(Meth)acrylic block copolymer, (meth)acrylic block copolymer latex, (meth)acrylic block copolymer latex composition, and molded article
A (meth)acrylic block copolymer with defined polymer blocks (A) and (B) addresses the challenge of producing low modulus, high tensile strength molded articles without vulcanizing agents, enhancing flexibility and heat resistance while reducing allergens and costs.
Patent Information
- Application Number
- JP2023509075
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-23
- Filing Date
- 2022-03-16
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2042-03-16
AI Technical Summary
Conventional (meth)acrylic block copolymers fail to produce molded articles with low modulus and high tensile strength without the use of vulcanizing agents and vulcanization accelerators, which are known to cause allergies and increase costs.
A (meth)acrylic block copolymer comprising specific polymer blocks (A) and (B) with defined glass transition temperatures and molecular weights, allowing for the production of dip-molded films with excellent flexibility, tensile properties, and heat aging resistance, even when vulcanizing agents and accelerators are reduced or omitted.
The solution achieves molded articles with improved mechanical strength and flexibility, reducing the need for vulcanizing agents and accelerators, thereby minimizing allergies and costs.
Smart Images

Figure 0007576157000001 
Figure 0007576157000002 
Figure 0007576157000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a (meth)acrylic block copolymer, a (meth)acrylic block copolymer latex, a (meth)acrylic block copolymer latex composition, and a molded article. [Background technology]
[0002] Natural rubber (NR), isoprene rubber (IR), and CR gloves are widely used as surgical gloves. NR and IR gloves have low modulus and excellent texture, but NR gloves have type I allergy caused by latex proteins, and IR gloves have type IV allergy caused by vulcanization accelerator di-o-tolylguanidine (DOTG), etc., which are issues, and allergy-free alternative materials are desired. CR gloves do not contain latex proteins or DOTG, but they have issues with the modulus increasing and the texture deteriorating after product storage due to the influence of vulcanization accelerator zinc dibutyldithiocarbamate (ZDBC) that remains unreacted during vulcanization. In addition, in order to obtain the desired mechanical strength of the chloroprene rubber composition, it is essential to use vulcanizing agents such as sulfur, zinc oxide, magnesium oxide, and vulcanization accelerators such as thiuram, dithiocarbamate, thiourea, guanidine, xanthogenate, and thiazole. Since vulcanization accelerators are causative substances of type IV allergies that cause skin diseases such as dermatitis, reducing or eliminating the use of vulcanization accelerators has become an important theme. In addition, since eliminating the use of vulcanization accelerators leads not only to a reduction in allergies but also to cost reduction, a rubber composition that exhibits sufficient mechanical strength without using vulcanization accelerators is desired.
[0003] As a technique relating to a (meth)acrylic block copolymer, Patent Document 1 discloses an invention relating to a star-shaped copolymer based on an aromatic vinyl and / or methacryl block and an acrylic block. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 5-500827 Summary of the Invention [Problem to be solved by the invention]
[0005] As described above, there has been a demand for a latex which is allergy-free and capable of obtaining a molded article having low modulus and high tensile strength with reduced amounts of a vulcanizing agent and a vulcanization accelerator or without the use of the vulcanizing agent and the vulcanization accelerator, but the conventional latex containing a (meth)acrylic block copolymer cannot provide a molded article having low modulus and high tensile strength without the use of a vulcanizing agent and a vulcanization accelerator.
[0006] Therefore, an object of the present invention is to provide a (meth)acrylic block copolymer, a (meth)acrylic block copolymer latex, and a (meth)acrylic block copolymer latex composition which can provide a dip-molded coating excellent in flexibility, tensile properties, and heat aging resistance even when the amounts of a vulcanizing agent and a vulcanization accelerator used are reduced or even when they are not used, and to provide a molded article excellent in flexibility, tensile properties, and heat aging resistance even when the amounts of a vulcanizing agent and a vulcanization accelerator used are reduced or even when they are not used. [Means for solving the problem]
[0007] According to the present invention, there is provided a (meth)acrylic block copolymer comprising a polymer block (A) and a (meth)acrylic polymer block (B), the (meth)acrylic block copolymer comprising 5 to 30 mass % of the polymer block (A) and 70 to 95 mass % of the (meth)acrylic polymer block (B), when the (meth)acrylic block copolymer is taken as 100 mass %, the polymer block (A) comprises a monomer unit derived from a monomer which gives a polymer having a glass transition temperature of 80° C. or higher upon homopolymerization, and the (meth)acrylic block copolymer has a tensile strength at break of 14 MPa or more as measured in accordance with JIS K 6251 after a coating obtained by dip-molding a (meth)acrylic block copolymer latex comprising the (meth)acrylic block copolymer is heat-treated at 130° C. for 30 minutes.
[0008] The present inventors have conducted intensive studies and have found that, in a (meth)acrylic block copolymer containing a polymer block (A) and a (meth)acrylic polymer block (B), by specifying the type of polymer block (A) and the blending amounts of polymer block (A) and polymer block (B) and adjusting the (meth)acrylic block copolymer so that the strength of a coating obtained by dip molding a (meth)acrylic block copolymer latex containing the (meth)acrylic block copolymer is at least a certain level, it is possible to obtain a (meth)acrylic block copolymer that can provide a dip-molded coating having excellent flexibility, tensile properties, and heat aging resistance even with reduced amounts of vulcanizing agents and vulcanization accelerators or without using them, which was difficult with conventional (meth)acrylic block copolymers, and have thus completed the present invention.
[0009] Preferably, the polymer block (A) is a (meth)acrylic block copolymer containing at least one monomer unit selected from the group consisting of an aromatic vinyl monomer unit, a methyl methacrylate monomer unit, and an acrylonitrile monomer unit. Preferably, in the above-described (meth)acrylic block copolymer, the polymer block (A) has a number average molecular weight of 10,000 or more. Preferably, the polymer block (B) is the above-described (meth)acrylic block copolymer having a (meth)acrylic monomer unit and a polyfunctional monomer unit. Preferably, the (meth)acrylic polymer block (B) is the (meth)acrylic block copolymer described above, which contains 0.05 to 10 mass % of the polyfunctional monomer unit when the (meth)acrylic polymer block (B) is taken as 100 mass %. Preferably, the polyfunctional monomer is the above-mentioned (meth)acrylic block copolymer containing the monomer represented by chemical formula (1) and an aromatic polyene monomer.
[0010] [ka] (In chemical formula (1), R1 and R2 each independently represent hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, a mercapto group, or a substituted or unsubstituted heterocyclyl group. W1 represents a saturated or unsaturated hydrocarbon group, a saturated or unsaturated cyclic hydrocarbon group, or a saturated or unsaturated hydrocarbon group or cyclic hydrocarbon group containing a hetero atom. Z1 represents oxygen, sulfur, or a structure represented by -NR0-. R0 represents hydrogen, chlorine, a substituted or unsubstituted alkyl group, an alkenyl group, an aryl group, a mercapto group, or a heterocyclyl group.)
[0011] According to another aspect of the present invention, there is provided a (meth)acrylic block copolymer latex comprising the above-described (meth)acrylic block copolymer. Preferably, the (meth)acrylic block copolymer latex contains 20 to 100% by mass of a toluene-insoluble matter relative to 100% by mass of the (meth)acrylic block copolymer latex. Preferably, the (meth)acrylic block copolymer latex has an average particle size of 300 nm or less as measured by dynamic light scattering. Preferably, the (meth)acrylic block copolymer latex is the above-mentioned (meth)acrylic block copolymer latex for use in a dip-molded article.
[0012] According to another aspect of the present invention, there is provided a (meth)acrylic block copolymer latex composition comprising the above-described (meth)acrylic block copolymer latex. Preferably, the (meth)acrylic block copolymer latex composition is the above-described (meth)acrylic block copolymer latex composition, in which, when the (meth)acrylic block copolymer latex contained in the (meth)acrylic block copolymer latex composition is taken as 100 mass%, the total content of the vulcanizing agent and the vulcanization accelerator is 5 mass% or less. According to another aspect of the present invention, there is provided a molded article comprising the above-described (meth)acrylic block copolymer latex composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below by illustrating the embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. In addition, each feature can be an invention independently. In this specification and claims, the expression "A to B" means A or more and B or less.
[0014] 1. (Meth)acrylic block copolymer The (meth)acrylic block copolymer according to the present invention is a block copolymer containing a polymer block (A) derived from a monomer that, upon homopolymerization, gives a polymer having a glass transition temperature of 80° C. or higher, and a (meth)acrylic polymer block (B) containing a (meth)acrylic monomer. The (meth)acrylic block copolymer also includes those having a structure in which block copolymers are chemically bonded to each other.
