Image forming device

By optimizing the crystallinity and dispersibility of carbon black in a thermoplastic resin-based intermediate transfer belt, the solution addresses mechanical strength and resistance issues, improving image quality and durability.

JP7581036B2Active Publication Date: 2024-11-12CANON KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020207098
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-14
Publication Date
2024-11-12
Estimated Expiration
2040-12-14

AI Technical Summary

Technical Problem

Existing intermediate transfer belts made of thermoplastic resin with carbon black face challenges in maintaining both mechanical strength and carbon black dispersibility, leading to image defects like white spots and belt breakage due to resistance fluctuations and discharge issues.

Method used

The intermediate transfer belt is composed of a thermoplastic resin with carbon black dispersed within specific crystallinity and particle size ranges, and controlled surface and central area dispersibility, ensuring mechanical strength and resistance stability.

Benefits of technology

This approach enhances the mechanical strength and dispersibility of carbon black, reducing discharge-induced image defects and belt durability, particularly in low humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581036000005
    Figure 0007581036000005
  • Figure 0007581036000006
    Figure 0007581036000006
  • Figure 0007581036000007
    Figure 0007581036000007
Patent Text Reader

Abstract

To achieve, in an intermediate transfer belt containing thermoplastic resin and carbon black, both mechanical strength and dispersibility of carbon black.SOLUTION: The degree of crystallinity of thermoplastic resin is 8% or more and 25% or less. The average primary particle diameter of carbon black is 10 nm or more and 30 nm or less. The content of carbon black is 15.0 pts.mass or more and 30.0 pts.mass or less based on 100 pts.mass of an intermediate transfer belt. When Li, Lo, Lc are respectively values of an L-function indicating dispersibility of carbon black to thermoplastic resin in an inner peripheral surface area and an outer peripheral surface area of the intermediate transfer belt, and a center area being a center part in a thickness direction of the intermediate transfer belt, (Li+Lo+Lc) / 3≤100 nm.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an intermediate transfer member that carries a toner image, and an image forming apparatus having the intermediate transfer member. [Background technology]

[0002] Conventionally, for example, in image forming apparatuses using an electrophotographic system, an intermediate transfer system has been widely used in which a toner image is primarily transferred onto an intermediate transfer body in a primary transfer section, and then the toner image is secondarily transferred onto a recording material such as paper in a secondary transfer section to output an image. The intermediate transfer body is also called an intermediate transfer belt.

[0003] As an intermediate transfer member, one has been proposed in which a conductive filler is added to a resin material to adjust the electrical resistance to a desired value (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-112942 A Summary of the Invention [Problem to be solved by the invention]

[0005] The intermediate transfer body used in the intermediate transfer method is usually suspended between two or more rollers and rotated under tension for a long period of time. Therefore, the intermediate transfer body is required to have high durability, and it is desirable for the intermediate transfer body to have excellent mechanical properties, particularly tensile elastic modulus and bending durability. For example, if the tensile elastic modulus of the intermediate transfer body is too low, the intermediate transfer belt will be distorted depending on the usage conditions, which will not only impair the durability of the intermediate transfer body itself, but will also cause image defects due to distortion or misalignment of the toner image transferred onto the surface of the intermediate transfer body. Poor bending durability will lead to breakage or cracking of the belt.

[0006] In an intermediate transfer body made of a resin composition mainly composed of a thermoplastic resin, it is possible to obtain an intermediate transfer body having the desired tensile strength, bending durability, and surface hardness by increasing the crystallinity of the resin composition by heating. However, when a sheet or resin film whose resistance is controlled to a semiconductive region by a conductive filler such as conductive carbon black is heated to above its melting point to modify the surface, slight temperature or pressure unevenness causes fluctuations in the resistance value, resulting in uneven resistance value. It is presumed that this is due to the fact that heating promotes the aggregation of the carbon black contained in the resin composition, which deteriorates the dispersibility of the carbon black.

[0007] In particular, in resin films made of thermoplastic resins, the resistance fluctuation becomes large at temperatures just below the melting point. This is presumably because, as the thermoplastic resin crystallizes, carbon black becomes more likely to precipitate at the crystallized sites of the thermoplastic resin, which in turn promotes the aggregation of carbon black (deterioration of dispersibility).

[0008] When the dispersion of the conductive filler in the intermediate transfer body, which is a resin film, becomes poor, image defects may occur, especially in low humidity environments. In the primary transfer section, if a gap occurs between the inner circumferential surface of the intermediate transfer body and the primary transfer roller, discharge occurs between the aggregated part of the conductive filler in the intermediate transfer body and the primary transfer roller, and the resistance of the intermediate transfer body decreases locally. Toner is not transferred to the part with the decreased resistance, and a white-out image (whiteout) occurs. This behavior is particularly noticeable when a metal roller is used as the primary transfer roller. In the secondary transfer section, if a gap occurs between the outer circumferential surface of the intermediate transfer body and the paper, discharge occurs between the aggregated part of the conductive filler in the intermediate transfer body and the paper, and the toner on the intermediate transfer body reverses its charge polarity due to the discharge, and the toner cannot be transferred to the paper, resulting in a whiteout image.

[0009] For the reasons described above, in an intermediate transfer belt made of a thermoplastic resin containing carbon black, it has been difficult to simultaneously ensure the mechanical strength of the intermediate transfer belt and improve the dispersibility of the carbon black.

[0010] SUMMARY OF THE PRESENT EMBODIMENTS The present invention has an object to provide an intermediate transfer belt made of a thermoplastic resin containing carbon black, which can ensure the mechanical strength of the intermediate transfer belt while improving the dispersibility of the carbon black. [Means for solving the problem]

[0011] The above problems can be solved by the means described below.

