Liquid crystal device and emulsion composition
The emulsion composition optimizes liquid crystal elements for controlled light transmission and clear visibility by using a specific configuration of refractive index anisotropy and particle distribution, addressing the limitations of existing technologies in light control and visibility.
Patent Information
- Application Number
- JP2023073881
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-01-29
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2039-01-25
AI Technical Summary
Existing liquid crystal elements, such as PDLC and guest-host liquid crystal systems, struggle to effectively control the amount of transmitted light, maintain clear visibility in a transparent state, and allow for easy shaping and cutting, while also addressing issues of polymer matrix reliability and light scattering.
A specific emulsion composition is used to disperse liquid crystal compositions with dichroic dyes within a polymer matrix, optimized for refractive index anisotropy, particle size, and distribution, sandwiched between transparent conductive substrates, allowing for a liquid crystal element that can switch between transparent and colored states with controlled light transmission and minimal haze.
The solution enables a liquid crystal element that can be cut and shaped, providing clear visibility with minimal turbidity in the transparent state and significant light transmission control, effectively managing solar radiation and reducing energy consumption.
Smart Images

Figure 0007578155000001 
Figure 0007578155000002 
Figure 0007578155000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal device and an emulsion composition, and more particularly to a liquid crystal device capable of switching between a transparent state and a colored state, and an emulsion composition that can be used in the liquid crystal device. [Background technology]
[0002] In recent years, there has been an increasing demand for smart glass, which can electrically switch the transparency of glass. Liquid crystal, electrochromic, SPD (Suspend Particle Device), etc. have been proposed as light-adjusting materials for use in smart glass. Among these, the liquid crystal method has attracted attention because it has an overwhelmingly short response time and does not cause stress to users.
[0003] Among the liquid crystal methods, PDLC (Polymer Dispersed Liquid Crystals) is widely known (Non-Patent Document 1). PDLC has a structure in which a liquid crystal-polymer composite film in which particulate liquid crystal is dispersed in a polymer matrix is sandwiched between two transparent conductive substrates.
[0004] Among PDLCs, normal mode operation is the most common. When no voltage is applied to a PDLC in normal mode operation, the liquid crystal molecules are oriented along the walls of the polymer matrix, resulting in a mismatch in the refractive index between the liquid crystal region and the polymer matrix. This mismatch causes light scattering and coloring, acting as a screen. On the other hand, when a voltage is applied to a PDLC, the liquid crystal molecules are oriented in the direction of the electric field, causing the refractive indexes of the liquid crystal region and the polymer matrix to match, allowing light to pass through and becoming transparent.
[0005] PDLC has been put to practical use as light-controlling shutters for the purpose of design and privacy protection in windows, doors, partitions, etc. of trains, automobiles, and other vehicles, as well as in buildings such as business buildings and hospitals. It is also used as a display device that displays characters and figures. In particular, when applied to windows, it is desirable for there to be as little turbidity as possible in the transparent state.
[0006] PDLC can be made into a film element because of its flexibility due to the aforementioned liquid crystal-polymer composite film structure. In addition, the film element can be cut and shaped. Taking advantage of these characteristics, users can easily apply it to glass.
[0007] In recent years, with the growing interest in energy conservation, attempts have been made to use smart glass in windows to reduce the heating and cooling load by controlling the amount of solar radiation entering a room. However, in the case of PDLC, although it is possible to switch between scattering and not scattering light, most of the scattering is forward scattering, so the light passes through the element. As a result, the amount of transmitted light cannot be controlled at all, and it does not contribute to energy conservation.
[0008] Patent documents 1 to 3 disclose guest-host liquid crystal type smart glass in which a dichroic dye is added to the liquid crystal. The guest-host liquid crystal type switches between a transparent state and a colored state by electrically switching the absorbance of the liquid crystal element, so that the amount of transmitted light can be controlled.
[0009] Patent Documents 4 and 5 disclose guest-host PDLC in which PDLC and guest-host liquid crystal are combined, and it is expected that a film element capable of controlling the amount of transmitted light will be developed.
[0010] In Patent Document 4, a liquid crystal-polymer composite film is produced by polymerization-induced phase separation using photopolymerization.
[0011] In Patent Document 5, a liquid crystal-polymer composite membrane is produced using an aqueous emulsion composition. The production method using this emulsion composition has the advantage that it is easier to obtain a desired membrane structure than the production method using polymerization-induced phase separation in Patent Document 4, and that there is no decrease in reliability due to poor curing of the polymer matrix. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2016-510907 A [Patent Document 2] JP 2016-536634 A [Patent Document 3] JP 2017-511895 A [Patent Document 4] JP 2011-190314 A [Patent Document 5] JP 2000-347223 A [Non-patent literature]
[0013] [Non-Patent Document 1] DAHiggins,Advanced Materials 2000,12,No.4 Summary of the Invention [Problem to be solved by the invention]
[0014] In order to make the guest-host liquid crystals shown in Patent Documents 1 to 3 into film elements that can be cut and shaped, a matrix that surrounds the liquid crystal and supports the film structure, such as PDLC, is required. In the case of PDLC produced using polymerization-induced phase separation by photopolymerization as described in Patent Document 4, poor curing of the polymer matrix occurs due to light absorption by the dye, resulting in a problem in the reliability of the liquid crystal element.
[0015] On the other hand, Patent Document 5 describes that if the birefringence (Δn) of the liquid crystal is 0.15 or less and the order parameter S of the dichroic dye is 0.75 or more, the change range of the visible light transmittance of the PDLC is 30% or more and the haze in the transparent state is 10% or less. However, the visible light transmittance here indicates the linear transmittance of linear light that does not include scattered light, and when forward scattered light is included, the range of change in the amount of transmitted light is still very small, which poses the problem that the amount of solar radiation is almost impossible to control. Furthermore, even though the haze in the transparent state is supposed to be 10% or less, the method described in Patent Document 5 only achieves a haze of 8%, which is unsatisfactory as the transparent state is very cloudy and visibility is blurred.
[0016] Previous studies had not provided a liquid crystal element that could electrically control the amount of transmitted light, ensured a clear field of view with little cloudiness in the transparent state, and could be cut and shaped. [Means for solving the problem]
[0017] As a result of investigation, the inventors have found that a method of measuring the total transmittance using a spectrophotometer and an integrating sphere in combination is appropriate for evaluating the amount of transmitted light including scattered light. Furthermore, as a result of intensive investigations into solving the above problems using the above measurement method, the inventors have found that the problems can be solved by a specific element configuration and specific haze and total transmittance. That is, the gist of the present invention lies in the following.
[0018] [1] An emulsion composition in which a liquid crystal composition is dispersed in a medium containing water, the medium being a medium in which a polymer is dispersed or dissolved, the liquid crystal composition containing a dichroic dye, the liquid crystal composition having a positive dielectric anisotropy, a refractive index anisotropy of the liquid crystal composition being 0.01 or more and 0.2 or less, and an average particle size of the liquid crystal composition being 4.9 μm or more and 50 μm or less. [2] The emulsion composition according to the above [1], wherein the total mass of the liquid crystal composition is 0.5 to 4 relative to the total mass of the polymer, which is 1. [3] The emulsion composition according to the above [1] or [2], wherein the coefficient of variation in particle size distribution of the liquid crystal composition is 0.001 or more and 0.8 or less. [4] The emulsion composition according to any one of the above [1] to [3], wherein the dichroic dye contains an anthraquinone dye. [5] The emulsion composition according to any one of the above [1] to [4], wherein the liquid crystal composition contains a dichroic dye in an amount of 3% or more and 20% or less. [6] The emulsion composition according to any one of the above [1] to [5], wherein the polymer contains polyurethane. [7] A liquid crystal-polymer composite film obtained by using the emulsion composition according to any one of the above [1] to [6]. [8] A liquid crystal device comprising: two substrates with transparent conductive films arranged so that their transparent conductive films face each other; and the liquid crystal-polymer composite film according to [7] above, sandwiched between the two substrates with transparent conductive films. Effect of the Invention
[0019] According to the present invention, there is provided a liquid crystal element that can be cut and shaped and that can electrically control the amount of transmitted light. In addition, in the element, there is little turbidity in the transparent state, and a clear field of view is ensured.
