Coating solution for manufacturing gas barrier laminates

A coating liquid with specific pH and components stabilizes PVA-based polymers, preventing aggregate sedimentation and maintaining gas barrier properties in high humidity, addressing the limitations of existing laminates by ensuring uniform film formation at lower temperatures.

JP7581646B2Active Publication Date: 2024-11-13TOPPAN HOLDINGS INC
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
JP2020073993
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-17
Publication Date
2024-11-13
Estimated Expiration
2040-04-17

AI Technical Summary

Technical Problem

Existing gas barrier laminates using PVA-based polymers suffer from deteriorating gas barrier properties in high humidity due to moisture absorption, and the formation of aggregates in coating liquids containing polycarboxylic acid polymers and polyvalent metal compounds leads to non-uniform films, necessitating high-temperature heat treatment that can damage base materials.

Method used

A coating liquid comprising a carboxyl group-containing polymer, polyvalent metal-containing particles, a high molecular weight dispersant, and an organic solvent, maintained at a pH of 4 to 6, which prevents sedimentation of aggregates and allows for uniform crosslinking at lower temperatures, ensuring stable gas barrier properties.

Benefits of technology

The solution maintains uniform gas barrier properties under high humidity conditions without high-temperature treatment, preventing aggregate sedimentation and ensuring consistent film formation, thus enhancing the durability and effectiveness of the laminate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581646000001
    Figure 0007581646000001
  • Figure 0007581646000002
    Figure 0007581646000002
  • Figure 0007581646000003
    Figure 0007581646000003
Patent Text Reader

Abstract

To render a coating liquid less susceptible to decrease in gas barrier properties due to sedimentation of aggregates.SOLUTION: A coating liquid for the production of a gas barrier multilayer body according to the present invention contains (A) a carboxy group-containing polymer, (B) polyvalent metal-containing particles, (C) a high molecular weight dispersant having an acidic group and (D) an organic solvent, while having a pH within the range of from 4 to 6 at 25°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas barrier laminate. [Background technology]

[0002] Food, medicine, cosmetics, agricultural chemicals, industrial products, and other items may deteriorate in quality due to oxygen when stored for a long period of time. For this reason, films and sheets with oxygen gas barrier properties are used as packaging materials for these items.

[0003] Conventionally, such packaging materials have often been used that have aluminum foil as a gas barrier layer. However, when using packaging materials that contain aluminum foil, the contents cannot be visually confirmed, and metal detectors cannot be used. Therefore, there has been a demand for development of packaging materials that have excellent gas barrier properties and are transparent, particularly in the food and pharmaceutical fields.

[0004] In response to such demands, gas barrier laminates have been used in which a layer made of polyvinylidene chloride (PVDC) is provided on a substrate by applying a coating liquid containing PVDC. The layer made of PVDC is transparent and has gas barrier properties.

[0005] However, there are concerns that PVDC generates dioxins when incinerated. Therefore, there has been a demand to switch from PVDC to non-chlorine-based materials. In response to this demand, for example, the use of polyvinyl alcohol (PVA)-based polymers instead of PVDC has been proposed.

[0006] A layer made of a PVA-based polymer is densified by hydrogen bonds of hydroxyl groups, and exhibits high gas barrier properties in a low humidity atmosphere. However, a layer made of a PVA-based polymer has a problem that hydrogen bonds are loosened by moisture absorption in a high humidity atmosphere, and gas barrier properties are significantly reduced. Therefore, gas barrier laminates using a layer made of a PVA-based polymer as a gas barrier layer often cannot be used as packaging materials for foods containing a lot of moisture, and their applications have been limited to packaging materials for dry foods, etc.

[0007] In order to further improve the gas barrier property, it has been proposed to add an inorganic layered compound to a PVA-based polymer (see Patent Document 1). However, even if an inorganic layered compound is added, the water resistance of the PVA-based polymer itself is not improved, and the problem of reduced gas barrier property in a high humidity atmosphere still remains.

[0008] In order to improve the gas barrier property under a high humidity atmosphere, it has been proposed to produce a gas barrier laminate by applying a coating liquid containing a PVA-based polymer and a polymer capable of forming a crosslinked structure with the PVA-based polymer to a substrate and then heat treating the substrate (see Patent Documents 2 to 6).

[0009] However, in order to obtain sufficient gas barrier properties using these techniques, it is necessary to perform a heat treatment after application of the coating liquid at a high temperature, for example, 150°C or higher, to form a crosslinked structure. Such a heat treatment can cause severe deterioration of the substrate depending on the substrate material, for example, when the substrate material is a polyolefin such as polypropylene (OPP) or polyethylene (PE). Therefore, there is a demand for a gas barrier laminate that can be produced under milder conditions.

[0010] As a method for forming a gas barrier layer, a method has been proposed in which a layer containing a polycarboxylic acid polymer such as polyacrylic acid is formed and the polycarboxylic acid polymer is ionically crosslinked with polyvalent metal ions (see Patent Documents 7 and 8).

[0011] This method does not require the high-temperature heat treatment performed in the methods described in Patent Documents 2 to 6. Therefore, polyolefin can be used as the substrate. In addition, the obtained gas barrier layer has excellent gas barrier properties even in a high humidity atmosphere. Therefore, the gas barrier laminate including this gas barrier layer can be used in applications where heat sterilization treatment such as boiling or retorting is performed.

[0012] However, when a polycarboxylic acid polymer and a polyvalent metal compound are allowed to coexist in a coating liquid, the polycarboxylic acid polymer and the polyvalent metal compound react with each other in the coating liquid, and precipitation is likely to occur. If precipitation occurs in the liquid, a uniform film cannot be formed. Therefore, in this method, when forming a gas barrier layer, a layer containing a polycarboxylic acid polymer and a layer containing a polyvalent metal compound are formed separately, or an aqueous solution of a polyvalent metal salt is brought into contact with the layer containing a polycarboxylic acid polymer. Therefore, this method has a problem in that more steps are required.

[0013] It has been proposed to set the water content of a coating liquid containing a polycarboxylic acid polymer, polyvalent metal compound particles, a surfactant, and an organic solvent to 1000 ppm or less (see Patent Document 9). In this coating liquid, the water content is 1000 ppm or less, so that the reaction between the polycarboxylic acid polymer and the polyvalent metal compound is suppressed. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] Japanese Patent Application Publication No. 6-093133 [Patent Document 2] JP 2000-289154 A [Patent Document 3] JP 2000-336195 A [Patent Document 4] JP 2001-323204 A [Patent Document 5] JP 2002-020677 A [Patent Document 6] JP 2002-241671 A [Patent Document 7] International Publication No. 2003 / 091317 [Patent Document 8] International Publication No. 2005 / 053954 [Patent Document 9] JP 2005-126528 A Summary of the Invention [Problem to be solved by the invention]

[0015] The coating liquid described in Patent Document 9 does not cause precipitation due to a reaction between a polycarboxylic acid polymer and a polyvalent metal compound as long as the liquid is managed to prevent inclusion of moisture in the liquid. However, the present inventors have found that this coating liquid may cause precipitation of aggregates for another reason, and as a result, a gas barrier laminate having high gas barrier properties may not be produced.

[0016] Therefore, an object of the present invention is to prevent deterioration of gas barrier properties caused by settling of aggregates in a coating liquid. [Means for solving the problem]

[0017] According to a first aspect of the present invention, there is provided a carboxy group-containing polymer (A), Contains oxides of polyvalent metals Polyvalent metal-containing particles (B), phosphate group and an organic solvent (D), and the coating liquid for producing a gas barrier laminate has a pH value at 25° C. in the range of 4 to 6.