[0012] In the present invention The image forming apparatus includes an image carrier that carries a toner image, an intermediate transfer belt onto which the toner image formed on the image carrier is primarily transferred, a metal roller that primarily transfers the toner image from the image carrier to the intermediate transfer belt, and a secondary transfer member that secondarily transfers the toner image from the intermediate transfer belt to a recording material, the intermediate transfer belt being made of a thermoplastic resin having carbon black dispersed therein, the thermoplastic resin having a degree of crystallinity of 8% or more and 25% or less, the carbon black having an average primary particle size of 10 nm or more and 30 nm or less, and the carbon black having a content of 10% or more and 10% or less. the intermediate transfer belt has a mass of 15.0 parts or more and 30.0 parts or less per 100 parts by mass, the outer circumferential surface region is a range from an outer circumferential surface on which a toner image is carried to 10 μm in the thickness direction, the inner circumferential surface region is a range from an inner circumferential surface on the back side of the outer circumferential surface to 10 μm in the thickness direction, and the central region is a range of 5 μm from a center in the thickness direction, and the values ​​of an L function indicating the dispersibility of the carbon black in the thermoplastic resin in the inner circumferential surface region, the outer circumferential surface region, and the central region are Li, Lo, and Lc, respectively, satisfying (Li+Lo+Lc) / 3≦100 nm and Li≦150 nm. It is characterized by the above. Effect of the Invention

[0013] According to the present invention, in an intermediate transfer belt made of a thermoplastic resin containing carbon black, it is possible to ensure the mechanical strength of the intermediate transfer belt while improving the dispersibility of the carbon black. [Brief description of the drawings]

[0014] [Figure 1] Schematic diagram of a cross section of an intermediate transfer member according to the present embodiment. [Diagram 2] 1 is a schematic cross-sectional view of an image forming apparatus using an intermediate transfer member according to the present embodiment; [Diagram 3] FIG. 2 is a diagram showing the molding process in this embodiment. [Figure 4] FIG. 1 shows the complex viscosity of the PEEK resin in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The intermediate transfer member and the method for producing the intermediate transfer member according to this embodiment will be described in more detail below with reference to the drawings.

[0016] 1. Image forming equipment First, an embodiment of an image forming apparatus using an intermediate transfer member (intermediate transfer belt) according to the present embodiment will be described. Fig. 1 is a schematic cross-sectional view of an image forming apparatus 100 according to the present embodiment. The image forming apparatus 100 according to the present embodiment is a tandem type color laser printer that employs an intermediate transfer method and is capable of forming a full-color image using an electrophotographic method.

[0017] The image forming apparatus 100 has a first, second, third, and fourth image forming units PY, PM, PC, and PK as a plurality of image forming units. The first, second, third, and fourth image forming units PY, PM, PC, and PK are arranged in this order along the moving direction of a flat portion (image transfer surface) of an intermediate transfer belt 7 described later. Elements having the same or corresponding functions or configurations in the first, second, third, and fourth image forming units PY, PM, PC, and PK may be generally described by omitting the suffixes Y (or y), M (or m), C (or c), and K (or k) of the reference characters indicating that the elements are for any color. In this embodiment, the image forming unit P is configured to have a photosensitive drum 1, a charging roller 2, an exposure device 3, a developing device 4, and a primary transfer roller 5 described later.

[0018] The image forming section P has a photosensitive drum 1, which is a drum-type (cylindrical) photosensitive body (electrophotographic photosensitive body) serving as an image carrier. The photosensitive drum 1 is formed by sequentially laminating a charge generating layer, a charge transport layer, and a surface protection layer on an aluminum cylinder serving as a base. The photosensitive drum 1 is driven to rotate in the direction of the arrow R1 in the figure (counterclockwise). The surface of the rotating photosensitive drum 1 is uniformly charged to a predetermined potential of a predetermined polarity (negative polarity in this embodiment) by a charging roller 2, which is a roller-shaped charging member serving as a charging means. During the charging process, a predetermined charging bias (charging voltage) containing a negative DC component is applied to the charging roller 2. The surface of the charged photosensitive drum 1 is scanned and exposed according to image information by an exposure device (laser scanner) 3 serving as an exposure means, and an electrostatic image (electrostatic latent image) is formed on the photosensitive drum 1.

[0019] The electrostatic image formed on the photosensitive drum 1 is developed (visualized) by supplying toner as a developer by a developing device 4 as a developing means, and a toner image (developer image) is formed on the photosensitive drum 1. During the development process, a predetermined development bias (developing voltage) including a negative DC component is applied to a developing roller 4a as a developer carrier provided in the developing device 4. In this embodiment, toner charged with the same polarity as the charging polarity of the photosensitive drum 1 (negative polarity in this embodiment) adheres to an exposed portion (image portion) on the photosensitive drum 1 where the absolute value of the potential has been reduced by exposure after being uniformly charged.

[0020] An intermediate transfer belt 7, which is an endless belt serving as an intermediate transfer body, is disposed so as to face the four photosensitive drums 1. The intermediate transfer belt 7 is stretched around a driving roller 71, a tension roller 72, and a secondary transfer opposing roller 73 serving as a plurality of tension rollers, and tensioned with a predetermined tension. The intermediate transfer belt 7 comes into contact with the photosensitive drums 1 and rotates (moves around) in the direction of the arrow R2 (clockwise) in the figure as the driving roller 71 is rotated. On the inner peripheral surface side of the intermediate transfer belt 7, a primary transfer roller 5, which is a roller-shaped primary transfer member serving as a primary transfer means, is disposed in correspondence with each photosensitive drum 1. The primary transfer roller 5 is pressed against the photosensitive drum 1 via the intermediate transfer belt 7, forming a primary transfer portion (primary transfer nip) T1 where the photosensitive drum 1 and the intermediate transfer belt 7 come into contact with each other. The toner image formed on the photosensitive drum 1 as described above is primarily transferred onto the rotating intermediate transfer belt 7 by the action of the primary transfer roller 5 at the primary transfer portion T1. During the primary transfer process, a primary transfer bias (primary transfer voltage) which is a DC voltage of the opposite polarity (positive polarity in this embodiment) to the normal charging polarity of the toner (charging polarity during the development process) is applied to the primary transfer roller 5. The primary transfer roller 5 is composed of a metallic rotating shaft and an elastic layer formed on the outer circumferential surface of the rotating shaft. The primary transfer roller 5 is often adjusted to a desired resistance value, but it may also be composed of a metal roller made of material such as SUM (sulfur and sulfur composite free-cutting steel) or SUS (stainless steel) that is straight in the thrust direction.

