Latex composition and dip-molded product

A latex composition combining nitrile group-containing conjugated diene and crosslinkable polymers with epoxy and carboxyl groups addresses the lack of chemical permeation resistance in gloves, providing improved grip and protection in chemical environments.

JP7574598B2Active Publication Date: 2024-10-29ZEON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020166424
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-10-29
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Existing gloves with excellent wet or dry grip properties lack sufficient chemical permeation resistance, particularly when handling chemicals like oil.

Method used

A latex composition is developed by mixing a nitrile group-containing conjugated diene polymer with a crosslinkable group-containing polymer, where the crosslinkable polymer includes epoxy and carboxyl group-containing monomer units, to achieve both excellent wet grip and chemical permeation resistance.

Benefits of technology

The resulting dip-molded articles exhibit enhanced wet grip properties and improved chemical permeation resistance, making them suitable for protective gloves in environments involving chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574598000001
    Figure 0007574598000001
Patent Text Reader

Abstract

To provide a latex composition capable of giving a dip-molded body having excellent wet grip property and chemical permeability resistance.SOLUTION: There is provided a latex composition obtained by mixing a latex of a nitrile group-containing conjugated diene-based polymer (A) and a latex of a crosslinking group-containing polymer (B), wherein the crosslinking group-containing polymer (B) contains a crosslinking group-containing monomer unit (b1) which is at least one selected from the group consisting of an epoxy group-containing monomer unit, a carboxyl group-containing monomer unit and a monomer unit having two carbon-carbon double bonds in a specific amount and the nitrile group-containing conjugated diene-based polymer (A) and the crosslinking group-containing polymer (B) have a specific glass transition temperature (Tg).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a latex composition, and more particularly to a latex composition which can give a dip-molded article having excellent wet grip properties and chemical permeation resistance. [Background technology]

[0002] Conventionally, protective gloves that have improved solvent resistance, gripping properties, abrasion resistance, etc. by covering fiber gloves with rubber, resin, etc. have been used for various purposes such as manufacturing work in factories, light work, construction work, agricultural work, etc.

[0003] From the viewpoint of workability, such protective gloves are required to have excellent wet grip properties when wet with water or oil, and excellent resistance to chemical permeation.

[0004] For example, Cited Document 1 discloses a glove having a fiber substrate, a first polymer composition that is attached to at least a portion of the fiber substrate to form a polymer coating, and a plurality of protrusion structures that are present on the polymer coating and contain a second polymer composition, wherein the polymer coating and the plurality of protrusion structures contain different polymer compositions. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2015 / 074106 Summary of the Invention [Problem to be solved by the invention]

[0006] According to the technology of Patent Document 1, gloves having excellent wet grip property or dry grip property can be obtained. However, Patent Document 1 does not consider chemical permeation resistance. Therefore, further improvement of chemical permeation resistance is required from the viewpoint of preventing permeation of chemicals when handling chemicals such as oil.

[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a latex composition which can give a dip-molded article having excellent wet grip properties and chemical permeation resistance. [Means for solving the problem]

[0008] As a result of intensive research by the present inventors to solve the above-mentioned problems, they have found that a latex composition comprising a mixture of a latex of a nitrile group-containing conjugated diene polymer (A) and a latex of a crosslinkable group-containing polymer (B), wherein the crosslinkable group-containing polymer (B) contains a specific amount of a crosslinkable group-containing monomer unit (b1), which is at least one type selected from the group consisting of an epoxy group-containing monomer unit, a carboxyl group-containing monomer unit, and a monomer unit having two carbon-carbon double bonds, and the nitrile group-containing conjugated diene polymer (A) and the crosslinkable group-containing polymer (B) have specific glass transition temperatures (Tg), can provide a dip-molded article having excellent wet grip properties and chemical permeation resistance, thereby completing the present invention.

[0009] That is, according to the present invention, there is provided a latex composition obtained by mixing a latex of a nitrile group-containing conjugated diene polymer (A) and a latex of a crosslinkable group-containing polymer (B), wherein the crosslinkable group-containing polymer (B) contains 1 to 100% by weight of a crosslinkable group-containing monomer unit (b1) and 0 to 99% by weight of a monomer unit (b2) copolymerizable with the crosslinkable group-containing monomer unit (b1), the crosslinkable group-containing monomer unit (b1) is at least one selected from the group consisting of an epoxy group-containing monomer unit, a carboxyl group-containing monomer unit, and a monomer unit having two carbon-carbon double bonds, the glass transition temperature (Tg) of the nitrile group-containing conjugated diene polymer (A) is 10°C or lower, and the glass transition temperature (Tg) of the crosslinkable group-containing polymer (B) is higher than 10°C.

[0010] In the latex composition of the present invention, it is preferred that the nitrile group-containing conjugated diene polymer (A) has a methyl ethyl ketone insoluble content of 50% by weight or less, and the crosslinkable group-containing polymer (B) has a methyl ethyl ketone insoluble content of 55% by weight or more. In the latex composition of the present invention, the crosslinkable group-containing monomer unit (b1) is preferably at least one selected from the group consisting of an epoxy group-containing monomer unit and a carboxyl group-containing monomer unit. In the latex composition of the present invention, the crosslinkable group-containing monomer unit (b1) is preferably at least one selected from the group consisting of an epoxy group-containing (meth)acrylic acid ester monomer unit, an allyl glycidyl ether unit, and a (meth)acrylic acid unit. In the latex composition of the present invention, the content of the crosslinkable group-containing polymer (B) is preferably 1 to 60 parts by weight based on 100 parts by weight of the polymer component.

[0011] According to the present invention, there is also provided a dip-molded article made using the above-mentioned latex composition. Furthermore, according to the present invention, there is provided a dip-molded article obtained by immersing a substrate in the above-mentioned latex composition. Effect of the Invention

[0012] According to the present invention, there is provided a latex composition which can give a dip-molded article having excellent wet grip properties and chemical permeation resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The latex composition of the present invention is a latex composition obtained by mixing a latex of a nitrile group-containing conjugated diene polymer (A) and a latex of a crosslinkable group-containing polymer (B), wherein the crosslinkable group-containing polymer (B) contains 1 to 100% by weight of a crosslinkable group-containing monomer unit (b1) and 0 to 99% by weight of a monomer unit (b2) copolymerizable with the crosslinkable group-containing monomer unit (b1), the crosslinkable group-containing monomer unit (b1) is at least one selected from the group consisting of an epoxy group-containing monomer unit, a carboxyl group-containing monomer unit, and a monomer unit having two carbon-carbon double bonds, the glass transition temperature (Tg) of the nitrile group-containing conjugated diene polymer (A) is 10°C or lower, and the glass transition temperature (Tg) of the crosslinkable group-containing polymer (B) is higher than 10°C.

[0014] The nitrile group-containing conjugated diene polymer (A) constituting the latex of the nitrile group-containing conjugated diene polymer (A) is not particularly limited, but for example, a copolymer of an α,β-ethylenically unsaturated nitrile monomer, a conjugated diene monomer, and other copolymerizable ethylenically unsaturated acid monomers used as necessary can be used.

[0015] The α,β-ethylenically unsaturated nitrile monomer is not particularly limited, but an ethylenically unsaturated compound having a nitrile group and preferably having 3 to 18 carbon atoms can be used. Examples of such α,β-ethylenically unsaturated nitrile monomers include acrylonitrile, methacrylonitrile, and halogen-substituted acrylonitrile, and among these, acrylonitrile is particularly preferred. These α,β-ethylenically unsaturated nitrile monomers may be used alone or in combination of two or more.

[0016] The content of the α,β-ethylenically unsaturated nitrile monomer units in the nitrile group-containing conjugated diene polymer is preferably 10 to 45% by weight, more preferably 20 to 40% by weight, and even more preferably 25 to 40% by weight, based on the total monomer units. By setting the content of the α,β-ethylenically unsaturated nitrile monomer units within the above range, the abrasion resistance and chemical permeation resistance of the resulting dip-molded article can be improved.

[0017] As the conjugated diene monomer, a conjugated diene monomer having 4 to 6 carbon atoms such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, etc. is preferred, 1,3-butadiene and isoprene are more preferred, and 1,3-butadiene is particularly preferred. These conjugated diene monomers may be used alone or in combination of two or more.