[0018] According to a second aspect of the present invention, there is provided the coating liquid according to the first aspect, wherein the polyvalent metal of the polyvalent metal-containing particles (B) is a divalent metal.

[0019] According to a third aspect of the present invention, there is provided the coating liquid according to the first or second aspect, wherein the polyvalent metal-containing particles (B) contain zinc oxide.

[0020] According to a fourth aspect of the present invention, there is provided the coating liquid according to any one of the first to third aspects, wherein the high molecular weight dispersant (C) contains a polyether phosphate ester.

[0021] According to a fifth aspect of the present invention, there is provided a coating liquid according to any one of the first to fourth aspects, in which the amount of the high molecular weight dispersant (C) is within a range of 1 to 30 parts by mass when the amount of the polyvalent metal-containing particles (B) is 100 parts by mass.

[0022] According to a sixth aspect of the present invention, there is provided the coating liquid according to any one of the first to fifth aspects, wherein the carboxyl group-containing polymer (A) has a number average molecular weight in the range of 5,000 to 50,000.

[0023] According to a seventh aspect of the present invention, there is provided a coating liquid according to any one of the first to sixth aspects, which has a water content of 50,000 ppm or less in terms of mass fraction.

[0024] According to an eighth aspect of the present invention, there is provided the coating liquid according to any one of the first to seventh aspects, wherein a ratio of the product (Bt) of the number of moles and the valence of the polyvalent metal contained in the polyvalent metal-containing particles (B) to the number of moles (At) of carboxy groups contained in the carboxy group-containing polymer (A) is 0.6 or more.

[0025] According to a ninth aspect of the present invention, there is provided a coating liquid according to any one of the first to eighth aspects, in which, when a first average particle size D1 immediately after production and a second average particle size D2 are measured after 8 hours from production under a temperature condition of 25°C, a ratio D2 / D1 of the second average particle size D2 to the first average particle size D1 is within a range of 0.8 to 1.3.

[0026] According to a tenth aspect of the present invention, there is provided a gas barrier laminate comprising a cured film of the coating liquid according to any one of the first to ninth aspects as a coating layer.

[0027] According to an eleventh aspect of the present invention, there is provided a film having a thickness in the range of 0.01 to 100 μm and an oxygen permeability of 1,000 cm measured under conditions of 30° C. and a relative humidity of 70%. 3 / (m 2 The gas barrier laminate according to a tenth aspect has a thermal conductivity of 1.0 MPa or less.

[0028] According to a twelfth aspect of the present invention, there is provided a packaging material comprising the gas barrier laminate according to the tenth or eleventh aspect.

[0029] According to a thirteenth aspect of the present invention there is provided a package comprising a packaging material according to the twelfth aspect.

[0030] According to a fourteenth aspect of the present invention, there is provided a packaged article including a package according to the thirteenth aspect and contents contained in the package.

[0031] According to a fifteenth aspect of the present invention, a method for producing a mixed liquid having a pH of 4 to 6 at 25° C. is provided, comprising mixing a polymer solution (I) and a polyvalent metal dispersion liquid (II), the polymer solution (I) containing a carboxy group-containing polymer (A) and an organic solvent (D), and the polyvalent metal dispersion liquid (II) is Contains oxides of polyvalent metals Polyvalent metal-containing particles (B); phosphate group and an organic solvent (D).

[0032] According to a sixteenth aspect of the present invention, there is provided the production method according to the fifteenth aspect, wherein the polymer solution (I) has a pH in the range of 3 to 7 at 25° C., and the polyvalent metal dispersion liquid (II) has a pH in the range of 3 to 7 at 25° C.

[0033] According to a seventeenth aspect of the present invention, there is provided a method for producing a gas barrier laminate, the method including producing the coating liquid by the method according to the fifteenth or sixteenth aspect, and forming a coating layer from the coating liquid.

[0034] According to an eighteenth aspect of the present invention, there is provided a method for producing a gas barrier laminate, comprising forming a coating layer from the coating liquid according to any one of the first to ninth aspects. Effect of the Invention

[0035] According to the present invention, it is possible to make it difficult for deterioration of gas barrier properties to occur due to settling of aggregates in a coating liquid. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following describes embodiments of the present invention, which are specific embodiments of any of the above aspects.

[0037] <Coating solution for manufacturing gas barrier laminate> The coating liquid for producing a gas barrier laminate according to an embodiment of the present invention (hereinafter, also simply referred to as the coating liquid) contains a carboxyl group-containing polymer (A), polyvalent metal-containing particles (B), a high molecular weight dispersing agent having an acidic group (C), and an organic solvent (D), and is characterized by having a pH at 25° C. in the range of 4 to 6.

[0038] [Carboxy Group-Containing Polymer (A)] The carboxyl group-containing polymer used in the coating liquid is a polymer having two or more carboxyl groups in the molecule, and is sometimes called a "polycarboxylic acid polymer." Representative examples of the carboxyl group-containing polymer include a homopolymer of a carboxyl group-containing unsaturated monomer, a copolymer of two or more kinds of carboxyl group-containing unsaturated monomers, a copolymer of a carboxyl group-containing unsaturated monomer and another polymerizable monomer, and a polysaccharide containing a carboxyl group in the molecule (also called a "carboxyl group-containing polysaccharide" or an "acidic polysaccharide").

[0039] The carboxy group includes not only a free carboxy group but also an acid anhydride group (specifically, a dicarboxylic acid anhydride group). The acid anhydride group may be partially ring-opened to form a carboxy group. A part of the carboxy group may be neutralized with an alkali. In this case, the degree of neutralization is preferably 20% or less.

[0040] Here, the "degree of neutralization" is a value obtained by the following method. That is, the carboxyl groups can be partially neutralized by adding an alkali (E) to the carboxyl group-containing polymer (A). In this case, the ratio of the number of moles (Et) of the alkali (E) to the number of moles (At) of the carboxyl groups contained in the carboxyl group-containing polymer (A) is the degree of neutralization.

[0041] In addition, a graft polymer obtained by graft polymerizing a carboxyl-containing unsaturated monomer onto a polymer not containing a carboxyl group, such as polyolefin, can also be used as the carboxyl-containing polymer. A polymer obtained by hydrolyzing a polymer having a hydrolyzable ester group, such as an alkoxycarbonyl group (e.g., a methoxycarbonyl group), to convert it into a carboxyl group can also be used.

[0042] The carboxyl group-containing unsaturated monomer is preferably an α,β-monoethylenically unsaturated carboxylic acid. Therefore, the carboxyl group-containing polymer includes a homopolymer of an α,β-monoethylenically unsaturated carboxylic acid, a copolymer of two or more kinds of α,β-monoethylenically unsaturated carboxylic acids, and a copolymer of an α,β-monoethylenically unsaturated carboxylic acid and another polymerizable monomer. The other polymerizable monomer is typically an ethylenically unsaturated monomer.

[0043] Examples of α,β-monoethylenically unsaturated carboxylic acids include unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; unsaturated dicarboxylic anhydrides such as maleic anhydride and itaconic anhydride; and mixtures of two or more of these. Among these, at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid is preferred, and at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, and maleic acid is more preferred.