[0021] A secondary transfer roller 8, which is a roller-shaped secondary transfer member serving as a secondary transfer means, is disposed at a position facing the secondary transfer opposing roller 73 on the outer peripheral surface side of the intermediate transfer belt 7. The secondary transfer roller 8 is pressed against the secondary transfer opposing roller 73 via the intermediate transfer belt 7, forming a secondary transfer section (secondary transfer nip) T2 where the intermediate transfer belt 7 and the secondary transfer roller 8 come into contact with each other. The toner image formed on the intermediate transfer belt 7 as described above is secondarily transferred by the action of the secondary transfer roller 8 at the secondary transfer section T2 onto a recording material (sheet, transfer material) S such as paper (paper) that is being conveyed while being sandwiched between the intermediate transfer belt 7 and the secondary transfer roller 8. During the secondary transfer process, a secondary transfer bias (secondary transfer voltage), which is a DC voltage of the opposite polarity to the normal charging polarity of the toner, is applied to the secondary transfer roller 8. In the secondary transfer, a transfer voltage of several kV is usually applied to ensure sufficient transfer efficiency. The recording material S is supplied to a conveying path by a pickup roller 13 from a cassette 12 in which the recording material S is stored. The recording material S supplied to the conveying path is conveyed to the secondary transfer portion T2 by a pair of conveying rollers 14 and a pair of registration rollers 15 in synchronization with the toner image on the intermediate transfer belt 7.

[0022] The recording material S onto which the toner image has been transferred is transported to a fixing device 9 as a fixing means. The fixing device 9 heats and pressurizes the recording material S carrying the unfixed toner image, thereby fixing (melting and bonding) the toner image onto the recording material S. The recording material S onto which the toner image has been fixed is discharged (output) to the outside of the main body of the image forming apparatus 100 by a pair of transport rollers 16, a pair of discharge rollers 17, etc.

[0023] Toner (primary transfer residual toner) remaining on the surface of the photosensitive drum 1 without being transferred to the intermediate transfer belt 7 in the primary transfer process is developed and collected by the developing device 4, which also serves as a photosensitive body cleaning means. Toner (secondary transfer residual toner) remaining on the surface of the intermediate transfer belt 7 without being transferred to the recording material S in the secondary transfer process is removed from the surface of the intermediate transfer belt 7 and collected by a belt cleaning device 11, which serves as an intermediate transfer body cleaning means. The belt cleaning device 11 is disposed downstream of the secondary transfer portion T2 and upstream of the most upstream primary transfer portion T1y in the rotation direction of the intermediate transfer belt 7 (at a position facing the drive roller 71 in this embodiment). The belt cleaning device 11 scrapes off the secondary transfer residual toner from the surface of the rotating intermediate transfer belt 7 by a cleaning blade, which serves as a cleaning member disposed so as to come into contact with the surface of the intermediate transfer belt 7, and stores it in a collection container 11b.

[0024] In this manner, in the image forming operation, the process of electrically transferring the toner image from the photosensitive drum 1 to the intermediate transfer belt 7 and from the intermediate transfer belt 7 to the recording material S is repeated. Furthermore, by repeating image formation on a large number of recording materials S, the electrical transfer process is further repeated.

[0025] 2. Intermediate transfer body The intermediate transfer belt 7 as an intermediate transfer body includes at least a base layer (substrate), and may be a laminated body composed of a plurality of layers including a surface layer (surface layer). FIG. 2 is a schematic cross-sectional view for explaining an example of the layer structure of the intermediate transfer belt 7. As shown in FIG. 2(a), the intermediate transfer belt 7 may be composed of a single layer (here, the single layer may also be referred to as the "base layer") 7a. As shown in FIG. 2(b), the intermediate transfer belt 7 may be composed of at least two layers, the base layer 7a and the surface layer 7b provided on the base layer 7a. For example, another layer such as an intermediate layer may be provided between the base layer 7a and the surface layer 7b. As will be described in detail below, the base layer 7a is a semiconductive film in which a conductive filler is contained in a resin.

[0026] 2-1. Structure and characteristics of intermediate transfer medium <Resin materials> The following can be used as the resin material for the base layer of an intermediate transfer belt composed of a single layer or an intermediate transfer belt composed of at least two layers. That is, thermoplastic resins such as polyphenylene sulfide (PPS), polyetherimide (PEI), polyetheretherketone (PEEK), etc. are usable. In particular, since the intermediate transfer belt is required to not stretch even when subjected to a tensile load over a long period of time and not to be worn on the surface by rubbing with a cleaning blade, polyetheretherketone (PEEK) is preferable. In addition, two or more of these resins may be selected and mixed as necessary.

[0027] <Conductive filler> At least one type of conductive filler, such as carbon black or metal particles, is blended into the resin material to impart electrical conductivity to the base layer. Of these, carbon black is preferred from the viewpoint of mechanical properties. Carbon black is called various names depending on its manufacturing method and raw materials. Specifically, it is called Ketjen black, furnace black, acetylene black, thermal black, gas black, etc.