[0018] The content of the conjugated diene monomer units in the nitrile group-containing conjugated diene polymer is preferably 40 to 80% by weight, more preferably 52 to 78% by weight, and further preferably 55 to 75% by weight, based on the total monomer units. By setting the content of the conjugated diene monomer units within the above range, the abrasion resistance and chemical permeation resistance of the resulting dip-molded article can be improved.

[0019] The nitrile group-containing conjugated diene polymer may be a copolymer of a monomer forming an α,β-ethylenically unsaturated nitrile monomer unit and a monomer forming a conjugated diene monomer unit with another copolymerizable ethylenically unsaturated acid monomer.

[0020] Such other copolymerizable ethylenically unsaturated acid monomers are not particularly limited, and examples thereof include carboxyl group-containing ethylenically unsaturated monomers, monocarboxylate group-containing ethylenically unsaturated monomers, dicarboxylate diester group-containing ethylenically unsaturated monomers, sulfonic acid group-containing ethylenically unsaturated monomers, and phosphoric acid group-containing ethylenically unsaturated monomers.

[0021] The carboxyl group-containing ethylenically unsaturated monomer is not particularly limited, but examples thereof include ethylenically unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid; ethylenically unsaturated polycarboxylic acids and anhydrides thereof such as fumaric acid, maleic acid, itaconic acid, maleic anhydride, and itaconic anhydride; and partial esters of ethylenically unsaturated polycarboxylic acids such as methyl maleate and methyl itaconate.

[0022] The monocarboxylate group-containing ethylenically unsaturated monomer is not particularly limited, but examples thereof include acrylic acid esters such as methyl acrylate; methacrylic acid esters such as methyl methacrylate; and crotonate esters such as methyl crotonate.

[0023] The dicarboxylate group-containing ethylenically unsaturated monomer is not particularly limited, but examples thereof include maleic acid diesters such as dimethyl maleate; itaconic acid diesters such as dimethyl itaconate; and the like.

[0024] Examples of the sulfonic acid group-containing ethylenically unsaturated monomer include, but are not limited to, vinyl sulfonic acid, methyl vinyl sulfonic acid, styrene sulfonic acid, (meth)allyl sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, and 2-acrylamide-2-hydroxypropanesulfonic acid.

[0025] The phosphoric acid group-containing ethylenically unsaturated monomer is not particularly limited, but examples thereof include (meth)acrylic acid-3-chloro-2-propyl phosphate, (meth)acrylic acid-2-ethyl phosphate, and 3-allyloxy-2-hydroxypropane phosphate.

[0026] These other copolymerizable ethylenically unsaturated acid monomers can be used as alkali metal salts or ammonium salts, and may be used alone or in combination of two or more. Among the above-mentioned other copolymerizable ethylenically unsaturated acid monomers, carboxyl group-containing ethylenically unsaturated monomers are preferred, ethylenically unsaturated monocarboxylic acids are more preferred, acrylic acid and methacrylic acid are even more preferred, and methacrylic acid is particularly preferred.

[0027] In the case where the nitrile group-containing conjugated diene polymer contains units of other copolymerizable ethylenically unsaturated acid monomers, the content of the units of other copolymerizable ethylenically unsaturated acid monomers is preferably 0.1 to 15% by weight, more preferably 1 to 10% by weight, and further preferably 2 to 8% by weight, based on the total monomer units.

[0028] The latex of the nitrile group-containing conjugated diene polymer (A) can be obtained, for example, by emulsion polymerization of a monomer mixture containing the above-mentioned monomers. In the emulsion polymerization, commonly used polymerization auxiliary materials such as an emulsifier, a polymerization initiator, and a molecular weight modifier can be used.

[0029] The emulsifier used in the emulsion polymerization is not particularly limited, but examples thereof include anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants, with anionic surfactants being preferred. Specific examples of anionic surfactants include fatty acid salts such as sodium laurate, potassium myristate, sodium palmitate, potassium oleate, sodium linolenate, and sodium rosinate; alkylbenzenesulfonates such as sodium dodecylbenzenesulfonate, potassium dodecylbenzenesulfonate, sodium decylbenzenesulfonate, potassium decylbenzenesulfonate, sodium cetylbenzenesulfonate, and potassium cetylbenzenesulfonate; alkylsulfosuccinates such as sodium di(2-ethylhexyl)sulfosuccinate, potassium di(2-ethylhexyl)sulfosuccinate, and sodium dioctylsulfosuccinate; alkyl sulfates such as sodium lauryl sulfate and potassium lauryl sulfate; polyoxyethylene alkyl ether sulfates such as sodium polyoxyethylene lauryl ether sulfate and potassium polyoxyethylene lauryl ether sulfate; and monoalkyl phosphates such as sodium lauryl phosphate and potassium lauryl phosphate.

[0030] The amount of the emulsifier used in the emulsion polymerization is preferably 0.5 to 10 parts by weight, more preferably 1 to 8 parts by weight, based on 100 parts by weight of the total monomers used.

[0031] The polymerization initiator is not particularly limited, but is preferably a radical initiator.The radical initiator is not particularly limited, but for example, inorganic peroxides such as sodium persulfate, potassium persulfate, ammonium persulfate, potassium perphosphate, and hydrogen peroxide; organic peroxides such as t-butyl peroxide, cumene hydroperoxide, p-menthane hydroperoxide, di-t-butyl peroxide, t-butylcumyl peroxide, acetyl peroxide, isobutyryl peroxide, octanoyl peroxide, dibenzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, and t-butylperoxyisobutyrate; azo compounds such as azobisisobutyronitrile, azobis-2,4-dimethylvaleronitrile, azobiscyclohexanecarbonitrile, and azobisisobutyric acid methyl; and the like.Among these, inorganic peroxides or organic peroxides are preferred, inorganic peroxides are more preferred, and persulfates are particularly preferred. These polymerization initiators may be used alone or in combination of two or more. The amount of the polymerization initiator used is preferably 0.01 to 2 parts by weight, more preferably 0.05 to 1.5 parts by weight, based on 100 parts by weight of the total monomers used.

[0032] The molecular weight regulator is not particularly limited, but examples thereof include α-methylstyrene dimer; mercaptans such as t-dodecyl mercaptan, n-dodecyl mercaptan, and octyl mercaptan; halogenated hydrocarbons such as carbon tetrachloride, methylene chloride, and methylene bromide; sulfur-containing compounds such as tetraethyl thiuram disulfide, dipentamethylene thiuram disulfide, and diisopropyl xanthogen disulfide; and the like. Among these, mercaptans are preferred, and t-dodecyl mercaptan is more preferred. These molecular weight regulators may be used alone or in combination of two or more. The amount of the molecular weight regulator used varies depending on the type, but is preferably 0.1 to 1.5 parts by weight, more preferably 0.2 to 1.0 parts by weight, based on 100 parts by weight of the total monomers used.

[0033] The emulsion polymerization is usually carried out in water. The amount of water used is preferably 80 to 500 parts by weight, more preferably 100 to 200 parts by weight, based on 100 parts by weight of the total monomers used.

[0034] In the emulsion polymerization, if necessary, polymerization secondary materials other than those described above may be further used. Examples of the polymerization secondary materials include a chelating agent, a dispersing agent, a pH adjuster, an oxygen scavenger, a particle size adjuster, etc., and the type and amount of these are not particularly limited.

[0035] Examples of the method of adding the monomers include a method of adding the monomers to be used in a reaction vessel all at once, a method of adding them continuously or intermittently as the polymerization proceeds, a method of adding a part of the monomers and reacting them to a specific conversion rate, and then polymerizing by adding the remaining monomers continuously or intermittently, and any of these methods may be adopted. When the monomers are mixed and added continuously or intermittently, the composition of the mixture may be constant or may be changed. In addition, the various monomers to be used may be mixed in advance and then added to the reaction vessel, or each monomer may be added to the reaction vessel separately.

[0036] The polymerization temperature during emulsion polymerization is not particularly limited, but is usually 0 to 95° C., and preferably 5 to 70° C. The polymerization time is not particularly limited, but is usually about 5 to 40 hours.

[0037] After the polymerization reaction is terminated, if desired, unreacted monomers may be removed and the solids concentration and pH may be adjusted.

