces between carbon particles or carbon particle aggregates is reduced, lithium diffusion in the negative electrode active material layer is facilitated, and an all-solid-state secondary battery excellent in both cycle characteristics and discharge rate characteristics can be obtained, which led to the present invention.

[0009] That is, a first aspect of the present invention is an all-solid-state secondary battery having, in this order, a positive electrode active material layer, a solid electrolyte layer, and a negative electrode active material layer that forms an alloy or compound with lithium, wherein the negative electrode active material layer has: (a) a nitrogen adsorption specific surface area of ​​0 m 2 / g over 100m 2 and (b) an amorphous carbon having an initial charge capacity of 100 ml / 100 g or less, based on the total mass of the negative electrode active material, the amorphous carbon satisfying at least one of (a) an initial charge capacity of 100 ml / 100 g or less, and (b) a DBP oil absorption of 150 ml / 100 g or more, the ratio of the initial charge capacity of the positive electrode active material layer to the initial charge capacity of the negative electrode active material layer satisfies the following formula (1): 0.01 (wherein a is the initial charge capacity (mAh) of the positive electrode active material layer, and b is the initial charge capacity (mAh) of the negative electrode active material layer).

[0010] In a second aspect of the present invention, the nitrogen adsorption specific surface area of ​​the amorphous carbon is 20 m 2 / g or more, 100m 2 / g or less.

[0011] In a third aspect of the present invention, the nitrogen adsorption specific surface area of ​​the amorphous carbon is 30 m 2 / g or more, 100m 2 / g or less.

[0012] A fourth aspect of the present invention is the all-solid-state secondary battery of any one of the first to third aspects, wherein the amorphous carbon has a DBP oil absorption of 150 ml / 100 g or more and 400 ml / 100 g or less.

[0013] A fifth aspect of the present invention is the all-solid-state secondary battery of the fourth aspect, wherein the amorphous carbon has a DBP oil absorption of 200 ml / 100 g or less.

[0014] A sixth aspect of the present invention is the all-solid-state secondary battery of any one of the first to fifth aspects, wherein the negative electrode active material layer further contains at least one selected from the group consisting of gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, indium, and zinc. ​

[0015] A seventh aspect of the present invention is the all solid state secondary battery of any one of the first to sixth aspects, wherein the negative electrode active material layer contains the amorphous carbon in a total amount of 33 mass % or more and 95 mass % or less based on the total mass of the negative electrode active material.

[0016] An eighth aspect of the present invention is the all solid state secondary battery of any one of the first to seventh aspects, wherein the amorphous carbon is carbon black.

[0017] A ninth aspect of the present invention is the all solid state secondary battery of any one of the first to eighth aspects, wherein the carbon black is at least one selected from the group consisting of furnace black, acetylene black, and ketjen black.

[0018] A tenth aspect of the present invention is a method for charging an all-solid-state secondary battery according to any one of the first to ninth aspects, comprising charging the all-solid-state secondary battery beyond an initial charge capacity of the negative electrode active material layer.

[0019] An eleventh aspect of the present invention is the method for charging the all-solid-state secondary battery of the tenth aspect, wherein the charge capacity is between two and 100 times the initial charge capacity of the negative electrode active material layer. Effect of the Invention

[0020] According to the present invention, it is possible to provide an all-solid-state secondary battery excellent in both cycle characteristics and discharge rate characteristics, and a charging method thereof. [Brief description of the drawings]

[0021] [Figure 1] 1 is a cross-sectional view illustrating a schematic configuration of an all-solid-state secondary battery according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a schematic configuration of the all-solid-state secondary battery according to the embodiment after the negative electrode active material layer is overcharged. [Diagram 3] FIG. 11 is a cross-sectional view showing a modified example of an all-solid-state secondary battery according to another embodiment of the present invention. [Figure 4]FIG. 11 is a cross-sectional view showing a modified example of an all-solid-state secondary battery according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] An embodiment of the all-solid-state secondary battery of the present invention will be described below. Note that the embodiment described below is an example of an all-solid-state secondary battery for embodying the technical idea of ​​the present invention, and the present invention is not limited to the following. In addition, the following description may explain mechanisms that can improve various characteristics of the all-solid-state secondary battery. These are mechanisms that the inventors have devised based on the knowledge they have obtained at the present time, and do not limit the technical scope of the present invention.

[0023] <1. Structure of all-solid-state secondary battery> The all-solid-state secondary battery 1 of this embodiment is a so-called lithium secondary battery that is charged and discharged by the movement of lithium ions between a positive electrode and a negative electrode. Specifically, the all-solid-state secondary battery 1 includes a positive electrode layer 10, a negative electrode layer 20, and a solid electrolyte layer 30 disposed between the positive electrode layer 10 and the negative electrode layer 20, as shown in FIG.

[0024] (1) Positive electrode layer The positive electrode layer 10 includes a positive electrode current collector 11 and a positive electrode active material layer 12 arranged in this order toward the negative electrode layer 20 .

[0025] The positive electrode current collector 11 is in the form of a plate or foil and is made of, for example, one metal selected from the group consisting of indium, copper, magnesium, stainless steel, titanium, iron, cobalt, nickel, zinc, aluminum, germanium, and lithium, or an alloy of two or more metals.

[0026] The positive electrode active material layer 12 reversibly absorbs and releases lithium ions. Specifically, the positive electrode active material layer 12 contains a positive electrode active material and a solid electrolyte.

[0027] As specific embodiments of the positive electrode active material, for example, lithium salts such as lithium cobaltate (hereinafter referred to as LCO), lithium nickelate, lithium nickel cobaltate, lithium nickel cobalt aluminum oxide (hereinafter referred to as NCA), lithium nickel cobalt manganese oxide (hereinafter referred to as NCM), lithium manganate, and lithium iron phosphate, and lithium sulfide can be mentioned. The positive electrode active material layer 12 may contain only one kind selected from these compounds as the positive electrode active material, or may contain two or more kinds.

[0028] The positive electrode active material preferably contains a lithium salt of a transition metal oxide having a layered rock salt structure among the above-mentioned lithium salts. Here, the "layered rock salt structure" means a structure in which oxygen atom layers and metal atom layers are alternately and regularly arranged in the <111> direction of the cubic rock salt structure, and as a result, each atomic layer forms a two-dimensional plane. The "cubic rock salt structure" means a sodium chloride type structure which is a kind of crystal structure. Specifically, it represents a structure in which the face-centered cubic lattices formed by each of the cations and anions are displaced from each other by 1 / 2 of the edge of the unit cell.

