Manufacturing method of electrolyte molded body and electrolyte molded body

The method addresses the handling and storage issues of sulfonylimide compounds in lithium ion batteries by forming sheet-like or tablet-shaped electrolyte molded bodies through compression and pulverization, ensuring easy handling and discharge while preserving electrolyte quality.

JP7581479B2Active Publication Date: 2024-11-12NIPPON SHOKUBAI CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023503841
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-01
Filing Date
2022-02-28
Publication Date
2024-11-12
Estimated Expiration
2042-02-28

AI Technical Summary

Technical Problem

Sulfonylimide compounds used in lithium ion secondary batteries are prone to blocking during storage or transportation due to their crystalline nature, and existing granulation methods can denature the electrolyte and result in small particle sizes that are difficult to handle.

Method used

A manufacturing method involving compression and pulverization processes to produce sheet-like or strip-like electrolyte molded bodies, or tablet-shaped electrolyte molded bodies, which reduces specific surface area and prevents excessive heating, allowing easy handling and discharge from containers.

Benefits of technology

The method produces electrolyte molded bodies that are easy to handle, reduce aggregate formation, and can be easily discharged from containers, maintaining electrolyte integrity and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581479000001
    Figure 0007581479000001
Patent Text Reader

Abstract

A method for producing a compact of an electrolyte containing a sulfonylimide compound represented by general formula (1) includes: a compression step for compressing and granulating the powdery electrolyte to obtain a sheet-shaped or strip-shaped electrolyte; and either a pulverization step for pulverizing the sheet-shaped or strip-shaped electrolyte to obtain a granular electrolyte compact or a tableting step for tableting the powdery electrolyte to obtain a tablet-shaped electrolyte compact. (1): LiN(R1SO2) (R2SO2) (R1 and R2 are the same or different and represent a fluorine atom and an alkyl group having 1-6 carbon atoms or a fluoroalkyl group having 1-6 carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing an electrolyte formed body and an electrolyte formed body. [Background technology]

[0002] Sulfonylimide compounds such as lithium bis(fluorosulfonyl)imide, which are used as electrolytes for lithium ion secondary batteries, are usually crystallized and dried, and the resulting powder is then packaged and shipped as is. The powdered sulfonylimide compounds have a problem in that they block during storage or transportation, and it takes a long time to discharge them from the container in the subsequent electrolyte solution preparation process.

[0003] For example, Patent Document 1 proposes a method for granulating an electrolyte for a lithium battery, which includes step 1 of feeding an electrolyte from a hopper into an extrusion granulator and extruding particulate matter, step 2 of vibration screening the electrolyte with a filter screen to screen out electrolytes with particle sizes larger than the screen openings, and step 3 of transporting the screened electrolyte into a stirring drum by a conveyer belt, stirring and mixing again, extruding the particles into granules, and then packaging and storing the electrolyte. In this granulation method, a granulation hole size in the extrusion granulator is in the range of 0.5-5 mm. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-184527 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the method of Patent Document 1, the electrolyte is put into an extrusion granulator to extrude particulate matter, and the screened electrolyte is stirred and mixed again to extrude and granulate particles, so that the electrolyte is subjected to more heat than necessary, which may cause the electrolyte to denature. In addition, the particle size of the granulated electrolyte is relatively small, so it is prone to scattering and difficult to handle.

[0006] The present disclosure has been made in consideration of the above points, and an object of the present disclosure is to provide a method for producing a molded body for an electrolyte containing a sulfonylimide compound, which is less likely to affect the electrolyte, is easy to handle, and can be easily discharged from a container, and to provide such an electrolyte molded body. [Means for solving the problem]

[0007] As a result of further investigations, the inventors of the present application have found that, in an electrolyte containing a sulfonylimide compound, by forming the electrolyte through a specific process, the specific surface area can be reduced, the formation of agglomerates during storage can be suppressed, and the electrolyte formed body can be easily removed from the container.

[0008] Specifically, the present disclosure is as follows. A method for producing an electrolyte formed body according to the present disclosure comprises the steps of: LiN(R 1 SO2)(R 2 SO2) (R 1 and R 2are the same or different and represent a fluorine atom, an alkyl group having 1 to 6 carbon atoms, or a fluoroalkyl group having 1 to 6 carbon atoms.) A method for producing an electrolyte molded body containing a sulfonylimide compound represented by (1), comprising a compression step of compressing and granulating the powdered electrolyte to obtain a sheet-like or rectangular electrolyte, and a pulverization step of pulverizing the sheet-like or rectangular electrolyte to obtain a granular electrolyte molded body. In the compression step, the powdered electrolyte may be passed between a pair of pressure rolls to compress and granulate the electrolyte, thereby obtaining a sheet-like or rectangular electrolyte having a longitudinal length of 10 mm to 100 mm. A roller compactor may be used in the compression step. A roll granulator may be used in the pulverization step. The particle size of the granular electrolyte molded body may be 1 mm to 10 mm. The electrolyte molded body may contain the powdered electrolyte.

[0009] The method for producing an electrolyte molded body of the present disclosure is a method for producing an electrolyte molded body containing a sulfonylimide compound represented by the general formula (1), and includes a tableting step of tableting the powdered electrolyte to obtain a tablet-shaped electrolyte molded body. The method may further include a drying step of drying the tablet-shaped electrolyte molded body. The method may further include a wetting step of wetting the powdered electrolyte or the tablet-shaped electrolyte molded body. A rotary tablet press may be used in the tableting step. The particle size of the tablet-shaped electrolyte molded body may be 5 mm or more and 25 mm or less. The electrolyte molded body may contain the powdered electrolyte.