[0020] The liquid crystal element of the present invention comprises two substrates with transparent conductive films arranged so that the transparent conductive films face each other, and a liquid crystal-polymer composite film sandwiched between the two substrates with transparent conductive films, the liquid crystal-polymer composite film having a polymer matrix and a liquid crystal region in which a liquid crystal composition is surrounded by the polymer matrix. The liquid crystal composition contains a dichroic dye, and the liquid crystal-polymer composite film can be switched between a transparent state and a colored state by application of a voltage. The difference in total transmittance between the transparent state and the colored state is 25% or more, and the haze in the transparent state is 6% or less. The liquid crystal-polymer composite film has a polymer matrix and a liquid crystal region in which a liquid crystal composition is surrounded by the polymer matrix, thereby forming a flexible liquid crystal element that can be cut and shaped. Since the difference in total transmittance between the transparent state and the colored state is 25% or more, it can be switched between a state in which the amount of transmitted light is large and a state in which the amount of transmitted light is small. For example, when the film is applied to a window as smart glass, it can control solar radiation and reduce the load on air conditioning. On the other hand, by keeping the haze in the transparent state at 6% or less, clear visibility with little turbidity is ensured, and visibility similar to that of ordinary window glass is obtained.
[0021] The liquid crystal element of the present invention is useful for windows, screens, displays, etc., due to the above-mentioned characteristics. For example, it can be used as a view blocking element in windows, partitions, etc. of buildings and vehicles. It can also be used as a display for advertisement boards, show windows, computer terminals, projections, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The present invention will be described in detail below. However, the following description is an example of an embodiment of the present invention, and the present invention is not limited to the contents of the following description as long as it does not exceed the gist of the present invention. The present invention can be modified and implemented as desired without departing from the gist of the present invention.
[0023] <Liquid crystal element> The liquid crystal element of the present invention is a liquid crystal element comprising two substrates with transparent conductive films arranged so that their transparent conductive films face each other, and a liquid crystal-polymer composite film sandwiched between the two substrates with transparent conductive films, the liquid crystal-polymer composite film having a polymer matrix and a liquid crystal region in which a liquid crystal composition is surrounded by the polymer matrix. The liquid crystal composition contains a dichroic dye, and the liquid crystal-polymer composite film can be switched between a transparent state and a colored state by application of a voltage. The liquid crystal-polymer composite film may be transparent when no voltage is applied and may be colored when a voltage is applied, or may be transparent when a voltage is applied and may be colored when no voltage is applied. In the present invention, the voltage refers to a DC voltage, an AC voltage, a pulse voltage, or a combination thereof, having an effective value equal to or greater than a threshold value.
[0024] In the present invention, the transparent state refers to the state of the liquid crystal-polymer composite film when the voltage is applied or when no voltage is applied, and the transparent state is the state in which the total transmittance of the liquid crystal-polymer composite film is greater when a voltage is applied or when no voltage is applied. In the present invention, the colored state refers to the state of the liquid crystal-polymer composite film when the voltage is applied or when no voltage is applied, and the transparent state is the state in which the total transmittance of the liquid crystal-polymer composite film is smaller when a voltage is applied or when no voltage is applied.
[0025] [Total transmittance] The total transmittance in this specification is measured by a method using a spectrophotometer equipped with an integrating sphere as specified in JIS B7081. In this specification, light refers to visible light (wavelength 380 nm to 780 nm), and the total transmittance is measured in the visible light region. The liquid crystal element of the present invention is characterized in that the difference in total transmittance between the transparent state and the colored state is 25% or more. By making the difference in total transmittance 25% or more, the amount of light transmitted through the liquid crystal element can be controlled. It is preferably 30% or more, and more preferably 35% or more. Furthermore, when the transmittance of the substrate with a transparent conductive film is low, the electrical resistance of the conductive film tends to be low, and the driving voltage and response time of the liquid crystal element tend to be good. Therefore, the difference in total transmittance is preferably 90% or less, more preferably 85% or less, and even more preferably 80% or less. In the liquid crystal element, it is sufficient that there is at least one wavelength range in which the difference in total transmittance between the transparent state and the colored state is 25% or more, and there may be two or more wavelength ranges.
[0026] There are no particular limitations on the method for achieving a difference in total transmittance of 25% or more, but examples of such methods include (1) increasing the light absorption of the dichroic dye in the colored state, (2) decreasing the light absorption of the dichroic dye in the transparent state, and (3) reducing the light that is backscattered into the transparent state. In order to increase the light absorption of the colored dichroic dye as in (1), (1-1) Increasing the extinction coefficient of the dichroic dye, (1-2) dissolving the dichroic dye in the liquid crystal composition in as large an amount as possible; (1-3) Reducing light scattering in a liquid crystal-polymer composite film in a colored state; (1-4) The absorption axis direction of the dichroic dye is aligned with the optical electric field vibration direction of the incident light. Furthermore, in order to reduce the light scattering of a liquid crystal-polymer composite film in a colored state as in (1-3), methods include making the extraordinary refractive index (ne) of the liquid crystal composition closer to the refractive index of the polymer matrix and making the average particle size (r) of the liquid crystal domains in a range sufficiently larger than the light wavelength. In order to reduce the light absorption of the dichroic dye in the transparent state as in (2), a method of increasing the order parameter of the dichroic dye can be given. In order to reduce the light that is backscattered in the transparent state as in (3), it is possible to employ methods such as bringing the ne of the liquid crystal composition closer to the refractive index of the polymer matrix and making the r of the liquid crystal region in a range sufficiently larger than the wavelength of light. The wavelength range in which the difference in total transmittance is 25% or more corresponds to the absorption wavelength range of the dichroic dye contained in the liquid crystal composition, so one method is to select a dichroic dye depending on the color to be produced.
[0027] The total transmittance in the transparent state is preferably 40% or more, more preferably 50% or more, and even more preferably 60% or more. The total transmittance in the colored state is preferably 50% or less, more preferably 40% or less, and even more preferably 30% or less. The total transmittance in the transparent state is always higher than that in the colored state. The range of total transmittance can be determined according to the application. For example, in applications where it is often desirable to observe the background, it is sufficient to prioritize transparency and set the total transmittance to a high range, such as 70% in the transparent state and 45% in the colored state, while in applications where it is often desirable to reduce the glare of external light, it is sufficient to set the total transmittance to a low range, such as 40% in the transparent state and 15% in the colored state.
[0028] [Haze] The haze in this specification is measured by the method of JIS K7136. The liquid crystal element of the present invention is characterized in that the haze in the transparent state is 6% or less. By having a haze in the transparent state of 6% or less, a clear view with little turbidity is ensured, and a view similar to that of ordinary window glass is obtained. The haze is preferably 4% or less, and more preferably 2% or less. On the other hand, taking into consideration the haze of the substrate with a transparent conductive film, the haze in the transparent state is preferably 0.1% or more, more preferably 0.3% or more, and even more preferably 0.5% or more. There are no particular limitations on the method for reducing the haze of a liquid crystal element in the transparent state to 6% or less. Examples include bringing the ordinary refractive index (no) of the liquid crystal composition closer to the refractive index of the polymer matrix, and setting the r of the liquid crystal region in a range sufficiently larger than the light wavelength.
[0029] The haze in the colored state is preferably 90% or less, more preferably 80% or less, and even more preferably 70% or less. By being 90% or less, the light absorption of the dichroic dye in the colored state can be increased, and the amount of transmitted light tends to be reduced. On the other hand, it is preferably 10% or more, more preferably 20% or more, and even more preferably 30% or more. By being 10% or more, the glare of external light tends to be reduced.
[0030] In particular, the present invention provides a liquid crystal element that can reduce the difference in total transmittance between the transparent state and the colored state to 25% or more and the haze in the transparent state to 6% or less by controlling the Δn (Δn=ne-no) of the liquid crystal composition and the m of the liquid crystal region within appropriate ranges.
[0031] [Liquid crystal-polymer composite film] The liquid crystal-polymer composite film included in the liquid crystal element of the present invention has a polymer matrix and a liquid crystal region in which a liquid crystal composition is surrounded by the polymer matrix. Such a liquid crystal-polymer composite film is generally known as PDLC. The liquid crystal-polymer composite film has a polymer matrix and a liquid crystal region in which the liquid crystal composition is surrounded by the polymer matrix, which gives the liquid crystal element flexibility. In addition, this structure minimizes leakage of the liquid crystal composition even when the liquid crystal element is cut, and the polymer matrix protects the liquid crystal composition from deterioration factors such as oxygen and moisture, making it possible to cut and shape the liquid crystal element.
[0032] The liquid crystal domains may be dispersed in the polymer matrix or may be regularly arranged. The shape of the liquid crystal domains may be any of a perfect sphere, a spheroid, a cylinder, a triangular prism, a square prism, a hexagonal prism, or any other polygonal prism, or these shapes may be distorted. Among these, a perfect sphere, a spheroid, a cylinder, a regular triangular prism, a regular square prism, a regular hexagonal prism, or any other regular polygonal prism, is preferred because the light scattering of the liquid crystal-polymer composite film is weakened, the light absorption of the dichroic dye during coloring is increased, and the haze in the transparent state tends to be reduced.
