Anode current collector for all-solid-state battery and anode for all-solid-state battery including the same

The use of metal-carbon composite particles on the negative electrode current collector addresses the challenge of inefficient lithium deposition in all-solid-state batteries, resulting in improved electrochemical performance.

JP7575572B2Active Publication Date: 2024-10-29LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023511651
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-14
Filing Date
2021-09-14
Publication Date
2024-10-29
Estimated Expiration
2041-09-14

AI Technical Summary

Technical Problem

Existing negative electrode current collectors for all-solid-state batteries face challenges in achieving high lithium electrodeposition efficiency, as conventional methods fail to provide uniform deposition and high charge/discharge efficiency.

Method used

A negative electrode current collector coated with metal-carbon composite particles, where the composite particles are chemically or physically attached to a conductive metal foil, allowing for uniform lithium electrodeposition and formation of a stable lithium plating film.

Benefits of technology

The metal-carbon composite particles enable uniform lithium electrodeposition, enhancing the efficiency of lithium metal plating and improving the electrochemical properties of all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575572000005
    Figure 0007575572000005
  • Figure 0007575572000006
    Figure 0007575572000006
  • Figure 0007575572000007
    Figure 0007575572000007
Patent Text Reader

Abstract

The present invention relates to metal-carbon composite particles, which can uniformly introduce metal particles onto the surface of a current collector and induce uniform electrodeposition of lithium between a coating layer made of the metal-carbon composite particles and a conductive metal, thereby forming a uniform lithium metal plating film on the surface of the negative electrode current collector.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode current collector for an all-solid-state battery having high electrodeposition efficiency for lithium metal, and a negative electrode for an all-solid-state battery including the same.

[0002] This application claims priority to Korean Patent Application No. 10-2020-0117954, filed on September 14, 2020, and the entire contents disclosed in the specification and drawings of that application are incorporated herein by reference. [Background technology]

[0003] In order to solve the safety issues of secondary batteries that use liquid electrolytes, there is a need to develop all-solid-state batteries that use solid electrolytes.

[0004] Lithium is not only the lightest metal, but also has a low reduction potential (-3.04V vs. SHE) and a large theoretical capacity (3860mAh / g), so it is being researched as a next-generation anode material. In the case of lithium secondary batteries that use lithium metal as an electrode, a thin lithium electrode is required to maximize the efficiency and energy density of the battery, but the existing physical rolling method for manufacturing lithium foil has limitations in manufacturing lithium foil with a certain thickness. Meanwhile, when manufacturing an all-solid-state battery, the anode is manufactured to include only a current collector that does not include anode active material (layer), and when lithium ions are reduced during charging, lithium is electrodeposited on the surface of the anode current collector, forming a lithium metal plating film, which allows the battery to operate.

[0005] Typically, a negative electrode current collector uses a conductive metal such as copper, and attempts have been made to improve the efficiency of lithium electrodeposition by modifying the metal surface (coating, etc.). Such methods include coating with a lithiophilic metal such as silver (Ag) or a carbon material such as carbon black. Alternatively, a mixture containing silver and carbon has been tried as a material for the coating layer, but the resistance and charge / discharge efficiency were not high. Therefore, there is a need to develop a negative electrode current collector or an inactive material negative electrode for all-solid-state batteries with improved electrochemical properties. Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention aims to provide a negative electrode current collector having high lithium electrodeposition efficiency by coating a surface of the negative electrode current collector with metal-carbon composite particles, and a negative electrode for an all-solid-state battery including the negative electrode current collector.

[0007] Another object of the present invention is to provide a method for producing the metal-carbon composite particles.

[0008] The objects and advantages of the present invention can be realized by the means and combinations thereof recited in the claims. [Means for solving the problem]

[0009] A first aspect of the present invention relates to a negative electrode current collector for an all-solid-state battery, the negative electrode current collector comprising an electrically conductive metal foil and a coating layer comprising metal-carbon composite particles on a surface of the metal foil, the metal-carbon composite particles comprising metal particles and carbon particles, one or more metal particles and one or more carbon particles being mutually adhered to each other, the composite particles having a particle size of 20 μm or less, and a metal content of 50 parts by weight or less per 100 parts by weight of carbon in the composite particles.

[0010] In a second aspect of the present invention, in the first aspect, the metal particles include one or more selected from the group consisting of Ni, Cu, Ag, Au, Pt, Al, Zn, and Bi.