[0010] The sulfonylimide compound represented by the general formula (1) may contain at least one of LiN(FSO2)2 and LiN(CF3SO2)2.

[0011] The electrolyte is represented by the general formula (2): LiPF a (C m F 2m+1 ) 6-a (a: 0≦a≦6, m: 1≦m≦4) (2), a compound represented by the general formula (3): LiBF b (Cn F 2n+1 ) 4-b (b:0≦b≦4, n:1≦n≦4) (3) and LiAsF6.

[0012] The electrolyte molded body of the present disclosure is a molded body of an electrolyte containing the sulfonylimide compound represented by the general formula (1), in which the ratio of the powdered electrolyte having an average particle diameter of 1300 μm or less in 100 parts by mass of the molded body is 10 parts by mass or less, and the molded body has a hardness of 10 N or more and 50 N or less. The particle diameter of the molded body may be 5 mm or more and 25 mm or less. Effect of the Invention

[0013] According to the present disclosure, it is possible to provide a method for producing a molded body for an electrolyte containing a sulfonylimide compound, which is unlikely to affect the electrolyte, is easy to handle, and can be easily discharged from a container, and to provide such an electrolyte molded body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiments of the present disclosure will be described in detail. The following description of the preferred embodiments is merely illustrative in nature and is not intended to limit the present disclosure, its application, or its uses.

[0015] (electrolyte) The electrolyte molded body obtained by the manufacturing method according to the present embodiment contains an electrolyte having the general formula (1): LiN(R 1 SO2)(R 2 SO2) (1) The sulfonylimide compound (hereinafter referred to as "sulfonylimide compound (1)" and a fluorine-containing sulfonylimide salt) is represented by the following formula:

[0016] In general formula (1), R 1 and R 2are the same or different (independently of each other) and represent a fluorine atom, an alkyl group having 1 to 6 carbon atoms, or a fluoroalkyl group having 1 to 6 carbon atoms.

[0017] Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a pentyl group, and a hexyl group. Among the alkyl groups having 1 to 6 carbon atoms, a linear or branched alkyl group having 1 to 6 carbon atoms is preferred, and a linear alkyl group having 1 to 6 carbon atoms is more preferred.

[0018] Examples of the fluoroalkyl group having 1 to 6 carbon atoms include an alkyl group having 1 to 6 carbon atoms in which some or all of the hydrogen atoms have been substituted with fluorine atoms. Examples of the fluoroalkyl group having 1 to 6 carbon atoms include a fluoromethyl group, a difluoromethyl group, a trifluoromethyl group, a fluoroethyl group, a difluoroethyl group, a trifluoroethyl group, and a pentafluoroethyl group. In particular, the fluoroalkyl group may be a perfluoroalkyl group.

[0019] Substituent R 1 and R 2 As the substituent R, a fluorine atom and a perfluoroalkyl group (for example, a perfluoroalkyl group having 1 to 6 carbon atoms, such as a trifluoromethyl group, a pentafluoroethyl group, a heptafluoropropyl group, etc.) are preferable, a fluorine atom, a trifluoromethyl group, and a pentafluoroethyl group are more preferable, a fluorine atom and a trifluoromethyl group are even more preferable, and a fluorine atom is even more preferable. 1 and R 2 may be the same or different from each other.

[0020] Examples of the sulfonylimide compound (1) include lithium bis(fluorosulfonyl)imide (LiN(FSO2)2, hereinafter also referred to as "LiFSI"), lithium bis(trifluoromethylsulfonyl)imide (LiN(CF3SO2)2, hereinafter also referred to as "LiTFSI"), lithium (fluorosulfonyl)(methylsulfonyl)imide, lithium (fluorosulfonyl)(ethylsulfonyl)imide, lithium (fluorosulfonyl)(trifluoromethylsulfonyl)imide, lithium (fluorosulfonyl)(pentafluoroethylsulfonyl)imide, lithium (fluorosulfonyl)(heptafluoropropylsulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, lithium bis(heptafluoropropylsulfonyl)imide, etc. The sulfonylimide compounds (1) may be used alone or in combination of two or more kinds.

[0021] Among the sulfonylimide compounds (1), from the viewpoint of improving battery performance, LiN(FSO2)2 and LiN(CF3SO2)2 are preferred, and LiN(FSO2)2 is more preferred. In other words, among the electrolyte molded bodies, the sulfonylimide compound (1) is preferably one containing at least one of LiN(FSO2)2 and LiN(CF3SO2)2, and more preferably one containing LiN(FSO2)2.

[0022] The sulfonylimide compound (1) may be a commercially available product or may be synthesized by a conventionally known method. The method for synthesizing the sulfonylimide compound (1) is not particularly limited, and any conventionally known method may be used. For example, methods described in WO 2011 / 149095, JP 2014-201453 A, JP 2010-168249 A, JP 2010-168308 A, JP 2010-189372 A, WO 2011 / 065502 A, JP-T-8-511274 A, WO 2012 / 108284 A, WO 2012 / 117961 A, WO 2012 / 118063 A, JP 2010-280586 A, JP 2010-254543 A, JP 2007-182410 A, WO 2010 / 010613 A, etc. can be mentioned. By the above-mentioned conventionally known method, a powder (solid) of the sulfonylimide compound (1) can be obtained.