[0038] The glass transition temperature (Tg) of the nitrile group-containing conjugated diene polymer (A) is 10°C or lower. If the glass transition temperature (Tg) of the nitrile group-containing conjugated diene polymer (A) exceeds 10°C, it becomes difficult to achieve both wet grip properties and chemical permeation resistance of the dip-molded article obtained. The glass transition temperature (Tg) of the nitrile group-containing conjugated diene polymer (A) is not particularly limited as long as it is 10°C or lower, but is preferably -45 to -10°C, more preferably -40 to -10°C. When the glass transition temperature (Tg) of the nitrile group-containing conjugated diene polymer (A) is in the above range, the flexibility of the dip-molded article obtained can be increased, and the wet grip properties can be further improved. The glass transition temperature (Tg) of the nitrile group-containing conjugated diene polymer (A) can be measured according to JIS K7121.

[0039] The methyl ethyl ketone insoluble content of the nitrile group-containing conjugated diene polymer (A) is not particularly limited, but is preferably 0.01 to 50% by weight, more preferably 0.1 to 30% by weight, and even more preferably 1 to 5% by weight. The methyl ethyl ketone insoluble content of the nitrile group-containing conjugated diene polymer (A) is an index showing the gel content of the nitrile group-containing conjugated diene polymer (A). When the methyl ethyl ketone insoluble content of the nitrile group-containing conjugated diene polymer (A) is within the above range, the flexibility of the obtained dip-molded product can be increased, and the wet grip property can be further improved.

[0040] In the present invention, the method for measuring the methyl ethyl ketone insoluble content of the nitrile group-containing conjugated diene polymer (A) may be, for example, the following method. That is, first, the latex of the nitrile group-containing conjugated diene polymer (A) is applied to a substrate by a casting method or the like, and then dried to obtain a dry film, and the weight of the dry film (this weight is referred to as "W1"). Next, the obtained dry film is immersed in methyl ethyl ketone under conditions of 25°C and 24 hours. Next, the weight of the film after immersion (this weight is referred to as "W2") is measured, and then the film is dried at 105°C for 3 hours to remove the methyl ethyl ketone. Then, the weight of the film after removal of the methyl ethyl ketone (this weight is referred to as "W3") is measured, and the methyl ethyl ketone insoluble content can be calculated from the results of these weight measurements according to the following formulas (1) and (2). Amount of methyl ethyl ketone insolubles (unit: weight%) = (W3 / W1) × 100 (1)

[0041] The method for adjusting the methyl ethyl ketone insoluble content of the nitrile group-containing conjugated diene polymer (A) is not particularly limited, and examples thereof include a method for adjusting the type or amount of a chain transfer agent used when producing a latex of the nitrile group-containing conjugated diene polymer (A), a method for adjusting the polymerization temperature, etc. For example, the more the amount of the chain transfer agent used, the lower the methyl ethyl ketone insoluble content tends to be, and the lower the polymerization temperature, the lower the methyl ethyl ketone insoluble content tends to be.

[0042] The median particle diameter of the nitrile group-containing conjugated diene polymer (A) constituting the latex of the nitrile group-containing conjugated diene polymer (A) is preferably 30 to 1000 nm, more preferably 50 to 500 nm, and even more preferably 70 to 200 nm. By setting the median particle diameter of the nitrile group-containing conjugated diene polymer (A) within the above range, the crosslinkable group-containing polymer (B) described later can be more satisfactorily finely dispersed in the nitrile group-containing conjugated diene polymer (A) in the obtained dip-molded article, thereby improving the flexibility of the obtained dip-molded article and further improving the wet grip property and chemical permeation resistance. The median particle diameter of the nitrile group-containing conjugated diene polymer (A) can be measured, for example, by a laser diffraction scattering method.

[0043] The crosslinkable group-containing polymer (B) constituting the latex of the crosslinkable group-containing polymer (B) used in the present invention contains 1 to 100% by weight of a crosslinkable group-containing monomer unit (b1) and 0 to 99% by weight of a monomer unit (b2) copolymerizable with the crosslinkable group-containing monomer unit (b1).

[0044] The crosslinkable group-containing polymer (B) contains, as the crosslinkable group-containing monomer unit (b1), at least one type selected from the group consisting of an epoxy group-containing monomer unit, a carboxyl group-containing monomer unit, and a monomer unit having two carbon-carbon double bonds.

[0045] The latex composition of the present invention is obtained by mixing the latex of the crosslinkable group-containing polymer (B) containing the crosslinkable group-containing monomer unit (b1) with the latex of the nitrile group-containing conjugated diene polymer (A), and the latex composition obtained by mixing these can provide a dip-molded article having excellent wet grip properties and chemical permeation resistance. The reason why the dip-molded article obtained by using the latex of the crosslinkable group-containing polymer (B) containing the crosslinkable group-containing monomer unit (b1) in the latex composition of the present invention can exhibit excellent wet grip properties and excellent chemical permeation resistance is not necessarily clear, but the following reasons are considered, for example. That is, the particulate crosslinkable group-containing polymer (B) used in the latex composition of the present invention contains the crosslinkable group-containing monomer unit (b1), and therefore can form a crosslinked structure with the nitrile group-containing conjugated diene polymer (A) or other components (for example, zinc oxide) that are mixed as necessary in the latex composition through the crosslinkable group-containing monomer unit (b1). Therefore, in the polymer layer formed from the latex composition of the present invention, a crosslinked structure can be formed between the crosslinkable group-containing polymer (B) and the nitrile group-containing conjugated diene polymer (A) and other components. By forming such a crosslinked structure, it is expected that the aggregation of the crosslinkable group-containing polymer (B) can be suppressed while dispersing the crosslinkable group-containing polymer (B) in the nitrile group-containing conjugated diene polymer (A) in the formed polymer layer, and further, the adhesion of the crosslinkable group-containing polymer (B) to the formed polymer layer can be improved. As a result of these actions due to the formation of the crosslinked structure, it is expected that the obtained dip-molded product can have both excellent wet grip properties and excellent chemical permeation resistance.

[0046] The epoxy group-containing monomer forming the epoxy group-containing monomer unit as the crosslinkable group-containing monomer unit (b1) is not particularly limited as long as it is a monomer having at least one epoxy group in one molecule, and examples thereof include glycidyl (meth)acrylate (abbreviation for "glycidyl acrylate and / or glycidyl methacrylate", the same applies below), 3,4-epoxybutyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, vinyl glycidyl ether, allyl glycidyl ether, 2-methylallyl glycidyl ether, 3,4-epoxy-1-butene, 3,4-epoxy-1-methyl-1-butene, 3,4-epoxy-1-pentene, 3,4-epoxy-3-methyl-1-pentene, 5,6-epoxy-1-hexene, 1,2-vinylcyclohexene monoepoxide, and styrene-p-glycidyl ether. Among these, epoxy group-containing (meth)acrylic acid ester or allyl glycidyl ether is preferred, glycidyl (meth)acrylate or allyl glycidyl ether is more preferred, glycidyl (meth)acrylate is further preferred, and glycidyl methacrylate is particularly preferred.

[0047] The carboxyl group-containing monomer forming the carboxyl group-containing monomer unit as the crosslinkable group-containing monomer unit (b1) is not particularly limited as long as it is a monomer having at least one carboxyl group in one molecule, and examples thereof include ethylenically unsaturated monocarboxylic acids such as (meth)acrylic acid and crotonic acid; ethylenically unsaturated polycarboxylic acids and their anhydrides such as fumaric acid, maleic acid, itaconic acid, maleic anhydride and itaconic anhydride; partial esters of ethylenically unsaturated polycarboxylic acids such as methyl maleate and methyl itaconate; etc. Among these, ethylenically unsaturated monocarboxylic acids are preferred, (meth)acrylic acid is more preferred, and methacrylic acid is even more preferred.

[0048] The unit of the monomer having two carbon-carbon double bonds as the crosslinkable group-containing monomer unit (b1) is a unit formed from a monomer having two carbon-carbon double bonds, and the unit has one carbon-carbon double bond. The monomer having two carbon-carbon double bonds forming the unit of the monomer having two carbon-carbon double bonds as the crosslinkable group-containing monomer unit (b1) is not particularly limited as long as it is a monomer having at least two carbon-carbon double bonds in one molecule, and examples thereof include conjugated diene monomers having 4 to 6 carbon atoms such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and chloroprene; non-conjugated diene monomers such as 1,5-hexadiene, 1,6-heptadiene, 1,7-octadiene, dicyclopentadiene, and 5-ethylidene-2-norbornene; and the like.

