Grain-finish artificial leather and its manufacturing method
By forming controlled open pores in a fiber entangled base material with a wet polyurethane layer and applying top coats, the method addresses issues of air and water permeability, dirt accumulation, and abrasion resistance in silver-finished artificial leather, achieving high water resistance and breathability.
Patent Information
- Application Number
- JP2020204419
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-09
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-12-09
AI Technical Summary
Conventional silver-finished artificial leather faces issues with air permeability, water permeability, dirt accumulation, high processing costs, limited design freedom, and reduced abrasion resistance, especially when ventilation holes are formed using needles, lasers, or transfer papers.
A method involving a base material with a fiber entangled body and a wet polyurethane porous layer, where a controlled solvent is applied to form open pores, followed by a first top coat and embossing with a heated embossing roll to adjust pore size and number, then a second top coat is applied to maintain ventilation and enhance abrasion resistance.
The method results in silver-finished artificial leather with high water resistance, breathability, and abrasion resistance, effectively preventing rainwater penetration and reducing stuffiness while maintaining a smooth surface.
Smart Images

Figure 0007576448000002 
Figure 0007576448000003 
Figure 0007576448000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a grain-finished artificial leather comprising a substrate including a fiber-entangled body and a wet-type porous polyurethane layer, and a method for producing the same. [Background technology]
[0002] There is known a grain-finished artificial leather having a grain-finished appearance similar to natural leather, which is used as a surface material for bags, clothing, shoes, etc. As such a grain-finished artificial leather, there is known a grain-finished artificial leather comprising a substrate including a fiber entanglement body and a wet-type polyurethane porous layer. Such grain-finished artificial leather can be used for products that come into contact with the human body. Examples of such uses include clothing materials, shoe upper materials, and back lining materials for backpacks. It is required that grain-finished artificial leather used for such uses does not become stuffy when worn. Methods for producing such grain-finished artificial leather that does not become stuffy have been proposed in the past.
[0003] For example, a method has been proposed in which holes are mechanically made on the surface of grain-finished artificial leather using a needle to form ventilation holes. Specifically, the following Patent Document 1 discloses a grain-finished artificial leather comprising a leather-like sheet made of a fine long fiber nonwoven fabric and a polymeric elastomer impregnated therein, and a grain surface layer formed on at least one side of the leather-like sheet, in which 10 to 100 pinholes / cm2, each having a major axis of 30 to 100 μm and a minor axis of 3 to 5 μm, are formed by piercing the grain surface layer and the leather-like sheet with a needle. 2 The present invention discloses a pinhole-finished, grain-finished artificial leather having the above-mentioned properties and used for the back lining of a backpack.
[0004] Also proposed is a grain-finished artificial leather in which ventilation holes are formed by opening holes by laser processing in a resin layer on the surface layer that becomes the grain surface layer.Specifically, the following Patent Document 2 discloses a grain-finished artificial leather in which a coating made of a polymeric elastomer is present on a substrate made of fibers and a porous polymeric elastomer, in which holes are present that penetrate the coating, and pores are present on the inner walls of the holes that communicate with the inside of the substrate, and the fibers and the polymeric elastomer are fused on the inner walls of the holes.
[0005] Also, for example, a grain-finished artificial leather has been proposed in which a resin layer on the surface, which becomes the grain surface layer, is formed by fusing fibers to form ventilation holes. Specifically, the following Patent Document 3 discloses a method for manufacturing a leather having a grain-finished artificial leather, in which a polyurethane fiber having a basis weight of 5 to 125 g / m is attached to at least one surface of a base layer made of a fiber-entangled nonwoven fabric and an elastic polymer contained therein. 2 This invention also discloses a method for producing a leather-like sheet, which comprises temporarily fixing the nonwoven fabric of the above-mentioned type by point bonding with a polyurethane resin, and then heat-sealing the polyurethane fibers and laminating and integrating the nonwoven fabric with a substrate layer. This invention also discloses a leather-like sheet obtained by this production method, which comprises a substrate layer made of a fiber-entangled nonwoven fabric and an elastic polymer contained therein, on at least one surface of which a discontinuous polyurethane layer is present, and further comprises a heat-sealed layer of nonwoven fabric made of polyurethane fibers present thereon.
[0006] Furthermore, for example, Patent Document 4 listed below discloses a grained leather-like sheet structure in which a film layer having holes is formed using peelable transfer paper having an uneven surface, and such a film layer is adhered to a substrate as a surface layer that becomes a grained surface layer.
[0007] For example, Patent Document 5 below discloses a method for producing a grain-finished artificial leather by forming an interconnected porous polyurethane layer on one side of a substrate made of fibrous material and a polymer elastomer, and then forming a finish polyurethane coating on the surface of the layer, in which a good solvent, a poor solvent, a mixed solvent of a good solvent and a poor solvent, or a mixed solvent of a good solvent and a non-solvent for polyurethane is applied to the surface of the interconnected porous polyurethane layer with a gravure mesh roll to generate open pores having a diameter of 5 to 40 μm on the surface, and then a finish polyurethane coating is formed, and the open pores in the interconnected porous polyurethane layer are also expressed as open pores in the finish polyurethane coating. 2 There are 200 or more per pore, and a finishing polyurethane coating is formed so as to cover the pore walls of the open pores and reach into the interconnected porous polyurethane layer, and the air permeability is 0.5 liters / cm 2 hr or more, moisture permeability is 6mg / cm 2 The present invention discloses a grain-finished artificial leather having a hardness of 1.0 hr or more. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2011-214196 A [Patent Document 2] JP 2010-248644 A [Patent Document 3] JP 2000-265378 A [Patent Document 4] JP 2003-27381 A [Patent Document 5] Japanese Patent Application Publication No. 8-041786 Summary of the Invention [Problem to be solved by the invention]
[0009] In the conventional breathable grain-finished artificial leather described above, although the breathability is improved, water may penetrate during rainy weather, dirt may get into the pores and the leather may become dirty easily, it may be difficult to color, and the cost may be low.
[0010] For example, in the case of grain-finished artificial leather in which holes are made using a needle as disclosed in Patent Document 1, there is a problem that the holes are easily blocked after the needle penetrates, making it difficult to obtain sufficient breathability, and if the pinhole is made too large, water becomes easily permeable and the area around the pinhole is easily stained. Also, in the case of grain-finished artificial leather in which holes are made using laser processing as disclosed in Patent Document 2, there is a problem that the processing cost is high.
[0011] In addition, for example, in the case of grain-finished artificial leather in which ventilation holes are formed by fusing fibers to form a surface resin layer that becomes the grain surface layer, as disclosed in Patent Document 3, in order to color the grain surface layer, it is necessary to color the fused fibers, and the degree of freedom in coloring is low.
[0012] In addition, for example, in the case of a grain-finished leather-like sheet structure manufactured by forming a film layer having holes using a peelable transfer paper having an uneven surface shape, and adhering such a film layer to a substrate as a surface layer that becomes a grain surface layer, as disclosed in Patent Document 4 below, the shape of the holes formed is limited by the uneven surface shape of the peelable transfer paper, so that the types of surface unevenness are limited, resulting in a problem of reduced freedom of design.