[0023] The sulfonylimide compound (1) may contain a production solvent used in the production of the sulfonylimide compound (1) (a residual solvent contained in the sulfonylimide compound (1) obtained by the above-mentioned conventionally known production method) within the scope of not impairing the object of the present invention. The residual solvent is a solvent used in the production reaction of the sulfonylimide compound (1) or a solvent used in the purification step. For example, water; alcohol-based solvents such as methanol, ethanol, propanol, and butanol; carboxylic acid-based solvents such as formic acid and acetic acid; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone; nitrile-based solvents such as isobutyronitrile, acetonitrile, valeronitrile, and benzonitrile; ester-based solvents such as ethyl acetate, isopropyl acetate, and butyl acetate; aliphatic ether-based solvents such as diethyl ether, diisopropyl ether, t-butyl methyl ether, and cyclopentyl methyl ether; halogen-based solvents such as HF; nitro group-containing solvents such as nitromethane and nitrobenzene; nitrogen-containing organic solvents such as ethylformamide and N-methylpyrrolidone; dimethyl sulfoxide; glyme-based solvents, toluene, o-xylene, m-xylene, p-xylene, benzene, ethylbenzene, isopropylbenzene, 1,2,3 aromatic hydrocarbon solvents such as 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, tetralin, cymene, methylethylbenzene, 2-ethyltoluene, chlorobenzene, and dichlorobenzene; pentane, hexane, heptane, octane, decane, dodecane, undecane, tridecane, decalin, 2,2,4,6,6-pentamethylheptane, isoparaffin (e.g., "Marukasol R" (a mixture of 2,2,4,6,6-pentamethylheptane and 2,2,4,4,6-pentamethylheptane manufactured by Maruzen Petrochemical Co., Ltd.), "Isopar (registered trademark) G" (a C9-C11 mixed isoparaffin manufactured by ExxonMobil), and "Isopar (registered trademark) E" (a C8-C10 mixed isoparaffin manufactured by ExxonMobil), dichloromethane, chloroform, 1,2-dichloroethane, and other chain aliphatic hydrocarbon solvents;Cycloaliphatic hydrocarbon solvents such as cyclohexane, methylcyclohexane, 1,2-dimethylcyclohexane, 1,3-dimethylcyclohexane, 1,4-dimethylcyclohexane, ethylcyclohexane, 1,2,4-trimethylcyclohexane, 1,3,5-trimethylcyclohexane, propylcyclohexane, butylcyclohexane, and "Swaclean 150" (a mixture of C9 alkylcyclohexanes manufactured by Maruzen Petrochemical Co., Ltd.); aromatic ether solvents such as anisole, 2-methylanisole, 3-methylanisole, and 4-methylanisole; ethylene carbonate, propylene carbonate, etc. Examples of the solvent include carbonate-based solvents such as butylene carbonate, dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate; chain ether-based solvents such as dimethoxymethane and 1,2-dimethoxyethane; cyclic ether-based solvents such as tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxane, and 4-methyl-1,3-dioxolane; cyclic ester-based solvents such as γ-butyrolactone and γ-valerolactone; sulfolane-based solvents such as sulfolane and 3-methylsulfolane; N,N-dimethylformamide, dimethyl sulfoxide, and N-methyloxazolidinone.

[0024] The electrolyte may contain the sulfonylimide compound (1), but may also contain other electrolytes (electrolytes other than the sulfonylimide compound (1)). Examples of other electrolytes include imide salts and non-imide salts.

[0025] Examples of the imide salt include other fluorine-containing sulfonylimide salts (hereinafter referred to as "other sulfonylimide compounds") different from the sulfonylimide compound (1). Examples of the other sulfonylimide compounds include non-lithium salts of the fluorine-containing sulfonylimides listed as the sulfonylimide compound (1) (for example, salts in which lithium (ion) in the sulfonylimide compound (1) is replaced with a cation other than lithium ion). Examples of salts in which a cation other than lithium ion is replaced include alkali metal salts such as sodium salts, potassium salts, rubidium salts, and cesium salts; alkaline earth metal salts such as beryllium salts, magnesium salts, calcium salts, strontium salts, and barium salts; aluminum salts; ammonium salts; and phosphonium salts. The other sulfonylimide compounds may be used alone or in combination of two or more kinds. In addition, the other sulfonylimide compounds may be commercially available products, or may be obtained by synthesis using a conventional method.

[0026] Examples of the non-imide salt include salts of non-imide anions and cations (lithium ions and the above-listed cations). [Case 2] LiPF a (C m F 2m+1 ) 6-a (a: 0≦a≦6, m: 1≦m≦4) (2) (hereinafter referred to as "fluorophosphate compound (2)"), [C3] LiBF b (C n F 2n+1 ) 4-b(b: 0≦b≦4, n: 1≦n≦4) Examples of the non-imide salt include a compound represented by formula (3) (hereinafter referred to as "fluoroborate compound (3)"), lithium salts such as lithium hexafluoroarsenate (LiAsF6), LiSbF6, LiClO4, LiSCN, LiAlF4, CF3SO3Li, LiC[(CF3SO2)3], LiN(NO2), and LiN[(CN)2; and non-lithium salts (for example, salts in which the lithium (ion) in these lithium salts is replaced with the above-mentioned cations (for example, NaBF4, NaPF6, NaPF3(CF3)3, etc.). The non-imide salts may be used alone or in combination of two or more kinds. In addition, the non-imide salts may be commercially available products, or may be obtained by synthesis using a conventional method.

