Pressure Sensor
A two-layer pressure-sensitive conductive member with distinct electrical resistances and thicknesses stabilizes resistance changes, addressing instability in conventional sensors for accurate pressure detection.
Patent Information
- Application Number
- JP2020068694
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-19
- Filing Date
- 2020-04-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-04-06
AI Technical Summary
Conventional pressure-sensitive conductive members using non-conductive elastomers exhibit unstable electrical resistance values under pressure, particularly at high pressures, making accurate pressure detection difficult.
A pressure-sensitive conductive member with a two-layer structure, comprising a first rubber layer with higher electrical resistance and a second rubber layer with lower resistance, where the first layer is thinner than the second, stabilized by electron beam crosslinking, ensuring stable pressure-sensitive behavior.
The two-layer structure provides stable electrical resistance changes in response to pressure, enabling accurate pressure detection across a wide range from low to high pressures, with flexibility and durability.
Smart Images

Figure 0007576923000004 
Figure 0007576923000005 
Figure 0007576923000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive conductive member and a pressure-sensitive sensor including the pressure-sensitive conductive member. [Background technology]
[0002] Conventionally, pressure-sensitive sensors that detect changes in resistance value according to the magnitude of pressure have been known. Pressure-sensitive sensors include sensors that use strain gauges and sensors that use piezoelectric ceramics, but these sensors tend to have high rigidity components and therefore tend to limit the shape of the pressure-sensitive sensor.
[0003] In recent years, in order to increase the degree of freedom in the shape of pressure-sensitive sensors, pressure-sensitive conductive members have been proposed that use elastomers as the material of the conductive member to impart flexibility. For example, Patent Document 1 discloses a pressure-sensitive conductive member in which nanometer-sized conductive fillers are dispersed in a non-conductive elastomer. By dispersing a specific conductive filler, the properties of the pressure-sensitive conductive member, such as the reproducibility of the electrical resistance value, are improved. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2007-220481 A Summary of the Invention [Problem to be solved by the invention]
[0005] In general, a pressure-sensitive sensor has an output characteristic (pressure-sensitive behavior) in which the electrical resistance value decreases as the pressure applied increases. Based on a curve representing this output characteristic, the magnitude of the applied pressure is detected from the measured electrical resistance value. Therefore, in order to detect pressure with high accuracy, it is necessary that the pressure-sensitive behavior is stable. However, with a pressure-sensitive conductive member using a conventional non-conductive elastomer, the electrical resistance value varies depending on the pressure, or the electrical resistance value increases with increasing pressure, so that stable pressure-sensitive behavior may not be obtained. In particular, it is difficult to obtain stable pressure-sensitive behavior under high pressure conditions.
[0006] The present invention has been made to address such circumstances, and aims to provide a pressure-sensitive conductive member that is flexible and exhibits stable pressure-sensing behavior, and a pressure-sensitive sensor that includes such a pressure-sensitive conductive member. [Means for solving the problem]
[0007] The pressure-sensitive conductive member of the present invention is a sheet-shaped pressure-sensitive conductive member whose electrical resistance value changes depending on pressure, and is constructed by laminating a first rubber layer in which a first conductive filler is dispersed in a first rubber component and a second rubber layer in which a second conductive filler is dispersed in a second rubber component, the first rubber layer being a layer having a higher electrical resistance value than the second rubber layer, and the thickness of the first rubber layer being less than 1 mm and smaller than the thickness of the second rubber layer.
[0008] The thickness of the pressure-sensitive conductive member, which is the total thickness of the first rubber layer and the second rubber layer, is 100 μm to 1000 μm, and the thickness of the first rubber layer is 20% or more and less than 50% of the thickness of the pressure-sensitive conductive member.
[0009] The volume resistance of the first rubber layer rate is 1.0×10 9 Ω cm~1.0×10 11 Ω·cm, and the volume resistivity of the second rubber layer rate is 1.0×10 1 Ω cm~1.0×103 It is characterized by a resistivity of Ω·cm.
[0010] The first rubber component and the second rubber component are characterized in that they are silicone rubbers.
[0011] The first conductive filler is graphite and carbon black, and the second conductive filler is carbon black.
[0012] The pressure-sensitive sensor of the present invention is a pressure-sensitive sensor that detects pressure by detecting changes in electrical resistance value, and is characterized in that it comprises a pair of electrodes and a pressure-sensitive conductive member arranged between the pair of electrodes, and the pressure-sensitive conductive member is the pressure-sensitive conductive member of the present invention. Effect of the Invention
[0013] The pressure-sensitive conductive member of the present invention is flexible because it is a laminate of a first rubber layer and a second rubber layer, each of which contains a conductive filler. The first rubber layer has a higher electrical resistance than the second rubber layer, and the thickness of the first rubber layer is less than 1 mm and is smaller than the thickness of the second rubber layer. Therefore, the first rubber layer functions as a pressure-sensitive layer and the second rubber layer functions as a conductive layer, and the change in electrical resistance in response to pressure is stable, resulting in good pressure-sensitive behavior.
