Sulfide-based all-solid-state battery including positive electrode active material coated with lithium niobate precursor and method for producing same

By coating the positive electrode active material with a lithium niobate precursor through a polyol process and dry mixing, the reactivity issues in sulfide-based all-solid-state batteries are mitigated, leading to improved performance and safety with a cost-effective manufacturing process.

JP7575167B2Active Publication Date: 2024-10-29LG ENERGY SOLUTION LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023509812
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-13
Filing Date
2021-08-11
Publication Date
2024-10-29
Estimated Expiration
2041-08-11

AI Technical Summary

Technical Problem

Sulfide-based all-solid-state batteries face issues of low ionic conductivity, high electrical resistance, and reduced lifespan due to reactivity between the positive electrode and sulfide-based solid electrolyte, with existing coating methods being costly and non-uniform.

Method used

Coating the positive electrode active material with a lithium niobate precursor produced by a polyol process, using a dry mixing method followed by heat treatment, to reduce reactivity and improve uniformity.

Benefits of technology

The method results in a sulfide-based all-solid-state battery with improved performance, reduced reactivity, enhanced safety, and a more economical manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575167000001
    Figure 0007575167000001
  • Figure 0007575167000002
    Figure 0007575167000002
  • Figure 0007575167000003
    Figure 0007575167000003
Patent Text Reader

Abstract

A sulfide-based all-solid-state battery and a method for manufacturing the same are disclosed. The sulfide-based all-solid-state battery includes a cathode active material coated with a lithium niobate precursor manufactured by a polyol process, which increases the capacity and improves safety of the sulfide-based all-solid-state battery and has low production costs.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This application claims the benefit of priority to U.S. patent application Ser. No. 16 / 992,274, filed Aug. 13, 2020, the entire disclosure of which is incorporated herein by reference.

[0002] The present invention relates to a sulfide-based all-solid-state battery including a cathode active material coated with a lithium niobate precursor and a method for manufacturing the same, and more particularly to a sulfide-based all-solid-state battery including a cathode active material coated with a lithium niobate precursor produced by a polyol process and a method for manufacturing the same. [Background technology]

[0003] Lithium ion secondary batteries have advantages over nickel-manganese batteries or nickel-cadmium batteries, such as higher energy density, lower self-discharge rate, and longer lifespan, but have been criticized for their disadvantages, such as safety issues regarding overheating and low output.

[0004] To overcome the problems of lithium-ion secondary batteries, all-solid-state batteries have been proposed as an alternative. All-solid-state batteries may have a structure including an electrolyte layer containing a solid electrolyte, a positive electrode layer and a negative electrode layer, each of which also contains a solid electrolyte, formed on both sides of the electrolyte layer, and a current collector bonded to each electrode.

[0005] All-solid-state batteries can be classified into oxide-based, polymer-based, and sulfide-based batteries depending on the raw material of the solid electrolyte. Sulfide-based all-solid-state batteries have superior lithium ion conductivity compared to other batteries. However, compared to existing batteries using liquid electrolytes, they have low ion conductivity and high electrical resistance between the positive electrode, negative electrode, and solid electrolyte, resulting in reduced lifespan and output, which have yet to be overcome.

[0006] The cathode active material and sulfide-based solid electrolyte react with each other at the interface to form a resistive material that hinders the operation of the solid-state battery, resulting in a decrease in the initial capacity and efficiency of the solid-state battery.

[0007] Conventional all-solid-state batteries improve their performance by coating the cathode active material with lithium niobate to reduce its reactivity with sulfide-based solid electrolytes. Patent Document 1 uses an organic solvent to coat the cathode active material with lithium niobate. This method has the drawback of requiring the solid electrolyte to be used after the remaining organic solvent has been completely evaporated to prevent reaction with the sulfide-based solid electrolyte. Furthermore, the use of lithium ethoxide or niobium ethoxide as a starting material to form lithium niobate results in high production costs and lengthy processes.

