Method for forming piezoelectric film and piezoelectric device
By employing a buffer layer and sputtering method to orient LiNbO3 or LiTaO3 films in the (012) plane direction, the method addresses the challenge of achieving high electromechanical coupling, enhancing the performance of piezoelectric devices.
Patent Information
- Application Number
- JP2021064232
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-04-05
AI Technical Summary
Existing methods for forming piezoelectric films using LiNbO3 or LiTaO3 struggle to achieve high electromechanical coupling coefficients due to challenges in controlling the orientation of the piezoelectric film, particularly when oriented in the (012) plane direction, which is essential for optimal performance.
A method involving the use of a buffer layer, such as LaNiO3, SrRuO3, or Ag, to orient the crystal structure of the piezoelectric film in the (012) plane direction, combined with a sputtering process to form the film, ensuring precise control over the film's orientation and enhancing the electromechanical coupling.
This approach allows for the formation of piezoelectric films with improved mechanical-electrical coupling coefficients, enabling better performance in devices like FBAR type filters by accurately aligning the crystal orientation of LiNbO3 or LiTaO3 films.
Smart Images

Figure 0007575335000002 
Figure 0007575335000003 
Figure 0007575335000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming a piezoelectric film and a piezoelectric device. [Background technology]
[0002] Demand in the communications field is increasing against the backdrop of the rapid expansion of the IoT-related market. Improvements in communication connection speed and bandwidth have led to a demand for improved filter performance. Currently, FBAR filters (Film Bulk Acoustic Resonators) and SAW filters (Surface Acoustic Wave filters) are the mainstream filters, and are differentiated by frequency band. For example, the bulk acoustic resonator described in Patent Document 1 is known as an FBAR filter.
[0003] As exemplified in Patent Document 1, aluminum nitride (AlN) is usually used for the piezoelectric film of an FBAR filter. However, in recent years, in order to further improve performance, materials with excellent electromechanical coupling coefficients have been required, and the development of Sc-doped AlN (Sc-AlN) has become active. In addition, the development of piezoelectric films using LiNbO3 or LiTaO3 instead of AlN has also become active.
[0004] LiNbO3 has a maximum electromechanical coupling coefficient of 50% for quasi-longitudinal waves when the bulk is cut in a 36° rotated Y-cut, while the electromechanical coupling coefficient of Sc-doped AlN (Sc-AlN) is at most 20%, suggesting its high potential performance. However, LiNbO3 is said to have a maximum electromechanical coupling coefficient when oriented in a direction equivalent to the 36° rotated Y-cut direction of a single crystal, so in order to form a piezoelectric film made of LiNbO3, the orientation direction must be accurately controlled in the thin film formation process. In addition, LiTaO3 is also said to have a high electromechanical coupling coefficient when oriented in the 36° rotated Y-cut direction, so the orientation direction must be controlled during thin film formation, just like LiNbO3. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-193168 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in order to configure an FBAR filter, it is necessary to form a lower electrode on a substrate, form a piezoelectric film made of a piezoelectric material on the lower electrode, and then form an upper electrode on the lower electrode. The material of the lower electrode can be, for example, molybdenum, ruthenium, tungsten, iridium, platinum, etc., but when a piezoelectric film made of LiNbO3 or LiTaO3 is formed on a lower electrode made of these materials, LiNbO3 or LiTaO3 is oriented in the c-axis direction, which is the direction corresponding to the Z-cut direction in a single crystal, and is not oriented in the (012) direction, which is the direction corresponding to the 36° rotated Y-cut direction, so the formed piezoelectric film cannot exhibit a high electromechanical coupling coefficient.
[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for forming a piezoelectric film that is capable of controlling the orientation of LiNbO3 or LiTaO3 when forming a LiNbO3 or LiTaO3 film by a sputtering method, and a piezoelectric device including such a piezoelectric film. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention employs the following configuration. [1] A method for forming a piezoelectric film made of LiNbO3 or LiTaO3, comprising the steps of: On the substrate forming a lower electrode layer on the lower electrode layer; A buffer layer that orients the crystal orientation of the piezoelectric film in the (012) plane direction. LaNiO3 and SrRuO 3 , LaCoO 3 or KNaNbO 3 Either one of forming said buffer layer above and forming the piezoelectric film by a sputtering method. [2] A method for forming a piezoelectric film made of LiNbO3 or LiTaO3, comprising the steps of: A method for forming a piezoelectric film, comprising the steps of: forming, on a substrate, Ag having a crystal orientation oriented in the (002) plane as a buffer layer that orients the crystal orientation of the piezoelectric film in the (012) plane and also serves as a lower electrode layer; and forming the piezoelectric film on the buffer layer by a sputtering method. [3] A method for forming a piezoelectric film made of LiNbO3 or LiTaO3, comprising the steps of: A method for forming a piezoelectric film, comprising: forming a TiN buffer layer on a substrate, which serves to orient the crystal orientation of the piezoelectric film in a (012) plane direction; forming a lower electrode layer on the buffer layer; and forming the piezoelectric film on the lower electrode layer by a sputtering method. [ 4 The buffer layer is LaNiO 3 Consists of The method for forming the piezoelectric film described in [1]. [ 5 The buffer layer is a layer formed of one of TiN, TiW, and TiWN on an Ag film. 2 13. A method for forming a piezoelectric film according to claim 12. [ 6 The sputtering method is a co-sputtering method using a first target made of niobium oxide or tantalum oxide and a second target made of lithium oxide. [1] Any one of items [5] The method for forming the piezoelectric film according to claim 1 。 [ 7 A substrate; A lower electrode; a buffer layer disposed on the lower electrode; a piezoelectric film made of LiNbO3 or LiTaO3 arranged on the buffer layer and having a crystal orientation oriented in the (012) plane direction; an upper electrode disposed on the piezoelectric film; The buffer layer is Perovskite structure LaNiO3, SrRuO 3 , LaCoO 3 or KNaNbO 3 Any one of That is, a piezoelectric device. [ 8 A substrate; a buffer layer disposed on the substrate and serving as a lower electrode; a piezoelectric film made of LiNbO3 or LiTaO3 arranged on the buffer layer and having a crystal orientation oriented in the (012) plane direction; an upper electrode disposed on the piezoelectric film; The buffer layer is Ag with crystal orientation along the (002) plane That is, a piezoelectric device. [ 9 A substrate; The above Base material a buffer layer disposed thereon; a lower electrode disposed on the buffer layer; a piezoelectric film made of LiNbO3 or LiTaO3 arranged on the lower electrode and having a crystal orientation oriented in the (012) plane direction; an upper electrode disposed on the piezoelectric film; The buffer layer is TiN That is, a piezoelectric device. [ 10 The buffer layer is LaNiO 3 Consists of , [ 7 ] A piezoelectric device according to the 。