[0014] The thickness of the pressure-sensitive conductive member, which is the total thickness of the first rubber layer and the second rubber layer, is 100 μm to 1000 μm, and the thickness of the first rubber layer is 20% or more and less than 50% of the thickness of the pressure-sensitive conductive member, which is suitable for a film-shaped pressure sensor and provides good pressure-sensing behavior. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a diagram showing a pressure-sensitive conductive member of the present invention. [Diagram 2] FIG. 2 is a diagram showing a pressure sensor of the present invention. [Diagram 3] FIG. 1 is a schematic diagram of a load test for measuring resistance against pressure. [Figure 4]1 is a graph showing the relationship between pressure and resistance value in Example 1 and Comparative Example 1. FIG. [Diagram 5] 13 is a graph showing the relationship between pressure and resistance value in Comparative Examples 2 and 3. FIG. [Figure 6] FIG. 11 is a graph showing the relationship between pressure and resistance value in Example 2. [Figure 7] FIG. 13 is a graph showing the relationship between pressure and resistance value in Examples 3 and 4. [Figure 8] FIG. 13 is a graph showing the relationship between pressure and resistance value in Examples 5 and 6. [Figure 9] FIG. 11 is a graph showing the relationship between pressure and resistance value in Example 7 and Comparative Example 4. [Figure 10] 1 is a graph showing the relationship between pressure and resistance value in Examples 2 to 6. FIG. [Figure 11] 1A to 1C are diagrams illustrating an example of a method for producing a pressure-sensitive conductive member of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present inventors have conducted extensive research to obtain excellent pressure-sensitive behavior for a pressure-sensitive conductive member made of rubber layers. As a result, they have found that by laminating two rubber layers with different electrical resistance values and setting the thickness of each layer, the change in electrical resistance value according to pressure can be stabilized. The present invention is based on this finding.
[0017] One embodiment of the pressure-sensitive conductive member of the present invention will be described with reference to FIG. 1. FIG. 1 is a cross-sectional view of a sheet-shaped pressure-sensitive conductive member. This pressure-sensitive conductive member is used, for example, as a conductive member of a pressure-sensitive sensor that detects the magnitude of pressure. As shown in FIG. 1, the pressure-sensitive conductive member 3 has a two-layer structure in which a first rubber layer 1 and a second rubber layer 2 are laminated. Since there is no adhesive layer between the layers and the rubber layers having electrical conductivity are in contact with each other, electrical conductivity is good and good pressure-sensitive behavior is obtained. Since the pressure-sensitive conductive member 3 is made of rubber layers, it is highly flexible and has excellent freedom of sensor shape. A pressure-sensitive conductive member made of such rubber layers exhibits a high electrical resistance value when no load is applied, and the electrical resistance value decreases when a load is applied. This is because the distance between the conductive fillers is shortened due to deformation caused by the load, and a conductive path is created by the conductive fillers.
[0018] The first rubber layer 1 is made of a rubber composition (hereinafter also referred to as the first rubber composition) in which a conductive filler (hereinafter also referred to as the first conductive filler) is blended with a rubber component (hereinafter also referred to as the first rubber component), and has electrical conductivity due to the conductive filler being dispersed in the layer. The second rubber layer 2 is made of a rubber composition (hereinafter also referred to as the second rubber composition) in which a conductive filler (hereinafter also referred to as the second conductive filler) is blended with a rubber component (hereinafter also referred to as the second rubber component), and has electrical conductivity due to the conductive filler being dispersed in the layer.
[0019] The first rubber component and the second rubber component are not particularly limited, and silicone rubber, ethylene-propylene-diene copolymer (EPDM), acrylonitrile butadiene rubber (NBR), natural rubber, butadiene rubber, styrene butadiene rubber, isoprene rubber, butyl rubber, nitrile rubber, chloroprene rubber, fluororubber, urethane rubber, etc. may be used. These may be used alone or in combination of two or more. Among these, it is preferable to use silicone rubber and EPDM. It is also preferable to use the same type of rubber for the first rubber component and the second rubber component. It is preferable that the silicone rubber has a Williams plasticity of 200 or less (after 10 minutes of remixing). The Williams plasticity is measured by a method specified in the plasticity test of JIS K 6249-8.