[0008] When a cathode active material is coated with lithium niobate by a dry coating method, the lithium niobate cannot uniformly coat the cathode active material, which makes it difficult to manufacture a sulfide-based all-solid-state battery at low cost and with high performance. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 4982866 Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention aims to solve the above-mentioned problems and to provide a sulfide-based all-solid-state battery in a stable and economical manner by coating a cathode active material with a lithium niobate precursor prepared by a polyol process. [Means for solving the problem]

[0011] According to one aspect of the present invention, the above and other objects can be achieved by providing a cathode active material coated with a lithium niobate precursor prepared by a polyol process, and a sulfide-based all-solid-state battery including the coated cathode active material.

[0012] The coating can be formed by dry mixing the positive electrode active material and the lithium niobate precursor without the need for a separate solvent.

[0013] The coating may be heat-treated by dry-mixing the positive electrode active material and the lithium niobate precursor, raising the temperature by 5°C per minute until the target temperature is reached, and then allowing it to cool naturally.

[0014] The lithium niobate precursor may include lithium niobate and a chelating agent.

[0015] The chelating agent may be one or more selected from the group consisting of citric acid, polyvinylpyrrolidone (PVP), carboxylic acid, and nitrogen-containing weak acid.

[0016] The lithium niobate precursor may be coated on the positive electrode active material in an amount of 1 nm to 100 nm.

[0017] The positive electrode active material may be lithium cobalt oxide. The lithium cobalt oxide is a positive electrode active material according to an embodiment of the present invention. Positive electrode active materials that can be used in lithium ion secondary batteries or all-solid-state batteries can also be used as the positive electrode active material of the present invention.

[0018] According to another aspect of the present invention, there is provided a method for coating a positive electrode active material, including: S1) mixing a polyol and a chelating agent to form a polyol precursor; S2) mixing lithium hydroxide and ammonium niobate oxalate hydrate with the polyol precursor to form a positive electrode active material coating material; and S3) coating a positive electrode active material with the positive electrode active material coating material.

[0019] In step S3), the positive electrode active material coating material and the positive electrode active material may be mixed and then heat-treated at 450° C. or more for 2 hours.

[0020] In addition, the heat treatment at 450° C. or more for 2 hours can be performed by increasing the temperature by 5° C. per minute until the target temperature is reached and then allowing it to cool naturally.

[0021] Also, step S2) can be performed dry.

[0022] The present invention can select and combine one or more of the above-mentioned configurations that are not contradictory to each other. [Effects of the Invention]

[0023] The present invention provides a sulfide-based all-solid-state battery including a coated positive electrode active material that has low reactivity between a sulfide-based solid electrolyte and a positive electrode active material and improved safety.

[0024] By uniformly coating the positive electrode active material with lithium niobate, the reactivity between the sulfide-based solid electrolyte and the positive electrode active material is reduced, and a sulfide-based all-solid-state battery with improved performance can be provided.

[0025] Furthermore, a simple and economical manufacturing method is provided by performing the coating method, which has conventionally been performed using a wet method, using a dry method. [Brief explanation of the drawings]

[0026] [Figure 1]1 is a flow chart of a method for coating a cathode active material with a lithium niobate precursor according to the present invention. [Figure 2] 1 is a chemical formula of a lithium niobate precursor prepared by the polyol process. [Figure 3] 1 is a scanning electron microscope (SEM) photograph of lithium niobate prepared by a polyol process according to the present invention. [Figure 4] 1 is a scanning electron microscope (SEM) photograph of a positive electrode active material coated with lithium niobate prepared by a polyol process according to the present invention. [Figure 5] 1 is a transmission electron microscope (TEM) photograph of a lithium niobate precursor according to the present invention. [Figure 6] 1 is a transmission electron microscope (TEM) photograph of a positive electrode active material coated with a lithium niobate precursor according to the present invention. [Figure 7] 1 is a graph comparing the specific capacity as a function of voltage between a sulfide-based all-solid-state battery according to the present invention and a sulfide-based all-solid-state battery manufactured using an uncoated cathode active material. [Figure 8] 1 is a graph comparing the capacity retention rate of a sulfide-based all-solid-state battery according to the present invention and a sulfide-based all-solid-state battery manufactured using an uncoated cathode active material. [Figure 9] 1 is a graph comparing impedance values ​​of a sulfide-based all-solid-state battery according to the present invention and a sulfide-based all-solid-state battery manufactured using an uncoated cathode active material. DETAILED DESCRIPTION OF THE INVENTION

[0027] Hereinafter, with reference to the accompanying drawings, a detailed description will be given of an embodiment of the present invention that will enable a person skilled in the art to easily carry out the present invention. However, in describing the operation principle of the preferred embodiment of the present invention in detail, detailed description of related well-known functions or configurations will be omitted if it is determined that such detailed description may unnecessarily obscure the gist of the present invention.