[0044] Other polymerizable monomers copolymerizable with α,β-monoethylenically unsaturated carboxylic acid, particularly ethylenically unsaturated monomers, include, for example, ethylene; α-olefins such as propylene, 1-butene, 1-pentene, 1-hexene, and 1-octene; saturated carboxylic acid vinyl esters such as vinyl acetate; acrylic acid alkyl esters such as methyl acrylate and ethyl acrylate; methacrylic acid alkyl esters such as methyl methacrylate and ethyl methacrylate; chlorine-containing vinyl monomers such as vinyl chloride and vinylidene chloride; fluorine-containing vinyl monomers such as vinyl fluoride and vinylidene fluoride; unsaturated nitriles such as acrylonitrile and methacrylonitrile; aromatic vinyl monomers such as styrene and α-methylstyrene; and itaconic acid alkyl esters. These ethylenically unsaturated monomers can be used alone or in combination of two or more. In addition, when the carboxy group-containing polymer is a copolymer of an α,β-monoethylenically unsaturated carboxylic acid and a saturated carboxylic acid vinyl ester such as vinyl acetate, a copolymer obtained by saponifying this copolymer to convert the saturated carboxylic acid vinyl ester units into vinyl alcohol units can also be used.

[0045] Examples of the carboxyl group-containing polysaccharides include acidic polysaccharides having a carboxyl group in the molecule, such as alginic acid, carboxymethylcellulose, and pectin. These acidic polysaccharides can be used alone or in combination of two or more. The acidic polysaccharides can also be used in combination with a (co)polymer of an α,β-monoethylenically unsaturated carboxylic acid.

[0046] When the carboxy group-containing polymer is a copolymer of an α,β-monoethylenically unsaturated carboxylic acid and another ethylenically unsaturated monomer, from the viewpoints of the gas barrier properties, hot water resistance, and water vapor resistance of the resulting film, the proportion of the number of moles of the α,β-monoethylenically unsaturated carboxylic acid monomer to the total number of moles of those monomers in the copolymer is preferably 60 mol % or more, more preferably 80 mol % or more, and particularly preferably 90 mol % or more.

[0047] The carboxyl group-containing polymer is preferably a homopolymer or copolymer obtained by polymerization of only α,β-monoethylenically unsaturated carboxylic acid, in that it is easy to obtain a film having excellent gas barrier properties, moisture resistance, water resistance, hot water resistance, and water vapor resistance, and also excellent gas barrier properties under high humidity conditions. When the carboxyl group-containing polymer is a (co)polymer consisting of only α,β-monoethylenically unsaturated carboxylic acid, its preferred specific examples are homopolymers, copolymers, and mixtures of two or more thereof obtained by polymerization of at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid. Among these, homopolymers and copolymers of at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, and maleic acid are more preferred.

[0048] As the carboxyl group-containing polymer, polyacrylic acid, polymethacrylic acid, polymaleic acid, and a mixture of two or more of them are particularly preferred. As the acidic polysaccharide, alginic acid is preferred. Among these, polyacrylic acid is particularly preferred because it is relatively easy to obtain and a film having excellent physical properties can be easily obtained.

[0049] The number average molecular weight of the carboxyl group-containing polymer is, for example, 200,000 or less. This number average molecular weight is preferably 100,000 or less, more preferably 90,000 or less, more preferably 80,000 or less, more preferably 70,000 or less, more preferably 60,000 or less, and particularly preferably 50,000 or less.

[0050] If the number average molecular weight of the carboxyl group-containing polymer is too large, it acts as a flocculant. As a result, the entire coating liquid may gel or precipitates may form in the coating liquid. The coating liquid that has gelled or precipitated cannot be used to form a coating film, or even if it can be used to form a coating film, it is extremely difficult to form a coating film with a uniform thickness and composition. Furthermore, the coating layer obtained from the coating film with a non-uniform thickness and composition also has a non-uniform thickness and composition, and the in-plane uniformity of gas barrier properties, mechanical properties, etc. is insufficient.

[0051] The number average molecular weight of the carboxy group-containing polymer is preferably 2,000 or more, more preferably 3,000 or more, even more preferably 4,000 or more, and particularly preferably 5,000 or more.

[0052] If the number-average molecular weight of the carboxyl group-containing polymer is too small, the viscosity of the coating liquid will be low. As a result, in the drying process after coating, convection (Marangoni convection) will occur in the coating liquid, making it extremely difficult to form a coating film with a uniform thickness and composition. Therefore, the in-plane uniformity of the resulting coating layer will be insufficient, making it difficult to obtain stable gas barrier properties and mechanical properties. In addition, if the number-average molecular weight of the carboxyl group-containing polymer is too small, the fracture stress of the coating film formed by the coating liquid will be low, increasing the risk of cracks occurring in the coating film during processing. It will be extremely difficult for a coating film with cracks to exhibit the desired gas barrier properties and mechanical properties.

[0053] Here, the "number average molecular weight" is a value obtained by measurement using gel permeation chromatography (GPC). In GPC measurement, the number average molecular weight of a polymer is generally measured in terms of standard polystyrene.

[0054] [Polyvalent metal-containing particles (B)] The polyvalent metal-containing particles used in the coating liquid are particles containing one or more polyvalent metals whose metal ions have a valence of 2 or more. The polyvalent metal-containing particles may be particles made of a polyvalent metal whose metal ions have a valence of 2 or more, particles made of a compound of a polyvalent metal whose metal ions have a valence of 2 or more, or a mixture thereof.

[0055] Specific examples of polyvalent metals include, but are not limited to, metals in Group 2A of the short periodic table, such as beryllium, magnesium, and calcium; transition metals, such as titanium, zirconium, chromium, manganese, iron, cobalt, nickel, copper, and zinc; and aluminum.

[0056] The polyvalent metal is preferably a divalent metal, and the polyvalent metal preferably forms a compound.

[0057] Specific examples of polyvalent metal compounds include, but are not limited to, oxides, hydroxides, carbonates, organic acid salts, and inorganic acid salts of polyvalent metals. Examples of organic acid salts include, but are not limited to, acetates, oxalates, citrates, lactates, phosphates, phosphites, hypophosphites, stearates, and monoethylenically unsaturated carboxylates. Examples of inorganic acid salts include, but are not limited to, chlorides, sulfates, and nitrates. Alkyl alkoxides of polyvalent metals can also be used as polyvalent metal compounds. These polyvalent metal compounds can be used alone or in combination of two or more.

[0058] Among the polyvalent metal compounds, from the viewpoints of dispersion stability of the coating liquid and the gas barrier properties of the laminate formed from the coating liquid, compounds of beryllium, magnesium, calcium, copper, cobalt, nickel, zinc, aluminum, and zirconium are preferred, and compounds of divalent metals such as beryllium, magnesium, calcium, copper, zinc, cobalt, and nickel are more preferred.

[0059] Preferred divalent metal compounds include, but are not limited to, oxides such as zinc oxide, magnesium oxide, copper oxide, nickel oxide, and cobalt oxide; carbonates such as calcium carbonate; organic acid salts such as calcium lactate, zinc lactate, and calcium acrylate; and alkoxides such as magnesium methoxide.

[0060] The polyvalent metal or polyvalent metal compound is used as particles, and the particle shape is maintained even in the coating liquid. From the viewpoint of the dispersion stability of the coating liquid and the gas barrier property of the laminate formed from the coating liquid, the average particle diameter of the polyvalent metal-containing particles is preferably within the range of 10 nm to 10 μm (or 10,000 nm), more preferably within the range of 12 nm to 1 μm (or 1,000 nm), even more preferably within the range of 15 nm to 500 nm, and particularly preferably within the range of 15 nm to 50 nm.

[0061] If the average particle size of the polyvalent metal-containing particles in the coating liquid is too large, the uniformity of the film thickness of the resulting coating layer, the flatness of the surface, and the ionic crosslinking reactivity with the carboxyl group-containing polymer are likely to be insufficient. If the average particle size of the polyvalent metal-containing particles is too small, the ionic crosslinking reaction with the carboxyl group-containing polymer may proceed early. In addition, it is difficult to uniformly disperse ultrafine particles with a particle size of less than 10 nm in the coating liquid.