[0020] As the first conductive filler and the second conductive filler, solid carbon materials such as graphite powder, conductive carbon black, carbon nanotubes, and fullerenes, metal powders such as copper powder, silver powder, and iron powder, and conductive metal oxides such as conductive tin oxide and conductive titanium oxide are used. These conductive fillers may be used alone or in combination of two or more. In particular, it is preferable that each of the first conductive filler and the second conductive filler is at least one of graphite powder and conductive carbon black.
[0021] In the present invention, the first rubber layer 1 is a layer having a higher electrical resistance value than the second rubber layer 2. The first rubber layer 1 mainly functions as a pressure-sensitive layer, and the second rubber layer 2 mainly functions as a conductive layer (low resistance layer). Volume resistance of the first rubber layer 1 rate is 1.0×10 9 Ω cm~1.0×10 11 Ω·cm, and the volume resistivity of the second rubber layer 2 rate is 1.0×10 1 Ω cm~1.0×10 3 It is preferably Ω·cm.
[0022] The electrical resistance value of each layer is adjusted by adjusting the type and amount of conductive filler in the rubber composition. For example, when the same type of conductive filler is used in the first rubber composition and the second rubber composition, the electrical resistance value of the second rubber layer 2 can be reduced by increasing the amount of the conductive filler in the second rubber composition compared to the first rubber composition. In addition, when the same amount of conductive filler is used in the first rubber composition and the second rubber composition, the electrical resistance value of the second rubber layer 2 can be reduced by adding a conductive filler with a smaller volume resistivity to the second rubber composition.
[0023] It is preferable to use graphite powder and conductive carbon black as the conductive filler of the first rubber layer 1. In this embodiment, the graphite powder is preferably contained in an amount of 20 to 70 parts by mass, and more preferably 30 to 50 parts by mass, per 100 parts by mass of the first rubber component. Also, the conductive carbon black is preferably contained in an amount of 1 to 10 parts by mass, and more preferably 1 to 5 parts by mass, per 100 parts by mass of the first rubber component.
[0024] On the other hand, conductive carbon black is preferred as the conductive filler of the second rubber layer 2. In this embodiment, the conductive carbon black is preferably contained in an amount of 10 to 30 parts by mass, and more preferably 10 to 20 parts by mass, per 100 parts by mass of the second rubber component.
[0025] Graphite powder is roughly divided into natural graphite and artificial graphite, and further includes flake graphite, scaly graphite, spherical graphite, etc., and any of them can be used. As the conductive filler used in the present invention, it is preferable to use artificial graphite, which is further isotropic spherical graphite. The average particle size of the spherical graphite is not particularly limited, but is preferably 5 to 50 μm, more preferably 5 to 20 μm. The average particle size can be measured, for example, using a particle size distribution measuring device using a laser light scattering method.
[0026] The conductive carbon black preferably has an average particle size of 10 to 50 nm, and more preferably has an average particle size of 20 to 50 nm. By setting the average particle size within the range of 10 to 50 nm, a sufficient electrical resistance value is easily obtained even with a small amount of the conductive carbon black.
[0027] In addition, each rubber layer constituting the pressure-sensitive conductive member of the present invention may contain other additives, such as vulcanizing agents, vulcanization accelerators, reinforcing agents, antioxidants, softening agents, and colorants, as long as the additives do not impair the effects of the present invention.
[0028] The thickness of each layer and conductive member will be described with reference to Fig. 1. The present invention is characterized in that the layer thickness t1 of the first rubber layer 1 is less than 1 mm and smaller than the layer thickness t2 of the second rubber layer 2. By forming the pressure-sensitive layer thinner than the low resistance layer, it becomes easier to stably detect changes in electrical resistance value according to pressure.
[0029] The layer thickness t1 of the first rubber layer 1 is preferably 30 μm to 500 μm, more preferably 50 μm to 200 μm, and even more preferably 50 μm to 100 μm. The layer thickness t2 of the second rubber layer 2 is thicker than the layer thickness t1 and is preferably 50 μm to 2000 μm, more preferably 100 μm to 500 μm, and even more preferably 100 μm to 200 μm.
[0030] The total thickness t of the pressure-sensitive conductive member, which is the sum of the thickness t1 of the first rubber layer 1 and the thickness t2 of the second rubber layer 2, is preferably 100 μm to 1000 μm, and more preferably 100 μm to 300 μm. Furthermore, the thickness t1 of the first rubber layer 1 is preferably 20% or more and less than 50%, more preferably 25% to 48%, and even more preferably 25% to 40%, of the total thickness t of the pressure-sensitive conductive member.