[0028] Furthermore, the same reference numerals are used throughout the drawings for parts having similar functions and actions. Throughout the specification, when a part is said to be connected to another part, this includes not only a direct connection but also an indirect connection via another element therebetween. Furthermore, unless otherwise specified, "including a certain element" does not mean that other elements are excluded, but that other elements may also be included.

[0029] Furthermore, descriptions that limit or add specific elements are applicable to all inventions and are not limited to a particular invention unless otherwise specified.

[0030] Furthermore, throughout the description of the present invention and the claims, the singular includes the plural unless otherwise stated.

[0031] Furthermore, throughout the description of the present invention and the claims, unless otherwise specified, "or" includes "and." Therefore, "including A or B" means three cases: including A, including B, or including both A and B.

[0032] Furthermore, all numerical ranges include the endpoints and all intermediate values ​​therebetween unless expressly stated to the contrary.

[0033] The present invention will now be described in more detail.

[0034] The present invention may include a positive electrode active material coated with a lithium niobate precursor prepared by a polyol process.

[0035] 1 is a flowchart showing a method for coating a positive electrode active material with a lithium niobate precursor according to the present invention. LCO refers to lithium cobalt oxide, which is a positive electrode active material, and LNO coating layer refers to the lithium niobate precursor prepared by a polyol process that is coated on the positive electrode active material.

[0036] As shown in FIG. 1, the cathode active material according to the present invention is dry-mixed with a lithium niobate precursor without the use of a separate solvent. The mixing method is not particularly limited in the present invention, and known methods can be used. This can be accomplished through a conventional mechanochemical reaction. Alternatively, conventional stirrers, mixers, a meteor ball mill, a mortar mixer, etc. can be used. When using a meteor ball mill, the lithium niobate precursor and the cathode active material can be mixed under conditions of 50 to 500 rpm, 0.1 to 10 hours, and 1 to 100 kWh / 1 kg.

[0037] There is no restriction on the moisture content of each particle as long as it is in a dry state, but it is preferable to dry each particle at 120°C for 6 hours.

[0038] The weight ratio of the lithium niobate precursor to the positive electrode active material is sufficient as long as the lithium niobate precursor is sufficient to coat the positive electrode active material. For example, the weight ratio of the lithium niobate precursor to the positive electrode active material may be 1-10:90-99, preferably 2-5:98-95.

[0039] The lithium niobate precursor and the positive electrode active material may be dry-mixed and then heat-treated at 400° C. or more. The heat treatment increases the bonding strength between the lithium niobate precursor and the positive electrode active material, thereby allowing the coated lithium niobate precursor to adhere to the positive electrode active material.

[0040] The heat treatment is performed by increasing the temperature by 5°C per minute until the target temperature is reached and then naturally cooling down. Preferably, the target temperature does not exceed 500°C. If heat of 500°C or higher is applied, the cobalt in the lithium cobalt oxide used as the positive electrode active material may diffuse into the lithium niobate precursor due to the high temperature and react with the sulfide-based solid electrolyte.

[0041] Here, the lithium niobate precursor and the positive electrode active material that have reached the target temperature may be left to cool naturally to 25° C. for 1 to 3 hours.

[0042] The heat treatment is performed in a single process to uniformly and evenly bond the lithium niobate precursor and the positive electrode active material and to prevent the formation of spaces between the lithium niobate precursor and the positive electrode active material.

[0043] After the heat treatment, the positive electrode active material may be coated with the lithium niobate precursor in an amount of 1 nm to 100 nm.

[0044] The polyol used in the polyol process is generally referred to as an alcohol containing two or more hydroxyl groups in the molecule. The polyol according to the present invention may be a material obtained by reacting an initiator having two or more hydroxyl or amine groups, i.e., a polyfunctional alcohol or an aromatic amine, with propylene oxide or ethylene oxide.