[11] A film made of one of TiN, TiW, and TiWN is laminated on the buffer layer. [ 8 ] A piezoelectric device according to the 。 [ 12 The thickness of the piezoelectric film is 300 nm or less. 7 ]~[ 11 ] A piezoelectric device according to any one of the above items. [ 13 When the piezoelectric film is subjected to an X-ray diffraction rocking curve measurement, the half-width of the X-ray diffraction peak of the (012) plane of the piezoelectric film is 10° or less. [ 7 ]~[ 12 ] A piezoelectric device according to any one of the above items. [ 14 ] [ 7 ]~[ 13 ] The piezoelectric device according to any one of the above items 1 to 5, wherein the piezoelectric device is an FBAR type filter or a SAW type filter. Effect of the Invention
[0009] According to the method for forming a piezoelectric film of the present invention, it is possible to provide a method for forming a piezoelectric film capable of controlling the orientation of LiNbO3 or LiTaO3, and a piezoelectric device including the piezoelectric film. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a piezoelectric device according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of a piezoelectric device according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing an example of a sputtering apparatus used in the method for forming a piezoelectric film according to an embodiment of the present invention. [Figure 4] FIG. 4 is a schematic cross-sectional view showing another example of a sputtering apparatus used in the method for forming a piezoelectric film according to an embodiment of the present invention. [Diagram 5] FIG. 5 is a process diagram illustrating a manufacturing process of a piezoelectric device according to an embodiment of the present invention. [Figure 6] FIG. 6 is a process diagram illustrating a manufacturing process of a piezoelectric device according to an embodiment of the present invention. [Figure 7] FIG. 7 is a process diagram illustrating a manufacturing process of a piezoelectric device according to an embodiment of the present invention. [Figure 8] FIG. 8 is a process diagram illustrating a manufacturing process of a piezoelectric device according to an embodiment of the present invention. [Figure 9] FIG. 9 is a process diagram illustrating a manufacturing process of a piezoelectric device according to an embodiment of the present invention. [Figure 10] FIG. 10 is a process diagram illustrating a manufacturing process of a piezoelectric device according to an embodiment of the present invention. [Figure 11] FIG. 11 is a process diagram illustrating a manufacturing process of a piezoelectric device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A method for forming a piezoelectric film and a piezoelectric device according to embodiments of the present invention will now be described with reference to the drawings.
[0012] First, a basic embodiment of the present invention will be described. Fig. 1 shows a schematic cross-sectional view of an example of a piezoelectric device according to this embodiment. The piezoelectric device shown in Fig. 1 includes a substrate 1, a buffer layer 2 disposed on the substrate 1, and a piezoelectric film 3 disposed on the buffer layer 2 and made of LiNbO3 or LiTaO3 with its crystal orientation oriented in the (012) plane direction. The buffer layer 2 is a layer that orients the crystal orientation of the piezoelectric film 3 in the (012) plane direction.
[0013] 2 is a schematic cross-sectional view showing another example of a piezoelectric device according to this embodiment. The piezoelectric device shown in Fig. 2 includes a substrate 1, a buffer layer 2 disposed on the substrate 1, an anti-oxidation film 4 disposed on the buffer layer 2, and a piezoelectric film 3 disposed on the anti-oxidation film 4. The buffer layer 2 is a layer that orients the crystal orientation of the piezoelectric film 3 in the (012) plane direction.
[0014] As will be described later, another layer may be laminated between the buffer layer 2 and the piezoelectric film 3.
[0015] There is no particular limitation on the substrate 1 as long as it can be used as a substrate in a thin film deposition process. The substrate 1 may be, for example, a semiconductor substrate made of single crystal silicon. Alternatively, the substrate 1 may be a semiconductor substrate made of single crystal silicon with a silicon oxide film formed on the surface.
[0016] An electrode layer for applying a voltage to the piezoelectric film 3 may be provided on the semiconductor substrate forming the base material 1. In this case, it is preferable that the buffer layer 2 and the piezoelectric film 3 are laminated on the electrode layer. Furthermore, when the buffer layer 2 is made of a conductor, the buffer layer 2 can also serve as the electrode layer. In this case, the buffer layer 2 and the piezoelectric film 3 serving as the electrode layer may be laminated on the semiconductor substrate forming the base material 1, or the buffer layer 2 serving as the electrode layer, the oxidation prevention film 4, and the piezoelectric film 3 may be laminated on the semiconductor substrate. The electrode layer is preferably made of a conductor or a semiconductor. Also, as described later, an electrode layer may be laminated as a separate layer between the buffer layer 2 and the piezoelectric film 3. Also, an adhesive layer may be formed between the base material 1 and the electrode layer. The adhesive layer may be, for example, a titanium oxide film.
[0017] The material of the electrode layer can be Pt, Mo, Ru, W, Ir, etc. If a piezoelectric film is directly formed on an electrode layer made of these materials, the crystal orientation of LiNbO3 or LiTaO3 will be oriented in the (001) plane direction, and it is difficult to orient it in the (012) plane direction.