[0011] In a third aspect of the present invention, in the first or second aspect, the carbon particles include at least one selected from natural graphite, artificial graphite, hard carbon, soft carbon, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon nanotubes, fullerene, carbon fiber, and carbon fluoride.

[0012] A fourth aspect of the present invention relates to a negative electrode for an all-solid-state battery, the negative electrode including a negative electrode current collector having any one of the first surface to the third surface and not including a negative electrode active material, and lithium is electrodeposited on and desorbed from the surface of the metal foil of the negative electrode current collector during operation of the battery.

[0013] A fifth aspect of the present invention is the fourth aspect, wherein the electrodeposition of lithium is formed between the metal foil and a coating layer.

[0014] A sixth aspect of the present invention is any one of the first to fifth aspects, wherein the metal particles and the carbon particles are attached by a chemical method, a physical method, or a combination of both.

[0015] A seventh aspect of the present invention relates to an all-solid-state battery, the all-solid-state battery including an anode according to the fourth or fifth aspect.

[0016] An eighth aspect of the present invention relates to a method for producing composite particles, the method comprising the steps of preparing a reaction liquid containing a metal salt and a carbon material, and reacting the metal salt and the carbon material in the reaction liquid so as to grow metal particles on the surface of the carbon material.

[0017] In a ninth aspect of the present invention, in the eighth aspect, a concentration of solids including a metal salt and a carbon material excluding a solvent in the reaction liquid is 30 wt % or less.

[0018] A tenth aspect of the present invention is the method according to the eighth or ninth aspect, wherein the metal salt is at least one of a chloride, an iodide, a cyanide, a bromide, a sulfide, a hydroxide, a phosphide, and a chloride hydrate of a metal.

[0019] In an eleventh aspect of the present invention, in any one of the eighth to tenth aspects, the metal salt is a chloride of one or more metals selected from Ni, Cu, Ag, Au, Pt, Al, Zn, and Bi. Effect of the Invention

[0020] The metal-carbon composite particles according to the present invention allow metal particles to be uniformly introduced onto the surface of a current collector, thereby inducing uniform electrodeposition of lithium between a coating layer made of the metal-carbon composite particles and a conductive metal, thereby forming a uniform lithium metal plating film on the surface of the negative electrode current collector.

[0021] In addition, the method for producing metal-carbon composite particles can composite fine metal particles and a carbon material. As a result, when the composite particles obtained are introduced into an all-solid-state battery, the effect of uniformly electrodepositing lithium on the surface of a current collector is achieved as described above.

[0022] The following drawings attached to this specification are for illustrating preferred embodiments of the present invention, and serve to further understand the technical idea of ​​the present invention together with the detailed description of the invention, so the present invention should not be interpreted as being limited to only the matters described in the drawings. In addition, the shape, size, scale, ratio, etc. of the elements in the drawings attached to this specification may be exaggerated in order to emphasize a clearer description. [Brief description of the drawings]

[0023] [Figure 1] FIG. 2 is a schematic diagram showing how lithium is electrodeposited onto a negative electrode current collector according to one embodiment of the present invention to form a plating film. [Diagram 2] 1 is a SEM image of the composite particles obtained from Example 1. [Diagram 3] 1 is a SEM image of the composite particles obtained from Example 2. [Figure 4] 1 is a SEM image of the composite particles obtained from Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the attached drawings. Prior to this, the terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as being in accordance with the meaning and concept of the technical idea of ​​the present invention, in accordance with the principle that the inventor himself can appropriately define the concept of the term in order to best describe the invention. Therefore, it should be understood that the embodiment described in this specification and the configuration shown in the drawings are only one most preferred embodiment of the present invention, and do not represent the entire technical idea of ​​the present invention, and therefore there may be various equivalents and modifications that can be substituted for them at the time of this application.

[0025] In addition, throughout the specification, when a part "includes" a certain component, this does not mean excluding other components, but means that it may further include other components, unless specifically stated to the contrary.

[0026] The terms "about," "substantially," and the like, used throughout this specification, when given the meaning inherent in the manufacturing and material tolerances, are used to mean a numerical value or a approximation thereof, and are used to prevent unconscionable infringers from unfairly using disclosures in which precise or absolute numerical values ​​are recited to aid in the understanding of this application.

[0027] Throughout this specification, the phrase "A and / or B" means "A or B, or all of these."