[0049] As the crosslinkable group-containing monomer unit (b1), at least one selected from the group consisting of an epoxy group-containing monomer unit and a carboxyl group-containing monomer unit is preferred, at least one selected from the group consisting of an epoxy group-containing (meth)acrylic acid ester monomer unit, an allyl glycidyl ether unit, and a (meth)acrylic acid unit is more preferred, and at least one selected from the group consisting of a (meth)acrylic acid glycidyl unit and a (meth)acrylic acid unit is even more preferred. In particular, when even better wet grip properties are required, as the crosslinkable group-containing monomer unit (b1), an epoxy group-containing monomer unit is preferred, at least one selected from the group consisting of an epoxy group-containing (meth)acrylic acid ester monomer unit and an allyl glycidyl ether unit is more preferred, and a (meth)acrylic acid glycidyl unit is even more preferred. In addition, when even better chemical permeation resistance is required, as the crosslinkable group-containing monomer unit (b1), a carboxyl group-containing monomer unit is preferred, and a (meth)acrylic acid unit is more preferred.

[0050] The content of the crosslinkable group-containing monomer unit (b1) in the crosslinkable group-containing polymer (B) may be 1 to 100% by weight based on the total monomer units, and is not particularly limited, but is preferably 5 to 100% by weight, more preferably 10 to 90% by weight, further preferably 20 to 80% by weight, and particularly preferably 30 to 70% by weight. By setting the content of the crosslinkable group-containing monomer unit (b1) within the above range, the chemical permeation resistance of the obtained dip-molded article can be further improved.

[0051] The crosslinkable group-containing polymer (B) may contain, in addition to the crosslinkable group-containing monomer unit (b1), a monomer unit (b2) copolymerizable with the crosslinkable group-containing monomer unit (b1) (hereinafter, sometimes referred to as monomer unit (b2)).

[0052] The monomer forming the monomer unit (b2) may be any monomer capable of copolymerizing with the crosslinkable group-containing monomer unit (b1), and is not particularly limited thereto. However, it is preferable that the monomer does not contain an epoxy group or a carboxyl group and has only one carbon-carbon double bond. Examples of the monomer unit (b2) include a monocarboxylic acid ester group-containing ethylenically unsaturated monomer, a dicarboxylic acid diester group-containing ethylenically unsaturated monomer, a sulfonic acid group-containing ethylenically unsaturated monomer, a phosphoric acid group-containing ethylenically unsaturated monomer, an α-olefin monomer, and an aromatic monomer. The monomer forming these monomer units (b2) may be used alone or in combination of two or more.

[0053] The monocarboxylic acid ester group-containing ethylenically unsaturated monomer capable of forming the monomer unit (b2) is not particularly limited, but may include acrylic acid esters such as methyl acrylate, methacrylic acid esters such as methyl methacrylate, and crotonate esters such as methyl crotonate.

[0054] The dicarboxylate group-containing ethylenically unsaturated monomer capable of forming the monomer unit (b2) is not particularly limited, but examples thereof include maleic acid diesters such as dimethyl maleate; itaconic acid diesters such as dimethyl itaconate; and the like.

[0055] The sulfonic acid group-containing ethylenically unsaturated monomer capable of forming the monomer unit (b2) is not particularly limited, but examples thereof include vinyl sulfonic acid, methyl vinyl sulfonic acid, styrene sulfonic acid, (meth)allyl sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, and 2-acrylamide-2-hydroxypropanesulfonic acid.

[0056] Examples of the phosphate group-containing ethylenically unsaturated monomer capable of forming the monomer unit (b2) include, but are not limited to, (meth)acrylic acid-3-chloro-2-propyl phosphate, (meth)acrylic acid-2-ethyl phosphate, and 3-allyloxy-2-hydroxypropane phosphate.

[0057] The α-olefin monomer capable of forming the monomer unit (b2) is not particularly limited, but examples thereof include ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene.

[0058] The aromatic monomer capable of forming the monomer unit (b2) is not particularly limited, but examples thereof include styrene, α-methylstyrene, and vinylpyridine.

[0059] As the monomer forming the monomer unit (b2), a monocarboxylate group-containing ethylenically unsaturated monomer is preferable, an acrylic acid ester or a methacrylic acid ester is more preferable, methyl acrylate or methyl methacrylate is further preferable, and methyl methacrylate is particularly preferable.

[0060] The content of the monomer unit (b2) in the crosslinkable group-containing polymer (B) may be 0 to 99% by weight based on the total monomer units, and is not particularly limited, but is preferably 0 to 95% by weight, more preferably 10 to 90% by weight, further preferably 20 to 80% by weight, and particularly preferably 30 to 70% by weight. By setting the content of the monomer unit (b2) within the above range, the chemical permeation resistance of the obtained dip-molded article can be further improved.

[0061] The latex of the crosslinkable group-containing polymer (B) can be obtained, for example, by emulsion polymerization of a monomer mixture containing the above-mentioned monomers.

[0062] The glass transition temperature (Tg) of the crosslinkable group-containing polymer (B) is more than 10°C. If the glass transition temperature (Tg) of the crosslinkable group-containing polymer (B) is 10°C or less, it is difficult to achieve both wet grip properties and chemical permeation resistance of the obtained dip-molded body. The glass transition temperature (Tg) of the crosslinkable group-containing polymer (B) is not particularly limited as long as it is more than 10°C, but is preferably 30°C or more, more preferably 40°C or more. In addition, the upper limit of the glass transition temperature (Tg) of the crosslinkable group-containing polymer (B) is not particularly limited, but is preferably 200°C or less, more preferably 150°C or less. When the glass transition temperature (Tg) of the crosslinkable group-containing polymer (B) is in the above range, the flexibility of the obtained dip-molded body can be increased, and the wet grip properties can be further improved. The glass transition temperature (Tg) of the crosslinkable group-containing polymer (B) can be measured according to JIS K7121.

[0063] The crosslinkable group-containing polymer (B) preferably has a methyl ethyl ketone insoluble content of 55 to 99% by weight, more preferably 70 to 97% by weight. The methyl ethyl ketone insoluble content is an index showing the gel content of the crosslinkable group-containing polymer (B). When the methyl ethyl ketone insoluble content of the crosslinkable group-containing polymer (B) is within the above range, the flexibility of the obtained dip-molded article can be increased.

[0064] In the present invention, the method for measuring the methyl ethyl ketone insoluble content of the crosslinkable group-containing polymer (B) can be, for example, the same method as that for the latex of the nitrile group-containing conjugated diene polymer (A) described above.

[0065] The method for adjusting the methyl ethyl ketone insoluble content of the crosslinkable group-containing polymer (B) constituting the latex of the crosslinkable group-containing polymer (B) is not particularly limited, and examples thereof include a method for adjusting the type and amount of a chain transfer agent used when producing the latex of the crosslinkable group-containing polymer (B), a method for adjusting the polymerization temperature, a method for adjusting the type of crosslinkable group-containing monomer unit (b1), the type of monomer unit (b2), the ratio of each monomer, weight average molecular weight, etc. constituting the crosslinkable group-containing polymer (B), etc.

[0066] The median particle diameter of the crosslinkable group-containing polymer (B) constituting the latex of the crosslinkable group-containing polymer (B) is preferably 80 to 200 nm, more preferably 80 to 150 nm, and even more preferably 80 to 100 nm. By setting the median particle diameter of the crosslinkable group-containing polymer (B) within the above range, the crosslinkable group-containing polymer (B) can be more satisfactorily finely dispersed in the nitrile group-containing conjugated diene polymer (A) in the obtained dip-molded article, thereby improving the flexibility of the obtained dip-molded article and further improving the wet grip property and chemical permeation resistance. The median particle diameter of the crosslinkable group-containing polymer (B) can be measured, for example, by a laser diffraction scattering method.

[0067] The latex composition of the present invention is a latex composition obtained by mixing a latex of a nitrile group-containing conjugated diene polymer (A) and a latex of a crosslinkable group-containing polymer (B), and preferably is obtained by mixing them in a latex state.