[0013] In addition, for example, when a grain-finished artificial leather having ventilation holes is manufactured by applying a good solvent, a poor solvent, a mixed solvent of a good solvent and a poor solvent, or a mixed solvent of a good solvent and a non-solvent for polyurethane with a gravure mesh roll to generate open holes with a diameter of 5 to 40 μm on the surface as disclosed in the following Patent Document 5, it is difficult to uniformly apply a small amount of solvent because the viscosity of the applied solvent is low, and when a large amount of solvent is applied, open holes with a pore size that is too large are likely to be generated, and only a product with low water resistance is obtained. In addition, the surface applied with the solvent is easily roughened, so that the surface is easily soiled and the abrasion resistance is easily reduced.
[0014] The present invention aims to provide a grain-finished artificial leather having a wet-processed polyurethane porous layer forming a grain surface layer, which has continuous open pores with a controlled pore size and number, thereby providing high water resistance that makes it difficult for rainwater to pass through, and breathability and abrasion resistance that appropriately suppress stuffiness. [Means for solving the problem]
[0015] As a result of various investigations, the present inventors have found that in the production of grain-finished artificial leather comprising a substrate including a fiber-entangled body, a wet-type polyurethane porous layer, and a top coat, if a solvent is simply applied to form air holes in the wet-type polyurethane porous layer and then a top coat is formed thereon in order to form open pores in the surface of the wet-type polyurethane porous layer, the size and number of the air hole openings cannot be controlled, and therefore, although breathability is obtained, a grain-finished artificial leather having high water resistance cannot be obtained.
[0016] In order to solve the above problems, the present inventors have discovered that a first top coat can be formed while forming continuous open pores whose size and number are controlled by applying a polyurethane solution containing a solvent that has high solubility in polyurethane to the surface of a wet polyurethane porous layer, thereby making it difficult for the solvent to penetrate into the wet polyurethane porous layer, and then embossing the surface of the first top coat with a heated embossing roll having a texture, thereby appropriately closing the formed continuous open pores, thereby controlling the size and number of the openings and eliminating surface roughness, and further applying a polyurethane solution containing a solvent that has low solubility in polyurethane to the surface of the embossed first top coat to form a second top coat without enlarging the openings, thereby obtaining a grain-finished artificial leather that combines high water resistance that makes it difficult for rainwater to pass through, and breathability and abrasion resistance that appropriately suppress stuffiness, thereby preventing stuffiness. This has led to the invention.
[0017] That is, one aspect of the present invention is a method for producing a substrate including a fiber entanglement and a wet-type polyurethane porous layer impregnated and laminated to the fiber entanglement, and forming a polyurethane porous layer on a surface of the wet-type polyurethane porous layer. , 1st Po The method comprises the steps of: gravure-coating a first polyurethane solution in which a recarbonate-based polyurethane is dissolved, dissolving the wet polyurethane porous layer to form open pores communicating in the thickness direction, and then drying the layer to form a first top coat; embossing the first top coat with a heated embossing roll having texture; and applying a pattern to the surface of the embossed first top coat. The second polyurethane includes a silicone-modified polycarbonate-based polyurethane. and a step of gravure-coating a second polyurethane solution in which a recarbonate-based polyurethane is dissolved, and then drying to form a second top coat, wherein the total thickness of the first top coat and the second top coat is 1 to 5 μm. The first polyurethane solution contains a mixed solvent containing 50 to 80% by mass of N,N-dimethylformamide and 20 to 50% by mass of cyclohexanone, and has a concentration of a first polycarbonate-based polyurethane of 5 to 10% by mass, a Zahn cup viscosity at 20°C of 10 to 40 seconds, and a viscosity of 20 to 60 g / m 2 The second polyurethane solution contains a mixed solvent containing 10 to 40 mass% of N,N-dimethylformamide, 25 to 35 mass% of cyclohexanone, and 20 to 40 mass% of acetone, and the concentration of the second polycarbonate-based polyurethane is 5 to 10 mass%, the Zahn cup viscosity at 20°C is 10 to 40 seconds, and the viscosity is 20 to 60 g / m 2 The coating amount was 100g, and the water resistance (hereinafter referred to simply as water resistance) measured in accordance with the water resistance test (hydrostatic pressure method) A method of JIS L 1092 (2009) "Waterproof test method for textile products" was 100g. 000mm or more The above is the permeability measured according to the method specified in JIS L 1096 (2010) "Testing method for woven and knitted fabrics" Method A (Fragile method). air (hereinafter simply referred to as breathability) is 0 .10cm 3 / cm 2This is a method for producing a grain-finished artificial leather in which the opening diameter and number of the holes are adjusted in each process so that the opening diameter and number of the holes are equal to or greater than 1 / 1000. According to this method for producing a grain-finished artificial leather, the first polyurethane solution is gravure-coated on the surface of the wet polyurethane porous layer, and the wet polyurethane porous layer is appropriately dissolved in a solvent to form open holes that communicate from the front surface to the back surface. Furthermore, by embossing the surface of the first top coat with a heated embossing roll having texture, some of the openings are blocked or made smaller, and large openings that reduce water resistance are blocked while an appropriate number of small openings that maintain breathability are left. Furthermore, the surface of the wet polyurethane porous layer is smoothed by embossing, so that the abrasion resistance is less likely to decrease. Then, by forming the second top coat without widening the openings, the surface becomes smooth, so that high abrasion resistance can be maintained, and openings that maintain high water resistance and are less likely to seep in during rainy weather can be left. Specifically, the water resistance of the obtained grain-finished artificial leather is 1000 mm or more, and the breathability is 0.1 cm. 3 / cm 2 The grain-finished artificial leather can be obtained by adjusting the opening diameter and number so that the opening diameter and number are equal to or more than s. As a result, the grain-finished artificial leather can be obtained which has high water resistance, breathability that appropriately suppresses stuffiness, and abrasion resistance.
[0018] In addition, the first polyurethane solvent The liquid, The polyurethane contains a mixed solvent containing 50 to 80% by mass of N,N-dimethylformamide and 20 to 50% by mass of cyclohexanone, has a concentration of 5 to 10% by mass, has a Zahn cup viscosity at 20°C of 10 to 40 seconds, and is 20 to 60 g / m 2 The second polyurethane solution contains a mixed solvent containing 10 to 40 mass% of N,N-dimethylformamide, 25 to 35 mass% of cyclohexanone, and 20 to 40 mass% of acetone, and the concentration of the second polyurethane is 5 to 10 mass%, the Zahn cup viscosity at 20°C is 10 to 40 seconds, and the viscosity is 20 to 60 g / m 2 This is applied in an amount of According toThe solvent contained in the first polyurethane solution forms an adequate number of interconnected open pores in the wet polyurethane porous layer, and the solvent contained in the second polyurethane solution does not dissolve the wet polyurethane porous layer too much, resulting in a grain-finished artificial leather having a top coat layer of an adequate thickness and in which the diameter and number of the interconnected open pores are adjusted as described above.