[0033] The size of the liquid crystal domains, when observed from the film surface, is preferably an average particle size of 2 μm or more, more preferably 5 μm or more. Also, it is preferably 50 μm or less, more preferably 30 μm or less. When the average particle size is larger than the lower limit, the light scattering of the liquid crystal-polymer composite film is weakened, and the haze in the transparent state tends to be reduced. At the same time, the light scattering of the colored liquid crystal-polymer composite film is weakened, which improves the efficiency of light absorption of the dichroic dye and tends to lower the total transmittance. When the average particle size is smaller than the upper limit above, the graininess of the liquid crystal region disappears and the uniformity of the appearance of the liquid crystal element tends to improve. The average particle size is the median diameter based on the number of particles. When observed from the film surface, if the shape of the liquid crystal domain is not a circle but an ellipse, a triangle, a rectangle, a hexagon or other polygon, or a distorted shape, the particle size may be determined by referring to the diameter of the smallest inclusive circle.
[0034] The coefficient of variation of the liquid crystal region is expressed as CV=σ / m, where m is the average particle size and σ is the standard deviation of normal distribution. The coefficient of variation is preferably 0.8 or less, more preferably 0.5 or less, more preferably 0.3 or less, and even more preferably 0.1 or less. By keeping the coefficient of variation at or below the upper limit, the number of small particles that cause scattering and large particles that cause graininess tends to be sufficiently reduced. On the other hand, the coefficient of variation is preferably equal to or greater than the lower limit, more preferably equal to or greater than 0.005, and even more preferably equal to or greater than 0.01. When the coefficient of variation is equal to or greater than 0.001, the productivity of the emulsion composition tends to improve.
[0035] In the particle size frequency distribution based on the number of liquid crystal regions, the particle size of 2 μm or less is preferably 20% or less in cumulative, more preferably 10% or less in cumulative, and even more preferably 5% or less in cumulative. By being 20% or less in cumulative, the light scattering of the liquid crystal-polymer composite film becomes weak, the light absorption of the dichroic dye in the colored state becomes large, and the haze in the transparent state tends to be small. On the other hand, the cumulative amount is preferably 0.1% or more, more preferably 0.5% or more, and even more preferably 1% or more. By having the cumulative amount be 0.1% or more, the productivity of the emulsion composition tends to be improved. Moreover, the particle size of 50 μm or more is preferably 20% or less in cumulative, more preferably 10% or less in cumulative, and even more preferably 5% or less in cumulative. By keeping the particle size at 20% or less in cumulative, the graininess of the liquid crystal region is eliminated, and the uniformity of the appearance of the liquid crystal element tends to be improved. On the other hand, the cumulative amount is preferably 0.1% or more, more preferably 0.5% or more, and even more preferably 1% or more. By having the cumulative amount be 0.1% or more, the productivity of the emulsion composition tends to be improved.
[0036] [Liquid Crystal Composition] The liquid crystal composition of the present invention contains a liquid crystal containing a dichroic dye. Such a liquid crystal composition is generally known as a guest-host liquid crystal. Although not particularly limited, the content of the dichroic dye in the liquid crystal composition is preferably 3% or more, more preferably 4% or more, and even more preferably 5% or more, and preferably 20% or less, more preferably 15% or less, and even more preferably 12% or less. By setting the content at or above the lower limit, the liquid crystal element tends to exhibit greater light absorption in the colored state, and the amount of transmitted light tends to be smaller, while by setting the content at or below the upper limit, separation or precipitation of the dichroic dye is less likely to occur, and the reliability of the liquid crystal element tends to be improved.
[0037] The liquid crystal composition may have either positive or negative dielectric anisotropy (Δε), but a positive one is preferable since it can increase the transmittance in the transparent state. The refractive index anisotropy (Δn) of the liquid crystal composition is preferably 0.01 or more and 0.2 or less. When Δn is equal to or less than the upper limit, light scattering at the interface between the polymer matrix and the liquid crystal region is maintained, and a decrease in haze in the transparent state tends to be suppressed. At the same time, light scattering in the colored state is also maintained, so that the efficiency of light absorption of the dichroic dye is suppressed, and the total transmittance tends to be increased. On the other hand, when Δn is equal to or more than the lower limit, the order parameter of the liquid crystal composition tends to be large.
[0038] The liquid crystal used in the liquid crystal composition may be a nematic liquid crystal, a cholesteric liquid crystal, a smectic liquid crystal, etc. In view of low cost, a nematic liquid crystal or a cholesteric liquid crystal is preferable. A chiral agent may be added to a nematic liquid crystal to form a cholesteric liquid crystal.
[0039] When using a known liquid crystal material as the liquid crystal, specifically, various low molecular compounds or mixtures such as biphenyl, phenylcyclohexane, cyclohexylcyclohexane, etc., as described in "Liquid Crystal Device Handbook" edited by the 142nd Committee of the Japan Society for the Promotion of Science, Nihon Kogyo Shimbunsha (1989), pages 152 to 192, and "Liquid Crystal Handbook" edited by the Liquid Crystal Handbook Editorial Committee, Maruzen Co., Ltd. (2000), pages 260 to 330, can be used. Also, polymer compounds or mixtures as described in "Liquid Crystal Handbook" edited by the Liquid Crystal Handbook Editorial Committee, Maruzen Co., Ltd. (2000), pages 365 to 415, can be used. Examples of compounds constituting nematic liquid crystals include the following compounds.
[0040] [ka]
[0041] Nematic liquid crystals and cholesteric liquid crystals having low viscosity and high dielectric anisotropy are preferred from the viewpoints of high-speed response of liquid crystal elements and ease of production of emulsions. The chiral agent may be any chiral compound that is compatible with the host liquid crystal, and may be a synthetic product or a commercially available product. The chiral agent may be one that exhibits liquid crystallinity by itself, or may have a polymerizable functional group. The chiral agent may be dextrorotatory or levorotatory, and a dextrorotatory chiral agent and a levorotatory chiral agent may be used in combination. In addition, a chiral agent having a large positive dielectric anisotropy and low viscosity is preferred from the viewpoint of reducing the driving voltage and response speed of a liquid crystal element, and a large Helical Twisting Power, which is an index of the force with which the chiral agent twists the liquid crystal, is preferred. Examples of the chiral agent include CB15 (product name, manufactured by Merck Co., Ltd.), C15 (product name, manufactured by Merck Co., Ltd.), S-811 (product name, manufactured by Merck Co., Ltd.), R-811 (product name, manufactured by Merck Co., Ltd.), S-1011 (product name, manufactured by Merck Co., Ltd.), and R-1011 (product name, manufactured by Merck Co., Ltd.).
[0042] The liquid crystal composition may contain additives within the range that does not impair the performance of the liquid crystal element of the present invention. Specifically, the liquid crystal composition may contain a polymer precursor, a polymerization initiator, a light stabilizer, an antioxidant, a thickener, a polymerization inhibitor, a photosensitizer, an adhesive, a defoamer, a surfactant, etc.
[0043] [Dichroic dye] The dichroic dye used in the liquid crystal composition may be any dichroic dye compound that is compatible with the host liquid crystal, and may be a positive dichroic dye or a negative dichroic dye. In addition, the dichroic dye itself may exhibit liquid crystallinity. Specifically, azo dyes, anthraquinone dyes, naphthoquinone dyes, perylene dyes, quinophthalone dyes, tetrazine dyes, benzothiadiazole dyes, etc. can be mentioned. When using a known dichroic dye, it is possible to use azo dyes, anthraquinone dyes, or mixtures thereof as described in "Liquid Crystal Device Handbook" edited by the 142nd Committee of the Japan Society for the Promotion of Science, Nihon Kogyo Shimbunsha (1989), pages 192 to 196 and 724 to 730. Among these, it is preferable to include anthraquinone dyes, since they tend to have a large absorption coefficient, a high solubility in liquid crystal, and high light resistance. The dichroic dye may be one type or a mixture of two or more types. Although there is no particular limitation, it is preferable that the dichroic dye contains an anthraquinone-based dye in an amount of 20% by mass or more, and more preferably 50% by mass or more.
[0044] Specific examples of the dichroic dye constituting the liquid crystal composition include the following compounds.
[0045] [ka]
[0046] In the above compounds, each X independently represents -NH- or -S-; R represents a hydrogen atom, an alkyl group, an alkoxy group, a cyclohexyl group which may have a substituent, a phenyl group, a phenylcyclohexyl group, or a cyclohexylcyclohexyl group.
[0047] [Polymer matrix] The polymer matrix of the present invention is not particularly limited, but is preferably selected so that its refractive index matches the ordinary refractive index (no) of the liquid crystal composition. Typically, the no of a liquid crystal composition is about 1.5, so that the refractive index is preferably 1.45 or more and 1.55 or less. Examples of polymers constituting the polymer matrix include natural polymers such as gelatin and gum arabic; synthetic polymers and modified products thereof such as polyvinyl alcohol, polyurethane, polyurea, polyacrylic, polyamine, polyamide, polyethylene, polypropylene, polystyrene, and polyacrylonitrile; copolymers such as methacrylate / acrylonitrile, urethane / acrylate, and acrylate / acrylonitrile; etc. A crosslinking structure may be introduced into the polymer using a crosslinking agent. The polymer is preferably one that is highly dispersible or soluble in water, and is preferably gelatin, polyvinyl alcohol, polyurethane, polyurea, polyacrylic, polyamine, or modified products thereof, more preferably polyvinyl alcohol, polyurethane, polyacrylic, or modified products thereof, and particularly preferably polyurethane, polyacrylic, or modified products thereof. The polymer may be used alone or in combination of two or more kinds.