[0015] 1.1 Polymer block (A) The polymer block (A) is a polymer block derived from a monomer that can give a polymer having a glass transition temperature of 80° C. or more when homopolymerized. By using such a monomer, the tensile strength at break of the obtained (meth)acrylic block copolymer is improved. It is preferable to use a monomer that can give a polymer having a glass transition temperature of 85° C. or more. From the viewpoint of moldability, a monomer that can give a polymer having a glass transition temperature of 150° C. or less is preferable, and a monomer that can give a polymer having a glass transition temperature of 120° C. or less is particularly preferable. The glass transition temperature is, for example, 80, 85, 90, 95, 100, 105, 110, 120, 130, 140, or 150° C., and may be within a range between any two of the values exemplified here. In this specification, the glass transition temperature is the extrapolated glass transition end temperature (T eg) measured in accordance with JIS K 7121. When the polymer block (A) is a polymer block obtained by polymerizing a monomer (A), the monomer (A) is preferably a monomer that, when the monomer A is homopolymerized to give a homopolymer (A) having a number average molecular weight of 10,000 to 30,000, has the above-mentioned glass transition temperature.
[0016] Examples of monomer units constituting the polymer block (A) include aromatic vinyl monomer units, methyl methacrylate monomer units, and acrylonitrile monomer units. Preferably, units derived from aromatic vinyl monomers are used, and styrene units are preferably used. The polymer block (A) may be a polymer block obtained by copolymerization of these monomers, or a polymer block composed of monomer units copolymerizable with these monomers, within the scope of the present invention.
[0017] The number average molecular weight of the polymer block (A) is preferably 10,000 or more from the viewpoint of the tensile properties and moldability of the obtained (meth)acrylic block copolymer. The number average molecular weight of the polymer block (A) can be, for example, 10000, 15000, 20000, 25000, or 30000, and may be within a range between any two of the numerical values exemplified here. In addition, the molecular weight distribution of the polymer block (A) is preferably 2.0 or less from the viewpoint of moldability. The molecular weight distribution of the polymer block (A) can be, for example, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2.0, and may be within a range between any two of the numerical values exemplified here. In this specification, the number average molecular weight and the weight average molecular weight are values calculated in terms of polystyrene measured by gel permeation chromatography (GPC) under the measurement conditions described below. Device name: HLC-8320 (Tosoh Corporation) Column: 3 TSKgel GMHHR-H in series Temperature: 40℃ Detection: Differential refractive index Solvent: Tetrahydrofuran Calibration curve: Prepared using standard polystyrene (PS).
[0018] 1.2 (Meth)acrylic polymer block (B) The (meth)acrylic polymer block (B) contains (meth)acrylic monomer units and is mainly composed of (meth)acrylic monomers. The (meth)acrylic polymer block (B) may contain polyfunctional monomer units. Furthermore, within the scope of the present invention, the (meth)acrylic polymer block (B) may be a polymer block containing (meth)acrylic monomer units, polyfunctional monomer units, and units derived from monomers copolymerizable therewith. When the (meth)acrylic polymer block (B) is taken as 100% by mass, the (meth)acrylic polymer block (B) preferably contains 90% by mass or more of structural units derived from (meth)acrylic monomers.
[0019] The content of each structural unit in the (meth)acrylic polymer block (B) is not particularly limited, but is preferably 90 to 99.95 mass% of the (meth)acrylic monomer unit and 0.05 to 10 mass% of the polyfunctional monomer unit. The content of the polyfunctional monomer unit in the (meth)acrylic polymer block (B) is, for example, 0.05, 0.50, 1.00, 2.00, 3.00, 4.00, 5.00, 6.00, 7.00, 8.00, 9.00, or 10.00 mass%, and may be within a range between any two of the numerical values exemplified here.
[0020] 1.2.1 (Meth)acrylic monomers Examples of the (meth)acrylic monomer according to one embodiment of the present invention include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, normal propyl acrylate, normal propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, normal butyl acrylate, normal butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, secondary butyl acrylate, secondary butyl methacrylate, tertiary butyl acrylate, tertiary butyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, normal octyl acrylate, normal octyl methacrylate, isooctyl acrylate, isooctyl methacrylate, normal nonyl acrylate, normal nonyl methacrylate, isononyl acrylate, and isononyl methacrylate. These may be used alone or in combination of two or more. The (meth)acrylic monomer according to one embodiment of the present invention is preferably a (meth)acrylate having an alkyl group having 2 to 10 carbon atoms, more preferably a (meth)acrylate having an alkyl group having 3 to 9 carbon atoms, and even more preferably a (meth)acrylate having an alkyl group having 4 to 8 carbon atoms. The (meth)acrylic monomer according to one embodiment of the present invention is preferably an acrylate.
[0021] 1.2.2 Polyfunctional monomers The polyfunctional monomer is used to improve the tensile properties and heat aging resistance of the dip-molded coating obtained. The polyfunctional monomer is a compound having two or more radical polymerizable groups in the molecule. From the viewpoints of flexibility, tensile strength at break, and moldability of the dip-molded coating obtained, a monomer represented by chemical formula (1) and an aromatic polyene monomer are preferably used. As the monomer represented by chemical formula (1), 1.9-nonanediol dimethacrylate, 1.9-nonanediol diacrylate, neopentyl glycol dimethacrylate, neopentyl glycol diacrylate, 1.6-hexanediol dimethacrylate, 1.6-hexanediol diacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, triethylene glycol diacrylate, polyethylene glycol dimethacrylate, and polyethylene glycol diacrylate are particularly preferably used. The aromatic polyene monomer is an aromatic polyene having 10 or more and 30 or less carbon atoms and having a plurality of double bonds (vinyl groups) and one or more aromatic groups. Examples of the aromatic polyene monomer include units derived from aromatic polyene monomers such as o-divinylbenzene, p-divinylbenzene, m-divinylbenzene, 1,4-divinylnaphthalene, 3,4-divinylnaphthalene, 2,6-divinylnaphthalene, 1,2-divinyl-3,4-dimethylbenzene, and 1,3-divinyl-4,5,8-tributylnaphthalene. Preferably, one or a mixture of two or more of ortho-divinylbenzene units, para-divinylbenzene units, and meta-divinylbenzene units is suitably used.
[0022] [ka] (In chemical formula (1), R1 and R2 each independently represent hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, a mercapto group, or a substituted or unsubstituted heterocyclyl group. W1 represents a saturated or unsaturated hydrocarbon group, a saturated or unsaturated cyclic hydrocarbon group, or a saturated or unsaturated hydrocarbon group or cyclic hydrocarbon group containing a hetero atom. Z1 represents oxygen, sulfur, or a structure represented by -NR0-. R0 represents hydrogen, chlorine, a substituted or unsubstituted alkyl group, an alkenyl group, an aryl group, a mercapto group, or a heterocyclyl group.)
[0023] 1.3 Content of each structural unit of (meth)acrylic block copolymer The content of each structural unit in the (meth)acrylic block copolymer is 5-30% by mass for polymer block (A) and 70-95% by mass for (meth)acrylic polymer block (B), preferably 5-15% by mass for polymer block (A) and 85-95% by mass for (meth)acrylic polymer block (B). When the polymer block (A) is 5% by mass or more, the tensile strength at break of the obtained (meth)acrylic block copolymer is improved. When the polymer block (A) is 30% by mass or less, the flexibility of the obtained (meth)acrylic block copolymer is improved. The polymer block (A) is preferably 15% by mass or less. When the (meth)acrylic polymer block (B) is 70% by mass or more, the flexibility of the obtained (meth)acrylic block copolymer is improved. The (meth)acrylic polymer block (B) is preferably 85% by mass or more. When the (meth)acrylic polymer block (B) is 95% by mass or less, the tensile strength at break of the obtained (meth)acrylic block copolymer is improved. When the (meth)acrylic block copolymer is taken as 100% by mass, the content of the polymer block (A) contained in the (meth)acrylic block copolymer is, for example, 5, 10, 15, 20, 25, or 30% by mass, and may be within a range between any two of the numerical values exemplified here. The (meth)acrylic block copolymer according to one embodiment of the present invention may contain polymer blocks other than the polymer block (A) and the polymer block (B) within a range that does not impair the object of the present invention. When the (meth)acrylic block copolymer is taken as 100% by mass, the total content of the polymer block (A) and the polymer block (B) is preferably 80% by mass or more, and more preferably 90% by mass or more. The (meth)acrylic block copolymer according to one embodiment of the present invention may be composed of polymer block (A) and polymer block (B), or may not contain other polymer blocks. The (meth)acrylic block copolymer may be a diblock copolymer of polymer block (A)-polymer block (B), which is composed of polymer block (A) and polymer block (B).
