Manufacturing method for grain-finished artificial leather
The described manufacturing process for grain-finished leather-like sheets addresses the challenge of high VOCs by using controlled heating and solvent composition, achieving low residual VOCs and maintaining adhesive strength and durability.
Patent Information
- Application Number
- JP2020209697
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-17
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-12-17
AI Technical Summary
Existing methods for producing grain-finished leather-like sheets using solvent-based polyurethane adhesives result in high residual volatile organic compounds (VOCs), which are difficult to reduce effectively, especially in applications requiring high durability.
A manufacturing process involving specific heating conditions and solvent composition for polyurethane solutions, including low and high-boiling organic solvents, to form a semi-dry adhesive layer, followed by controlled heating steps to minimize VOCs, specifically using polyurethane and solvents like methyl ethyl ketone and N,N-dimethylformamide.
The process significantly reduces residual VOCs in the leather-like sheets, maintaining adhesive strength and durability, as demonstrated by the low solvent retention rates and stable adhesive processability.
Smart Images

Figure 0007578480000002 
Figure 0007578480000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a grain-finish leather-like sheet for reducing the amount of residual volatile organic compounds. [Background technology]
[0002] 2. Description of the Related Art Grain-finished leather-like sheets, such as grain-finished artificial leather having a grain-finished appearance similar to grain-finished leather, are known and are used as covering materials for bags, clothing, shoes, and the like.
[0003] In the manufacturing process of grain-finish leather-like sheets, volatile organic compounds (VOCs) such as N,N-dimethylformamide (DMF) are often used as a polyurethane solvent. In recent years, there have been strict demands for the reduction of VOC emissions due to legal regulations and voluntary restrictions, etc., in order to prevent air pollution.
[0004] In the manufacture of grain-finish leather-like sheets, DMF is often used as a solvent for the polyurethane solution for the adhesive layer that bonds the grain-finish resin layer to the fiber substrate. In the manufacturing process of grain-finish leather-like sheets, it is required to recover as much DMF as possible that is generated during the process. For this reason, as a clean process that does not use DMF, a manufacturing method has been realized in which the fiber substrate manufacturing process and the process of impregnating the fiber substrate with polyurethane are made aqueous using a solvent mainly composed of water.
[0005] In the manufacturing process of the water-based grain-finish leather-like sheet, if the polyurethane adhesive is made water-based, it is possible to further reduce the amount of VOC emissions. Such a proposal has been made. For example, the following Patent Document 1 discloses a two-component curing water-based adhesive as a water-based polyurethane adhesive used in the manufacture of synthetic leather, which contains a base agent containing an aqueous polyurethane resin and a curing agent containing a polyisocyanate compound, and the polyisocyanate compound has a biuret bond or is modified with trimethylolpropane.
[0006] However, water-based polyurethane adhesives still have problems such as difficulty in obtaining sufficiently high adhesive strength and difficulty in obtaining sufficient durability compared to polyurethane adhesives containing organic solvents. For this reason, for example, in the manufacture of grain-finished leather-like sheets used in applications requiring high durability such as vehicle seats, polyurethane solutions containing solvent-based polyurethane and organic solvents such as DMF are still used as polyurethane adhesives. For this reason, there is a strong demand for technology to reduce the organic solvent remaining in grain-finished artificial leather using solvent-based polyurethane. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2010-229267 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention aims to provide a method for producing a grain-finish leather-like sheet that can reduce the amount of VOCs remaining in the grain-finish artificial leather when a polyurethane solution containing an organic solvent is used to bond a fiber substrate and a grain-finish surface resin layer. [Means for solving the problem]
[0009] One aspect of the present invention includes a step of forming a polyurethane surface resin layer on a release paper, a step of applying a polyurethane solution for an adhesive layer to the surface of the polyurethane surface resin layer, a step of forming a polyurethane adhesive layer in a semi-dried state by heating the polyurethane solution for the adhesive layer applied to the surface of the polyurethane surface resin layer under first heating conditions, a step of bonding a fiber substrate and the polyurethane surface resin layer via the polyurethane adhesive layer to form a laminated integrated sheet, a step of heating the laminated integrated sheet under second heating conditions, a step of peeling the release paper from the heated laminated integrated sheet to form a grain-finished leather-like sheet, and a step of heating the grain-finished leather-like sheet under third heating conditions, wherein the polyurethane solution for the adhesive layer contains polyurethane, 20 to 50 mass % of a low-boiling point organic solvent having a boiling point of 70 to 100°C, and 6 to 15 mass % of a high-boiling point organic solvent having a boiling point of 120 to 160°C, and the coating amount of the polyurethane solution is 60 to 160 g / m 2 and the coating amount of the high boiling point organic solvent is 22 g / m 2 The first heating condition includes heating at a temperature 5 to 15°C lower than the boiling point of the low-boiling organic solvent for 20 seconds or more during the temperature increase process, and the second and third heating conditions include heating at a temperature 10 to 40°C lower than the boiling point of the high-boiling organic solvent for 30 seconds or more during the temperature increase process. Examples of the low-boiling organic solvent include methyl ethyl ketone, and examples of the high-boiling organic solvent include N,N-dimethylformamide. Effect of the Invention
[0010] According to the present invention, a method for producing grain-finish leather-like sheets can be provided that can reduce the amount of residual VOCs when a polyurethane solution containing an organic solvent is used to adhere a grain-finish surface resin layer to a fiber substrate. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view of a grain-finished leather-like sheet 10 produced by the method for producing a grain-finished leather-like sheet of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] FIG. 1 is a schematic cross-sectional view of a grain-finished leather-like sheet 10 produced by the method for producing a grain-finished leather-like sheet of the present embodiment.