[0028] The present invention relates to a negative electrode current collector and a negative electrode for an electrochemical device including the negative electrode current collector. The electrochemical device may be an all-solid-state battery using a solid electrolyte as an electrolyte material. The all-solid-state battery may be a lithium ion secondary battery.

[0029] In the present invention, the negative electrode current collector may include a metal foil and a coating layer including metal-carbon composite particles formed on at least one surface of the metal foil.

[0030] In the present invention, the negative electrode current collector may be applied to the manufacture of a battery in a state where an electrode active material is not applied thereto. That is, the negative electrode current collector serves as an inactive material negative electrode in an all-solid-state battery, and during charging of the battery, lithium may be electrodeposited on the surface of the metal foil to perform an electrochemical reaction. FIG. 1 is a schematic diagram of the reaction of lithium being electrodeposited on the surface of the negative electrode current collector and metal foil of the present invention. Referring to this figure, the negative electrode current collector has a metal foil and a coating layer formed on the surface of the metal foil. In the drawing, reference numeral 21 indicates a state where composite particles are gathered. As shown in the figure, the coating layer may have a form of a porous layer in which pores are formed, and during charging, lithium ions may pass through the coating layer to reach the surface of the metal foil, and these may be electrodeposited to form a lithium metal layer 22. In the present invention, the term "electrodeposition" may have the meaning of deposition.

[0031] The metal foil may have a thickness of 3 to 500 μm. The metal foil is not particularly limited as long as it is conductive and does not induce chemical changes in an electrochemical device to which the current collector according to the present invention is applied. For example, copper, gold, stainless steel, aluminum, nickel, titanium, aluminum-cadmium alloy, etc. may be used. In one embodiment of the present invention, the metal foil may have fine irregularities on the surface to strengthen the binding force with the coating layer or the lithium metal plating film electrodeposited on the metal foil. Meanwhile, in one embodiment of the present invention, the metal foil may have various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a nonwoven fabric, etc.

[0032] In the present invention, the coating layer may have a thickness of 5 to 50 μm, but is not particularly limited to this range. In one embodiment of the present invention, the metal-carbon composite particles in the coating layer may be contained in a range of 90% by weight or more with respect to 100% by weight of the coating layer. For example, the composite particles may be contained in a range of 95% by weight or more, or 97% by weight or more with respect to 100% by weight of the coating layer.

[0033] In one embodiment of the present invention, the metal-carbon composite particles have a form in which carbon particles and metal particles are attached to each other or one of the particles is coated on the surface of the other. In the present invention, the term "attached / coated" may mean that the carbon particles and the metal particles are physically and / or chemically bonded to each other.

[0034] 2 to 4 respectively show SEM images of the metal-carbon composite particles obtained in Examples 1 to 3. Referring to these, the metal-carbon composite particles have a state in which carbon particles and metal particles are adhered to each other.

[0035] In one embodiment of the present invention, the metal-carbon composite particles may have a size (diameter) of 20 μm or less based on the longest diameter of the particle. Within this range, the composite particles may have a particle size of 10 μm or less, 5 μm or less, or 1 μm or less. Meanwhile, the composite particles may include a plurality of the carbon particles. Also, the composite particles may include a plurality of the metal particles. In one embodiment of the present invention, the particle diameter may be measured using a laser diffraction method.

[0036] In one embodiment of the present invention, the carbon particles may include natural graphite, artificial graphite, hard carbon, soft carbon, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon nanotubes, fullerene, carbon fiber, and carbon fluoride.

[0037] In the present invention, the metal particles are lithiophilic metals, such as Ni, Cu, Ag, Au, Pt, Al, Zn, and Bi. The metal particles may be one or a combination of two or more of these. The incorporation of the lithiophilic metals is advantageous for the stable and uniform formation of a lithium layer on the surface of the current collector.

[0038] Meanwhile, in one embodiment of the present invention, the metal content in the metal-carbon composite particles may be in the range of 1 to 50 parts by weight based on 100 parts by weight of the carbon material.