[0068] The content of the nitrile group-containing conjugated diene polymer (A) and the content of the crosslinkable group-containing polymer (B) in the latex composition of the present invention are not particularly limited, but the content of the nitrile group-containing conjugated diene polymer (A) in 100 parts by weight of the polymer component contained in the latex composition (in the case where only the nitrile group-containing conjugated diene polymer (A) and the crosslinkable group-containing polymer (B) are contained as the polymer component, the total of 100 parts by weight of the nitrile group-containing conjugated diene polymer (A) and the crosslinkable group-containing polymer (B)) is preferably 40 to 99 parts by weight, more preferably 50 to 95 parts by weight, and even more preferably 60 to 80 parts by weight. The content of the crosslinkable group-containing polymer (B) relative to 100 parts by weight of the polymer component contained in the latex composition is preferably 1 to 60 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 20 to 40 parts by weight. Furthermore, the content ratio of the nitrile group-containing conjugated diene polymer (A) and the crosslinkable group-containing polymer (B) in the latex composition of the present invention is preferably 99:1 to 40:60, more preferably 95:5 to 50:50, and even more preferably 80:20 to 60:40, in terms of the weight ratio of "nitrile group-containing conjugated diene polymer (A):crosslinkable group-containing polymer (B)". By setting the contents of the nitrile group-containing conjugated diene polymer (A) and the crosslinkable group-containing polymer (B) within the above ranges, the wet grip property and chemical permeation resistance of the obtained dip-molded article can be further improved.

[0069] Moreover, the latex composition of the present invention preferably further contains a sulfur-based crosslinking agent in addition to the latex of the nitrile group-containing conjugated diene polymer (A) and the latex of the crosslinkable group-containing polymer (B).

[0070] The sulfur-based crosslinking agent is not particularly limited, but examples thereof include powdered sulfur, sulfur flowers, precipitated sulfur, colloidal sulfur, surface-treated sulfur, insoluble sulfur, and other sulfur; sulfur-containing compounds such as sulfur chloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, dibenzothiazyl disulfide, caprolactam disulfide, phosphorus-containing polysulfide, and polymeric polysulfides; sulfur-donating compounds such as tetramethylthiuram disulfide, dimethyldithiocarbamate selenium, and 2-(4'-morpholinodithio)benzothiazole; etc. These sulfur-based crosslinking agents may be used alone or in combination of two or more.

[0071] The content of the sulfur-based crosslinking agent is preferably 0.01 to 5 parts by weight, more preferably 0.05 to 3 parts by weight, and further preferably 0.1 to 2 parts by weight, based on 100 parts by weight of the polymer component contained in the latex composition.

[0072] In addition to the sulfur-based crosslinking agent, the latex composition of the present invention preferably further contains a crosslinking accelerator (vulcanization accelerator) and zinc oxide. The crosslinking accelerator (vulcanization accelerator) is not particularly limited, but examples thereof include dithiocarbamic acids such as diethyldithiocarbamic acid, dibutyldithiocarbamic acid, di-2-ethylhexyldithiocarbamic acid, dicyclohexyldithiocarbamic acid, diphenyldithiocarbamic acid, and dibenzyldithiocarbamic acid, and zinc salts thereof; 2-mercaptobenzothiazole, 2-mercaptobenzothiazole zinc, 2-mercaptothiazoline, dibenzothiazyl disulfide, and 2-(2,4-dinitrophenylthio)benzo. Thiazole, 2-(N,N-diethylthiocarbamoylthio)benzothiazole, 2-(2,6-dimethyl-4-morpholinothio)benzothiazole, 2-(4'-morpholinodithio)benzothiazole, 4-morpholinyl-2-benzothiazyl disulfide, 1,3-bis(2-benzothiazyl mercaptomethyl)urea, etc., are included, and among these, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, 2-mercaptobenzothiazole, and zinc 2-mercaptobenzothiazole are preferred. These crosslinking accelerators may be used alone or in combination of two or more.

[0073] The content of the crosslinking accelerator is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the polymer components contained in the latex composition. The content of the zinc oxide is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the polymer components contained in the latex composition.

[0074] The latex composition of the present invention may further contain a water-soluble polymer.

[0075] Examples of the water-soluble polymer include vinyl compounds such as polyvinyl alcohol and polyvinylpyrrolidone, cellulose derivatives and salts thereof such as hydroxyethyl cellulose, hydroxypropyl cellulose and carboxymethyl cellulose, polycarboxylic acid compounds and sodium salts thereof such as polyacrylic acid, polyoxyethylene derivatives such as polyethylene glycol ether, etc. As the water-soluble polymer, cellulose derivatives and salts thereof are preferred, and carboxymethyl cellulose and its sodium salt are more preferred.

[0076] The water-soluble polymer may be any polymer that is soluble in water, and the solubility of the water-soluble polymer in water is not particularly limited, but is preferably 1 g or more, more preferably 7 g or more, and particularly preferably 10 g or more, per 100 g of water at a temperature of 25° C. The upper limit of the solubility of the water-soluble polymer in water is not particularly limited, but is usually 1,000 g or less.

[0077] The weight average molecular weight (Mw) of the water-soluble polymer is not particularly limited, but is preferably 100 or more, more preferably 1,000 or more, and is preferably 5,000,000 or less, more preferably 3,000,000 or less.

[0078] The content of the water-soluble polymer is preferably 0.01 to 10 parts by weight, and more preferably 0.1 to 5 parts by weight, based on 100 parts by weight of the polymer component contained in the latex composition.

[0079] The solid content of the latex composition of the present invention is preferably 20 to 65% by weight, more preferably 30 to 60% by weight, and further preferably 35 to 55% by weight. By controlling the solid content of the latex composition to be within the above range, the transport efficiency of the latex composition can be improved, and the viscosity of the latex composition becomes appropriate, improving the handleability of the latex composition.

[0080] The pH of the latex composition of the present invention is preferably 5 to 13, more preferably 7 to 10, and further preferably 7.5 to 9. By adjusting the pH of the latex composition within the above range, the mechanical stability is improved and the generation of coarse aggregates during transportation of the latex composition can be suppressed, and the viscosity of the latex composition becomes appropriate, improving the handleability of the latex composition.

[0081] The viscosity of the latex composition of the present invention at 25°C is preferably 2,000 to 100,000 mPa·s, more preferably 2,500 to 50,000 mPa·s, and further preferably 3,000 to 20,000 mPa·s. The viscosity of the latex composition at 25°C can be measured, for example, using a Brookfield viscometer at 25°C and a rotation speed of 6 rpm. The viscosity of the latex composition at 25°C can be adjusted, for example, by adjusting the concentration of the polymer component in the latex composition or by adding a compound having a thickening effect to the latex composition.

[0082] The latex composition of the present invention may contain fillers such as carbon black, silica, calcium carbonate, aluminum silicate, magnesium silicate, calcium silicate, magnesium oxide, zinc (meth)acrylate, magnesium (meth)acrylate, titanium oxide, etc. The latex composition of the present invention may contain, if necessary, predetermined amounts of additives other than the water-soluble salts and fillers, such as antioxidants, antioxidants, preservatives, antibacterial agents, wetting agents, dispersants, pigments, dyes, reinforcing agents, and pH adjusters.

[0083] The latex composition of the present invention can be prepared, for example, by mixing the above-mentioned components. The order of mixing the components is not particularly limited, but from the viewpoint of further increasing the dispersibility of each component, it is preferable to previously mix the latex of the conjugated diene polymer (A) and the latex of the polymer (B), and then add and mix each component to be blended as necessary. The method of mixing the latex of the conjugated diene polymer (A) and the latex of the polymer (B) is not particularly limited, but from the viewpoint of further increasing the dispersibility, it is preferable to mix the latex of the conjugated diene polymer (A) and the latex of the polymer (B) in the latex state (latex blend).

[0084] <Dip-molded body> The dip-molded article of the present invention is a molded article obtained by using the above-mentioned latex composition of the present invention.

[0085] The dip-molded article of the present invention is a molded article obtained by using the latex composition of the present invention described above, and therefore has at least a polymer layer containing the above-mentioned nitrile group-containing conjugated diene polymer (A) and the above-mentioned crosslinkable group-containing polymer (B). The preferred range of the content ratio of the nitrile group-containing conjugated diene polymer (A) and the crosslinkable group-containing polymer (B) in the dip-molded article of the present invention is the same as the preferred range of the content ratio of the nitrile group-containing conjugated diene polymer (A) and the crosslinkable group-containing polymer (B) in the latex composition of the present invention described above.

[0086] The dip-molded article may be a dip-molded article made of a latex composition obtained by immersing a dip-molding mold in a latex composition such as the above-mentioned latex composition of the present invention, or may be a laminate of a substrate and a polymer layer made of a latex composition obtained by immersing the substrate in a latex composition. In the following, a case where the dip-molded article of the present invention is a laminate of a substrate and a polymer layer made of a latex composition will be described as an example, but the present invention is not limited to such an embodiment.