[0029] As such a lithium salt of a transition metal oxide having a layered rock salt structure, for example, LiNi x Co y Al z O 2 (NCA), or LiNi x Co y Mn z O 2 (NCM) (however, 0 <x <1, 0 <y <1, 0 <z <1, and x + y + z = 1), etc., lithium salts of ternary transition metal oxides can be mentioned. By the positive electrode active material layer 12 containing a lithium salt of a ternary transition metal oxide having such a layered rock salt structure as the positive electrode active material, the energy density and thermal stability of the all-solid-state secondary battery 1 can be improved.

[0030] Here, examples of the shape of the positive electrode active material include particle shapes such as a perfect sphere and an oval sphere. The particle size of the positive electrode active material is not particularly limited, and may be within a range applicable to the positive electrode active material of a conventional all-solid-state secondary battery. The content of the positive electrode active material in the positive electrode active material layer 12 is also not particularly limited, and may be within a range applicable to the positive electrode layer of a conventional all-solid-state secondary battery.

[0031] The positive electrode active material may be covered with a coating layer. This coating layer may be a known coating layer for the positive electrode active material of an all-solid-state secondary battery. Specific examples of the material for the coating layer include Li 2 O-ZrO 2 etc.

[0032] The solid electrolyte contained in the positive electrode active material layer 12 may be the same as or different from the solid electrolyte contained in the solid electrolyte layer 30 described below.

[0033] Furthermore, the positive electrode active material layer 12 may further contain, in addition to the positive electrode active material and the solid electrolyte, for example, a known conductive assistant, a binding agent (binder), a filler, a dispersant, and the like.

[0034] (2) Negative electrode layer The negative electrode layer 20 includes a negative electrode current collector 21 and a negative electrode active material layer 22 arranged in this order toward the positive electrode layer 10 .

[0035] The negative electrode current collector 21 is in the form of a plate or foil. The negative electrode current collector 21 is preferably made of a material that does not react with lithium, i.e., does not form any alloy or compound. Examples of materials that make up the negative electrode current collector 21 include copper, stainless steel, titanium, iron, cobalt, and nickel. The negative electrode current collector 21 may be made of any one of these metals, or may be made of an alloy or clad material of two or more metals.

[0036] The negative electrode active material layer 22 contains a negative electrode active material that forms an alloy or a compound with lithium. The negative electrode active material layer 22 contains amorphous carbon as a negative electrode active material that forms an alloy or a compound with lithium. Specific examples of amorphous carbon include carbon black such as acetylene black, furnace black, and ketjen black, and graphene. The negative electrode active material layer 22 may contain one or more types of amorphous carbon selected from these.

[0037] The all-solid-state secondary battery 1 of this embodiment is characterized in that the negative electrode active material layer 22 contains, as the negative electrode active material, amorphous carbon that satisfies at least one of the following (a) or (b), in a total amount of 33 mass% or more relative to the total mass of the negative electrode active material: (a) Nitrogen adsorption specific surface area is 0m 2 / g over 100m 2 / g or less (b) DBP oil absorption amount is 150ml / 100g or more

[0038] (Nitrogen adsorption specific surface area is 0m 2 / g over 100m 2 / g or less) The nitrogen adsorption specific surface area of ​​the amorphous carbon contained as the negative electrode active material is 100 m 2 By making the carbon particle size equal to or less than 1 / g, the particle size of the carbon increases, and the number of times that lithium is conducted through the grain boundaries of the carbon particles decreases. This facilitates the diffusion of lithium in the negative electrode active material layer 22. As a result, lithium is less likely to be isolated in the negative electrode layer during discharge, and the cycle characteristics and discharge rate characteristics of the all-solid-state secondary battery 1 can be improved.

[0039] The nitrogen adsorption specific surface area of ​​the amorphous carbon contained as the negative electrode active material is 20 m 2 / g or more, and 2 / g or more is more preferable, and 2 When the lower limit of the nitrogen adsorption specific surface area of ​​the amorphous carbon is within this range, the discharge rate characteristics can be further improved.

[0040] Here, the "nitrogen adsorption specific surface area" of the amorphous carbon contained in the negative electrode active material layer 22 as the negative electrode active material refers to the nitrogen adsorption specific surface area of ​​the one type of amorphous carbon when the negative electrode active material layer 22 contains one type of amorphous carbon, or refers to the nitrogen adsorption specific surface area of ​​each of the multiple types of amorphous carbon when the negative electrode active material layer 22 contains multiple types of amorphous carbon.

[0041] The nitrogen adsorption specific surface area of ​​the amorphous carbon contained in the negative electrode active material layer 22 can be measured by the nitrogen adsorption method (JIS K6217-2:2001). Specifically, amorphous carbon such as carbon black, which has been degassed once at a high temperature of about 300°C, is cooled to liquid nitrogen temperature under a nitrogen atmosphere. The mass increase (nitrogen adsorption amount) of the carbon sample after reaching an equilibrium state and the nitrogen atmosphere pressure at that time are measured, and the nitrogen adsorption specific surface area can be calculated by applying the BET (Brunauer-Emmett-Teller) equation.

[0042] (DBP oil absorption amount is 150ml / 100g or more) By making the DBP oil absorption of the amorphous carbon contained as the negative electrode active material 150 ml / 100 g or more, the size of the aggregate (primary agglomerate) of the carbon particles becomes large, and the diffusion of lithium through the inside of the aggregate becomes easy. Therefore, the diffusion of lithium becomes easy in the negative electrode active material layer 22, and lithium is less likely to be isolated in the negative electrode layer during discharge, and the cycle characteristics and discharge rate characteristics of the all-solid-state secondary battery 1 are improved.

[0043] The DBP oil absorption of the amorphous carbon contained as the negative electrode active material is preferably 400 ml / 100 g or less, more preferably 200 ml / 100 g or less. When the upper limit of the DBP oil absorption of the amorphous carbon is in such a range, the discharge rate characteristics can be further improved.

[0044] Here, the "DBP oil absorption" of the amorphous carbon contained in the negative electrode active material layer 22 as the negative electrode active material means the DBP oil absorption of the one type of amorphous carbon when the negative electrode active material layer 22 contains one type of amorphous carbon, or means the DBP oil absorption of each of the multiple types of amorphous carbon when the negative electrode active material layer 22 contains multiple types of amorphous carbon.