[0027] <Method of manufacturing electrolyte molded body> The method for producing an electrolyte molded product according to this embodiment uses a powdered electrolyte as a starting material. In other words, the starting material is a powder (solid) of an electrolyte containing the sulfonylimide compound (1), and may be a powder of an electrolyte containing only the sulfonylimide compound (1) (i.e., a powdered sulfonylimide compound (1)).

[0028] <Method of manufacturing granular electrolyte molded body> The method for producing an electrolyte molded body according to this embodiment is characterized in that it includes a compression step and a pulverization step (hereinafter also referred to as a "method for producing granular electrolyte molded body").

[0029] (Compression process) The compression process is a process of compressing and granulating the powdered electrolyte. As a method of compressing and granulating the powdered electrolyte, for example, the powdered electrolyte is extruded and passed between a pair of pressure rolls to be consolidated (compression granulated). In this way, the compression process employs compression granulation rather than extrusion granulation, which may cause the electrolyte to be overheated. In this compression process, the powdered electrolyte is compressed and granulated to produce a sheet-shaped or strip-shaped electrolyte, rather than extrusion granulating the powdered electrolyte to produce a particulate substance. The sheet-shaped or strip-shaped electrolyte is obtained in a single compression process, which prevents the electrolyte from being heated more than necessary.

[0030] In the compression step, a roller compactor (compression granulator) can be suitably used. The roller compactor is not particularly limited, and a general commercially available product can be used.

[0031] In the compression step, the pressure (roll pressure) for compressing and granulating the powdered electrolyte is not particularly limited and may be appropriately adjusted depending on the type of electrolyte (salt composition), the amount of residual solvent, the hardness and size of the molded body, etc., but is preferably 3 MPa or more, more preferably 5 MPa or more, and even more preferably 10 MPa or more. In addition, the upper limit is preferably 50 MPa or less, more preferably 40 MPa or less, and even more preferably 30 MPa or less, from the viewpoint of preventing the electrolyte from being heated more than necessary.

[0032] The temperature at which the compression step is carried out is not particularly limited, and is, for example, room temperature (about 25° C.).

[0033] When a roller compactor is used in the compression step, the roll gap is not particularly limited, but is preferably 0.1 mm or more, more preferably 0.3 mm or more, and the upper limit is preferably 10 mm or less, more preferably 0.7 mm or less.

[0034] The compression step produces a sheet or strip-shaped electrolyte. The size of the sheet or strip-shaped electrolyte is not particularly limited, and the longitudinal length is preferably 10 mm to 100 mm, more preferably 10 mm to 80 mm, even more preferably 10 mm to 70 mm, and even more preferably 10 mm to 60 mm. The transverse length is preferably 5 mm to 50 mm, more preferably 5 mm to 30 mm, and even more preferably 5 mm to 20 mm. The thickness is preferably 0.1 mm to 5 mm, and more preferably 0.1 mm to 3 mm.

[0035] (Crushing process) The pulverization step is a step of pulverizing the sheet-like or rectangular electrolyte obtained in the compression step, to obtain a granular electrolyte compact.

[0036] In the pulverization step, a vibration mill, a roll granulator, a knuckle type pulverizer, a roll mill, a high-speed rotary pulverizer (pin mill, hammer mill, screw mill), a cylindrical mixer, etc. can be used. Among these, from the viewpoint of controlling the particle size of the electrolyte molded body, a roll granulator is preferred, and a roll granulator with a screen is more preferred. The roll granulator is not particularly limited, and a general commercially available product can be used.

[0037] The temperature at which the grinding step is carried out is not particularly limited, and is, for example, room temperature (about 25° C.).

[0038] In the pulverization step, when a roll granulator or a roll granulator with a screen is used, the groove pitch is not particularly limited, but is preferably 1 mm to 25 mm, more preferably 1 mm to 10 mm, and even more preferably 5 mm to 8 mm. In addition, when a roll granulator with a screen is used, the screen diameter is not particularly limited, but is preferably 1 mm to 25 mm, more preferably 1 mm to 10 mm, and even more preferably 5 mm to 8 mm.

[0039] (Other processes) The method for producing the granular electrolyte molded body may further include a classification step, if necessary. The classification step is a step of separating the granular electrolyte molded body from the powdered electrolyte that could not be formed into a molded body. The classification operation is not particularly limited, and may be, for example, sieving using a sieve.

[0040] According to the method for producing a granular electrolyte molded product including the above-mentioned compression step, pulverization step, and other steps as necessary, the particle size of the obtained granular electrolyte molded product is preferably 2 mm or more, more preferably 5 mm or more, and even more preferably more than 5 mm. The upper limit is preferably 10 mm or less, more preferably 8 mm or less. The particle size can be measured, for example, with a vernier caliper.

[0041] The granular electrolyte molded body may contain a powdered electrolyte. The average particle size of the powdered electrolyte is not particularly limited, but is, for example, 1300 μm (1.3 mm) or less, preferably 1000 μm (1 mm) or less, more preferably 700 μm or less, in order to distinguish it from the granular electrolyte molded body. In this specification, the average particle size means the 50% mass average particle size based on JIS Z 8801-1. The 50% mass average particle size is calculated, for example, by the method described in the Examples below.