[0087] The substrate is not particularly limited, but when the dip-molded article is used as a protective glove, a fiber substrate can be suitably used. The fiber substrate is not particularly limited, but for example, a fiber made of twisted monofilament yarn can be used, and the twisted yarn can be woven into a glove shape. The average thickness of the fiber substrate is preferably 50 to 3,000 μm, more preferably 100 to 2,000 μm.

[0088] The dip-molded article can be produced, for example, by immersing a substrate in a latex composition to form a polymer layer made of the latex composition on the substrate. In this case, it is preferable to immerse the substrate in the latex composition in a state in which the substrate is covered in advance with a mold having a desired shape.

[0089] The mold for covering the substrate is not particularly limited, and various materials such as ceramic, glass, metal, and plastic can be used. The shape of the mold can be a desired shape according to the shape of the final product. For example, when the dip-molded product is used as a protective glove, it is preferable to use various types of molds for gloves, such as a mold having a shape from the wrist to the fingertips, as the mold for covering the substrate.

[0090] In addition, before immersing the substrate in the latex composition, it is preferable to immerse the substrate in a coagulant solution in advance to adhere the coagulant solution to the substrate. In this case, it is preferable to immerse the substrate in the coagulant solution in a state in which the substrate is covered with a mold having a desired shape in advance. Examples of the mold having a desired shape include those mentioned above. In addition, it is preferable to remove the solvent contained in the coagulant solution by drying after adhering the coagulant solution to the substrate. The drying temperature at this time is not particularly limited and may be selected depending on the solvent used, but is preferably 10 to 80°C, more preferably 15 to 70°C. In addition, the drying time is not particularly limited, but is preferably 600 to 1 second, more preferably 300 to 5 seconds.

[0091] Next, the substrate with the coagulant solution applied thereto is placed over a molding die of a desired shape and is then immersed in the latex composition to coagulate the latex composition and form a polymer layer made of the latex composition on the substrate.

[0092] After the substrate is immersed in the latex composition, it is preferable to dry the substrate. The drying temperature is not particularly limited, but is preferably 10 to 80° C., and more preferably 15 to 80° C. The drying time is not particularly limited, but is preferably 120 minutes to 5 seconds, and more preferably 60 minutes to 10 seconds.

[0093] When a latex composition containing a sulfur-based crosslinking agent is used, the latex composition may be aged in advance (also referred to as pre-vulcanization).

[0094] The temperature condition for aging is not particularly limited, but is preferably 20 to 50° C. The aging time is preferably 4 hours or more and 120 hours or less, more preferably 24 hours or more and 72 hours or less, from the viewpoint of preventing peeling between the substrate and the polymer layer made of the latex composition and from the viewpoint of improving the abrasion resistance of the obtained dip-molded article.

[0095] Next, it is preferable to heat the latex composition attached to the substrate to crosslink the polymer components contained in the latex composition.

[0096] The heating temperature for crosslinking is preferably 60 to 160° C., more preferably 80 to 150° C. By setting the heating temperature within the above range, the time required for the crosslinking reaction can be shortened to improve the productivity of the dip-molded article, and the oxidative deterioration of the polymer component due to excessive heating can be suppressed to improve the physical properties of the obtained dip-molded article. The heating time for crosslinking may be appropriately selected depending on the heating temperature, but is usually 5 to 120 minutes.

[0097] For the dip-formed article thus obtained, it is preferable to remove water-soluble impurities (emulsifiers, water-soluble polymers, coagulants, etc.) from the polymer layer by immersing the polymer layer formed on the substrate in hot water at 20 to 80° C. for about 0.5 to 60 minutes, if necessary. Although the treatment of immersing the polymer layer in hot water may be carried out after crosslinking the polymer components in the polymer layer, it is preferable to carry out the treatment before crosslinking the polymer components in the polymer layer, in order to more efficiently remove water-soluble impurities.

[0098] After immersion in warm water, drying may be further performed. The drying temperature and drying time in this case are not particularly limited, but can be the same as the drying temperature and drying time in the drying step after immersion in the latex composition described above.

[0099] Then, after forming a polymer layer on the substrate while the substrate is covered with the mold as described above, the substrate is detached from the mold (or demolded) to obtain a dip-molded article. The detachment method can be a method of peeling from the mold by hand or by using water pressure or compressed air pressure.

[0100] Before or after the dip-molded article is detached from the molding die, it may be further subjected to a heat treatment (post-crosslinking step) for 10 to 120 minutes at a temperature of 60 to 120° C. After the dip-molded article is detached from the molding die, a surface treatment layer may be formed on the inner and / or outer surface of the dip-molded article by a chlorination treatment, a coating treatment or the like.

[0101] The dip-molded article thus obtained is a polymer layer made of the latex composition of the present invention formed on a substrate by coagulation using a coagulant, and therefore the thickness of the polymer layer is preferably relatively thick, such as 0.05 to 1.0 mm, more preferably 0.06 to 0.8 mm, even more preferably 0.07 to 0.7 mm, and particularly preferably more than 0.3 mm and 0.7 mm or less. By making the thickness of the polymer layer within the above range, the abrasion resistance of the obtained dip-molded article can be improved.

[0102] The dip-molded article of the present invention uses the above-mentioned latex composition of the present invention, and therefore has excellent oil grip properties, flexibility, and chemical permeation resistance, and can be suitably used, for example, for glove applications, particularly for protective gloves. In the above, the dip-molded article of the present invention is a laminate of a substrate and a polymer layer made of a latex composition, but as described above, the present invention is not limited to such an embodiment, and it is of course possible to use, for example, a dip-molded article made of a latex composition obtained by immersing a dip-molding mold in a latex composition. EXAMPLES

[0103] The present invention will be described below in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" are by weight unless otherwise specified. Tests and evaluations were performed according to the following.

[0104] <Glass transition temperature (Tg)> The glass transition temperature (Tg) of each polymer (polymers (A-1), (B-1) to (B-6) and (B'-7)) was measured using a differential thermal analyzer ("EXSTAR DSC6220" manufactured by SII NanoTechnology Inc.) in accordance with JIS K7121.

[0105] <Methyl ethyl ketone insoluble content> Each latex of the polymers (polymers (A-1), (B-1) to (B-6) and (B'-7)) was applied to a substrate by a casting method, and dried at 25°C for 120 hours to obtain a dry film. The weight of the dry film obtained (this weight is referred to as "W1") was measured. Next, the dry film obtained was immersed in methyl ethyl ketone at 25°C for 24 hours, and the weight of the film after immersion (this weight is referred to as "W2") was measured. The film was then dried at 105°C for 3 hours to remove the methyl ethyl ketone. The weight of the film after removal of the methyl ethyl ketone (this weight is referred to as "W3") was measured, and the weight measurement results were used to calculate the methyl ethyl ketone insoluble content according to the following formula (1). Amount of methyl ethyl ketone insolubles (unit: weight%) = (W3 / W1) × 100 (1)

[0106] <Particle size of polymer particles> The median particle diameter of the latex of each polymer (polymer (A-1), (B-1) to (B-6) and (B'-7)) was measured by a laser diffraction scattering method using a particle size measuring device (Beckman Coulter "LS13320").

[0107] <Wet grip (oil grip)> A cylindrical metal mold weighing 0.6 kg and a weight weighing 0.5 kg were prepared, and test oil IRM903 was applied to the metal mold. Then, workers were asked to wear protective gloves and lift the metal mold with the test oil IRM903 applied. Once they were able to lift it, weights were added one by one, and the maximum weight they could lift was calculated. A total of two workers performed the same task, and the average value of the maximum weight they could lift was calculated. The higher the maximum weight they could lift, the better the wet grip (oil grip) was judged to be.

[0108] <Chemical permeability resistance> The oil permeability was measured according to the following procedure. (1) A protective glove was cut into a suitable circular shape to be used as a sample. (2) The weight of the filter paper (W1) was measured. (3) The weight (W2) of 2 mL of test oil IRM903 was measured and placed in a reagent bottle. (4) The sample was placed on top of a reagent bottle containing test oil IRM903 so that the rubber layer of the sample was in contact with the liquid. (5) The reagent bottle and the sample were firmly attached using a fixture. (6) To allow the test oil IRM903 to come into contact with the sample, the reagent bottle was turned upside down, placed on a piece of filter paper whose weight (W1) had been measured in advance, and left at room temperature. (7) After leaving it for 72 hours, the weight of the filter paper (W3) was measured. (8) The percentage of the test oil IRM903 that permeated the sample (oil permeability) was calculated using the following formula. Oil permeability (%) = (W3-W1) ÷ W2 × 100 It can be determined that the smaller the oil permeability value, the better the resistance to chemical permeation against chemicals such as oil.