[0013] Referring to FIG. 1, the grain-finished leather-like sheet 10 comprises a textile substrate 1 and a polyurethane resin layer 3 adhered to one surface of the textile substrate 1 via a polyurethane adhesive layer 2. The resin layer including the polyurethane adhesive layer 2 and the polyurethane resin layer 3 forms a grain-finished resin layer. The grain-finished resin layer is a layer that gives the grain-finished leather-like sheet 10 an appearance and feel similar to the grain of natural leather. The polyurethane resin layer 3 may be a single layer or may have a multi-layer structure consisting of an intermediate layer and a top layer. The grain-finished leather-like sheet 10 is a grain-finished leather-like sheet with a low residual amount of VOC, which is produced by the production method described below.
[0014] Hereinafter, one embodiment of the method for producing the grain-finished leather-like sheet of the present invention will be described in detail. The method for producing the grain-finished leather-like sheet of this embodiment includes the steps of forming a polyurethane surface resin layer (hereinafter also simply referred to as a surface resin layer) on a release paper, applying a polyurethane solution for adhesive layer to the surface of the polyurethane surface resin layer, heating the polyurethane solution for adhesive layer applied to the surface of the polyurethane surface resin layer under a first heating condition to form a semi-dried polyurethane adhesive layer (hereinafter also simply referred to as an adhesive layer), bonding the fiber base material and the polyurethane surface resin layer via the polyurethane adhesive layer to form a laminated integrated sheet, heating the laminated integrated sheet under a second heating condition, peeling off the release paper from the heated laminated integrated sheet to form a grain-finished leather-like sheet, and heating the grain-finished leather-like sheet under a third heating condition. In such a manufacturing method, the polyurethane solution for the adhesive layer contains polyurethane, 20 to 50 mass % of a low-boiling point organic solvent having a boiling point of 70 to 100°C, and 6 to 15 mass % of a high-boiling point organic solvent having a boiling point of 120 to 160°C, and the coating amount thereof is 60 to 160 g / m 2and the coating amount of the high boiling point organic solvent is 22 g / m 2 The first heating condition includes heating during the temperature increase process at a temperature range of 5 to 15°C lower than the boiling point of the low-boiling point organic solvent for 20 seconds or more, and the second heating condition and the third heating condition include heating during the temperature increase process at a temperature range of 10 to 40°C lower than the boiling point of the high-boiling point organic solvent for 30 seconds or more. Each step will be described in detail below.
[0015] [Process of forming a surface resin layer on release paper] In the manufacturing method of this embodiment, a film of a surface resin layer to be adhered to the surface of a fiber substrate is formed on a release paper. The film of the surface resin layer is formed, for example, as follows.
[0016] A polyurethane solution or molten resin for forming a surface resin layer is applied onto the release paper and then solidified to form a film of the surface resin layer.
[0017] Examples of polyurethanes for forming the surface resin layer include polycarbonate-based polyurethanes, polyether-based polyurethanes, polyester-based polyurethanes, and copolymer polyurethanes such as polycarbonate-polyether copolymer polyurethanes and polycarbonate-polyester copolymer polyurethanes.
[0018] The method of forming the surface resin layer by applying a polyurethane solution onto a release paper includes a method of applying the polyurethane solution onto the release paper and then drying it. The surface resin layer may have a single layer structure formed from the same polyurethane, or may be a laminate having a multilayer structure consisting of an intermediate layer and a top layer obtained by laminating different types of polyurethane. The surface resin layer may or may not have a foamed structure.
[0019] In addition, the surface resin layer may contain a coloring material and other additives, etc., as necessary. In addition, the release paper is not particularly limited, but a smooth release paper or a release paper having an uneven surface to give a grain pattern is preferably used.
[0020] The thickness of the surface resin layer is not particularly limited, but is preferably 10 to 200 μm, and more preferably 20 to 100 μm.
[0021] [A step of forming a semi-dried adhesive layer by heating the polyurethane solution for adhesive layer applied to the surface of the surface resin layer under the first heating condition] Next, in this process, a polyurethane solution for the adhesive layer is applied to the surface of the surface resin layer formed on the release paper as described above, and then heating is performed under the first heating conditions to form a semi-dry adhesive layer.
[0022] The polyurethane solution for the adhesive layer contains polyurethane and a specific solvent for dissolving the polyurethane, as described below. If necessary, it may contain a crosslinking agent or a crosslinking accelerator. The polyurethane solution for the adhesive layer may contain additives such as an antioxidant, a light resistance agent, and an antibacterial agent, in addition to a colorant such as a pigment.
[0023] Examples of polyurethanes contained in the polyurethane solution for the adhesive layer include polycarbonate-based polyurethanes, polyether-based polyurethanes, polyester-based polyurethanes, and copolymer polyurethanes such as polycarbonate-polyether copolymer polyurethanes and polycarbonate-polyester copolymer polyurethanes. Among these, polycarbonate-based polyurethanes and polyether-based polyurethanes are particularly preferred because they are excellent in hydrolysis resistance and therefore make it easier to ensure durability.
