Surface Acoustic Wave Devices
By employing LiNbO3 or LiTaO3 single crystal piezoelectric substrates with specific Euler angles and isotropic base materials, the sound speed of surface acoustic waves is reduced, allowing for miniaturized devices with enhanced frequency characteristics for smartphone filters.
Patent Information
- Application Number
- JP2023530404
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-21
- Filing Date
- 2022-06-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-16
AI Technical Summary
Existing surface acoustic wave devices face challenges in miniaturization and frequency reduction due to limitations in sound speed and substrate materials, leading to increased size and interference in frequency bands used by smartphones.
The use of LiNbO3 or LiTaO3 single crystal piezoelectric substrates with specific Euler angles and isotropic base substrates, combined with high-density interdigital electrodes, reduces sound speed and allows for miniaturization without increasing element size, while maintaining high impedance ratios and suppressing spurious components.
This configuration achieves a surface acoustic wave device with reduced sound speed, enabling smaller size and lower frequency operation with improved bandwidth and impedance ratios, suitable for compact filters in smartphones.
Smart Images

Figure 0007575023000005 
Figure 0007575023000006 
Figure 0007575023000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface acoustic wave device. [Background technology]
[0002] The 700MHz to 3GHz frequency band, which is mainly used by smartphones and other devices, has nearly 80 bands and is very congested. Of these bands, the low-frequency band from 700MHz to 1.3GHz has the least radio interference and allows for the most effective use of frequencies. For this reason, there is a demand for miniaturization of filters such as duplexers in the low-frequency band used by smartphones and other devices due to the increasing functionality of smartphones and other devices in recent years.
[0003] Conventionally, duplexers and other filters use bulk acoustic wave (BAW) devices that use piezoelectric thin films such as AlN or ScAlN, or surface acoustic wave (SAW) devices that use LiNbO3 (LN) or LiTaO3 (LT). In BAW devices, the AlN and ScAlN films used are polycrystalline films with a c-axis orientation, so the vibration mode of the bulk waves used is only the thickness-longitudinal vibration of the longitudinal wave. The sound velocity of this longitudinal wave is (c33 D / density) 1 / 2 It is represented by (c33 D is the elastic stiffness constant), and the resonant frequency is basically determined by the sound speed / (2 × film thickness). In the c-axis orientation, a transverse wave, which has half the sound speed of a longitudinal wave, cannot be excited, so in order to lower the resonant frequency, the piezoelectric thin film must be made thicker while still using a longitudinal wave. However, forming a thick piezoelectric thin film causes the underlying Si substrate to warp or crack significantly, and the electrode size also increases in proportion to the thickness of the piezoelectric thin film. For this reason, in the low-frequency range of BAW devices, the size of the filter becomes extremely large, making it difficult to realize.
[0004] On the other hand, in a SAW device using LN or LT, the resonant frequency f is determined by f=V / λ, where V is the sound velocity of the substrate and λ is the period (wavelength) of the interdigital transducer (IDT). Therefore, in order to lower the resonant frequency, λ should be increased or V should be decreased. However, if the wavelength λ is increased, the element size becomes large, and it is not possible to meet the demand for miniaturization. Therefore, attempts are being made to lower the frequency by using a substrate with a low sound velocity and a small V. For example, the sound velocity of commonly used LN and LT is 3800 m / s, but there are some that use high-density electrodes as interdigital transducers to reduce the sound velocity of the substrate (for example, see Non-Patent Document 1). The amount of reduction in sound velocity in this case is 18%, and the actual sound velocity is 3026 m / s. The impedance ratio in this case is 66 dB.
[0005] Depending on the application, a filter is required to have a bandwidth of 5% to 30%. The bandwidth of the filter is approximately twice that of the resonator, and the fractional bandwidth of the resonator is roughly given by the square of the coupling coefficient / 2. Since the bandwidth depends on the coupling coefficient in this way, LN substrates and LT substrates that have the coupling coefficient required for the filter bandwidth have traditionally been used. On the other hand, the higher the impedance ratio, the better, and as a rough guideline, it is considered desirable to have an impedance ratio of 65 dB or more.
[0006] Here, the impedance ratio is 20×log(Za / Zr), where Zr is the impedance at the resonant frequency fr and Za is the impedance at the anti-resonant frequency fa. The bandwidth is (fa-fr) / fr. [Prior art documents] [Non-patent literature]
[0007] [Non-Patent Document 1] M. Mimura, D. Ajima, C. Konoma, and T. Murase, “Small sized band 20 SAW duplexer using low acoustic velocity Rayleigh SAW on LiNbO3 substrate”, Proc. IEEE Ultrasonics Symp. 2017, DOI: 10.1109 / ULTSYM.2017.8092596 Summary of the Invention [Problem to be solved by the invention]
[0008] In the surface acoustic wave device described in Non-Patent Document 1, which uses high-density electrodes as interdigital transducers, the sound speed of the propagating surface acoustic wave can be reduced to approximately 3000 m / s. However, in order to utilize surface acoustic waves of lower frequencies, it is necessary to further reduce the sound speed.
[0009] The present invention has been made in light of these problems, and aims to provide a surface acoustic wave device that can further reduce the sound speed of propagating surface acoustic waves, thereby enabling miniaturization and lower frequency. [Means for solving the problem]
[0010] In order to achieve the above object, the present invention provides a surface acoustic wave device comprising a piezoelectric substrate made of a single crystal of LiNbO3 or LiTaO3, and a dielectric layer having a density of 8100 kg / m 3The piezoelectric substrate has the above interdigital transducer and a base substrate made of a material that is isotropic with respect to the propagation of elastic waves or quartz and provided on the other surface of the piezoelectric substrate, wherein the piezoelectric substrate has Euler angles of (-5° to 35°, 95° to 110°, 0°±5°) when made of a single crystal of LiNbO3, and Euler angles of (-5° to 35°, 113° to 142°, 0°±5°) when made of a single crystal of LiTaO3, and the base substrate has a sound velocity of a propagating longitudinal wave slower than 8431 m / s, or a sound velocity of a propagating transverse wave slower than 5341 m / s, or a density smaller than that of the piezoelectric substrate. The sound velocity of the excited and propagating surface acoustic wave must be 3000 m / s or less. It is characterized by:
[0011] The surface acoustic wave device according to the present invention has a density equal to or greater than the density of Al (2700 kg / m 3 ), or 8100 kg / m 3 By using the above high density interdigital transducer and using an undersubstrate in which the sound velocity of the propagating longitudinal wave is slower than 8431 m / s, or in which the sound velocity of the propagating transverse wave is slower than 5341 m / s, or in which the density is lower than that of the piezoelectric substrate, the sound velocity of the propagating surface acoustic wave can be further reduced. By using a glass substrate or a quartz substrate, which are isotropic in terms of the propagation of the acoustic wave, as the undersubstrate, the sound velocity of the excited and propagating surface acoustic wave can be reduced to 3000 m / s or less. This can also reduce the resonant frequency of the propagating surface acoustic wave, making it possible to lower the frequency. In addition, the sound velocity can be reduced without changing the wavelength of the propagating surface acoustic wave. This eliminates the need to increase the element size, making it possible to reduce the size.
[0012] The surface acoustic wave device of the present invention can suppress spurious signals and increase the impedance ratio by using a single crystal of LiNbO3 with Euler angles of (-5° to 35°, 95° to 110°, 0°±5°) or a single crystal of LiTaO3 with Euler angles of (-5° to 35°, 113° to 142°, 0°±5°) as a piezoelectric substrate.
[0013] In the surface acoustic wave device according to the present invention, the interdigital transducer has a density of 8100 kg / m 3 As long as it meets the above requirements, it may be made of any material, for example, a Cu electrode, a Mo electrode, a Pt electrode, an alloy, a multilayer metal film, or the like.
[0014] In the surface acoustic wave device according to the present invention, when the piezoelectric substrate is made of a single crystal of LiNbO3 and the base substrate is made of a quartz substrate, the Euler angles of the piezoelectric substrate are preferably (-5° to 35°, 95° to 106°, 0°±5°). When the piezoelectric substrate is made of a single crystal of LiNbO3 and the base substrate is made of a glass substrate, the Euler angles of the piezoelectric substrate are preferably (-5° to 35°, 97° to 110°, 0°±5°). When the piezoelectric substrate is made of a single crystal of LiTaO3, the base substrate is preferably made of a glass substrate, and in particular, the Euler angles of the piezoelectric substrate are preferably (-5° to 35°, 115° to 125° or 127° to 140°, 0°±5°). In this case, spurious can be more effectively suppressed, and a relatively high impedance ratio can be obtained.