[0039] FIG. 1 attached below shows an anode current collector according to the present invention and a mechanism by which lithium is electrodeposited on the anode current collector to form a lithium metal plating film. Referring to this figure, a coating layer of a predetermined thickness is formed on the surface of a metal foil, and the coating layer includes metal-carbon composite particles having the structural characteristics described above. In one embodiment of the present invention, the coating layer has a layered structure formed integrally by filling the composite particles, and has a porous structure having pores due to interstitial volumes between the composite particles. The pores can be provided as a passage for lithium ions during charging and discharging of the battery. Thus, the anode current collector is provided in a state free of an electrode active material for battery manufacture, and during the first charge in the activation process of the battery, lithium ions provided from the positive electrode pass through the coating layer and are electrodeposited on the surface of the metal foil to form a plating film. Thus, the anode that has undergone the activation process can include electrodeposited lithium (Li-plating). The lithium plated on the negative electrode can continuously deposit and release lithium ions during the charging and discharging process of the lithium secondary battery, thereby contributing to the reversible capacity of the negative electrode.

[0040] In one embodiment of the present invention, the metal-carbon composite particles can be produced by the following method.

[0041] First, a reaction liquid is prepared by dispersing a metal salt and a carbon material in a solvent. Examples of the solvent include organic solvents such as NMP (N-methylpyrrolidone), DMF (dimethylformamide), acetone, and dimethylacetamide, alcohols having 3 or less carbon atoms, and water. These solvents may be used alone or in combination. However, the solvent is not limited to the above components, and is not particularly limited as long as it does not affect the physical and / or chemical properties of the components to be added, such as the metal salt and the carbon material. In a specific embodiment of the present invention, the metal salt may be prepared in a solution state (first solution) dissolved in water or alcohol. Also, the carbon material may be prepared by dispersing it in an organic solvent (second solution). The first and second solutions thus prepared may be mixed to provide a reaction liquid. In one embodiment of the present invention, the concentration of solids excluding the solvent in the reaction liquid may be adjusted to a range of 30 wt% or less, 20 wt% or less, 10 wt% or less, 5 wt% or less, or 3 wt% or less. Meanwhile, the amount of metal salt and solid content in the reaction solution can be adjusted to an appropriate range in consideration of the size of the composite particles to be finally obtained and the content of metal particles in the composite particles.

[0042] The metal salt is in the form of a salt of a metal to be introduced into the composite particles, and examples of the metal salt include chloride, iodide, cyanide, bromide, sulfide, hydroxide, phosphide, and chloride hydrate of the metal, and may include one or more of these. The metal is a lithium affinity metal as described above, and in a specific embodiment of the present invention, the metal may be silver (Ag). As a specific example, the metal salt may be AgCN, which is a cyanide form of silver (Ag).

[0043] The dispersion method is not limited to a specific method, and a known mixing device such as a paste mixer may be used.

[0044] Next, the reaction solution is maintained at about 25° C. or heated to a temperature higher than this to induce the growth of metal particles on the surface of the carbon material. The metal particles grow on the surface of the carbon material in a manner that the metal is introduced to the surface of the carbon material by the reduction of the metal ions, and then the metal ions are repeatedly reduced using the metal ions as seeds. In one embodiment of the present invention, when silver (Ag) is introduced to the surface of the carbon particles, AgCN diluted in ethanol may be used. The method for producing metal-carbon composite particles according to the present invention has an advantage that the size of the metal particles can be very finely controlled. The size of the metal particles can be controlled by adjusting the amount of metal salt to be added or by adjusting the amount of solvent when mixing the carbon material and the metal salt to adjust the reaction rate. Next, when the metal particles grow to a predetermined size, the reaction is terminated and the solution is removed by filtration to obtain metal-carbon composite particles. The particles can be washed with water to remove excess carbon material if necessary. The metal-carbon composite particles can also be finally obtained by filtering, washing, and drying.

[0045] As described above, when the metal-carbon composite particles are obtained, they can be coated on a metal foil used as a current collector, such as nickel, copper, or aluminum, to manufacture a negative electrode current collector. The method for manufacturing the negative electrode current collector is not limited to a specific method as long as it is a method capable of forming a coating layer of a predetermined thickness containing the metal-carbon composite particles on the surface of the metal foil. In a specific embodiment of the present invention, the method for manufacturing the current collector can be exemplified as follows. First, a binder resin is added to a suitable organic solvent such as acetone or NMP to prepare a binder solution, and the composite particles are added and mixed therein to prepare a slurry for forming a coating layer. The slurry is then applied to the metal foil and dried to manufacture a negative electrode current collector. The binder resin can be, but is not limited to, a fluorine-based binder such as PVDF, PVDF-HFP, PVDF-TFE, or PVDF-TrFE, or an acrylic binder. The binder solution can have a solid content excluding the organic solvent in a range of 3 to 10 wt%. Meanwhile, in the slurry for forming the coating layer, the weight ratio of the composite particles to the binder resin may be adjusted to a range of 90: 10 to 99: 1. The coating may be performed by selecting at least one appropriate method from among known methods such as doctor blade, dip coating, gravure coating, and slot coating.