[0045] The DBP oil absorption of the amorphous carbon contained in the negative electrode active material layer 22 can be calculated by measuring the DBP oil absorption in accordance with JIS K6217-4:2008. Specifically, dibutyl phthalate (DBP) is titrated with a constant-speed burette into a sample that is being stirred by a rotor. As DBP is added, the mixture changes from a freely flowing powder to a slightly viscous mass. The end point of this measurement is when the torque generated by the change in viscosity characteristic reaches a set value or a certain percentage of the maximum torque obtained from the torque curve. The DBP oil absorption (ml / 100g) can be calculated by dividing the volume (ml) of DBP at the end point by the mass (g) of the sample and multiplying the result by 100.

[0046] The negative electrode active material layer 22 may contain only amorphous carbon as a negative electrode active material that forms an alloy or compound with lithium, or may further contain, in addition to amorphous carbon, at least one element selected from the group consisting of gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, indium, and zinc.

[0047] Here, when at least one selected from gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, indium, and zinc is contained as the negative electrode active material, the particle size of the negative electrode active material is preferably 4 μm or less, and more preferably 100 nm or less. With such a particle size, the output characteristics and cycle characteristics of the all-solid-state secondary battery 1 are further improved. Here, the particle size of the negative electrode active material is measured, for example, using a laser type particle size distribution system, as a median diameter (so-called D 50) can be used. The lower limit of the particle size is not particularly limited, but may be 10 nm. This effect can be obtained by containing at least one selected from gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, indium, and zinc in a total amount of 5 mass % or more in the negative electrode active material layer 22.

[0048] (Amorphous carbon content is 33% or more by mass in total) If the content of amorphous carbon satisfying the above condition (a) or (b) in the negative electrode active material layer 22 is less than 33 mass% in total, it is not possible to sufficiently improve the cycle characteristics and discharge rate characteristics of the all-solid-state secondary battery 1. Therefore, the content of amorphous carbon satisfying the above condition (a) or (b) in the negative electrode active material layer 22 needs to be 33 mass% or more in total.

[0049] On the other hand, the upper limit of the content of amorphous carbon satisfying the above condition (a) or (b) is not particularly limited, but it is preferably, for example, 95 mass % or less.

[0050] Here, the "content" of amorphous carbon in the negative electrode active material layer 22 means the ratio of the total mass of one or more types of amorphous carbon that satisfy the above-mentioned condition (a) or (b) to the total mass of the negative electrode active material contained in the negative electrode active material layer 22, which is taken as 100 mass%.

[0051] The content of amorphous carbon in the negative electrode active material layer 22 that satisfies the above-mentioned condition (a) or (b) can be measured, for example, by the following method. First, the carbon content in the negative electrode active material layer 22 is measured by a combustion method. Specifically, a sample of the negative electrode active material layer 22 is heated to a high temperature under a helium stream mixed with oxygen, and the carbon dioxide generated is quantified to measure the carbon content in the negative electrode active material layer 22. Furthermore, the particle size distribution is estimated by a laser scattering method, and the number of types of amorphous carbon contained in the negative electrode active material layer 22 is measured. Furthermore, the particle size and structure are observed using a transmission electron microscope (TEM). By combining the above measurement and observation results, information on the number of types of amorphous carbon contained in the negative electrode active material layer 22, the content rate of each type of amorphous carbon, and the particle size and structure of each type of amorphous carbon can be obtained, and the content of amorphous carbon in the negative electrode active material layer 22 that satisfies the above-mentioned condition (a) or (b) can be measured. Of course, the content of amorphous carbon in the negative electrode active material layer 22 that satisfies the above-mentioned condition (a) or (b) in the finished all-solid-state secondary battery 1 can also be estimated from the manufacturing conditions of the negative electrode active material layer 22 (the nitrogen adsorption specific surface area of ​​various amorphous carbons, the DBP oil absorption and content, the content of other negative electrode active materials, etc.).

[0052] The negative electrode active material layer 22 may further contain a binder. By containing a binder, the negative electrode active material layer 22 can be stabilized on the negative electrode current collector 21. Examples of materials constituting the binder include resin materials such as styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene. The binder may be composed of at least one type selected from these resin materials.

[0053] Furthermore, the negative electrode active material layer 22 may contain additives used in conventional all-solid-state secondary batteries, such as a filler, a dispersant, an ion conductive agent, and the like, as appropriate.

[0054] (3) Solid electrolyte layer The solid electrolyte layer 30 is disposed between the positive electrode layer 10 and the negative electrode layer 20 (specifically, between the positive electrode active material layer 12 and the negative electrode active material layer 22). The solid electrolyte layer 30 contains a solid electrolyte capable of transferring ions.

[0055] The solid electrolyte is composed of, for example, a solid electrolyte material mainly composed of sulfide (hereinafter referred to as a sulfide-based solid electrolyte material). 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiX (X is a halogen element such as I or Cl), Li 2 SP 2 S 5 -Li 2 O, Li 2 SP 2 S 5 -Li 2 O-LiI, Li 2 S-SiS 2 , Li 2 S-SiS 2 - LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S.B. 2 S 3 , Li 2 SP 2 S 5 -Z m S n (m and n are positive numbers, Z is Ge, Zn or Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2S-SiS 2 -Li p MO q (p and q are positive numbers, and M is any of P, Si, Ge, B, Al, Ga, and In). The solid electrolyte may be composed of one material selected from these sulfide-based solid electrolyte materials, or may be composed of two or more materials.

[0056] As the solid electrolyte, it is preferable to use, among the above-mentioned sulfide solid electrolyte materials, those containing sulfur (S), phosphorus (P) and lithium (Li) as constituent elements. 2 SP 2 S 5 It is more preferable to use a sulfide-based solid electrolyte material containing Li 2 SP 2 S 5 When using a material containing Li 2 S and P 2 S 5 The mixing molar ratio with Li 2 S:P 2 S 5 It is preferable that the ratio is selected in the range of 50:50 to 90:10.

[0057] The solid electrolyte may be in an amorphous state, a crystalline state, or a mixture of an amorphous state and a crystalline state.

[0058] The solid electrolyte layer 30 may further contain a binder. Examples of the binder material include resins such as styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, and polyacrylic acid. The binder material may be the same as or different from the material constituting the binder in the positive electrode active material layer 12 and the negative electrode active material layer 22.