[0048] (Polyurethane) Polyurethanes are classified according to the skeleton of polyisocyanate and polyol. Examples of polyisocyanate skeletons include aliphatic polyurethanes made of aliphatic carbon skeletons, and aromatic polyurethanes containing aromatic rings in polyisocyanates. Among these, aliphatic polyisocyanates are preferred because of their high light resistance. Examples of polyol skeletons include polyethers, polyesters, and polycarbonates, and among these, polyethers are preferred because of their good film adhesion.
[0049] (Polyacrylic) Polyacrylic is composed of various acrylate polymers, and examples of acrylic monomers include compounds represented by the following formula (1).
[0050] [ka]
[0051] In the above formula (1), X 1each independently represents a hydrogen atom or a methyl group, R 1 represents a hydrogen atom, a halogen atom, a hydroxyl group, a linear or branched alkyl group having from 1 to 20 carbon atoms which may have a substituent, a linear or branched alkoxy group having from 1 to 20 carbon atoms which may have a substituent, or a cyclic hydrocarbon group having from 1 to 10 carbon atoms which may have a substituent.
[0052] Polyacrylic may be copolymerized with monomers other than acrylate, and examples of the copolymers include acrylate-styrene, acrylate-vinyl acetate, acrylate-acrylonitrile, acrylate-urethane, acrylate-ester, acrylate-silicone, etc. The main chain may be composed of a copolymer of acrylate and other monomers, or other polymers may be grafted onto the polyacrylic main chain.
[0053] The polymer matrix may contain low molecular weight substances within the range that does not impair the performance of the liquid crystal element of the present invention. Specific examples of such substances include light stabilizers, antioxidants, thickeners, polymerization inhibitors, photosensitizers, adhesives, defoamers, and surfactants.
[0054] [Ratio of Liquid Crystal Composition to Polymer Matrix] In the liquid crystal-polymer composite film of the present invention, the ratio of the total mass of the liquid crystal composition to the total mass of the polymer matrix is preferably 0.5 or more, more preferably 1 or more, and more preferably 4 or less, more preferably 3 or less, assuming that the total mass of the liquid crystal composition is 1. When the total mass of the liquid crystal composition is equal to or greater than the lower limit relative to the total mass of the polymer matrix, the haze in the transparent state tends to be low and the driving voltage tends to be low. Also, when the total mass of the liquid crystal composition is equal to or less than the upper limit relative to the total mass of the polymer matrix, the impact resistance and adhesion of the liquid crystal-polymer composite film tend to be improved.
[0055] [Example of liquid crystal element configuration] Representative configurations of the liquid crystal element of the present invention will be described below, but the present invention is not limited to these.
[0056] [substrate] Examples of the material for the substrate include inorganic transparent substances such as glass and quartz, and colorless and transparent substances such as metals, metal oxides, semiconductors, ceramics, plastic plates, plastic films, etc. These substrates may be used as a single plate or may be laminated in multiple layers. The substrate may be provided with a hard coat layer for the purpose of protecting it from scratches and dirt, or with a sharp cut layer or band pass layer for blocking light rays in a specific wavelength range.
[0057] [Transparent conductive film] The electrodes are formed on the substrate by, for example, forming a thin film of a metal oxide, metal, semiconductor, organic conductive material, etc., on the entire surface or part of the substrate by a known coating method, printing method, deposition method such as sputtering, etc. Alternatively, the electrodes may be formed by partially etching after forming a conductive thin film. In particular, in order to obtain a large-area liquid crystal element, it is desirable to use an electrode substrate in which an ITO (mixture of indium oxide and tin oxide) electrode is formed on a transparent polymer film such as PET by deposition method such as sputtering, printing method, etc., from the viewpoint of productivity and processability. In addition, wiring for connecting between electrodes or between the electrodes and the outside may be provided on the substrate. For example, the substrate may be a segment driving electrode substrate, a matrix driving electrode substrate, an active matrix driving electrode substrate, etc.
[0058] Furthermore, the electrode surface provided on the substrate may be entirely or partially covered with a protective film or an alignment film made of an organic compound such as polyimide, polyamide, silicon, or a cyan compound, an inorganic compound such as SiO2, TiO2, or ZrO2, or a mixture thereof. The substrate may be subjected to an alignment treatment so as to align the liquid crystal with respect to the substrate surface. When the substrate is oriented, for example, both substrates may be homogeneous or homeotropic, or one substrate may be homogeneous and the other substrate may be homeotropic, so-called hybrid. For these alignment treatments, the electrode surface may be directly rubbed, a normal alignment film such as polyimide used in TN liquid crystal, STN liquid crystal, etc. may be used, or a photo-alignment treatment may be performed.
[0059] The opposing substrate may have an adhesive layer containing a resin body on the periphery thereof to adhere and support the substrate. The end or cut surface of the liquid crystal element of the present invention can be sealed with tapes such as adhesive tape, thermocompression tape, and thermosetting tape, curable resins such as thermosetting resins, photocurable resins, moisture-curable resins, room-temperature curable adhesives, anaerobic adhesives, epoxy adhesives, silicone adhesives, fluororesin adhesives, polyester adhesives, and vinyl chloride adhesives, or thermoplastic resins, to prevent the liquid crystal composition from seeping out. This sealing may also have the effect of preventing the liquid crystal element from deteriorating. In this case, the end surface may be protected by covering the entire end surface, or by pouring curable resins or thermoplastic resins into the liquid crystal element from the end surface and solidifying the resins, and then covering the end surface with tapes.
[0060] Between the opposing substrates, there may be provided a spacer such as a spherical or cylindrical glass, plastic, ceramic, or plastic film. The spacer may be included as a component of the emulsion composition of the present invention so that it is present in the liquid crystal-polymer composite film between the substrates, or it may be dispersed on the substrates during assembly of the liquid crystal element, or may be mixed with an adhesive so that it is present in the adhesive layer.
[0061] [Method for producing liquid crystal-polymer composite film] The liquid crystal-polymer composite film of the present invention can be produced by applying an emulsion composition onto an electrode substrate and drying it. As the application method, a known application method such as bar coating, blade coating, knife coating, die coating, screen coating, microgravure roll coating, reverse roll coating, kiss roll coating, dip roll coating, spin coating, spray coating, etc. may be used. Depending on the properties of the substrate, the substrate may be washed as appropriate. The wet film thickness at the time of coating is preferably 10 μm or more, more preferably 20 μm or more. Also, it is preferably 50 μm or less, more preferably 40 μm or less. When the wet film thickness is equal to or more than the upper limit, there is a tendency that the liquid crystal particles are not coarse and dense, and the coating can be performed uniformly. Also, when the wet film thickness is equal to or less than the lower limit, there is a tendency that the driving voltage is reduced to a practical value, and the haze in the transparent state is reduced. The drying temperature when the emulsion composition is applied and dried is preferably 40° C. or higher, more preferably 60° C. or lower. Also, it is preferably 120° C. or lower, more preferably 100° C. or lower. By setting the drying temperature to the above lower limit or higher, the drying time is shortened to a practical time, and the amount of water remaining in the film is reduced, which tends to improve the reliability of the liquid crystal element. Also, by setting the drying temperature to the above upper limit or lower, the emulsion composition tends to be less likely to undergo structural destruction such as coalescence or inversion during drying.
[0062] <Emulsion Composition> The emulsion composition of the present invention is an emulsion in which a liquid crystal composition is dispersed in a medium containing water, and a polymer is dispersed or dissolved in the medium, and is characterized in that the liquid crystal composition contains a dichroic dye, the dielectric anisotropy of the liquid crystal composition is positive, the refractive index anisotropy of the liquid crystal composition is 0.01 or more and 0.2 or less, and the average particle size of the liquid crystal composition is more than 2 μm and less than 50 μm.