[0062] The average particle size of the polyvalent metal-containing particles can be measured by measuring and counting using a scanning electron microscope or a transmission electron microscope when the sample is a dry solid. The average particle size of the polyvalent metal-containing particles in the coating liquid can be measured by a light scattering method (Reference: "Fine Particle Engineering System", Vol. I, pp. 362-365, Fuji Techno System (2001)).

[0063] The polyvalent metal-containing particles in the coating liquid exist as primary particles, secondary particles, or a mixture of these, but in many cases, judging from the average particle size, it is assumed that they exist as secondary particles.

[0064] [High molecular weight dispersant (C)] In the above coating liquid, a dispersant is used to improve the dispersibility of the polyvalent metal-containing particles. The dispersant used in this coating liquid is a high molecular weight dispersant having an acidic group.

[0065] The dispersant is a surfactant. A surfactant is a compound that has both hydrophilic and lipophilic groups in the molecule. Surfactants include anionic, cationic, and amphoteric ionic surfactants, as well as nonionic surfactants. In the coating liquid, an anionic or nonionic surfactant or a combination thereof is used as the high molecular weight dispersant.

[0066] Anionic surfactants include, for example, carboxylic acid type, sulfonic acid type, sulfate type, and phosphate type. Examples of carboxylic acid type anionic surfactants include aliphatic monocarboxylates, polyoxyethylene alkyl ether carboxylates, N-acylsarcosinates, and N-acylglutamates. Examples of sulfonic acid type anionic surfactants include dialkyl sulfosuccinates, alkanesulfonates, alpha olefin sulfonates, linear alkylbenzene sulfonates, alkyl (branched) benzene sulfonates, naphthalene sulfonate-formaldehyde condensates, alkyl naphthalene sulfonates, and N-methyl-N-acyltaurates. Examples of sulfate type anionic surfactants include alkyl sulfates, polyoxyethylene alkyl ether sulfates, and oil sulfates. Examples of phosphate type anionic surfactants include alkyl phosphates, polyoxyethylene alkyl ether phosphates, and polyoxyethylene alkyl phenyl ether phosphates.

[0067] Examples of the nonionic surfactant include ester-type surfactants, such as glycerin fatty acid esters, sorbitan fatty acid esters, and sucrose fatty acid esters.

[0068] Among these surfactants, surfactants having a phosphoric acid group such as phosphate esters are preferred, and polyether phosphate esters are particularly preferred.

[0069] The high molecular weight dispersant (surfactant) preferably has a number average molecular weight of at least 2,000, more preferably at least 5,000, and even more preferably at least 10,000. If the molecular weight of the dispersant is too small, it is difficult to stably disperse the polyvalent metal-containing particles in the coating liquid.

[0070] The high molecular weight dispersant (surfactant) preferably has a number average molecular weight of not more than 300,000, more preferably not more than 200,000, and even more preferably not more than 150,000. If the molecular weight of the dispersant is excessively large, the particles cannot be sufficiently refined during dispersion, and the transparency of the coating film decreases.

[0071] Dispersants having acidic groups are easily bonded to polyvalent metals. In addition, the dispersants used here have a high molecular weight, so they have a high ability to stably maintain the dispersion state of polyvalent metal-containing particles. Therefore, by using a high molecular weight dispersant having acidic groups, it is possible to realize a state in which polyvalent metal-containing particles are uniformly distributed, and to maintain this state for a long period of time.

[0072] [Organic solvent (D)] In the coating liquid, an organic solvent is used as a solvent or dispersion medium. As the organic solvent, a polar organic solvent capable of dissolving a carboxyl group-containing polymer is generally used, but an organic solvent having no polar group (heteroatom or atomic group having a heteroatom) may be used in combination with the polar organic solvent.

[0073] Examples of organic solvents that can be preferably used include alcohols such as methanol, ethanol, isopropanol, n-propanol, and n-butanol; and polar organic solvents such as dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, tetramethylurea, hexamethylphosphoric triamide, and γ-butyrolactone.

[0074] In addition to the above polar organic solvents, hydrocarbons such as benzene, toluene, xylene, hexane, heptane, and octane, ketones such as acetone and methyl ethyl ketone, halogenated hydrocarbons such as dichloromethane, esters such as methyl acetate, and ethers such as diethyl ether can be used as appropriate. Hydrocarbons such as benzene that do not have a polar group are generally used in combination with a polar organic solvent.

[0075] The coating liquid may contain only an organic solvent as a solvent or dispersion medium, but may further contain water. By containing water, the solubility of the carboxyl group-containing polymer can be improved, and the coating property and workability of the coating liquid can be improved. The water content of this coating liquid may be 100 ppm or more, 1,000 ppm or more, 1,500 ppm or more, or 2,000 ppm or more by mass fraction.

[0076] When a carboxyl group-containing polymer having a small number average molecular weight is used, this coating liquid is unlikely to cause precipitation or gelation even at a water content that would cause precipitation or gelation in a coating liquid using a carboxyl group-containing polymer having a large number average molecular weight. The water content of this coating liquid is preferably 50,000 ppm or less, more preferably 30,000 ppm or less, even more preferably 10,000 ppm or less, and particularly preferably 5,000 ppm or less, in terms of mass fraction.

[0077] 〔composition〕 The coating liquid contains a carboxy group-containing polymer (A), polyvalent metal-containing particles (B), a high molecular weight dispersant (C), and an organic solvent (D), and is a dispersion in which the polyvalent metal-containing particles are dispersed.

[0078] The ratio (hereinafter also referred to as equivalent ratio) of the product (Bt) of the number of moles of the polyvalent metal contained in the polyvalent metal-containing particle (B) and the valence to the number of moles (At) of the carboxyl group contained in the carboxyl group-containing polymer (A) is preferably 0.6 or more. This ratio is more preferably 0.8 or more, and particularly preferably 1.0 or more. The upper limit of this ratio is usually 10.0, preferably 2.0. If this ratio is too small, the properties such as gas barrier property, hot water resistance, and water vapor resistance of the laminate formed with the coating layer from the coating liquid are reduced.

[0079] The above-mentioned equivalent ratio can be determined, for example, as follows: An example will be described in which the carboxyl group-containing polymer is polyacrylic acid and the polyvalent metal compound is magnesium oxide.

[0080] Polyacrylic acid has a molecular weight of 72 per monomer unit, and has one carboxy group per monomer molecule. Therefore, the amount of carboxy groups in 100 g of polyacrylic acid is 1.39 moles. The above-mentioned equivalent ratio of 1.0 in a coating liquid containing 100 g of polyacrylic acid means that the coating liquid contains magnesium oxide in an amount that neutralizes 1.39 moles of carboxy groups. Therefore, in order to make the above-mentioned equivalent ratio in a coating liquid containing 100 g of polyacrylic acid 0.6, it is sufficient to add magnesium oxide in an amount that neutralizes 0.834 moles of carboxy groups to the coating liquid. Here, the valence of magnesium is divalent, and the molecular weight of magnesium oxide is 40. Therefore, in order to make the above-mentioned equivalent ratio in a coating liquid containing 100 g of polyacrylic acid 0.6, it is sufficient to add 16.68 g (0.417 moles) of magnesium oxide to the coating liquid.

[0081] The organic solvent is used in an amount sufficient to uniformly dissolve the carboxyl group-containing polymer and uniformly disperse the polyvalent metal-containing particles. Therefore, the organic solvent used is one that dissolves the carboxyl group-containing polymer but does not substantially dissolve the polyvalent metal compound and can disperse it in the form of particles.