[0059] (4)Initial charge capacity ratio The all-solid-state secondary battery 1 of this embodiment is configured so that the initial charge capacity of the positive electrode active material layer 12 is excessively large relative to the initial charge capacity of the negative electrode active material layer 22. As described later, in this embodiment, the all-solid-state secondary battery 1 is charged (i.e., overcharged) beyond the initial charge capacity of the negative electrode active material layer 22. At the beginning of charging, lithium is absorbed in the negative electrode active material layer 22. That is, the negative electrode active material forms an alloy or a compound with the lithium ions transferred from the positive electrode layer 10. When charging is performed beyond the initial charge capacity of the negative electrode active material layer 22, as shown in FIG. 2, lithium is precipitated on the back side of the negative electrode active material layer 22, that is, between the negative electrode current collector 21 and the negative electrode active material layer 22, and a metal layer 23 is formed by this lithium. The metal layer 23 is mainly composed of lithium (i.e., metallic lithium). Such a phenomenon occurs when the negative electrode active material is composed of a specific material, that is, a material that forms an alloy or a compound with lithium. During discharge, the lithium in the negative electrode active material layer 22 and the metal layer 23 is ionized and moves to the positive electrode layer 10 side. Therefore, lithium can be used as the negative electrode active material in the all-solid-state secondary battery 1. Furthermore, since the negative electrode active material layer 22 covers the metal layer 23, it functions as a protective layer for the metal layer 23 and can suppress the deposition and growth of dendritic metallic lithium. This suppresses short circuits and capacity reduction of the all-solid-state secondary battery 1, and thus improves the characteristics of the all-solid-state secondary battery 1.

[0060] Specifically, in the all-solid-state secondary battery 1 of this embodiment, the ratio of the initial charge capacity of the positive electrode active material layer 12 to the initial charge capacity of the negative electrode active material layer 22, that is, the initial charge capacity ratio, satisfies the following formula (1). 0.01 (where a is the initial charge capacity (mAh) of the positive electrode active material layer 12, and b is the initial charge capacity (mAh) of the negative electrode active material layer 22).

[0061] ​When the initial charge capacity ratio is 0.01 or less, the characteristics of the all-solid-state secondary battery 1 deteriorate. The reason for this is that the negative electrode active material layer 22 does not function sufficiently as a protective layer. For example, when the thickness of the negative electrode active material layer 22 is very thin, the capacity ratio may be 0.01 or less. In this case, the negative electrode active material layer 22 may collapse due to repeated charging and discharging, and dendritic metallic lithium may precipitate and grow. As a result, the characteristics of the all-solid-state secondary battery 1 deteriorate. Therefore, the initial charge capacity ratio is set to be more than 0.01. On the other hand, if the initial charge capacity ratio is 0.5 or more, the amount of lithium deposited in the negative electrode decreases, resulting in a decrease in battery capacity. Therefore, the initial charge capacity ratio is set to less than 0.5.

[0062] (Method of measuring initial charge capacity) The initial charge capacity of each of the positive electrode active material layer 12 and the negative electrode active material layer 22 can be measured as follows.

[0063] The initial charge capacity of the positive electrode active material layer 12 can be obtained, for example, by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer 12. When multiple types of positive electrode active materials are used, the value of the charge capacity density x mass is calculated for each positive electrode active material, and the sum of these values ​​is taken as the initial charge capacity of the positive electrode active material layer 12.

[0064] The initial charge capacity of the negative electrode active material layer 22 is calculated in a similar manner. That is, the initial charge capacity of the negative electrode active material layer 22 can be obtained, for example, by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the negative electrode active material layer 22. When multiple types of negative electrode active materials are used, the value of the charge capacity density x mass is calculated for each negative electrode active material, and the sum of these values ​​is taken as the initial charge capacity of the negative electrode active material layer 22.

[0065] Here, the charge capacity density of the positive electrode active material and the negative electrode active material is a capacity estimated using an all-solid-state half cell using lithium metal as the counter electrode.

[0066] The initial charge capacities of the positive electrode active material layer 12 and the negative electrode active material layer 22 may be directly measured by a measurement using an all-solid-state half cell. Specific methods for directly measuring the initial charge capacities include the following methods.

[0067] First, the initial charge capacity of the positive electrode active material layer 12 is measured by preparing an all-solid-state half cell using the positive electrode active material layer 12 as the working electrode and Li as the counter electrode, and performing CC-CV charging from the OCV (open circuit voltage) to the upper limit charge voltage. The upper limit charge voltage is defined in the JIS C 8712:2015 standard, and refers to 4.25 V for lithium cobalt oxide-based positive electrodes, and a voltage obtained by applying the provisions of A.3.2.3 (safety requirements when applying a different upper limit charge voltage) of JIS C 8712:2015 for other positive electrodes. The initial charge capacity of the negative electrode active material layer 22 is measured by preparing an all-solid-state half cell using the negative electrode active material layer 22 as the working electrode and Li as the counter electrode, and performing CC-CV charging from the OCV (open circuit voltage) to 0.01 V.

[0068] The all-solid-state half-cell described above can be produced, for example, by the following method. The positive electrode active material layer 12 or the negative electrode active material layer 22 for which the initial charge capacity is to be measured is punched out into a disk shape with a diameter of 13 mm. 200 g of the same solid electrolyte powder as that used in the all-solid-state secondary battery 1 is solidified at 40 MPa to form a pellet shape with a diameter of 13 mm and a thickness of about 1.5 mm. This pellet is placed inside a cylinder with an inner diameter of 13 mm, and the positive electrode active material layer 12 or the negative electrode active material layer 22 punched into a disk shape is placed on one side of the pellet, and a lithium foil with a diameter of 13 mm and a thickness of 0.03 mm is placed on the other side. Furthermore, stainless steel disks are placed one by one on both sides, and the whole is pressurized in the axial direction of the cylinder at a pressure of 300 MPa to 1000 MPa for one minute to integrate the contents. It is preferable to apply a pressure of 300 MPa or more when integrating the contents, since this makes it easier for the contents to adhere to each other. Moreover, even if the pressure is increased above 1000 MPa, the effect becomes flat at higher pressures, so it is preferable to set the pressure at 1000 MPa or less. This can be sealed in a case so that a constant pressure of 22 MPa is applied to create an all-solid-state half-cell.

[0069] <2. Manufacturing method of all-solid-state secondary battery> Next, a description will be given of a method for manufacturing the all-solid-state secondary battery 1. The all-solid-state secondary battery 1 according to this embodiment can be obtained by forming the positive electrode layer 10, the negative electrode layer 20, and the solid electrolyte layer 30, respectively, and then laminating the above layers.

[0070] (1) Positive electrode layer production process First, materials constituting the positive electrode active material layer 12 (positive electrode active material, binder, etc.) are added to a non-polar solvent to prepare a slurry (which may be a paste). Next, the obtained slurry is applied onto the prepared positive electrode current collector 11. This is dried to obtain a laminate. Next, the obtained laminate is pressed using, for example, hydrostatic pressure to obtain the positive electrode layer 10. Note that the pressing step may be omitted.