[0046] Meanwhile, a secondary battery including an anode including the anode current collector of the present invention, a solid electrolyte membrane, and a cathode may be provided. In one embodiment of the present invention, the anode may include only the anode current collector according to the present invention without a separate anode active material layer when provided during the manufacture of the secondary battery. In addition, the anode may have a lithium metal plating film formed by electrodeposition of lithium ions after the first charge / discharge, and the plating film may serve as the anode active material layer.

[0047] In the present invention, the solid electrolyte membrane is provided between the negative electrode and the positive electrode in the all-solid-state battery, and serves to electrically insulate the negative electrode from the positive electrode and to serve as an ion transfer path between the negative electrode and the positive electrode. Each of the solid electrolyte membranes may be provided in the form of a sheet containing a solid electrolyte material. If necessary, the solid electrolyte membrane may further contain a binder resin for the shape maintenance stability of the membrane.

[0048] The solid electrolyte material may include at least one selected from a sulfide-based solid electrolyte material, an oxide-based solid electrolyte material, and a polymer-based solid electrolyte material.

[0049] In the present invention, the method for producing the solid electrolyte membrane is not limited to a specific method as long as the solid electrolyte membrane is provided in the form of a sheet containing a solid electrolyte material. For example, the solid electrolyte membrane may be prepared by a method in which a solid electrolyte material is put into a solvent to prepare a slurry for producing the electrolyte membrane, and the slurry is then applied to a release film and dried. The release film is removed from the solid electrolyte membrane before laminating the positive electrode and the solid electrolyte membrane in a step described below.

[0050] The positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on a surface of the positive electrode current collector. The active material layer may include a plurality of electrode active material particles and a solid electrolyte material. In one embodiment of the present invention, the positive electrode may further include at least one of a conductive material and a binder resin, if necessary. In addition, various additives may be further included for the purpose of complementing or improving the electrochemical characteristics of the positive electrode. In the present invention, the method of manufacturing the positive electrode is not particularly limited as long as it can be provided in a sheet shape including the positive electrode active material and the solid electrolyte. For example, the positive electrode may be prepared by a method in which the positive electrode active material and the solid electrolyte material are put into a solvent to prepare a slurry for manufacturing the positive electrode, and then the slurry is applied to a current collector and dried.

[0051] The positive electrode active material is not limited to a specific component as long as it can be used as a positive electrode active material for lithium ion secondary batteries. Non-limiting examples include layered compounds such as lithium manganese complex oxides (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), and lithium nickel oxide (LiNiO2), as well as compounds substituted with one or more transition metals; 1+x Mn 2-x Lithium manganese oxides such as LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, and Cu2V2O7; and the chemical formula LiNi 1-x M x Lithium nickel oxide with Ni site represented by the chemical formula LiMnO2 (where M=Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x=0.01 to 0.3); 2-x M x The positive electrode may contain one or a mixture of two or more of the following solid electrolyte materials: a lithium manganese composite oxide represented by LiMn2O2 (wherein M=Co, Ni, Fe, Cr, Zn, or Ta, and x=0.01 to 0.1) or Li2Mn3MO8 (wherein M=Fe, Co, Ni, Cu, or Zn); LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion; a disulfide compound; and Fe2(MoO4)3. In the present invention, the positive electrode may contain one or more of a polymer-based solid electrolyte, an oxide-based solid electrolyte, and a sulfide-based solid electrolyte as a solid electrolyte material.

[0052] In one embodiment of the present invention, the all-solid-state battery may be manufactured by sequentially stacking a positive electrode, a solid electrolyte membrane, and a negative electrode, and applying pressure to bring the layers into close contact with each other.

[0053] In the present invention, the pressing process may be any method that can ensure bonding between the electrode and the solid electrolyte membrane and appropriate porosity. In a specific embodiment of the present invention, the pressing may be appropriately selected from known pressing methods such as roll pressing, compression pressing, and cold isostatic pressing (CIP), and is not limited to any one of these methods.