[0028] As the carbon black, various known ones can be used. Specific examples include Ketjen black, furnace black, acetylene black, thermal black, and gas black. Among these, acetylene black and furnace black are preferred because they contain fewer impurities, have a lower frequency of foreign matter defects when molded into a film shape together with the above-mentioned thermoplastic resin, and are easy to obtain the desired conductivity. Specific examples of acetylene black include the "Denka Black" series (manufactured by Denki Kagaku Kogyo Co., Ltd.), the "Mitsubishi Conductive Filler" series (manufactured by Mitsubishi Chemical Corporation), the "Vulcan" series (manufactured by Cabot Corporation), the "Brintex" series (manufactured by Degussa Co., Ltd.), and "SRF" (manufactured by Asahi Carbon Co., Ltd.). Specific examples of furnace black include the "Touka Black" series (manufactured by Tokai Carbon Co., Ltd.), the "Asahi Carbon Black" series (manufactured by Asahi Carbon Co., Ltd.), and the "Niteron" series (manufactured by Shin-Nichika Carbon Co., Ltd.).

[0029] <Primary particle size of carbon black> The conductive filler to be added has an average primary particle size of preferably 10 nm or more and 30 nm or less. If a conductive filler having an average primary particle size of less than 10 nm is used, the filler is likely to re-aggregate, and the heat resistance is reduced, making it difficult to use the filler in an intermediate transfer body. On the other hand, if a conductive filler having a particle size of more than 30 nm is used, dispersibility is likely to deteriorate when aggregates are generated, and the resistance of the intermediate transfer body is likely to decrease due to discharge. Therefore, by using an average primary particle size within the above range, good resistance retention without defects can be obtained.

[0030] <Conductive filler content> The content of the conductive filler to be added is selected in consideration of the ability to impart the necessary conductivity to the belt member, mechanical strength such as bending resistance and elastic modulus of the belt member, and thermal conductivity. If the content of the conductive filler is too high, the conductivity may increase too much or the mechanical strength may decrease, so it is preferable to keep the content at 30.0 wt% or less.

[0031] On the other hand, if the content is too small, the conductivity of the belt member may become too small, or it may become difficult to maintain a good dispersion state of the conductive filler inside the intermediate transfer belt, so the content of the conductive filler is preferably 15.0 wt% or more, and more preferably 20.0 wt% or more. In other words, it is preferably 15.0 parts by mass or more and 30.0 parts by mass or less per 100 parts by mass of the intermediate transfer belt.

[0032] <Crystallization degree> Thermoplastic resins are made of entangled string-like polymers, and are broadly divided into two types, crystalline resins and amorphous resins, depending on the properties when solidified. When the temperature is lowered from the temperature of the molten state, the molecules are entangled while moving in the molten state, but as the temperature is lowered, the molecular motion slowly subsides and some resins are partially aligned at the crystallization temperature (Tc). This is called a crystalline resin, and those that solidify while remaining randomly entangled are called amorphous resins. The crystallinity is calculated by calculating the proportion of the crystalline region (C) among the crystalline region (C) and the amorphous region (G) of the resin solid. The crystallinity is used as an index of the strength, rigidity, transparency, molding shrinkage, etc. of the resin material. In this embodiment, the crystallinity is measured by wide-angle X-ray diffraction (XRD), and if the crystallinity is less than 8%, it is considered to be in an amorphous state. In this embodiment, the crystallinity of the thermoplastic resin is preferably 8% or more and 25% or less. If the crystallinity of the thermoplastic resin is less than 8%, the mechanical strength of the intermediate transfer belt is reduced, and if the crystallinity is more than 25%, the carbon black will aggregate.

[0033] <Dispersibility> Dispersibility is evaluated by the L function described later. In the primary transfer section, when a metal roller is used as the primary transfer member, the L function value of the inner peripheral surface of the intermediate transfer body is preferably 150 nm or less. If the L function is greater than 150 nm, the resistance of the intermediate transfer body is likely to decrease due to discharge in the primary transfer section. That is, as described later, when the value of the L function indicating the dispersibility of carbon black in the thermoplastic resin in the inner peripheral surface region of the intermediate transfer belt is Li, Li≦150 nm is preferable.

[0034] When a metal roller is used as the primary transfer member, the reason why the resistance of the intermediate transfer body is likely to decrease due to discharge at the primary transfer section is as follows. That is, when the primary transfer member is a metal roller, if the intermediate transfer body is opposed to the photosensitive drum so as to be nipped between the metal roller and the photosensitive drum, the photosensitive drum may be damaged. For this reason, the photosensitive drum and the metal roller are offset from each other in the moving direction of the intermediate transfer body so that the intermediate transfer body is not nipped between them. For this reason, when the primary transfer member is a metal roller, if the intermediate transfer body is wavy, a gap may be generated at the primary transfer section, and discharge is likely to occur. On the other hand, when the primary transfer member is a sponge roller, the photosensitive drum and the sponge roller nip the intermediate transfer body to form the primary transfer section. For this reason, even if the intermediate transfer body is wavy, no gap is generated at the primary transfer section, and discharge is unlikely to occur.

[0035] In the secondary transfer portion, the average value of the L function in the central region, the inner peripheral surface, and the outer peripheral surface of the intermediate transfer body is preferably 100 nm or less. If the L function value is more than 100 nm, a decrease in the resistance of the intermediate transfer body due to discharge is likely to occur in the secondary transfer portion.

[0036] That is, as described later, the values ​​of the L function indicating the dispersibility of carbon black in the thermoplastic resin in the inner peripheral surface region, the outer peripheral surface region, and the central region, which is the center in the thickness direction of the intermediate transfer belt, are Li, Lo, and Lc, respectively, where (Li+Lo+Lc) / 3≦100 nm is preferable.