[0045] The polyols can be roughly classified into polyether polyols and polyester polyols. The polyol used in the present invention is preferably polyether polyol rather than polyester polyol, which is vulnerable to heat and moisture.

[0046] The polyol process is a method for producing fine powders by dissolving a salt, hydroxide, or oxidized inorganic compound precursor in such alcohols to form reducible metal ions, and then heating the solution to an appropriate temperature to induce a reduction reaction of the metal ions within the solution.

[0047] The polyol solvent used here varies in reducing power and interaction with metal ions depending on the type, which affects the setting of the appropriate synthesis temperature and the size and shape of the particles synthesized thereafter, and in some cases may even convert the produced particles into hydroxides and oxides.

[0048] In the polyol process, the lithium niobate precursor goes through the following four stages:

[0049] a) Metal ions are reduced to metal atoms, b) aggregation of metal atoms into nuclei; c) The nuclei grow into metal nanoparticles, d) Stabilization of metal nanoparticles with stabilizers.

[0050] In the first step, the precursor metal salt is dissolved in a liquid polyol, and after the dissolved salt is reduced by the polyol, nano-sized particles are generated from the solution through a process of nucleation and growth of metal particles. After that, the metal nanoparticles are stabilized by a stabilizer.

[0051] The lithium niobate precursor formed by the polyol process has a size of 100 nm or less. As described above, the nanoparticle-sized lithium niobate precursor is formed as a highly concentrated colloid, and the polyol process provides advantages of uniform particle size, excellent dispersion, and no need for a separate reducing agent.

[0052] Figure 2 shows the chemical formula of the lithium niobate precursor formed by the polyol process. The lithium niobate precursor shown in Figure 2 can be formed by mixing lithium hydroxide and ammonium niobate oxalate hydrate. Conventional lithium niobate precursors use expensive lithium ethylate and niobium ethylate, but the lithium niobate precursor of the present invention is formed by the polyol process and can be formed from lithium hydroxide and ammonium niobate oxalate hydrate, which are less expensive than lithium ethylate and niobium ethylate.

[0053] Lithium niobate can be obtained by mixing the lithium hydroxide with ammonium niobate oxalate hydrate, and a polyol process for the lithium niobate precursor can be performed by mixing a chelating agent with the lithium niobate. The chelating agent can be one selected from the group consisting of citric acid, polyvinylpyrrolidone (PVP), carboxylic acid, and a weak acid containing a nitrogen element. The chelating agent can be included in an amount of 1 to 10 parts by weight per 100 parts by weight of the lithium niobate.

[0054] The cathode active material according to the present invention may be a sulfur carbon composite including a porous carbon material, a compound capable of impregnating an electrolyte solution, and sulfur, and at least one of an inner surface and an outer surface of the porous carbon material may be a sulfur carbon composite including a coating layer including a compound capable of impregnating an electrolyte solution.

[0055] The positive electrode active material may include, in addition to the positive electrode active material particles, a layered compound such as lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals; 1+x Mn 2-x O4 (where x is 0 to 0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, and Cu2V2O7; and the chemical formula LiNi1-x M x O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, x = 0.01 to 0.3); Ni-site type lithium nickel oxide; chemical formula LiMn 2-x M x Lithium manganese composite oxides expressed as LiMnO2 (where M = Co, Ni, Fe, Cr, Zn, or Ta, x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu, or Zn); LiMn2O4, in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion; disulfide compounds; Fe2(MoO4)3, NCM622, and any one or mixture of these, or other known materials may be used. Among these, it is preferable to use lithium cobalt oxide, which is the most excellent because it has a high energy density and is inexpensive.

[0056] The average particle size of the positive electrode active material is not limited in the present invention, but may be in the range of 1 nm to 30 μm.

[0057] The solid electrolyte according to the present invention is a sulfide-based solid electrolyte and includes sulfide-based particles. The sulfide-based particles may be used by coating or modifying their surfaces, and the sulfide-based solid electrolyte may be prepared from a mixture containing the particles by a dry or wet process.

