Moisture and oxygen barrier laminate with improved durability and flexibility
The laminate with an inorganic barrier and a siloxane-based protective layer addresses the trade-off between durability and flexibility, ensuring robust barrier performance under deformation.
Patent Information
- Application Number
- JP2023534968
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-06
- Filing Date
- 2021-12-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-12-09
AI Technical Summary
Barrier laminates used for packaging face a trade-off between durability and flexibility, leading to deterioration of barrier properties upon deformation such as bending due to separation or tearing between layers.
A moisture and oxygen barrier laminate is developed with an inorganic barrier layer and a protective layer formed on a transparent substrate, where the protective layer includes an organic copolymer containing repeating units derived from a siloxane compound, enhancing interlayer adhesion and improving both durability and flexibility.
The laminate maintains excellent interlayer adhesion and barrier properties even under deformation, such as bending, thereby providing improved durability and flexibility while maintaining effective moisture and oxygen barrier performance.
Smart Images

Figure 0007579980000001 
Figure 0007579980000002 
Figure 0007579980000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate having improved moisture and oxygen barrier properties with improved durability and flexibility. [Background technology]
[0002] 2. Description of the Related Art Barrier laminates in which an inorganic thin film such as aluminum oxide is formed on the surface of a plastic substrate are used for packaging a variety of products such as food and electronic devices.
[0003] However, such a barrier laminate has a problem in that when it is subjected to deformation such as bending, the barrier properties deteriorate due to separation or tearing between the layers.
[0004] Therefore, various researches have been conducted to improve the durability and flexibility of the barrier laminate, for example, by introducing a primer layer between the plastic substrate and the inorganic thin film to improve adhesion, or by laminating a polymer coating layer of various compositions on the inorganic thin film.
[0005] However, since there is generally a trade-off between durability and flexibility of a barrier laminate, it is difficult to simultaneously satisfy both of these characteristics. Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a moisture and oxygen barrier laminate having improved durability and flexibility. [Means for solving the problem]
[0007] Hereinafter, a moisture and oxygen barrier laminate according to an embodiment of the present invention will be described.
[0008] Unless otherwise defined herein, all technical and scientific terms have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. The terms used in the description of the present invention are merely for the purpose of effectively describing a specific embodiment and are not intended to limit the present invention.
[0009] As used herein, the singular forms include the plural forms unless the phrase clearly dictates to the contrary.
[0010] As used herein, the meaning of "comprising" is to embody certain features, regions, constants, steps, operations, elements, components and / or components, and does not exclude the presence or addition of other particular features, regions, constants, steps, operations, elements, components and / or groups.
[0011] The present invention can be modified in various ways and can have various forms, and will be described in detail below by taking specific examples as examples. However, this is not intended to limit the present invention to the specific disclosed form, but it should be understood that the present invention includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.
[0012] In this specification, when the positional relationship of two parts is described using, for example, "on," "at the top," "below," "to the side," etc., one or more other parts may be located between the two parts, unless the expressions "immediately" or "directly" are used.
[0013] In this specification, when a temporal relationship is described using, for example, "after," "following," "next to," or "before," it can also include cases where the relationship is not consecutive, since the expressions "immediately" or "directly" are not used.
[0014] As used herein, the term "at least one" should be understood to include all possible combinations of one or more of the associated items.
[0015] According to one embodiment of the invention, The present invention includes an inorganic barrier layer and a protective layer formed in sequence on one surface of a transparent substrate, The protective layer contains an organic copolymer containing a repeating unit derived from a siloxane compound. A laminate is provided.
[0016] As a result of the inventors' continued research, it has been found that when the protective layer containing an organic copolymer containing a repeating unit derived from a siloxane compound is formed on the inorganic barrier layer, a moisture and oxygen barrier laminate having improved durability and flexibility can be provided.
[0017] The organic copolymer containing a repeating unit derived from the siloxane compound not only enables the barrier properties and flexibility of the laminate to be improved, but also improves the interlayer adhesion of the laminate, thereby enabling the durability to be improved.
[0018] In other words, the organic copolymer containing repeating units derived from the siloxane compound can simultaneously improve the durability and flexibility of the laminate, which are known to be in a trade-off relationship.
[0019] According to one embodiment of the invention, the laminate may have a structure including an inorganic barrier layer and a protective layer formed in sequence on one surface of a transparent substrate.