[0071] (2) Negative electrode layer production process First, materials (negative electrode active material, binder, etc.) constituting the negative electrode active material layer 22 are added to a polar solvent or a non-polar solvent to prepare a slurry (which may be a paste). Next, the obtained slurry is applied onto the prepared negative electrode current collector 21. This is dried to obtain a laminate. Next, the obtained laminate is pressed using, for example, hydrostatic pressure to prepare the negative electrode layer 20. Note that the pressing step may be omitted.

[0072] (3) Solid electrolyte layer production process The solid electrolyte layer 30 can be made of a solid electrolyte formed from a sulfide-based solid electrolyte material.

[0073] First, the starting material (e.g., Li 2 S, P 2 S 5 etc.) to obtain a sulfide-based solid electrolyte material.

[0074] For example, when using the melt quenching method, a sulfide-based solid electrolyte material can be produced by mixing a predetermined amount of starting materials, forming them into pellets, reacting them in a vacuum at a predetermined reaction temperature, and then quenching them. 2 S and P 2 S 5 The reaction temperature of this mixture is preferably 400° C. to 1000° C., and more preferably 800° C. to 900° C. The reaction time is preferably 0.1 hours to 12 hours, and more preferably 1 hour to 12 hours. The quenching temperature of the reaction product is usually 10° C. or lower, and preferably 0° C. or lower, and the quenching rate is usually about 1° C. / sec to 10000° C. / sec, and preferably about 1° C. / sec to 1000° C. / sec.

[0075] In addition, when using the mechanical milling method, the starting raw materials are stirred and reacted using a ball mill, etc., to produce a sulfide-based solid electrolyte material. Note that the stirring speed and stirring time in the mechanical milling method are not particularly limited, but the faster the stirring speed, the faster the production rate of the sulfide-based solid electrolyte material can be, and the longer the stirring time, the higher the conversion rate of the raw materials to the sulfide-based solid electrolyte material can be.

[0076] The resulting mixed raw material (sulfide-based solid electrolyte material) is then heat-treated at a specified temperature and pulverized to produce a particulate solid electrolyte. If the solid electrolyte has a glass transition point, it may change from amorphous to crystalline by heat treatment.

[0077] Next, the solid electrolyte obtained by the above method can be formed into a film by a known film forming method such as an aerosol deposition method, a cold spray method, or a sputtering method to produce the solid electrolyte layer 30. The solid electrolyte layer 30 may be formed by pressing solid electrolyte particles alone. The solid electrolyte layer 30 may also be formed by mixing the solid electrolyte, a solvent, and a binder, applying and drying the mixture, and applying pressure.

[0078] (4)Lamination process The positive electrode layer 10 and the negative electrode layer 20 are disposed so as to sandwich the solid electrolyte layer 30, and the resulting structure is pressurized using, for example, hydrostatic pressure, thereby making it possible to obtain the all-solid-state secondary battery 1 according to this embodiment.

[0079] In addition, when the all-solid-state secondary battery 1 produced by the above method is operated and charged and discharged, the all-solid-state secondary battery 1 may be subjected to pressure. The pressure may be 0.5 MPa or more and 10 MPa or less. The pressure may be applied by sandwiching the all-solid-state battery 1 between two hard plates such as stainless steel, brass, aluminum, glass, etc., and tightening the two plates with a screw. In the all-solid-state battery according to this embodiment, when the charging and discharging are repeated, the metallic lithium precipitated between the interface layer and the negative electrode active material layer may be ionized and dissolved, causing a void. Therefore, by setting the pressure to 0.5 MPa or more, it is possible to suppress the occurrence of the void and to easily suppress the decrease in the battery output. In addition, if the pressure is too large, the battery tends to be short-circuited. Therefore, it is preferable that the pressure is 10 MPa or less.

[0080] <3. Charging method of all-solid-state secondary batteries> Next, a method for charging the all-solid-state secondary battery 1 will be described.

[0081] The method for charging the all-solid-state secondary battery 1 of this embodiment is characterized in that the all-solid-state secondary battery 1 is charged beyond the charge capacity of the negative electrode active material layer 22 (that is, overcharged).

[0082] At the beginning of charging, lithium is absorbed in the negative electrode active material layer 22. When charging is performed beyond the charge capacity of the negative electrode active material layer 22, as shown in FIG. 2, lithium is precipitated on the back side of the negative electrode active material layer 22, that is, between the negative electrode current collector 21 and the negative electrode active material layer 22, and the lithium forms a metal layer 23 that did not exist at the time of manufacture. During discharge, the lithium in the negative electrode active material layer 22 and the metal layer 23 is ionized and moves to the positive electrode layer 10 side. Therefore, in the all-solid-state secondary battery 1, lithium can be used as the negative electrode active material. Furthermore, since the negative electrode active material layer 22 covers the metal layer 23, it can function as a protective layer for the metal layer 23 and can suppress the precipitation and growth of dendritic metallic lithium. This suppresses short-circuiting and capacity reduction of the all-solid-state secondary battery 1, and ultimately improves the characteristics of the all-solid-state secondary battery 1. In addition, in this embodiment, since the metal layer 23 is not formed in advance, the manufacturing cost of the all-solid-state secondary battery 1 can be reduced.

[0083] If the charge amount of the all-solid-state secondary battery 1 is less than twice the initial charge capacity of the negative electrode active material layer 22, the amount of lithium precipitated in the negative electrode layer 20 may decrease, resulting in a decrease in battery capacity. For this reason, it is preferable that the charge amount of the all-solid-state secondary battery 1 is twice or more the initial charge capacity of the negative electrode active material layer 22. On the other hand, if the charge amount of the all-solid-state secondary battery 1 is more than 100 times the initial charge capacity of the anode active material layer 22, the thickness of the anode layer 20 becomes insufficient, and the anode layer 20 may collapse due to repeated charging and discharging, causing dendrites to precipitate and grow. Therefore, it is preferable that the charge amount of the all-solid-state secondary battery 1 is 100 times or less the initial charge capacity of the anode active material layer 22.

[0084] The metal layer 23 is not limited to being formed between the negative electrode current collector 21 and the negative electrode active material layer 22 as shown in Fig. 2, but may be formed inside the negative electrode active material layer 22 as shown in Fig. 3. Furthermore, the metal layer 23 may be formed both between the negative electrode current collector 21 and the negative electrode active material layer 22 and inside the negative electrode active material layer 22 as shown in Fig. 4.