[0015] In the surface acoustic wave device according to the present invention, the interdigital transducer is preferably made of Cu electrodes and has a thickness of 0.077λ×0.5 / MR to 0.4λ×0.5 / MR, where λ is the wavelength and MR is the metallization ratio. In this case, the sound velocity of the excited and propagating surface acoustic wave can be reduced to 3000 m / s or less. In order to further reduce the sound velocity of the propagating surface acoustic wave, the thickness of the interdigital transducer is preferably 0.08λ×0.5 / MR or more, more preferably 0.115λ×0.5 / MR or more, and even more preferably 0.123λ×0.5 / MR or more.
[0016] In the surface acoustic wave device according to the present invention, the interdigital transducer is made of a material other than Cu, and its wavelength is λ, its metallization ratio is MR, and its average density is ρ ave Then, the thickness is 0.077λ×8930×0.5 / (MR×ρ ave )~0.4λ×8930×0.5 / (MR×ρave In this case, the sound velocity of the propagating surface acoustic wave can be reduced to 3000 m / s or less. In order to further reduce the sound velocity of the propagating surface acoustic wave, the thickness of the interdigital transducer is preferably 0.08λ×8930×0.5 / (MR×ρ ave ) or more, and 0.115λ×8930×0.5 / (MR×ρ ave ) or more, and 0.123λ×8930×0.5 / (MR×ρ ave ) or more is even more preferable.
[0017] In the surface acoustic wave device according to the present invention, the thickness of the piezoelectric substrate is preferably 0.14λ to 5λ, where λ is the wavelength of the interdigital transducer, in which case ripples can be suppressed and a relatively high impedance ratio can be obtained.
[0018] In the surface acoustic wave device according to the present invention, the interdigital transducer is made of a Cu electrode, the base substrate is made of a quartz substrate, and the thickness of the interdigital transducer is h and the wavelength is λ, the thickness of the piezoelectric substrate is t given by: When 0.06λ≦h<0.16λ, t≧11.2-125.3×h+228×h 2 +796.5×h 3 When 0.16λ≦h≦0.4λ, t≧2-21.7×h+84.1×h 2 -108.1×h 3 In this case as well, it is possible to suppress the occurrence of ripples and obtain a high impedance ratio.
[0019] In the surface acoustic wave device according to the present invention, the interdigital transducer is made of a material other than Cu, the base substrate is made of a quartz substrate, and the thickness of the interdigital transducer is h, the wavelength is λ, the metallization ratio is MR, and the average density is ρ ave Let H = h × MR × ρ ave / (8930×0.5), the thickness t of the piezoelectric substrate is When 0.06λ≦H<0.16λ, t≧11.2-125.3×H+228×H 2 +796.5×H 3 When 0.16λ≦H≦0.4λ, t≧2-21.7×H+84.1×H 2 -108.1×H 3 In this case as well, it is possible to suppress the occurrence of ripples and obtain a high impedance ratio.
[0020] In the surface acoustic wave device according to the present invention, the interdigital transducer is made of a Cu electrode, the base substrate is made of a glass substrate, and the thickness of the interdigital transducer is h and the wavelength is λ, the thickness of the piezoelectric substrate is t given by: (I) The density of the base substrate is 3100 kg / m 3 ~8015kg / m 3 So, When 0.06λ≦h<0.4λ, t≧5.1-60.9×h+257.7×h 2 -361.3×h 3 (II) the density of the base substrate is 2225 kg / m 3 ~3100kg / m 3 So, When 0.06λ≦h<0.13λ, t≧1.956-28×h+311×h 2 -1376.8×h 3 When 0.13λ≦h<0.4λ, t≧3.5-40.5×h+163.4×h 2 -218.2×h 3 (III) the density of the base substrate is 2100 kg / m 3 ~2225kg / m 3 So, When 0.06λ≦h<0.4λ, t≧5.07-62.3×h+265.7×h 2 -373×h 3 In this case as well, it is possible to suppress the occurrence of ripples and obtain a high impedance ratio.
[0021] In the surface acoustic wave device according to the present invention, the interdigital transducer is made of a material other than Cu, the base substrate is made of a glass substrate, and the thickness of the interdigital transducer is h, the wavelength is λ, the metallization ratio is MR, and the average density is ρ ave Let H = h × MR × ρ ave / (8930×0.5), the thickness t of the piezoelectric substrate is (I) The density of the base substrate is 3100 kg / m 3 ~8015kg / m 3 So, When 0.06λ≦H<0.4λ, t≧5.1-60.9×H+257.7×H 2 -361.3×H 3 (II) the density of the base substrate is 2225 kg / m 3 ~3100kg / m 3 So, When 0.06λ≦H<0.13λ, t≧1.956-28×H+311×H 2 -1376.8×H 3 When 0.13λ≦H<0.4λ, t≧3.5-40.5×H+163.4×H 2 -218.2×H 3 (III) the density of the base substrate is 2100 kg / m 3 ~2225kg / m 3 So, When 0.06λ≦H<0.4λ, t≧5.07-62.3×H+265.7×H 2 -373×H 3 In this case as well, it is possible to suppress the occurrence of ripples and obtain a high impedance ratio.
[0022] In the surface acoustic wave device according to the present invention, the base substrate has a linear expansion coefficient of 4.0×10 -6(1 / °C) or less, and the ratio of the thickness of the base substrate to the thickness of the piezoelectric substrate is preferably 15 or more. In this case, the influence of temperature changes can be suppressed. In this case, in order to further suppress the influence of temperature changes, the base substrate has a linear expansion coefficient of 0.5×10 -6 (1 / ° C.) or less, and the ratio of the thickness of the base substrate to the thickness of the piezoelectric substrate is preferably 10 or more.
[0023] In the surface acoustic wave device according to the present invention, it is preferable that the piezoelectric substrate is made of a single crystal of LiNbO3, the thickness of the interdigital transducer is 0.06λ to 2λ, and the base substrate is made of a quartz substrate, where λ is the wavelength of the interdigital transducer. In this case, the impedance ratio can be increased.
[0024] The surface acoustic wave device according to the present invention includes a piezoelectric substrate made of a single crystal of LiNbO3 or LiTaO3, and a , density 8100kg / m 3 The above a piezoelectric substrate having an interdigital transducer and a quartz substrate provided on the other surface of the piezoelectric substrate, the combination of a bonding surface of the piezoelectric substrate and a bonding surface of the quartz substrate being such that the Euler angles are: The back surface is (0°,90°~270°,0°) and the front surface is (0°,θ,90°), The back surface of (0°, 270°~450°, 0°) and the front surface of (0°, θ, 270°), The back surface of (0°,90°~270°,0°) and the front surface of (0°,θ,0°), The back surface of (0°,270°~450°,0°) and the front surface of (0°,θ,0°) Either one of The sound velocity of the excited and propagating surface acoustic wave is 3000 m / s or less. In this case, a large impedance ratio can be obtained.
[0025] Here, the Euler angles (φ, θ, ψ) are in a right-handed system and represent the cut surface of the piezoelectric substrate and the propagation direction of the elastic wave. That is, the X-axis is rotated counterclockwise by φ around the Z-axis, relative to the X, Y, and Z crystal axes of the LT or LN that constitute the piezoelectric substrate, to obtain the X'-axis. Next, the Z-axis is rotated counterclockwise by θ around the X'-axis to obtain the Z'-axis. At this time, the Z'-axis is the normal, and the plane including the X'-axis is the cut surface of the piezoelectric substrate. Also, the direction of the counterclockwise rotation of the X'-axis by ψ around the Z'-axis is the propagation direction of the elastic wave. Also, the axis perpendicular to the X'-axis and Z'-axis obtained by moving the Y-axis through these rotations is the Y'-axis.