[0019] Another aspect of the present invention is a sheet-like material comprising: a fiber-entangled body; a wet-type polyurethane porous layer impregnated and laminated with the fiber-entangled body to be integrated; and a top coat having a thickness of 1 to 5 μm and containing a polycarbonate-based polyurethane. A grain-finished artificial leather having a grain-finished texture, Top Cor The material contains silicone modified polycarbonate polyurethane. The surface is grained and has open pores that communicate from the surface to the back surface of the wet polyurethane porous layer. , surface 1cm 2 The number of openings with a major axis of 0.5 μm or more and 40 μm or less per unit area is 100 or more and less than 200, the number of openings with a major axis of more than 20 μm and 40 μm or less per unit area is less than 20, and the number of openings with a major axis of more than 40 μm is 0. water Degree 1 000mm or more Above, and Ventilation Sex is 0 .10cm 3 / cm 2 Such grain-finished artificial leather has high water resistance, breathability that appropriately suppresses stuffiness, and abrasion resistance. Effect of the Invention
[0021] According to the present invention, a grain-finished artificial leather having a wet-type polyurethane porous layer forming a grain surface layer is obtained, which has high water resistance, breathability that appropriately suppresses stuffiness, and abrasion resistance. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a schematic cross-sectional view of a grain-finished artificial leather 10 according to an embodiment. [Diagram 2] FIG. 2 is a photograph of the surface of the wet-type polyurethane porous layer of the grain-finished artificial leather obtained in Example 1, observed under a microscope at 45 times magnification. [Diagram 3]FIG. 3 is a photograph of the surface of the wet-processed polyurethane porous layer of the grain-finished artificial leather obtained in Comparative Example 1, observed under a microscope at 45 times magnification. [Figure 4] FIG. 4 is a photograph of the surface of the wet-processed polyurethane porous layer of the grain-finished artificial leather obtained in Comparative Example 2, observed under a microscope at 100 times. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, one embodiment of the grain-finished artificial leather according to the present invention will be described. The grain-finished artificial leather of this embodiment comprises a fiber entanglement body, a wet-type polyurethane porous layer impregnated and laminated with the fiber entanglement body to be integrated, and a top coat having a thickness of 1 to 5 μm containing a polycarbonate-based polyurethane. The material contains silicone modified polycarbonate polyurethane. The surface is grained and has open pores that communicate from the surface to the back surface of the wet polyurethane porous layer. , surface 1cm 2 The number of openings with a major axis of 0.5 μm or more and 40 μm or less per unit area is 100 or more and less than 200, the number of openings with a major axis of more than 20 μm and 40 μm or less per unit area is less than 20, and the number of openings with a major axis of more than 40 μm is 0. Water resistance of 1000mm or more and breathability of 0.10cm 3 / cm 2 The grain-finished artificial leather of this embodiment is described in detail below with reference to the drawings and a representative production method thereof.
[0024] FIG. 1 shows a schematic cross-sectional view of a grain-finished artificial leather 10. In FIG. 1, 1 is a fiber-entangled body, 2 is a wet polyurethane porous layer impregnated and laminated on the fiber-entangled body 1, and 3 is a polyurethane top coat laminated on the wet polyurethane porous layer. The wet polyurethane porous layer 2 includes a grain surface layer 2a that is not integrated with the fiber-entangled body 1 in the wet polyurethane porous layer 2 and is laminated on the surface of the fiber-entangled body 1, and an impregnated layer 2b that is impregnated into the fiber-entangled body 1 and is integrated with the fiber-entangled body 1 in the wet polyurethane porous layer 2. The wet polyurethane porous layer 2 includes voids v that form a porous structure. A top coat 3 containing a polycarbonate-based polyurethane and having a thickness of 1 to 5 μm is further laminated on the surface of the wet polyurethane porous layer 2. The grain-finished artificial leather 10 includes open holes h that communicate from the front surface to the back surface of the wet polyurethane porous layer 2 and open to the surfaces of the wet polyurethane porous layer 2 and the top coat 3. The outer surface of the grain-finished artificial leather is embossed with an embossing roll (not shown).
[0025] A method for producing the grain-finished artificial leather according to this embodiment will be described below.
[0026] In the method for producing the grain-finished artificial leather of this embodiment, first, a substrate is prepared that includes a fiber-entangled body and a wet-processed polyurethane porous layer that is impregnated with, laminated on, and integrated with the fiber-entangled body.
[0027] The fiber structure of the entangled fiber body is not particularly limited, and examples thereof include nonwoven fabric, woven fabric, knitted fabric, and an entangled body of a combination thereof, and preferably includes nonwoven fabric, or an entangled body of a nonwoven fabric and a woven fabric.
[0028] The resin forming the fiber entanglement is not particularly limited. Specifically, for example, polyamide resins such as polyamide 6, polyamide 66, polyamide 610, polyamide 10, polyamide 11, polyamide 12, and polyamide 6-12; aromatic polyester resins such as polyethylene terephthalate (PET), modified polyethylene terephthalate, polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polytriethylene terephthalate, polyhexamethylene terephthalate, polypropylene terephthalate, and polyethylene naphthalate; polylactic acid, polyethylene succinate, polybutylene succinate, and polybutylene terephthalate; Examples of the resin include polyester resins such as aliphatic polyester resins such as succinate adipate and polyhydroxybutyrate-polyhydroxyvalerate copolymers; polyolefin resins such as polypropylene, polyethylene, polybutene, polymethylpentene, chlorine-based polyolefins, ethylene-vinyl acetate copolymers, and styrene-ethylene copolymers; modified polyvinyl alcohol resins formed from modified polyvinyl alcohols containing 25 to 70 mol % of ethylene units; and crystalline elastomers such as polyurethane elastomers, polyamide elastomers, and polyester elastomers. Among these, polyamide resins and aromatic polyester resins are preferred because of their excellent balance of various properties.
[0029] The fiber fineness and form are not particularly limited. For example, the fiber may be a regular fiber having an average fineness of more than 1 dtex, or an ultrafine fiber having an average fineness of less than 1 dtex. The fiber form may be a solid fiber or a fiber having voids such as a hollow fiber or a lotus root-like fiber. Among these, ultrafine fibers having an average fineness of 0.0001 to 0.1 dtex are preferred because they provide an excellent balance between the texture such as flexibility and durability. The average fineness is calculated as an average value calculated using the density of the resin forming the fiber from 15 uniformly selected fiber diameters by photographing a cross section parallel to the thickness direction of the grain-finished artificial leather at 3000 times magnification using a scanning electron microscope (SEM).
[0030] The thickness of the fiber-entangled body is not particularly limited, but is preferably, for example, about 0.3 to 3 mm, and more preferably about 0.5 to 1.5 mm.
[0031] The substrate includes a fiber-entangled body and a wet-type porous polyurethane layer that is impregnated with and laminated on the fiber-entangled body to form an integrated structure. Such a substrate can be obtained, for example, by impregnating a fiber-entangled body with a polyurethane solution that undergoes wet coagulation (hereinafter referred to as a wet-coagulating polyurethane solution), applying the same wet-coagulating polyurethane solution to the surface of the fiber-entangled body, and then immersing the fiber-entangled body in an aqueous coagulating liquid such as water or a mixed solvent of water and DMF to wet-coagulate the porous polyurethane.