[0054] In the present invention, the conductive material is usually added in an amount of 1 to 30 wt% based on the total weight of the mixture containing the electrode active material in the electrode active material layer. Such a conductive material is not particularly limited as long as it has conductivity without inducing a chemical change in the battery. For example, the conductive material may include one or a mixture of two or more conductive materials selected from graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives.

[0055] In the present invention, the binder resin is not particularly limited as long as it is a component that helps the active material and conductive material to be bonded and to the current collector. For example, polyvinylidene fluoride polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene butadiene rubber, fluororubber, various copolymers, etc. The binder resin may be usually contained in a range of 1 to 30 wt% or 1 to 10 wt% relative to 100 wt% of the electrode layer.

[0056] Meanwhile, in the present invention, each electrode active material layer may contain one or more additives such as an oxidation stabilizing additive, a reduction stabilizing additive, a flame retardant, a heat stabilizer, an antifogging agent, etc., as necessary.

[0057] In the present invention, the sulfide-based solid electrolyte material contains sulfur (S) and has the ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and may include Li-PS-based glass or Li-PS-based glass ceramic. Non-limiting examples of such sulfide-based solid electrolytes include Li2S-P2S5, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, Li2S-GeS2-ZnS, and may include one or more of these. However, the present invention is not particularly limited to these.

[0058] The oxide-based solid electrolyte material contains oxygen (O) and has the ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table. Non-limiting examples of this include LLTO-based compounds, Li6La2CaTa2O 12 , Li6La2ANb2O 12 (A is Ca or Sr), Li2Nd3TeSbO 12 , LiBO 2.5 N 0.5 , Li9SiAlO8, LAGP compounds, LATP compounds, Li 1+x Ti 2-x Al x Siy(PO4) 3-y (where 0≦x≦1, 0≦y≦1), LiAl x Zr 2-x (PO4)3 (where 0≦x≦1, 0≦y≦1), LiTi x Zr 2-x(PO4)3 (where 0≦x≦1, 0≦y≦1), LISICON-based compounds, LIPON-based compounds, Perovskite-based compounds, Nasicon-based compounds, and LLZO-based compounds may be included, but are not limited thereto.

[0059] In the solid electrolyte material, in the case of the positive electrode, an electrolyte material having excellent oxidation stability may be used as the solid electrolyte. In the case of the negative electrode, an electrolyte material having excellent reduction stability may be used as the solid electrolyte. However, the present invention is not limited thereto, and since the electrode mainly plays a role of transferring lithium ions, a material having high ion conductivity, for example, 10 -7 s / cm or more, or 10 -5 Any material having a viscosity of s / cm or higher can be used, and there is no limitation to a specific component.

[0060] The present invention also provides a battery module including the secondary battery as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source, where specific examples of the device include, but are not limited to, a power tool powered by an electric motor, electric vehicles including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), and the like, electric two-wheeled vehicles including electric bicycles (E-bikes) and electric scooters (E-scooters), electric golf carts, and power storage systems.

[0061] The present invention will be described in more detail below with reference to examples. However, the following examples are merely illustrative of the present invention and are not intended to limit the scope of the present invention.

[0062] 1. Example (1) Manufacturing of metal-carbon composite particles Example 1 A reaction solution was prepared by mixing AgCN dissolved in ethanol and a carbon material (Super C65) dispersed in NMP. The solid concentration in the reaction solution was 21 wt%, and the amount of Ag was 33 parts by weight per 100 parts by weight of the carbon material. The reaction solution was left at room temperature for a predetermined time to allow silver particles to grow on the surface of the carbon material particles. After the reaction was completed, the reaction solution was filtered to obtain a composite particle powder. When the entire amount of AgCN added in the reaction participated in the reaction and no further particle growth occurred, the reaction was terminated. FIG. 2 is an SEM image of the composite particles obtained in Example 1. It was confirmed that rod-shaped silver particles and carbon particles were attached to each other to form composite particles.

[0063] Example 2 A reaction solution was prepared by mixing AgCN dissolved in ethanol and a carbon material (Super C65) dispersed in NMP. The solid concentration in the reaction solution was 1.1 wt%, and the weight ratio of Ag was 33% relative to 100 parts by weight of the carbon material. The reaction solution was left at room temperature for a predetermined time to allow silver particles to grow on the surface of the carbon material particles. After the reaction was completed, the reaction solution was filtered to obtain a composite particle powder. When all of the AgCN added in the reaction participated in the reaction and no further particle growth occurred, the reaction was terminated. FIG. 3 is an SEM image of the composite particles obtained in Example 2. It was confirmed that the silver particles and the carbon material particles were attached to each other to form composite particles.