[0024] The concentration of the solid content including polyurethane contained in the polyurethane solution for adhesive layer of the present embodiment is preferably 10 to 70 mass %, more preferably 20 to 60 mass %. If the concentration of the solid content including polyurethane is too high, the viscosity tends to be too high and the coatability tends to be reduced, whereas if the concentration of the solid content including polyurethane is too low, it tends to be difficult to adjust the film thickness of the coating film.
[0025] The polyurethane solution for the adhesive layer contains polyurethane, 20 to 50 mass % of a low-boiling organic solvent having a boiling point of 70 to 100°C, and 6 to 15 mass % of a high-boiling organic solvent having a boiling point of 120 to 160°C.
[0026] Examples of low-boiling organic solvents having a boiling point of 70 to 100° C. include methyl ethyl ketone (MEK, boiling point 79.64° C.), ethyl acetate (AcOEt, boiling point 77.1° C.), isopropyl alcohol (IPA, boiling point 82.4° C.), ethanol (EtOH, boiling point 78.4° C.), acetonitrile (AcCN, boiling point 82° C.), etc. Among these, methyl ethyl ketone is particularly preferred because it has little odor and is easy to handle.
[0027] Examples of high-boiling organic solvents having a boiling point of 120 to 160° C. include N,N-dimethylformamide (DMF, boiling point 153° C.), cyclohexanone (CH, boiling point 155.65° C.), butyl acetate (boiling point 126° C.), etc. Among these, N,N-dimethylformamide is particularly preferred because of its high solubility in the polyurethane resin for the adhesive layer.
[0028] The polyurethane solution for the adhesive layer may contain solvents other than low-boiling organic solvents and high-boiling organic solvents as necessary. Specific examples of such solvents other than low-boiling organic solvents and high-boiling organic solvents include ultra-low-boiling organic solvents with a boiling point of less than 70° C. and medium-boiling organic solvents with a boiling point of 100 to 120° C. It is preferable not to contain ultra-high-boiling organic solvents with a boiling point of more than 160° C., since they are difficult to volatilize and tend to remain.
[0029] Examples of ultra-low boiling organic solvents with a boiling point of less than 70°C include acetone (AC, boiling point 56.5°C) and methyl acetate (AcOMe, boiling point 57°C). Examples of medium boiling organic solvents with a boiling point of 100 to 120°C include 1,4-dioxane (DO, boiling point 101.3°C) and toluene (PhMe, boiling point 110.63°C). Examples of ultra-high boiling organic solvents with a boiling point of more than 160°C include dimethylacetamide (DMAc, boiling point 165°C), diethylformamide (DEF, boiling point 177°C), diethylacetamide (DEAc, boiling point 182-186°C), and N-methylpyrrolidone (NMP, boiling point 202°C).
[0030] The polyurethane solution for the adhesive layer contains 20 to 50 mass %, preferably 25 to 40 mass %, of a low-boiling organic solvent at 70 to 100°C. If the content of the low-boiling organic solvent is less than 20 mass %, the content of the high-boiling organic solvent becomes relatively high, which makes it easier for VOCs to remain. If the content of the low-boiling organic solvent exceeds 50 mass %, the volatility of the polyurethane solution for the adhesive layer becomes high, and the stability of the concentration and viscosity of the polyurethane solution for the adhesive layer over time tends to decrease.
[0031] The polyurethane solution for the adhesive layer contains 6 to 15 mass %, preferably 7 to 14 mass %, of a high-boiling organic solvent having a boiling point of 120 to 160°C. If the content of the high-boiling organic solvent is less than 6 mass %, the content of the low-boiling organic solvent is relatively high, so that the volatility of the solvent increases, the stability of the polyurethane solution for the adhesive layer decreases, and the adhesive processability decreases. Furthermore, the adjustment range of the solubility parameter of the polyurethane solution for the adhesive layer becomes narrow, so that the polyurethane solution for the adhesive layer swells the surface resin layer, and problems such as the surface resin layer lifting off the release paper before being bonded to the fiber substrate are likely to occur. If the content of the high-boiling organic solvent exceeds 15 mass %, VOCs are likely to remain.
[0032] The polyurethane solution for the adhesive layer may contain an ultra-low boiling organic solvent having a boiling point of less than 70°C in an amount of 30% by mass or less, or even 15% by mass or less. If the polyurethane solution contains 30% by mass or more of an ultra-low boiling organic solvent, the volatility of the solvent becomes too high, and the stability of the solution over time tends to decrease. The polyurethane solution for the adhesive layer may contain 30% by mass or less, or even 20% by mass or less of a medium boiling organic solvent, and 1% by mass or less, or even 0.1% by mass or less of a high boiling organic solvent. If the polyurethane solution contains 30% by mass or more of a medium boiling organic solvent or 1% by mass or more of a high boiling organic solvent, the amount of VOC remaining in the grain-finished artificial leather tends to increase.