[0026] By defining the Euler angles in this way, for example, the 40° rotated Y-plate X-direction propagation is expressed as (0°, -50°, 0°) in Euler angles, and the 40° rotated Y-plate 90° X-direction propagation is expressed as (0°, -50°, 90°) in Euler angles. When cutting out a piezoelectric substrate at a desired Euler angle, an error of up to ±0.5° may occur for each component of the Euler angle. Regarding the characteristics of elastic waves, there is almost no difference in characteristics due to a deviation of about ±5° for φ and ψ among the Euler angles (φ, θ, ψ). In addition, (0°, θ+360°, 0°) is an equivalent plane to the Euler angles (0°, θ, 0°). On the other hand, (0°, θ+180°, 0°) is not an equivalent plane to (0°, θ, 0°) in Euler angles, but they are in a relationship of the front and back of the substrate. However, since an acoustic wave device exhibits the same characteristics on both sides, the orientation of the front and back of the substrate is also considered to be equivalent surfaces, except for bonding substrates under certain conditions, such as those shown in Figure 15 below.
[0027] The metallization ratio (MR) of an interdigital transducer (IDT) is the ratio of the width F of the interdigital transducer's fingers along the propagation direction of the surface acoustic wave to half the period (λ) of the fingers (the sum of the width F of the fingers and the gap G between the fingers), and is given by MR=F / (F+G)=2×F / λ. Effect of the Invention
[0028] According to the present invention, it is possible to provide a surface acoustic wave device that can further reduce the sound velocity of the propagating surface acoustic wave, thereby enabling miniaturization and lowering of the frequency. [Brief description of the drawings]
[0029] [Figure 1] 1 is a side view showing a surface acoustic wave device according to an embodiment of the present invention; [Diagram 2] 1 is a graph showing the frequency characteristics of a surface acoustic wave device having a conventional (a) Al electrode (thickness 0.08λ) / (0°, 38°, 0°) LN structure and (b) Al electrode (thickness 0.08λ) / (0°, 97°, 0°) LN structure. [Diagram 3] 1 is a graph showing the frequency characteristics of a surface acoustic wave device made of Cu electrodes (thickness 0.18λ) / (0°, 97°, 0°) LN (thickness 0.6λ) / (0°, 132°45', 0°) quartz according to an embodiment of the present invention. [Figure 4] 1 is a graph showing the frequency characteristics of a surface acoustic wave device made of Cu electrodes (thickness 0.18λ) / (0°, 120°, 0°) LN (thickness 0.6λ) / (0°, 132°45', 0°) quartz according to an embodiment of the present invention. [Diagram 5] This is a graph showing the relationship between the Euler angle θ of the LN substrate and the resonant sound velocity (phase velocity) for a surface acoustic wave device consisting of a Cu electrode (thickness 0.18λ) / (0°,θ,0°) LN (thickness 0.6λ) / (0°,132°45',0°) quartz crystal and a Cu electrode (thickness 0.18λ) / (0°,θ,0°) LN (thickness 0.6λ) / (0°,132°45',90°) quartz crystal according to an embodiment of the present invention. [Figure 6] 6A is a graph showing the relationship between the Euler angle θ of the LN substrate and the bandwidth of the acoustic wave device shown in FIG. 5, (b) a graph showing an enlarged portion of (a), (c) a graph showing the relationship between the Euler angle θ of the LN substrate and the impedance ratio, and (d) a graph showing an enlarged portion of (c). [Figure 7]1 is a graph showing the relationship between the Euler angle θ of the quartz substrate and the impedance ratio for a surface acoustic wave device consisting of a Cu electrode (thickness 0.14λ) / (0°, 101°, 0°) LN (thickness 1.5λ) / (0°, θ, 0°) quartz and a Cu electrode (thickness 0.14λ) / (0°, 101°, 0°) LN (thickness 1.5λ) / (0°, θ, 90°) quartz according to an embodiment of the present invention. [Figure 8] 1A is a graph showing the relationship between the Euler angle θ of the LT substrate and the impedance ratio of the resonant sound velocity on the low velocity side (LSAW) for a surface acoustic wave device consisting of a Cu electrode (thickness 0.12λ) / (0°, θ, 0°) LT (thickness 0.8λ) / ZE glass, and a Cu electrode (thickness 0.12λ) / (0°, θ, 0°) LT (thickness 1.0λ) / ZE glass according to an embodiment of the present invention; and FIG. 1B is a graph showing the relationship between the Euler angle θ of the LT substrate and the impedance ratio of the resonant sound velocity on the low velocity side and high velocity side (Rayleigh wave), with a portion of (a) enlarged. [Figure 9] 1 is a graph showing the relationship between the thickness of the Cu electrode and the resonant sound velocity (sound velocity Vr at resonant frequency fr, and sound velocity Va at anti-resonant frequency fa) for a surface acoustic wave device consisting of (a) Cu electrode / (0°, 101°, 0°) LN (thickness 1λ) / (0°, 132°45', 0°) quartz and (b) Cu electrode / (0°, 101°, 0°) LN (thickness 1λ) / glass (BI glass, ZE glass, quartz glass) according to an embodiment of the present invention. [Figure 10] 1 is a graph showing the relationship between the thickness of the LN substrate and the impedance ratio of a surface acoustic wave device made of Cu electrodes (thicknesses 0.10λ, 0.13λ, 0.20λ) / (0°, 101°, 0°) LN / ZE glass according to an embodiment of the present invention. [Figure 11] 13 is a graph showing the frequency characteristics of a surface acoustic wave device according to an embodiment of the present invention, which is composed of (a) a Cu electrode (thickness 0.05λ) / (0°, 101°, 0°) LN (thickness 0.4λ) / (0°, 160°, 90°) quartz and (b) a Cu electrode (thickness 0.14λ) / (0°, 101°, 0°) LN (thickness 1.0λ) / (0°, 160°, 90°) quartz. [Figure 12] 1 is a graph showing the relationship between the thickness h of the Cu electrode and the thickness t of the LN substrate in a surface acoustic wave device consisting of Cu electrodes / (0°, 101°, 0°) LN / (0°, 160°, 90°) quartz in an embodiment of the present invention. [Figure 13] 13 is a graph showing the relationship between the thickness h of the Cu electrode and the thickness t of the LN substrate for a surface acoustic wave device consisting of a Cu electrode / (0°, 101°, 0°) LN / underlying substrate according to an embodiment of the present invention, when the density of the underlying substrate is (a) Group I (3100 kg / m3 to 8015 kg / m3), (b) Group II (2225 kg / m3 to 3100 kg / m3), and (c) Group III (2100 kg / m3 to 2225 kg / m3). [Figure 14] 1 is a graph showing the relationship between (a) the ratio of the thickness of the base substrate to the thickness of the LN substrate, and (b) the ratio of the thickness of the base substrate to the thickness of the LT substrate, and the temperature coefficient of frequency (TCF) of a surface acoustic wave device according to an embodiment of the present invention. [Figure 15] 13 is a graph showing the relationship between the thickness of an LN substrate and the impedance ratio of a surface acoustic wave device in which a Cu electrode (thickness 0.12λ) is formed on the surface of an LN substrate according to an embodiment of the present invention, and (a) the positive side of the LN substrate is bonded to a 70°Y90°X quartz substrate, and (b) the negative side of the LN substrate is bonded to a 70°Y90°X quartz substrate. [Figure 16] 1 is a graph showing frequency characteristics of a surface acoustic wave device made of Cu electrode (thickness 0.08λ) / 11° YXLN (thickness 0.7λ) / single crystal Si according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Hereinafter, an embodiment of the present invention will be described with reference to the drawings and examples. 1 to 16 show a surface acoustic wave (SAW) device according to an embodiment of the present invention. As shown in FIG. 1, a surface acoustic wave device 10 has a piezoelectric substrate 11, an interdigital transducer (IDT) 12, and an underlying substrate 13.
[0031] Piezoelectric substrate 11 is made of LiNbO3 single crystal (LN) or LiTaO3 single crystal (LT). Piezoelectric substrate 11 preferably has a thickness of 0.14λ to 0.5λ, where λ is the period (wavelength) of the electrode fingers of interdigital transducer 12. Interdigital transducer 12 has a density of 0.14λ to 0.5λ, which is the density of Al (2700 kg / m 3 ), or 8100 kg / m 3 Made of the above materials, it is formed by a photolithography process or the like on one surface of piezoelectric substrate 11. Interdigital electrode 12 is made of, for example, a Cu electrode, a Mo electrode, a Pt electrode, an alloy, a multilayer metal film, or the like.