[0020] According to another embodiment of the present invention, the laminate may have a structure including an inorganic barrier layer and a protective layer formed in sequence on both sides of the transparent substrate, respectively.
[0021] In the present invention, the transparent substrate may be a plastic film having transparency and flexibility.
[0022] Specifically, the transparent substrate may be a plastic film containing one or more polymers selected from the group consisting of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), cycloolefin polymer (COP), cycloolefin copolymer (COC), polycarbonate (PC), and poly(methyl methacrylate) (PMMA). Among these, a polyethylene terephthalate film is suitable for use as the transparent substrate because it has both transparency and flexibility while also being excellent in strength.
[0023] According to one embodiment of the invention, the transparent substrate can have a thickness of 5 μm to 300 μm.
[0024] In order to ensure that the substrate has an appropriate strength, the thickness of the transparent substrate is preferably 5 μm or more. However, if the substrate is too thick, the flexibility may decrease. Therefore, the thickness of the transparent substrate is preferably 300 μm or less.
[0025] More preferably, the thickness of the transparent substrate may be from 5 μm to 250 μm, alternatively from 10 μm to 250 μm, alternatively from 10 μm to 200 μm, alternatively from 10 μm to 150 μm, alternatively from 10 μm to 100 μm.
[0026] If necessary, the transparent substrate may be surface-treated to improve its surface wettability or adhesion to the inorganic barrier layer, etc. Non-limiting examples of the surface treatment may include plasma treatment, corona treatment, glow discharge treatment, etc.
[0027] On the other hand, the inorganic barrier layer is a thin film made of an inorganic material, and is laminated on one surface of the transparent substrate.
[0028] The inorganic barrier layer is transparent and enables the laminate to exhibit moisture and oxygen barrier properties.
[0029] Such inorganic barrier layers may be comprised of one or more inorganic materials selected from the group consisting of silicon oxide, silicon oxynitride, silicon nitride, aluminum oxide, and aluminum nitride.
[0030] According to one embodiment of the invention, the inorganic barrier layer may have a thickness of 1 nm to 200 nm.
[0031] In order to achieve appropriate physical properties as a barrier layer, the inorganic barrier layer is preferably 1 nm or more in thickness. However, if the inorganic barrier layer is too thick, curling due to stress may occur, or cracks may occur even when the layer is bent slightly. Therefore, the inorganic barrier layer is preferably 200 nm or less in thickness.
[0032] More preferably, the thickness of the inorganic barrier layer may be from 1 nm to 150 nm, alternatively from 5 nm to 150 nm, alternatively from 5 nm to 100 nm, alternatively from 10 nm to 100 nm.
[0033] According to one embodiment of the invention, the inorganic barrier layer can be formed on the transparent substrate by a conventional method in the technical field to which the present invention pertains.
[0034] For example, the inorganic barrier layer may be formed by a method selected from physical vapor deposition (PVD) and chemical vapor deposition (CVD).
[0035] Preferably, the deposition method of the inorganic barrier layer may be selected from evaporation methods such as thermal evaporation and electron-beam evaporation; or sputtering.
[0036] As an example, the evaporation method is the most basic method for forming a thin film, in which a metal or nonmetal source is heated, evaporated, and condensed on the surface of a substrate at a low temperature to form a thin film. According to one embodiment of the invention, among the evaporation methods, thermal evaporation can be suitably selected as a method for laminating the inorganic barrier layer. The thermal evaporation is performed at an initial vacuum of 10 -4 This requires a vapor pressure of about 1000 torr, and is a deposition method in which electricity is passed through a boat carrying the source to be evaporated, and the source is heated using the resistance heat generated in the boat. The deposition speed in thermal evaporation can be changed by adjusting the amount of current supplied to the filament. In addition, oxide films (AlOx, SiOx, etc.) can be formed by reacting reactive gas (oxygen gas) introduced.
[0037] As another example, the sputtering method can be suitably used since it has excellent reproducibility and can easily form a dense thin film over a large area. Preferably, reactive sputtering using an inorganic target and a reactive gas (e.g., oxygen) can be used as a method for laminating the inorganic barrier layer. In the reactive sputtering method, the reactive gas is additionally introduced into the system in addition to argon (Ar) as a plasma generating gas. In the reactive sputtering method, it is preferable to precisely control the amount of the reactive gas in the system using a device such as a plasma emission monitor or a mass flow controller. This is because the stoichiometric ratio of the inorganic thin film to be formed must be consistent. By adjusting the amount of the reactive gas introduced, stable film formation is possible, and the inorganic barrier layer having excellent barrier properties can be formed.