[0042] <Effects> According to the manufacturing method of the granular electrolyte molded body of the present disclosure, the following effects can be obtained: A powdered electrolyte containing a sulfonylimide compound is molded into a granular electrolyte by a compression step and a pulverization step. In the compression step, the powdered electrolyte is compressed and granulated, so that the sheet-like or strip-like electrolyte obtained is prevented from being subjected to heat more than necessary, and the electrolyte is less likely to be affected. In addition, the granular electrolyte molded body is obtained through the compression step and the pulverization step without adding components such as a binder to the electrolyte, so that the electrolyte is also less likely to be affected in this respect. Furthermore, in the pulverization process, the sheet- or strip-shaped electrolyte is pulverized to obtain a granular electrolyte molded product having a predetermined particle size (e.g., 2 mm to 10 mm), which is less likely to scatter and is easier to handle (improved handling properties). Furthermore, the granular electrolyte compact has a small specific surface area, which suppresses the formation of agglomerates (blocking) during storage or transportation, making it easy to remove from the container (removal from the container does not take much time). As described above, in an electrolyte containing a sulfonylimide compound, a granular molded product can be produced which does not affect the electrolyte, is easy to handle, and can be easily discharged from a container.

[0043] <Method of manufacturing tablet-shaped electrolyte molded body> Furthermore, as a method for manufacturing an electrolyte molded body according to this embodiment, which is different from the above-mentioned method for manufacturing a granular electrolyte molded body, is characterized in that it includes a tableting process (hereinafter also referred to as a "method for manufacturing a tablet-shaped electrolyte molded body").

[0044] (tableting process) The tableting process is a process of tableting a powdered electrolyte. In this specification, tableting refers to compressing a powdered electrolyte to make it possible to retain a predetermined shape (for example, a tablet shape). Specifically, the tableting process is a process of compression molding a powdered electrolyte using upper and lower dies. In this way, in the tableting process, compression molding is adopted instead of extrusion granulation (extrusion molding) in which the electrolyte may be excessively heated. In this tableting process, the powdered electrolyte is compressed to produce a tablet-shaped electrolyte molded body, rather than extrusion granulating the powdered electrolyte to produce a particulate substance. The tablet-shaped electrolyte molded body is obtained only by the tableting process, so that the electrolyte is prevented from being heated more than necessary.

[0045] In the tableting step, a tablet press, preferably a rotary tablet press, etc., can be used. The rotary tablet press is not particularly limited, and a general commercially available product can be used.

[0046] In the tableting step, the pressure (tabletting pressure) for compressing the powdered electrolyte may be appropriately adjusted depending on the type of electrolyte (salt composition), the amount of residual solvent, the hardness and size of the compact, etc., and is not particularly limited as long as it is equal to or higher than the minimum pressure required to maintain the shape of the tablet, but is preferably 3 kN or more, more preferably 5 kN or more, and even more preferably 10 kN or more. In addition, the upper limit is preferably 150 kN or less, more preferably 100 kN or less, and even more preferably 50 kN or less, from the viewpoint of preventing the electrolyte from being heated more than necessary.

[0047] The temperature at which the tableting step is carried out is not particularly limited, and is, for example, room temperature (about 25° C.).

[0048] When a tablet press or rotary tablet press is used in the tableting step, the punch tip diameter is not particularly limited, but is preferably 1 mm or more and 25 mm or less, more preferably 5 mm or more and 15 mm or less, and even more preferably 5 mm or more and 10 mm or less.

[0049] (Other processes) The method for producing a tablet-shaped electrolyte molded product may further include at least one of a classification step, a drying step, and a wetting step, as necessary.

[0050] The classification step is a step of separating tablet-shaped electrolyte molded bodies from powder-shaped electrolyte that could not be molded into bodies. The classification operation is not particularly limited, and examples thereof include sieving using a sieve.

[0051] The drying step is a step of drying the tablet-shaped electrolyte molded body. The drying method is not particularly limited, and examples thereof include a method of heating the tablet-shaped electrolyte molded body to a temperature at which the residual solvent in the tablet-shaped electrolyte molded body can evaporate. The drying step may be performed under reduced pressure, in an inert gas atmosphere such as nitrogen, or in an inert gas flow.

[0052] The wetting step is a step of wetting a powdered electrolyte with a solvent or the like, or wetting a tablet-shaped electrolyte molded body with a solvent or the like. That is, the wetting step may be a step before the tableting step or a step after the tableting step. The wetting method is not particularly limited, and examples thereof include a method of adding the above-mentioned solvent to a powdered electrolyte or a tablet-shaped electrolyte molded body.

[0053] According to the manufacturing method of tablet-shaped electrolyte molded products including the above tableting step and other steps as necessary, the particle size of the obtained tablet-shaped electrolyte molded products is preferably 5 mm or more, more preferably more than 5 mm. The upper limit is preferably 25 mm or less, more preferably 15 mm or less, and even more preferably 10 mm or less. The particle size can be measured, for example, with a vernier caliper.

[0054] The tablet-shaped electrolyte molded body may contain a powdered electrolyte. The average particle size of the powdered electrolyte is not particularly limited, but is, for example, 1300 μm (1.3 mm) or less, preferably 1000 μm (1 mm) or less, more preferably 700 μm or less, in order to distinguish it from the tablet-shaped electrolyte molded body. In this specification, the average particle size means the 50% mass average particle size based on JIS Z 8801-1. The 50% mass average particle size is calculated, for example, by the method described in the Examples below.