[0033] A preferred combination for the polyurethane solution for the adhesive layer as described above is a mixed solvent containing MEK and DMF, specifically, a mixed solvent containing 20 to 70 mass %, or even 25 to 60 mass %, MEK and 5 to 15 mass %, or even 6 to 14 mass %, DMF, which may contain other solvents as the remainder, is preferred because it makes it less likely that VOCs will remain in the grain-finish leather-like sheet.
[0034] The method for applying the polyurethane solution for the adhesive layer to the surface of the polyurethane surface resin layer is not particularly limited, and a comma coater, a comma reverse coater, a knife coater, a gravure coater, etc. can be used. Among them, it is preferable to apply the solution using a comma coater because it is easy to control the amount of coating.
[0035] The coating amount of polyurethane solution for the adhesive layer is 60 to 160 g / m 2 and 70-150g / m 2 , and even 80 to 140 g / m 2 By applying the polyurethane solution for the adhesive layer to the surface resin layer formed on the release paper in such an amount, VOCs are less likely to remain in the grain-finished leather-like sheet. 2If the coating amount exceeds 60 g / m, heat is not transferred to the entire coating during the drying process, and only the surface layer dries preferentially and forms a film, making it difficult for the organic solvent inside to volatilize. As a result, VOCs tend to remain. Also, if the coating amount of the polyurethane solution for the adhesive layer is more than 60 g / m, 2 If it is less than this, it becomes difficult to form an adhesive layer of sufficient thickness.
[0036] The amount of polyurethane solution applied for the adhesive layer was 22 g / m2 of high boiling point organic solvent. 2 Less than 20 g / m 2 The adhesive layer polyurethane solution is applied in such a manner that the application amount of the high boiling point organic solvent is 22 g / m 2 By applying the coating amount as described below, the high-boiling point organic solvent is less likely to remain on the grain-finished leather-like sheet after going through each heating step described below. 2 If the concentration exceeds this range, the high boiling point organic solvent is likely to remain in the grain-finished leather-like sheet.
[0037] Then, the polyurethane solution for the adhesive layer applied to the surface resin layer formed on the release paper is heated under a first heating condition to volatilize part of the organic solvent, thereby forming a semi-dry polyurethane adhesive layer with an appropriately adjusted viscosity.
[0038] The first heating is performed under first heating conditions including heating for 30 seconds or more at a temperature range of 5 to 15°C lower than the boiling point of the low-boiling point organic solvent contained in the polyurethane solution for the adhesive layer during the temperature rise process. When two or more types of low-boiling point organic solvents are contained, the boiling point of the low-boiling point organic solvent with the lowest boiling point is used as the reference. The temperature rise process means a process of raising the temperature from a low temperature side to a high temperature side, and not a process of lowering the temperature from a high temperature side to a low temperature side.
[0039] The first heating is a process for preferentially volatilizing a portion of the low-boiling organic solvent contained in the polyurethane solution for the adhesive layer and adjusting the viscosity of the polyurethane solution for the adhesive layer when it is bonded to the fiber substrate. This first heating forms a polyurethane adhesive layer in a semi-dried state.
[0040] Here, the semi-dried polyurethane adhesive layer means a state in which a part of the low boiling point solvent contained in the polyurethane solution for the adhesive layer has been preferentially evaporated, specifically, a state in which about 20 to 80% of the total amount of the low boiling point solvent contained in the polyurethane solution for the adhesive layer has been evaporated.
[0041] The first heating is preferably performed, for example, with a hot air dryer, particularly a conveyor-type hot air dryer in which the temperature can be set for each zone. The first heating conditions are set according to the type of low-boiling organic solvent, and include heating in the temperature range of 5 to 15°C lower than the boiling point of the low-boiling organic solvent for 30 seconds or more during the temperature rise process. By heating in this manner, foaming caused by the sudden volatilization of the low-boiling organic solvent in the polyurethane solution for the adhesive layer when heating from the low-temperature side to the high-temperature side can be suppressed, and thus the high adhesive strength of the adhesive layer formed can be maintained. The temperature and time under each heating condition are specified from the temperature profile actually measured by placing a thermometer in the hot air dryer. In addition, if there is an instantaneous fluctuation in the temperature profile due to measurement error or the characteristics of the dryer, the center value of the fluctuation is taken as the actual temperature measurement value.
[0042] The first heating condition is not particularly limited as long as it includes heating in the temperature range of 5 to 15°C lower than the boiling point of the low-boiling organic solvent for 30 seconds or more during the temperature rise process, and the temperature profile until the temperature is 15°C lower than the boiling point of the low-boiling organic solvent is appropriately adjusted while considering the permeability of the polyurethane solution for the adhesive layer into the fiber substrate. Specifically, for example, when the fiber substrate has a high specific gravity or is oil-repellent and the polyurethane solution for the adhesive layer does not easily permeate into the fiber substrate, it is preferable to adjust the temperature rise rate until the temperature is 15°C lower than the boiling point of the low-boiling organic solvent to increase the total amount of heat applied in order to promote the permeation. In addition, when the fiber substrate has a low specific gravity or is lipophilic and the polyurethane solution for the adhesive layer permeates too much into the fiber substrate, it is preferable to adjust the temperature rise rate until the temperature is 15°C lower than the boiling point of the low-boiling organic solvent to increase the total amount of heat applied in order to suppress the polyurethane solution for the adhesive layer from excessively permeating into the fiber substrate. In this way, it is preferable to adjust the temperature profile until the temperature reaches 15°C lower than the boiling point of the low-boiling organic solvent in the first heating condition, taking into consideration the permeability of the polyurethane solution for the adhesive layer of the fiber substrate. Also, it is preferable that the temperature is lowered to room temperature immediately after heating at a temperature range of 5 to 15°C lower than the boiling point of the low-boiling organic solvent for 30 seconds or more, in order to prevent the adjusted viscosity from fluctuating.