[0063] The liquid crystal composition contained in the emulsion composition is not particularly limited, and may be any of the liquid crystal compositions used in the liquid crystal element described above. The water-containing medium contained in the emulsion composition is also not particularly limited, and may be pure water or a mixture of water and an organic solvent. Examples of the organic solvent include alcohols, ketones, ethers, esters, carboxylic acids, amines, etc. The organic solvent may be water-soluble or oil-soluble to the extent that it is slightly soluble in water, but it is preferable to mix it in an amount that dissolves uniformly in water. Examples of the polymer dispersed or dissolved in the medium include natural polymers such as gelatin and gum arabic; synthetic polymers such as polyvinyl alcohol, polyurethane, polyurea, polyacrylic, polyamine, polyamide, polyethylene, polypropylene, polystyrene, and polyacrylonitrile, and modified products thereof; and copolymers such as methacrylate / acrylonitrile, urethane / acrylate, and acrylate / acrylonitrile. The polymer is preferably one that is highly dispersible or soluble in water, and gelatin, polyvinyl alcohol, polyurethane, polyurea, polyacrylic, polyamine, and modified products thereof are preferred, polyvinyl alcohol, polyurethane, polyacrylic, and modified products thereof are more preferred, and polyurethane is particularly preferred. The polymer may be used alone or in combination of two or more kinds.
[0064] In the present invention, the dispersion of a polymer refers to a state in which polymer particles are suspended in a medium, and the dissolution of a polymer refers to a state in which the polymer is dissociated into sufficiently small particles by solvation to form a homogeneous system. For details on the dispersion and dissolution of polymers, see "Color Materials," Color Materials Association (2004), Vol. 77, No. 4, pp. 169-176.
[0065] In the emulsion composition, the liquid crystal composition is dispersed in a medium containing water. The liquid crystal composition may be dispersed in a liquid state or may be dispersed in the form of microencapsulated liquid crystal in which the periphery of the liquid crystal composition is encapsulated with a polymer, a silica compound, inorganic nanoparticles, or the like. Examples of polymers that can be used as capsules in microcapsule liquid crystals include natural polymers such as gelatin and gum arabic; synthetic polymers such as polyvinyl alcohol, polyurethane, polyurea, polyacrylic, polyamine, polyamide, polyethylene, polypropylene, polystyrene, and polyacrylonitrile, and modified versions thereof; and copolymers such as methacrylate / acrylonitrile, urethane / acrylate, and acrylate / acrylonitrile.
[0066] The emulsion composition may contain additives within the range that does not impair the performance of the liquid crystal element of the present invention. Specific examples of additives include surfactants, emulsifiers, dispersants, anti-settling agents, film-forming assistants, leveling agents, light stabilizers, antioxidants, thickeners, polymerization inhibitors, photosensitizers, adhesives, and defoamers.
[0067] The refractive index anisotropy (Δn) of the liquid crystal composition is preferably 0.01 or more and 0.2 or less. When Δn is equal to or less than the upper limit, the light scattering of the liquid crystal-polymer composite film is weakened, the light absorption of the dichroic dye in the colored state is increased, and the haze in the transparent state tends to be reduced. On the other hand, when Δn is equal to or more than the lower limit, the order parameter of the liquid crystal composition is increased, and the light absorption of the dichroic dye in the transparent state tends to be reduced.
[0068] The particle size of the liquid crystal composition is preferably 2 μm or more, more preferably 5 μm or more, and more preferably 50 μm or less, and more preferably 30 μm or less. When the average particle size is larger than the lower limit, the light scattering at the interface between the polymer matrix and the liquid crystal region in the liquid crystal-polymer composite film is weakened, and the haze in the transparent state tends to be smaller. At the same time, the light scattering in the colored state is also weakened, and the efficiency of light absorption of the dichroic dye is improved, and the total transmittance in the colored state tends to be lower. In addition, when the average particle size is smaller than the upper limit, the graininess of the liquid crystal region is eliminated, and the uniformity of the appearance of the liquid crystal element tends to be improved. Note that the average particle size is the median diameter based on the number of particles.
[0069] In the particle size distribution based on the number of particles of the liquid crystal composition, the coefficient of variation CV is σ / m, where m is the average particle size and σ is the standard deviation of normal distribution. The coefficient of variation (CV) is preferably 0.8 or less, more preferably 0.5 or less, more preferably 0.3 or less, and even more preferably 0.1 or less. When the coefficient of variation is equal to or less than the upper limit, the number of small particles that cause scattering and large particles that cause graininess tend to be sufficiently reduced. On the other hand, the coefficient of variation is preferably equal to or greater than the lower limit, more preferably equal to or greater than 0.005, and even more preferably equal to or greater than 0.01. When the coefficient of variation is equal to or greater than 0.001, the productivity of the emulsion composition tends to improve.
[0070] In the particle size frequency distribution based on the number of liquid crystal regions, the particle size of 2 μm or less is preferably 20% or less in cumulative, more preferably 10% or less in cumulative, and even more preferably 5% or less in cumulative. By being 20% or less in cumulative, the light scattering of the liquid crystal-polymer composite film is weakened, the light absorption of the dichroic dye in the colored state is increased, and the haze in the transparent state tends to be reduced. On the other hand, the cumulative amount is preferably 0.1% or more, more preferably 0.5% or more, and even more preferably 1% or more. A cumulative amount of 0.1% or more is preferable because the productivity of the emulsion composition is improved. Moreover, the particle size of 50 μm or more is preferably 20% or less in cumulative, more preferably 10% or less in cumulative, and even more preferably 5% or less in cumulative. By keeping the particle size at 20% or less in cumulative, the graininess of the liquid crystal region is eliminated, and the uniformity of the appearance of the liquid crystal element tends to be improved. On the other hand, the cumulative amount is preferably 0.1% or more, more preferably 0.5% or more, and even more preferably 1% or more. A cumulative amount of 0.1% or more is preferable because the productivity of the emulsion composition is improved.
[0071] The ratio of the total mass of the liquid crystal composition to the total mass of the polymer dispersed or dissolved in the medium is preferably 0.5 or more, more preferably 1 or more, and is preferably 4 or less, more preferably 3 or less. When the total mass of the liquid crystal composition is equal to or greater than the lower limit relative to the total mass of the polymer, the haze in the transparent state of the liquid crystal element obtained by using the emulsion composition tends to be low and the driving voltage tends to be low. Also, when the total mass of the liquid crystal composition is equal to or less than the upper limit relative to the total mass of the polymer, the impact resistance and adhesion of the liquid crystal element obtained by using the emulsion composition tends to be improved.
[0072] [Dichroic dye] The dichroic dye contained in the emulsion composition is not particularly limited, and may be any of the dichroic dyes used in the liquid crystal element described above. Among them, it is preferable to contain an anthraquinone dye, since it has a large absorption coefficient, a high solubility in the liquid crystal, and tends to have high light resistance. The dichroic dye may be one type or a mixture of two or more types. Although there is no particular limitation, it is preferable that the dichroic dye contains an anthraquinone-based dye in an amount of 20% by mass or more, and more preferably 50% by mass or more.
[0073] [Method of producing emulsion composition] The method for producing the emulsion composition of the present invention is not particularly limited, but it can be produced, for example, as follows. Manufacturing method (1) A liquid crystal composition as an oil phase and a water-containing medium as an aqueous phase are mixed, and after an emulsification process, a liquid in which a polymer is dispersed or dissolved in the aqueous medium is added. Production method (2) A liquid in which a polymer is dispersed or dissolved is mixed with a liquid crystal composition as an oil phase and a medium containing water as an aqueous phase, and an emulsification step is carried out. Manufacturing method (3): A powder or slurry of microencapsulated liquid crystal, in which the peripheral portion of the liquid crystal composition is encapsulated with a polymer, a silica compound, inorganic nanoparticles, etc., is mixed with a medium containing water, and after a dispersion process, a liquid in which a polymer is dispersed or dissolved is added to the medium containing water. Production method (4) A dispersion step is carried out by mixing the powder or slurry of the microencapsulated liquid crystal with a liquid in which a polymer is dispersed or dissolved in a medium containing water. Among these, production methods (1) and (3) are preferred because they allow the emulsification step or dispersion step to be carried out while the mixture is in a low viscosity state, making it possible to produce the liquid crystal composition with low energy consumption, and further, making it easy to control the particle size of the liquid crystal composition.