[0037] <Number of conductive points> When a metal roller is used as the primary transfer member, the number of conductive points on the inner peripheral surface of the intermediate transfer member is set to 230 / μm. 2 It is preferable to set the number of conductive points to 230 or more. This makes it possible to suppress the resistance drop of the intermediate transfer body due to discharge even if a gap occurs between the intermediate transfer body and the metal roller. 2If the number is less than 100, discharges occurring in the gap between the primary transfer roller and the intermediate transfer body may occur locally, causing deep discharge marks on the circumferential surface of the intermediate transfer body. Discharge marks are caused by deterioration (carbonization) of the resin, which makes the area more conductive than the surrounding area, i.e., has a lower electrical resistance. This reduces the surface resistivity of the circumferential surface of the intermediate transfer body. The more conductive points there are, the less concentrated the discharges will be, and the number is selected according to the resistance range required for the intermediate transfer body.

[0038] 2-2. Manufacturing method of intermediate transfer member In the present invention, the base layer of the intermediate transfer member composed of a single layer or the intermediate transfer member composed of at least two layers is (1) A molding step of melting a resin composition containing a resin material and a conductive filler at a temperature equal to or higher than the melting temperature of the resin material and molding the resin composition into a tubular shape. (2) A heating and pressurizing process in which the tubular tube obtained in the molding process is sandwiched between a hollow cylindrical inner mold and a hollow cylindrical outer mold with controlled inner surface roughness, and heated to an arbitrary temperature between the glass transition temperature and the crystallization onset temperature of the resin composition at a heating rate of 10°C / min or more, and the tubular tube is pressurized to 10 kgf / cm2 or more in that temperature range, cooled to a temperature below the glass transition point, and removed from the mold. The steps (1) and (2) are described below.

[0039] <Forming process> In the molding process, a resin composition containing a resin material and a conductive filler is molded into a cylindrical tube-like belt shape (tubular tube) using an extrusion molding method. The resin composition used to mold the semiconductive tubular tube of this embodiment can be prepared using any method and equipment. For example, each raw material component can be premixed using a mixer such as a Henschel mixer or a tumbler, and a filler such as glass fiber can be added and further mixed as necessary, and then kneaded and extruded using a single-screw or twin-screw extruder to form molding pellets. A method of preparing a master batch using a portion of the necessary components and mixing this master batch with the remaining components may be adopted. In addition, in order to increase the dispersibility of each raw material component, it is also possible to crush a portion of the raw materials used, mix them with a uniform particle size, and melt extrude them.

[0040] As the extruder in the extrusion molding method, either a single-screw extruder having one screw in a barrel or cylinder or a multi-screw extruder having two or more screws combined can be used. A resin composition containing a resin material and 15 to 30 parts by weight of a conductive filler is supplied from a supply hole in a supply section, and while advancing toward a die by the rotation of the screw, it is completely melted by receiving thermal energy from the barrel or cylinder and mechanical energy from the screw. Then, the resin composition is supplied in a fixed amount to the tip of the extruder while controlling the temperature within a range of from the melting point (Tm) to Tm+80°C, and is melt-extruded into a film from an annular die. Next, the inner peripheral surface of the molten tube is brought into contact with a cooling mandrel controlled to a temperature within a range of from the glass transition temperature (Tg) to Tg, and rapidly cooled and solidified, while the outer surface is gradually cooled using an external heating device controlled to a temperature of from Tm-60°C to Tm to control the crystallinity of the inner surface and the outer surface. The temperature of the resin composition in the extruder is within a range of Tm+20 to 80°C, preferably Tm+30 to 70°C, more preferably Tm+40 to 60°C. The resin temperature can be represented by the die temperature. The molten resin composition drawn down from the die slip is taken up and molded into a film (including a tubular film), and the take-up speed is controlled to adjust the film thickness to a desired value.

[0041] The temperature of the cooling roll or cooling mandrel that is in contact with the molten film (including tubular film) when cooling it is within the range of Tg-60°C to Tg. If the cooling temperature is too high, the resin crystallizes and the semiconductive film tends to become brittle. If the cooling temperature is too low, the cooling becomes uneven, making it difficult to obtain a semiconductive film with excellent flatness and thickness stability.

[0042] When the resin composition is continuously melt-extruded from the die, the aggregation of the conductive filler is promoted as the crystallization progresses, so it is essential that the resulting tubular film is in an amorphous state. The annular die, its temperature control form and shape, and the passing speed of the resin at each location must be carefully selected because they greatly affect the crystallization of the resin. In this embodiment, as shown in FIG. 3, the pellet material is supplied to a single-screw extruder set at a temperature of 340°C to 400°C to melt it, and the resin belt material PE is melt-extruded into a tube shape downward from the lip 31r through the spiral die 31. At this time, the drawing speed is adjusted to stretch the material in the axial direction, and the inner surface of the tube in a nearly molten state is brought into contact with the cooling mandrel 32 to be rapidly cooled, while the outer surface is slowly cooled using an external heating device 33 to control the crystallinity of the inner surface and the outer surface. The passing speed of the resin at the lip 31r and the cooling mandrel 32 was 1.7 mm / s and 30 mm / s, respectively. The cooling mandrel 32 is equipped with a heater and a water cooling device (not shown), and the temperature of the mirror-finished copper surface can be set to any temperature within a range equal to or higher than the cooling water temperature. Temperature-adjusted cooling water is supplied to the water supply pipe 32i, and the cooling water is circulated from the drain pipe 32e to the water supply pipe 32i via a thermostatic bath and a circulation pump. The molten resin was solidified and phase-changed to create a tubular body having a thickness of 60 μm, so that the cooling processes for the front layer and the back layer are different.

[0043] <Heat and pressure process> The tubular tube obtained in the molding process is sandwiched between a hollow cylindrical inner mold and a hollow cylindrical outer mold with controlled inner surface roughness. It is then heated to a desired temperature between the glass transition temperature (Tg) and the crystallization onset temperature (Ts), and pressurized to 10 kgf / cm2 or more in that temperature range, and then cooled to a temperature below the glass transition point and removed from the mold. This allows the degree of crystallization to be increased without causing aggregation of the conductive filler.