[0018] Specifically, the buffer layer 2 is preferably made of Ag, LaNiO3, or TiN, whose crystal orientation is oriented in the (002) plane direction. By forming the buffer layer 2, when a piezoelectric film made of LiNbO3 or LiTaO3 is laminated on the buffer layer 2, the crystal orientation of LiNbO3 or LiTaO3 can be oriented in the (012) plane direction. The buffer layer 2 is preferably made of a conductor or a semiconductor. Also, SrRuO3, LaCoO3, KNaNbO3, or the like, which have a perovskite structure similar to LaNiO3, can be used as the buffer layer 2.
[0019] Furthermore, as described above, when the buffer layer 2 is made of a conductor such as Ag, it may function as an electrode when applying a voltage to the piezoelectric film 3. When the buffer layer 2 made of Ag is formed on the substrate 1 made of single crystal silicon, if a silicon oxide film, which is a natural oxide film, exists on the surface of the substrate 1, it is preferable to remove the silicon oxide film in advance by known hydrofluoric acid treatment or dry etching.
[0020] Furthermore, when the buffer layer 2 is made of Ag, an anti-oxidation film 4 may be laminated on the buffer layer 2 as shown in FIG.
[0021] The thickness of the buffer layer 2 is preferably in the range of 10 to 150 nm, more preferably in the range of 30 to 150 nm, and further preferably in the range of 40 to 100 nm. When the buffer layer 2 has a sufficient thickness, the piezoelectric film 3 can be oriented in a desired crystal orientation. Furthermore, when the buffer layer 2 is not excessively thick, electrical conductivity can be ensured, and a voltage can be applied to the piezoelectric film 3.
[0022] The oxidation-resistant film 4 is preferably made of one of TiN, TiW, and TiWN. The oxidation-resistant film 4 prevents oxidation of the buffer layer 2 and also suppresses oxidation of the oxidation-resistant film itself. The oxidation-resistant film 4 is preferably a layer that orients the crystal orientation of the piezoelectric film 3 in the (012) plane direction, like the buffer layer 2. This allows the crystal orientation of the surface of the piezoelectric film 3 to be oriented in the (012) plane direction even when the piezoelectric film 3 is formed on the oxidation-resistant film 4. Furthermore, by forming the oxidation-resistant film 4 on the buffer layer 2, even when the atmosphere is an oxidizing atmosphere during the deposition of the piezoelectric film 3, oxidation of the surface of the buffer layer 2 can be suppressed, and oxidation of the oxidation-resistant film 4 itself is also suppressed. This prevents the formation of an oxide layer on the buffer layer 2, and allows the crystal orientation of the piezoelectric film 3 to be oriented in the (012) plane direction. Furthermore, the oxidation-resistant film 4 is preferably made of a conductor or a semiconductor.
[0023] The thickness of the oxidation-resistant film 4 is preferably in the range of 10 to 200 nm, and more preferably in the range of 40 to 100 nm. When the oxidation-resistant film 4 has a sufficient thickness, it is possible to sufficiently suppress oxidation of the buffer layer 2, and also to orient the piezoelectric film 3 in a desired crystal orientation. When the oxidation-resistant film 4 is not excessively thick, it is possible to ensure electrical conductivity, and it becomes possible to apply a voltage to the piezoelectric film 3.
[0024] The piezoelectric film 3 is made of LiNbO3 or LiTaO3 with a crystal orientation oriented in the (012) plane direction on the surface. Both LiNbO3 and LiTaO3 are complex oxides with a trigonal ilmenite-like structure and have similar crystal structures. LiNbO3 and LiTaO3 have a mechanical and electrical coupling coefficient (quasi-longitudinal wave) of up to about 50% in the plane corresponding to the 36° rotated Y-cut direction in the single crystal, and can be suitably used for piezoelectric devices. Conventionally, when LiNbO3 or LiTaO3 is formed by a thin film formation process, only the one oriented in the C-axis direction ((001) plane direction) is obtained. In this embodiment, however, by forming the piezoelectric film 3 on the buffer layer 2 by a sputtering method, the one oriented in the (012) plane direction is obtained, and the film thickness is extremely thin, which can significantly improve the characteristics of the piezoelectric device.
[0025] The thickness of the piezoelectric film 3 is not particularly limited, but is preferably 300 nm or less, and may be 200 nm or less. By making the thickness of the piezoelectric film 3 300 nm or less, for example, when the piezoelectric film 3 is used as a piezoelectric film of a high frequency filter, a resonance frequency of 12.23 GHz can be obtained, and even if a signal of 10 GHz band is input, it can function as a filter. In the conventional technology, when a piezoelectric film made of LiNbO3 or LiTaO3 oriented in the (012) plane direction is obtained, there is no other means than cutting it out from a single crystal, and in this case, it is extremely difficult to cut out a film with a thickness of 300 nm or less from a single crystal. However, since the piezoelectric film 3 of this embodiment can be formed by a sputtering method as described later, it is easy to make the film thickness 300 nm or less.
[0026] The thickness of the piezoelectric film 3 is not limited to 300 nm or less, and may be adjusted according to the resonant frequency band required for the piezoelectric device. For example, the lower limit may be 40 nm or more, and the upper limit may be 2000 nm or less, but the thickness of the piezoelectric film 3 is not limited to the range of 40 to 2000 nm.
[0027] Furthermore, the half-width of the X-ray diffraction peak of the (012) plane of the piezoelectric film 3 is preferably 10° or less. The half-width is measured by subjecting the piezoelectric film 3 to an X-ray diffraction rocking curve measurement (so-called ω measurement). When the half-width is 10° or less, the crystallinity of the piezoelectric film 3 is improved, and the mechanical / electrical coupling coefficient can be further increased. The half-width is more preferably 2° or less.