[0074] As the liquid in which a polymer is dispersed or dissolved in a medium containing water, a commercially available aqueous resin emulsion can be used. Specific examples are shown below. Water-based urethane emulsion: NeoRez R-9660, NeoRez R-972, NeoRez R-9637, NeoRez R-9679, NeoRez R-960, NeoRez R-2170, NeoRez R-966, NeoRez R-967, NeoRez R-986, NeoRez R-9603, NeoRez R-4000, NeoRez R-9404, NeoRez R-600, NeoRez R-650, NeoRez R-1010 manufactured by DSM; Superflex 126, Superflex 130, Superflex 150, Superflex 150HS, Superflex 170, Superflex 210, Superflex 300, Superflex 420, Superflex manufactured by Daiichi Kogyo Seiyaku Co., Ltd. 420NS, Superflex 460, Superflex 460S, Superflex 470, Superflex 500M, Superflex 620, Superflex 650, Superflex 740, Superflex 820, Superflex 830HS, Superflex 860, Superflex 870, Superflex E-2000, Superflex E-4800, NICCA Chemical Co., Ltd. Neosticker 200, Neosticker 400, Neosticker 700, Neosticker 1200, Neosticker X-7096, Evafanol HA-107C, Evafanol HA-50C, Evafanol HA-170, Evafanol HA-560, Evafanol HA-15, Evafanol AP-12, Evafanol APC-55. Water-based acrylic emulsion: NeoCryl A-633, NeoCryl A-639, NeoCryl A-655, NeoCryl A-662, NeoCryl A-1091, NeoCryl A-1092, NeoCryl A-1093, NeoCryl A-1094, NeoCryl A-2091, NeoCryl A-2092, NeoCryl A-6016, NeoCryl A-6057, NeoCryl A-6069, NeoCryl A-6092, NeoCryl A-614, NeoCryl A-550, NeoCryl A-1105, NeoCryl A-1125, NeoCryl A-1127, NeoCryl XK-12, NeoCryl XK-16, NeoCryl XK-30, NeoCryl XK-36, NeoCryl XK-52, NeoCryl XK-190, NeoCryl XK-188, NeoCryl XK-240, Japan Coating Resin Co., Ltd. Rikabond 702, Rikabond 727, Rikabond 743N, Rikabond 745, Rikabond 752, Rikabond 801, Rikabond 940, Rikabond 972, Rikabond 1711, Rikabond 1752, Rikabond 6520, Rikabond 6720, Rikabond 7110, Rikabond 7180, Rikabond 7525, Rikabond 7820, Rikabond 8020, Rikabond 8030, Rikabond DM60, Rikabond DM772, Rikabond DM774, Rikabond LDM6740, Rikabond LDM7522, Rikabond LDM7523, Rikabond ES-65, Rikabond ES-90, Rikabond ET-700, Rikabond ET-831, Rikabond HS-5, Rikabond HS-531, Rikabond AP-601, Rikabond AP-96, Rikabond AP-620, Rikabond AP-700, Rikabond AP-80, Rikabond 710A, Rikabond 730L, Rikabond 731L, Rikabond 952B, Rikabond 966A, Rikabond 7320, Rikabond 7400, Rikabond FK-420, Rikabond FK-64S, Rikabond FK-66IS, FK-66N, FK-68H, Rikabond FK-471, Rikabond FK-475, RikabondFK-489, Rikabond FK-284, Rikabond FK-600S, Rikabond FK-3830, Rikabond FK-3840, Rikabond FK-6100, Mowinyl VDM7410, Mowinyl 4061, Mowinyl 4080, Mowinyl 4090, Mowinyl 4050, Mowinyl S-71, Mowinyl 461, Mowinyl 650, Mowinyl AP-60L, Mowinyl 490. Among the above, NeoRez R-966, NeoRez R-967, NeoCryl A-1125, NeoCryl A-1127, Rikabond FK-471, Mowinyl 4061, Mowinyl 4080 and Mowinyl 4090 are preferred because they have excellent dispersion stability of the oil phase.
[0075] In order to obtain a stable emulsion, it is preferable to add a surfactant or dispersion stabilizer before the emulsification step or the dispersion step. The surfactant is not particularly limited, and may be ionic or nonionic, low molecular or high molecular, non-reactive or reactive. The amount of the surfactant added is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, based on the liquid crystal composition. Also, it is preferably 20% by mass or less, more preferably 10% by mass or less. When the surfactant is in the above range, the dispersion of the emulsion is stabilized, and the particle size of the liquid crystal composition tends to be controlled within a desired range.
[0076] The surfactant may be added to the liquid crystal composition or to a medium containing water depending on the solubility. Examples of the surfactant include anionic surfactants such as carboxylates, sulfonates, sulfates, and phosphates; Cationic surfactants such as amine salts and quaternary ammonium salts; amphoteric surfactants such as alkylamino fatty acid salts, alkylamine oxides, betaines, sulfobetaines, amidosulfobetaines, carbobetaines, and imidazolines; Examples of the surfactants include ether types such as polyoxyethylene alkyl ethers, polyoxyethylene alkylaryl ethers, polyoxyethylene aralkyl ethers, polyoxyethylene aralkyl aryl ethers, polyoxyethylene polyoxypropylene block adducts, alkyl glucosides, and polyether-modified silicones; ester types such as glycerin fatty acid esters, sorbitan fatty acid esters, and sucrose fatty acid esters; ester / ether types such as polyoxyethylene fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and polyoxyethylene sucrose fatty acid esters; acetyl types such as acetyl-modified polyvinyl alcohol; and nonionic surfactants such as fatty acid alkanolamides. Among these, anionic surfactants are preferred because of their high water solubility and dispersion stability, and sulfonates are particularly preferred.Nonionic surfactants are also preferred because they tend to increase the electrical reliability of liquid crystal elements.Among these, ether or ester types are preferred, and polyoxyethylene alkyl ethers, polyoxyethylene alkyl aryl ethers, polyoxyethylene aralkyl ethers, polyoxyethylene aralkyl aryl ethers, polyoxyethylene polyoxypropylene block adducts, acetyl-modified polyvinyl alcohol, and the like are particularly preferred.
[0077] The dispersion stabilizer is not particularly limited, and examples thereof include polymers such as polyvinyl alcohol, polyvinylpyrrolidone, methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, polyethylene glycol, polyacrylic acid, polymethacrylic acid, polyurethane, polyamine, polyamide, polyether, maleic acid copolymer, gelatin, starch, chitosan, and corn starch, and modified products thereof; Copolymers such as methacrylate / acrylonitrile, urethane / acrylate, and acrylate / acrylonitrile; Examples of the fine particles include inorganic oxide fine particles such as silica fine particles, titania fine particles, and alumina fine particles. Among these, polyvinyl alcohol, modified polyvinyl alcohol, polyurethane, polyamide, etc. are preferred because of their high dispersion stability.
[0078] The polyvinyl alcohol has a saponification degree of preferably 80 mol % or more, more preferably 85 mol % or more, and preferably 95 mol % or less, more preferably 91 mol % or less. When the saponification degree is within these ranges, the solubility in a medium containing water tends to be high. The degree of polymerization of polyvinyl alcohol is preferably at least 100, and more preferably at least 300. The degree of polymerization is preferably at most 2500, and more preferably at most 1000. Within these ranges, the film tends to have excellent flexibility. Specifically, these are manufactured by Nippon Synthetic Chemical Industry Co., Ltd.: GOHSENOL GL-03, GOHSENOL GL-05, GOHSENOL GM-14L, GOHSENOL GM14, GOHSENOL GH-17, GOHSENOL GH-20, GOHSENOL GH-23, GOHSENOL AL-06, GOHSENOL P-610, and GOHSENOL C-500; and Kuraray Co., Ltd.: Kuraray Poval 25-88KL, Kuraray Poval 32-97KL, Kuraray Poval 3-86SD, Kuraray Poval 105-88KX, and Kuraray Poval 200-88KX. Examples of the polyvinyl chloride include Denka Poval H-12, Denka Poval H-17, Denka Poval H-24, Denka Poval B-05, Denka Poval B-17, Denka Poval B-20, Denka Poval B-24, and Denka Poval B-33, all of which are manufactured by Denka Corporation.
[0079] In producing the emulsion composition, the emulsification method and dispersion method are not particularly limited, and examples thereof include a method of mechanically crushing particles using a stirrer, homogenizer, homomixer, disperser, high-pressure emulsifier, blender, colloid mill, ultrasonic disperser, etc.; a method of extruding a liquid through pores using a porous membrane, microchannel, inkjet, etc.; and the like. Among the above, the method of using a porous membrane to push the liquid through the pores (membrane emulsification method) is preferred because it allows precise control of the particle size distribution and is easy to manufacture. There is no particular restriction on the porous membrane, but shirasu porous glass, etc. can be used.