[0032] Underlying substrate 13 is made of a material that is isotropic with respect to the propagation of elastic waves, or quartz crystal. Underlying substrate 13 is made of a material in which the sound velocity of longitudinal waves propagating therethrough is slower than 8431 m / s, or a material in which the sound velocity of transverse waves propagating therethrough is slower than 5341 m / s, or a material whose density is lower than that of piezoelectric substrate 11. Underlying substrate 13 is provided on the other surface of piezoelectric substrate 11, i.e., the surface opposite interdigital transducer 12. Underlying substrate 13 has a linear expansion coefficient of 4.0×10 -6 (1 / ° C.) or less is preferable. The base substrate 13 is made of, for example, a quartz substrate or a glass substrate.
[0033] Next, the operation will be described. The surface acoustic wave device 10 has a density of 8100 kg / m 3 By using the above-described high-density interdigital transducer 12 and by using an underlying substrate 13 in which the acoustic velocity of the propagating acoustic waves is slower than the acoustic velocity of the acoustic waves propagating through the piezoelectric substrate 11, the acoustic velocity of the propagating surface acoustic waves can be further reduced. This also reduces the resonant frequency of the propagating surface acoustic waves, making it possible to lower the frequency. In addition, the acoustic velocity can be reduced without changing the wavelength of the propagating surface acoustic waves. This eliminates the need to increase the element size, making it possible to reduce the size.
[0034] Below, we will show examples and comparative examples of the surface acoustic wave device 10, and describe their structures as "interdigital transducer (IDT) / piezoelectric substrate / underlying substrate" or "interdigital transducer (IDT) / piezoelectric substrate" (in the case of the comparative example).
[0035] [Conventional surface acoustic wave devices] The frequency characteristics of a SAW resonator with an Al electrode (thickness 0.08λ) / (0°, 38°, 0°) LN structure, which is currently in practical use, were determined and are shown in Figure 2(a). Here, λ is the period (wavelength) of the electrode fingers of the interdigital electrode (same below). In Figure 2(a), the horizontal axis is shown as the sound velocity obtained by multiplying the IDT wavelength λ and the frequency. As shown in Figure 2(a), the resonance sound velocity was 3810 m / s and the anti-resonance sound velocity was 3960 m / s. The bandwidth (BW) was 3.8% and the impedance ratio was 50 dB.
[0036] Similarly, the frequency characteristics of a SAW resonator with an Al electrode (thickness 0.08λ) / (0°, 97°, 0°) LN structure were determined and are shown in Figure 2(b). In Figure 2(b) as well, the horizontal axis is shown as the sound velocity obtained by multiplying the IDT wavelength λ by the frequency. As shown in Figure 2(b), the resonance sound velocity was 3790 m / s and the anti-resonance sound velocity was 4460 m / s. The bandwidth (BW) was 17.7% and the impedance ratio was 62 dB. Since the leakage component was large in the piezoelectric substrate with this azimuth angle, many ripples were generated within the bandwidth, and it is considered that the device cannot be used as is.
[0037] [Example of the present invention] The frequency characteristics of a SAW resonator consisting of Cu electrodes (thickness 0.18λ) / (0°,97°,0°) LN (thickness 0.6λ) / (0°,132°45',0°) quartz, which is a combination of an interdigital electrode made of high-density electrodes and a quartz substrate on the same LN substrate as in Figure 2(b), are shown in Figure 3. The metallization ratio (MR) of the interdigital electrode is 0.5 (same below). As shown in Figure 3, the resonant sound velocity was 2020 m / s and the anti-resonant sound velocity was 2310 m / s. The bandwidth (BW) was 14.5% and the impedance ratio was 80 dB.
[0038] As shown in Figure 3, compared to the conventional SAW resonator shown in Figure 2(a), it was confirmed that the resonant sound velocity was reduced by 47% and the impedance ratio was increased by 30 dB. Also, compared to the conventional SAW resonator shown in Figure 2(b), it was confirmed that the resonant sound velocity was reduced by 47% and the impedance ratio was increased by 18 dB, and furthermore, there was no ripple and no leakage component. From these facts, it can be said that the surface acoustic wave device shown in Figure 3 has very good characteristics.
[0039] Next, the frequency characteristics of a SAW resonator consisting of Cu electrodes (thickness 0.18λ) / (0°, 120°, 0°) LN (thickness 0.6λ) / (0°, 132°45', 0°) and quartz crystal were obtained and are shown in Figure 4. Note that this SAW resonator differs from the one in Figure 3 only in the azimuth angle of the LN substrate. As shown in Figure 4, even in this case, resonator characteristics with a wide band and high impedance ratio due to leaky SAW (LSAW) are obtained on the low frequency side, but it was confirmed that large spurious due to Rayleigh waves occurs in the high velocity range. From the results shown in Figures 3 and 4, it is believed that there is an optimal azimuth angle at which no spurious occurs in the LN substrate or LT substrate.
[0040] Next, the relationship between the Euler angle θ of the LN substrate and the resonance sound velocity (Phase velocity), bandwidth, and impedance ratio of the low-velocity side (LSAW) and high-velocity side (Rayleigh wave) of the SAW resonator consisting of Cu electrode (thickness 0.18λ) / (0°,θ,0°) LN (thickness 0.6λ) / (0°,132°45',0°) quartz and Cu electrode (thickness 0.18λ) / (0°,θ,0°) LN (thickness 0.6λ) / (0°,132°45',90°) quartz was obtained, and is shown in Figure 5 and Figure 6 (a) to (d), respectively. Figure 6 (c) and (d) also show the relationship between the Euler angle θ and the impedance ratio when the base substrate is changed from a quartz substrate to a glass substrate made of Pyrex (registered trademark) glass.
[0041] As shown in Figure 4, two resonance characteristics may be observed due to spurious. In Figures 5 and 6, ○, ▲, and * indicate the low-velocity resonance sound velocity when using quartz substrates of (0°, 132° 45', 0°) and (0° 132° 45', 90°), respectively, and in Figures 5 and 6, □, ▼, and × indicate the high-velocity resonance sound velocity when using quartz substrates of (0°, 132° 45', 0°) and (0° 132° 45', 90°), respectively. As shown in Figure 5, it was confirmed that there is almost no difference in the resonance characteristics due to differences in the azimuth angle of the quartz substrate. In addition, when the Euler angles (φ, θ, ψ) are in the range of -5° to 35°, the values are almost the same as when φ = 0°.
[0042] As shown in FIG. 6(a), it was confirmed that at the resonance sound velocity on the low speed side, a bandwidth of 6% or more was obtained at θ=58°-125°, and 10% or more was obtained at θ=70°-117°. However, as shown in FIG. 6(b), which is an enlargement of FIG. 6(a), it was confirmed that at θ=94° or less and 107° or more, Rayleigh waves on the high frequency side were slightly excited, and no excitation was observed at θ=95°-106°. Also, as shown in FIG. 6(c), it was confirmed that, at the resonance sound velocity on the low speed side, impedance ratios of 70dB or more were obtained at θ=69°-117°, 75dB or more at θ=78°-110°, and 80dB or more at θ=80°-104° were obtained for the quartz substrate. However, as shown in FIG. 6(d), which is an enlargement of FIG. 6(c), the largest impedance ratio was obtained at θ=90°-94°, but slight excitation of Rayleigh waves was observed. The excitation is not observed when θ=95° to 106°, and it is most preferable to use an LN substrate with this Euler angle. As shown in FIG. 6(c), it was confirmed that, in the case of a glass substrate, the impedance ratio is 66 dB or more when θ=81° to 123°, 68 dB or more when θ=83° to 120°, and 70 dB or more when θ=87° to 114° at the low resonance sound velocity. However, as shown in FIG. 6(d), the azimuth angle at which the spurious due to Rayleigh waves is not excited is θ=97° to 110°, and it is most preferable to use an LN substrate with this Euler angle. Note that glass substrates with SiO2 content of 50% show the same tendency.
[0043] Next, the relationship between the Euler angle θ of the quartz and the impedance ratio of a SAW resonator consisting of a Cu electrode (thickness 0.14λ) / (0°,101°,0°) LN (thickness 1.5λ) / (0°,θ,0°) quartz and a Cu electrode (thickness 0.14λ) / (0°,101°,0°) LN (thickness 1.5λ) / (0°,θ,90°) quartz was calculated and shown in Figure 7. As shown in Figure 7, it was confirmed that the impedance ratio was constant regardless of the Euler angle of the quartz substrate.