[0055] The content (ratio) of powdered electrolyte (fine powder having an average particle size equal to or less than the above upper limit) in 100 parts by mass (100% by mass) of the tablet-shaped electrolyte molded body is 10 parts by mass (10% by mass) or less, and preferably 5 parts by mass (5% by mass) or less, from the viewpoint of improving handleability. In other words, the tablet-shaped electrolyte molded body has a small amount of fine powder.

[0056] The hardness (particle hardness) of the tablet-shaped electrolyte molded body is 10N or more and 50N or less. When the hardness of the electrolyte molded body is equal to or more than the above lower limit, it is possible to maintain the shape during transportation (improved handling) compared to extrusion granulation (extrusion molding). In addition, when the hardness is equal to or less than the above upper limit, the inconvenience of poor economic efficiency due to the high processing speed required for dissolving in the electrolyte is suppressed. From the above viewpoint, the lower limit of the hardness is preferably 20N or more, and the upper limit is preferably 40N or less, more preferably 30N or less.

[0057] The increase rate of the SUS components contained in the tablet-shaped electrolyte molded body (tablet after molding) relative to the stainless steel (SUS) components (the sum of Fe, Ni, Cr, etc., the same applies below) contained in the powdered electrolyte (powder before molding) is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and most preferably below the lower limit of measurement (ND, about 0% by mass). The SUS components contained in the tablet-shaped electrolyte molded body are preferably 5 ppm by mass or less. Note that the above-mentioned manufacturing method for granular electrolyte molded body and manufacturing method for tablet-shaped electrolyte molded body are molded using metal (mainly stainless steel (SUS)) equipment, but can minimize the inclusion (increase) of SUS components (Fe, Ni, Cr, etc.) in the electrolyte molded body. Among them, the manufacturing method for tablet-shaped electrolyte molded body, which includes a tableting process and passes through a metal device only once, is considered to be able to further reduce the inclusion (increase) of SUS components in the electrolyte molded body in terms of the number of times passing through a metal device in the manufacturing process, compared to the manufacturing method for granular electrolyte molded body, which includes a compression process and a pulverization process and passes through a metal device multiple times.

[0058] <Effects> According to the manufacturing method of tablet-shaped electrolyte molded body of the present disclosure, the following effects can be obtained: A powdered electrolyte containing a sulfonylimide compound is molded into a tablet-shaped electrolyte by a tableting process. In the tableting process, the powdered electrolyte is compressed and molded, so that the application of more heat than necessary to the obtained tablet-shaped electrolyte molded body is suppressed, and the electrolyte is less likely to be affected. In addition, the tablet-shaped electrolyte molded body is obtained through the tableting process without adding components such as a binder to the electrolyte, so that the electrolyte is also less likely to be affected in this respect. Furthermore, tablet-shaped electrolyte molded bodies having a predetermined particle size (for example, 5 mm to 25 mm) are less likely to scatter and are easier to handle (improved handling). Furthermore, tablet-shaped electrolyte molded bodies have a small specific surface area, which suppresses the formation of agglomerates (blocking) during storage or transportation, making them easier to remove from containers (removal from containers does not take much time). As described above, for an electrolyte containing a sulfonylimide compound, a tablet-shaped molded product can be produced which does not affect the electrolyte, is easy to handle, and can be easily discharged from a container.

[0059] Furthermore, the electrolyte molded body (tablet-shaped) of the present disclosure can provide the following effects. The tablet-shaped electrolyte compact has a hardness within a specified range, which makes it highly soluble in the electrolyte solution, making it easy to prepare the electrolyte solution. The tablet-shaped electrolyte compact has a particle size distribution with a small amount of fine powder, making it easy to handle when preparing the electrolyte. Tablet-shaped electrolyte compacts are less likely to cause problems such as clogging when discharged from a container. - Tablet-shaped electrolyte compacts do not have a heating history during each process, so they generate less ions and have high performance when used in batteries (performance degradation is suppressed). The tablet-shaped electrolyte compact prevents the inclusion (increase) of SUS components caused by the device.

[0060] <Application> The electrolyte molded body obtained by the manufacturing method of the present disclosure is used, for example, in batteries (batteries having a charge / discharge mechanism), electricity storage (electrochemical) devices (or ion conductor materials constituting these), etc. Specifically, the electrolyte molded body can be used, for example, as an electrolyte constituting primary batteries, secondary batteries (e.g., lithium (ion) secondary batteries), fuel cells, electrolytic capacitors, electric double layer capacitors, solar cells, electrochromic display elements, etc. EXAMPLES

[0061] The present disclosure will be described below based on examples. Note that the present disclosure is not limited to the following examples, and the following examples can be modified or changed based on the spirit of the present disclosure, and are not excluded from the scope of the present disclosure.