[0082] The high molecular weight dispersant is used in an amount sufficient to stably disperse the polyvalent metal-containing particles. The amount of the high molecular weight dispersant in the coating liquid is preferably 1 to 30 parts by weight, more preferably 5 to 25 parts by weight, and even more preferably 10 to 20 parts by weight, based on 100 parts by weight of the polyvalent metal-containing particles.

[0083] If the amount of the high molecular weight dispersant is too small, it becomes difficult to disperse the polyvalent metal-containing particles in the coating liquid so that their average particle size becomes sufficiently small, and as a result, it becomes difficult to obtain a coating liquid in which the polyvalent metal-containing particles are uniformly dispersed, and it becomes difficult to form a coating film with a uniform thickness when applied to a substrate.

[0084] Also, if the amount of the high molecular weight dispersant is too small, the polyvalent metal-containing particles are likely to aggregate or settle in the coating liquid. Therefore, the amount of polyvalent metal-containing particles contained in the coating film may be significantly different between immediately after the start of use of the coating liquid for coating and when the remaining amount of the coating liquid is reduced after repeated coating. As a result, there may be a significant difference in gas barrier properties between the gas barrier laminate produced immediately after the start of use of the coating liquid for coating and the gas barrier laminate produced when the remaining amount of the coating liquid is reduced.

[0085] If the amount of the high molecular weight dispersant is too large, this can cause a decrease in the dispersion stability of the particles in the coating liquid and a decrease in the gas barrier properties of the coating film.

[0086] The coating liquid has a pH in the range of 4 to 6 at 25°C. The pH of the coating liquid at 25°C is preferably in the range of 4.5 to 6. If the pH is too low, precipitation of aggregates may occur immediately after the production of the coating liquid. If the pH is too high, precipitation of aggregates occurs immediately after the production of the coating liquid or occurs after a certain time has elapsed since the production of the coating liquid, making it impossible to produce a gas barrier laminate having high gas barrier properties.

[0087] [Method of producing coating liquid] To produce the coating liquid, first, a polymer solution (I) is prepared by uniformly dissolving a carboxyl group-containing polymer (A) in an organic solvent (D). For example, when using commercially available polyacrylic acid as a starting material, the polyacrylic acid is uniformly dissolved in an organic solvent (D) to prepare a polyacrylic acid solution.

[0088] On the other hand, the polyvalent metal-containing particles (B), the high molecular weight dispersant (C), and the organic solvent (D) are mixed and, if necessary, a dispersion treatment is performed to prepare a polyvalent metal dispersion liquid (II). The dispersion treatment is performed so that the average particle diameter of the polyvalent metal-containing particles (B) becomes a predetermined value. If the average particle diameter of the polyvalent metal-containing particles (B) in the mixed liquid before the dispersion treatment is 10 μm or less, the dispersion treatment may not be performed, but even in that case, it is preferable to perform the dispersion treatment. By performing the dispersion treatment, the aggregation of the polyvalent metal-containing particles (B) is dissolved, the coating liquid is stabilized, and the transparency of the gas barrier laminate obtained by applying the coating liquid is increased. Furthermore, when the coating liquid is applied and the coating film is dried, the crosslinking between the carboxyl group-containing polymer and the polyvalent metal ions is easily promoted, and a gas barrier laminate having good gas barrier properties is easily obtained.

[0089] Dispersion methods include those using a high-speed stirrer, homogenizer, ball mill, or bead mill. In particular, dispersion using a ball mill or bead mill can achieve high efficiency, and therefore a coating liquid with a stable dispersion state can be obtained in a relatively short time. In this case, the diameter of the balls or beads is preferably small, preferably 0.1 to 1 mm.

[0090] The polymer solution (I) and the polyvalent metal dispersion (II) prepared as above are mixed to prepare a coating liquid.

[0091] The polymer solution (I) preferably has a pH at 25° C. in the range of 3 to 7, and more preferably in the range of 4 to 6. The polyvalent metal dispersion (II) preferably has a pH at 25° C. in the range of 3 to 7, and more preferably in the range of 4 to 7. The absolute value of the difference between the pH of the polymer solution (I) at 25° C. and the pH of the polyvalent metal dispersion (II) at 25° C. is preferably 4 or less, and more preferably 3 or less.

[0092] When the pH is set as above, when the polymer solution (I) and the polyvalent metal dispersion (II) are mixed, the carboxyl group-containing polymer and the polyvalent metal-containing particles are uniformly distributed, and the variation in crosslink density in the coating layer of the gas barrier laminate can be reduced, making it possible to prevent deterioration of the gas barrier properties caused by the presence of portions with low crosslink density.

[0093] The total concentration of the components other than the organic solvent in the above coating liquid is preferably within the range of 0.1 to 60% by mass, more preferably 0.5 to 25% by mass, and particularly preferably 1 to 10% by mass, in order to obtain a coating film or coat layer of a desired thickness with high workability.

[0094] The above coating liquid may contain various additives such as other polymers, thickeners, stabilizers, ultraviolet absorbers, antiblocking agents, softeners, inorganic layered compounds (e.g., montmorillonite), and colorants (dyes, pigments), as necessary. The above coating liquid may further contain other dispersants such as polyamines as a dispersant in addition to the high molecular weight dispersant (C) having an acidic group.

[0095] In the coating solution obtained in this manner, the carboxyl group-containing polymer and the polyvalent metal-containing particles are uniformly distributed, and this state is maintained by the combination of the high molecular weight dispersant and a pH within a specified range. That is, the coating solution does not cause precipitation of aggregates immediately after production, and maintains this state even after a certain time has passed since production.

[0096] For example, when the first average particle diameter D1 immediately after production of this coating liquid and the second average particle diameter D2 8 hours after production under a temperature condition of 25°C are measured, the ratio D2 / D1 of the second average particle diameter D2 to the first average particle diameter D1 is preferably within a range of 0.8 to 1.3. Note that the "average particle diameter" here is a value obtained by a dynamic light scattering method.

[0097] Therefore, when this coating liquid is used, deterioration of the gas barrier properties caused by settling of aggregates in the coating liquid is unlikely to occur.

[0098] <Gas barrier laminate> The gas barrier laminate according to an embodiment of the present invention comprises a substrate and a gas barrier layer provided on at least one surface of the substrate, and is characterized in that the gas barrier layer comprises a cured film of the coating liquid described above as a coating layer.

[0099] [Base material] There are no particular limitations on the substrate in the gas barrier laminate, and various types of substrates can be used.

[0100] The material constituting the substrate is not particularly limited, and various types of materials can be used, such as plastic or paper.

[0101] The substrate may be a single layer made of a single material, or may be a multi-layer made of multiple materials, such as a substrate in which a plastic film is laminated to paper.

[0102] Of the above materials, plastics are preferred as the material for the substrate, since they can be molded into various shapes and can be given gas barrier properties to further expand the range of applications.

[0103] Examples of plastics include, but are not limited to, polyolefin resins such as polyethylene and polypropylene; polyester resins such as polyethylene terephthalate, polyethylene-2,6-naphthalate, polybutylene terephthalate, and copolymers thereof; polyamide resins such as nylon-6, nylon-66, nylon-12, metaxylylene adipamide, and copolymers thereof; styrene resins such as polystyrene, styrene-butadiene copolymer, and styrene-butadiene-acrylonitrile copolymer; poly(meth)acrylic acid esters; polyacrylonitrile; polyvinyl acetate; ethylene-vinyl acetate copolymer; ethylene-vinyl alcohol copolymer; polycarbonate; polyarylate; regenerated cellulose; polyimide; polyetherimide; polysulfone; polyethersulfone; polyetherketone; and ionomer resins.