[0038] On the other hand, the protective layer is laminated on the inorganic barrier layer.
[0039] The protective layer can minimize cracks or separation between layers in the inorganic barrier layer due to deformation such as bending.
[0040] In particular, the protective layer comprises an organic copolymer that includes repeating units derived from a siloxane compound.
[0041] The organic copolymer containing a repeating unit derived from the siloxane compound not only enables the barrier properties and flexibility of the laminate to be improved, but also enables the interlayer adhesion of the laminate to be improved, thereby enabling the durability to be improved.
[0042] Preferably, the organic copolymer is a block copolymer containing a repeating unit derived from the siloxane compound and a repeating unit containing a urethane group (-NHCOO-). The organic copolymer contains a soft segment which is a repeating unit containing the urethane group, and a hard segment which is a repeating unit derived from the siloxane compound. This allows the organic copolymer to exhibit excellent barrier properties, durability, and heat resistance due to the hard segment, and excellent flexibility and interlayer adhesion due to the soft segment.
[0043] According to one embodiment of the invention, the organic copolymer preferably contains 1 to 40% by weight of the repeating unit derived from the siloxane compound and 60 to 99% by weight of the repeating unit containing the urethane group.
[0044] In order to achieve excellent barrier properties, durability, and heat resistance due to the hard segment, the organic copolymer preferably contains 1 wt% or more of the repeating unit derived from the siloxane compound. However, if the content of the repeating unit derived from the siloxane compound is too high, the flexibility of the protective layer may decrease. Therefore, the organic copolymer preferably contains 40 wt% or less of the repeating unit derived from the siloxane compound.
[0045] More preferably, the organic copolymer is 1 to 40% by weight of the repeating unit derived from the siloxane compound and 60 to 99% by weight of the repeating unit containing a urethane group; Alternatively, 1 to 30% by weight of the repeating unit derived from the siloxane compound and 70 to 99% by weight of the repeating unit containing a urethane group; Alternatively, 1 to 20% by weight of the repeating unit derived from the siloxane compound and 80 to 99% by weight of the repeating unit containing a urethane group; Alternatively, 1 to 15% by weight of the repeating unit derived from the siloxane compound and 85 to 99% by weight of the repeating unit containing a urethane group; Alternatively, 5 to 15% by weight of the repeating unit derived from the siloxane compound and 85 to 95% by weight of the repeating unit containing a urethane group; Alternatively, it may contain 10 to 15% by weight of the repeating unit derived from the siloxane compound and 85 to 90% by weight of the repeating unit containing the urethane group.
[0046] According to one embodiment of the invention, the siloxane compound may be a polysiloxane terminated at both ends with a carbinol group (group). That is, in order to easily introduce a repeating unit derived from the siloxane compound into the organic copolymer, the siloxane compound is preferably a polysiloxane terminated at both ends with a carbinol group.
[0047] More preferably, the siloxane compound may be a polysiloxane represented by the following Chemical Formula 1:
[0048] [Chemical formula 1] TIFF0007579980000001.tif31123
[0049] In the above Chemical Formula 1, R 1 ~R 6 are each independently a monovalent C 1-10 is a hydrocarbon radical, R 7and R 8 are each independently a divalent C 1-10 It is a hydrocarbon radical.
[0050] As an example, in the formula 1, 1 ~R 6 may each independently be a methyl group, an ethyl group, a propyl group, or a phenyl group; 7 and R 8 may each independently be a methylene group, an ethylene group, a propylene group, or a phenylene group.
[0051] Specifically, the siloxane compound may be polydimethylsiloxane, polydiethylsiloxane, polydipropylsiloxane, or polydiphenylsiloxane, both ends of which are terminated with carbinol groups.
[0052] According to one embodiment of the present invention, the repeating unit including the urethane group contained in the organic copolymer may be represented by the following Chemical Formula 2.
[0053] [Chemical formula 2] TIFF0007579980000002.tif33123
[0054] In the above Chemical Formula 2, Ar is C 1-3 C substituted or unsubstituted with alkyl groups 6-30 is an arylene group, L 1 and L 2 are each independently a direct bond or C 1-5 is an alkylene group, L 3 is C 1-5 It is an alkylene group.