[0058] The sulfide-based particles are not particularly limited in the present invention and may be any known sulfide-based material used in the field of lithium batteries. The sulfide-based material may be commercially available or may be prepared by a crystallization process from an amorphous sulfide-based material.

[0059] Typically, Li6PS5Cl (LPSCl), Thio-LISICON (Li 3.25 Ge 0.25 P 0.75S4), Li2S-P2S5-LiCl, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, Li3PS4, Li7P3S 11 , LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, Li 10 GeP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , Li7P3S 11 Includes:

[0060] The conductive material according to the present invention is carbon-based, and is not particularly limited as long as it is conductive without causing any chemical change in the battery, and examples thereof include any one or more selected from the group consisting of graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0061] The binder according to the present invention is not particularly limited in the present invention, and known binders can be used. The binder is any one selected from the group consisting of N,N-bis[3-(triethoxysilyl)propyl]urea, polyethylene oxide (PEO), poly(vinylidene fluoride) (PVDF), and poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-co-HFP), or a mixture of two or more thereof, or N,N-bis[3-(triethoxysilyl)propyl]urea, polyethylene oxide (PEO), poly(vinylidene fluoride) (PVDF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-co-HFP), acrylonitrile-based The rubber composition may be any one selected from the group consisting of conjugated diene rubber latex such as styrene butadiene rubber (SBR), acrylonitrile butadiene rubber (NBR), methyl methacrylate butadiene rubber (MBR), butadiene rubber (BR), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers, or a mixture of two or more of these.

[0062] The sulfide-based all-solid-state battery according to the present invention includes the steps of: S1) mixing a polyol and a chelating agent to form a polyol precursor; S2) mixing lithium hydroxide and ammonium niobate oxalate hydrate with the polyol precursor to form a cathode active material coating material; and S3) coating a cathode active material with the cathode active material coating material.

[0063] Here, a chelating agent may not be added in step S1).

[0064] The step S2) can be carried out by a dry mixing method without using a separate solvent, as described above.

[0065] In step S3), the positive electrode active material coating material and the positive electrode active material are mixed together, and then the mixture is heat-treated at 450° C. for 2 hours.

[0066] The heat treatment can be performed by increasing the temperature by 5°C per minute from room temperature (25°C) until the target temperature is reached, and then allowing it to cool naturally to 25°C.

[0067] FIG. 3 is a scanning electron microscope (SEM) image of lithium niobate prepared by a polyol process according to the present invention, and FIG. 4 is a scanning electron microscope (SEM) image of a cathode active material coated with lithium niobate prepared by a polyol process according to the present invention. As shown in FIGS. 3 and 4, the lithium niobate precursor prepared by a polyol process according to the present invention uniformly coats the cathode active material. When the lithium niobate precursor uniformly coats the cathode active material, it prevents the cathode active material from reacting with the sulfide-based solid electrolyte, thereby improving the performance of sulfide-based all-solid-state batteries. Furthermore, dry coating of the cathode active material for sulfide-based all-solid-state batteries reduces the risk of the sulfide-based solid electrolyte reacting with moisture, thereby improving safety and shortening the process.

[0068] This can be seen in more detail in FIGS.

[0069] FIG. 5 is a transmission electron microscope (TEM) photograph of the lithium niobate precursor according to the present invention, and FIG. 6 is a transmission electron microscope (TEM) photograph of the positive electrode active material coated with the lithium niobate precursor according to the present invention.

[0070] As shown in FIG. 5, the lithium niobate precursor according to the present invention has a uniformly distributed shape due to the polyol process.

[0071] As shown in Figure 5, Grey, CK, NbL, and OK represent Li, C, Nb, and O, respectively, and it can be seen that the reaction of lithium niobate with polyol results in each element being uniformly distributed in the precursor.

[0072] In addition, as shown in Figure 6, the uniformly distributed lithium niobate precursor (NbL) is uniformly coated on the uniformly distributed cathode active material (CoK), preventing the cathode active material from reacting with the sulfide-based solid electrolyte.

[0073] The present invention also provides a battery pack including the sulfide-based all-solid-state battery according to the present invention as a unit cell, and a device including the battery pack as a power source. Specifically, the battery pack can be used as a power source for devices requiring high-temperature safety, long cycle characteristics, and high rate characteristics. Suitable examples of such devices include, but are not limited to, mobile electronic devices, wearable electronic devices, power tools powered by battery-based motors, electric vehicles (EVs), hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), and power storage devices.