[0109] <Production Example 1> (Preparation of Latex of Nitrile Group-Containing Conjugated Diene Polymer (A-1)) In a polymerization reactor, 68 parts of 1,3-butadiene as a conjugated diene monomer, 27 parts of acrylonitrile as an α,β-ethylenically unsaturated nitrile monomer, 5 parts of methacrylic acid as an ethylenically unsaturated monocarboxylic acid monomer, 0.5 parts of t-dodecyl mercaptan, 132 parts of ion-exchanged water, 3 parts of sodium dodecylbenzenesulfonate, 0.5 parts of sodium salt of β-naphthalenesulfonic acid formalin condensate, 0.3 parts of potassium persulfate, and 0.05 parts of sodium salt of ethylenediaminetetraacetate were charged, and the polymerization temperature was maintained at 30 to 40°C to carry out polymerization until the polymerization conversion rate reached 94%, thereby obtaining a latex of a copolymer. Then, after removing unreacted monomers from the obtained copolymer latex, the pH and solid content concentration of the copolymer latex were adjusted to obtain a latex of a nitrile group-containing conjugated diene polymer (A-1) having a solid content concentration of 40% by weight and a pH of 8.

[0110] The monomer composition of the nitrile group-containing conjugated diene polymer (A-1) contained in the latex of the obtained nitrile group-containing conjugated diene polymer (A-1) was measured, and the monomer composition was almost the same as the charged ratio. In addition, the glass transition temperature (Tg), methyl ethyl ketone insoluble content, and median diameter of the nitrile group-containing conjugated diene polymer (A-1) contained in the latex of the obtained nitrile group-containing conjugated diene polymer (A-1) were measured according to the above-mentioned method, and the glass transition temperature (Tg) was -27°C and the median diameter was 126 nm.

[0111] <Production Example 2> (Preparation of latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1)) In a polymerization reactor, 5 parts of glycidyl methacrylate, 95 parts of methyl methacrylate, 6 parts of benzenesulfonic acid ester of 1,1'-oxybistetrapropylene derivative, 0.1 parts of t-dodecyl mercaptan, 200 parts of ion-exchanged water, 1.5 parts of potassium persulfate, and 0.1 parts of sodium ethylenediaminetetraacetate were charged, and polymerization was carried out while maintaining the polymerization temperature at 30 to 70°C, and the reaction was continued until the polymerization conversion rate reached 95%, thereby obtaining a polymer latex. Then, by adjusting the pH and solid content concentration of the polymer latex, a latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1) with a solid content concentration of 30% by weight and pH=8.5 was obtained. The glass transition temperature (Tg), methyl ethyl ketone insoluble content, and median diameter of the glycidyl methacrylate-methyl methacrylate copolymer (B-1) contained in the obtained latex of the glycidyl methacrylate-methyl methacrylate copolymer (B-1) were measured according to the above-mentioned methods. The results are shown in Table 1.

[0112] <Production Example 3> (Preparation of latex of glycidyl methacrylate-methyl methacrylate copolymer (B-2)) Except for changing the amount of glycidyl methacrylate used from 5 parts to 10 parts and the amount of methyl methacrylate used from 95 parts to 90 parts, polymerization was carried out in the same manner as in Production Example 2 to obtain a polymer latex. Then, by adjusting the pH and solid content concentration of the polymer latex, a latex of glycidyl methacrylate-methyl methacrylate copolymer (B-2) with a solid content concentration of 30% by weight and pH=8.5 was obtained and measured in the same manner as in Production Example 2. The results are shown in Table 1.

[0113] <Production Example 4> (Preparation of latex of glycidyl methacrylate-methyl methacrylate copolymer (B-3)) Except for changing the amount of glycidyl methacrylate used from 5 parts to 30 parts and the amount of methyl methacrylate used from 95 parts to 70 parts, polymerization was carried out in the same manner as in Production Example 2 to obtain a polymer latex. Then, by adjusting the pH and solid content concentration of the polymer latex, a latex of glycidyl methacrylate-methyl methacrylate copolymer (B-3) with a solid content concentration of 30% by weight and pH=8.5 was obtained and measured in the same manner as in Production Example 2. The results are shown in Table 1.

[0114] <Production Example 5> (Preparation of latex of glycidyl methacrylate-methyl methacrylate copolymer (B-4)) Except for changing the amount of glycidyl methacrylate used from 5 parts to 70 parts and the amount of methyl methacrylate used from 95 parts to 30 parts, polymerization was carried out in the same manner as in Production Example 2 to obtain a polymer latex. Then, by adjusting the pH and solid content concentration of the polymer latex, a latex of glycidyl methacrylate-methyl methacrylate copolymer (B-4) with a solid content concentration of 30% by weight and pH=8.5 was obtained and measured in the same manner as in Production Example 2. The results are shown in Table 1.

[0115] <Production Example 6> (Preparation of latex of glycidyl methacrylate polymer (B-5)) Except for changing the amount of glycidyl methacrylate used from 5 parts to 100 parts and not using methyl methacrylate, polymerization was performed in the same manner as in Production Example 2 to obtain a polymer latex. A polymer latex was obtained. Then, the pH and solid content concentration of the polymer latex were adjusted to obtain a latex of glycidyl methacrylate polymer (B-5) with a solid content concentration of 30% by weight and pH=8.5, and the measurements were performed in the same manner as in Production Example 2. The results are shown in Table 1.

[0116] <Production Example 7> (Preparation of latex of methacrylic acid-methyl methacrylate copolymer (B-6)) Except for using methacrylic acid instead of glycidyl methacrylate, polymerization was carried out in the same manner as in Production Example 3 to obtain a polymer latex. Then, the pH and solid content concentration of the polymer latex were adjusted to obtain a latex of methacrylic acid-methyl methacrylate copolymer (B-6) having a solid content concentration of 30% by weight and a pH of 8.5, and the measurements were carried out in the same manner as in Production Example 2. The results are shown in Table 1.

[0117] <Production Example 8> (Preparation of latex of methyl methacrylate polymer (B'-7)) Polymerization was performed in the same manner as in Production Example 2 to obtain a polymer latex, except that glycidyl methacrylate was not used and the amount of methyl methacrylate used was changed from 5 parts to 100 parts. Then, the pH and solid content concentration of the polymer latex were adjusted to obtain a latex of a methyl methacrylate polymer (B'-7) having a solid content concentration of 30% by weight and a pH of 8.5, and the measurements were performed in the same manner as in Production Example 2. The results are shown in Table 1.

[0118] <Example 1> (Preparation of aqueous dispersion of colloidal sulfur) An aqueous dispersion of colloidal sulfur with a solids concentration of 50% by weight was prepared by grinding and stirring 1.0 part of colloidal sulfur (manufactured by Hosoi Chemical Industry Co., Ltd.), 0.5 part of a dispersant (manufactured by Kao Corporation, product name "Demol N"), 0.0015 parts of a 5 wt% aqueous potassium hydroxide solution (manufactured by Wako Pure Chemical Industries, Ltd.) in a ball mill for 48 hours.

[0119] (Preparation of aqueous dispersions of zinc dibutyldithiocarbamate, zinc oxide, and titanium oxide) An aqueous dispersion of zinc dibutyldithiocarbamate, an aqueous dispersion of zinc oxide, and an aqueous dispersion of titanium oxide were prepared in the same manner as above, except that zinc dibutyldithiocarbamate (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), zinc oxide (manufactured by Seido Chemical Industry Co., Ltd.), and titanium oxide were used instead of colloidal sulfur, respectively.

[0120] (Preparation of Latex Composition) The latex of the nitrile group-containing conjugated diene polymer (A-1) obtained above and the latex of the glycidyl methacrylate-methyl methacrylate copolymer (B-1) obtained above were mixed in a weight ratio of "nitrile group-containing conjugated diene polymer (A-1):glycidyl methacrylate-methyl methacrylate copolymer (B-1)" of 70:30, and 5% by weight of potassium hydroxide was added to prepare a polymer latex composition having a solid content of 45% by weight and a pH of 8.