[0032] Specific examples of polyurethanes contained in the wet coagulation polyurethane solution include polyester glycol-based polyurethanes having polyethylene adipate, polybutylene adipate, polypropylene adipate, polyhexamethylene adipate, polycaprolactone, polymethylvalerolactone, or the like as a polyol component, polypropylene glycol-based polyurethanes, polytetramethylene glycol-based polyurethanes, polycarbonate-based polyurethanes, and polytetramethylene glycol-polycarbonate copolymer-based polyurethanes.
[0033] In addition, examples of the solvent contained in the wet coagulation polyurethane solution include mixed solvents that have high solubility in polyurethane, such as N,N-dimethylformamide (DMF) and water as the main components, and, as necessary, cyclohexanone (CHN), tetrahydrofuran (THF), methyl ethyl ketone (MEK), acetone (Ac), dioxane, isopropyl alcohol, toluene, etc.
[0034] The wet-coagulated polyurethane solution may contain additives such as a coagulation regulator, an antioxidant, a light resistance agent, and an antibacterial agent, in addition to a colorant such as a pigment.
[0035] In the substrate, the fiber-entangled body is impregnated in advance with a wet-coagulating polyurethane solution, and the wet-coagulating polyurethane solution is then applied to the surface of the fiber-entangled body, which is then immersed in the coagulating liquid to coagulate, thereby forming a polyurethane porous layer that is impregnated into and laminated onto the fiber-entangled body and is integrated therewith, the polyurethane porous layer including an impregnated layer that is impregnated into the interior of the fiber-entangled body and is integrated with the fiber-entangled body, and an area that becomes a grain surface layer in which porous polyurethane is laminated alone on the surface of the fiber-entangled body.
[0036] The polyurethane porous layer may have a single layer structure formed from the same polyurethane, or may have a multi-layer structure in which different types of polyurethane are coated in layers and then coagulated by immersion in a coagulating liquid.
[0037] The total thickness of the wet polyurethane porous layer is preferably 100 to 600 μm, more preferably 200 to 400 μm. The thickness of the region of the wet polyurethane porous layer that becomes the grain surface layer laminated on the surface is preferably 50 to 500 μm, more preferably 100 to 300 μm. The total thickness of the substrate is preferably 800 to 3000 μm, more preferably 1200 to 2000 μm.
[0038] The mass ratio of the fiber entanglement and the wet polyurethane porous layer constituting the grain-finished artificial leather (fiber entanglement / wet polyurethane porous layer) is preferably 40 / 60 to 70 / 30, more preferably 50 / 50 to 60 / 40, in terms of a good balance between texture and shape stability. If the ratio of the wet polyurethane porous layer is too high, the texture tends to be rubber-like, and if the ratio of the fiber entanglement is too high, the shape stability tends to decrease.
[0039] Next, a first polyurethane solution in which a polycarbonate-based polyurethane is dissolved is gravure-coated onto the surface of the wet polyurethane porous layer of the substrate thus prepared, dissolving the wet polyurethane porous layer to form open pores that communicate in the thickness direction, and then drying to form a first top coat. By applying the first polyurethane solution and dissolving the wet polyurethane porous layer with the solvent contained in the first polyurethane solution, it is possible to generate open pores that communicate from the front surface to the back surface.
[0040] The first polyurethane solution contains a solvent that has high solubility for polyurethane and the first polyurethane.
[0041] Examples of solvents that have high solubility in polyurethane include solvents that are mainly N,N-dimethylformamide (DMF, boiling point 153° C.) and, if necessary, are mixed with solvents such as cyclohexanone (CHN, boiling point 156° C.), tetrahydrofuran (THF, boiling point 66° C.), methyl ethyl ketone (MEK, boiling point 80° C.), dioxane (boiling point 101° C.), toluene (boiling point 111° C.), and isopropyl alcohol (IPA, boiling point 124° C.) to adjust the solubility. Among these, a mixed solvent containing DMF and CHN, specifically, a mixed solvent containing 50 to 80 mass %, or even 60 to 70 mass %, DMF, 20 to 50 mass %, or even 25 to 40 mass %, and other polar solvents such as THF as the remainder, is preferred because it is easy to adjust the pore size and number to an appropriate value. In addition, CHN has a boiling point close to that of DMF and is more soluble in polyurethane than DMF. Therefore, CHN contributes to making it difficult for large openings to form by suppressing the rapid evaporation of DMF during drying, which would otherwise cause the polyurethane to rapidly form a film.
[0042] The first polyurethane is blended as a thickener for forming the first top coat and for increasing the solution viscosity of the first polyurethane solution. The first polyurethane includes polycarbonate polyurethanes such as polycarbonate polyurethane, silicone-modified polycarbonate polyurethane, and polytetramethylene glycol-polycarbonate copolymer polyurethane in order to form a first top coat having high abrasion resistance. Silicone-modified polycarbonate polyurethane is preferably used because of its particularly excellent abrasion resistance.
[0043] The first polyurethane solution may contain additives such as antioxidants, light resistance agents, and antibacterial agents, in addition to colorants such as pigments.
[0044] The Zahn cup viscosity of the first polyurethane solution is preferably 10 to 40 seconds, more preferably 15 to 35 seconds, and particularly preferably 20 to 30 seconds. If the Zahn cup viscosity of the first polyurethane solution is too low, it becomes difficult to apply a small amount of the solution uniformly by gravure coating, and the interconnected open pores having a large opening diameter tend to be formed non-uniformly, resulting in a low water resistance. If the Zahn cup viscosity of the first polyurethane solution is too high, the viscosity becomes too high and it becomes difficult to apply a small amount of the solution uniformly by gravure coating, and the solution is also difficult to penetrate into the wet polyurethane porous layer, resulting in a tendency to make it difficult to form sufficient interconnected open pores.
[0045] The concentration of the first polyurethane in the first polyurethane solution is preferably 5 to 10% by mass, more preferably 6 to 9% by mass, and particularly preferably 7 to 8% by mass. If the concentration of the first polyurethane is too low, the first polyurethane solution cannot be adequately thickened, and non-uniform interconnected open pores with large variations in opening size are likely to be formed. If the concentration is too high, the viscosity of the first polyurethane solution becomes too high, making it difficult for the solution to penetrate into the wet polyurethane porous layer, and making it difficult to form sufficient interconnected open pores.
[0046] The first polyurethane solution is applied to the surface of the wet-type porous polyurethane layer using a gravure roll. The gravure roll preferably has cells engraved on its surface with a mesh size of 65 to 180, more preferably 100 to 130, from the viewpoint of uniform application of an appropriate amount of the first polyurethane solution.