[0024] 1.4 Molecular weight of (meth)acrylic block copolymer The weight average molecular weight of the (meth)acrylic block copolymer is not particularly limited, but from the viewpoint of moldability, it is preferably from 50,000 to 600,000, and particularly preferably from 100,000 to 500,000.
[0025] 1.5 Method for producing (meth)acrylic block copolymer The method for producing the (meth)acrylic block copolymer according to the present invention will be described. The polymerization method is not particularly limited, and the copolymer can be produced by a known method such as solution polymerization, emulsion polymerization, or bulk polymerization, but emulsion polymerization is preferable for obtaining the desired (meth)acrylic block copolymer.
[0026] The polymerization method is not particularly limited as long as the desired (meth)acrylic block copolymer can be obtained, but the copolymer can be produced by a two-stage polymerization process consisting of a polymerization step 1 for synthesizing a polymer block (A) and a polymerization step 2 for synthesizing a (meth)acrylic polymer block (B).
[0027] (Polymerization step 1) The polymerization step 1 will be specifically described. In the polymerization step 1, the monomers constituting the polymer block (A) are subjected to living radical emulsion polymerization to synthesize the polymer block (A). The polymer block (A) obtained here preferably has the above-mentioned glass transition temperature. The emulsifier used in the emulsion polymerization is not particularly limited, but an anionic or nonionic emulsifier is preferable from the viewpoint of emulsion stability. In particular, it is preferable to use an alkali metal salt of rosin acid because it can provide the obtained (meth)acrylic block copolymer with appropriate strength and prevent excessive shrinkage and breakage. From the viewpoint of efficient polymerization reaction, the concentration of the emulsifier is preferably 5 to 50% by mass relative to 100% by mass of the monomers constituting the polymer block (A). As the radical polymerization initiator, a known radical polymerization initiator can be used, for example, potassium persulfate, benzoyl peroxide, hydrogen peroxide, azo compounds, etc. can be used. The amount of pure water added is preferably 100 to 300% by mass relative to 100% by mass of the monomers constituting the polymer block (A). When the amount of added pure water is 300% by mass or less, the toluene insoluble content of the obtained (meth)acrylic block copolymer falls within the above-mentioned specific numerical range, and the tensile strength at break is more likely to be improved. The polymerization temperature may be appropriately determined depending on the type of monomer, but is preferably 10 to 100°C, and particularly preferably 20 to 80°C.
[0028] (Polymerization step 2) In the polymerization step 2, pure water, an emulsifier, and a (meth)acrylic monomer, and if necessary, a multifunctional monomer are added to the latex containing the polymer block (A) obtained by the living radical emulsion polymerization in the polymerization step 1, and emulsion polymerization is performed to obtain a latex containing the target (meth)acrylic block copolymer. The (meth)acrylic monomer may be added all at once or in portions. The polymerization temperature in the polymerization step 2 is preferably 10 to 50°C from the viewpoint of ease of polymerization control. The polymerization reaction is terminated by adding a polymerization terminator. Examples of the polymerization terminator include thiodiphenylamine, 4-tert-butylcatechol, and 2,2'-methylenebis-4-methyl-6-tert-butylphenol. After the emulsion polymerization is completed, The unreacted monomer can be removed by a conventional method such as vacuum distillation.
[0029] To the latex containing the (meth)acrylic block copolymer obtained in the polymerization step 2, a freezing stabilizer, an emulsion stabilizer, a viscosity modifier, an antiaging agent, a preservative, etc. may be added after polymerization as long as the object of the present invention is not impaired.
[0030] (Recovery process) The method for recovering the (meth)acrylic block copolymer from the latex containing the (meth)acrylic block copolymer is not particularly limited, and any known method can be used, such as a method of recovering the copolymer by immersing the copolymer in a coagulation liquid or a method of precipitating the copolymer using a poor solvent such as methanol.
[0031] The (meth)acrylic block copolymer preferably has a functional group having a structure represented by the following chemical formula (2) or (3).
[0032] [ka] (In chemical formula (2), R3 represents any one of hydrogen, chlorine, a substituted or unsubstituted alkyl group, an alkenyl group, an aryl group, a mercapto group, and a heterocyclyl group.) [ka]
[0033] The terminal structure represented by the above chemical formula (2) or chemical formula (3) is introduced into a block copolymer by emulsion polymerization in the presence of a known RAFT agent. The compound leading to the structure represented by the above chemical formula (2) is not particularly limited, and general compounds can be used, such as dithiocarbamates and dithioesters. Specifically, benzyl 1-pyrrole carbodithioate (common name: benzyl 1-pyrrole dithiocarbamate), benzyl phenyl carbodithioate, 1-benzyl-N,N-dimethyl-4-aminodithiobenzoate, 1-benzyl-4-methoxydithiobenzoate, 1-phenylethyl imidazole carbodithioate (common name: 1-phenylethyl imidazole dithiocarbamate), benzyl-1-(2-pyrrolidinone) carbodithioate, etc. oate) (common name: benzyl-1-(2-pyrrolidinone)dithiocarbamate), benzyl phthalimidyl carbodithioate, (common name: benzyl phthalimidyl dithiocarbamate), 2-cyanoprop-2-yl-1-pyrrole carbodithioate, (common name: 2-cyanoprop-2-yl-1-pyrrole dithiocarbamate), 2-cyanobut-2-yl-1-pyrrole carbodithioate, (common name: 2-cyanobut-2-yl- 1-Pyrrole dithiocarbamate), benzyl-1-imidazole carbodithioate, (common name benzyl-1-imidazole dithiocarbamate), 2-cyanoprop-2-yl-N,N-dimethyldithiocarbamate, benzyl-N,N-diethyldithiocarbamate, cyanomethyl-1-(2-pyrrolidone)dithiocarbamate, 2-(ethoxycarbonylbenzyl)prop-2-yl-N,N-diethyldithiocarbamate, 1-phenyl nylethyl dithiobenzoate, 2-phenylprop-2-yl dithiobenzoate, 1-acetate-1-yl-ethyl dithiobenzoate, 1-(4-methoxyphenyl)ethyl dithiobenzoate, benzyl dithioacetate, ethoxycarbonylmethyl dithioacetate, 2-(ethoxycarbonyl)prop-2-yl dithiobenzoate, 2-cyanoprop-2-yl dithiobenzoate, tert-butyl dithiobenzoate, 2,4,4-Trimethylpent-2-yldithiobenzoate, 2-(4-chlorophenyl)-prop-2-yldithiobenzoate, 3-vinylbenzyldithiobenzoate, 4-vinylbenzyldithiobenzoate, benzyldiethoxyphosphinyldithioformate, tert-butyltrithioperbenzoate, 2-phenylprop-2-yl-4-chlorodithiobenzoate, naphthalene-1-carboxylic acid-1-methyl-1-phenyl-ethyl ester, 4-cyano-4-methyl-4-thiobenzylsulfanylbutyric acid, dibenzyltetrathioterephthalate, carboxymethyldithiobenzoate, poly(ethylene oxide) with dithiobenzoate end groups, poly(ethylene oxide) with 4-cyano-4-methyl-4-thiobenzylsulfanylbutyric acid end groups, 2-[(2-phenylethanethioyl)sulfanyl]propanoic acid, 2-[(2-phenylethanethioyl)sulfanyl]propanoic acid 1H-pyrazole-1-carbodithioate potassium, cyanomethyl-3,5-dimethyl-1H-pyrazole-1-carbodithioate, cyanomethyl-N-methyl-N-phenyldithiocarbamate, benzyl-4-chlorodithiobenzoate, phenylmethyl-4-chlorodithiobenzoate, 4-nitrobenzyl-4-chlorodithiobenzoate, phenylprop-2-yl- Examples of the chlorodithiobenzoate include 4-chlorodithiobenzoate, 1-cyano-1-methylethyl-4-chlorodithiobenzoate, 3-chloro-2-butenyl-4-chlorodithiobenzoate, 2-chloro-2-butenyldithiobenzoate, benzyldithioacetate, 3-chloro-2-butenyl-1H-pyrrole-1-dithiocarboxylic acid, and 2-cyanobutan-2-yl 4-chloro-3,5-dimethyl-1H-pyrazole-1-carbodithioate. Among these, benzyl 1-pyrrolecarbodithioate and benzylphenylcarbodithioate are particularly preferred.