[0044] The heating temperature is from the glass transition temperature to the peak temperature where the viscosity starts decreasing, which is the crystallization start temperature, as can be determined by dynamic mechanical analysis (DMA) (Figure 4). In the dynamic mechanical analysis (DMA) of PEEK shown in Figure 1, the glass transition temperature is the temperature where the viscosity starts decreasing in the graph, and the crystallization start temperature is the range up to the peak temperature where the viscosity starts decreasing in the graph. If the degree of crystallinity is high, there is no significant decrease in viscosity. Also, the decrease in viscosity from the glass transition temperature to the crystallization start temperature increases the faster the heating rate. It is necessary to heat the material to reach the desired heating temperature at a heating rate of 10°C / min or more. If the heating rate is slow, the proportion of recrystallization increases at a lower temperature, and the peak of viscosity decrease does not appear, making it difficult to transfer the mold surface by heat in this temperature range.

[0045] When a thermoplastic resin containing a conductive filler is heated, the viscosity of the matrix thermoplastic resin decreases, and the dispersion state of the conductive filler changes. Therefore, in the heating and pressurizing process in a state where the resin is heated to above the melting point, it is thought that slight temperature or pressure variations will cause large fluctuations and unevenness in the resistance value. In addition, when the resin is heated to a temperature far above the crystallization onset temperature, even if the temperature does not reach the melting point, the tubular tube shrinks significantly during cooling and the crystallization degree becomes too high, making it difficult to remove the resin from the mold after cooling.

[0046] In contrast, when a thermoplastic resin composition in an amorphous state containing a conductive filler is heated and pressurized in a temperature range from the glass transition temperature to the crystallization onset temperature, the viscosity increases due to the recrystallization of the thermoplastic resin, and therefore there is no excessive decrease in viscosity, and the dispersion state of the conductive filler is less affected.

[0047] 2-3. Method for evaluating the amount of carbon black contained in the base layer In this embodiment, the amount of carbon black contained in the intermediate transfer body can be evaluated by thermogravimetric analysis (TGA). In this embodiment, a thermogravimetric analyzer (TGA851e / SDTA) manufactured by Mettler Toledo Corporation was used. By heating at 600°C for 1 hour in a nitrogen gas atmosphere, the thermoplastic resin in the ITB is decomposed and removed, making it possible to evaluate the weight of only the contained carbon.

[0048] 2-4. Method for evaluating the primary particle size of carbon black contained in the base layer Observation of the carbon black contained in the resin composition is performed using a transmission electron microscope (TEM), but preparation of a thin specimen before observation is performed using a known method. For example, the specimen can be thinned using an ion beam, a diamond knife, or the like. In the following embodiment, the specimen is cut using Leica's "ULTRACUT-S" to obtain a cut specimen for observation with a thickness of about 40 nm, and a transmission electron microscope (TEM) is Hitachi's H-7100FA, and a TEM image is obtained under the measurement conditions of TE mode and an acceleration voltage of 100 kV. Known image analysis software can be used to analyze the obtained TEM image. For example, the product name: "WinROOF" manufactured by Mitani Shoji Co., Ltd. and the product name: "ImagePro" manufactured by Nippon Roper Co., Ltd. are representative examples of image analysis software. In this embodiment, the product name: "WinROOF" manufactured by Mitani Shoji Co., Ltd. was used. Then, the diameters of 50 primary particles of carbon black were measured, and the average value was taken as the average primary particle size.

[0049] 2-5. Method for evaluating dispersibility In the intermediate transfer body (conductive belt) to be measured, the dispersion state of the conductive filler was measured in a range of 10 μm in the thickness direction from the surface side carrying the toner image (referred to as the outer peripheral surface region). In addition, the dispersion state of the conductive filler was measured in a range of 10 μm in the thickness direction from the back side of the outer peripheral surface (referred to as the inner peripheral surface region). In addition, the dispersion state of the conductive filler was measured in a range of 5 μm from the center of the thickness direction center of the intermediate transfer body to the front side and the back side (hereinafter referred to as the central region). The measurement procedure was as follows.

[0050] First, the conductive belt is cut into strips of approximately 10 mm x 10 mm in the surface direction using a cutter knife or the like, and then embedded in epoxy resin. After hardening, cross-sectional samples are prepared using abrasive paper. SEM images are taken at a magnification of 20,000 times for the surface, back, and center of each cross-sectional sample obtained using a Philips XL-30 SFEG. If the contrast is unclear, appropriate black and white emphasis processing and smoothing processing are performed. For example, software such as Photoshop and ImageJ can be used for image processing.

[0051] Next, the coordinates of the center of gravity of the conductive filler in the field of view width are obtained, and the K function is calculated by the following formula.

[0052]

number

[0053] Here, d is the distance in the image, i and j are indices that indicate particles in the image, λ is the particle density in the image (the number of particles per unit area), and n is the number of particles in the image. ij is the ratio (area B / area A) of "area A of circle i with radius d centered on the coordinates of the center of gravity of particle i" to "area B of the part of circle i with radius d centered on the coordinates of the center of gravity of particle i that is included in the image." wi is used to correct underestimation due to the fact that particles do not exist outside the image when particle i exists near the image boundary. Id (i,j) is a function that takes the value 1 if the center of gravity of particle j is within a circle of radius d centered on the center of gravity of particle i, and takes the value 0 otherwise. (See Ripley BD, J. Appl. Prob, 13, 255 (1976)) Furthermore, the L function is calculated for the obtained K function using the following formula.