[0074] The structure of these devices and the methods for fabricating them are well known in the art and will not be discussed in detail here.

[0075] 7 to 9, a sulfide-based all-solid-state battery according to the present invention is used as an example, and a battery in which a positive electrode active material was not synthesized using a lithium niobate precursor as in the present invention is used as a comparison example, and then the specific capacity, capacity retention rate, and impedance value according to voltage are compared.

[0076] The sulfide-based all-solid-state battery used in this example was prepared by: 1) adding 8.6456 mg of citric acid to 100 ml of triethylene glycol (TEG) and mixing for 20 minutes; 2) adding 0.4616 mg of lithium hydroxide and 3.0298 mg of ammonium niobate(v) oxalate hydrate to this mixture at room temperature and synthesizing the mixture at 230°C for 3 hours; 3) gradually cooling the mixture, separating it using a centrifuge, washing it 7-8 times with ethanol, and drying it in a vacuum oven at 50°C to 200°C to form a cathode active material coating. 4) Coating the cathode active material, LiCoO2, with the cathode active material coating. The cathode active material coating and the cathode active material were mixed with a stirrer, and the temperature was raised from room temperature to 450°C in 5°C increments until it reached 450°C, at which point the temperature was maintained for 3 hours without further increase. 5) After 3 hours had passed, the positive electrode active material coating material and the positive electrode active material were gradually cooled to room temperature to obtain a coated positive electrode active material.

[0077] 6) The coated positive electrode active material was then mixed with carbon black, a conductive material, and polyvinylidene fluoride, a binder, and then coated onto an aluminum positive electrode current collector. 7) The electrode slurry was uniformly dispersed on the current collector using a doctor blade and then dried in a vacuum oven at 50°C to 200°C to form a positive electrode. The positive electrode was then stacked with a solid electrolyte layer formed using an LPS-based electrolyte, a sulfide-based solid electrolyte, and an anode using copper as a current collector to form a unit cell.

[0078] For the sulfide-based all-solid-state battery used as a comparative example, a unit cell was formed in the same manner as in the above-described examples, except that a cathode active material not coated with the cathode active material coating material was used.

[0079] 7 is a graph comparing the specific capacity as a function of voltage between a sulfide-based all-solid-state battery according to the present invention and a sulfide-based all-solid-state battery fabricated using an uncoated cathode active material. The unit cell was charged under the conditions of (CC / CV): 0.1 C / 4.15 V, 0.02 C cutoff, and 30 min of rest, and discharged under the conditions of (CC): 0.1 C, 3 V cutoff. The specific capacity value was calculated based on the weight of the cathode, including the cathode material and gas diffusion layer.

[0080] As shown in FIG. 7, the oxygen reduction curve corresponding to the first cycle of the Example is 132 mAh / g, and the oxygen release curve is 120 mAh / g, which is a difference of about 92.0%. On the other hand, the oxygen reduction curve of the Comparative Example is 108 mAh / g, and the oxygen release curve is 92 mAh / g, which is a difference of about 86.1% in the initial charge-discharge characteristics. This confirms that the Example has superior charge-discharge characteristics.

[0081] FIG. 8 is a graph comparing the capacity retention rate of a sulfide-based all-solid-state battery according to the present invention and a sulfide-based all-solid-state battery manufactured using an uncoated cathode active material.

[0082] In FIG. 8, charging was performed under the conditions of (CC / CV): 0.1C / 4.25V, 0.02C, cut-off, 30 min rest, and discharging was performed under the conditions of (CC): 0.1C, 3V cut-off. This process was repeated 50 times.

[0083] As shown in FIG. 8, the sulfide-based all-solid-state battery according to the embodiment of the present invention not only has a higher initial capacity than the comparative example, but also has a better capacity retention rate than the comparative example.

[0084] FIG. 9 is a graph comparing the impedance values ​​of a sulfide-based all-solid-state battery according to the present invention and a sulfide-based all-solid-state battery manufactured using an uncoated cathode active material.