[0034] The compound leading to the structure represented by the above chemical formula (3) is not particularly limited, and a general compound can be used, for example, 2-cyano-2-propyldodecyltrithiocarbonate, dibenzyltrithiocarbonate, butylbenzyltrithiocarbonate, 2-[[(butylthio)thioxomethyl]thio]propionic acid, 2-[[(dodecylthio)thioxomethyl]thio]propionic acid, 2-[[(butylthio)thioxomethyl]thio]succinic acid, 2-[[(dodecylthio)thioxomethyl]thio]succinic acid, 2-[[(dodecylthio)thioxomethyl]thio] ]-2-methylpropionic acid, 2,2'-[carbonothioylbis(thio)]bis[2-methylpropionic acid], 2-amino-1-methyl-2-oxoethylbutyl trithiocarbonate, benzyl 2-[(2-hydroxyethyl)amino]-1-methyl-2-oxoethyltrithiocarbonate, 3-[[[(tert-butyl)thio]thioxomethyl]thio]propionic acid, cyanomethyldodecyltrithiocarbonate, diethylaminobenzyltrithiocarbonate, dibutylaminobenzyltrithiocarbonate and other trithiocarbonates are particularly preferred. Among these, dibenzyltrithiocarbonate and butylbenzyltrithiocarbonate are particularly preferred.
[0035] The (meth)acrylic copolymer according to one embodiment of the present invention preferably has at least one structure selected from the group consisting of a structure derived from a polyfunctional monomer, a structure represented by chemical formula (2), and a structure represented by chemical formula (3).
[0036] 2. (Meth)acrylic block copolymer latex The (meth)acrylic block copolymer latex according to one embodiment of the present invention contains the (meth)acrylic block copolymer described above. The (meth)acrylic block copolymer latex according to one embodiment of the present invention is preferably for use in a dip-molded product. The latex according to one embodiment of the present invention can be immersed in a coagulating liquid and molded to obtain a dip-molded product. The dip-molded product can be suitably used for gloves, balloons, catheters, boots, and the like.
[0037] The latex of the present embodiment can be obtained by a method in which the liquid at the end of polymerization synthesized by emulsion polymerization described in the above-mentioned method for producing the (meth)acrylic block copolymer is used as a latex as it is, or a method in which the recovered (meth)acrylic block copolymer is forcibly emulsified using an emulsifier to obtain a latex, and the like. The method in which the liquid at the end of polymerization synthesized by emulsion polymerization is used as a latex as it is is preferable because a latex can be obtained easily.
[0038] 2.1 Toluene insolubles in (meth)acrylic block copolymer latex The (meth)acrylic block copolymer latex according to one embodiment of the present invention preferably contains 20 to 100% by mass of toluene insoluble matter, more preferably 70 to 100% by mass, based on 100% by mass of the (meth)acrylic block copolymer latex. When the toluene insoluble matter is equal to or more than the lower limit, the block copolymers contain a structure in which they are chemically bonded to each other, and therefore the tensile strength at break is thought to be improved. The toluene insoluble matter can be, for example, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100% by mass, and may be within a range between any two of the numerical values exemplified here. In this specification, the toluene insoluble matter is calculated by dissolving a freeze-dried latex containing a (meth)acrylic block copolymer in toluene, centrifuging the mixture, separating the gel fraction using a 200-mesh wire net, and measuring the mass of the dried product, and then calculating the amount from the following formula. (Mass of solid obtained by separating and drying gel fraction) / (Mass of solid obtained by freeze-drying latex containing (meth)acrylic block copolymer)×100 The toluene-insoluble content can be adjusted by controlling the types and amounts of raw materials blended during polymerization of the (meth)acrylic block copolymer as well as the polymerization conditions, and by controlling the type and amount of polymer blocks, for example, the type and amount of polyfunctional monomer units, and the type, amount and structure of functional groups derived from a RAFT agent or the like.
[0039] 2.2 Average particle size of (meth)acrylic block copolymer latex The average particle size of the (meth)acrylic block copolymer latex measured by dynamic light scattering is preferably 300 nm or less, more preferably 250 nm or less, and even more preferably 200 nm or less, from the viewpoint of mechanical stability of the latex. The lower limit can be, for example, 100 nm or more. The average particle size can be, for example, 100, 120, 140, 150, 160, 170, 180, 190, 200, 220, 240, 260, 280, or 300 nm, and may be within a range between any two of the numerical values exemplified here. In this specification, the average particle size is the average particle size measured by dynamic light scattering and calculated by photon correlation spectroscopy. The average particle size can be adjusted by controlling the type and amount of the (meth)acrylic block copolymer latex blended and the production conditions, for example, by the stirring conditions during emulsion polymerization.
[0040] 2.3 Mechanical stability of (meth)acrylic block copolymer latex The mechanical stability of the (meth)acrylic block copolymer latex according to one embodiment of the present invention is preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less. The mechanical stability of the (meth)acrylic block copolymer latex can be evaluated by the measurement method described in the Examples. The mechanical stability can be adjusted by controlling the type and amount of the (meth)acrylic block copolymer latex and the production conditions, for example, by controlling the average particle size of the (meth)acrylic block copolymer latex.
[0041] 2.4 Tensile properties of (meth)acrylic block copolymer latex The (meth)acrylic block copolymer of this embodiment can provide an unvulcanized dip-molded coating that does not contain a vulcanizing agent or a vulcanization accelerator and has a tensile strength at break of 14 MPa or more measured according to JIS K 6251 after heat-treating a dip-molded coating obtained by dip-molding a (meth)acrylic block copolymer latex containing the (meth)acrylic block copolymer for 30 minutes. The unvulcanized dip-molded coating has flexibility and exhibits sufficient mechanical strength even without containing a vulcanizing agent or a vulcanization accelerator. The tensile strength at break is more preferably 15 MPa or more, even more preferably 16 MPa or more, even more preferably 17 MPa or more, and particularly preferably 20 MPa or more. The upper limit is not particularly limited, but is, for example, 30 MPa or less. The tensile strength at break may be, for example, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30 MPa, or may be within a range between any two of the values exemplified herein.
[0042] The (meth)acrylic block copolymer according to one embodiment of the present invention has a tensile strength at break measured in accordance with JIS K 6251 after a dip-molded coating obtained by dip-molding a (meth)acrylic block copolymer latex containing the (meth)acrylic block copolymer is heat-treated at 30° C. for 30 minutes and then subjected to a heat aging test at 100° C. for 22 hours, preferably 14 MPa or more, more preferably 15 MPa or more, even more preferably 16 MPa or more, even more preferably 17 MPa or more, and particularly preferably 20 MPa or more. The upper limit is not particularly limited, but is, for example, 30 MPa or less.
[0043] Furthermore, the (meth)acrylic block copolymer of this embodiment has an elongation at break of preferably 900% or more, more preferably 905% or more, and even more preferably 910% or more, as measured in accordance with JIS K 6251 after a dip-molded coating obtained by dip-molding a (meth)acrylic block copolymer-containing (meth)acrylic block copolymer latex is heat-treated at 130° C. for 30 minutes. The upper limit is not particularly limited, but is, for example, 1300% or less.
[0044] The (meth)acrylic block copolymer according to one embodiment of the present invention is a dip-molded coating obtained by dip-molding a (meth)acrylic block copolymer latex containing the (meth)acrylic block copolymer, which is then heat-treated at 30° C. for 30 minutes and then subjected to a heat aging test at 100° C. for 22 hours. The elongation at break measured in accordance with JIS K 6251 is preferably 900% or more, more preferably 905% or more, and even more preferably 910% or more. The upper limit is not particularly limited, but is, for example, 1300% or less.
[0045] The (meth)acrylic block copolymer of this embodiment has a modulus at 500% elongation measured in accordance with JIS K 6251 after a dip-molded coating obtained by dip-molding a (meth)acrylic block copolymer latex containing the (meth)acrylic block copolymer is heat-treated at 130° C. for 30 minutes. The modulus is preferably 3.0 MPa or less, more preferably 2.9 MPa or less, and even more preferably 2.8 MPa or less. The lower limit is not particularly limited, but is, for example, 1.0 MPa or more.
[0046] In the (meth)acrylic block copolymer according to one embodiment of the present invention, a dip-molded coating obtained by dip-molding a (meth)acrylic block copolymer latex containing the (meth)acrylic block copolymer is heat-treated at 30° C. for 30 minutes, and then subjected to a heat aging test at 100° C. for 22 hours. The modulus at 500% elongation measured in accordance with JIS K 6251 is preferably 3.0 MPa or less, more preferably 2.9 MPa or less, and even more preferably 2.8 MPa or less. The lower limit is not particularly limited, but is, for example, 1.0 MPa or more. The dip-molded coating can be obtained by the method described in the Examples, and the dip-molded coating can be obtained without using a vulcanizing agent or a vulcanization accelerator during molding.
[0047] The tensile strength at break, elongation at break and modulus at 500% elongation of the dip-molded coating obtained by dip-molding a (meth)acrylic block copolymer latex containing a (meth)acrylic block copolymer can be adjusted by adjusting the content of polyfunctional monomer units contained in the (meth)acrylic polymer block (B) or the content of the (meth)acrylic polymer block (B) in the (meth)acrylic block copolymer, or by adjusting the type and amount of functional groups introduced by polymerization in the presence of a RAFT agent described below.