[0064] Example 3 A reaction solution was prepared by mixing AgCN dissolved in ethanol and a carbon material (Super C65) dispersed in NMP. The solid concentration in the reaction solution was 1.0 wt%, and the weight ratio of Ag was 11% relative to 100 parts by weight of the carbon material. The reaction solution was left at room temperature for a predetermined time to allow silver particles to grow on the surface of the carbon material particles. After the reaction was completed, the reaction solution was filtered to obtain a composite particle powder. When all of the AgCN added in the reaction participated in the reaction and no further particle growth occurred, the reaction was terminated. FIG. 4 is an SEM image of the composite particles obtained in Example 3. It was confirmed that the silver particles and the carbon material particles were attached to each other to form composite particles.

[0065] The content ratios during the production of the composite particles obtained in each of the above production examples are shown in Table 1 below.

[0066] [Table 1]

[0067] (2) Manufacturing of current collectors 1) Examples 1 to 3 A binder solution was prepared by adding PVDF, which is a binder resin, to NMP. The binder solution had a binder resin concentration of about 6 wt%. The composite particles obtained from each of Examples 1 to 3 were added to NMP to obtain a dispersion. The binder solution and the dispersion were mixed using a paste mixer to prepare a slurry for forming a coating layer. The prepared slurry for forming a coating layer was then applied to a nickel thin film with a gap of 100 μm using a doctor blade and dried, finally obtaining a negative electrode current collector having a coating layer with a thickness of 10 μm. The content ratio of each component during the preparation of the coating layer in each of the above examples is shown in Table 2 below.

[0068] [Table 2]

[0069] 2. Comparative Example 1 and Comparative Example 2 A binder solution was prepared by adding PVDF, a binder resin, to NMP. The binder solution had a binder resin concentration of about 6 wt%. Meanwhile, Super C65 and Ag powder (particle size about 50 nm) were added to NMP to obtain a dispersion. The binder solution and the dispersion were mixed using a paste mixer to prepare a slurry for forming a coating layer. The prepared slurry for forming a coating layer was then applied to a nickel thin film with a doctor blade at a gap of 100 μm and dried, finally obtaining a negative electrode current collector having a coating layer with a thickness of 10 μm. The content ratio of each component during the preparation of the coating layer in each of the above examples is shown in Table 3 below.

[0070] [Table 3]

[0071] 3. Comparative Example 3 Ketjen Black (Lion Specialty Chemicals, D50=34nm) and Li2S-P2S5 (D50=0.5μm) were mixed in a weight ratio of 2:1, then heptane was added and the resultant mixture was mixed for 3 minutes using a homogenizer (SMT Corporation, UH-50) to obtain a slurry for forming a coating layer. The slurry for forming the coating layer was then applied to a nickel thin film with a doctor blade at a gap of 100μm and dried, finally obtaining a negative electrode current collector with a coating layer of 10μm thickness.

[0072] 4. Battery manufacturing Cathode active material LiNi 0.8 Co 0.1 Mn 0.1O2, solid electrolyte Li2S-P2S5, binder (NBR), and conductive material (VGCF) were mixed in anisole in a weight ratio of 75.5:22.1:1.5:1 to prepare a slurry (solid content 70wt%) for forming a positive electrode active material layer. This was applied to one side of an aluminum thin film (approximately 10μm thick) and dried at 60℃ for 6 hours to prepare a positive electrode.

[0073] A solid electrolyte Li2S-P2S5 and a binder (NBR) were added to anisole in a weight ratio of 95:5 to prepare a slurry (solid content 60wt%) for forming a solid electrolyte membrane. The slurry was mixed in a Thinky mixer at a speed of 2,000 rpm for 1 minute. This was applied to one side of a release sheet made of polyethylene terephthalate material, dried overnight under room temperature and pressure conditions, and the release sheet was removed to prepare a solid electrolyte membrane. The thickness of the solid electrolyte membrane was 50μm.

[0074] Thereafter, the positive electrode / solid electrolyte membrane / negative electrode current collector (Examples 1 to 3 and Comparative Examples 1 to 3) were laminated in this order and pressurized at a pressure of 500 MPa for 5 minutes to manufacture a secondary battery.