[0043] The first heating is provided for the purpose of volatilizing a portion of the low boiling point solvent to increase viscosity, and does not have a significant effect on the final remaining amount of VOCs.
[0044] The thickness of the adhesive layer is preferably 5 to 150 μm, more preferably 20 to 100 μm. If the adhesive layer is too thick, the bending resistance tends to decrease, and the adhesive strength tends to decrease.
[0045] The total thickness of the surface resin layer and adhesive layer is preferably about 10 to 300 μm, more preferably 30 to 200 μm, and even more preferably about 50 to 150 μm, from the viewpoint of maintaining a balance between mechanical properties and texture.
[0046] [Fiber base material containing entangled fibers] Next, the preparation of the fiber substrate containing the fiber entanglement to which the surface resin layer is bonded will be described. As the fiber substrate, any fiber substrate that is mainly made of nonwoven fabric, woven fabric, knitted fabric, or a combination thereof, and further impregnated with a polymeric elastomer as necessary, which has been conventionally used in the manufacture of grain-finished leather-like sheets, is used without any particular limitation. Among these, a fiber substrate containing a nonwoven fabric, particularly a nonwoven fabric containing ultrafine fibers with a fineness of 0.5 dtex or less impregnated with a polymeric elastomer, is preferred because it is easy to obtain a dense grain-finished leather-like sheet with high mechanical strength.
[0047] The fineness and form of the fibers are not particularly limited. For example, the fineness may be regular fibers with a fineness of more than 1 dtex, or ultrafine fibers with a fineness of less than 1 dtex. The form of the fibers may be solid fibers or fibers with voids such as hollow fibers or lotus root-like fibers. In particular, it is preferable that the fibers contain ultrafine fibers with a fineness of 0.5 dtex or less, or even 0.0001 to 0.2 dtex, because it is easy to obtain a grain-finished leather-like sheet with low fiber density unevenness and high homogeneity.
[0048] The type of resin forming the fibers is not particularly limited. Specifically, for example, aromatic polyester resins such as polyethylene terephthalate (PET), modified polyethylene terephthalate, polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polytriethylene terephthalate, polyhexamethylene terephthalate, polypropylene terephthalate, and polyethylene naphthalate; aliphatic polyester resins such as polylactic acid, polyethylene succinate, polybutylene succinate, polybutylene succinate adipate, and polyhydroxybutyrate-polyhydroxyvalerate copolymer; and polyester resins such as poly Examples of the resins include polyamide-based resins such as amide 6, polyamide 66, polyamide 610, polyamide 10, polyamide 11, polyamide 12, and polyamide 6-12; polyolefin-based resins such as polypropylene, polyethylene, polybutene, polymethylpentene, chlorine-based polyolefins, ethylene-vinyl acetate copolymers, and styrene-ethylene copolymers; modified polyvinyl alcohol-based resins formed from modified polyvinyl alcohols containing 25 to 70 mol% of ethylene units; and crystalline elastomers such as polyurethane-based elastomers, polyamide-based elastomers, and polyester-based elastomers. Among these, polyamide-based resins and aromatic polyester-based resins are preferred because they have an excellent balance of various properties. These may be used alone or in combination of two or more.
[0049] The method for producing the fibers is not particularly limited, and may be, for example, a method in which a resin is melted at a temperature equal to or higher than the melting point and extruded from an extruder to form a melt spinning fiber, a dry solution spinning method in which a polymer solution is extruded through a fine hole and the solvent is evaporated, or a wet solution spinning method in which a polymer solution is spun into a non-solvent. A nonwoven fabric of ultrafine fibers can be obtained, for example, by entangling ultrafine fiber-generating fibers such as islands-in-the-sea composite fibers to form a fiber entanglement body, and then subjecting the fiber to an ultrafine fiber processing.
[0050] The fiber substrate may include a polymeric elastomer impregnated into the entangled fiber body. The type of polymeric elastomer impregnated into the entangled fiber body is not particularly limited, but specific examples include various polymeric elastomers such as polyurethane, acrylic elastomers such as acrylonitrile-butadiene copolymers and copolymers of acrylic acid esters or methacrylic acid esters, polyamide elastomers, and silicone rubber. Among these, polyurethane is particularly preferred because it provides a good feel. The soft segment of polyurethane may include one of polyester units, polyether units, and polycarbonate units, or may be used in combination. The polymeric elastomer may be used alone or in combination of two or more types.
[0051] When the fiber substrate contains a polymer elastomer, the mass ratio of the fiber entanglement to the polymer elastomer (fiber entanglement / polymer elastomer) is preferably in the range of 99 / 1 to 30 / 70.If the polymer elastomer content is too high, the grain-finished leather-like sheet obtained tends to have a hard, rubber-like feel.