[0031] In each rubber layer of the pressure-sensitive conductive member of the present invention, the rubber component is preferably crosslinked. As a crosslinking method, chemical crosslinking such as radiation crosslinking or press vulcanization can be used. As a vulcanizing agent used in press vulcanization, organic peroxides such as dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, 1,3-bis-(t-butylperoxy-isopropyl)benzene, t-butylcumyl peroxide, and di-t-butyl peroxide can be used. The blending amount of the vulcanizing agent is preferably 0.5 parts by mass to 3 parts by mass with respect to 100 parts by mass of the rubber component. If the blending amount of the vulcanizing agent is too small, crosslinking may be insufficient and strength may decrease, and if the blending amount of the vulcanizing agent is too large, the crosslinking density may be too high and sufficient flexibility may not be obtained.
[0032] Examples of radiation crosslinking include electron beams, gamma rays, and X-rays. In the present invention, electron beam irradiation is preferred from the viewpoint of easy control of the effect of the radiation shielding layer. The electron beam irradiation conditions are an acceleration voltage of 50 kV to 1000 kV, preferably 200 kV to 500 kV, and an irradiation dose of 50 kGy to 400 kGy, preferably 50 kGy to 200 kGy. If the irradiation condition is an acceleration voltage of less than 50 kV, the electron beam penetration depth in the thickness direction is low, and there is a risk of uncrosslinked parts remaining. If the irradiation dose exceeds 400 kGy, there is a risk of over-crosslinking, which may result in insufficient flexibility.
[0033] The method for producing the pressure-sensitive conductive member of the present invention will be described below.
[0034] When the pressure-sensitive conductive member of the present invention is thin (for example, the thickness of the pressure-sensitive conductive member is 1000 μm or less), it can be obtained by sequentially coating a coating film with a paint of the second rubber composition and a paint of the first rubber composition, and then irradiating the film with an electron beam.
[0035] (1) Coating of the second rubber composition The second rubber composition is dissolved in a solvent, filtered, and degassed to obtain a coating material of the second rubber composition. Any solvent capable of dissolving the rubber component may be used, for example, toluene. The obtained coating material is applied to a coating film (for example, a PET film having a thickness of 50 μm). Any coating method capable of forming a coating film, such as a comma bar method, a spray method, a dipping method, or a brush coating method, may be used. After coating, the coating material of the second rubber composition is dried. Drying is performed, for example, in a thermostatic chamber at 90° C. for about 10 minutes.
[0036] (2) Coating of the first rubber composition The first rubber composition is dissolved in a solvent, filtered, and degassed to obtain a paint for the first rubber composition. The same solvent as that for the paint for the second rubber composition can be used as the solvent. The obtained paint is applied to the surface of the second rubber composition after drying. After application, the paint is dried under the same drying conditions as those for the paint for the second rubber composition. Then, a cover film (same as the coating film) is attached to the surface of the first rubber composition after drying.
[0037] (3) Electron beam irradiation The obtained coated body is irradiated with an electron beam from one side or both sides. When irradiating both sides, specifically, first, the first rubber layer side is irradiated with an electron beam under the above-mentioned electron beam irradiation conditions. Then, the second rubber layer side is irradiated with an electron beam under the same irradiation conditions. This crosslinks the rubber components in the first rubber layer and the rubber components in the second rubber layer, respectively, to obtain the pressure-sensitive conductive member of the present invention. The electron beam irradiation may be performed in the order of the second rubber layer side first. Also, depending on the coating thickness and the conditions of the electron beam irradiation device used for processing, it is possible to irradiate only one side.
[0038] Furthermore, the manufacturing method of the pressure-sensitive conductive member of the present invention is not limited to the above manufacturing method. For example, when considering production on a production line, a method such as that shown in Fig. 11 can also be adopted. The method of Fig. 11 will be described below.
[0039] First, the second rubber composition is dissolved in a solvent, filtered, and degassed to obtain a coating material of the second rubber composition. The obtained coating material is applied to a coating film 24. After application, the coating material of the second rubber composition is dried. Then, a cover film (not shown) is attached to the surface of the dried second rubber composition 22, and a predetermined length is temporarily wound up.
[0040] Next, the first rubber composition is dissolved in a solvent, filtered, and degassed to obtain a coating material of the first rubber composition. The obtained coating material is applied to a coating film 23. After application, the coating material of the first rubber composition is dried. Thereafter, while peeling off the cover film (not shown) of the second rubber composition prepared earlier, the surface of the second rubber composition 22 is bonded to the surface of the first rubber composition 21 as shown in FIG. 11, and a predetermined length is taken up. The coating film 24 of the second rubber composition 22 finally becomes the cover film. The obtained coating body 25 is irradiated with an electron beam as shown in (3) above to obtain a pressure-sensitive conductive member.