[0048] The dip-molded coating obtained from the (meth)acrylic block copolymer latex of this embodiment may contain a vulcanizing agent or a vulcanization accelerator. When the dip-molded coating contains a vulcanizing agent and a vulcanization accelerator, the total content of the vulcanizing agent and the vulcanization accelerator can be 5% by mass or less, more preferably 1% by mass or less, and more preferably 0.1% by mass, based on 100% by mass of the (meth)acrylic block copolymer latex contained in the dip-molded coating. However, since the unvulcanized dip-molded coating has sufficient mechanical strength even without the vulcanizing agent and the vulcanization accelerator, it is preferable that the unvulcanized dip-molded coating does not contain the vulcanizing agent and the vulcanization accelerator from the viewpoints of reducing allergies and reducing costs.
[0049] 3. (Meth)acrylic block copolymer latex composition A (meth)acrylic block copolymer latex composition according to one embodiment of the present invention contains a (meth)acrylic block copolymer latex containing the above-mentioned (meth)acrylic block copolymer.
[0050] 3.1 Components contained in the (meth)acrylic block copolymer latex composition The (meth)acrylic block copolymer latex composition according to the present embodiment contains a (meth)acrylic block copolymer. Raw materials other than the (meth)acrylic block copolymer are not particularly limited and can be appropriately selected according to the purpose and application. Examples of raw materials that can be contained in the latex composition / rubber composition containing the (meth)acrylic block copolymer include vulcanizing agents, vulcanization accelerators, fillers or reinforcing agents, plasticizers, processing aids and lubricants, antioxidants, and silane coupling agents.
[0051] The latex composition of the present embodiment may contain a vulcanizing agent or a vulcanization accelerator. When the latex composition according to the present embodiment contains a vulcanizing agent and / or a vulcanization accelerator, the total content of the vulcanizing agent and the vulcanization accelerator can be 5% by mass or less, more preferably 1% by mass or less, and more preferably 0.1% by mass, based on the (meth)acrylic block copolymer latex contained in the (meth)acrylic block copolymer latex composition, when the latex composition is taken as 100% by mass. However, the latex composition containing the (meth)acrylic block copolymer of the present embodiment exhibits sufficient mechanical strength even without vulcanization. For this reason, it is preferable that the latex composition does not contain a vulcanizing agent or a vulcanization accelerator from the viewpoints of reducing allergies and reducing costs.
[0052] As the antiaging agent for improving heat resistance, a primary antiaging agent that traps radicals to prevent autoxidation and a secondary antiaging agent that renders hydroperoxide harmless, which are used in normal rubber applications, can be added. The antiaging agents can be added in a ratio of 0.1 to 10 parts by mass, preferably 2 to 5 parts by mass, per 100 parts by mass of the latex component in the latex composition. These antiaging agents can be used alone or in combination of two or more kinds. Examples of the primary antiaging agent include phenol-based antiaging agents, amine-based antiaging agents, acrylate-based antiaging agents, imidazole-based antiaging agents, carbamic acid metal salts, and waxes. Examples of the secondary antiaging agent include phosphorus-based antiaging agents, sulfur-based antiaging agents, and imidazole-based antiaging agents. Examples of antioxidants include, but are not limited to, N-phenyl-1-naphthylamine, alkylated diphenylamine, octylated diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, p-(p- Toluenesulfonylamido)diphenylamine, N,N'-di-2-naphthyl-p-phenyl Nylenediamine, N,N'-diphenyl-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-phenyl-N'-(1,3-dimethylbutyric acid N-phenyl-N'-(3-methacryloyloxy-2-phenyl)-p-phenylenediamine -hydroxypropyl)-p-phenylenediamine, 1,1,3-tris-(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 4,4'-butylidenebis-(3 -Methyl-6-t-butylphenol), 2,2-thiobis(4-methyl-6-t-butylphenol), 7-octadecyl-3-(4'-hydroxy-3',5'-di-t-butyl tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, pentaerythritol-tetrakis Rakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,4-bis(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4 -hydroxy)-hydrocinnamamide, 2,4-bis[(octylthio)methyl]-o-cresol, 3,5-di-t-butyl-4-hydroxybenzyl-phosphonate-diethyl ester, tetrakis[methylene(3,5-di-t-butyl-4-hydroxyhydrocinnamate)]methane, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate ester and 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, tris(nonylphenyl)phosphite, tris(mixed mono- and di-nonylphenyl)phosphite, diphenyl mono(2-ethylhexyl)phosphite sphite, diphenyl monotridecyl phosphite, diphenyl isodecyl phosphite, diphenyl isooctyl phosphite, diphenyl nonylphenyl phosphite, triphenyl phosphite, tris(tridecyl) phosphite, triisodecyl phosphite, tris(2-ethylhexyl) phosphite, tris(2,4-di-t-butylphenyl) phosphite, tetraphenyl dipropylene glycol diphosphite, tetraphenyl tetra(tridecyl) pentaerythritol tetraphosphite, 1,1,3-tris(2-methyl-4-di-tridecyl phosphite-5-t-butylphenyl) butane, 4,4'-butylidenebis-(3-methyl-6-t-butyl-di-tridecyl phosphite Sulfite), 2,2'-ethylidenebis(4,6-di-t-butylphenol) fluoro Rophosphite, 4,4'-isopropylidene-diphenol alkyl (C12-C1 5) Phosphite, cyclic neopentanetetraylbis(2,4-di-t-butylphenyl phosphite), cyclic neopentanetetraylbis(2,6-di-t-butyl-4-phenyl phosphite), cyclic neopentanetetraylbis(nonylphenyl phosphite), bis(nonylphenyl)pentaerythritol diphosphite, dibutyl hydrogen phosphite, distearyl pentaerythritol diphosphite and hydrogenated bisphenol A pentaerythritol phosphite polymer, 2-mercaptobenzimidazole, butylated reaction product of p-cresol and dicyclopentadiene, etc.
[0053] The latex composition can be produced in a conventional manner using known machines and devices.
[0054] 4. Molded body A molded article according to one embodiment of the present invention contains the above-mentioned (meth)acrylic block copolymer latex composition, and preferably consists of the above-mentioned (meth)acrylic block copolymer latex composition. The components that the molded article according to one embodiment of the present invention may contain are as described above for the (meth)acrylic block copolymer latex composition. The properties that the molded article according to one embodiment of the present invention may have are as described above for the tensile properties of the (meth)acrylic block copolymer latex. EXAMPLES
[0055] The present invention will be described below with reference to examples and comparative examples, but these are merely illustrative and do not limit the content of the present invention.
[0056] Example 1 (Polymerization step 1) Synthesis of polymer block (A-1) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. The polymerization was started by adding 3.82 g of hydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044). 20 ml of the obtained latex was sampled for measuring physical properties, and the remaining latex was used in the polymerization step 2.
[0057] The sampled latex was mixed with a large amount of methanol to precipitate the resin, which was then filtered and dried to obtain a sample of polymer block (A-1). The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A) were determined from the obtained sample. The analysis results are shown in Table 1. The methods for measuring the "number average molecular weight," "molecular weight distribution," and "glass transition temperature" will be described later.
[0058] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-1) After the polymerization step 1, when the internal temperature dropped to 45°C, 4480g of normal butyl acrylate monomer and 91.4g of 1,9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and the remaining latex was used to prepare a film for evaluation.
[0059] Using a part of the sampled latex, the average particle size of the latex and the mechanical stability of the latex were measured. The analysis results are shown in Table 1. The measurement method will be described later. The sampled latex was mixed with a large amount of methanol to precipitate the resin content, which was then filtered and dried to obtain a sample of a (meth)acrylic block copolymer. The content (mass%) of the polymer block (A-1) and the (meth)acrylic polymer block (B-1) of the normal butyl acrylate block copolymer was determined from the obtained sample by analysis. The analysis results are shown in Table 1. The measurement method will be described later. The toluene insoluble content was determined from the sampled latex. The analysis results are shown in Table 1. The measurement method will be described later.