[0055] As an example, in Formula 2, Ar may be a phenylene group or a phenylene group substituted with a methyl group; 1 and L 2 each may be a direct bond, a methylene group, or an ethylene group;3 can be a methylene group, an ethylene group, a propylene group, or a butylene group.
[0056] As a non-limiting example, the repeating unit including the urethane group may be represented by the following Formula 3:
[0057] [Chemical formula 3] TIFF0007579980000003.tif32123
[0058] According to one embodiment of the invention, the organic copolymer is obtained by a condensation polymerization reaction between the siloxane compound and a polyurethane having a repeating unit including a urethane group.
[0059] In this case, the siloxane compound may have a weight average molecular weight (Mw) of 1500 to 2500 g / mol, alternatively 1600 to 2500 g / mol, alternatively 1600 to 2300 g / mol, alternatively 1700 to 2300 g / mol, or alternatively 1700 to 2000 g / mol.
[0060] The polyurethane may have a weight average molecular weight (Mw) of 10,000 to 30,000 g / mol, alternatively 12,000 to 30,000 g / mol, alternatively 12,000 to 28,000 g / mol, alternatively 15,000 to 28,000 g / mol, alternatively 15,000 to 25,000 g / mol.
[0061] In the present invention, the weight average molecular weight (Mw) can be measured by completely dissolving the compound to be measured in a solvent and then utilizing gel permeation chromatography (GPC) under the following conditions.
[0062] -Analytical equipment: PL-GPC 220 system -Column: 2 x PLGEL MIXED-B (7.5 x 300 mm) -Solvent: Trichlorobenzene (TCB) + 0.04 wt% dibutylhydroxytoluene (BHT) (after drying with 0.1% CaCl2 )(CaCl 2 (after drying at -Injector, detected temperature: 160℃ -Flow rate: 1.0ml / min -Injection volume: 200μl -Standard sample: polystyrene
[0063] According to another embodiment of the invention, the organic copolymer may be obtained by reacting the siloxane compound with an excess of a diisocyanate compound to prepare a polysiloxane terminated with an isocyanate group; and reacting the polysiloxane terminated with an isocyanate group with a diol compound to provide the organic copolymer.
[0064] The protective layer can be formed on the inorganic barrier layer by a conventional method in the technical field to which the present invention pertains.
[0065] For example, the protective layer may be laminated by a wet coating method, such as a bar coating method, a spin coating method, a roller coating method, a spray coating method, an air knife coating method, a flow coating method, a curtain coating method, a direct gravure method, a slit reverse method, etc.
[0066] As another example, the protective layer can be laminated onto the inorganic barrier layer using an adhesive or adhesive film.
[0067] According to one embodiment of the present invention, the protective layer may include a mixture of the organic copolymer and a silane coupling agent, that is, the protective layer may further include a silane coupling agent capable of improving adhesion to the inorganic barrier layer.
[0068] According to one embodiment of the invention, the protective layer can have a thickness of 1 nm to 1000 nm.
[0069] In order to achieve appropriate physical properties as a protective layer, the thickness of the protective layer is preferably 1 nm or more. However, if the protective layer is too thick, flexibility is reduced and curling due to stress may occur. Therefore, the thickness of the protective layer is preferably 1000 nm or less.
[0070] More preferably, the thickness of the protective layer may be from 5 nm to 1000 nm, alternatively from 5 nm to 800 nm, alternatively from 10 nm to 800 nm, alternatively from 50 nm to 700 nm, alternatively from 100 nm to 700 nm, alternatively from 200 nm to 600 nm.
[0071] According to one embodiment of the invention, the laminate can be used as a food packaging material. According to another embodiment of the invention, the laminate can be applied to various electronic elements such as liquid crystal display elements, solar cells, touch panels, organic EL elements, organic TFTs, organic semiconductor sensors, organic light-emitting devices, film capacitors, inorganic EL elements, and color filters, or can be used as packaging materials for the electronic elements.
[0072] The laminate according to the present invention, by containing the above-mentioned layer structure and components, can maintain excellent interlayer adhesion even when subjected to deformation such as bending, and can therefore exhibit excellent moisture and oxygen barrier properties.