[0047] The amount of the first polyurethane applied is 20 to 60 g / m 2 , and even 30 to 50 g / m 2 , especially 35~45g / m 2 By applying the first polyurethane solution to the surface of the wet polyurethane porous layer in such an amount, the wet polyurethane porous layer is dissolved in the solvent in the first polyurethane solution, and continuous open pores are formed that connect the front surface to the back surface of the wet polyurethane porous layer. The solvent is then dried to form a first top coat having openings of continuous open pores. The drying conditions are appropriately adjusted depending on the type of solvent, etc., but for example, drying conditions in a hot air dryer set at 100 to 120°C for 5 to 30 seconds or until the remaining amount of DMF is about 100 to 10,000 ppm are preferred.
[0048] The thickness of the first top coat thus formed is preferably about 1 to 3 μm. The openings on the surface of the first top coat are preferably 1 cm2 or less. 2 It is preferable that the number of openings having a major axis of 0.5 μm or more and 20 μm or less is 1000 to 3000, the number of openings having a major axis of more than 20 μm and 40 μm or less is 100 to 500, and the number of openings exceeding 40 μm is 200 or less per unit area, from the viewpoint of easily obtaining a grain-finished artificial leather having openings of the size and number described below.
[0049] Next, the surface of the formed first topcoat is embossed with a heated embossing roll. By embossing in this manner, the openings in the surface of the first topcoat are deformed by embossing, large openings are blocked, and small openings tend to remain. In addition, the surface of the first topcoat becomes smooth.
[0050] The shape of the embossing roll is not particularly limited, but an embossing roll with a height difference of about 20 to 100 μm is preferably used. The surface temperature of the embossing roll is appropriately selected so that the shape of the embossing can be properly transferred and small openings tend to remain. Specifically, for example, it is preferably 150 to 190° C., more preferably 160 to 180° C. If the surface temperature of the embossing roll is too high, the openings tend to be too blocked or the overall texture tends to be hard. If the surface temperature of the embossing roll is too low, the shape of the embossing cannot be properly transferred or large openings tend to be difficult to block.
[0051] The opening of the surface of the first top coat embossed by the embossing roll is 1 cm 2 It is preferable that the number of openings having a major axis of 0.5 μm or more and 20 μm or less is 100 to 500, the number of openings having a major axis of more than 20 μm and 40 μm or less is 10 to 100, and the number of openings exceeding 40 μm is 10 or less per one piece, from the viewpoint of easily obtaining a grain-finished artificial leather having openings of the size and number described below.
[0052] In the production of the grain-finished artificial leather of this embodiment, the embossed surface of the first top coat is The second polyurethane includes a silicone-modified polycarbonate-based polyurethane. A second polyurethane solution in which a recarbonate-based polyurethane is dissolved is gravure coated and then dried to form a second top coat.
[0053] The solvent contained in the second polyurethane solution is preferably lower in solubility for polyurethane than the solvent contained in the first polyurethane solution. As the solvent contained in the second polyurethane solution, for example, a solvent mainly containing DMF and mixed with a polar solvent such as cyclohexanone (CHN), tetrahydrofuran (THF), dioxane, isopropyl alcohol, etc., and a ketone such as acetone (Ac) or methyl ethyl ketone (MEK) is preferably used in order to adjust the solubility as necessary. Among them, a mixed solvent of DMF, CHN, and Ac, specifically, a mixed solvent of DMF, CHN, and Ac, in which DMF is 10 to 40 mass%, or more preferably 15 to 35 mass%, CHN is 25 to 35 mass%, or more preferably 30 to 35 mass%, and Ac is 20 to 40 mass%, or more preferably 25 to 35 mass%, and the remainder may contain other solvents such as THF or MEK, is preferred in terms of ease of adjusting the openings to an appropriate diameter and number.
[0054] The second polyurethane forms the second top coat, closes large openings, and makes it easier for small openings to remain appropriately. As the second polyurethane forming the second top coat, polycarbonate polyurethanes such as polycarbonate polyurethane, silicone-modified polycarbonate polyurethane, and polytetramethylene glycol-polycarbonate copolymer polyurethane are used because of their excellent abrasion resistance. In addition, silicone-modified polycarbonate polyurethanes are used because of their particularly excellent abrasion resistance. Includes
[0055] The second polyurethane solution may also contain additives such as antioxidants, light resistance agents, antibacterial agents, water and oil repellents, as well as colorants such as pigments.
[0056] The Zahn cup viscosity of the second polyurethane solution is preferably 10 to 40 seconds, more preferably 15 to 25 seconds. If the Zahn cup viscosity of the second polyurethane solution is too low, the viscosity is too low and the liquid is not transferred uniformly, so that a top coat of sufficient thickness is not formed. If the Zahn cup viscosity is too high, the top coat tends to become a continuous film, and the openings tend to be blocked too much.
[0057] In order to adjust the second polyurethane solution to have such a solution viscosity, the concentration of the second polyurethane in the second polyurethane solution is preferably 5 to 10 mass%, more preferably 6 to 9 mass%, and particularly preferably 7 to 8 mass%. If the concentration of the second polyurethane is too low, a top coat of sufficient thickness will not be formed, whereas if it is too high, the top coat will tend to become a continuous film and the openings will tend to be blocked too much.
[0058] The second polyurethane solution is applied to the surface of the first top coat using a gravure roll. The gravure roll preferably has cells engraved on its surface with a size of 65 to 180 mesh, more preferably 100 to 130 mesh, from the viewpoint of being able to uniformly apply an appropriate amount of the second polyurethane solution.
[0059] The amount of the second polyurethane solution applied is 20 to 60 g / m 2 , and even 30 to 50 g / m 2 , especially 35~45g / m 2 If the amount of the second polyurethane solution applied is too large, the topcoat tends to become a continuous film and the openings tend to be blocked, and if the amount of the second polyurethane solution applied is too small, the topcoat tends not to be formed with sufficient thickness. Then, by drying the solvent, a second topcoat with appropriate openings remaining is formed. The drying conditions are appropriately adjusted depending on the type of solvent, etc., but for example, the conditions of drying in a hot air dryer set at 100 to 120°C for 5 to 30 seconds or until the remaining amount of DMF is 3000 ppm or less are preferred.
[0060] In this way, a second topcoat is formed on the surface of the first topcoat that has been embossed by the embossing roll. The thickness of the second topcoat is preferably about 1 to 3 μm.
[0061] Furthermore, the total thickness of the first top coat and the second top coat is 1 to 5 μm, and preferably 2 to 4 μm. If the layer thickness of the top coat including the first top coat and the second top coat is less than 1 μm, the effect of improving abrasion resistance becomes insufficient, and if it exceeds 5 μm, water resistance and breathability decrease, the texture becomes hard, and bending resistance becomes poor.
[0062] The grain-finished artificial leather of the present embodiment can be obtained by the above-described manufacturing method. The grain-finished artificial leather obtained by the above-described manufacturing method has both high water resistance and breathability that appropriately suppresses stuffiness.
[0063] Specifically, the water resistance of the grain-finished artificial leather of this embodiment is preferably 1000 mm or more in the water resistance test described below, from the viewpoint of maintaining high water resistance.