[0080] A crosslinking agent may be used in the emulsion composition as appropriate. The use of a crosslinking agent tends to improve the water resistance and impact resistance of the liquid crystal-polymer composite film. The crosslinking agent is not particularly limited, and examples thereof include epoxy compounds such as ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerol diglycidyl ether, polyglycerin polyglycidyl ether, and diglycidylaniline; Epoxysilane compounds such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyldimethoxymethylsilane, γ-glycidoxypropyldiethoxymethylsilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltriethoxysilane; Aminosilane compounds such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane; mercaptosilane compounds such as γ-mercaptopropyltrimethoxysilane; Hydrazide compounds such as carbodihydrazide, oxalic dihydrazide, adipic dihydrazide, sebacic dihydrazide, and isophthalic dihydrazide; Semicarbazide resin; Polycarbodiimide resins; Aziridine-based (ethyleneimino group-containing) compounds such as tetramethylolmethane-tris(β-aziridinylpropionate), trimethylolpropane-tris(β-aziridinylpropionate), methylenebis[N-(1-aziridinylcarbonyl)-4-aniline], N,N'-hexamethylenebis(1-aziridinecarboxamide), and N,N'-hexaaminoethylene-1,6-bis(1-aziridinecarboxamide); Acetoacetoxy group-containing compounds;Oxazoline group-containing compounds; Polyethylene polyamines;Polyethyleneimines;Polyamide polyamines;Polyamide polyureas;Alkylated polymethylol melamines;Glyoxal; Examples of the isocyanate include water-dispersible isocyanates, blocked isocyanates, carbodiimide group-containing compounds, bisvinyl sulfones, and lactic acid titanates. When an epoxy compound or an epoxysilane compound is used, a catalyst such as an imidazole compound, an amine compound, or a phosphorus compound may be added. Among the above, hydrazide compounds, oxazoline group-containing compounds, carbodiimide group-containing compounds, and blocked isocyanates are preferred because they have a high crosslinking rate and low toxicity. Any combination of a polymer and a crosslinking agent can be used, but combinations of polyurethane and an oxazoline group-containing compound, polyurethane and a carbodiimide group-containing compound, polyurethane and a blocked isocyanate, and polyacrylic and a hydrazide compound tend to have high crosslinking reactivity and are therefore preferred.
[0081] The amount of the crosslinking agent added is not particularly limited, but is preferably 0.1% by mass or more, more preferably 1% by mass or more, based on the resin to be crosslinked. Also, it is preferably 20% by mass or less, more preferably 10% by mass or less. When the amount of the crosslinking agent added is within the above range, the water resistance and impact resistance of the liquid crystal-polymer composite film tend to be improved and the flexibility is maintained. The timing of addition of the crosslinking agent may be a one-liquid type in which the crosslinking agent is added to the emulsion composition from the beginning, or a two-liquid type in which the crosslinking agent is added immediately before application to the substrate.
[0082] The viscosity of the emulsion composition is preferably 10 mPa·s or more, more preferably 100 mPa·s or more, and is preferably 10,000 mPa·s or less, more preferably 2,000 mPa·s or less. If the viscosity is within the above range, it becomes easy to apply a uniform film thickness, and the application speed can be increased, which tends to increase productivity. In order to keep the viscosity within the above range, viscosity adjusters such as thickeners, thixotropic agents, and viscosity reducers may be used. Viscosity adjusters are not particularly limited, but include polyvinyl alcohol, polyvinylpyrrolidone, methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, polyethylene glycol, polyacrylic acid, polymethacrylic acid, polyurethane, polyamine, polyamide, maleic acid copolymer, gelatin, starch, chitosan, corn starch, and other polymers and modified products thereof; copolymers such as methacrylate / acrylonitrile, urethane / acrylate, and acrylate / acrylonitrile; inorganic oxide fine particles such as silica fine particles, titania fine particles, and alumina fine particles. Among the above, polyvinyl alcohol and its modified products, polyurethane, and polyamide tend to be able to achieve both viscosity adjustment and particle dispersion stability, and are therefore preferred.
[0083] The content of the liquid crystal composition in the emulsion composition is preferably 20% by mass or more, more preferably 30% by mass or more, and more preferably 70% by mass or less, more preferably 65% by mass or less. When the content of the liquid crystal composition is within the above range, repelling that occurs when the emulsion composition is applied to a substrate is suppressed, and it tends to be easy to keep the particle size and viscosity of the liquid crystal composition within the above range.
[0084] The particle size of the polymer used in the emulsion composition is preferably 1 nm or more, more preferably 10 nm or more. Also, it is preferably 1000 nm or less, more preferably 200 nm or less. By being within the above range, it tends to be easier to keep the viscosity of the emulsion composition within the above range. Also, the molecular weight of the polymer is 1.0×10 3 More than 1.0×10 is preferable. 4 More preferably, 1.0×10 6 Less than or equal to 1.0×10 is preferred. 5 The following is more preferable. By being within the above range, it tends to be easier to keep the viscosity of the emulsion composition within the above range. EXAMPLES
[0085] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as the gist of the present invention is not exceeded.
[0086] [Example 1] 96% by mass of nematic liquid crystal with Δn=0.08 and Δε=+5.0 was mixed with 4% by mass of anthraquinone dichroic dye represented by (D-1), and D-1 was dissolved to obtain liquid crystal composition (L-1). 50% by mass of 4% by mass of sodium dodecylbenzenesulfonate aqueous solution was added to 50% by mass of L-1, and emulsified by passing through Shirasu porous glass to obtain o / w emulsion (E-1). To 45 parts by mass of E-1, 38 parts by mass of Neorez R-967 (manufactured by DSM), an aqueous latex containing 40% by mass of polyurethane particles, was added, and 4.4 parts by mass of modified polyamide AQH-800 (manufactured by Kusumoto Chemicals) with a non-volatile content of 10 wt% was further added, and the mixture was stirred until uniform, to obtain emulsion composition (I-1). The average particle size of the liquid crystal composition in I-1 was 6.2 μm, and the coefficient of variation was 0.57. When the mass of the polymer (P-1) dispersed or dissolved in the aqueous phase in I-1 was 1, the mass of L-1 was 1.44.
[0087] [ka]
[0088] The substrate used was a 125μm thick PET film with a transparent ITO electrode formed on it. I-1 was applied to the ITO of this substrate with a bar coater to a wet thickness of 30μm and dried at 80℃ to obtain a liquid crystal-polymer composite film. When the liquid crystal-polymer composite film was observed from above with a microscope, it was found to have a structure in which liquid crystal particles with an average particle size of 7.6 μm and a coefficient of variation of 0.25 were dispersed in the polymer matrix. The film and another substrate were attached face-to-face at 80° C. to obtain a liquid crystal element (F-1). F-1 was flexible and could be cut with scissors to any desired shape.
[0089] F-1 showed normal mode operation, colored blue when the voltage was off, and became transparent when the voltage was on (50Vrms). When the voltage was off, the haze was 50.7% and the total transmittance was 62.6% at λmax=670nm. When a voltage of 50Vrms was applied, the haze was 2.1% and the total transmittance was 32.0% at λmax=670nm, showing ΔT=30.7%. When the background was visually observed through the transparent F-1, there was little turbidity and a clear view was ensured.
[0090] [Example 2] Except for changing the average particle size of the liquid crystal composition in the emulsion composition to 2.9 μm and the coefficient of variation to 0.31, emulsion composition I-2 was obtained in the same manner as in Example 1. In I-2, assuming that the mass of the polymer (P-1) dispersed or dissolved in the aqueous phase was 1, the mass of L-1 was 1.44.
[0091] Using I-2, a liquid crystal element (F-2) was obtained in the same manner as in Example 1. When the liquid crystal-polymer composite film of F-2 was observed from above the film surface with a microscope, it had a structure in which a liquid crystal composition with an average particle size of 4.3 μm and a coefficient of variation of 0.20 was dispersed in a polymer matrix. F-2 was flexible and could be cut with scissors to be shaped. F-2 showed normal mode operation, colored blue when the voltage was off, and became transparent when the voltage was on (50Vrms). When the voltage was off, the haze was 51.2% and the total transmittance was 63.7% at λmax=670nm. When a voltage of 50Vrms was applied, the haze was 4.1% and the total transmittance was 34.9% at λmax=670nm, showing ΔT=28.8%. When the background was visually observed through the transparent F-2, there was little turbidity and a clear view was ensured.
[0092] [Example 3] 96% by mass of nematic liquid crystal with Δn=0.12 and Δε=+10.8 and 4% by mass of dichroic dye represented by (1) were mixed, and anthraquinone dichroic dye (D-1) was dissolved to obtain liquid crystal composition (L-2). Except for changing the liquid crystal composition to L-2, an emulsion composition (I-3) was obtained in the same manner as in Example 1. The average particle size of the liquid crystal composition in I-3 was 7.3 μm, and the coefficient of variation was 0.34. When the mass of the polymer (P-1) dispersed or dissolved in the aqueous phase in I-3 was taken as 1, the mass of L-2 was 1.44. A liquid crystal element (F-3) was obtained using I-3 in the same manner as in Example 1. When the liquid crystal-polymer composite film of F-3 was observed from above the film surface with a microscope, it had a structure in which a liquid crystal composition with an average particle size of 8.5 μm and a coefficient of variation of 0.29 was dispersed in a polymer matrix. F-3 was flexible and could be cut with scissors to be shaped.
[0093] F-3 showed normal mode operation, colored blue when the voltage was off, and became transparent when the voltage was on (50Vrms). When the voltage was off, the haze was 50.6% and the total transmittance was 61.0% at λmax=670nm. When a voltage of 50Vrms was applied, the haze was 3.9% and the total transmittance was 32.3% at λmax=670nm, showing ΔT=28.7%. When the background was visually observed through the transparent F-3, there was little turbidity and a clear view was ensured.