[0062] <Example 1 Series> Example 1 10 kg of powdered LiFSI (manufactured by Nippon Shokubai Co., Ltd., average particle size: 5-500 μm, mode diameter: 263 μm, the same applies below) was put into a roller compactor (manufactured by Kurimoto Iron Works Co., Ltd., model: MRCP-200) and compressed with a roll gap of 0.5 mm and a pressure of 20 MPa to obtain a strip-shaped material (strip-shaped electrolyte) and a powdered material with a longitudinal length of 50 mm. Next, the strip-shaped material and the powdered material were pulverized with a screen-equipped granulator (manufactured by Kurimoto Iron Works Co., Ltd., model: RGS-1512) with a screen diameter of 6 mm and classified with a 1 mm sieve to obtain a mixture of 3 kg of granular material (granular electrolyte compact) with a particle diameter of 6 mm and 7 kg of powdered material (powdered electrolyte, average particle size: 2-1300 μm, mode diameter: 272 μm). The resulting mixture of granular and powdery substances was filled into a 1 L container and stored at room temperature (approximately 25°C) for one month. After storage, the contents (mixture) were discharged from the container, and could be discharged from the outlet (diameter 45 mm) without any agglomerates.

[0063] Example 2 10 kg of powdered LiFSI was fed from a hopper into a rotary tablet press (manufactured by Kikusui Seisakusho Co., Ltd., model: VIRG 0518SR3AZ, the same applies below) equipped with a punch and die with a diameter of 5 mm, and tableted continuously for 2 hours (tabletting pressure: 10 kN) to obtain a mixture of 9.7 kg of tablet-shaped substance (tablet-shaped electrolyte compact) with a particle size of 5 mm and 0.3 kg of powdered substance (powdered electrolyte, average particle size: 0.5 to 600 μm, mode diameter: 280 μm). The obtained mixture of tablet-shaped substance and powdered substance was filled in a 1 L container and stored at room temperature (about 25 ° C) for one month. After storage, the contents (mixture) were discharged from the container, and could be discharged from the discharge port (diameter 45 mm) without any agglomerates.

[0064] Example 3 10 kg of powdered LiFSI was fed from a hopper into a rotary tablet press equipped with a 6 mm diameter punch and tableted continuously for 2 hours (tabletting pressure: 10 kN) to obtain a mixture of 9.8 kg of tablet-shaped substance (tablet-shaped electrolyte compact) with a particle size of 6 mm and 0.2 kg of powdered substance (powdered electrolyte, average particle size: 0.5-650 μm, mode diameter: 262 μm). The obtained mixture of tablet-shaped substance and powdered substance was filled in a 1 L container and stored at room temperature (about 25 ° C) for one month. After storage, the contents (mixture) were discharged from the container, and could be discharged from the outlet (diameter 45 mm) without any agglomerates.

[0065] Comparative Example 1 Powdered LiFSI was filled into a 1L container and stored at room temperature (approximately 25°C) for one month. After storage, when the contents (powdered LiFSI) were discharged from the container, aggregates larger than the outlet (diameter 45 mm) were found, and they could not be discharged without being crushed.

[0066] It was found that in Example 1, which includes a compression step and a pulverization step, and Examples 2 and 3, which include a tableting step, the contents (electrolyte molded bodies) after storage for one month could be discharged from the container without pulverization, compared to Comparative Example 1, which does not include these steps. This shows that the electrolyte molded bodies obtained in Examples 1, 2 and 3 could be easily discharged from the container.

[0067] <Example 2 Series> Example 4 Using 10 kg of powdered LiFSI in the same manner as in Example 2, a mixture of 9.7 kg of tablet-shaped material (tablet-shaped electrolyte compact) having a particle size of 5 mm and 0.3 kg of powdered material (powdered electrolyte (fine powder), average particle size: 0.5 to 600 μm, mode diameter: 280 μm) was obtained. The physical properties of the obtained compact were measured according to the following methods, including particle size distribution (powdered material / compact), the proportion of powdered material in 100 parts by mass of the compact (fine powder proportion), hardness, dissolution rate, ion content, and SUS component content. The results are shown in Table 1.

[0068] [Measurement of particle size of electrolyte compact] The particle size was determined by measuring the smallest length with a caliper.

[0069] [Measurement of the average particle size of powdered electrolyte] 50 g of the powdered electrolyte was placed into a sieve based on the standard JIS Z 8801-1, and after placing the top and bottom lids, the sieve was vibrated up and down 300 times, after which the particle size distribution was measured and the 50% mass average particle size was calculated.

[0070] [Hardness measurement] The molded bodies (number of samples: 5) obtained in Example 4 were set in a digital hardness tester (KHT-20N, Fujiwara Seisakusho Co., Ltd.) and the hardness was measured. The average hardness obtained by averaging the measurement results of the 5 samples was adopted as the hardness of the molded body.

[0071] [Measurement of dissolution rate] In a 50 mL screw tube equipped with a stirrer tip, 11 g of the LiFSI compact obtained in Example 4 and 29 g of dimethyl carbonate were placed and stirred with a magnetic stirrer. The time from the start of stirring until the compact was completely dissolved was measured by visual observation.

[0072] [Measurement of ion content] 0.1 g of the LiFSI compact obtained in Example 4 was weighed out and placed in a 20 mL polypropylene (PP) vial, and diluted 100 times with deionized water to prepare a measurement solution. - ), sulfamate ion, chloride ion (Cl - ), sulfate ion (SO4 2- The amount (concentration) of each ion in the above sample was measured by ion chromatography under the following measurement conditions: Equipment: Thermo Fisher Scientific DIONEX INTEGRION HPIC ·Eluent: 7~18 mmol / L KOH Column: Dionex IonPac AS17-C 4 mm I.D. x 250 mm.