[0060] Example 2 (Polymerization step 1) Synthesis of polymer block (A-2) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a heating / cooling jacket. 3333 g of pure water, 160 g of disproportionated potassium rosinate (Harima Chemicals), 26.0 g of potassium hydroxide, 13.3 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 250 g of styrene monomer, and 4.33 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was adjusted to 80° C. and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 2.73 g of dihydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-2) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0061] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-2) After the polymerization step 1, when the internal temperature dropped to 45°C, 5584g of normal butyl acrylate monomer and 114.0g of 1.9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-2) and the (meth)acrylic polymer block (B-2) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0062] Example 3 (Polymerization step 1) Synthesis of polymer block (A-3) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 5733 g of pure water, 275 g of disproportionated potassium rosinate (Harima Chemicals), 44.7 g of potassium hydroxide, 22.9 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 430 g of styrene monomer, and 7.45 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 4.69 g of dihydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-3) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0063] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-3) After the polymerization step 1, when the internal temperature dropped to 45°C, 3094g of normal butyl acrylate monomer and 63.1g of 1.9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-3) and the (meth)acrylic polymer block (B-3) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0064] Example 4 (Polymerization step 1) Synthesis of polymer block (A-4) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 3.82 g of dihydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-4) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0065] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-4) After the polymerization step 1, when the internal temperature dropped to 45°C, 4480g of normal butyl acrylate monomer and 91.4g of 1.9-nonanediol diacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-4) and the (meth)acrylic polymer block (B-4) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0066] Example 5 (Polymerization step 1) Synthesis of polymer block (A-5) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 3.82 g of hydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-5) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0067] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-5) After the polymerization step 1, when the internal temperature dropped to 45°C, 4480g of normal butyl acrylate monomer and 91.4g of Light Ester EG (manufactured by Kyoeisha Chemical Co., Ltd.), which is ethylene glycol diacrylate, were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-5) and the (meth)acrylic polymer block (B-5) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0068] Example 6 (Polymerization step 1) Synthesis of polymer block (A-6) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 3.82 g of hydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-6) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0069] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-6) After the polymerization step 1, when the internal temperature dropped to 45°C, 4480g of normal butyl acrylate monomer and 93.3g of divinylbenzene were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-6) and the (meth)acrylic polymer block (B-6) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0070] Example 7 (Polymerization step 1) Synthesis of polymer block (A-7) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 5450 g of pure water, 262 g of disproportionated potassium rosinate (Harima Chemicals), 42.5 g of potassium hydroxide, 21.8 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 2500 g of styrene monomer, and 43.3 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was adjusted to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propane] was used as a polymerization initiator. Polymerization was initiated by adding 27.3 g of dihydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-7) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0071] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-7) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 2732g of pure water, 131g of disproportionated potassium rosinate (Harima Chemicals), 21.3g of potassium hydroxide, 10.9g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, trade name: Demol N), and 783g of latex containing the polymer block (A-7) produced in polymerization step 1 were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. Then, 3000g of normal butyl acrylate monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the normal butyl acrylate monomer reached 80%, the polymerization was stopped by adding a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, and the unreacted normal butyl acrylate monomer was removed by vacuum distillation. For the measurement of physical properties, 20 ml of the obtained latex was sampled, and the remaining latex was used to prepare a film for evaluation. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-7) and the (meth)acrylic polymer block (B-7) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0072] Example 8 (Polymerization step 1) Synthesis of polymer block (A-8) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 3.82 g of hydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-8) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0073] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-8) After the polymerization step 1, when the internal temperature dropped to 45°C, 4480g of normal butyl acrylate monomer and 91.4g of triallyl isocyanurate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and the remaining latex was used to prepare a film for evaluation. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-8) and the (meth)acrylic polymer block (B-8) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0074] Example 9 (Polymerization step 1) Synthesis of polymer block (A-9) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 3.82 g of hydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-9) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0075] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-9) After the polymerization step 1, when the internal temperature dropped to 45°C, 4480g of normal butyl acrylate monomer and 91.4g of hydroxypivalic acid neopentyl glycol acrylic acid adduct (manufactured by Kyoeisha Chemical Co., Ltd.) were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-9) and the (meth)acrylic polymer block (B-9) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0076] Example 10 (Polymerization step 1) Synthesis of polymer block (A-10) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 3.82 g of hydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-10) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0077] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-10) After the polymerization step 1, when the internal temperature dropped to 45°C, 4480g of normal butyl acrylate monomer and 91.4g of trimethylolpropane triacrylate (Kyoeisha Chemical Co., Ltd.) were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-10) and the (meth)acrylic polymer block (B-10) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0078] Example 11 (Polymerization step 1) Synthesis of polymer block (A-11) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 6667 g of pure water, 320 g of disproportionated potassium rosinate (Harima Chemicals), 52.0 g of potassium hydroxide, 26.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 500 g of styrene monomer, and 6.50 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 4.09 g of dihydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-11) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0079] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-11) After the polymerization step 1, when the internal temperature dropped to 45°C, 1607g of normal butyl acrylate monomer and 32.8g of 1.9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-11) and the (meth)acrylic polymer block (B-11) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0080] Example 12 (Polymerization step 1) Synthesis of polymer block (A-12) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a heating / cooling jacket. 5450 g of pure water, 262 g of disproportionated potassium rosinate (Harima Chemicals), 42.5 g of potassium hydroxide, 21.8 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 2500 g of styrene monomer, and 32.5 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was adjusted to 80° C. and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazoline-2-yl)propane] was used as a polymerization initiator. Polymerization was initiated by adding 20.5 g of dihydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-12) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0081] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-12) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 1188g of pure water, 57g of disproportionated potassium rosinate (Harima Chemicals), 9.3g of potassium hydroxide, 4.8g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, trade name: Demol N), and 3147g of latex containing the polymer block (A-12) produced in polymerization step 1 were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. Then, 3000g of normal butyl acrylate monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the normal butyl acrylate monomer reached 80%, the polymerization was stopped by adding a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For the measurement of physical properties, 20 ml of the obtained latex was sampled, and the remaining latex was used to prepare a film for evaluation. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-12) and the (meth)acrylic polymer block (B-12) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0082] Example 13 (Polymerization step 1) Synthesis of polymer block (A-13) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of methyl methacrylate monomer, and 4.14 g of butyl-2-cyanoisopropyl trithiocarbonate were charged, the internal temperature was set to 80°C, and the mixture was stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-isopropyl)phenyl]- ... Polymerization was initiated by adding 2.87 g of [midazolin-2-yl]propane dihydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-13) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0083] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-13) After the polymerization step 1, when the internal temperature dropped to 45°C, 4424g of normal butyl acrylate monomer and 90.3g of 1.9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-13) and the (meth)acrylic polymer block (B-13) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0084] Comparative Example 1 (Polymerization step 1) Synthesis of polymer block (A-14) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a heating / cooling jacket. 3067 g of pure water, 147 g of disproportionated potassium rosinate (Harima Chemicals), 23.9 g of potassium hydroxide, 12.3 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 230 g of styrene monomer, and 3.99 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 2.51 g of dihydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-14) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0085] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-14) After the polymerization step 1, when the internal temperature dropped to 45°C, 7278g of normal butyl acrylate monomer and 148.5g of 1.9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-14) and the (meth)acrylic polymer block (B-14) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0086] Comparative Example 2 (Polymerization step 1) Synthesis of polymer block (A-15) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 6667 g of pure water, 320 g of disproportionated potassium rosinate (Harima Chemicals), 52.0 g of potassium hydroxide, 26.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 500 g of styrene monomer, and 4.27 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 2.69 g of hydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-15) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0087] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-15) After the polymerization step 1, when the internal temperature dropped to 45°C, 1607g of normal butyl acrylate monomer and 32.8g of 1.9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-15) and the (meth)acrylic polymer block (B-15) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0088] Comparative Example 3 Synthesis of copolymers containing only (meth)acrylic polymer blocks (B-16) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 3600 g of pure water, 175 g of disproportionated potassium rosinate (Harima Chemicals), 28.4 g of potassium hydroxide, 16.0 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 4000 g of normal butyl acrylate monomer, 81.6 g of 1.9-nonanediol dimethacrylate, and 4.72 g of butyl benzyl trithiocarbonate were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dichloride was used as a polymerization initiator. 2.96 g of hydrogen (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044) was added to initiate polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20 ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex and the mechanical stability of the latex were determined by analysis in the same manner as in Example 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0089] Comparative Example 4 (Polymerization step 1) Synthesis of polymer block (A-17) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4616 g of pure water, 206 g of disproportionated potassium rosinate (Harima Chemicals), 2.3 g of potassium hydroxide, 46.2 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 462 g of styrene monomer, and 9.2 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was adjusted to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propane] was used as a polymerization initiator. 6.0 g of hydrogen dichloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044) was added to initiate polymerization. 20 ml of the obtained latex was sampled for measuring physical properties, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-16) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0090] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-17) After the polymerization step 1, when the internal temperature dropped to 45°C, 4154g of normal butyl acrylate monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-17) and the (meth)acrylic polymer block (B-17) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0091] Comparative Example 5 (Polymerization step 1) Synthesis of polymer block (A-18) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4616 g of pure water, 206 g of disproportionated potassium rosinate (Harima Chemicals), 2.3 g of potassium hydroxide, 46.2 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 692 g of styrene monomer, and 9.2 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was adjusted to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propane] was used as a polymerization initiator. Polymerization was initiated by adding 6.0 g of hydrogen dichloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). 20 ml of the obtained latex was sampled for property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-18) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0092] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-18) After the polymerization step 1, when the internal temperature dropped to 45°C, 3924g of normal butyl acrylate monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of normal butyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted normal butyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, and the content (mass%) of the polymer block (A-18) and the (meth)acrylic polymer block (B-18) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1. In addition, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1.