[0073] One of the key attributes of a flexible barrier material is its resistance to repeated deformation, known as flex durability or Gelboflex. Such a property can be evaluated by the Gelboflex test.
[0074] The test may be performed in accordance with ASTM F392 (Standard Practice for Conditioning Flexible Barrier Materials for Flex Durability) using a Gelbo Flex Tester.
[0075] For example, in the test, the laminate sample is attached to the mandrel of the Gelbo Flex Tester. The bending motion consists of a horizontal motion (compression) combined with a twisting motion to repeatedly twist and bend the laminate. The bending speed is 45-60 cycles per minute. After a predetermined number of strokes, the laminate sample is inspected. The inspection checks the amount of change in moisture barrier properties, oxygen barrier properties, and peel test results of the laminate sample before and after the Gelbo Flex test. Effect of the Invention
[0076] The moisture and oxygen barrier laminate according to the present invention has improved durability and flexibility. The laminate can maintain excellent interlayer adhesion even when subjected to deformation such as bending, and therefore can exhibit excellent moisture and oxygen barrier properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0077] Preferred examples are presented below for understanding the present invention. However, the following examples are merely for illustrating the present invention and are not intended to limit the present invention thereto.
[0078] Production Example 1 (Production of Organic Copolymer) Polydimethylsiloxane (weight average molecular weight 1810 g / mol, manufacturer: Shin-Esu Chemical) terminated at both ends with carbinol groups was prepared. Polyurethane (weight average molecular weight 20000 g / mol, manufacturer: Mitsui Chemical) having the repeating unit of the following chemical formula 3 was prepared.
[0079] [Chemical formula 3] TIFF0007579980000004.tif31123
[0080] In a polymerization reactor, 1.5 g (15 wt%) of the polydimethylsiloxane (solid content 100 wt%) and 25.75 g (85 wt%) of the polyurethane (solid content 33 wt%) were stirred at 100 to 200 rpm, and then 115.6 g of a solvent, isopropyl alcohol (IPA), was added to the reactor, and a condensation polymerization reaction was carried out for 2 hours at 80°C with stirring at 300 to 400 rpm.
[0081] Through the condensation polymerization reaction, a block copolymer (solid content 7 wt %) having the repeating unit derived from the polydimethylsiloxane and the repeating unit of Chemical Formula 3 was obtained.
[0082] Production Example 2 (Production of Organic Copolymer) A block copolymer was obtained in the same manner as in Production Example 1, except that 1 g (10 wt %) of the polydimethylsiloxane and 27.27 g (90 wt %) of the polyurethane were placed in the polymerization reactor and subjected to a condensation polymerization reaction.
[0083] Example 1 A PET film with a thickness of 12 μm was prepared as a transparent substrate. The PET film was fixed to the plate of a thermal evaporation device (model name: Daon-100-TE, manufacturer: DAON) with tape, and an Al chip (purity 99.999%) was placed on the evaporation boat. Then, a rotary pump and a diffusion pump were operated to create a vacuum (4.4X10 -5 The inorganic barrier layer was formed by depositing aluminum oxide (AlOx) to a thickness of 10 nm on the PET film under the conditions of an evaporation rate of 2.0 Å / s, an oxygen flow rate of 23 sccm, an operating time of 19.8 s, and an applied current of 175.2 A.
[0084] The block copolymer-containing solution obtained in Preparation Example 1 was bar coated (#6, thickness 550 nm) on the inorganic barrier layer, and dried with hot air (100° C., 12 s) to form a protective layer having a thickness of 550 nm.
[0085] A laminate including the inorganic barrier layer and the protective layer, which were formed in this order on the transparent substrate by the above method, was obtained.
[0086] Example 2 A laminate was obtained in the same manner as in Example 1, except that 1 wt % of a silane coupling agent (product name: KBM403, manufacturer: Shin-Etsu Chemical) was further added to the block copolymer-containing solution based on the total weight of the solution.
[0087] Example 3 A laminate was obtained in the same manner as in Example 1, except that the block copolymer obtained in Production Example 2 was used instead of Production Example 1.
[0088] Comparative Example 1 A laminate was obtained in the same manner as in Example 1, except that the protective layer was not formed on the inorganic barrier layer.