[0044] The temperature coefficient of frequency (TCF), which indicates the frequency shift with respect to the temperature change per 1°C, is negative for LN and LT substrates regardless of the azimuth angle, but for quartz substrates, there are also azimuth angles that show a positive TCF. Therefore, the TCF is improved by combining an LN or LT substrate that shows a negative TCF with a quartz substrate with an azimuth angle that shows a positive TCF. For this reason, the quartz substrate preferably has an Euler angle θ at which the TCF of the Rayleigh wave is positive, and is preferably (0°±5°, 0° to 132°, 0°±5°), (0°±5°, 0° to 45°, 90°±5°), or (0°±5°, 172° to 180°, 90°±5°). The quartz crystal substrate may have an Euler angle θ at which the TCF of the leaky SAW (LSAW) is positive, and is preferably (0°±5°, 0° to 17°, 0°±5°), (0°±5°, 25° to 65°, 0°±5°), (0°±5°, 132° to 180°, 0°±5°), (0°±5°, 0° to 42°, 90°±5°), or (0°±5°, 125° to 180°, 90°±5°). When the Euler angles (φ, θ, ψ) are in the range of -5° to 35°, the angle shows almost the same value as when φ=0°±5°.
[0045] Next, the relationship between the Euler angle θ of the LT substrate and the impedance ratio of the resonance sound velocity on the low-velocity side (LSAW) and high-velocity side (Rayleigh wave) of the SAW resonators consisting of Cu electrode (thickness 0.12λ) / (0°,θ,0°) LT (thickness 0.8λ) / ZE glass and Cu electrode (thickness 0.12λ) / (0°,θ,0°) LT (thickness 1.0λ) / ZE glass was obtained and shown in Figures 8(a) and (b). ZE glass has a density of 2500 kg / m 3 The glass has a longitudinal wave velocity of 6498 m / s, a shear wave velocity of 3979 m / s, a Young's modulus of 95 GPa, and a Poisson's ratio of 0.2. As shown in FIG. 8(a), it was confirmed that the same relationship was obtained regardless of the thickness of the LT substrate. It was also confirmed that an impedance ratio of 66 dB or more was obtained when θ=80°-126°, and 70 dB or more was obtained when θ=90°-118°. However, as shown in FIG. 8(b), which is an enlarged view of FIG. 8(a), the Euler angle at which the spurious on the high-frequency side (Rayleigh wave) is 4 dB or less is θ=113°-142°, and the Euler angle at which it is 2 dB or less is θ=115°-125° and 127°-140°. From this, it can be said that it is preferable to use LT substrates with these Euler angles. Note that glass substrates with SiO2 components accounting for 50% show the same tendency.
[0046] Next, the relationship between the thickness of the Cu electrodes and the resonant sound velocity (sound velocity Vr at resonant frequency fr, and sound velocity Va at anti-resonant frequency fa) of a SAW resonator consisting of Cu electrodes / (0°,101°,0°)LN(thickness 1λ) / (0°,132°45',0°)quartz crystal was obtained and shown in Figure 9(a). As shown in Figure 9(a), it was confirmed that at sound velocity Vr, a resonant sound velocity of 3300m / s or less can be obtained when the Cu electrode thickness is 0.06λ or more, 3000m / s or less can be obtained when the Cu electrode thickness is 0.08λ or more, and 2500m / s or less can be obtained when the Cu electrode thickness is 0.123λ or more.
[0047] Next, the relationship between the thickness of the Cu electrodes and the resonant sound velocity (sound velocity Vr at the resonant frequency fr, and sound velocity Va at the anti-resonant frequency fa) of a SAW resonator consisting of Cu electrodes / (0°, 101°, 0°) LN (thickness 1λ) / glass (BI glass, ZE glass, quartz glass) was calculated and shown in Figure 9(b). BI glass has a density of 5630 kg / m3 The glass has a longitudinal wave velocity of 4373 m / s, a shear wave velocity of 2491 m / s, a Young's modulus of 90 GPa, and a Poisson's ratio of 0.26. As shown in Figure 9(b), it was confirmed that there is almost no difference in the sound velocity depending on the type of glass. In addition, it was confirmed that, for the sound velocity Vr, a resonant sound velocity of 3000 m / s or less can be obtained when the Cu electrode thickness is 0.077λ or more, and a resonant sound velocity of 2500 m / s or less can be obtained when the Cu electrode thickness is 0.115λ or more. In both cases of Figures 9(a) and (b), the resonant sound velocity decreases as the Cu electrode becomes thicker, but with current exposure technology, the electrode thickness is limited to 0.4λ.
[0048] 9(a) and (b) are for the case where the metallization ratio of the Cu electrode is 0.5, and the resonant sound velocity is inversely proportional to the metallization ratio. Therefore, if the metallization ratio of the Cu electrode is MR, the thickness of the Cu electrode that can obtain a certain resonant sound velocity is the thickness when the metallization ratio is 0.5 multiplied by 0.5 / MR.
[0049] In addition, the resonant sound velocity is inversely proportional not only to the metallization ratio but also to the electrode density and film thickness of the interdigital transducer. For this reason, when using Mo electrodes, Pt electrodes, alloys, multilayer metal films, etc. other than Cu electrodes, the metallization ratio of the electrodes is MR and the average density is ρ ave Then, the film thickness h at a given resonant sound velocity is defined as the film thickness of the Cu electrode (metallization ratio 0.5) at which the resonant sound velocity is obtained, h Cu , density ρ Cu (8930kg / m 3 ) can be calculated using the following formula (1). h=h Cu ×ρ Cu ×0.5 / (MR×ρ ave ) (1)
[0050] Using this formula (1), when the interdigital transducer is made of electrodes other than Cu, the thickness of the electrodes that can obtain the same resonant sound velocity is the thickness of a Cu electrode with a metallization ratio of 0.5 multiplied by 8930×0.5 / (MR×ρ ave ) is the value.
[0051] Next, the relationship between the thickness of the LN substrate and the impedance ratio of a SAW resonator consisting of Cu electrodes (thicknesses 0.10λ, 0.13λ, 0.20λ) / (0°, 101°, 0°) LN / ZE glass was obtained, and is shown in Figure 10. As shown in Figure 10, the same tendency was observed regardless of the thickness of the Cu electrodes, and it was confirmed that an impedance ratio of 70 dB or more was obtained when the thickness of the LN substrate was 0.17λ to 5λ. It was also confirmed that ripples were generated when the LN thickness was 0.15λ or less.
[0052] Next, the frequency characteristics of the SAW resonators consisting of Cu electrode (thickness 0.05λ) / (0°,101°,0°) LN (thickness 0.4λ) / (0°,160°,90°) quartz and Cu electrode (thickness 0.14λ) / (0°,101°,0°) LN (thickness 1.0λ) / (0°,160°,90°) quartz were obtained and are shown in Figure 11(a) and (b), respectively. As shown in Figure 11, it was confirmed that ripples were generated around 2.8 GHz in (a), and no ripples were generated in (b). From this, it is considered that there exists an optimal range for the relationship between the electrode thickness of the interdigital transducer and the thickness of the piezoelectric substrate in which no ripples are generated.
[0053] Therefore, in a SAW resonator consisting of Cu electrode / (0°, 101°, 0°) LN / (0°, 160°, 90°) quartz, the thickness of the Cu electrode and the thickness of the LN substrate were changed to find the range in which ripples do not occur. The results are shown in Figure 12. The range above the curve shown in Figure 12 is the range in which ripples do not occur, and it was confirmed that ripples occur when the thickness of the LN is smaller than 0.14λ. It was confirmed that the same results as in Figure 12 were obtained for the azimuth angles of the LN substrate and quartz substrate shown in Figures 5 to 8. The metallization ratio of the Cu electrode is 0.5.
[0054] If the thickness of the Cu electrode is h and the thickness of the LN substrate is t, the range in which no ripples occur can be expressed as follows from the approximation curve of the curve shown in FIG. When 0.06λ≦h<0.16λ, t≧11.2-125.3×h+228×h 2 +796.5×h 3 When 0.16λ≦h≦0.4λ, t≧2-21.7×h+84.1×h 2 -108.1×h 3 Although not shown in Fig. 12, the thickness of the LN substrate when the Cu electrode thickness is 0.4λ is almost the same as when the Cu electrode thickness is 0.3λ. Furthermore, the impedance ratio is the same up to a LN substrate thickness of 5λ.