[0028] Furthermore, another electrode layer for applying a voltage to the piezoelectric film 3 may be provided on the piezoelectric film 3. The other electrode layer is preferably made of a conductor or a semiconductor. The other electrode layer may be made of the same material and have the same thickness as the electrode layer described above.
[0029] The piezoelectric device of this embodiment is preferably used as an FBAR type filter or a SAW type filter. Furthermore, the piezoelectric device of this embodiment can also be applied to an XBAR (Bulk Acoustic Wave Plate wave device) and a HAL (Hetero Acoustic Layer) SAW. In addition, it can also be applied to a coating layer between a positive electrode active material and a solid electrolyte of an all-solid-state battery, and to an optical modulation device.
[0030] According to the piezoelectric device of this embodiment, since it has a piezoelectric film 3 made of LiNbO3 or LiTaO3 oriented in the (012) plane on the film surface, the mechanical and electrical coupling coefficient is high, and it is possible to exhibit an excellent piezoelectric effect. Furthermore, the piezoelectric film 3 in which the half-width of the X-ray diffraction peak of the (012) plane is set to 10° or less has a higher mechanical and electrical coupling coefficient and can exhibit a more excellent piezoelectric effect.
[0031] Furthermore, the piezoelectric device of this embodiment can function as a filter by arranging electrode layers on both sides in the thickness direction of the piezoelectric film 3. In particular, it can function as an FBAR type filter.
[0032] Next, a method for forming the piezoelectric film of this embodiment will be described. The method for forming a piezoelectric film in this embodiment is a method for forming a piezoelectric film 3 made of LiNbO3 or LiTaO3, in which a buffer layer 2 is formed on a substrate 1, and the piezoelectric film 3 is formed above the buffer layer 2 by a sputtering method.
[0033] The buffer layer 2 may be formed on the substrate 1, or an electrode layer may be formed on the substrate 1 and the buffer layer 2 may be formed thereon. The means for forming the buffer layer 2 is not particularly limited, but it is preferable to form it by a sputtering method. When forming the buffer layer 2 made of LaNiO3, it is preferable to form it by an RF sputtering method, and in particular, a reactive sputtering method in which oxygen is introduced into the atmospheric gas is preferable. When forming the buffer layer 2 made of Ag, it may be a DC sputtering method or an RF sputtering method. In addition, TiN, SrRuO3, LaCoO3, KNaNbO3, etc. may be formed as the buffer layer 2. In addition, the buffer layer 2 may be formed on the substrate 1, an electrode layer may be formed on the buffer layer 2, and the piezoelectric film 3 may be formed on the electrode layer.
[0034] Fig. 3 shows a schematic diagram of a sputtering apparatus preferably used for forming the buffer layer 2, the antioxidant film 4, and the piezoelectric film 3. The sputtering apparatus shown in Fig. 3 includes a substrate electrode 11 that also serves as a substrate stage, a cathode electrode 12 that is disposed at a distance from the substrate electrode 11, and a target 13 attached to the cathode electrode 12.
[0035] The substrate 1 is placed on the substrate electrode 11. The substrate electrode 11 has a built-in heater (not shown) that can heat the substrate 1. A bias power supply (not shown) is connected to the substrate electrode 11. A cathode power supply (not shown) is connected to the cathode electrode 12. The substrate electrode 11, the cathode electrode 12, and the target 13 are housed in a chamber (not shown). The inside of the chamber can be controlled to a vacuum atmosphere.
[0036] The conditions for forming the buffer layer 2 are as follows: the composition of the target 13 is LaNiO3, Ag or TiN, the substrate temperature is in the range of 250 to 800°C, the film formation pressure is 0.1 to 1.0 Pa, the Ar flow rate is 0 to 100 sccm, the O2 flow rate is 0 to 15 sccm, the N2 flow rate is 0 to 50 sccm, the power in the case of RF sputtering is 100 to 15,000 W (frequency 13.56 MHz), and the power in the case of DC sputtering is 100 to 15,000 W.
[0037] Next, an oxidation-resistant film 4 may be formed on the buffer layer 2. The method for forming the oxidation-resistant film 4 is not particularly limited, but it may be formed by a sputtering method, either an RF sputtering method or a DC sputtering method, and in particular, a reactive sputtering method in which nitrogen is introduced into the atmospheric gas is preferable.
[0038] The conditions for forming the oxidation-resistant film 4 are as follows: target composition is Ti or TiW, substrate temperature is in the range of room temperature (25°C) to 400°C, film formation pressure is 0.1 to 1 Pa, Ar flow rate is 0 to 30 sccm, N2 flow rate is 0 to 40 sccm, power in the case of RF sputtering is 100 to 15,000 W (frequency 13.56 MHz), and power in the case of DC sputtering is 100 to 15,000 W.
[0039] Next, a piezoelectric film 3 made of LiNbO3 or LiTaO3 is formed on the buffer layer 2 or the oxidation prevention film 4. The piezoelectric film 3 is formed by sputtering. Among them, it is preferable to form it by RF sputtering, and particularly, reactive sputtering in which oxygen is introduced into the atmospheric gas is preferable.
[0040] The conditions for forming the piezoelectric film 3 are as follows: target composition is LiNbO3 or LiTaO3, substrate temperature is in the range of 300 to 650°C, film formation pressure is 0.1 to 1.0 Pa, Ar flow rate is 50 to 150 sccm, O2 flow rate is 0.1 to 50 sccm, and RF sputtering power is 50 to 2800 W (frequency 13.56 MHz). This results in a piezoelectric film 3 whose surface crystal orientation is oriented in the (012) plane.
[0041] As another method, a co-sputtering method using a first target made of niobium oxide or tantalum oxide and a second target made of lithium oxide may be performed. The niobium oxide or tantalum oxide may be a composite oxide such as LiNbO3 or LiTaO3 in addition to Nb2O5 or Ta2O5. The first target may be a target made of niobium or tantalum metal.