[0052] The thickness of the fiber base material is not particularly limited, but is preferably, for example, about 0.3 to 3 mm, and more preferably about 0.5 to 1.5 mm.
[0053] [Step of forming a laminated integrated sheet by bonding a fiber base material and a surface resin layer via an adhesive layer] The adhesive layer is laminated on the surface resin layer formed on the release paper, and the organic solvent is partially evaporated by the first heating to adjust the viscosity, and the adhesive layer is pressed and bonded to the surface of the fiber substrate to produce an integrated laminated sheet. The integration is performed, for example, by passing the laminate formed by overlapping the adhesive layer formed on the release paper and the fiber substrate through a press roll having a predetermined clearance.
[0054] The clearance formed in the press roll is, for example, 20 to 90%, or more preferably 30 to 80%, of the thickness of the fiber substrate, from the viewpoint of sufficient adhesion between the fiber substrate and the surface resin layer via the adhesive layer. In this way, a laminated integrated sheet is obtained in which the surface resin layer on the release paper and the fiber substrate are bonded together via the adhesive layer.
[0055] [Step of subjecting the laminated integrated sheet to second heating] Similarly to the first heating, the second heating is preferably performed, for example, with a hot air dryer, particularly a conveyor-type hot air dryer in which the temperature can be set for each zone. In the step of performing the second heating, heating is performed under second heating conditions including heating in a temperature range of 10 to 40°C lower than the boiling point of the high-boiling point organic solvent for 30 seconds or more during the temperature increase process. It is preferable that the temperature is decreased to room temperature immediately after heating in a temperature range of 10 to 40°C lower than the boiling point of the high-boiling point organic solvent for 30 seconds or more in order to suppress thermal degradation of the polyurethane due to excessive heating.
[0056] In the second heating, most of the organic solvent remaining in the laminated integrated sheet is volatilized. The second heating conditions include heating at a temperature range that is 10 to 40°C lower than the boiling point of the high-boiling organic solvent for 30 seconds or more, preferably 60 seconds or more, and more preferably 120 seconds or more.
[0057] In the second heating, the temperature profile is not particularly limited as long as the heating is performed in a temperature range of 10 to 40°C lower than the boiling point of the high-boiling organic solvent for 30 seconds or more during the temperature rise process, but it is preferable that the temperature is lowered to room temperature immediately after the heating is held, in order to suppress thermal deterioration of polyurethane due to excessive heating. In addition, for example, in the first heating, the volatilization of the low-boiling solvent may be insufficient by prioritizing the adjustment of the viscosity. In such a case, if the temperature is raised rapidly to a temperature 40°C lower than the boiling point of the high-boiling organic solvent, the low-boiling solvent remaining in the adhesive layer may suddenly expand and foam. In such a case, a temperature profile in which the temperature is raised slowly to a temperature 40°C lower than the boiling point of the high-boiling organic solvent is preferable. In addition, for example, a temperature profile in which the temperature is raised to a temperature 40°C lower than the boiling point of the high-boiling organic solvent after being held for 30 seconds in a temperature range of 40 to 50°C lower than the boiling point of the high-boiling organic solvent may be used.
[0058] [Step of forming a grained leather-like sheet by peeling off the release paper from the laminated integrated sheet after the second drying] The laminated integrated sheet is wound into a roll, and then is typically aged for several hours to several days at a temperature of 40° C. to 90° C. to completely harden the adhesive polyurethane layer. After aging is complete, the release paper is peeled off to obtain a grain-finished leather-like sheet.
[0059] [Step of subjecting grain-finished leather-like sheet to third heating] The grain-finished leather-like sheet after peeling off the release paper is subjected to a third heating step, which includes heating the sheet at a temperature 10 to 40°C lower than the boiling point of the high-boiling organic solvent for 30 seconds or more during the temperature rise process. The third heating step can remove the organic solvent more efficiently than the second heating step performed while the sheet is integrated with the release paper. By performing the third heating step, it is possible to remove most of the organic solvent remaining in the grain-finished leather-like sheet.
[0060] Similarly to the first and second heating, the third heating is preferably performed, for example, with a hot air dryer, particularly a conveyer-type hot air dryer in which the temperature can be set for each zone. The third heating also includes heating in a temperature rise process in which the temperature is maintained at a range of 10 to 40°C lower than the boiling point of the high-boiling organic solvent for 30 seconds or more, preferably 60 seconds or more, and more preferably 120 seconds or more. In addition, it is preferable that the temperature is lowered to room temperature immediately after heating in which the temperature is maintained at a range of 10 to 40°C lower than the boiling point of the high-boiling organic solvent for 30 seconds or more, in order to suppress thermal deterioration of the polyurethane due to excessive heating.
[0061] The third heating may also include a step of heating at a temperature lower than 40° C. lower than the boiling point of the high-boiling point organic solvent, if necessary. For example, the conditions may be such that heating is performed for 30 seconds at a temperature 50° C. lower than the boiling point of the high-boiling point organic solvent, followed by heating for 30 seconds at a temperature 30° C. lower than a peak temperature within a range of temperatures 10 to 40° C. lower than the boiling point of the high-boiling point organic solvent, and then maintaining the mixture at the peak temperature for 30 seconds or more. EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples, although the scope of the present invention is not limited to these examples in any way.