[0055] When an electrode other than a Cu electrode is used, the thickness h of the electrode can be calculated by the formula (1). Cu If H is the thickness of the LN and t is the thickness of the LN, the range in which ripples do not occur can be expressed as follows: When 0.06λ≦H<0.16λ, t≧11.2-125.3×H+228×H 2 +796.5×H 3 When 0.16λ≦H≦0.4λ, t≧2-21.7×H+84.1×H 2 -108.1×H 3 Here, H=h×MR×ρ ave / (8930×0.5).
[0056] In addition, when the base substrate is not a quartz substrate but an isotropic substrate such as a glass substrate, the range in which ripples do not occur varies depending on the density of the substrate. In a SAW resonator consisting of a Cu electrode / (0°, 101°, 0°) LN / base substrate, the material of the base substrate is divided into Group I (3100 kg / m 3 ~8015kg / m 3 ), Group II (2225kg / m 3 ~3100kg / m 3 ), Group III (2100kg / m 3 ~2225kg / m 3) and the range in which ripples do not occur was determined for each group. The results are shown in Figures 13(a) to (c). The range above the curves shown in each figure is the range in which ripples do not occur, and it was confirmed that ripples occur when the LN thickness is less than 0.17λ. Examples of glass substrates etc. included in each group are shown in Table 1. For reference, Table 1 also shows the density, longitudinal wave sound velocity, and shear wave sound velocity of quartz, LN, LT, single crystal Si, and polycrystalline Si.
[0057] [Table 1]
[0058] If the thickness of the Cu electrode is h and the thickness of the LN substrate is t, the range in which no ripples occur can be expressed as follows from the approximation curves of the curves shown in each figure. In groove I shown in FIG. 13(a), When 0.06λ≦h≦0.4λ, t≧5.1-60.9×h+257.7×h 2 -361.3×h 3 In the groove II shown in FIG. 13(b), When 0.06λ≦h<0.13λ, t≧1.956-28×h+311×h 2 -1376.8×h 3 When 0.13λ≦h≦0.4λ, t≧3.5-40.5×h+163.4×h 2 -218.2×h 3 In the groove III shown in FIG. When 0.06λ≦h≦0.4λ, t≧5.07-62.3×h+265.7×h 2 -373×h 3 Although not shown, the upper limit of the thickness of the LN substrate is 5λ.
[0059] When an electrode other than a Cu electrode is used, the thickness h of the electrode can be calculated by the formula (1). Cu If H is the thickness of the LN substrate and t is the thickness of the LN substrate, the range in which no ripples occur can be expressed as follows: In groove I shown in FIG. 13(a), When 0.06λ≦H≦0.4λ, t≧5.1-60.9×H+257.7×H 2 -361.3×H 3 In the groove II shown in FIG. 13(b), When 0.06λ≦H<0.13λ, t≧1.956-28×H+311×H 2 -1376.8×H 3 When 0.13λ≦H≦0.4λ, t≧3.5-40.5×H+163.4×H 2 -218.2×H 3 In the groove III shown in FIG. When 0.06λ≦H≦0.4λ, t≧5.07-62.3×H+265.7×H 2 -373×H 3 Here, H=h×MR×ρ ave / (8930×0.5).
[0060] Next, when the piezoelectric substrate is made of an LN substrate, the relationship between the ratio of the thickness of the substrate to the thickness of the LN substrate and the temperature coefficient of frequency (TCF), which indicates the frequency shift per 1°C of temperature change, was calculated for substrates with various linear expansion coefficients, and is shown in Figure 14(a). As shown in Figure 14(a), for substrates with a linear expansion coefficient of 0.5×10 -6 It was confirmed that the absolute value of the TCF is 20 ppm / ℃ or less when the thickness ratio is 10 or more and the absolute value of the TCF is small for the base substrate with a linear expansion coefficient of 4.0×10 -6It was confirmed that when the thickness ratio is 15 or more for a substrate with a linear expansion coefficient of 4.0×10 -6 It can be said that it is sufficient to use a base substrate having a thickness of (1 / ° C.) or less and determine the thicknesses of the base substrate and the LN substrate so that the ratio of the thickness of the base substrate to the thickness of the LN substrate is 15 or more.
[0061] Similarly, when the piezoelectric substrate is made of an LT substrate, the relationship between the ratio of the thickness of the substrate to the thickness of the LT substrate and the temperature coefficient of frequency (TCF), which indicates the frequency shift per 1°C of temperature change, was calculated for substrates with various linear expansion coefficients, and is shown in Figure 14(b). As shown in Figure 14(b), -6 It was confirmed that the absolute value of the TCF is 10 ppm / ℃ or less when the thickness ratio is 10 or more and the absolute value of the TCF is small for the base substrate with a linear expansion coefficient of 4.0×10 -6 It was confirmed that when the thickness ratio of the base substrate is 15 or more, the absolute value of the TCF is 15 ppm / ℃ or less. In addition, the linear expansion coefficient is 8.4 × 10 -6 It was confirmed that when the thickness ratio is 15 or more for a substrate with a linear expansion coefficient of 4.0×10 -6 (1 / ℃) or less, and the thicknesses of the base substrate and the LT substrate should be determined so that the ratio of the thickness of the base substrate to the thickness of the LT substrate is at least 15. Table 2 shows examples of the linear expansion coefficients of various materials that can be used to form the substrate.
[0062] [Table 2]
[0063] Next, the relationship between the thickness of the LN substrate and the impedance ratio was calculated for a SAW resonator in which a Cu interdigital electrode (thickness 0.12λ) was formed on the surface (negative side) of an LN substrate with Euler angles of (0°, 105°, 0°) and a surface equivalent to the back surface (positive side) of the LN substrate was joined to the surface (negative side) of a quartz substrate with 70°Y90°X [Euler angles of (0°, 160°, 90°)], and for a SAW resonator in which a Cu interdigital electrode (thickness 0.12λ) was formed on the surface (positive side) of an LN substrate with Euler angles of (0°, 285°, 0°) and a surface equivalent to the back surface (negative side) of the LN substrate was joined to the surface (negative side) of a quartz substrate with 70°Y90°X. The results are shown in Figure 15. As shown in FIG. 15, when the thickness of the LN substrate is 0.06λ to 2λ, the impedance ratio of the LN substrate in which the positive surface of the LN substrate is bonded to the quartz substrate is 0.3 to 3.5 dB higher than that of the LN substrate in which the negative surface of the LN substrate is bonded to the quartz substrate.
[0064] Next, a SAW resonator was formed by bonding a 0.17λ-thick (0°, 101° or 281°, 0°) LN substrate with an angle of 0°, 160° or 340°, 0-270° quartz substrate, and forming a Cu interdigital electrode (thickness 0.1λ) on the surface of the LN substrate. The results of investigating the bandwidth and impedance ratio (Z ratio) are shown in Table 3. Note that when the Euler angles (φ, θ, ψ) are θ=-90° to 90° (±360°), the front surface of each substrate is the positive side and the back surface is the negative side. Also, when θ=90° to 270° (±360°), the front surface of each substrate is the negative side and the back surface is the positive side. For example, the (0°,101°,0°)LN and (0°,281°,0°)LN in Table 3 are in a front-back relationship, with the front side of the former LN substrate being the negative side and the back side being the positive side, and the front side of the latter LN substrate being the positive side and the back side being the negative side. That is, the code on the left side of the "Polarity" column in Table 3 indicates the polarity of the front side of the substrate, and the code on the right side indicates the polarity of the back side of the substrate.
[0065] [Table 3]
[0066] As shown in Table 3, for the combination of LN and (0°, 160° or 340°, 90° or 270°) quartz, it was confirmed that a SAW resonator in which a (0°, 101°, 0°) LN back surface (positive side) is bonded to a (0°, 160°, 90°) quartz surface (negative side) or a (0°, 340°, 90°) quartz surface (positive side) exhibits an impedance 2.0 dB higher than a SAW resonator in which an LN back surface (positive side) with the same Euler angles is bonded to a (0°, 160°, 270°) quartz surface (negative side) or a (0°, 340°, 270°) quartz surface (positive side).