[0085] By charging the all-solid-state secondary battery 1, lithium is precipitated in layers between the negative electrode current collector 21 and the negative electrode active material layer 22 or inside the negative electrode active material layer 22, so that it is possible to suppress the generation of voids inside the all-solid-state secondary battery 1 due to charging and discharging. As a result, it is possible to suppress the increase in pressure inside the all-solid-state secondary battery 1 due to charging and discharging, compared to a case in which lithium is not precipitated in layers.

[0086] As described above, the negative electrode active material layer 22 contains amorphous carbon and, if necessary, one or more selected from the group consisting of gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, indium, and zinc as the negative electrode active material, so that in the case of overcharging, the deposition of lithium on the surface of the negative electrode active material layer 22 on the side of the solid electrolyte layer 30 can be suppressed. As a result, the deposition and growth of dendritic metallic lithium can be suppressed. This suppresses short-circuiting and capacity reduction of the all-solid-state secondary battery, and ultimately improves the characteristics of the all-solid-state secondary battery. EXAMPLES

[0087] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and may be modified within the scope of the above and below-described aims, and all such modifications are within the technical scope of the present invention.

[0088] Example 1 <1. Sample preparation> First, samples (Nos. 1 to 12) of all-solid-state secondary batteries containing amorphous carbon as the negative electrode active material layer were prepared by the following procedure. Each sample of the all-solid-state secondary battery had the same configuration except for the type of amorphous carbon contained in the negative electrode active material layer.

[0089] (1) Preparation of the positive electrode layer LiNi as the positive electrode active material 0.8 Co 0.15 Al 0.05 O 2(NCA) was prepared. This positive electrode active material was treated with Li 2 O-ZrO 2 The solid electrolyte was Li, an Argyrodite-type crystal. 6 P.S. 5 Cl was prepared. Polytetrafluoroethylene (Teflon (registered trademark) binder manufactured by DuPont) was prepared as a binder. Carbon nanofiber (CNF) was prepared as a conductive assistant. These materials were then mixed in a mass ratio of positive electrode active material: solid electrolyte: conductive assistant: binder = 88: 12: 2: 1. The mixture was stretched into a sheet to prepare a positive electrode active material sheet. This positive electrode active material sheet was then formed into a size of about 1.7 cm square and pressed onto a positive electrode current collector made of 18 μm thick aluminum foil to prepare a positive electrode layer.

[0090] (2) Preparation of the negative electrode layer A negative electrode layer containing silver particles and amorphous carbon as the negative electrode active material was prepared as follows. First, 6 g of amorphous carbon (carbon black) and 2 g of silver particles (average particle size about 60 nm, indicated as "Ag" in Table 1) were placed in a container, and 5.1 g of N-methylpyrrolidone (NMP) solution containing 7.77 mass% of binder (#9300 manufactured by Kureha Corporation) was added thereto. Next, NMP was added little by little to this mixed solution while stirring to prepare a slurry. This slurry was applied to a negative electrode current collector made of SUS304 foil with a thickness of 10 μm using a blade coater. Then, it was dried in air at about 80° C. for about 20 minutes, and then vacuum dried at 100° C. for about 12 hours. This laminate was punched out to about 2 cm square to prepare a negative electrode layer. However, this negative electrode layer had a protruding portion, which was used as a negative electrode terminal of a battery as described later. In this manner, the negative electrode layers used in Samples No. 1 to 12 were prepared.

[0091] Here, the negative electrode layer used in each of Samples No. 1 to No. 12 was prepared using one type of amorphous carbon having the nitrogen adsorption specific surface area and DBP oil absorption amount shown in Table 1. The amorphous carbon used in preparing the negative electrode layers of Samples No. 1 to No. 10 was furnace black (represented as "FB" in Table 1). The amorphous carbon used in preparing the negative electrode layers of Samples No. 11 and No. 12 was acetylene black and Ketjen black (represented as "AB" and "KB" in Table 1, respectively). The amorphous carbon contained in the negative electrode active material was prepared so that the nitrogen adsorption specific surface area, DBP oil absorption amount, and content of amorphous carbon in the negative electrode active material layer were the values ​​shown in Table 1. It was confirmed by the above-mentioned measurement method that the nitrogen adsorption specific surface area and DBP oil absorption amount of the amorphous carbon contained in the negative electrode active material layer were the values ​​shown in Table 1 in the samples of the manufactured all-solid-state secondary batteries. The negative electrode layers used in each of Samples No. 1 to 12 were prepared so that the content of amorphous carbon in the negative electrode active material layer was the value shown in Table 1.

[0092] (3) Preparation of solid electrolyte layer The aforementioned Li 6 P.S. 5 A rubber-based binder (A334 manufactured by ZEON) was added to the Cl solid electrolyte in an amount of 1% by mass relative to the mass of the solid electrolyte. A slurry was produced by adding xylene and diethylbenzene to this mixture while stirring it. The slurry was applied onto a nonwoven fabric using a blade coater and dried in air at 40°C. The resulting laminate was vacuum-dried at 40°C for 12 hours. The laminate was punched out to a size of approximately 2.2 cm square to produce a solid electrolyte layer.

[0093] (4) Fabrication of all-solid-state secondary batteries The prepared positive electrode layer, solid electrolyte layer, and negative electrode layer were stacked in this order and sealed in a laminate film in a vacuum to prepare all-solid-state secondary battery samples No. 1 to 12. Here, a part of each of the positive electrode collector and the negative electrode collector was protruded from the laminate film so as not to break the vacuum of the battery. These protruding parts were used as the terminals of the positive electrode layer and the negative electrode layer. Furthermore, this all-solid-state secondary battery was subjected to hydrostatic pressure treatment at 490 MPa for 30 minutes. Furthermore, this all-solid-state secondary battery was sandwiched between two stainless steel plates with a thickness of about 1 cm on both sides in the stacking direction. Each of the two stainless steel plates had four holes at the same positions, and the all-solid-state secondary battery was arranged to be contained inside the rectangle formed by the four holes. In this state, a bolt was passed through each of the four holes so as to penetrate the two stainless steel plates from the outside of the two stainless steel plates. Thereafter, the four bolts were tightened with nuts so as to press down the two stainless steel plates from the outside, thereby applying a pressure of approximately 4 MPa to the all-solid-state secondary battery.