[0093] Comparative Example 6 Preparation of a mixture of homopolymers of polymer block (A) and homopolymers of (meth)acrylic polymer block (B) (Synthesis of homopolymer of polymer block (A)) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. Polymerization was initiated by adding 3.82 g of N,N-dihydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). When the polymerization rate of the styrene monomer reached 95%, the polymerization was terminated by adding a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator. 20 ml of the obtained latex was sampled for measuring physical properties. The number average molecular weight, molecular weight distribution, and glass transition temperature of the homopolymer of the polymer block (A) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 2.
[0094] (Synthesis of homopolymer of (meth)acrylic polymer block (B)) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 3960 g of pure water, 193 g of disproportionated potassium rosinate (Harima Chemicals), 31.2 g of potassium hydroxide, 17.6 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 4400 g of normal butyl acrylate monomer, 89.8 g of 1.9-nonanediol dimethacrylate, and 5.19 g of butyl benzyl trithiocarbonate were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dichloride was used as a polymerization initiator. Polymerization was initiated by adding 3.26 g of hydrogen (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044). When the polymerization rate of the normal butyl acrylate monomer reached 80%, the polymerization was terminated by adding a 10 mass% aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, and the unreacted normal butyl acrylate monomer was removed by reduced pressure distillation.
[0095] (Mixing of homopolymer latex of polymer block (A) and homopolymer latex of (meth)acrylic polymer block (B)) 4000 g of the obtained homopolymer latex of the polymer block (A) and 4000 g of the homopolymer latex of the (meth)acrylic polymer block (B) were charged into a 10 L capacity autoclave equipped with a stirrer and a jacket for heating and cooling, and the inside temperature was set to 45° C. and stirred at 200 rpm. For physical property measurement, 20 ml of the obtained latex was sampled, and the remaining latex was used to prepare a film for evaluation. The average particle size of the latex, the mechanical stability of the latex, and the contents (mass%) of the homopolymer of the polymer block (A) and the homopolymer of the (meth)acrylic polymer block (B) in the polymer obtained by mixing, and the toluene insoluble content were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 2.
[0096] Example 14 (Polymerization step 1) Synthesis of polymer block (A-19) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. The polymerization was started by adding 3.82 g of hydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044). 20 ml of the obtained latex was sampled for measuring physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-19) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0097] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-19) After the polymerization step 1, when the internal temperature dropped to 45°C, 4480g of ethylhexyl acrylate monomer and 91.4g of 1.9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of the ethylhexyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted ethylhexyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The contents (mass%) of the polymer block (A-19) and the (meth)acrylic polymer block (B-19) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0098] Example 15 (Polymerization step 1) Synthesis of polymer block (A-20) Polymerization was carried out using a 10 L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of disproportionated potassium rosinate (Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 2,2'-azobis[2-(2-imidazolin-2-yl)propanediol] was used as a polymerization initiator. The polymerization was started by adding 3.82 g of hydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044). 20 ml of the obtained latex was sampled for measuring physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-20) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0099] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-20) After the polymerization step 1, when the internal temperature dropped to 45°C, 4480g of octyl acrylate monomer and 91.4g of 1.9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of the octyl acrylate monomer reached 80%, a 10% by mass aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted octyl acrylate monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The contents (mass%) of the polymer block (A-20) and the (meth)acrylic polymer block (B-20) of the (meth)acrylic block copolymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0100] [analysis] (Measurement of number average molecular weight and molecular weight distribution of polymer block (A)) The number average molecular weight and molecular weight distribution are values calculated as polystyrene by gel permeation chromatography (GPC) and are values measured under the measurement conditions described below. Device name: HLC-8320 (Tosoh Corporation) Column: 3 TSKgel GMHHR-H in series Temperature: 40℃ Detection: Differential refractive index Solvent: Tetrahydrofuran Calibration curve: Prepared using standard polystyrene (PS).
[0101] (Glass transition temperature of polymer block (A)) The glass transition temperature was measured using a differential scanning calorimeter in accordance with JIS K 7121 by the following method. Device name: DSC1 (Mettler Toledo) Procedure: Under a nitrogen flow of 50 ml / min, the sample was heated to 120°C at a rate of 10°C / min, kept at 120°C for 10 minutes, then cooled to -60°C. The sample was then heated to 120°C at a rate of 10°C / min to obtain a DSC curve. The glass transition temperature was determined as the temperature at the intersection of a straight line extending the base line on the high temperature side to the low temperature side and a tangent line drawn at the point where the slope of the curve on the high temperature side of the peak is maximum.
[0102] (Measurement of the Contents of Polymer Block (A) and (Meth)acrylic Polymer Block (B) in (Meth)acrylic Block Copolymer) The measurements were carried out using pyrolysis gas chromatogram and 1H-NMR as follows. Pyrolysis gas chromatogram Instrument name: HP5890-II Column: DB-5 0.25 mm diameter x 30 m (film thickness 1.0 μm) Column temperature: 50℃(5min)→10℃ / min→150℃→25℃ / min→300℃ Inlet temperature: 250℃ Detector temperature: 280℃ Detector: FID 1H-NMR device name: JNM-ECX-400 (manufactured by JEOL Ltd.) Procedure: A (meth)acrylic block copolymer consisting of a polymer block (A) and a (meth)acrylic polymer block (B) not containing a polyfunctional monomer unit was measured by pyrolysis gas chromatography, and a calibration curve was prepared from the area ratio of the peak derived from the polymer block (A) to the peak derived from the (meth)acrylic polymer block (B) and the contents of the polymer block (A) and the (meth)acrylic polymer block (B) in the (meth)acrylic block copolymer obtained by measuring 1H-NMR. A sample of the (meth)acrylic block copolymer precipitated by mixing the sampled latex with methanol was measured by pyrolysis gas chromatography, and the contents of the polymer block (A) and the (meth)acrylic polymer block (B) in the (meth)acrylic block copolymer were obtained from the area ratio of the peak derived from the polymer block (A) to the peak derived from the (meth)acrylic polymer block (B) using the calibration curve prepared above.
[0103] [Measurement of toluene insolubles] The latex obtained in the polymerization step 2 was freeze-dried, and 1 g of the solid was cut into 2 mm squares, placed in a conical beaker, and dissolved in toluene for 16 hours. After that, the mixture was centrifuged, and the gel fraction was separated using a 200 mesh wire net. The dried mass was measured, and the toluene insoluble fraction was calculated using the following formula. (Mass of solid obtained by separating and drying gel fraction) / (Mass of solid obtained by freeze-drying latex containing (meth)acrylic block copolymer)×100
[0104] (Measurement of average particle size of latex) 0.1 g of the sampled latex was dissolved in 50 g of pure water, and the sample was measured by dynamic light scattering using ELSZ-2 manufactured by Otsuka Electronics Co., Ltd., and the average particle size of the latex was calculated by photon correlation spectroscopy.
[0105] (Measurement of mechanical stability of latex) The mechanical stability of the latex was measured in accordance with JIS K 6392 using a Maron mechanical stability tester by the following method. Procedure: The sampled latex was filtered through a wire net to remove impurities, and then the filtered latex was adjusted to 20°C and 50g was weighed into a test container. The test container was attached to a tester and measured for 10 minutes with a load of 10kg. After the measurement, the sample in the test container was filtered through an 80-mesh wire net that had been dried at 125°C for 1 hour and cooled in a desiccator, and the 80-mesh wire net and precipitate were dried in a dryer at 125°C for 1 hour and then cooled in a desiccator, and the 80-mesh wire net and precipitate were weighed. The total solid content (unit: %) of the sampled latex was calculated in accordance with JIS K 6387. Next, the coagulation rate (unit: mass%) of the latex was calculated using the following formula. [(Mass of 80 mesh wire net and precipitate after drying (unit: g)) - (Mass of 80 mesh wire net (unit: g))] / [50 × ((Total solid content of latex (unit: mass%)) / 100)] × 100 The obtained coagulation rate of the latex was regarded as the mechanical stability of the latex. A latex mechanical stability of 1% by mass or less was regarded as an acceptable level.