[0089] Comparative Example 2 A laminate was formed in the same manner as in Example 1, except that the protective layer was formed by bar coating the polydimethylsiloxane (weight average molecular weight 1810 g / mol, manufacturer: Shin-Etsu Chemical) terminated at both ends with a carbinol group instead of the block copolymer-containing solution onto the inorganic barrier layer.
[0090] Comparative Example 3 A laminate was formed in the same manner as in Example 1, except that a polyurethane (weight average molecular weight 20,000 g / mol, manufacturer: Mitsui Chemical) having a repeating unit of the chemical formula 3 was bar-coated on the inorganic barrier layer to form the protective layer, instead of the block copolymer-containing solution.
[0091] Comparative Example 4 A 12 μm thick PET film was prepared as a transparent substrate. The PET film was fixed to the plate of a thermal evaporation device (model name: Daon-100-TE, manufacturer: DAON) with tape, and an Al chip (purity 99.999%) was placed on the boat. The rotary pump and diffusion pump were then operated to create a vacuum (4.4X10 -5 Under the conditions of evaporation rate 2.0 Å / s, oxygen flow rate 23 sccm, working time 19.8 s, and applied current 175.2 A, aluminum oxide (AlOx) was evaporated to a thickness of 10 nm on the PET film to form an inorganic barrier layer.
[0092] Next, silicon oxide (SiOx) was deposited on the inorganic barrier layer to a thickness of 100 nm using the same thermal evaporation equipment as above to form an inorganic protective layer. Specifically, the PET film on which the inorganic barrier layer was formed was fixed to the plate of the thermal evaporation equipment with tape, SiO chips (silicon monoxide, purity 99.999%) were placed on a boat, and a rotary pump and a diffusion pump were operated to create a vacuum state (4.4X10 -5 The inorganic protective layer was formed by depositing silicon oxide (SiOx) to a thickness of 100 nm on the inorganic barrier layer under the conditions of an evaporation rate of 140.0 Å / s, an oxygen flow rate of 10 sccm, an operation time of 19.8 s, and an applied current of 140 A.
[0093] A laminate including the inorganic barrier layer and the inorganic protective layer, which were formed in this order on the transparent substrate by the above method, was obtained.
[0094] Test Example (1) Evaluation of moisture barrier properties Using a moisture permeability analyzer (model: AQUATRAN 2 WVTR Analyzer, manufacturer: Mocon), the standard test method of ASTM F1249 was used to measure the moisture permeability at 50 cm under conditions of 40°C and 90% relative humidity. 2 After mounting the laminate sample, the moisture permeation rate (g / m 2 *day) was measured.
[0095] (2) Evaluation of oxygen barrier properties Using an oxygen transmission rate analyzer (model name: OX-Tran 2 / 21 OTR Analyzer, manufacturer: Mocon), the standard test method of ASTM D3985 was used to measure the oxygen transmission rate at 50 cm under conditions of 23°C and 0% relative humidity. 2 After mounting the laminate sample, the oxygen permeation rate (cc / m 2 *day) was measured.
[0096] (3) Peel test An adhesive composition was prepared by mixing 15.3 g of a main component (product name: TM-585-60K, solid content 60 wt%), 1.9 g of a hardener component (product name: CAT-10, solid content 75 wt%), and 25.2 g of a solvent (ethyl acetate). The adhesive composition was bar-coated (#12, thickness 5 μm standard) on the protective layer of the laminate, and then dried with hot air (100°C, 20 s) to form an adhesive layer with a thickness of 5 μm. A CPP film was laminated on the adhesive layer, and aged at 45°C for 1 day to prepare a test sample.
[0097] Two pieces of double-sided tape were attached to the measurement plate of a peel tester (model name: AR-1000, manufacturer: ChemInstruments), and then the test sample cut to a width of 2.5 cm was attached to the plate. A 180° peel test was performed according to the standard test method of ASTM D3330 to obtain the peel strength value (gf / cm).
[0098] (4) Gelbo flex test The laminates obtained in the above Examples and Comparative Examples were subjected to a Gelbo flex test by the following method.
[0099] The test was performed using a Gelbo Flex Tester (model name: G0005, manufacturer: IDM Instruments) according to the standard test method of ASTM F392. Specifically, a nylon fiber and a cast (non-oriented) polypropylene (CPP) film were sequentially laminated using an adhesive on the other side of the transparent substrate, on which the inorganic barrier layer and the protective layer of the laminate were not formed, to prepare a test sample. The test sample was attached to the mandrel of the Gelbo Flex Tester. The test setting provided a 440 degree twisting motion in the first 90 mm of the stroke, followed by a 65 mm linear horizontal motion. At this time, the bending motion speed was set to 50 cycles per minute.