[0094] <2.Initial charging capacity> For the produced all-solid-state secondary battery samples No. 1 to 12, the initial charge capacity (mAh) of the positive electrode active material layer and the initial charge capacity (mAh) of the negative electrode active material layer were measured as follows. Specifically, an all-solid-state half cell was prepared by the method described in paragraphs

[0067] to

[0068] above. Then, the positive electrode active material layer was used as the working electrode and Li as the counter electrode, and CC-CV charging was performed from the OCV (open voltage) to the upper limit charging voltage (specifically, 4.25 V) to measure the initial charge capacity of the positive electrode active material layer. In addition, an all-solid-state half cell was prepared using the negative electrode active material layer as the working electrode and Li as the counter electrode, and CC-CV charging was performed from the OCV (open voltage) to 0.01 V to measure the negative electrode active material layer. The initial charge capacity (mAh) and initial charge capacity ratio of the positive electrode active material layer and the negative electrode active material layer in each sample obtained by the measurement are shown in Table 1.

[0095] <3. Characterization> The fabricated all-solid-state secondary batteries of Samples 1 to 12 were subjected to a charge-discharge cycle test as described below, and the battery characteristics were evaluated.

[0096] (1) Charge / discharge cycle test The all-solid-state secondary battery was placed in a thermostatic chamber at 60°C and a charge-discharge cycle test was performed. In the first cycle, the current was 0.5 mA / cm until the battery voltage reached 4.25 V. 2 The battery was charged at a constant current of 0.5 mA / cm until the current reached 0.2 mA, and then at a constant voltage of 4.25 V until the battery voltage reached 2.5 V. 2 In the second and third cycles, the battery was charged under the same conditions as in the first cycle, with a constant current of 1.67 mA / cm. 2 , 5.0mA / cm 2 The battery was discharged at a constant current of 0.5 mA / cm until the battery voltage reached 2.5 V. From the fourth cycle onwards, the discharge current was increased to 0.5 mA / cm 2 This was repeated for 105 cycles or more, and the battery characteristics of each sample were evaluated.

[0097] (2) Cycle characteristics The cycle characteristics of the all-solid-state secondary battery were evaluated by the capacity retention rate in a charge-discharge cycle test. Specifically, the ratio of the discharge capacity (mAh) at the 105th cycle to the discharge capacity (mAh) at the 5th cycle in the charge-discharge cycle test was defined as the "capacity retention rate (%)." Samples with a capacity retention rate of 88% or more were evaluated as having "excellent cycle characteristics." The measurement results of the capacity retention rate for each sample are shown in Table 1.

[0098] (3) Discharge rate characteristics The discharge rate characteristics of all-solid-state secondary batteries were evaluated by the discharge capacity ratio in a charge-discharge cycle test. Specifically, the ratio (%) of the discharge capacity (mAh) in the third cycle to the discharge capacity (mAh) in the second cycle in the charge-discharge cycle test was defined as the "discharge capacity ratio (%)." Samples with a discharge capacity ratio of 92% or more were evaluated as having "excellent discharge rate characteristics." The measurement results of the discharge capacity ratio for each sample are shown in Table 1.

[0099] [Table 1]

[0100] <4. Evaluation> As shown in Table 1, all of Samples 1, 2, 4 to 7, and 10 to 12 met the requirements of the present invention ((a) nitrogen adsorption specific surface area of ​​0 m 2 / g over 100m 2 The all-solid-state secondary battery is an embodiment that satisfies the above requirements. (a) The amorphous carbon satisfies at least one of (a) a DBP oil absorption of 150 ml / 100 g or less, and (b) a DBP oil absorption of 150 ml / 100 g or more, and contains 33 mass % or more of the amorphous carbon relative to the total mass of the negative electrode active material. All of the samples of these all-solid-state secondary batteries had a capacity retention rate of 88% or more and a discharge capacity ratio of 92% or more, and it was confirmed that they were excellent in both cycle characteristics and discharge rate characteristics. The nitrogen adsorption specific surface area was 30 m 2 / g or more and 100m 2 Samples Nos. 1, 4, 5, 7, and 11, which contain 33 mass % or more of amorphous carbon with a nitrogen adsorption specific surface area of ​​30 m 2 It was found that the discharge capacity ratio was higher and the discharge rate characteristics were further improved compared to sample No. 10, which had a DBP oil absorption of less than 150 ml / 100 g. Also, samples Nos. 1, 2, and 6, which had a DBP oil absorption of 150 ml / 100 g or more and 200 ml / 100 g or less, had higher capacity retention rates and discharge capacity ratios compared to sample No. 4, which had a DBP oil absorption of more than 200 ml / 100 g. This shows that, if the type of amorphous carbon contained is the same, the cycle characteristics and discharge rate characteristics can be further improved by setting the DBP oil absorption to 200 ml / 100 g or less.

[0101] In contrast, Samples Nos. 3, 8, and 9 are all-solid-state secondary batteries as comparative examples that do not satisfy any of the requirements (nitrogen adsorption specific surface area, DBP oil absorption) defined in the present invention, and these samples were inferior in at least either the cycle characteristics or the discharge rate characteristics.

[0102] Specifically, samples Nos. 3, 8, and 9 all had a nitrogen adsorption specific surface area of ​​100 m 2The cyclic characteristics were poor, with a DBP oil absorption of less than 150 ml / 100 g and a particle size of more than 100 μm / g. The reason for the poor cyclic characteristics is believed to be that the particle size and aggregates are small, so that lithium must diffuse across many grain boundaries and aggregate interfaces in order to diffuse through the negative electrode layer. In other words, it is believed to be difficult for lithium to reach the interface between the active material and the solid electrolyte during discharge, resulting in a large amount of lithium being isolated within the negative electrode layer.

[0103] Example 2 In Example 2, samples (Nos. 13 to 16) of all-solid-state secondary batteries in which the content of amorphous carbon contained in the negative electrode active material layer was changed were produced by the following procedure.

[0104] Specifically, one type of amorphous carbon (furnace black) having a nitrogen adsorption specific surface area and DBP oil absorption amount shown in Table 2 and silver particles (average particle size: about 60 nm) were prepared as the negative electrode active material. Then, the amorphous carbon and the silver particles were mixed so that the content of the amorphous carbon relative to the total mass of the negative electrode active material in the negative electrode active material layer was the value shown in Table 2, and the negative electrode layer was produced in the same manner as in Example 1.

[0105] In addition, a positive electrode layer and a solid electrolyte layer were prepared in the same manner as in Example 1, and these were laminated with a negative electrode layer to prepare all-solid-state secondary battery samples Nos. 13 to 16. Then, the prepared samples were evaluated for various battery characteristics in the same manner as in Example 1. The results are shown in Table 2.