[0075] 5. Comparison of electrochemical properties All-solid-state batteries were manufactured using the electrode assemblies obtained in Examples 1 to 3 and Comparative Examples 1 to 3, and the charge capacity, discharge capacity, and initial efficiency after the first charge and discharge were measured. The charge and discharge were performed in CC-CV mode at 0.05C up to 4.25V (0.01C cut off), and discharged at 0.05C up to 3V. The charge and discharge were performed under the condition of 65°C. In addition, AC impedance was measured under the condition of an amplitude of 10mV and a scan range of 500kHz to 20MHz using an EIS analyzer (VMP3, Bio-logic science instruments). The results are shown in Table 4 below. When Example 1 and Comparative Example 1, which have the same silver content, are compared, it was confirmed that the battery including the negative electrode current collector according to the present invention has excellent electrochemical properties. In addition, in the case of Example 3 and Comparative Example 2, which have the same silver content, it was confirmed that the battery according to the Example has excellent electrochemical properties such as charge and discharge efficiency. On the other hand, it was confirmed that Comparative Example 3 has a much lower initial efficiency.

[0076] [Table 4] [Explanation of symbols]

[0077] 1 Lithium-ion 3 Metal foil 4 Inside the battery (filled with electrolyte, etc.) 21 A state in which composite particles are gathered 22 Lithium metal layer

Claims

1. A negative electrode for an all-solid-state battery comprising a negative electrode current collector, The negative electrode current collector includes an electrically conductive metal foil and a coating layer including metal-carbon composite particles on a surface of the metal foil, The metal-carbon composite particles include metal particles and carbon particles, and one or more metal particles and one or more carbon particles are attached to each other. The composite particles have a particle size of 20 μm or less, and the composite particles have a metal content of 50 parts by weight or less per 100 parts by weight of carbon. The negative electrode does not contain a negative electrode active material, The negative electrode current collector is a negative electrode for an all-solid-state battery, in which lithium is electrodeposited on and desorbed from the surface of the metal foil during operation of the battery.

2. 2. The negative electrode for an all-solid-state battery according to claim 1, wherein the metal particles contain at least one selected from the group consisting of Ni, Cu, Ag, Au, Pt, Al, Zn, and Bi.

3. 3. The negative electrode for an all-solid-state battery according to claim 1 or 2, wherein the carbon particles include at least one selected from the group consisting of natural graphite, artificial graphite, hard carbon, soft carbon, carbon black, acetylene black, channel black, furnace black, lamp black, thermal black, carbon nanotubes, fullerene, carbon fiber, and carbon fluoride.

4. The negative electrode for an all-solid-state battery according to claim 1 , wherein the electrodeposition of lithium is formed between the metal foil and a coating layer.

5. The negative electrode for an all-solid-state battery according to claim 1 , wherein the metal particles and the carbon particles are attached by a chemical method, a physical method, or a combination of both methods.

6. An all-solid-state battery comprising the negative electrode according to claim 1 .

7. A method for making composite particles for use in a negative electrode for an all-solid-state battery, comprising the steps of: A method for producing composite particles, comprising the steps of preparing a reaction solution containing a metal salt and a carbon material, and reacting the metal salt and the carbon material in the reaction solution so that metal particles grow on the surface of the carbon material.

8. 8. The method for producing composite particles according to claim 7, wherein a concentration of solids including the metal salt and the carbon material excluding the solvent in the reaction liquid is 30 wt% or less.

9. 9. The method for producing composite particles according to claim 7 or 8, wherein the metal salt is at least one of a chloride, an iodide, a cyanide, a bromide, a sulfide, a hydroxide, a phosphide, and a chlorohydrate of a metal.

10. The method for producing composite particles according to any one of claims 7 to 9, wherein the metal salt is a chloride of one or more metals selected from Ni, Cu, Ag, Au, Pt, Al, Zn, and Bi.

Citation Information

Patent Citations

  • Solid electrolytic capacitor and method of manufacturing cathode material therefor

    JP2006269570A

  • Negative electrode for secondary battery, and secondary battery

    JP2013033685A

  • Composite of carbon black and metal

    JP2013216971A

  • Carbon nanomaterial coating method

    JP2016526092A

  • All-solid battery and negative electrode

    JP2019036391A