[0085] In FIG. 9, the unit cell was stored in a fully charged state at 60° C. for two weeks, and then disassembled from the glove box and the AC impedance of the unit cell was measured.

[0086] As shown in FIG. 9, the unit cell according to the embodiment has a lower interfacial resistance between the positive electrode and the solid electrolyte than the comparative example.

[0087] Therefore, it can be seen that when a cathode active material is dry-coated with a lithium niobate precursor prepared by a polyol process as in the present invention, the performance of a sulfide-based all-solid-state battery is superior to that when the cathode active material is not coated with a lithium niobate precursor.

[0088] Although specific portions of the contents of the present invention have been described in detail above, it will be apparent to those skilled in the art that such specific techniques are merely preferred embodiments and do not limit the scope of the present invention. It is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of ​​the present invention, and it goes without saying that such changes and modifications also fall within the scope of the accompanying claims.

Claims

1. A method for producing a sulfide-based all-solid-state battery, comprising: Coating a positive electrode active material, The coating comprises: S1) mixing a polyol and a chelating agent to form a polyol precursor; S2) mixing the polyol precursor with lithium hydroxide and ammonium niobate oxalate hydrate to form a lithium niobate precursor, and then drying the resulting mixture; S3) dry-mixing the positive electrode active material and the lithium niobate precursor.

2. The method for producing a sulfide-based all-solid-state battery according to claim 1, wherein the coating is performed by dry-mixing the positive electrode active material and the lithium niobate precursor and then performing a heat treatment at 400° C. or more.

3. 3. The method for producing a sulfide-based all-solid-state battery according to claim 2, wherein the coating is performed by dry-mixing the positive electrode active material and the lithium niobate precursor, increasing the temperature by 5° C. per minute until a target temperature is reached, and then naturally cooling the mixture.

4. The method for producing a sulfide-based all-solid-state battery according to any one of claims 1 to 3, wherein the lithium niobate precursor contains lithium niobate and a chelating agent.

5. 5. The method for producing a sulfide-based all-solid-state battery according to claim 4, wherein the chelating agent is at least one selected from the group consisting of citric acid, polyvinylpyrrolidone (PVP), a carboxylic acid, and a weak acid containing a nitrogen element.

6. The method for producing a sulfide-based all-solid-state battery according to any one of claims 1 to 5, wherein the lithium niobate precursor is coated on the positive electrode active material in an amount of 1 nm to 100 nm or less.

7. The method for producing a sulfide-based all-solid-state battery according to any one of claims 1 to 6, wherein the positive electrode active material is lithium cobalt oxide.

8. S1) mixing a polyol and a chelating agent to form a polyol precursor; S2) mixing the polyol precursor with lithium hydroxide and ammonium niobate oxalate hydrate to form a lithium niobate precursor, and then drying the resulting mixture; S3) dry mixing a positive electrode active material with the lithium niobate precursor.

9. 9. The method of claim 8, wherein in step S3), the lithium niobate precursor and the positive active material are mixed, and then heat-treated at 450° C. or more for 2 hours.

10. 10. The method of claim 9, wherein the heat treatment at 450° C. or more for 2 hours is performed by increasing the temperature by 5° C. per minute until the target temperature is reached and then naturally cooling the temperature.

11. The method for producing a sulfide-based all-solid-state battery according to any one of claims 1 to 7, wherein the weight ratio of the lithium niobate precursor to the positive electrode active material is 1 to 10:90 to 99.

12. The method for producing a sulfide-based all-solid-state battery according to claim 3 , wherein the target temperature does not exceed 500° C.

13. The method for coating a positive electrode active material according to claim 8 , wherein the polyol is a polyether polyol or a polyester polyol.

14. The method for coating a positive electrode active material according to claim 10, wherein the target temperature does not exceed 500°C.

Citation Information

Patent Citations

  • JP1974082866A

  • Lithium-transition metal oxide powder and manufacturing method thereof, cathode active material for lithium ion battery, and lithium ion secondary battery

    JP2012074240A

  • Method for manufacturing active material composite powder

    JP2017059303A

  • Lithium niobate and manufacturing method thereof

    JP2020035607A

  • Manufacturing method of positive electrode layer

    JP2020035608A