[0041] As another manufacturing method, instead of molding by coating, each rubber composition may be molded into a sheet by molding with a mold, extrusion molding, or portioned molding, in which case press vulcanization is suitable. In the case of molding by coating, since it can be directly processed into a film-like electrode, it is possible to suppress the variation in the contact resistance between the electrode and the pressure-sensitive conductive member. In addition, it is preferable in that it is easier to make a long thin film and laminate two layers (multiple layers) of thin films compared to portioned or extrusion, and the thickness precision is also good.
[0042] One embodiment of the pressure-sensitive sensor of the present invention is shown in Fig. 2. Fig. 2 is a cross-sectional view of the pressure-sensitive sensor of the present invention. The pressure-sensitive sensor 4 includes a pair of electrodes 5, 6 and a pressure-sensitive conductive member 3 of the present invention between the pair of electrodes 5, 6. The pair of electrodes 5, 6 are connected to a power source (not shown) and a detector (not shown).
[0043] The material of the electrodes 5 and 6 is not particularly limited, and examples thereof include metal electrodes made of metals such as copper, silver, aluminum, gold, and platinum, and film-like electrodes formed by applying or printing a metal paste of copper, silver, aluminum, etc. onto a PET film, etc. Specific examples of the metal electrodes that can be used include copper foil, silver foil, aluminum foil, and gold-plated foil.
[0044] The thickness of the electrodes 5 and 6 is not particularly limited, but is preferably 50 to 250 μm from the viewpoints of flexibility and durability. For example, by using a film-like electrode prepared by screen printing or the like, the sensor shape has a high degree of freedom and can be applied to various shapes.
[0045] As shown in the examples described later, the pressure-sensitive conductive member of the present invention provides the same electrical resistance value regardless of whether pressure is applied from the first rubber layer or the second rubber layer, and therefore can be used in a pressure-sensitive sensor regardless of the direction in which pressure is applied.
[0046] 2, when a pressure is applied from, for example, the electrode 5 side of the pressure-sensitive sensor 4 while a certain voltage is applied, the pressure-sensitive conductive member 3 deforms, and the conductive filler in each rubber layer becomes dense due to the deformation, causing a change in the electrical resistance value in the thickness direction. The magnitude of the pressure can be detected by detecting this change in electrical resistance value with a detector.
[0047] The pressure-sensitive conductive member of the present invention has excellent output characteristics over a wide range of pressure conditions from low pressure to high pressure. Therefore, the pressure-sensitive sensor of the present invention can be used as a pressure-sensitive sensor capable of detecting a wide range of pressures from low pressure to high pressure. For example, the maximum measurement pressure can be set to 300 kPa or more, for example, the maximum measurement pressure can be set to 500 kPa or 1000 kPa. Since the pressure-sensitive sensor of the present invention can measure even under high pressure conditions, it can be used as a pressure-sensitive sensor for managing luggage in a warehouse, detecting damage to infrastructure facilities (elevated roads, tunnel walls, etc.), etc. In addition, since the shape has a high degree of freedom and can be made long, it can be used for large structures. EXAMPLES
[0048] First, the behavior of the electrical resistance value against pressure was examined using conductive members with different layer structures. A pressure-sensitive conductive member with a two-layer structure was used in Example 1 and Comparative Example 1. A pressure-sensitive conductive member with a single layer structure consisting of only the first rubber layer was used in Comparative Example 2 and Comparative Example 3. Table 1 shows the composition and layer thickness of the rubber composition in each test example.
[0049] [Table 1]
[0050] Example 1 A second rubber composition was obtained by blending 20 parts by mass of carbon black as a conductive filler with 100 parts by mass of silicone rubber, and further blending 1.5 parts by mass of a vulcanizing agent. This rubber composition was molded into a sheet shape, and the obtained molded body was placed in a frame gauge. The molded body was pressed between hot plates and vulcanized under the conditions of a vulcanization temperature of 164°C, a vulcanization time of 20 minutes, and a vulcanization pressure of 10 MPa. Thereafter, secondary vulcanization (annealing treatment) was performed under the conditions of a vulcanization temperature of 200°C and a vulcanization time of 4 hours, to obtain a second rubber layer having a thickness of 2 mm. Next, 100 parts by mass of silicone rubber was mixed with 40 parts by mass of graphite and 5 parts by mass of carbon black as conductive fillers to obtain a first rubber composition. This rubber composition was dissolved in a toluene solution so that the solid content of the rubber composition was 30% by mass, and the solution was filtered and degassed to obtain a coating material of the first rubber composition. This coating material was applied to a PET film having a thickness of 50 μm. After coating, the coating material was dried under conditions of a drying temperature of 90° C. and a drying time of 10 minutes. After drying, a PET film having a thickness of 50 μm was attached to the surface of the coating body, and electron beam irradiation was performed under conditions of an acceleration voltage of 250 kV, an exposure dose of 100 kGy, and a feed rate of 10 m / min to obtain a first rubber layer having a thickness of 0.1 mm. The obtained first rubber layer and second rubber layer were overlapped to obtain a pressure-sensitive conductive member.