[0054]

number

[0055] And, as shown below, the simple sum of L(d) calculated every 10 nm from 0 nm to 500 nm is defined as the L function value in this case. L(0)=(K(0) / π) (1 / 2) L(10)=(K(10) / π) (1 / 2) -10 : L(490)=(K(490) / π) (1 / 2) -490 L(500)=(K(500) / π) (1 / 2) -500 L function value = L(0) + L(10) + + L(490) + L(500)

[0056] The range of d, 0 to 500 nm, used to calculate the L function indicates the radius of a circle centered on each particle in the image. If the image range of the SEM used for evaluation becomes too small relative to d=500 nm, which is the maximum radius of the measurement circle, the error will be large, so the SEM magnification during measurement is limited to 20,000 times. The size of the actual observation area included in the image taken under these conditions depends on the measurement means and the size of the area where "information other than the image part included in the image" is displayed, but the short side is approximately 3 to 4 μm and the long side is approximately 5 to 6 μm. "Information other than the image part included in the image" refers to information such as magnification and scale, and the part where this information is displayed is not included in the measurement target.

[0057] Furthermore, in each of the following examples, the L function value is calculated in each of the following regions (1) to (3). (1) A region whose center is 5 μm away from the toner image carrying surface (outer peripheral surface) in the thickness direction (2) A region whose center is 5 μm away from the back side (inner surface) of the outer peripheral surface of (1) in the thickness direction. (3) Region centered on the center in the thickness direction Table 1 shows the L function values ​​in each of the above regions (1) to (3).

[0058] 2-6.Method of measuring crystallinity Methods for measuring the crystallinity of a thermoplastic crystalline resin include differential scanning calorimetry (DSC), wide-angle X-ray diffraction, small-angle X-ray scattering, infrared absorption, density, etc. In this example, the crystallinity was calculated by a peak multiple separation method using a wide-angle X-ray diffraction method (X-ray diffractometer "Ultima IV" (product name) manufactured by Rigaku Corporation).

[0059] The scanning angle was 2θ = 5 to 45°, and the peaks near 2θ = 18.8° (= 110 plane), 20.95° (= 113 plane), 23.1° (= 200 plane), and 28.85° (= 213 plane) were analyzed as crystalline peaks of the thermoplastic resin PEEK.

[0060] 2-7.Measuring method for number of conductive points The current measurement function of a scanning electron microscope (E-sweep / Nano Navei; manufactured by SII Nano Technology) was used for the measurement. The back side of the sample was coated with AuPd and fixed to the sample stage with Ag tape. The cantilever was SI-DF3-R, the measurement area was 8 μm × 8 μm, and the number of data points in the X and Y directions was 256 points. The scanning frequency was 0.5 Hz, the initial DIF value was 0.55 to 0.65, and the cantilever deflection was -1. The I gain was fixed at 0.04, the P gain was fixed at 0.02, and the A gain was fixed at 0. The measurement environment was room temperature, and the pressure was reduced to 5E-3 Pa to remove adsorbed water before the measurement. The conductive point was the point where a current of -5 pA or more flows when the applied voltage was -40 V.

[0061] [Example 1] In this example, SB#285 (DBP oil absorption = 101 ml / 100 g, primary particle size = 26 nm) manufactured by Asahi Carbon Co., Ltd. was used as the conductive filler. Polyether ether ketone (PEEK, glass transition temperature 145°C, crystallization onset temperature 165°C, melting point 335°C) was used as the thermoplastic resin. A tubular tube was obtained using a single-screw extruder (Plastic Engineering Research Institute Co., Ltd.) equipped with a spiral cylindrical die at the tip. The produced tubular tube was then subjected to a heating and pressurizing process to produce an intermediate transfer belt. The blending amounts of each material, and the conditions of the molding process and the heating and pressurizing process are as follows. <Blend amount> Carbon black: SB#285 28 parts by weight Resin material: PEEK (Victrex, 450G) 72 parts by weight <Conditions for molding process> Output: 6kg / h Die temperature: 380℃ External heating device temperature: 300℃ Cooling mandrel temperature: 140℃ <Conditions for the heating and pressurizing process> Heating temperature: 160℃ The measurement results for the characteristics of the intermediate transfer member thus prepared are shown in Table 1.

[0062] [Comparative Example 1] In this comparative example, the intermediate transfer member was produced in the same manner as in Example 1, except that the blending amounts of carbon black and PEEK resin used as the conductive filler were changed. The conductive filler and resin materials used in Comparative Example 1 are as follows. <Blend amount> Carbon black: SB#285 35 parts by weight Resin material: PEEK (Victrex, 450G) 65 parts by weight The results of measurements of the prepared intermediate transfer member are shown in Table 1.

[0063] [Comparative Example 2] In this comparative example, an intermediate transfer member was produced in the same manner as in Example 1, except that Tokai Carbon Co., Ltd.'s Toka Black #7270SB (DBP oil absorption amount = 37 to 79 ml / 100 g, primary particle size = 36 nm) was used as the conductive filler. The conductive filler and resin material used in Comparative Example 2 are as follows.

[0064] <Blend amount> Carbon black: #7270SB 28 parts by weight Resin material: PEEK (Victrex, 450G) 72 parts by weight The measurement results of the intermediate transfer member thus prepared are as shown in Table 1. [Comparative Example 3] In this comparative example, an intermediate transfer member was produced in the same manner as in Example 1, except that the die temperature in the molding step was changed to 450°C.

[0065] The results of measurements of the prepared intermediate transfer member are shown in Table 1.

[0066] [Comparative Example 4] In this comparative example, the production was carried out in the same manner as in Example 1, except that the temperature of the cooling mandrel in the molding process was changed to 60°C. However, the thickness unevenness of the tubular body was significantly large, and an intermediate transfer body could not be obtained.

[0067] [Comparative Example 5] In this comparative example, an intermediate transfer member was produced in the same manner as in Example 1, except that the temperature of the cooling mandrel in the molding step was changed to 170°C.

[0068] The results of measurements of the prepared intermediate transfer member are shown in Table 1.

[0069] [Comparative Example 6] In this comparative example, an intermediate transfer member was produced in the same manner as in Example 1, except that the temperature of the cooling mandrel in the molding process was changed to 230°C.

[0070] The results of measurements of the prepared intermediate transfer member are shown in Table 1.