[0104] When the gas barrier laminate is used as a food packaging material, the substrate is preferably made of polyethylene, polypropylene, polyethylene terephthalate, nylon-6 or nylon-66.

[0105] As the plastic constituting the substrate, one type may be used alone, or two or more types may be blended and used.

[0106] The plastic may contain additives. The additives may be appropriately selected from known additives such as pigments, antioxidants, antistatic agents, ultraviolet absorbers, and lubricants depending on the application. The additives may be used alone or in combination of two or more.

[0107] The form of the substrate is not particularly limited, and examples thereof include a film, a sheet, a cup, a tray, a tube, and a bottle. Among these, a film is preferable.

[0108] When the substrate is a film, the film may be a stretched film or an unstretched film.

[0109] There are no particular limitations on the thickness of the film, but from the viewpoint of the mechanical strength and processability of the resulting gas barrier laminate, it is preferably in the range of 1 to 200 μm, and more preferably in the range of 5 to 100 μm.

[0110] The surface of the substrate may be subjected to plasma treatment, corona treatment, ozone treatment, flame treatment, or radical activation treatment using ultraviolet (UV) or electron beams, etc., so that the coating liquid can be applied without being repelled by the substrate. The treatment method is appropriately selected depending on the type of substrate.

[0111] [Coat layer] The coating layer is a cured film of the coating liquid. That is, the coating layer is formed from the coating liquid, specifically, the coating liquid is applied to a substrate and the coating film is dried. As described above, the coating layer contains a carboxyl group-containing polymer ionically crosslinked with polyvalent metal ions, and exhibits excellent gas barrier properties even in a high humidity atmosphere.

[0112] The coating layer may be provided on one surface or on both surfaces of the substrate. The coating layer may be provided directly on the surface of the substrate, or may be provided on the surface of one or more other layers (for example, an anchor coating layer) provided on the substrate. The method for forming the coating layer will be described in detail later.

[0113] The thickness of the coating layer is not particularly limited, but from the viewpoints of formability and handling during formation of the gas barrier laminate, it is preferably in the range of 0.01 to 100 μm, more preferably in the range of 0.1 to 10 μm, and even more preferably in the range of 0.1 to 0.5 μm.

[0114] [Other layers] The gas barrier laminate may further include one or more layers other than the substrate and the coating layer, if necessary.

[0115] For example, the gas barrier layer of the gas barrier laminate may consist of only a coating layer, or may further include one or more other layers in addition to the coating layer. For example, a layer made of an inorganic compound such as aluminum oxide, silicon oxide, and aluminum may be formed on the surface of a substrate by a sputtering method, an ion plating method, or the like.

[0116] The gas barrier laminate may further include an anchor coat layer between the substrate and the coat layer for the purposes of increasing the adhesion between the substrate and the coat layer and enabling the coating liquid to be applied to the substrate without being repelled by the substrate.

[0117] The anchor coat layer can be formed by a conventional method using a known anchor coat agent.

[0118] Examples of the anchor coating agent include those containing resins such as polyurethane resin, acrylic resin, melamine resin, polyester resin, phenol resin, amino resin, and fluororesin.

[0119] In addition to the resin, the anchor coating agent may further contain an isocyanate compound for the purpose of improving adhesion and hot water resistance. The isocyanate compound may be any compound having one or more isocyanate groups in the molecule, and examples thereof include hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, and tolylene diisocyanate.

[0120] The anchor coating agent may further contain a liquid medium for dissolving or dispersing the resin and the isocyanate compound. The thickness of the anchor coat layer is not particularly limited.

[0121] The gas barrier laminate may, as necessary, further comprise another layer laminated via an adhesive onto the coating layer provided on the substrate, or onto a surface of the substrate on which no coating layer is provided, or may further comprise another layer formed by extrusion lamination of an adhesive resin.

[0122] The other layers to be laminated can be appropriately selected according to the purpose of imparting strength, sealing properties, easy opening when sealed, design, light blocking properties, moisture resistance, etc., and are not particularly limited, but examples thereof include those made of the same material as the plastics described above for the substrate. In addition, paper, aluminum foil, etc. may be used.

[0123] The thickness of the other layer to be laminated is preferably in the range of 1 to 1000 μm, more preferably in the range of 5 to 500 μm, even more preferably in the range of 5 to 200 μm, and particularly preferably in the range of 5 to 150 μm. The other layer to be laminated may be one type or two or more types.

[0124] The gas barrier laminate may further include a printed layer, if necessary. The printed layer may be formed on a coating layer provided on a substrate, or may be formed on a surface of a substrate on which no coating layer is provided. In addition, when another layer is laminated, the printed layer may be formed on the other layer to be laminated.

[0125] [Method for producing gas barrier laminate] The gas barrier laminate can be produced by a production method including a step of forming a coating layer by applying the above-mentioned coating liquid to a substrate and drying the coating film. This production method can further include a step of laminating another layer and a step of forming a print layer, etc., before and / or after the step of forming the coating layer, as necessary.

[0126] The method for applying the coating liquid is not particularly limited, but examples thereof include methods using an air knife coater, a direct gravure coater, a gravure offset coater, an arc gravure coater, a reverse roll coater such as a top feed reverse coater, a bottom feed reverse coater, or a nozzle feed reverse coater, a five-roll coater, a lip coater, a bar coater, a bar reverse coater, or a die coater.

[0127] The method for drying the coating film is not particularly limited, but examples thereof include a method of natural drying, a method of drying in an oven set at a predetermined temperature, and a method using a dryer attached to a coater, such as an arch dryer, a floating dryer, a drum dryer, or an infrared dryer.

[0128] Drying conditions can be appropriately selected depending on the drying method, etc. For example, in a method of drying in an oven, the drying temperature is preferably within the range of 40 to 150° C., more preferably within the range of 45 to 150° C., and particularly preferably within the range of 50 to 140° C. The drying time varies depending on the drying temperature, but is preferably within the range of 0.5 seconds to 10 minutes, more preferably within the range of 1 second to 5 minutes, and particularly preferably within the range of 1 second to 1 minute.

[0129] It is presumed that during or after drying, the carboxyl group-containing polymer contained in the coating film reacts with the polyvalent metal-containing particles to introduce an ionic crosslinking structure. In order to fully advance the ionic crosslinking reaction, it is preferable to age the dried film for about 1 second to 10 days in an atmosphere with a relative humidity of preferably 20% or more, more preferably 40 to 100%, and at a temperature of preferably 5 to 200°C, more preferably 20 to 150°C.

[0130] The gas barrier laminate thus obtained is ionically crosslinked, and therefore has excellent moisture resistance, water resistance, hot water resistance, and water vapor resistance. This gas barrier laminate has excellent gas barrier properties not only under low humidity conditions but also under high humidity conditions. This gas barrier laminate preferably has an oxygen transmission rate of 1,000 cm, measured at 30°C and a relative humidity of 70% according to JIS K-7126 B method (constant pressure method) and the method described in ASTM D3985. 3 / (m 2 ·day·MPa) or less, more preferably 500cm 3 / (m 2 ·day·MPa) or less, particularly preferably 100 cm 3 / (m 2 The lower the oxygen permeability, the better. There is no particular lower limit for the oxygen permeability, but it is usually 0.1 cm 3 / (m 2 ·day·MPa) or more.

[0131] As described above, in this coating liquid, the carboxyl group-containing polymer and the polyvalent metal-containing particles are uniformly distributed, and this state is maintained even after a certain time has passed since the production of the coating liquid. Therefore, when this coating liquid is used, it is possible to prevent a large difference in the amount of polyvalent metal-containing particles contained in the coating film between immediately after the start of use of the coating liquid for coating and when the remaining amount of the coating liquid becomes small after repeated coating. Therefore, it is possible to prevent the production of a gas barrier laminate with insufficient gas barrier properties. In this way, when the above coating liquid is used, the deterioration of gas barrier properties due to the precipitation of aggregates in the coating liquid is unlikely to occur.