[0121] Then, the aqueous dispersions of each compounding agent prepared above were added to 100 parts of the polymer component of the polymer latex composition obtained above, so that the solid content was calculated as 1.0 part of colloidal sulfur, 1.0 part of zinc dibutyldithiocarbamate, 1.5 parts of zinc oxide, and 3.0 parts of titanium oxide. When the aqueous dispersions of each compounding agent were added, a predetermined amount was slowly added while stirring the latex composition. After each compounding agent was uniformly mixed, 0.30 parts of carboxymethylcellulose (manufactured by Daicel Corporation, trade name "Daicel2200", weight average molecular weight: 550,000, acid amount: 3.7 mmol / g) was added as a water-soluble polymer to adjust the solid content concentration, thereby obtaining a latex composition with a solid content concentration of 40% by weight and a viscosity of 3,000 mPa·s at 25°C.

[0122] (Preparation of coagulant solution) A coagulant solution was prepared by dissolving calcium nitrate as a coagulant in methanol at a ratio of 3.0% by weight.

[0123] (Manufacture of protective gloves) First, the latex composition obtained above was aged (also called pre-vulcanization) at a temperature of 30°C for 48 hours. Next, a ceramic glove mold covered with a glove-shaped fiber substrate (material: nylon, linear density: 300 denier, gauge number: 13 gauge, thickness: 0.8 mm) was immersed in the coagulant solution prepared above for 5 seconds, and after being pulled out of the coagulant solution, was dried at a temperature of 30°C for 1 minute. Thereafter, the ceramic glove mold was immersed in the aged latex composition for 5 seconds, and after being pulled out of the aged latex composition, was dried at a temperature of 30°C for 30 minutes, and then heated at a temperature of 70°C for 10 minutes to crosslink the material, thereby forming a polymer layer having a thickness of 0.6 mm on the fiber substrate. Then, the ceramic glove mold on which the polymer layer was formed was immersed in hot water at 60°C for 90 seconds to dissolve water-soluble impurities from the polymer layer, and then dried at a temperature of 30°C for 10 minutes, and then heat-treated at a temperature of 125°C for 30 minutes to crosslink the polymer in the polymer layer. Next, the fiber substrate on which the polymer layer was formed was peeled off from the ceramic glove mold to obtain a protective glove. Then, the wet grip property and chemical permeation resistance were measured using the obtained protective glove. The results are shown in Table 1.

[0124] <Example 2> A protective glove was obtained in the same manner as in Example 1, except that the latex of the nitrile group-containing conjugated diene polymer (A-1) and the latex of the glycidyl methacrylate-methyl methacrylate copolymer (B-1) were mixed in a weight ratio of "nitrile group-containing conjugated diene polymer (A-1):glycidyl methacrylate-methyl methacrylate copolymer (B-1)" of 90:10, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0125] <Example 3> A protective glove was obtained in the same manner as in Example 1, except that the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-2) was used instead of the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1), and the amount of carboxymethyl cellulose was changed from 0.30 parts to 0.57 parts, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0126] <Example 4> A protective glove was obtained in the same manner as in Example 2, except that the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-2) was used instead of the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1), and the amount of carboxymethyl cellulose was changed from 0.30 parts to 0.57 parts, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0127] <Example 5> A protective glove was obtained in the same manner as in Example 1, except that the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-3) was used instead of the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1), and the amount of carboxymethyl cellulose was changed from 0.30 parts to 0.57 parts, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0128] <Example 6> A protective glove was obtained in the same manner as in Example 2, except that the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-3) was used instead of the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1), and the amount of carboxymethyl cellulose was changed from 0.30 parts to 0.37 parts, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0129] <Example 7> A protective glove was obtained in the same manner as in Example 1, except that the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-4) was used instead of the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1) and the amount of carboxymethyl cellulose was changed from 0.30 parts to 0.57 parts, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0130] <Example 8> A protective glove was obtained in the same manner as in Example 2, except that the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-4) was used instead of the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1), and the amount of carboxymethyl cellulose was changed from 0.30 parts to 0.37 parts, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0131] <Example 9> A protective glove was obtained in the same manner as in Example 1, except that the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1) was replaced with the latex of glycidyl methacrylate polymer (B-5) and the amount of carboxymethyl cellulose was changed from 0.30 parts to 0.57 parts, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0132] <Example 10> A protective glove was obtained in the same manner as in Example 1, except that the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1) was replaced with the latex of methacrylic acid-methyl methacrylate copolymer (B-6) and the amount of carboxymethyl cellulose was changed from 0.30 parts to 0.35 parts, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0133] <Example 11> A protective glove was obtained in the same manner as in Example 2, except that the latex of glycidyl methacrylate-methyl methacrylate copolymer (B-1) was replaced with the latex of methacrylic acid-methyl methacrylate copolymer (B-6) and the amount of carboxymethyl cellulose was changed from 0.30 parts to 0.57 parts, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0134] <Comparative Example 1> Instead of the polymer latex composition obtained by mixing the latex of the nitrile group-containing conjugated diene polymer (A-1) and the latex of the glycidyl methacrylate-methyl methacrylate copolymer (B-1), the latex of the nitrile group-containing conjugated diene polymer (A-1) was used as the polymer latex composition, and the amount of carboxymethylcellulose used was changed from 0.30 parts to 0.53 parts. The protective glove was obtained in the same manner as in Example 1, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0135] <Comparative Example 2> A protective glove was obtained in the same manner as in Example 1, except that the latex of the glycidyl methacrylate-methyl methacrylate copolymer (B-1) was replaced with the latex of the methyl methacrylate polymer (B'-7) and the amount of carboxymethyl cellulose was changed from 0.30 parts to 0.77 parts, and measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0136] [Table 1]

[0137] As shown in Table 1, the latex composition is prepared by mixing the latex of the nitrile group-containing conjugated diene polymer (A) and the latex of the crosslinkable group-containing polymer (B), and the crosslinkable group-containing polymer (B) contains a specific amount of the crosslinkable group-containing monomer unit (b1), which is at least one selected from the group consisting of an epoxy group-containing monomer unit, a carboxyl group-containing monomer unit, and a monomer unit having two carbon-carbon double bonds. As a result, the obtained dip-molded article has excellent wet grip properties and chemical permeation resistance (Examples 1 to 11).

[0138] On the other hand, when the latex of the crosslinkable group-containing polymer (B) was not blended, the obtained dip-molded article was inferior in wet grip property or chemical permeation resistance (Comparative Examples 1 and 2).

Claims

1. A latex composition comprising a mixture of a latex of a nitrile group-containing conjugated diene polymer (A) and a latex of a crosslinkable group-containing polymer (B), the crosslinkable group-containing polymer (B) is composed solely of 1 to 100% by weight of a crosslinkable group-containing monomer unit (b1) and 0 to 99% by weight of a monocarboxylate group-containing ethylenically unsaturated monomer unit (b2); the crosslinkable group-containing monomer unit (b1) is at least one selected from the group consisting of an epoxy group-containing monomer unit, a carboxyl group-containing monomer unit, and a monomer unit having two carbon-carbon double bonds; The latex composition, wherein the nitrile group-containing conjugated diene polymer (A) has a glass transition temperature (Tg) of 10°C or lower, and the crosslinkable group-containing polymer (B) has a glass transition temperature (Tg) of more than 10°C.

2. 2. The latex composition according to claim 1, wherein the nitrile group-containing conjugated diene polymer (A) has a methyl ethyl ketone insoluble content of 50% by weight or less, and the crosslinkable group-containing polymer (B) has a methyl ethyl ketone insoluble content of 55% by weight or more.

3. 3. The latex composition according to claim 1, wherein the crosslinkable group-containing monomer unit (b1) is at least one selected from the group consisting of an epoxy group-containing monomer unit and a carboxyl group-containing monomer unit.

4. The latex composition according to any one of claims 1 to 3, wherein the crosslinkable group-containing monomer unit (b1) is at least one selected from the group consisting of an epoxy group-containing (meth)acrylic acid ester monomer unit, an allyl glycidyl ether unit, and a (meth)acrylic acid unit.

5. 5. The latex composition according to claim 1, wherein the content of the crosslinkable group-containing polymer (B) is 1 to 60 parts by weight based on 100 parts by weight of the polymer component.

6. A dip-molded article obtained by using the latex composition according to any one of claims 1 to 5.

7. A dip-molded article obtained by immersing a substrate in the latex composition according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Working glove

    JP2007231428A

  • Carboxylic acid-modified nitrile copolymer latex for dip molding, latex composition for dip molding containing the same, and molded articles produced therefrom.

    JP2014530289A

  • Aqueous coating agent for concrete protection and method for forming concrete protection film

    JP2023013548A

  • Supported glove having grip features

    WO2015074106A1