[0106] [Table 2]

[0107] As shown in Table 2, all of Samples 13 to 18 satisfy the requirement of the present invention ((a) nitrogen adsorption specific surface area of ​​0 m 2 / g over 100m 2 / g or less, or (b) DBP oil absorption of 150 ml / 100 g or more, and 33 mass % or more of amorphous carbon with respect to the total mass of the negative electrode active material. It was confirmed that all of these all-solid-state secondary battery samples had a capacity retention rate of 88% or more and a discharge capacity ratio of 92% or more, and were excellent in both cycle characteristics and discharge rate characteristics. In addition, a short circuit occurred in sample 13 before the 105th cycle, but as long as the short circuit did not occur, both the cycle characteristics and discharge rate characteristics were high and the battery was sufficiently usable. From the results of Samples No. 13 to 18, it is considered that the content of amorphous carbon relative to the total mass of the negative electrode active material is preferably 33 mass% or more and 95 mass% or less, and more preferably 33 mass% or more and 87.5 mass% or less, relative to the total mass of the negative electrode active material.

[0108] Example 3 In Example 3, samples (Nos. 19 and 20) of all-solid-state secondary batteries containing amorphous carbon as the negative electrode active material layer were produced by the following procedure.

[0109] Specifically, one type of amorphous carbon (Ketjen black) having a nitrogen adsorption specific surface area and DBP oil absorption amount shown in Table 3 and platinum particles (average particle size: about 1 μm) were prepared as the negative electrode active material. Then, the amorphous carbon and the platinum particles were mixed so that the content of the amorphous carbon relative to the total mass of the negative electrode active material in the negative electrode active material layer was the value shown in Table 3, and the negative electrode layer was produced in the same manner as in Example 1.

[0110] In addition, a positive electrode layer and a solid electrolyte layer were prepared in the same manner as in Example 1, and these were laminated with a negative electrode layer to prepare all-solid-state secondary battery samples No. 19 and 20. Various battery characteristics were evaluated for the prepared samples in the same manner as in Example 1. The results are shown in Table 3.

[0111] [Table 3]

[0112] As shown in Table 3, both Samples 19 and 20 met the requirements of the present invention ((a) nitrogen adsorption specific surface area of ​​0 m 2 / g over 100m 2 / g or less, or (b) DBP oil absorption of 150 ml / 100 g or more, and 33 mass % or more of amorphous carbon with respect to the total mass of the negative electrode active material. It was confirmed that all of these samples of all solid state secondary batteries had a capacity retention rate of 88% or more and a discharge capacity ratio of 92% or more, and were excellent in both cycle characteristics and discharge rate characteristics. From this result, it was confirmed that the effect of the present invention can be obtained by using a mixture of amorphous carbon and platinum as the negative electrode active material. [Explanation of symbols]

[0113] 1 All-solid-state secondary battery 10 Positive electrode layer 11 Positive electrode current collector 12 Cathode active material layer 20 Negative electrode layer 21 Negative electrode current collector 22 Negative electrode active material layer 23 Metal layer 30 Solid electrolyte layer

Claims

1. An all-solid-state secondary battery having, in this order, a positive electrode active material layer, a solid electrolyte layer, and a negative electrode active material layer that forms an alloy or a compound with lithium, The negative electrode active material layer is (a) Nitrogen adsorption specific surface area is 0 m 2 / g over 100m 2 / g or less, and (b) DBP oil absorption amount is 150 ml / 100 g or more and 400 ml / 100 g or less, The amorphous carbon that satisfies both of the above items is contained in an amount of 33% by mass or more and 95% by mass or less based on the total mass of the negative electrode active material, a ratio of an initial charge capacity of the positive electrode active material layer to an initial charge capacity of the negative electrode active material layer satisfies the following formula (1): 0.01<b / a<0.5 (1) (wherein a is the initial charge capacity (mAh) of the positive electrode active material layer, and b is the initial charge capacity (mAh) of the negative electrode active material layer).

2. The nitrogen adsorption specific surface area of ​​the amorphous carbon is 20 m 2 / g or more, 100m 2 The all-solid-state secondary battery according to claim 1, wherein the capacitance is 0.1 to 0.5 μm.

3. The nitrogen adsorption specific surface area of ​​the amorphous carbon is 30 m 2 / g or more, 100m 2 The all-solid-state secondary battery according to claim 2 , wherein the capacitance is 0.1 μm or less.

4. The all-solid-state secondary battery according to any one of claims 1 to 3, wherein the amorphous carbon has a DBP oil absorption of 200 ml / 100 g or less.

5. The all-solid-state secondary battery according to any one of claims 1 to 4, wherein the negative electrode active material layer further contains at least one selected from the group consisting of gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, indium and zinc.

6. The all-solid-state secondary battery according to any one of claims 1 to 5, wherein the amorphous carbon is carbon black.

7. 7. The all-solid-state secondary battery according to claim 6, wherein the carbon black is at least one selected from the group consisting of furnace black, acetylene black, and Ketjen Black (registered trademark).

8. 8. The all-solid-state secondary battery according to claim 1 , further comprising a negative electrode current collector laminated on a surface of the negative electrode active material layer opposite to the solid electrolyte layer, the negative electrode current collector being a foil made of stainless steel.

9. 9. The all-solid-state secondary battery according to claim 1, wherein the positive electrode active material layer, the solid electrolyte layer, and the negative electrode active material layer are sealed with a laminate film.

10. A method for producing the all-solid-state secondary battery according to any one of claims 1 to 9, A method for producing an all-solid-state secondary battery, comprising laminating a positive electrode active material layer, a solid electrolyte layer, and a negative electrode active material layer in this order, and pressurizing the laminate using hydrostatic pressure.

11. The method for producing an all-solid-state secondary battery according to claim 10, wherein the pressurization is performed at a pressure of 300 MPa or more.

12. A method for using an all-solid-state secondary battery according to claim 9, characterized in that the all-solid-state secondary battery is charged and discharged while being pressed in a state where it is sandwiched between two hard plates.

13. The method for using an all-solid-state secondary battery according to claim 12, wherein the pressurization is performed at a pressure of 0.5 MPa or more and 10 MPa or less.

14. A method for charging an all-solid-state secondary battery according to any one of claims 1 to 9, comprising charging the all-solid-state secondary battery beyond an initial charge capacity of the negative electrode active material layer.

15. The method for charging an all-solid-state secondary battery according to claim 14, wherein the charge capacity is between 2 times and 100 times the initial charge capacity of the negative electrode active material layer.

Citation Information

Patent Citations

  • All-solid battery

    JP2008103284A

  • Nonaqueous electrolyte battery

    JP2011086554A

  • Solid state battery manufacturing method

    JP2013196933A

  • Lithium ion secondary battery, and method of manufacturing the same

    JP2015118772A

  • Lithium secondary battery

    JP2016100088A