[0132] <Packaging materials, packages and packaged articles> A packaging material according to an embodiment of the present invention includes the gas barrier laminate described above. This packaging material is used, for example, in the production of a package for packaging an article.

[0133] A package according to an embodiment of the present invention includes the above-described packaging material. This package may be made of the above-mentioned packaging material, or may include the above-mentioned packaging material and other members. In the former case, the package may be, for example, the above-mentioned packaging material formed into a bag shape. In the latter case, the package may be, for example, a container including the above-mentioned packaging material as a lid and a cylindrical container body with a bottom.

[0134] In this package, the packaging material may be a molded product. As described above, this molded product may be a container such as a bag, or a part of a container such as a lid. Specific examples of the package or a part thereof include a bag, a spouted pouch, a laminated tube, an infusion bag, a container lid, and a paper container.

[0135] There is no particular limitation on the application of this packaging material, and this packaging material can be used to package various items.

[0136] A packaging article according to an embodiment of the present invention includes the above-described package and contents contained therein.

[0137] As described above, the gas barrier laminate has excellent gas barrier properties. Therefore, the packaging material and package containing this gas barrier laminate are preferably used as packaging materials and packages for items that are easily deteriorated by the influence of oxygen and water vapor, and particularly as packaging materials and packages for food. These packaging materials and packages are also preferably used as packaging materials and packages for packaging chemicals such as agricultural chemicals and medicines, medical equipment, machine parts, and industrial materials such as precision materials.

[0138] The gas barrier laminate does not deteriorate in gas barrier properties or interlayer adhesion when subjected to heat sterilization such as boiling or retort treatment, and tends to improve the gas barrier properties or interlayer adhesion. Therefore, the packaging material and the packaging body may be a packaging material for heat sterilization and a packaging body for heat sterilization, respectively.

[0139] The packaging material for heat sterilization and the package for heat sterilization are used for packaging articles that are to be subjected to a heat sterilization treatment after packaging. Examples of products that are subjected to heat sterilization treatment after packaging include food products such as curry, stew, soup, sauce, and processed meat products.

[0140] Examples of the heat sterilization treatment include boiling and retort treatment. Boiling is a moist heat sterilization process for preserving food and the like. In boiling, a packaged article in which the contents such as food are packaged in the above-mentioned package is usually subjected to moist heat sterilization at atmospheric pressure at a temperature of 60 to 100°C for 10 to 120 minutes, although this depends on the contents. Boiling is usually performed using a hot water bath. There are two types of boiling: a batch type in which the packaged article is immersed in a hot water bath at a constant temperature and removed after a certain time, and a continuous type in which the packaged article is sterilized by passing it through a hot water bath in a tunnel style.

[0141] Retort processing is a process for sterilizing microorganisms such as mold, yeast, and bacteria by pressurizing and heating in order to generally preserve food, etc. In retort processing, a packaged article in which food is packaged in the above-mentioned package is usually subjected to pressurized sterilization and heating treatment at a pressure of 0.15 to 0.3 MPa and a temperature of 105 to 140° C. for 10 to 120 minutes. Retort devices include a steam type that uses heated steam and a hot water type that uses pressurized superheated water, and they are used appropriately depending on the sterilization conditions of the food, etc., that is the content. EXAMPLES

[0142] Specific examples of the present invention are described below. (Example 1) The carboxyl group-containing polymer (A) was dissolved in 2-propanol by heating. As the carboxyl group-containing polymer (A), polyacrylic acid (AC-10LP, manufactured by Toa Gosei Co., Ltd.) having a number average molecular weight of 50,000 was used. In this manner, a polymer solution (I) was prepared that contained the carboxyl group-containing polymer (A) at a concentration of 10% by mass and had a pH in the range of 4 to 5 at 25°C. Hereinafter, this polymer solution (I) is referred to as "polymer solution 1."

[0143] A high molecular weight dispersant (C) having an acidic group was dissolved in 2-propanol. As the high molecular weight dispersant (C), a polyether phosphate ester (Disparlon (registered trademark) DA-375, manufactured by Kusumoto Chemical Industries Co., Ltd., solid content 100 mass %) was used. Next, polyvalent metal-containing particles (B) were added thereto and stirred. As the polyvalent metal-containing particles (B), zinc oxide (FINEX (registered trademark)-30, manufactured by Sakai Chemical Industry Co., Ltd.) with an average primary particle diameter of 35 nm was used.

[0144] The obtained liquid was subjected to a dispersion treatment for 1 hour using a planetary ball mill (P-7 manufactured by Fritsch). Zirconia beads with a diameter of 0.2 mm were used for this dispersion treatment. The beads were then sieved from this liquid, and the pH was adjusted using an inorganic acid. In this manner, a polyvalent metal dispersion liquid (II) was obtained, which contains polyvalent metal-containing particles (B) at a concentration of 30% by mass, contains high molecular weight dispersant (C) in an amount of 10 parts by mass per 100 parts by mass of polyvalent metal-containing particles (B), and has a pH of 4 at 25°C. Hereinafter, this polyvalent metal dispersion liquid (II) is referred to as "polyvalent metal dispersion liquid 1".

[0145] Next, the polymer solution 1, the polyvalent metal dispersion liquid 1, and 2-propanol were mixed and stirred for 15 minutes to prepare the coating liquid 1. In this coating liquid 1, the ratio of the product of the number of moles of zinc and the valence to the number of moles of carboxyl groups contained in the polyacrylic acid, that is, the equivalent ratio, was set to 1.0. This coating liquid 1 had a pH of 5.1 at 25°C. In addition, this coating liquid 1 had a water content of 50,000 ppm or less in mass fraction.

[0146] This coating liquid 1 was left to stand at a temperature of 25°C for 8 hours after its production. Then, this coating liquid 1 was applied to one side of a biaxially stretched polyethylene terephthalate film (Lumirror (registered trademark) P60, manufactured by Toray Film Processing Co., Ltd., thickness 12 μm) using a bar coater (ROD No. 8, manufactured by Yasuda Seiki Seisakusho Co., Ltd., wet film thickness 20 μm). This coating film was dried in an oven at 50°C for 1 minute to form a coating layer. In this manner, a laminate 1 was obtained.

[0147] Next, an unstretched polypropylene film (ZK93-FM, 60 μm thick, manufactured by Toray Film Processing Co., Ltd.) was dry laminated onto the surface of the coating layer side of the laminate 1 via a two-component polyurethane adhesive (Takelac A-525 / Takenate A-52, manufactured by Mitsui Chemicals, Inc.), and aging was performed at 40°C for 3 days to obtain laminate film 1.

[0148] (Example 2) Polyvalent metal dispersion liquid 2 was prepared in the same manner as described above for polyvalent metal dispersion liquid 1, except that, as the high molecular weight dispersant (C) having an acidic group, a polyether phosphate ester amine (Disparlon (registered trademark) DA-325, manufactured by Kusumoto Chemical Industries, Ltd., 100% solids content) was used instead of a polyether phosphate ester (Disparlon (registered trademark) DA-375, manufactured by Kusumoto Chemical Industries, Ltd., 100% solids content) and the amount of high molecular weight dispersant (C) per 100 parts by mass of polyvalent metal-containing particles (B) was changed from 10 parts by mass to 15 parts by mass.