[0073] [Measurement of SUS component content] 0.5 g of the LiFSI compact obtained in Example 4 was weighed out and placed in a 20 mL PP vial, and diluted with approximately 9.5 g of 4% nitric acid to prepare a measurement solution. Metal (SUS) components such as Cr, Fe, and Ni contained in the measurement solution were analyzed by high-frequency inductively coupled plasma atomic emission spectrometry (ICP-AES). The device used was an ICPE-9000 (manufactured by Shimadzu Corporation).

[0074] Comparative Example 2 10 kg of powdered LiFSI was melted at 145°C. The obtained molten LiFSI was sucked up with a dropper while still at 140-145°C, and quickly dropped onto a SUS304 plate heated to 60°C, and solidified to obtain 10 kg of pellets (electrolyte compact) with a particle size of 4.8 mm (the pellets did not contain any powdery material (fine powder)). The above reaction and operation were carried out in a dry room with a dew point of -50°C or less. The physical properties of the obtained pellets were measured in the same manner as in Example 4. The results are shown in Table 1.

[0075] Comparative Example 3 Powdered LiFSI (100% fine powder) was used and each physical property was measured in the same manner as in Example 4. The results are shown in Table 1.

[0076] [Table 1]

Claims

1. A method for producing a molded electrolyte body containing a sulfonylimide compound represented by general formula (1), comprising the steps of: a compression step of compressing and granulating the powdered electrolyte to obtain a sheet or strip of electrolyte; and a crushing step of crushing the sheet-like or rectangular electrolyte to obtain a granular electrolyte molded body. LiN (R 1 SO 2 ) (R 2 SO 2 ) (R 1 and R 2 are the same or different and represent a fluorine atom, an alkyl group having 1 to 6 carbon atoms, or a fluoroalkyl group having 1 to 6 carbon atoms.) (1)

2. 2. The method for producing an electrolyte molded body according to claim 1, wherein in the compression step, the powdered electrolyte is passed between a pair of pressure rolls to be compressed and granulated, thereby obtaining a sheet-like or strip-like electrolyte having a longitudinal length of 10 mm or more and 100 mm or less.

3. The method for producing an electrolyte formed article according to claim 1 or 2, wherein a roller compactor is used in the compressing step.

4. The method for producing an electrolyte formed body according to any one of claims 1 to 3, wherein a roll granulator is used in the pulverizing step.

5. The method for producing an electrolyte molded body according to any one of claims 1 to 4, wherein the granular electrolyte molded body has a particle size of 1 mm or more and 10 mm or less.

6. A method for producing a molded electrolyte body containing a sulfonylimide compound represented by general formula (1), comprising the steps of: The powdered electrolyte is compressed into tablets to obtain a tablet-shaped electrolyte compact, A method for producing an electrolyte molded product, wherein the powdered electrolyte as a starting material contains only the powdered sulfonylimide compound represented by the general formula (1). LiN (R 1 SO 2 ) (R 2 SO 2 ) (R 1 and R 2 are the same or different and represent a fluorine atom, an alkyl group having 1 to 6 carbon atoms, or a fluoroalkyl group having 1 to 6 carbon atoms.) (1)

7. The method for producing an electrolyte molded body according to claim 6 , further comprising a drying step of drying the tablet-shaped electrolyte molded body.

8. The method for producing an electrolyte molded body according to claim 6 , further comprising a wetting step of wetting the powdered electrolyte or the tablet-shaped electrolyte molded body.

9. The method for producing an electrolyte molded body according to any one of claims 6 to 8, wherein a rotary tablet press is used in the tableting step.

10. The method for producing an electrolyte molded body according to any one of claims 6 to 9, wherein the tablet-shaped electrolyte molded body has a particle size of 5 mm or more and 25 mm or less.

11. The sulfonylimide compound represented by the general formula (1) is LiN(FSO 2 ) 2 and LiN(CF 3 SO 2 ) 2 The method for producing an electrolyte formed article according to any one of claims 1 to 10, comprising:

12. The electrolyte is a compound represented by general formula (2), a compound represented by general formula (3), and LiAsF 6 The method for producing an electrolyte formed article according to any one of claims 1 to 11, further comprising at least one selected from the group consisting of: LiPF a (C m F 2m+1 ) 6-a (a: 0≦a≦6, m:1≦m≦4) (2) LiBF b (C n F 2n+1 ) 4-b(b: 0≦b≦4, n:1≦n≦4) (3)

13. A molded body of an electrolyte containing a sulfonylimide compound represented by general formula (1), The proportion of the powdered electrolyte having an average particle diameter of 1,300 μm or less in 100 parts by mass of the molded body is 10 parts by mass or less, The hardness of the molded body is 10 N or more and 50 N or less, The electrolyte comprises only the sulfonylimide compound represented by the general formula (1). LiN (R 1 SO 2 ) (R 2 SO 2 ) (R 1 and R 2 are the same or different and represent a fluorine atom, an alkyl group having 1 to 6 carbon atoms, or a fluoroalkyl group having 1 to 6 carbon atoms.) (1)

14. The electrolyte molded article according to claim 13, wherein the particle size of the molded article is 5 mm or more and 25 mm or less.

Citation Information

Patent Citations

  • Composite solid electrolyte, preparation method thereof and lithium ion battery

    CN111403805A

  • Method for granulating lithium battery electrolyte

    JP2020184527A