[0042] A schematic diagram of a sputtering apparatus for carrying out the co-sputtering method is shown in Fig. 4. The sputtering apparatus shown in Fig. 4 includes a substrate electrode 21 that also serves as a substrate stage, two cathode electrodes 22 and 23 arranged at a distance from the substrate electrode 21, a first target 24 attached to one of the cathode electrodes 22, and a second target 25 attached to the other cathode electrode 23.
[0043] A plurality of substrates 1 can be placed on the substrate electrode 21. The substrate electrode 21 has a built-in heater (not shown) that can heat the substrates 1. The substrate electrode 21 is also connected to a driving means (not shown) and can rotate. By rotating the substrate electrode 21, the substrates 1 placed on the substrate electrode 21 come to face the first target 24 and the second target 25 alternately.
[0044] Furthermore, a bias power supply (not shown) is connected to the substrate electrode 21. Moreover, cathode electrodes 22 and 23 are each connected to a cathode power supply (not shown).
[0045] The substrate electrode 21, the cathode electrodes 22, 23, the first target 24 and the second target 25 are accommodated in a chamber (not shown), the inside of which can be controlled to a vacuum atmosphere.
[0046] In the method for forming a piezoelectric film of this embodiment, a piezoelectric film 3 made of LiNbO3 or LiTaO3 is formed by sputtering on a buffer layer 2 or an oxidation resistant film 4. By selecting a material for the buffer layer 2 or the oxidation resistant film 4 that orients the crystal orientation of the piezoelectric film 3 in the (012) plane direction, the piezoelectric film 3 made of LiNbO3 or LiTaO3 formed thereon is oriented in the (012) plane direction on the film surface. This increases the mechanical and electrical coupling coefficient of the piezoelectric film 3, enabling it to exhibit an excellent piezoelectric effect.
[0047] In particular, by using a buffer layer 2 made of TiN, LaNiO3, or Ag with a crystal orientation oriented in the (002) plane direction, it becomes easy to orient the crystal orientation of the piezoelectric film 3 made of LiNbO3 or LiTaO3 in the (012) plane direction, allowing the piezoelectric film 3 to exhibit an excellent piezoelectric effect. Also, a buffer layer made of SrRuO3, LaCoO3, KNaNbO3, etc. may be used as the buffer layer 2 for orienting the crystal orientation of the piezoelectric film 3 in the (012) plane direction.
[0048] Furthermore, by forming an oxidation prevention film 4 on the buffer layer 2, the piezoelectric film 3 made of LiNbO3 or LiTaO3 can be formed while preventing the buffer layer 2 from being oxidized, and the crystal orientation can be controlled to a preferred orientation.
[0049] Next, a more specific embodiment of the present invention will be described.
[0050] 5 and 6 show a manufacturing process for an FBAR type filter as an example of the piezoelectric device of this embodiment. 5(a), a recess 31a that will later become a cavity is formed on a semiconductor substrate 31, and a sacrificial layer 32 is formed in the recess 31a. The semiconductor substrate 31 provided with the sacrificial layer 32 serves as the base material 1. An example of the semiconductor substrate 31 is a single crystal silicon substrate. A silicon oxide film (not shown) may be formed as a passivation film on the surface of the single crystal silicon substrate.
[0051] 5(b), a lower electrode layer 33 made of Pt, Mo, Ru, W, Ir, or the like is formed on the semiconductor substrate 31 and the sacrificial layer 32. The lower electrode layer 33 is preferably formed by DC sputtering using a target of Pt, Mo, Ru, W, Ir, or the like. The thickness of the lower electrode layer 33 is in the range of, for example, 10 to 200 nm.
[0052] 5(c), a buffer layer 2 made of LaNiO3 is formed on the lower electrode layer 33. The manufacturing conditions of the buffer layer 2 are as described above. As a result, the buffer layer 2 orients the crystal orientation of the piezoelectric film 3 in the (012) plane direction. The thickness of the buffer layer 2 is, for example, in the range of 10 to 100 nm.
[0053] Next, as shown in Fig. 5(d), a piezoelectric film 3 made of LiNbO3 or LiTaO3 is formed on the buffer layer 2. The manufacturing conditions of the piezoelectric film 3 are as described above. As a result, the crystal orientation of the piezoelectric film 3 is oriented in the (012) plane direction within the surface of the piezoelectric film 3. The thickness of the piezoelectric film 3 is, for example, in the range of 300 nm or less.
[0054] 6(a), an upper electrode layer 34 made of Pt, Mo, Ru, W, Ir, or the like is formed on the piezoelectric film 3. The upper electrode layer 34 is preferably formed by DC sputtering using a target of Pt, Mo, Ru, W, Ir, or the like. The thickness of the upper electrode layer 34 is in the range of, for example, 10 to 200 nm.
[0055] 6(b), the upper electrode layer 34 and the piezoelectric film 3 are patterned into a predetermined planar shape by photolithography and etching. The upper electrode layer 34 and the piezoelectric film 3 are preferably patterned so as to remain at least above the sacrificial layer 32. As a result, a laminate K1 consisting of the lower electrode layer 33, the buffer layer 2, the piezoelectric film 3 and the upper electrode layer 34 is formed on the sacrificial layer 32.
[0056] Next, as shown in Fig. 6(c), the sacrificial layer 32 is removed to form a cavity C under the laminate K1. In this manner, the piezoelectric device of this embodiment is obtained. The piezoelectric device shown in Fig. 6(c) functions as an FBAR type filter.
[0057] Next, FIG. 7 and FIG. 8 show a manufacturing process for an FBAR type filter, which is another example of the piezoelectric device of this embodiment. As shown in FIG. 7(a), in the same manner as in FIG. 5(a), a recess 31a that will later become a cavity is formed on a semiconductor substrate 31, and a sacrificial layer 32 is formed in the recess 31a.