[0063] [Example 1] On the release paper, apply 170 g / m of the polyurethane solution for the surface resin layer, which has the composition shown below, evenly. 2 After coating, the coating was dried at 90° C. for 1 minute and then at 120° C. for 1 minute to form a polyurethane surface resin layer having a thickness of 30 μm.
[0064] (Polyurethane solution for surface resin layer) Polyether polyurethane solution (Rezamin ME-8115LP, solids 30%, MEK 21%, DMF 49%, manufactured by Dainichi Seika Chemicals Co., Ltd.): 100 parts by weight ·MEK: 30 parts by mass ·DMF: 40 parts by mass White pigment: 10 parts by weight
[0065] Next, a polyurethane solution for the adhesive layer was prepared having the composition shown below.
[0066] (Polyurethane solution for adhesive layer) Polyether polyurethane solution (Rezamin UD-8310NTT, manufactured by Dainichi Seika Chemicals Co., Ltd., solid content 60%, MEK 30%, DMF 10%): 100 parts by weight MEK (low boiling point organic solvent, boiling point 79.6°C): 30 parts by weight DMF (high boiling point organic solvent, boiling point 153°C): 10 parts by weight Isocyanate-based crosslinking agent (NE crosslinking agent manufactured by Dainichi Seika Chemicals Co., Ltd.): 10 parts by weight Crosslinking reaction accelerator (UD-103 accelerator crosslinking agent manufactured by Dainichi Seikagaku Kogyo Co., Ltd.): 1 part by mass
[0067] The proportion of the low boiling point organic solvent in the polyurethane solution for the adhesive layer was 39.7 mass %, and the proportion of the high boiling point organic solvent was 13.2 mass %.
[0068] Then, the polyurethane solution for the adhesive layer is applied to the surface of the surface resin layer at 150 g / m 2 The coating amount of the high boiling point organic solvent was 19.9 g / m 2 It was.
[0069] Then, as the first heating step, the applied polyurethane solution for the adhesive layer was heated from room temperature to 70°C in 5 seconds in a hot air dryer and held at 70°C for 30 seconds, and then the heating was stopped to form an adhesive layer that was dried to a semi-dry state.
[0070] The semi-dried adhesive layer formed in this manner and laminated on the surface resin layer on the release paper was placed in contact with the surface of the fiber substrate, and pressed with a roll having a clearance of about 70% of the thickness of the fiber substrate. In this way, a laminated integrated sheet was produced. The fiber substrate was a 0.1 dtex polyester fiber nonwoven fabric impregnated with polyurethane, with a polyester fiber / polyurethane ratio of 70 / 30 (mass ratio) and a basis weight of 430 g / m.2 An artificial leather substrate having a thickness of 1.0 mm was used.
[0071] Then, in the second heating step, the laminated integrated sheet was heated in a hot air dryer from room temperature to 120°C over 90 seconds, held at 120°C for 60 seconds, and then the heating was stopped.
[0072] The mixture was then left at 70° C. for 2 days to mature the mixture in order to complete crosslinking of the polyurethane.
[0073] The release paper was then peeled off from the laminated integrated sheet to obtain a grain-finished leather-like sheet.
[0074] Then, in the third heating step, the grain-finish leather-like sheet was heated in a hot air dryer from room temperature to 120°C in 5 seconds, held at 120°C for 60 seconds, and then the heating was stopped.
[0075] Thus, grain-finished leather-like sheets were produced. The residual organic solvent rate and processing stability of the obtained grain-finished leather-like sheets were evaluated as follows.
[0076] (Quantitative analysis of DMF and DEF) The residual amounts of DMF and DEF were measured in accordance with ISO / TS 16189:2013 as follows. The grain-finished leather-like sheet, which had been appropriately sampled and sealed for VOC measurement in a zippered plastic bag, was shredded into 3 mm square pieces, and 1 g was weighed out as a test piece. The pieces were then placed in a 20 ml vial and sealed with a Teflon (registered trademark)-coated silicone septum. Then, DMF-d 7 The remaining organic solvent was extracted by adding 10 ml of a methanol solution containing DMF to the vial and leaving it at 70°C for 1 hour. The resulting extract was analyzed using GS / MS, and the amounts of DMF and DEF were quantified from the peak positions and areas to calculate the residual rates.
[0077] (Quantitative determination of MEK, ethyl acetate, toluene, anone) The residual amount of organic solvents was measured by headspace GC / MS. First, the grained leather-like sheet, which had been appropriately sampled and sealed for VOC measurement in a zippered plastic bag, was shredded into 3 mm squares, and 1 g was weighed out as a test piece. The test piece was then placed in a 10 ml vial and sealed with a Teflon-coated silicone septum. Toluene-d 8 After 10 μg was injected with a microsyringe, it was set in a headspace sampler and heated at 120° C. for 45 minutes. The headspace portion that had reached equilibrium was introduced from the headspace sampler to a GC / MS, and the amounts of each solvent, MEK, ethyl acetate, toluene, and anone, were quantified from the peak positions and areas, and the residual rates were calculated.