[0064] The grain-finished artificial leather of the present embodiment has a breathability of 0.1 cm in a breathability test described later. 3 / cm 2 ·s or more, even 0.3cm 3 / cm 2 In the case of use in products that come into contact with the human body, it is preferable that the thickness be 1.0 s or more, since this can suppress stuffiness.
[0065] Such grain-finished artificial leather has open pores on the surface that are open and communicate from the surface to the back surface. The openings on the surface of the wet-processed polyurethane porous layer of the grain-finished artificial leather or on the surface of the top coat formed as required are within 1 cm2 of the surface. 2 The number of openings with a major axis of 0.5 μm to 40 μm is less than 200 per unit, and 0 or more 200 Less than one There are less than 20 openings with a major axis of more than 20 μm and less than 40 μm, and 0 or more 2 0 Less than one and preferably the number of openings larger than 40 μm is 0.
[0066] The grain-finished artificial leather of the present embodiment described above is preferably used as the outer material of products that come into contact with the human body, such as clothing materials, shoe upper materials, and back lining materials for backpacks. EXAMPLES
[0067] The present invention will be described in more detail below with reference to examples, although the scope of the present invention is not limited to these examples in any way.
[0068] First, the evaluation methods of the present embodiment will be described.
[0069] (Water resistance) The water resistance test was conducted according to the method specified in the Water Resistance Test (Hydrostatic Pressure Method) Method A of JIS L 1092 (2009) "Waterproof Test Method for Textile Products". Specifically, five test pieces were cut to 150 mm x 150 mm from the grain-finished artificial leather. Then, in an atmosphere of room temperature 23°C and relative humidity 65%, the test pieces were attached to a specified water resistance test device so that the front side of the test pieces were exposed to water, and the water in the leveling device was raised at a rate of 600 mm / min ± 30 mm / min, and the water level was measured in mm when water came out from three places on the back side of the test pieces. This water resistance (mm) measurement was conducted five times, and the average value was regarded as the water resistance of the grain-finished artificial leather.
[0070] (Breathability) The air permeability test was carried out according to the method stipulated in the Air Permeability A Method (Fragile Method) of JIS L 1096 (2010) "Testing Methods for Woven and Knitted Fabrics". Specifically, five test pieces were cut to 200 mm x 200 mm from the grain-finished artificial leather. Then, in an atmosphere of room temperature 23°C and relative humidity 65%, the test pieces were attached to one end of the cylinder of a specified testing machine, and the intake fan and air holes were adjusted using a rheostat so that the inclined barometer indicated a pressure of 125 Pa, and the pressure indicated by the vertical barometer at that time was measured. From the measured pressure and the type of air hole used, the volume of air (cm3) passing through the test piece was calculated using the conversion table attached to the testing machine. 3 / cm 2 s) was calculated. The average value of the five test results was then calculated.
[0071] (Measurement of Zahn cup viscosity of polyurethane solution) Zahn cup viscosity at 20° C. was measured using Zahn cup No. 4 in accordance with ASTM D4212. The average value of the results of three measurements was regarded as the Zahn cup viscosity of the polyurethane solution.
[0072] (Topcoat thickness) An arbitrary cross section parallel to the thickness direction of the grain-finished artificial leather was observed with a SEM at 300x magnification. The film thickness of the topcoat was then measured at 10 randomly selected points, and the average value was calculated.
[0073] (Taber abrasion) A test piece was prepared by attaching double-sided tape to the back surface of the grain-finished artificial leather and cutting it into a circle with a diameter of 10.6 cm, and then weighed precisely on a specified balance. Next, the test piece was set on a turntable and attached to the vertical drive shaft of a Taber abrasion tester. Then, an arm equipped with an abrasion wheel (H-22 (manufactured by Daito Electron Co., Ltd.)) was lowered onto the measurement surface, and the grain-finished artificial leather was abraded under the conditions of a load of 500 g and a rotation speed of 1000 times. After abrasion up to 1000 rotations, the test piece was removed, the abrasion debris attached to the test piece was thoroughly removed with a brush, and the test piece was weighed precisely on a specified balance, and the abrasion loss (mg) was measured. The abrasion loss was calculated as the difference in weight before and after abrasion. The average value of the results of three measurements was taken as the abrasion loss of the grain-finished artificial leather.
[0074] (Measurement of the number of openings) The surface of the grain-finished artificial leather was photographed at three random locations with a scanning electron microscope at a magnification of 40 to 50 times, with an area of 5 to 8 mm 2 Photograph so that the number of openings is counted, and the total of the three locations is 1 cm 2 The results were converted into numbers per person.
[0075] [Example 1] 50 parts by mass of polyethylene (sea component) and 50 parts by mass of polyamide 6 (island component) were melt spun in the same melt system to produce islands-in-sea type composite fibers with a fineness of 15 dtex. The islands-in-sea type composite fibers were then stretched 2.5 times, crimped, and cut into staple fibers with a fiber length of 51 mm. The staple fibers were then opened by a card and a fiber web was formed by a cross-wrapper weber. The fiber webs were cross-wrapped, overlapped, and needle-punched for entanglement, resulting in a fiber weight of 650 g / m. 2 As a result, a fiber entanglement was obtained.
[0076] The fiber entanglement was then impregnated with a 13% dimethylformamide (DMF) solution of polyester polyurethane. The polyester polyurethane is a copolymer of polyethylene propylene adipate, 4,4'-diphenylmethane diisocyanate (MDI) and ethylene glycol (EG), and has a 100% modulus of 100 kg / cm. 2 Immediately after that, a 26% DMF solution of the same polyester polyurethane was applied to the surface of the fiber entanglement at 40 g / m 2 Then, 75 g / m of a 20% DMF solution of polycarbonate-based polyurethane was applied to the upper surface. 2 The main components of the polycarbonate polyurethane are polyhexacarbonate glycol, polymethylene propylene adipate, and methylene diamine, and it is a copolymer further copolymerized with n-hexane diisocyanate, MDI, and EG. The 100% modulus is 40 kg / cm 2 The material was a polycarbonate-based polyurethane.
[0077] The fiber entanglement impregnated or coated with each polyurethane was then immersed in a coagulation bath (40°C) of DMF / water = 30 / 70 for 30 minutes to coagulate each polyurethane into a porous form, and then washed with water. The polyethylene in the islands-in-the-sea composite fiber was then extracted and removed with toluene to convert it into ultrafine fibers. In this way, a substrate having a thickness of 1.6 mm was obtained, which included an entanglement of fiber bundles of ultrafine fibers of polyamide 6 with an average fineness of 0.01 dtex and a porous wet polyurethane porous layer. The total thickness of the wet polyurethane porous layer was 250 μm.
[0078] On the other hand, a polyurethane solution containing a mixed solvent of N,N-dimethylformamide (DMF), cyclohexanone (CHN), and tetrahydrofuran (THF) in a mass ratio of 70 / 25 / 5 (DMF / CHN / THF), a concentration of the first polyurethane of 7.5 mass%, and a pigment content of 5 mass% in the solid content was prepared as the first polyurethane solution. The Zahn cup viscosity of the first polyurethane solution was 20 seconds. The first polyurethane was a polycarbonate-based polyurethane with a 100% modulus of 9 MPa.