[0100] After 50 cycles of strokes, the laminate was collected from the test sample, and the (1) evaluation of moisture barrier property, (2) evaluation of oxygen barrier property, and (3) peel test were performed again.
[0101] [Table 1]
[0102] [Table 2]
[0103] Referring to Table 1, the laminates according to the examples have excellent initial moisture and oxygen barrier properties, and in particular, they exhibit excellent moisture and oxygen barrier properties and peel properties even after the Gelbo flex test. In addition, when an organic copolymer having a relatively high content of repeating units including a urethane group is applied to the protective layer, it shows excellent peel strength although the moisture and oxygen barrier properties are somewhat lower.
[0104] In contrast, referring to Table 2, the laminate of Comparative Example 1 had poor initial moisture and oxygen barrier properties compared to the Examples, and the laminates of Comparative Examples 1 to 3 exhibited significant deterioration in the properties after the Gelbo flex test. The laminate of Comparative Example 4 exhibited the best initial moisture and oxygen barrier properties, but the properties rapidly deteriorated after the Gelbo flex test.
Claims
1. The present invention includes an inorganic barrier layer and a protective layer formed in sequence on one surface of a transparent substrate, the protective layer comprises an organic copolymer, the organic copolymer being a block copolymer comprising 1 to 40% by weight of a repeating unit derived from a siloxane compound and 60 to 99% by weight of a repeating unit containing a urethane group (—NHCOO—); the organic copolymer is obtained by a condensation polymerization reaction between the siloxane compound having a weight average molecular weight of 1500 to 2500 g / mol and a polyurethane having a weight average molecular weight of 10000 to 30000 g / mol and a repeating unit including a urethane group, A laminate, wherein the siloxane compound is a polysiloxane terminated at both ends with a carbinol group.
2. The laminate according to claim 1 , wherein the siloxane compound is a polysiloxane represented by the following chemical formula 1: [Chemical formula 1] (In the above Chemical Formula 1, R 1 ~R 6 are each independently a monovalent C 1-10 is a hydrocarbon radical, R 7 and R 8 are each independently a divalent C 1-10 It is a hydrocarbon radical.
3. The R 1 ~R 6 are each independently a methyl group, an ethyl group, a propyl group, or a phenyl group, 7 and R 8 The laminate according to claim 2 , wherein each of the groups independently represents a methylene group, an ethylene group, a propylene group, or a phenylene group.
4. The laminate according to claim 1 , wherein the repeating unit containing a urethane group is represented by the following chemical formula 2: [Chemical formula 2] (In the above Chemical Formula 2, Ar is C 1-3 C substituted or unsubstituted with an alkyl group 6-30 is an arylene group, L 1 and L 2 are each independently a direct bond or C 1-5 is an alkylene group, L 3 is C 1-5 It is an alkylene group.
5. The laminate according to claim 1 , wherein the protective layer comprises a mixture of the organic copolymer and a silane coupling agent.
6. The laminate according to claim 1, wherein the transparent substrate is a plastic film containing one or more polymers selected from the group consisting of polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, cycloolefin polymer, cycloolefin copolymer, polycarbonate, and poly(methyl methacrylate).
7. 2. The laminate according to claim 1, wherein the inorganic barrier layer comprises one or more inorganic substances selected from the group consisting of silicon oxide, silicon oxynitride, silicon nitride, aluminum oxide, and aluminum nitride.
8. The laminate according to claim 1 , wherein the transparent substrate has a thickness of 5 μm to 300 μm.
9. The laminate of claim 1 , wherein the inorganic barrier layer has a thickness of 1 nm to 200 nm.
10. The stack of claim 1 , wherein the protective layer has a thickness of 1 nm to 1000 nm.
Citation Information
Patent Citations
Barrier film and laminate using barrier film
JP2003205573A
A multilayer article comprising a first layer of thermoset polyurethane
JP2004516958A
Package
JP2006522695A
Protective film
JP2012134445A
Transparent weather-resistant barrier sheet, and manufacturing of the barrier sheet by lamination, extrusion lamination, or extrusion coating.