[0067] On the other hand, it was confirmed that a SAW resonator in which the (0°, 281°, 0°) LN back surface (negative surface) is bonded to the (0°, 160°, 270°) quartz surface (negative surface) or (0°, 340°, 270°) quartz surface (positive surface) also exhibits an impedance 2.0 dB higher than a SAW resonator in which the LN back surface (negative surface) with the same Euler angles is bonded to the (0°, 160°, 90°) quartz surface (negative surface) or (0°, 340°, 90°) quartz surface (positive surface). As such, even if the polarity of the bonding surfaces is changed, the impedance ratio and difference show the same values, so it can be said that the combination of the azimuth angle of the LN substrate and the azimuth angle of the quartz substrate are more important than the positive and negative surfaces of the LN substrate and the quartz substrate.
[0068] Next, as shown in Table 3, for the combination of LN and (0°, 160° or 340°, 0° or 180°) quartz, it was confirmed that a SAW resonator in which a (0°, 101°, 0°) LN back surface (positive side) is bonded to a (0°, 160°, 0°) quartz surface (negative side) or a (0°, 340°, 0°) quartz surface (positive side) exhibits an impedance 2.2 dB higher than a SAW resonator in which an LN back surface (positive side) with the same Euler angles is bonded to a (0°, 160°, 180°) quartz surface (negative side) or a (0°, 340°, 180°) quartz surface (positive side).
[0069] On the other hand, it was confirmed that a SAW resonator in which the (0°,281°,0°) LN back surface (negative surface) is bonded to the (0°,160°,0°) quartz surface (negative surface) or (0°,340°,0°) quartz surface (positive surface) also exhibits an impedance 2.2 dB higher than a SAW resonator in which the LN back surface (negative surface) with the same Euler angles is bonded to the (0°,160°,180°) quartz surface (negative surface) or (0°,340°,180°) quartz surface (positive surface). As such, even if the polarity of the bonding surfaces is changed, the impedance ratio and difference show the same values, so it can be said that even in this combination, the combination of the azimuth angle of the LN substrate and the azimuth angle of the quartz substrate are more important than the positive and negative surfaces of the LN substrate and the quartz substrate.
[0070] It was also confirmed that the obtained bandwidth and impedance ratio differ depending on the combination of azimuth angles of the LN substrate and quartz substrate, regardless of whether they are on the positive or negative side, as shown in Table 3. The same results were obtained with Al electrodes, Pt electrodes, and other electrodes other than Cu electrodes, confirming that this phenomenon is not dependent on the electrode material.
[0071] From the results in Table 3, it is believed that the following four combinations of LN substrates and quartz substrates will provide a large impedance ratio. (0°,90°~270°,0°) LN and (0°,θ,90°) Quartz (0°,270°~450°,0°) LN and (0°,θ,270°) Quartz (0°,90°~270°,0°) LN and (0°,θ,0°) quartz (0°,270°~450°,0°) LN and (0°,θ,0°) Quartz
[0072] Furthermore, when the orientation of the LN substrate that provides a larger impedance ratio is taken into consideration, the more desirable combination is as follows: (0°,95°~110°,0°) LN and (0°,θ,90°) Quartz (0°,275°~290°,0°) LN and (0°,θ,270°) Quartz (0°,95°~110°,0°) LN and (0°,θ,0°) Quartz (0°,275°~290°,0°) LN and (0°,θ,0°) quartz
[0073] Next, a SAW resonator was formed by bonding a 0.17λ-thick (0°,132° or 312°,0°) LT substrate to a (0°,150° or 330°,ψ) quartz substrate, and forming a Cu interdigital electrode (0.08λ thick) on the surface of the LT substrate. The results of investigating the bandwidth (BW) and impedance ratio (Z ratio) are shown in Table 4. Note that, like the LN mentioned above, the (0°,132°,0°) LT and (0°,312°,0°) LT have a front-back relationship, with the front side of the former being the negative side and the back side being the positive side. The latter is the opposite.
[0074] [Table 4]
[0075] As shown in Table 4, for the combination of LT and (0°, 150° or 330°, 90° or 270°) quartz crystal, it was confirmed that a SAW resonator in which the (0°, 132°, 0°) LT back surface (positive side) is joined to the (0°, 150°, 90°) quartz crystal front surface (negative side) or the (0°, 330°, 90°) quartz crystal front surface (positive side) exhibits an impedance 1.6 dB higher than a SAW resonator in which the LT back surface (positive side) with the same Euler angles is joined to the (0°, 150°, 270°) quartz crystal front surface (negative side) or the (0°, 330°, 270°) quartz crystal front surface (positive side).
[0076] On the other hand, it was confirmed that the SAW resonator in which the (0°, 312°, 0°) LT back surface (negative surface) was joined to the (0°, 150°, 270°) quartz surface (negative surface) or (0°, 330°, 270°) quartz surface (positive surface) also showed impedance 1.6 dB higher than the SAW pendulum in which the LT back surface (positive surface) with the same Euler angle was joined to the (0°, 150°, 90°) quartz surface (negative surface) or (0°, 330°, 90°) quartz surface (positive surface). As such, even if the polarity of the joined surfaces is changed, the impedance ratio and the difference show the same values, so it can be said that the combination of the azimuth angle of the LN substrate and the azimuth angle of the quartz substrate are more important than the positive and negative surfaces of the LN substrate and the quartz substrate.
[0077] Next, as shown in Table 4, for the combination of LT and (0°, 150° or 330°, 0° or 180°) quartz crystal, it was confirmed that a SAW resonator in which the (0°, 132°, 0°) LT back surface (positive side) is joined to the (0°, 150°, 0°) quartz crystal front surface (negative side) or the (0°, 330°, 0°) quartz crystal front surface (positive side) exhibits impedance approximately 2.4 dB higher than a SAW resonator in which the LT back surface (positive side) with the same Euler angles is joined to the (0°, 150°, 180°) quartz crystal front surface (negative side) or the (0°, 330°, 180°) quartz crystal front surface (positive side).
[0078] On the other hand, it was confirmed that the SAW resonator in which the (0°, 312°, 0°) LT back surface (negative surface) was bonded to the (0°, 150°, 0°) quartz surface (negative surface) or the (0°, 330°, 0°) quartz surface (positive surface) also showed impedance 2.4 dB higher than the SAW resonator in which the LT back surface (negative surface) with the same Euler angle was bonded to the (0°, 150°, 180°) quartz surface (negative surface) or the (0°, 330°, 180°) quartz surface (positive surface). As such, even if the polarity of the bonding surfaces is changed, the impedance ratio and the difference show the same values, so it can be said that even in this combination, the combination of the azimuth angle of the LN substrate and the azimuth angle of the quartz substrate are more important than the positive and negative surfaces of the LN substrate and the quartz substrate.
[0079] In addition, it was confirmed that the obtained bandwidth and impedance ratio differ depending on the combination of the azimuth angles of the LT substrate and quartz substrate, regardless of whether they are on the positive or negative side, as shown in Table 4. The same results were obtained with Al electrodes, Pt electrodes, and other electrodes other than Cu electrodes, and it was also confirmed that this phenomenon is not dependent on the electrode material.
[0080] From the results in Table 4, it is believed that the following four combinations of LT substrates and quartz substrates will provide a large impedance ratio. (0°,90°~270°,0°)LT and (0°,θ,90°)quartz (0°,270°~450°,0°)LT and (0°,θ,270°)quartz (0°,90°~270°,0°)LT and (0°,θ,0°)quartz (0°,270°~450°,0°)LT and (0°,θ,0°)quartz
[0081] Furthermore, when considering the orientation of the LT board that provides a larger impedance ratio, a more desirable combination is as follows: (0°,113°~142°,0°)LT and (0°,θ,90°)quartz (0°,293°~322°,0°)LT and (0°,θ,270°)quartz (0°,113°~142°,0°)LT and (0°,θ,0°)quartz (0°,293°~322°,0°)LT and (0°,θ,0°)quartz
[0082] It was also confirmed that when the base substrate was a glass substrate, no difference was observed between the positive and negative bonding surfaces of the LN substrate and LT substrate.