[0079] In addition, a polyurethane solution containing a mixed solvent containing DMF, CHN, and acetone (Ac) in a mass ratio of 30 / 35 / 35 (DMF / CHN / Ac) and a concentration of the second polyurethane of 7.3 mass% was prepared as a second polyurethane solution. The Zahn cup viscosity of the second polyurethane solution was 15 seconds. The second polyurethane was a silicone-modified polycarbonate-based polyurethane with a 100% modulus of 5 MPa.
[0080] The first polyurethane solution was applied to the surface of the porous polyurethane of the substrate at 40 g / m 2 The coating amount was applied using a 110 mesh gravure roll, and the coating was dried by passing through a hot air dryer at 110° C. and a speed of 8 m / min for about 10 seconds. In this way, a first top coat was formed.
[0081] Then, the surface of the first top coat after drying was pressed with an embossing roll having a hair-like texture at a roll temperature of 170°C and a pressing pressure of 6 kg / cm. 2 The embossing was performed at a processing speed of 2 m / min.
[0082] Then, the second polyurethane solution was applied to the embossed surface of the first top coat at a rate of 40 g / m 2 The coating amount was applied with a 110 mesh gravure roll, and the coating was dried by passing through a hot air dryer at 110° C. and a speed of 8 m / min for about 10 seconds. In this way, a second top coat was formed.
[0083] In this way, grain-finished artificial leather was obtained. It was evaluated according to the above-mentioned evaluation method. The results are shown in Table 1.
[0084] [Table 1]
[0085] [Example 2] A grain-finished artificial leather was produced in the same manner as in Example 1, except that the formation of the top coat was changed as follows. A first polyurethane solution was prepared in which the concentration of the first polyurethane was changed to 9% by mass, and the concentration of the pigment in the solid content was changed to 8% by mass. The Zahncup viscosity of the first polyurethane solution was 23 seconds. The first polyurethane was a polycarbonate-based polyurethane with a 100% modulus of 9 MPa. Then, the first polyurethane solution was applied at 50 g / m2 onto the surface of the porous polyurethane of the substrate. 2 The coating amount was applied with a 110 mesh gravure roll, and the mixture was dried for about 10 seconds in a hot air dryer at 110°C and a speed of 8 m / min. In this way, a first top coat was formed. Then, grain-finished artificial leather was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0086] [Example 3] A grain-finished artificial leather was produced in the same manner as in Example 1, except that the formation of the top coat was changed as follows. A first polyurethane solution was prepared in which the concentration of the first polyurethane was changed to 6% by mass, and the pigment in the solid content was changed to 5% by mass. The Zahncup viscosity of the first polyurethane solution was 18 seconds. The first polyurethane was a polycarbonate-based polyurethane with a 100% modulus of 9 MPa. Then, the first polyurethane solution was applied to the surface of the porous polyurethane of the substrate at a rate of 30 g / m. 2 The coating amount was applied with a 110 mesh gravure roll, and the mixture was dried for about 10 seconds in a hot air dryer at 110°C and a speed of 8 m / min. In this way, a first top coat was formed. Then, grain-finished artificial leather was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0087] [Example 4] In Example 1, the fiber-entangled body after needle punching was impregnated with a 13% dimethylformamide (DMF) solution of polyester-based polyurethane. Immediately thereafter, a 26% DMF solution of the same polyester-based polyurethane was applied to the surface of the fiber-entangled body at 40 g / m 2 Then, on the top of that, 75 g / m of a 20% DMF solution of polycarbonate-based polyurethane, which was mixed with white pigments, yellow pigments, and red pigments to give it a beige color, was applied. 2 was applied.
[0088] The fiber-entangled bodies impregnated or coated with each polyurethane were then immersed in a coagulation bath (40°C) of DMF / water = 30 / 70 for 30 minutes to coagulate each polyurethane into a porous form, and then washed with water. The polyethylene in the islands-in-the-sea composite fibers was then extracted and removed with toluene to convert them into ultrafine fibers. In this way, a substrate with a thickness of 1.6 mm was obtained, which contained fiber bundles of ultrafine fibers of polyamide 6 with an average fineness of 0.01 dtex and porous polyurethane.
[0089] On the other hand, a polyurethane solution containing a mixed solvent containing DMF, CHN, and THF in a mass ratio of 65 / 30 / 5 (DMF / CHN / THF) and a concentration of the first polyurethane of 7.5 mass% was prepared as the first polyurethane solution. The Zahn cup viscosity of the first polyurethane solution was 15 seconds. The first polyurethane was a polycarbonate-based polyurethane with a 100% modulus of 9 MPa. Then, the first polyurethane solution was applied at 40 g / m2 onto the surface of the porous polyurethane of the substrate. 2 The coating amount was applied using a 110 mesh gravure roll, and the coating was dried by passing through a hot air dryer at 110° C. and a speed of 8 m / min for about 10 seconds. In this way, a first top coat was formed. Thereafter, grain-finished artificial leather was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0090] [Example 5] Except for changing the formation of the top coat as follows, the same procedure as in Example 1 was repeated to produce grain-finished artificial leather and evaluate it. The results are shown in Table 1.
[0091] As the second polyurethane solution, a polyurethane solution containing a mixed solvent with a mass ratio of 15 / 30 / 15 / 15 / 25 (DMF / CHN / THF / methyl ethyl ketone (MEK) / Ac) and a concentration of the second polyurethane of 7.5 mass% was prepared. The Zahn cup viscosity of the second polyurethane solution was 17 seconds. The second polyurethane was a silicone modified polycarbonate polyurethane with a 100% modulus of 8 MPa.
[0092] Then, the second polyurethane solution was applied at 40 g / m2 onto the surface of the first top coat embossed in the same manner as in Example 1. 2 The coating amount was applied with a 110 mesh gravure roll and dried for about 10 seconds in a hot air dryer at 110°C and a speed of 8 m / min. In this way, a second top coat was formed. In this way, grain-finished artificial leather was produced and evaluated. The results are shown in Table 1.
[0093] [Comparative Example 1] A grain-finished artificial leather was produced and evaluated in the same manner as in Example 1, except that the second top coat was not formed. The results are shown in Table 1.
[0094] [Comparative Example 2] In Example 1, instead of the first polyurethane solution, DMF was used at 40 g / m 2 The coating amount was 110 mesh gravure roll. The Zahn cup viscosity of DMF was 6 seconds. Thereafter, a first polyurethane solution in which the same first polyurethane as in Example 1 was dissolved was added at 40 g / m 2 The coating amount was applied with a 110 mesh gravure roll. The first polyurethane solution contained a mixed solvent containing DMF, cyclohexanone, and tetrahydrofuran in a mass ratio of 65 / 30 / 5 (DMF / cyclohexanone / tetrahydrofuran), had a first polyurethane concentration of 7.5 mass%, and was a polyurethane solution with a Zahn cup viscosity of 15 seconds. The first polyurethane was a polycarbonate-based polyurethane with a 100% modulus of 9 MPa. Thereafter, embossing was performed in the same manner as in Example 1.