[0058] Next, as shown in FIG. 7(b), a buffer layer 2 made of Ag is formed. The buffer layer 2 made of Ag also functions as the lower electrode of the piezoelectric device. The manufacturing conditions of the buffer layer 2 are as described above. As a result, the crystal orientation of the buffer layer 2 made of Ag is oriented in the (002) plane direction within the surface of the buffer layer 2. The thickness of the buffer layer 2 is, for example, in the range of 10 to 100 nm.
[0059] Next, as shown in Fig. 7(c), a piezoelectric film 3 made of LiNbO3 or LiTaO3 is formed on the buffer layer 2 in the same manner as in Fig. 5(d). The manufacturing conditions of the piezoelectric film 3 are as described above. As a result, the crystal orientation of the piezoelectric film 3 is oriented in the (012) plane direction within the surface of the piezoelectric film 3. The thickness of the piezoelectric film 3 is, for example, in the range of 300 nm or less.
[0060] Next, as shown in FIG. 8(a), an upper electrode layer 34 made of Pt, Mo, Ru, W, Ir or the like is formed on the piezoelectric film 3.
[0061] 8(b), the upper electrode layer 34 and the piezoelectric film 3 are patterned into a predetermined planar shape by photolithography and etching. The upper electrode layer 34 and the piezoelectric film 3 are preferably patterned so as to remain at least above the sacrificial layer 32. As a result, a laminate K2 consisting of the buffer layer 2, the piezoelectric film 3, and the upper electrode layer 34, which functions as a lower electrode, is formed on the sacrificial layer 32.
[0062] Next, as shown in Fig. 8(c), the sacrificial layer 32 is removed to form a cavity C under the laminate K2. In this manner, the piezoelectric device of this embodiment is obtained. The piezoelectric device shown in Fig. 8(c) functions as an FBAR type filter.
[0063] Next, FIG. 9 and FIG. 10 show a manufacturing process for an FBAR type filter as yet another example of the piezoelectric device of this embodiment. As shown in FIG. 9(a), in the same manner as in FIG. 5(a), a recess 31a that will later become a cavity is formed on a semiconductor substrate 31, and a sacrificial layer 32 is formed in the recess 31a.
[0064] Next, as shown in Fig. 9(b), a buffer layer 2 made of Ag is formed in the same manner as in Fig. 7(b). The buffer layer 2 made of Ag also functions as the lower electrode of the piezoelectric device.
[0065] 9(c), an oxidation-resistant film 4 made of one of TiN, TiW, and TiWN is formed on the buffer layer 2. The manufacturing conditions of the oxidation-resistant film 4 are as described above. The oxidation-resistant film 4 orients the crystal orientation of the piezoelectric film in the (012) plane direction. The thickness of the oxidation-resistant film 4 is, for example, in the range of 10 to 100 nm.
[0066] Next, as shown in Fig. 9(d), a piezoelectric film 3 made of LiNbO3 or LiTaO3 is formed on the oxidation resistant film 4 in the same manner as in Fig. 5(d). The manufacturing conditions of the piezoelectric film 3 are as described above. As a result, the crystal orientation of the piezoelectric film 3 is oriented in the (012) plane direction within the surface of the piezoelectric film 3. The thickness of the piezoelectric film 3 is, for example, in the range of 300 nm or less.
[0067] Next, as shown in FIG. 10(a), an upper electrode layer 34 made of Pt, Mo, Ru, W, Ir or the like is formed on the piezoelectric film 3.
[0068] 10(b), the upper electrode layer 34 and the piezoelectric film 3 are patterned into a predetermined planar shape by photolithography and etching. The upper electrode layer 34 and the piezoelectric film 3 are preferably patterned so as to remain at least above the sacrificial layer 32. As a result, a laminate K3 is formed on the sacrificial layer 32, which is composed of the buffer layer 2 functioning as a lower electrode, the oxidation prevention film 4, the piezoelectric film 3, and the upper electrode layer 34.
[0069] Next, as shown in Fig. 10(c), the sacrificial layer 32 is removed to form a cavity C under the laminate K3. In this manner, the piezoelectric device of this embodiment is obtained. The piezoelectric device shown in Fig. 10(c) functions as an FBAR type filter.
[0070] Next, FIG. 11 shows a manufacturing process for an FBAR type filter as yet another example of the piezoelectric device of this embodiment. 11(a), a semiconductor substrate 31 having a silicon oxide film 31a formed thereon is prepared. The semiconductor substrate 31 is preferably a single crystal silicon substrate.
[0071] Next, as shown in FIG. 11(b), a buffer layer 2 made of Ag is formed. The buffer layer 2 made of Ag also functions as the lower electrode of the piezoelectric device. The manufacturing conditions of the buffer layer 2 are as described above. As a result, the crystal orientation of the buffer layer 2 made of Ag is oriented in the (002) plane direction on the surface thereof, and the crystal orientation of the piezoelectric film is oriented in the (012) plane direction. An oxidation prevention film may be further formed on the buffer layer 2.
[0072] 11(c), a piezoelectric film 3 made of LiNbO3 or LiTaO3 is formed on the buffer layer 2. The manufacturing conditions of the piezoelectric film 3 are as described above. As a result, the crystal orientation of the piezoelectric film 3 is oriented in the (012) plane direction within the surface of the piezoelectric film 3.
[0073] 11(d), an upper electrode layer 34 made of Pt, Mo, Ru, W, Ir, or the like is formed on the piezoelectric film 3. As a result, a laminate K4 is formed that functions as a lower electrode and is made up of the buffer layer 2, the piezoelectric film 3, and the upper electrode layer 34.
[0074] Next, as shown in FIG. 11(e), an insulating film 35 is formed so as to cover the semiconductor substrate 31 and the laminate K4.