[0051] The volume resistance of the first rubber layer rate is 9.3 x 10 9 Ω·cm (measured with a Yokogawa Hewlett-Packard 4329A HIGH RESISTANCE METER at 500 V applied), and the volume resistivity of the second rubber layer rate is 9.4 × 10 1 The electrical resistance of the first rubber layer was 1.0×10 3 Ω~1.0×10 6 Ω, and the electrical resistance of the second rubber layer is 1.0×10 0 Ω~1.0×10 3 It was Omega.
[0052] Comparative Example 1 In the same manner as in Example 1, a second rubber layer having a thickness of 2 mm was obtained. Next, 40 parts by mass of graphite and 5 parts by mass of carbon black were mixed as conductive fillers into 100 parts by mass of silicone rubber, and 0.75 parts by mass of a vulcanizing agent was further mixed to obtain a first rubber composition. This composition was molded into a sheet, and the molded body obtained was press-vulcanized and secondary vulcanized (annealed) under the above-mentioned conditions to obtain a first rubber layer having a thickness of 1 mm. The first rubber layer and the second rubber layer thus obtained were laminated together to form a pressure-sensitive conductive member.
[0053] Comparative Example 2 A first rubber composition was obtained by blending 40 parts by mass of graphite and 5 parts by mass of carbon black as conductive fillers into 100 parts by mass of silicone rubber. This rubber composition was dissolved in a toluene solution so that the solid content of the rubber composition was 30% by mass, and the solution was filtered and degassed to obtain a coating material of the first rubber composition. This coating material was applied to a PET film having a thickness of 50 μm. After coating, the coating material was dried under conditions of a drying temperature of 90° C. and a drying time of 10 minutes. After drying, a PET film having a thickness of 50 μm was attached to the surface of the coated body, and electron beam irradiation was performed under conditions of an acceleration voltage of 250 kV, an exposure dose of 100 kGy, and a feed speed of 10 m / min, to obtain a pressure-sensitive conductive member consisting of a first rubber layer having a thickness of 0.1 mm.
[0054] Comparative Example 3 A pressure-sensitive conductive member was produced in the same manner as for the first rubber layer of Comparative Example 1.
[0055] The electrical resistance value of each pressure-sensitive conductive member obtained was measured by a test device shown in FIG. 3. The test device 11 has an upper plate 12 to which a pressure F is applied, and a lower plate 13. A pair of electrodes 15, 16 are provided between these plates via a pair of insulating plates (e.g., Bakelite plates) 14, 14. In the test of FIG. 3, a copper cylinder with a diameter of 20 mm was used as the electrode 15 on the pressure side, and a copper foil plate was used as the electrode 16. The electrodes 15, 16 are each connected to a detector 17. In the test, the pressure-sensitive conductive member 3 was sandwiched between the electrodes 15, 16, and a pressure F was applied under the following test conditions while a predetermined voltage was applied, and the electrical resistance value in the thickness direction of the pressure-sensitive conductive member was measured. A DC voltage / current source 6240B manufactured by ADC Corporation was used as the detector. Figures in which the pressure and the change in resistance value are plotted are shown in FIG. 4 and FIG. 5.
[0056] <Test conditions> Compression testing machine: SV-201 tensile / compression testing machine manufactured by Imada Manufacturing Co., Ltd. Pressure: 0~1000kPa Pressurization speed: approx. 0.2 mm / min Pressurized area: 314mm 2 Applied voltage: DC 3V or DC 10V
[0057] In the tests, the orientation of the pressure-sensitive conductive member with respect to pressure was also examined. As shown in Figure 3, a test in which the first rubber layer 1 of the pressure-sensitive conductive member 3 was arranged facing the load side was designated as pattern A. On the other hand, a test in which the second rubber layer 2 of the pressure-sensitive conductive member 3 was arranged facing the load side was designated as pattern B. Note that unless otherwise specified in the figures, the test results for pattern A are shown.