[0083] Next, the frequency characteristics of a SAW resonator consisting of Cu electrode (thickness 0.08λ) / 11°YXLN (thickness 0.7λ) / single crystal Si (longitudinal wave sound velocity 8431 m / s, shear wave sound velocity 5844 m / s) were obtained and are shown in Fig. 16. As shown in Fig. 16, it was confirmed that the sound velocity was high because a single crystal Si substrate with a high sound velocity was used as the base substrate. It was also confirmed that a large spurious was excited in a high-order mode with a sound velocity about 1.4 times the resonance sound velocity, and good characteristics were not obtained. Similarly, when polycrystalline Si with a longitudinal wave sound velocity of 8945 m / s and a shear wave sound velocity of 5341 m / s was used as the base substrate, the excitation of a large spurious was confirmed. It was also confirmed that when quartz with a longitudinal wave sound velocity of 6360 m / s and a shear wave sound velocity of 4676 m / s was used as the base substrate, good characteristics without spurious were obtained. For this reason, it is desirable to use a base substrate in which the longitudinal wave velocity is slower than 8431 m / s, or a base substrate in which the shear wave velocity is slower than 5341 m / s. [Explanation of symbols]
[0084] 10 Surface acoustic wave devices 11 Piezoelectric substrate 12 Interdigital Electrode 13 Underlying substrate
Claims
1. LiNbO 3 or LiTaO 3 A piezoelectric substrate made of a single crystal of A piezoelectric substrate having a density of 8100 kg / m 3 The interdigital electrodes described above, a base substrate made of a material that is isotropic with respect to the propagation of elastic waves or quartz and provided on the other surface of the piezoelectric substrate; The piezoelectric substrate is LiNbO 3 When the material is made of a single crystal of LiTaO, the Euler angles are (-5° to 35°, 95° to 110°, 0°±5°), and 3 When the crystal is made of a single crystal of the above, the Euler angles are (-5° to 35°, 113° to 142°, 0°±5°), The base substrate has a longitudinal wave propagating at a sound velocity lower than 8431 m / s, or a shear wave propagating at a sound velocity lower than 5341 m / s, or has a density lower than that of the piezoelectric substrate; The sound velocity of the excited and propagating surface acoustic wave is 3000 m / s or less. A surface acoustic wave device.
2. The piezoelectric substrate is LiNbO 3 The Euler angles are (-5° to 35°, 95° to 106°, 0°±5°); The base substrate is made of a quartz crystal substrate.
2. The surface acoustic wave device according to claim 1.
3. The piezoelectric substrate is LiNbO 3 The Euler angles are (-5° to 35°, 97° to 110°, 0°±5°); The base substrate is made of a glass substrate.
2. The surface acoustic wave device according to claim 1.
4. The piezoelectric substrate is LiTaO 3 It consists of a single crystal of The base substrate is made of a glass substrate.
2. The surface acoustic wave device according to claim 1.
5. The piezoelectric substrate is LiTaO 3 The Euler angles are (-5° to 35°, 115° to 125° or 127° to 140°, 0°±5°); The base substrate is made of a glass substrate.
2. The surface acoustic wave device according to claim 1.
6. 6. The surface acoustic wave device according to claim 1, wherein the interdigital transducer is made of a Cu electrode and has a thickness of 0.077λ×0.5 / MR to 0.4λ×0.5 / MR, where λ is the wavelength and MR is the metallization ratio.
7. The interdigital transducer is made of a material other than Cu, and its wavelength is λ, its metallization ratio is MR, and its average density is ρ ave Then, the thickness is 0.077λ×8930×0.5 / (MR×ρ ave ) ~ 0.4λ × 8930 × 0.5 / (MR × ρ ave 6. The surface acoustic wave device according to claim 1, wherein the surface acoustic wave device is a multilayer structure.
8. 6. The surface acoustic wave device according to claim 1, wherein the thickness of the piezoelectric substrate is 0.14λ to 5λ, where λ is the wavelength of the interdigital transducer.
9. The interdigital transducer is made of Cu electrodes, the base substrate is a quartz substrate, If the thickness of the interdigital transducer is h and the wavelength is λ, the thickness t of the piezoelectric substrate is given by: When 0.06λ≦h<0.16λ, t≧11.2-125.3×h+228×h 2 +796.5×h 3 When 0.16λ≦h≦0.4λ, t≧2-21.7×h+84.1×h 2 -108.1×h 3 3. The surface acoustic wave device according to claim 1, wherein
10. the interdigital transducer is made of a material other than Cu; the base substrate is a quartz substrate, The thickness of the interdigital transducer is h, the wavelength is λ, the metallization ratio is MR, and the average density is ρ ave Let H = h × MR × ρ ave / (8930×0.5), the thickness t of the piezoelectric substrate is When 0.06λ≦H<0.16λ, t≧11.2-125.3×H+228×H 2 +796.5×H 3 When 0.16λ≦H≦0.4λ, t≧2-21.7×H+84.1×H 2 -108.1×H 3 3. The surface acoustic wave device according to claim 1, wherein
11. The interdigital transducer is made of Cu electrodes, The base substrate is made of a glass substrate, If the thickness of the interdigital transducer is h and the wavelength is λ, the thickness t of the piezoelectric substrate is given by: (I) The density of the base substrate is 3100 kg / m 3 ~8015kg / m 3 So, When 0.06λ≦h<0.4λ, t≧5.1-60.9×h+257.7×h 2 -361.3×h 3 (II) The density of the base substrate is 2225 kg / m 3 ~3100kg / m 3 So, When 0.06λ≦h<0.13λ, t≧1.956-28×h+311×h 2 -1376.8×h 3 When 0.13λ≦h<0.4λ, t≧3.5-40.5×h+163.4×h 2 -218.2×h 3 (III) The density of the base substrate is 2100 kg / m 3 ~2225kg / m 3 So, When 0.06λ≦h<0.4λ, t≧5.07-62.3×h+265.7×h 2 -373×h 3 6. The surface acoustic wave device according to claim 1, wherein
12. the interdigital transducer is made of a material other than Cu; The base substrate is made of a glass substrate, The thickness of the interdigital transducer is h, the wavelength is λ, the metallization ratio is MR, and the average density is ρ ave Let H = h × MR × ρ ave / (8930×0.5), the thickness t of the piezoelectric substrate is (I) The density of the base substrate is 3100 kg / m 3 ~8015kg / m 3 So, When 0.06λ≦H<0.4λ, t≧5.1-60.9×H+257.7×H 2 -361.3×H 3 (II) The density of the base substrate is 2225 kg / m 3 ~3100kg / m 3 So, When 0.06λ≦H<0.13λ, t≧1.956-28×H+311×H 2 -1376.8×H 3 When 0.13λ≦H<0.4λ, t≧3.5-40.5×H+163.4×H 2 -218.2×H 3 (III) The density of the base substrate is 2100 kg / m 3 ~2225kg / m 3 So, When 0.06λ≦H<0.4λ, t≧5.07-62.3×H+265.7×H 2 -373×H 3 6. The surface acoustic wave device according to claim 1, 3, 4 or 5,
13. The base substrate has a linear expansion coefficient of 4.0×10 -6 6. The acoustic wave device according to claim 1, wherein the thermal expansion coefficient is 1 / [deg.] C. or less.
14. The piezoelectric substrate is LiNbO 3 and the thickness of the interdigital transducer is 0.06λ to 2λ, where λ is the wavelength of the interdigital transducer. The base substrate is made of a quartz crystal substrate.
2. The surface acoustic wave device according to claim 1.
15. LiNbO 3 or LiTaO 3 a piezoelectric substrate made of a single crystal of A piezoelectric substrate having a density of 8100 kg / m 3 The interdigital electrodes described above, a quartz crystal substrate provided on the other surface of the piezoelectric substrate; The combination of the bonding surface of the piezoelectric substrate and the bonding surface of the quartz substrate is, in terms of Euler angles, A back surface of (0°, 90° to 270°, 0°) and a front surface of (0°, θ, 90°), A back surface of (0°, 270° to 450°, 0°) and a front surface of (0°, θ, 270°), A back surface of (0°, 90° to 270°, 0°) and a front surface of (0°, θ, 0°), The back surface of (0°, 270° to 450°, 0°) and the front surface of (0°, θ, 0°) (θ is an arbitrary angle), The sound velocity of the excited and propagating surface acoustic wave is 3000 m / s or less. A surface acoustic wave device.
Citation Information
Patent Citations
Filter with surface acoustic wave device for carrier aggregation system
JP2019036963A
Acoustic wave device and composite substrate
JP2020065158A
Acoustic wave device
JP2020182137A
Elastic surface-wave device
WO2011046117A1
Elastic wave device
WO2018097016A1