[0094] [Example 4] An emulsion composition (I-4) was obtained in the same manner as in Example 1, except that the amount of Neorez R-967 added to 45 parts by mass of E-1 was changed to 21.8 parts by mass. The average particle size of the liquid crystal composition in I-4 was 6.0 μm, and the coefficient of variation was 0.31. In I-4, the mass of the polymer (P-3) dispersed or dissolved in the aqueous phase was 1, and the mass of L-1 was 2.51.
[0095] A liquid crystal element (F-4) was obtained using I-4 in the same manner as in Example 1. When the liquid crystal-polymer composite film of F-4 was observed from above the film surface under a microscope, it had a structure in which a liquid crystal composition with an average particle size of 7.7 μm and a coefficient of variation of 0.21 was dispersed in a polymer matrix. F-4 was flexible and could be cut with scissors to be shaped. F-4 showed normal mode operation, colored blue when the voltage was off, and became transparent when the voltage was on (50Vrms). When the voltage was off, the haze was 35.2% and the total transmittance was 68.6% at λmax=670nm. When a voltage of 50Vrms was applied, the haze was 1.2% and the total transmittance was 43.5% at λmax=670nm, showing ΔT=25.1%. When the background was visually observed through the transparent F-4, there was little turbidity and a clear view was ensured.
[0096] [Comparative Example 1] 96% by mass of nematic liquid crystal with Δn=0.240 and Δε=15.6 was mixed with 4% by mass of dichroic dye represented by (1), and anthraquinone dichroic dye (D-1) was dissolved to obtain liquid crystal composition (L-3). Except for changing the liquid crystal composition to L-3, an emulsion composition (I-5) was obtained in the same manner as in Example 1. The average particle size of the liquid crystal composition in I-5 was 5.9 μm, and the coefficient of variation was 0.24. When the mass of the polymer (P-1) dispersed or dissolved in the aqueous phase in I-3 was taken as 1, the mass of L-3 was 1.44. A liquid crystal element (F-5) was obtained using I-5 in the same manner as in Example 1. When the liquid crystal-polymer composite film of F-5 was observed from above the film surface under a microscope, it had a structure in which a liquid crystal composition with an average particle size of 6.8 μm and a coefficient of variation of 0.19 was dispersed in a polymer matrix. F-5 was flexible and could be cut with scissors to be shaped.
[0097] The F-5 showed normal mode operation, colored blue when the voltage was off, and became transparent when the voltage was on (50 Vrms). When the voltage was off, the haze was 89.0% and the total transmittance was 66.4% at λmax=670 nm. When a voltage of 50 Vrms was applied, the haze was 10.4% and the total transmittance was 42.0% at λmax=670 nm, showing ΔT=24.4%. When the background was visually observed through the F-5 in the transparent state, the visibility was very cloudy and blurred.
[0098] [Comparative Example 2] Except for changing the average particle size of the liquid crystal composition in the emulsion composition to 1.2 μm and the variation coefficient to 0.16, emulsion composition I-6 was obtained in the same manner as in Example 1. In I-6, when the mass of the polymer (P-1) dispersed or dissolved in the aqueous phase was taken as 1, the mass of L-1 was 1.44.
[0099] A liquid crystal element (F-6) was obtained using I-6 in the same manner as in Example 1. When the liquid crystal-polymer composite film of F-6 was observed from above the film surface under a microscope, it had a structure in which a liquid crystal composition with an average particle size of 1.9 μm and a coefficient of variation of 0.18 was dispersed in a polymer matrix. F-6 was flexible and could be cut with scissors to be shaped. F-6 showed normal mode operation, colored blue when the voltage was off, and became transparent when the voltage was on (50Vrms). When the voltage was off, the haze was 49.3% and the total transmittance was 62.5% at λmax=670nm. When a voltage of 50Vrms was applied, the haze was 15.2% and the total transmittance was 41.5% at λmax=670nm, showing ΔT=21.0%. When the background was visually observed through the transparent F-6, the visibility was very cloudy and blurred.
[0100] [Example 5] E-1 17 parts by weight of NeoCryl A-1125 (DSM), a water-based latex containing polyacrylic particles and a crosslinking agent adipic acid dihydrazide in total 20% by weight, The mixture was stirred until it became uniform, to obtain an emulsion composition (I-7). The average particle size of the liquid crystal composition in I-7 was 4.9 μm, and the variation coefficient was 0.37. When the mass of the polymer (P-4) dispersed or dissolved in the aqueous phase in I-7 was 1, the mass of L-1 was 1.67.
[0101] A liquid crystal element (F-7) was obtained using I-7 in the same manner as in Example 1. When the liquid crystal-polymer composite film of F-7 was observed from above the film surface with a microscope, it had a structure in which a liquid crystal composition with an average particle size of 5.1 μm and a coefficient of variation of 0.39 was dispersed in a polymer matrix. F-7 was flexible and could be cut with scissors to be shaped. F-7 showed normal mode operation, colored blue when the voltage was off, and became transparent when the voltage was on (50Vrms). When the voltage was off, the haze was 73.1% and the total transmittance was 38.9% at λmax=670nm. When a voltage of 50Vrms was applied, the haze was 3.4% and the total transmittance was 69.1% at λmax=670nm, showing ΔT=30.2%. When the background was visually observed through the transparent F-7, there was little turbidity and a clear view was ensured.
[0102] [Example 6] E-1 50 parts by mass of Licabond FK-471 (manufactured by Japan Coating Resin Co., Ltd.), an aqueous latex containing polyacrylic particles and a crosslinking agent adipic acid dihydrazide in total at 55% by mass, and 10 parts by mass of a 20% by mass aqueous solution of polyvinyl alcohol with a saponification degree of 86.5 mol% to 89.0 mol% and a polymerization degree of 500, were added and stirred until uniform to obtain an emulsion composition (I-8). The average particle size of the liquid crystal composition in I-8 was 5.9 μm, and the coefficient of variation was 0.27. In I-8, the mass of the polymer (P-5) dispersed or dissolved in the aqueous phase was taken as 1, and the mass of L-8 was 1.26.
[0103] A liquid crystal element (F-8) was obtained using I-8 in the same manner as in Example 1. When the liquid crystal-polymer composite film of F-8 was observed from above the film surface under a microscope, it had a structure in which a liquid crystal composition with an average particle size of 6.1 μm and a coefficient of variation of 0.30 was dispersed in a polymer matrix. F-8 was flexible and could be cut with scissors to be shaped. The F-8 showed normal mode operation, colored blue when the voltage was off, and became transparent when the voltage was on (50Vrms). When the voltage was off, the haze was 60.9% and the total transmittance was 39.1% at λmax=670nm. When a voltage of 50Vrms was applied, the haze was 3.1% and the total transmittance was 68.1% at λmax=670nm, showing ΔT=29.0%. When the background was visually observed through the F-8 in the transparent state, there was little turbidity and a clear view was ensured.
Claims
1. An emulsion composition in which a liquid crystal composition is dispersed in a medium containing water, The medium is a medium in which a polymer is dispersed or dissolved, The liquid crystal composition contains a dichroic dye, the liquid crystal composition has a positive dielectric anisotropy, the liquid crystal composition has a refractive index anisotropy of 0.01 or more and 0.12 or less; The emulsion composition, wherein the liquid crystal composition has an average particle size of 4.9 μm or more and 30 μm or less.
2. 2. The emulsion composition according to claim 1, wherein the total mass of the liquid crystal composition is 0.5 to 4 relative to the total mass of the polymer being 1.
3. 3. The emulsion composition according to claim 1, wherein the liquid crystal composition has a coefficient of variation in particle size distribution of 0.001 or more and 0.8 or less.
4. 4. The emulsion composition according to claim 1, wherein the dichroic dye comprises an anthraquinone dye.
5. 5. The emulsion composition according to claim 1, wherein the liquid crystal composition contains a dichroic dye in an amount of 3% to 20%.
6. 6. The emulsion composition according to claim 1, wherein the polymer comprises a polyurethane.
7. 7. A liquid crystal-polymer composite film having a film obtained by applying the emulsion composition according to claim 1 onto an electrode substrate and drying it.
8. A liquid crystal element comprising: two substrates with transparent conductive films arranged so that their transparent conductive films face each other; and the liquid crystal-polymer composite film according to claim 7 sandwiched between the two substrates with transparent conductive films.
Citation Information
Patent Citations
Liquid crystal film and liquid crystal display element formed by using the same and production thereof
JP1993224191A
Display element
JP1997090430A
Production of liquid crystal display panel and liquid crystal supplying head and liquid crystal injector
JP1997244006A
Production of liquid crystal drop
JP1999133386A
Liquid crystal display device
JP1999271787A