[0078] (Adhesion processing stability) The adhesive processing stability was evaluated according to the following criteria. A: The adhesive processing was possible without any problems. B: The formed adhesive layer was swollen by the organic solvent, but adhesion was possible. C: The adhesive layer was poorly dried, had significant swelling or foaming, or had a poor appearance, and was not able to achieve practical adhesion.
[0079] The results are shown in Table 1 below.
[0080] [Table 1]
[0081] [Examples 2 to 7 and Comparative Examples 1 to 9] A grain-finish leather-like sheet was prepared in the same manner as in Example 1, except that the application amount of the polyurethane solution for the adhesive layer, the compounding composition of the polyurethane solution for the adhesive layer, and the heating conditions for the first heating step, the second heating step, and the third heating step were changed as shown in Table 1. In Comparative Example 4, the following polyurethane solution for the adhesive layer was used.
[0082] (Polyurethane solution for adhesive layer) Polyether polyurethane (solids 60%, MEK 30%, DEF 10%): 100 parts by weight MEK (low boiling point organic solvent, boiling point 79.6°C): 30 parts by weight DEF (ultra-high boiling point organic solvent, boiling point 176-177°C): 10 parts by weight Isocyanate-based crosslinking agent (NE crosslinking agent manufactured by Dainichi Seika Chemicals Co., Ltd.): 10 parts by weight Crosslinking reaction accelerator (UD-103 accelerator crosslinking agent manufactured by Dainichi Seikagaku Kogyo Co., Ltd.): 1 part by mass The grain-finished leather-like sheet was then evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0083] Referring to Table 1, all of the grain-finished artificial leathers obtained in Examples 1 to 6, which employ the method for producing a grain-finished leather-like sheet according to the present invention, had a significantly small amount of residual solvent. On the other hand, the grain-finished artificial leather obtained in Comparative Example 1, which did not undergo the third heating, had a large amount of residual solvent. Moreover, the grain-finished artificial leather obtained in Comparative Example 2, which used a polyurethane solution for adhesive layer with too high a ratio of high-boiling-point organic solvent, had a large amount of residual solvent even after the third heating. Moreover, the grain-finished artificial leather obtained in Comparative Example 3, which used a large amount of polyurethane solution for adhesive layer, also had a large amount of residual solvent even after the third heating. Moreover, the grain-finished artificial leather obtained in Comparative Example 5, which used a low temperature for the third heating, also had a large amount of residual solvent. Moreover, the grain-finished artificial leather obtained in Comparative Example 7, which used a too high ratio of low-boiling-point organic solvent, had an unstable adhesive processability due to too low a viscosity of the polyurethane solution for adhesive layer. In the grain-finished artificial leather obtained in Comparative Example 8, in which the temperature of the first heating was too high, the viscosity of the polyurethane solution for the adhesive layer increased too rapidly, resulting in unstable adhesive processability.In addition, in the grain-finished artificial leather obtained in Comparative Example 9, in which the temperature of the second heating was too high, the adhesive layer foamed, resulting in poor appearance. [Explanation of symbols]
[0084] 1. Fiber base material 2 Polyurethane adhesive layer 3 Polyurethane resin layer 10. Silver-finished leather-like sheet
Claims
1. forming a polyurethane surface resin layer on a release paper; applying a polyurethane solution for an adhesive layer to a surface of the polyurethane surface resin layer; A step of forming a polyurethane adhesive layer in a semi-dried state by heating the polyurethane solution for adhesive layer applied to the surface of the polyurethane surface resin layer under a first heating condition; forming a laminated integrated sheet by bonding a fiber substrate and the polyurethane surface resin layer via the polyurethane adhesive layer; Heating the laminated integrated sheet under a second heating condition; a step of peeling off the release paper from the heated laminated integrated sheet to form a grain-finished leather-like sheet; and heating the grain-finished leather-like sheet under a third heating condition. The polyurethane solution for the adhesive layer contains polyurethane, 20 to 50 mass % of a low-boiling organic solvent having a boiling point of 70 to 100° C., and 6 to 15 mass % of a high-boiling organic solvent having a boiling point of 120 to 160° C.; The coating amount is 60 to 160 g / m 2 and the coating amount of the high boiling point organic solvent is 22 g / m 2 is as follows: the first heating condition includes heating the mixture at a temperature that is 5 to 15° C. lower than the boiling point of the low-boiling organic solvent for 20 seconds or more during a temperature rise process; The second heating condition and the third heating condition include heating the mixture at a temperature 10 to 40° C. lower than the boiling point of the high-boiling point organic solvent for 30 seconds or more during a temperature rise process.
2. The low boiling point organic solvent includes methyl ethyl ketone, and the high boiling point organic solvent includes N,N-dimethylformamide; The method for producing a grain-finished leather-like sheet according to claim 1, wherein the temperature maintained for 20 seconds or more under the first heating condition is in the range of 65 to 75°C, and the temperatures maintained for 30 seconds or more under the second heating condition and the third heating condition are in the range of 115 to 143°C.
Citation Information
Patent Citations
JP1973018803B1
Polyurethane elastic fiber nonwoven fabric and its production and synthetic leather using the same
JP2000248454A
Base material for artificial leather, various artificial leathers with the same as base, and method for manufacturing the base material for artificial leather
JP2005171426A
Two-pack aqueous adhesive for synthetic leather
JP2010229267A
Method for producing grained artificial leather
JP2015113535A