[0058] The pressure-sensitive behaviors shown in FIG. 5 are all the results of pressure-sensitive conductive members with a single layer structure. In Comparative Example 2, the layer thickness was as thin as 0.1 mm, and as the pressure was increased, the resistance value fell outside the measurable range of the detector, resulting in results only under low pressure conditions, but the variation in resistance value was large. In Comparative Example 3, the resistance value increased with increasing pressure. Normally, the resistance value would decrease gradually with increasing pressure, so these pressure-sensitive behaviors are not suitable for a pressure-sensitive conductive member.
[0059] Comparative Example 1 shown in FIG. 4 is a pressure-sensitive conductive member with a two-layer structure in which a second rubber layer is added to the conductive member (first rubber layer with a thickness of 1 mm) of Comparative Example 3. However, similar to the pressure-sensitive behavior of Comparative Example 3 (see FIG. 5), the resistance value increased with increasing pressure. In contrast, Example 1 shown in FIG. 4 is a pressure-sensitive conductive member with a two-layer structure in which a second rubber layer is added to the conductive member (first rubber layer with a thickness of 0.1 mm) of Comparative Example 2, and as shown in FIG. 4, the resistance value decreased gradually with increasing pressure, showing excellent pressure-sensitive behavior.
[0060] Next, the thickness of each rubber layer of the pressure-sensitive conductive member was examined in detail. Table 2 shows the rubber composition of each test example, and Table 3 shows the layer thickness of each test example. In Examples 2 to 7, a pressure-sensitive conductive member with a two-layer structure was used, and in Comparative Example 4, a pressure-sensitive conductive member with a single-layer structure consisting of only the first rubber layer was used.
[0061] [Table 2]
[0062] [Table 3]
[0063] Examples 2 to 7 A second rubber composition was obtained by blending 20 parts by mass of carbon black as a conductive filler into 100 parts by mass of silicone rubber. This rubber composition was dissolved in a toluene solution so that the solid content of the rubber composition was 23% by mass, and the solution was filtered and degassed to obtain a coating material of the second rubber composition. This coating material was applied to a 50 μm-thick PET film so that the layer thickness after drying was the desired thickness, and the coating material was dried under the conditions of a drying temperature of 90° C. and a drying time of 10 minutes. Next, 100 parts by mass of silicone rubber was mixed with 40 parts by mass of graphite and 5 parts by mass of carbon black as conductive fillers to obtain a first rubber composition. This rubber composition was dissolved in a toluene solution so that the solid content of the rubber composition was 30% by mass, and the solution was filtered and degassed to obtain a paint of the first rubber composition. This paint was applied to the surface of the dried second rubber layer so that the layer thickness after drying was the desired thickness, and then the paint was dried under the conditions of a drying temperature of 90°C and a drying time of 10 minutes. After drying, a 50 μm thick PET film was laminated to the surface of the coated body, and electron beam irradiation was performed from the first rubber layer side and from the second rubber layer side under conditions of an acceleration voltage of 300 kV, an exposure dose of 100 kGy, and a feed speed of 10 m / min to crosslink the first rubber layer and the second rubber layer, thereby obtaining a two-layer pressure-sensitive conductive component.
[0064] Comparative Example 4 A first rubber composition was obtained by blending 40 parts by mass of graphite and 5 parts by mass of carbon black as conductive fillers into 100 parts by mass of silicone rubber. This rubber composition was dissolved in a toluene solution so that the solid content of the rubber composition was 30% by mass, and the solution was filtered and degassed to obtain a coating material of the first rubber composition. This coating material was applied to a PET film having a thickness of 50 μm. After coating, the coating material was dried under conditions of a drying temperature of 90° C. and a drying time of 10 minutes. After drying, a PET film having a thickness of 50 μm was attached to the surface of the coated body, and electron beam irradiation was performed under conditions of an acceleration voltage of 250 kV, an exposure dose of 100 kGy, and a feed rate of 10 m / min, to obtain a pressure-sensitive conductive member consisting of a first rubber layer having a thickness of 140 μm.
[0065] The electrical resistance value of each of the obtained pressure-sensitive conductive members was measured under the above-mentioned test conditions using the test device shown in Fig. 3. As with the above, the DC voltage / current source 6240B manufactured by ADC Corporation was used as the detector. The measurement results are shown in Figs. 6 to 9.
[0066] As shown in Figs. 6 to 8, the pressure-sensitive conductive members of Examples 2 to 6 exhibited good pressure-sensitive behavior. As the thickness of each of the first and second rubber layers increased, the variation in resistance tended to increase. Furthermore, no significant difference was observed between patterns A and B. As shown in Fig. 6, stable pressure-sensitive behavior was exhibited even when the voltage applied to the pressure-sensitive conductive member was different, 3V and 10V.