[0075] Next, as shown in Fig. 11(f), a cavity C is formed under the laminate K4 by performing via processing from the back side of the semiconductor substrate 31. In this manner, the piezoelectric device of this embodiment is obtained. The piezoelectric device shown in Fig. 11(f) functions as an FBAR type filter.
[0076] Furthermore, the piezoelectric device of this embodiment is not limited to the form shown in FIG. 1 and FIG. 2. For example, a buffer layer 2 may be formed on a substrate 1, an electrode layer (lower electrode) may be formed on the buffer layer, and a piezoelectric film 3 made of LiNbO3 or LiTaO3 with a crystal orientation oriented in the (012) plane direction may be formed on the electrode layer. Another electrode layer (upper electrode) may be formed on the piezoelectric film 3. In this case, the buffer layer 2 is a layer that orients the electrode layer in (002) and orients the crystal orientation of the piezoelectric film 3 made of LiNbO3 or LiTaO3 in the (012) plane direction. More preferably, by selecting a TiN film for the buffer layer 2 and a Pt film for the electrode layer (lower electrode), it is possible to orient the electrode layer in (002) and orient the crystal orientation of the piezoelectric film 3 made of LiNbO3 or LiTaO3 in the (012) plane direction. The thickness range of each layer and each film may be as described above. Such a piezoelectric device functions as an FBAR type filter. EXAMPLES
[0077] Examples of the present invention will now be described.
[0078] Example 1 After forming a titanium oxide film as an adhesive layer on the surface of a semiconductor substrate made of single crystal silicon, a lower electrode layer made of Pt was formed. The lower electrode layer was formed by DC sputtering using Pt as a target. The thickness of the lower electrode layer was set to 100 nm. The deposition conditions for the lower electrode layer were a substrate temperature of 500°C, deposition pressure of 0.38 Pa, Ar flow rate of 30 sccm, and DC sputtering power of 500 W.
[0079] Next, a buffer layer made of LaNiO3 was formed on the lower electrode layer. The buffer layer was formed by DC sputtering using LaNiO3 as a target. The thickness of the buffer layer was set to 100 nm. The deposition conditions for the buffer layer were a substrate temperature of 400°C, deposition pressure of 0.23 Pa, Ar flow rate of 8 sccm, oxygen flow rate of 12 sccm, and DC sputtering power of 500 W with pulse application at a frequency of 20 kHz.
[0080] Next, a piezoelectric film made of LiNbO3 was formed on the buffer layer. The piezoelectric film was formed by RF sputtering using LiNbO3 as a target. The thickness of the piezoelectric film was 200 nm. The deposition conditions for the piezoelectric film were a substrate temperature of 550°C, deposition pressure of 0.50 Pa, Ar flow rate of 100 sccm, oxygen flow rate of 1 sccm, and RF sputtering power of 100 W (frequency of 13.56 MHz).
[0081] Next, an upper electrode layer made of Pt was formed on the piezoelectric film. The upper electrode layer was formed by DC sputtering using Pt as a target. The thickness of the upper electrode layer was set to 100 nm. The deposition conditions of the upper electrode layer were the same as those of the lower electrode layer. In this way, the piezoelectric device of Example 1 was manufactured.
[0082] Example 2 A lower electrode layer made of Ag, which also served as a buffer layer, was formed on the surface of a semiconductor substrate made of single crystal silicon. The lower electrode layer was formed by DC sputtering using Ag as a target. The thickness of the lower electrode layer was set to 100 nm. The deposition conditions for the lower electrode layer were a substrate temperature of 400°C, deposition pressure of 0.25 Pa, Ar flow rate of 80 sccm, and DC sputtering power of 500 W. Before forming the buffer layer made of Ag, the natural oxide film on the surface of the semiconductor substrate made of single crystal silicon was removed with hydrofluoric acid.
[0083] Next, an oxidation prevention layer made of TiN was formed on the lower electrode layer made of Ag. The oxidation prevention layer was formed by DC sputtering using Ti as a target. The thickness of the oxidation prevention layer was set to 100 nm. The deposition conditions for the oxidation prevention layer were a substrate temperature of 400°C, deposition pressure of 0.1 Pa, N2 flow rate of 40 sccm, and DC sputtering power of 12,000 W.
[0084] Next, a piezoelectric film made of LiNbO3 was formed on the oxidation prevention layer. The piezoelectric film was formed by RF sputtering using LiNbO3 as a target. The thickness of the piezoelectric film was 200 nm. The deposition conditions for the piezoelectric film were a substrate temperature of 550°C, deposition pressure of 0.50 Pa, Ar flow rate of 100 sccm, oxygen flow rate of 1 sccm, and RF sputtering power of 100 W (frequency of 13.56 MHz).
[0085] Example 3 A buffer layer made of TiN was formed on the surface of a semiconductor substrate made of single crystal silicon. The buffer layer was formed by DC sputtering using Ti as a target. The thickness of the buffer layer was 100 nm. The deposition conditions for the buffer layer were a substrate temperature of 400°C, deposition pressure of 0.1 Pa, N2 flow rate of 40 sccm, and DC sputtering power of 12,000 W.
[0086] Next, a lower electrode layer made of Pt was formed on the buffer layer made of TiN. The lower electrode layer was formed by DC sputtering using Pt as a target. The thickness of the lower electrode layer was set to 100 nm. The deposition conditions for the lower electrode layer were a substrate temperature of 300°C, deposition pressure of 0.38 Pa, Ar flow rate of 30 sccm, and DC sputtering power of 500 W.
[0087] Next, a piezoelectric film made of LiNbO3 was formed on the lower electrode layer. The piezoelectric film was formed by RF sputtering using LiNbO3 as a target. The thickness of the piezoelectric film was 200 nm. The deposition conditions for the piezoelectric film were a substrate temperature of 550°C, deposition pressure of 0.50 Pa, Ar flow rate of 100 sccm, oxygen flow rate of 1 sccm, and RF sputtering power of 100 W (frequency of 13.56 MHz).