[0106] [Preparation of samples for tensile tests] (Preparation of latex containing (meth)acrylic block copolymer) To 100 parts by mass (solid content equivalent) of the (meth)acrylic block copolymer in the latex obtained in the polymerization step 2, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (product name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) as an antiaging agent, 0.3 parts by mass of sodium lauryl sulfate (product name "EMAL 10", manufactured by Kao Corporation), and water were added to adjust the solid content concentration of the blend to 30% by mass, and the mixture was mixed at 20°C for 16 hours using a ceramic ball mill to prepare the blend. (Film Creation) A ceramic cylinder with an outer diameter of 50 mm was immersed for 1 second in a coagulation liquid containing 62 parts by mass of water, 35 parts by mass of potassium nitrate tetrahydrate, and 3 parts by mass of calcium carbonate, and then removed. After drying for 4 minutes, the cylinder was immersed for 2 minutes in the latex prepared above. The cylinder was then washed with running water at 45°C for 1 minute, and heated at 130°C for 30 minutes to remove moisture, producing a film (140 x 150 mm, thickness: 0.2 mm) for tensile testing.
[0107] [Evaluation of tensile properties] The prepared film was heat-treated at 130°C for 30 minutes, and then the modulus at 500% elongation, tensile strength at break, and elongation at break were measured in accordance with JIS K 6251. The pass level was determined to be 3.0 MPa or less for the modulus at 500% elongation, 14 MPa or more for the tensile strength at break, and 900% or more for the elongation at break.
[0108] [Evaluation of thermal aging properties] The prepared film was subjected to a heat aging test at 100°C for 22 hours in a forced circulation heat aging tester, and then the modulus at 500% elongation, tensile strength at break, and elongation at break were measured in accordance with JIS K 6251. A modulus at 500% elongation of 3.0 MPa or less, a tensile strength at break of 14 MPa or more, and an elongation at break of 900% or more were considered to be acceptable.
[0109] Example 16 Synthesis of (meth)acrylic block copolymer latexes by forced emulsification method (Polymerization step 1) Synthesis of polymer block (A-21) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 4616g of tetrahydrofuran, 87.5g of styrene monomer, and 1.5g of benzyl butyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 0.49g of azobisisobutyronitrile (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: AIBN) was added as a polymerization initiator to start polymerization. 20ml of the obtained solution was sampled for physical property measurement, and the remaining latex was used in the next polymerization step. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-19) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 3.
[0110] (Polymerization step 2) Synthesis of (meth)acrylic polymer block (B-21) After the polymerization step 1, when the internal temperature dropped to 45°C, 1120g of normal butyl acrylate monomer and 22.8g of 1,9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of the normal butyl acrylate monomer reached 80%, the polymerization was terminated by adding a 10% by mass tetrahydrofuran solution of phenothiazine, which is a polymerization terminator, and the unreacted normal butyl acrylate monomer and tetrahydrofuran were removed by reduced pressure distillation to obtain a (meth)acrylic block copolymer sample.
[0111] (Forced emulsification process) Forced emulsification of (meth)acrylic block copolymer 350 g of the (meth)acrylic block copolymer obtained in the polymerization step 2 was dissolved in 4200 g of benzene. 4725 g of pure water, 70 g of disproportionated potassium rosinate (manufactured by Harima Chemicals Co., Ltd.), 0.78 g of potassium hydroxide, and 1.4 g of sodium salt of β-naphthalenesulfonic acid formalin condensate (manufactured by Kao Corporation, product name: Demol N) were added to the obtained solution, and the mixture was forcedly emulsified using a homogenizer. Benzene and water were removed by distillation under reduced pressure so that the solid content concentration of the obtained latex was 50%, and a (meth)acrylic block copolymer latex was obtained. For physical property measurement, 20 ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The average particle size of the latex, the mechanical stability of the latex, the content (mass%) of the polymer block (A-21) and the (meth)acrylic polymer block (B-21) of the (meth)acrylic block copolymer, and the toluene insoluble content were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 3.
[0112] [Table 1] JPEG0007576157000006.jpg248154
[0113] [Table 2]
[0114]
Table 3
Claims
1. A (meth)acrylic block copolymer comprising a polymer block (A) and a (meth)acrylic polymer block (B), The (meth)acrylic block copolymer has the following properties when the (meth)acrylic block copolymer is taken as 100% by mass: The polymer block (A) is contained in an amount of 5 to 30% by mass, The (meth)acrylic polymer block (B) is contained in an amount of 70 to 95% by mass, The polymer block (A) contains a monomer unit derived from a monomer which, upon homopolymerization, gives a polymer having a glass transition temperature of 80° C. to 150° C., The polymer block (B) has a (meth)acrylic monomer unit and a polyfunctional monomer unit, The (meth)acrylic block copolymer is a (meth)acrylic block copolymer having a tensile strength at break of 14 MPa or more as measured in accordance with JIS K 6251 after a coating obtained by dip-molding a (meth)acrylic block copolymer latex containing the (meth)acrylic block copolymer is heat-treated at 130°C for 30 minutes (excluding those in which the polymer block (A) contains 30 to 99% by mass of monomer units derived from a maleimide compound).
2. A (meth)acrylic block copolymer comprising a polymer block (A) and a (meth)acrylic polymer block (B), The (meth)acrylic block copolymer has the following properties when the (meth)acrylic block copolymer is taken as 100% by mass: The polymer block (A) is contained in an amount of 5 to 30% by mass, The (meth)acrylic polymer block (B) is contained in an amount of 70 to 95% by mass, the polymer block (A) is composed of monomer units derived from a monomer which, upon homopolymerization, gives a polymer having a glass transition temperature of 80° C. to 150° C., The polymer block (B) has a (meth)acrylic monomer unit and a polyfunctional monomer unit, The (meth)acrylic block copolymer has a tensile strength at break of 14 MPa or more as measured in accordance with JIS K 6251 after a coating obtained by dip-molding a (meth)acrylic block copolymer latex containing the (meth)acrylic block copolymer is heat-treated at 130°C for 30 minutes.
3. 3. The (meth)acrylic block copolymer according to claim 1 or 2, wherein the polymer block (A) contains at least one monomer unit selected from the group consisting of an aromatic vinyl monomer unit, a methyl methacrylate monomer unit, and an acrylonitrile monomer unit.
4. The (meth)acrylic block copolymer according to any one of claims 1 to 3, wherein the polymer block (A) has a number average molecular weight of 10,000 or more.
5. The (meth)acrylic block copolymer according to any one of claims 1 to 4, wherein the (meth)acrylic polymer block (B) contains the polyfunctional monomer unit in an amount of 0.05 to 10% by mass, based on 100% by mass of the (meth)acrylic polymer block (B).
6. The (meth)acrylic block copolymer according to any one of claims 1 to 5, wherein the polyfunctional monomer comprises a monomer represented by chemical formula (1) or an aromatic polyene monomer. [Formula 1] (In chemical formula (1), R 1 and R 2 each independently represents hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, a mercapto group, or a substituted or unsubstituted heterocyclyl group. 1 represents a saturated or unsaturated hydrocarbon group, a saturated or unsaturated cyclic hydrocarbon group, or a saturated or unsaturated hydrocarbon group or cyclic hydrocarbon group containing a hetero atom. 1 is oxygen, sulfur or -NR 0 R represents a structure represented by the formula: 0represents any one of hydrogen, chlorine, a substituted or unsubstituted alkyl group, alkenyl group, aryl group, mercapto group, and heterocyclyl group.)
7. A (meth)acrylic block copolymer latex comprising the (meth)acrylic block copolymer according to any one of claims 1 to 6.
8. The (meth)acrylic block copolymer latex according to claim 7, wherein the (meth)acrylic block copolymer latex contains 20 to 100% by mass of a toluene-insoluble matter relative to 100% by mass of the (meth)acrylic block copolymer latex.
9. The (meth)acrylic block copolymer latex according to claim 7 or 8, wherein the (meth)acrylic block copolymer latex has an average particle size of 300 nm or less as measured by a dynamic light scattering method.
10. The (meth)acrylic block copolymer latex according to any one of claims 7 to 9, which is for use in a dip-molded product.
11. A (meth)acrylic block copolymer latex composition comprising the (meth)acrylic block copolymer latex according to any one of claims 7 to 10.
12. The (meth)acrylic block copolymer latex composition according to claim 11, wherein a total content of a vulcanizing agent and a vulcanization accelerator is 5 mass% or less when the (meth)acrylic block copolymer latex contained in the (meth)acrylic block copolymer latex composition is 100 mass%.
13. A molded article comprising the (meth)acrylic block copolymer latex composition according to claim 11 or 12.
Citation Information
Patent Citations
ABA type block copolymer with crosslinked structure
JP1991009914A
STAR COPOLYMER AND METHOD FOR MAKING THE SAME
JP1993500827A
Emulsion-type pressure-sensitive adhesive
JP2003155463A
Block copolymer, method for producing same, and use of same
WO2017073287A1
Triblock copolymer and method for producing triblock copolymer
WO2020145206A1