[0067] Fig. 9 shows a graph plotting Example 7 and Comparative Example 4. The pressure-sensitive conductive member of the single-layer structure of Comparative Example 4 has the same electrical resistance value as the pressure-sensitive conductive member of Example 7, and the layer thickness is relatively close, but the resistance value varies as shown in Fig. 9. In contrast, Example 7 showed a stable curve in the graph and excellent pressure-sensitive behavior.
[0068] In the above-mentioned Examples and Comparative Examples, copper electrodes were used as the electrodes, but even when other electrodes are used, the pressure-sensitive conductive member according to the present invention exhibits good pressure-sensitive behavior. For example, FIG. 10 shows the change in resistance value of the conductive member of Examples 2 to 6 when silver electrodes are used instead of copper electrodes. Two film-type electrodes were used as the silver electrodes. Each pressure-sensitive conductive member was sandwiched between a pair of silver electrodes, and pressure was applied under the above-mentioned conditions using a copper cylinder having a diameter of 20 mm as a pressure member via a cloth cushioning material. A DC voltage / current source 6240B manufactured by ADC Corporation was used as the detector.
[0069] As shown in Fig. 10, the pressure-sensitive conductive members of Examples 2 to 6 exhibited good pressure-sensitive behavior even in the case of silver electrodes. The pressure-sensitive behavior in Fig. 10 was superior to that in Fig. 6 to Fig. 8. Copper cylinders and copper foil were used as electrodes in Fig. 6 to Fig. 8, whereas a silver film electrode was used in Fig. 10, and it is believed that the contact resistance due to the difference in electrode (shape) affected the stability of the pressure-sensitive behavior. [Industrial Applicability]
[0070] The pressure-sensitive conductive member of the present invention has flexibility and exhibits stable pressure-sensitive behavior, and therefore can be widely used as a pressure-sensitive conductive member, and can detect the magnitude of pressure with high accuracy when applied to a pressure-sensitive sensor, etc. It is particularly suitable for a pressure-sensitive sensor with a wide pressure range. [Explanation of symbols]
[0071] 1 First rubber layer 2 Second rubber layer 3 Pressure-sensitive conductive material 4. Pressure Sensor 5 electrodes 6 electrodes 11 Test Equipment 12 Top Plate 13 Lower Plate 14 Insulating plate 15 electrodes 16 electrodes 17 Detector 21 First rubber composition 22 Second rubber composition 23 Coated Film 24 Coated Film 25 Coated body
Claims
1. A pressure sensor that detects pressure by detecting a change in electrical resistance and has a maximum measurable pressure of 300 kPa or more and 1000 kPa or less, a pair of electrodes; and a sheet-like pressure-sensitive conductive member disposed between the pair of electrodes, the sheet-like pressure-sensitive conductive member having an electrical resistance (Ω) that changes in a thickness direction in response to pressure; the pressure-sensitive conductive member is configured by laminating a first rubber layer having a first conductive filler dispersed in a first rubber component and a second rubber layer having a second conductive filler dispersed in a second rubber component; the first rubber layer has a higher electrical resistance (Ω) in a thickness direction than the second rubber layer, and the first rubber layer has a thickness of less than 1 mm and is smaller than a thickness of the second rubber layer; the thickness of the pressure-sensitive conductive member, which is the total thickness of the first rubber layer and the second rubber layer, is 100 μm to 300 μm; a thickness of the first rubber layer is equal to or greater than 20% and less than 50% of a thickness of the pressure-sensitive conductive member; 1. A pressure-sensitive sensor comprising: said first conductive filler material being graphite and carbon black; and said second conductive filler material being carbon black and not graphite.
2. The volume resistivity of the first rubber layer is 1.0×10 9 Ω・cm~1.0×10 11 Ω cm, and the volume resistivity of the second rubber layer is 1.0×10 1 Ω・cm~1.0×10 3 2. The pressure-sensitive sensor according to claim 1, wherein the resistance is Ω·cm.
3. 3. The pressure-sensitive sensor according to claim 1, wherein the first rubber component and the second rubber component are silicone rubber.
Citation Information
Patent Citations
Pressure sensitive conductive rubber sheet
JP1987090906A
Pressure sensitive conductive rubber sheet
JP1987114202A
Pressure sensitive resistor
JP1989042804A
Pressure-sensitive conductive elastomer
JP2007220481A
Pressure-sensitive resistor element
JP2008256399A