[0088] Comparative Example 1 A piezoelectric device of Comparative Example 1 was manufactured in the same manner as in Example 1 above, except that a piezoelectric film was formed on a lower electrode layer without forming a buffer layer.
[0089] For the piezoelectric devices of Examples 1 to 3 and Comparative Example 1, the crystal orientation (in-plane orientation) of the piezoelectric film was confirmed by X-ray diffraction measurement. In addition, the half-width of the X-ray diffraction peak of the (012) plane of the piezoelectric film was measured. The half-width was measured by X-ray diffraction rocking curve measurement. The results are shown in Table 1.
[0090] [Table 1]
[0091] As shown in Table 1, the piezoelectric films of Examples 1 to 3 had in-plane crystal orientation on their surfaces aligned in the (012) plane. The half-width of the piezoelectric films was 10° or less, and the crystallinity was excellent. Therefore, it was expected that the piezoelectric films would exhibit an excellent mechanical and electrical coupling coefficient.
[0092] On the other hand, in Comparative Example 1, a piezoelectric film was formed on a lower electrode layer without forming a buffer layer, so that the in-plane crystal orientation of the surface of the piezoelectric film was oriented in the (001) plane direction, and it was expected that the mechanical and electrical coupling coefficient would be lower than those of Examples 1 to 3. [Explanation of symbols]
[0093] 1...substrate, 2...buffer layer, 3...piezoelectric film, 4...anti-oxidation film, 33...lower electrode layer (lower electrode), 34...upper electrode layer (upper electrode).
Claims
1. LiNbO 3 or LiTaO 3 A method for forming a piezoelectric film comprising the steps of: A method for forming a piezoelectric film, comprising forming a lower electrode layer on a substrate, forming a buffer layer on the lower electrode layer that orients the crystal orientation of the piezoelectric film in the (012) plane direction and is made of any one of LaNiO3, SrRuO3, LaCoO3 or KNaNbO3 having a perovskite structure, and forming the piezoelectric film on the buffer layer by a sputtering method.
2. A method for forming a piezoelectric film made of LiNbO3 or LiTaO3, comprising the steps of: A method for forming a piezoelectric film, comprising the steps of: forming, on a substrate, Ag having a crystal orientation oriented in the (002) plane as a buffer layer that orients the crystal orientation of the piezoelectric film in the (012) plane and also serves as a lower electrode layer; and forming the piezoelectric film on the buffer layer by a sputtering method.
3. A method for forming a piezoelectric film made of LiNbO3 or LiTaO3, comprising the steps of: A method for forming a piezoelectric film, comprising: forming a TiN buffer layer on a substrate, the TiN buffer layer orienting the crystal orientation of the piezoelectric film in a (012) plane direction; forming a lower electrode layer on the buffer layer; and forming the piezoelectric film on the lower electrode layer by a sputtering method.
4. 2. The method for forming a piezoelectric film according to claim 1, wherein the buffer layer is made of LaNiO 3 .
5. 3. The method for forming a piezoelectric film according to claim 2, wherein the buffer layer is a film made of one of TiN, TiW, and TiWN laminated on an Ag film.
6. 6. The method for forming a piezoelectric film according to claim 1, wherein the sputtering method is a co-sputtering method using a first target made of niobium oxide or tantalum oxide and a second target made of lithium oxide.
7. A substrate; A lower electrode; a buffer layer disposed on the lower electrode; A LiNbO layer is disposed on the buffer layer and has a crystal orientation oriented in the (012) plane direction. 3 or LiTaO 3 A piezoelectric film comprising: an upper electrode disposed on the piezoelectric film; A piezoelectric device, wherein the buffer layer is any one of LaNiO3, SrRuO3, LaCoO3, and KNaNbO3 having a perovskite structure.
8. A substrate; a buffer layer disposed on the substrate and serving as a lower electrode; A LiNbO layer is disposed on the buffer layer and has a crystal orientation oriented in the (012) plane direction. 3 or LiTaO 3 A piezoelectric film comprising: an upper electrode disposed on the piezoelectric film; A piezoelectric device, wherein the buffer layer is made of Ag with a crystal orientation oriented in the (002) plane direction.
9. A substrate; a buffer layer disposed on the substrate; a lower electrode disposed on the buffer layer; A LiNbO film is disposed on the lower electrode and has a crystal orientation oriented in the (012) plane direction. 3 or LiTaO 3 A piezoelectric film comprising: an upper electrode disposed on the piezoelectric film; The buffer layer is TiN.
10. The piezoelectric device according to claim 7 , wherein the buffer layer is made of LaNiO 3 .
11. The piezoelectric device of claim 8, wherein a film of one of TiN, TiW, and TiWN is laminated on the buffer layer.
12. The piezoelectric device according to claim 7 , wherein the piezoelectric film has a thickness of 300 nm or less.
13. 13. The piezoelectric device according to claim 7, wherein a half-width of an X-ray diffraction peak of a (012) plane of the piezoelectric film is 10° or less when an X-ray diffraction rocking curve measurement is performed on the piezoelectric film.
14. 14. The piezoelectric device according to claim 7, which is an FBAR type filter or a SAW type filter.
Citation Information
Patent Citations
Surface acoustic wave device and manufacturing method therefor
JP2003101372A
Piezoelectric element, piezoelectric actuator, piezoelectric pump, inkjet recording head, inkjet printer, surface acoustic wave device, thin-film piezo-resonator, frequency filter, oscillator, electronic circuit, and electronic device
JP2006186258A
Piezoelectric laminate and device including the same
JP2007251387A
Method for producing piezoelectric layer
JP2007314378A
Bulk acoustic resonator and manufacturing method thereof
JP2019193168A