[0095] [Comparative Example 3] A grain-finished artificial leather was produced and evaluated in the same manner as in Comparative Example 2, except that the amount of the second polyurethane solution applied was changed. The results are shown in Table 1.
[0096] [Comparative Example 4] A grain-finished artificial leather was obtained in the same manner as in Example 1, except that the following polyurethane solution was applied as the first polyurethane solution in Example 1. The first polyurethane solution contained a mixed solvent containing DMF, cyclohexanone, tetrahydrofuran, methyl ethyl ketone, and acetone in a mass ratio of 15 / 30 / 15 / 15 / 25 (DMF / cyclohexanone / tetrahydrofuran / methyl ethyl ketone / acetone), had a first polyurethane concentration of 7.5 mass%, had a Zahn cup viscosity of 20 seconds, and was a polyurethane solution containing 6 mass% of pigment in the solid content. The first polyurethane was a silicone-modified polyester polyurethane with a 100% modulus of 8 MPa.
[0097] [Comparative Example 5] In Example 5, after the first polyurethane solution was applied, it was dried in a dryer at 110°C for about 10 seconds, and then the second polyurethane solution was applied, and then embossing was performed. In the same manner as in Example 5, except for this, a grain-finished artificial leather was obtained and evaluated.
[0098] [Comparative Example 6] In Example 3, the first polyurethane solution was 30 g / m 2 Instead of the first polyurethane solution being applied with a 110 mesh gravure roll at a coating weight of 70 g / m 2 A grain-finished artificial leather was obtained and evaluated in the same manner as in Example 1, except that the coating amount was applied using a 55 mesh gravure roll. The grain-finished artificial leather obtained had a lack of surface smoothness and was inferior in quality.
[0099] All of the grain-finished artificial leathers obtained in Examples 1 to 5 had high water resistance, breathability that moderately suppresses stuffiness, and abrasion resistance. On the other hand, the grain-finished artificial leather obtained in Comparative Example 1, in which the second polyurethane solution was not applied, had low water resistance and abrasion resistance because the large openings were not fully blocked. Moreover, the grain-finished artificial leathers obtained in Comparative Examples 2 and 3, in which only a solvent was applied instead of applying the viscosity-adjusted first polyurethane solution, also had low water resistance and abrasion resistance because the large openings were not fully blocked. Although the grain-finished artificial leather obtained in Comparative Example 4, in which the solubility of the solvent in the first polyurethane solution was too high, had high water resistance but extremely low breathability. Moreover, the grain-finished artificial leather obtained in Comparative Example 5, in which the second top coat was formed instead of embossing the first top coat and then the embossing roll was applied, had low breathability because the openings were too fully blocked. In addition, the grain-finish artificial leather obtained in Comparative Example 6, in which too much of the first polyurethane solution was applied and too many interconnected open pores were formed, had excellent abrasion resistance but poor water resistance and breathability. [Explanation of symbols]
[0100] 1 Base material 2. Wet polyurethane porous layer 2a Lamination area of wet polyurethane porous layer (grain surface layer) 2b Lamination area of wet polyurethane porous layer (impregnated layer) 3. Top coat 10 Silver-tone artificial leather v void h Communication open hole
Claims
1. A step of preparing a substrate including a fiber-entangled body and a wet-type porous polyurethane layer impregnated and laminated to the fiber-entangled body to be integrated therewith; a step of gravure-coating a first polyurethane solution, in which a first polycarbonate-based polyurethane is dissolved, onto a surface of the wet polyurethane porous layer to dissolve the wet polyurethane porous layer and form open pores communicating in a thickness direction, and then drying the solution to form a first top coat; embossing the first topcoat with a heated, textured embossing roll; a step of gravure-coating a second polyurethane solution, in which a second polycarbonate-based polyurethane containing a silicone-modified polycarbonate-based polyurethane is dissolved, on the surface of the embossed first top coat, and then drying the second polyurethane solution to form a second top coat; the total thickness of the first top coat and the second top coat is 1 to 5 μm; The first polyurethane solution contains a mixed solvent containing 50 to 80% by mass of N,N-dimethylformamide and 20 to 50% by mass of cyclohexanone, the concentration of the first polycarbonate-based polyurethane is 5 to 10% by mass, the Zahn cup viscosity at 20° C. is 10 to 40 seconds, and the coating amount is 20 to 60 g / m 2 ; the second polyurethane solution contains a mixed solvent containing 10 to 40% by mass of N,N-dimethylformamide, 25 to 35% by mass of cyclohexanone, and 20 to 40% by mass of acetone, the concentration of the second polycarbonate-based polyurethane is 5 to 10% by mass, the Zahn cup viscosity at 20° C. is 10 to 40 seconds, and the coating amount is 20 to 60 g / m 2 ; The water resistance measured in accordance with the water resistance test (hydrostatic pressure method) A method of JIS L 1092 (2009) "Waterproof test method for textile products" is 1000 mm or more, and the air permeability measured in accordance with the method specified in the air permeability A method (Fragile type method) of JIS L 1096 (2010) "Fabric test method for woven and knitted fabrics" is 0.10 cm 3 / cm 2 and adjusting the opening diameter and number of the open holes in each step so that the grain-finished artificial leather has a grain-finished artificial leather grain size of 100 mm or more.
2. A grain-finished artificial leather comprising: a fiber-entangled body; a wet-processed polyurethane porous layer impregnated with and laminated on the fiber-entangled body to be integrated; and a top coat having a thickness of 1 to 5 μm and containing a polycarbonate-based polyurethane, The top coat contains a silicone-modified polycarbonate-based polyurethane and has a grained surface. the wet polyurethane porous layer has open pores extending from the surface to the back surface of the wet polyurethane porous layer, the number of openings having a major axis of 0.5 μm or more and 40 μm or less per cm 2 of said surface is 100 or more and less than 200, the number of openings having a major axis of more than 20 μm and 40 μm or less per cm 2 of said surface is 10 or more and less than 20, and the number of openings having a major axis of more than 40 μm is 0, The water resistance measured in accordance with the water resistance test (hydrostatic pressure method) A method of JIS L 1092 (2009) "Testing method for waterproofness of textile products" is 1000 mm or more, and the air permeability measured in accordance with the method specified in the air permeability A method (Fragile type method) of JIS L 1096 (2010) "Testing method for woven and knitted fabrics" is 0.10 cm 3 / cm 2 A grain-finished artificial leather having a grain-finish finish of s or more.
3. The surface 1 cm 2 3. The grain-finished artificial leather according to claim 2, wherein the number of openings having a major axis of 0.5 μm or more present per unit area is less than 200.
Citation Information
Patent Citations
Silvered-type synthetic leather substitute and its production
JP1996041786A
Leather-like sheetlike material and its production
JP1996269875A
Leather like sheet having good ventilation and its production
JP2000265378A
Sheet structure and method for producing the same
JP2003027381A
Grained artificial leather and method for producing the same
JP2010248644A