[0071] [Comparative Example 7] In this comparative example, an intermediate transfer member was produced in the same manner as in Example 1, except that the die temperature in the molding step was changed to 400°C and the cooling mandrel temperature was changed to 180°C.

[0072] The results of measurements of the prepared intermediate transfer member are shown in Table 1.

[0073] [Comparative Example 8] In this comparative example, an intermediate transfer member was produced in the same manner as in Example 1, except that the temperature of the external heating device in the molding process was changed to 250°C.

[0074] The results of measurements of the prepared intermediate transfer member are shown in Table 1.

[0075] [Comparative Example 9] In this comparative example, the production was carried out in the same manner as in Example 1, except that the temperature of the external heating device in the molding process was changed to 380°C. However, the thickness unevenness of the tubular body was significantly large, and an intermediate transfer body could not be obtained.

[0076] [Comparative Example 10] In this comparative example, an intermediate transfer member was prepared in the same manner as in Example 1, except that the heating temperature in the heating and pressurizing step was changed to 100°C.

[0077] The results of measurements of the prepared intermediate transfer member are shown in Table 1.

[0078] [Comparative Example 11] In this comparative example, the preparation was carried out in the same manner as in Example 1, except that the heating temperature in the heating and pressing step was changed to 270°C, but the tubular body broke during cooling in the heating and pressing step, and an intermediate transfer body could not be obtained. Under the conditions of Comparative Example 11, the crystallinity was 27%, and the mechanical strength of the belt body was insufficient.

[0079] In the heating and pressurizing step, if heating is continued beyond the end point of crystallization or if the heating time is prolonged, crystallization will progress. The progress of crystallization may promote aggregation of carbon black, which may deteriorate dispersibility. Therefore, it is necessary to set the heating and pressurizing conditions so that the crystallinity achieved in the heating and pressurizing step is preferably 25% or less, more preferably 20% or less.

[0080] [Verification of each embodiment] Using the image forming apparatus shown in Figure 1, a durability test was conducted in which A3-size plain paper (CS068, Canon) was continuously fed in a low humidity environment (23°C / 5%) up to 600k sheets. Every time 10k sheets were fed, 5 sheets of image X, which was printed entirely in halftone only by the image forming unit PK, were output in succession. The images obtained in this way were evaluated for blank images according to the following criteria.

[0081] Whiteout A: Regarding image X, no blank images are found in any of the five sheets. B: For image X, a blank image is confirmed in one of the five images. C: For image X, blank images are observed in any 3 out of 5 images.

[0082] Mechanical properties A: There is no break in the belt, and no distortion or color shift of the toner image is observed. B: The belt is not broken, but distortion or color shift of the toner image is observed. C: Belt breakage occurs.

[0083] (Image and mechanical strength evaluation results) The evaluation results of the produced intermediate transfer belts are shown in Table 2. For those in which blank images were confirmed in Image X, it is believed that the particle size of the carbon black used was large and that the dispersibility of the conductive agent in the intermediate transfer body was deteriorated due to re-aggregation during the molding process. In this case, it is believed that the blank images were generated by discharge occurring in the gap between the inner circumferential surface of the intermediate transfer body and the primary transfer roller in the primary transfer section, or between the outer circumferential surface of the intermediate transfer body and the paper in the secondary transfer section.

[0084] In addition, in cases where belt breakage or color shift was confirmed during testing, this was believed to be due to the intermediate transfer belt having a low degree of crystallinity, which made it impossible to impart the desired tensile strength, bending durability, and surface hardness.

[0085] In Example 1, both the blank image and the mechanical strength were good.

[0086] [Table 1]

[0087] [Table 2] [Explanation of symbols]

[0088] 1 Photosensitive drum 2 Primary charging device 3. Exposure equipment 4. Developing device 5 Primary transfer roller 7 Intermediate transfer belt 8 Secondary transfer outer roller 9 Fixing device 12 Cassettes 13 Pickup roller 15 Resist roller 71 Intermediate transfer belt tension roller (drive roller) 72 Intermediate transfer belt tension roller (tension roller) 73 Intermediate transfer belt tension roller (secondary transfer inner roller) 10 Base layer 11 Surface layer

Claims

[Claim 1] An image forming apparatus including: an image carrier that carries a toner image; an intermediate transfer belt onto which the toner image formed on the image carrier is primarily transferred; a metal roller that primarily transfers the toner image from the image carrier to the intermediate transfer belt; and a secondary transfer member that secondarily transfers the toner image from the intermediate transfer belt to a recording material, the intermediate transfer belt is made of a thermoplastic resin having carbon black dispersed therein, the thermoplastic resin having a degree of crystallinity of 8% or more and 25% or less, the carbon black having an average primary particle size of 10 nm or more and 30 nm or less, and a content of the carbon black of 15.0 parts by mass or more and 30.0 parts by mass or less per 100 parts by mass of the intermediate transfer belt; When an outer peripheral surface region is a region extending from an outer peripheral surface on which a toner image is carried to 10 μm in the thickness direction, an inner peripheral surface region is a region extending from an inner peripheral surface on the back side of the outer peripheral surface to 10 μm in the thickness direction, and a central region is a region extending from a center in the thickness direction to 5 μm in each direction, and values ​​of an L function indicating the dispersibility of the carbon black in the thermoplastic resin in the inner peripheral surface region, the outer peripheral surface region, and the central region are Li, Lo, and Lc, respectively, 1. An image forming apparatus, comprising: (Li+Lo+Lc) / 3≦100 nm; and Li≦150 nm.

Citation Information

Patent Citations

  • Semi-conductive film, charge control member, and method for producing semi-conductive film

    JP2005112942A

  • Electrophotographic belt and method of manufacturing the same

    JP2010082906A

  • Method for evaluating temporal stability of electric resistance of electrophotographic belt

    JP2012177811A

  • Extrusion-molded tubular body, tubular body unit, intermediate transfer body, recording medium conveyance body, and image forming apparatus

    JP2016045218A