[0149] Next, Coating Liquid 2 was prepared in the same manner as described above for Coating Liquid 1, except that Polyvalent Metal Dispersion Liquid 2 was used instead of Polyvalent Metal Dispersion Liquid 1. This Coating Liquid 2 had a pH of 4.9 at 25°C.

[0150] Next, a laminate 2 was obtained in the same manner as described above for the laminate 1, except that this coating liquid 2 was used instead of the coating liquid 1. Then, a laminate film 2 was obtained in the same manner as described above for the laminate film 1, except that this laminate 2 was used instead of the laminate 1.

[0151] (Example 3) Polyvalent metal dispersion liquid 3 was prepared in the same manner as described above for polyvalent metal dispersion liquid 1, except that a polyether phosphate amine (Disparlon (registered trademark) DA-325, manufactured by Kusumoto Chemical Industries, Ltd., solid content 100% by mass) was used as the high molecular weight dispersant (C) having an acidic group instead of a polyether phosphate ester (Disparlon (registered trademark) DA-375, manufactured by Kusumoto Chemical Industries, Ltd., solid content 100% by mass).

[0152] Next, Coating Liquid 3 was prepared in the same manner as described above for Coating Liquid 1, except that Polyvalent Metal Dispersion Liquid 3 was used instead of Polyvalent Metal Dispersion Liquid 1. This Coating Liquid 3 had a pH of 4.5 at 25°C.

[0153] Next, a laminate 3 was obtained in the same manner as described above for the laminate 1, except that this coating liquid 3 was used instead of the coating liquid 1. Then, a laminate film 3 was obtained in the same manner as described above for the laminate film 1, except that this laminate 3 was used instead of the laminate 1.

[0154] (Example 4) Polyvalent metal dispersion liquid 4 was prepared in the same manner as described above for polyvalent metal dispersion liquid 1, except that a polyether phosphate amine (Disparlon (registered trademark) DA-325, manufactured by Kusumoto Chemical Industries, Ltd., solid content 100% by mass) was used as the high molecular weight dispersant (C) having an acidic group instead of a polyether phosphate ester (Disparlon (registered trademark) DA-375, manufactured by Kusumoto Chemical Industries, Ltd., solid content 100% by mass), and the amount of high molecular weight dispersant (C) per 100 parts by mass of polyvalent metal-containing particles (B) was changed from 10 parts by mass to 30 parts by mass.

[0155] Next, Coating Liquid 4 was prepared in the same manner as described above for Coating Liquid 1, except that Polyvalent Metal Dispersion Liquid 4 was used instead of Polyvalent Metal Dispersion Liquid 1. This Coating Liquid 4 had a pH of 5.2 at 25°C.

[0156] Next, a laminate 4 was obtained in the same manner as described above for the laminate 1, except that this coating liquid 4 was used instead of the coating liquid 1. Then, a laminate film 4 was obtained in the same manner as described above for the laminate film 1, except that this laminate 4 was used instead of the laminate 1.

[0157] (Example 5: Comparative Example) Polyvalent metal dispersion liquid 5 was prepared in the same manner as described above for polyvalent metal dispersion liquid 1, except that the high molecular weight dispersant (C) was omitted and pH adjustment with inorganic acid was not performed. Next, coating liquid 5 was prepared in the same manner as described above for coating liquid 1, except that polyvalent metal dispersion liquid 5 was used instead of polyvalent metal dispersion liquid 1. This coating liquid 5 caused precipitation of aggregates immediately after preparation. Therefore, the production of a laminate and a laminate film using coating liquid 5 was not performed.

[0158] (Example 6: Comparative Example) Polyvalent metal dispersion liquid 6 was prepared in the same manner as described above for polyvalent metal dispersion liquid 1, except that, as the high molecular weight dispersant (C) having an acidic group, a polyether phosphate amine (Disparlon (registered trademark) DA-325, manufactured by Kusumoto Chemical Industries, Ltd., 100% solids content) was used instead of a polyether phosphate ester (Disparlon (registered trademark) DA-375, manufactured by Kusumoto Chemical Industries, Ltd., 100% solids content), the amount of high molecular weight dispersant (C) relative to 100 parts by mass of polyvalent metal-containing particles (B) was changed from 10 parts by mass to 15 parts by mass, and the pH was adjusted to 2.5 instead of 4 with an inorganic acid.

[0159] Next, Coating Liquid 6 was prepared in the same manner as described above for Coating Liquid 1, except that Polyvalent Metal Dispersion Liquid 6 was used instead of Polyvalent Metal Dispersion Liquid 1. This Coating Liquid 6 had a pH of 3.1 at 25°C.

[0160] Immediately after preparation, the coating solution 6 caused precipitation of aggregates, and therefore, no laminate or laminate film was produced using the coating solution 6.

[0161] (Example 7: Comparative Example) Polyvalent metal dispersion liquid 7 was prepared in the same manner as described above for polyvalent metal dispersion liquid 1, except that a polyether phosphate amine (Disparlon (registered trademark) DA-325, manufactured by Kusumoto Chemical Industries, Ltd., 100% solids content) was used as the high molecular weight dispersant (C) having an acidic group instead of a polyether phosphate ester (Disparlon (registered trademark) DA-375, manufactured by Kusumoto Chemical Industries, Ltd., 100% solids content), the amount of high molecular weight dispersant (C) per 100 parts by mass of polyvalent metal-containing particles (B) was changed from 10 parts by mass to 15 parts by mass, and no pH adjustment was performed with an inorganic acid.

[0162] Next, Coating Liquid 6 was prepared in the same manner as described above for Coating Liquid 1, except that Polyvalent Metal Dispersion Liquid 7 was used instead of Polyvalent Metal Dispersion Liquid 1. This Coating Liquid 7 had a pH of 6.2 at 25°C.

[0163] Next, laminate 7 was obtained in the same manner as described above for laminate 1, except that this coating liquid 7 was used instead of coating liquid 1. Then, laminate film 7 was obtained in the same manner as described above for laminate film 1, except that this laminate 7 was used instead of laminate 1.

[0164] (Example 8: Comparative Example) Polyvalent Metal Dispersion Liquid 8 was prepared in the same manner as described above for Polyvalent Metal Dispersion Liquid 1, except that the pH was not adjusted with an inorganic acid.

[0165] Next, Coating Liquid 8 was prepared in the same manner as described above for Coating Liquid 1, except that Polyvalent Metal Dispersion Liquid 8 was used instead of Polyvalent Metal Dispersion Liquid 1. This Coating Liquid 8 had a pH of 6.4 at 25°C.

[0166] Next, a laminate 8 was obtained in the same manner as described above for the laminate 1, except that this coating liquid 8 was used instead of the coating liquid 1. Then, a laminate film 8 was obtained in the same manner as described above for the laminate film 1, except that this laminate 8 was used instead of the laminate 1.

[0167] (Example 9) Polymer solution 9, having a pH value in the range of 4 to 5 at 25° C., was prepared in the same manner as described above for polymer solution 1, except that polyacrylic acid having a number average molecular weight of 250,000 (AC-10LHP, manufactured by Toa Gosei Co., Ltd.) was used as the carboxy group-containing polymer (A) instead of polyacrylic acid having a number average molecular weight of 50,000 (AC-10LP, manufactured by Toa Gosei Co., Ltd.).

[0168] Next, Coating Liquid 9 was prepared in the same manner as described above for Coating Liquid 2, except that Polymer Solution 9 was used instead of Polymer Solution 1. This Coating Liquid 9 had a pH of 5.5 at 25°C.

[0169] Next, a laminate 9 was obtained in the same manner as described above for the laminate 1, except that this coating liquid 9 was used instead of the coating liquid 1. Then, a laminate film 9 was obtained in the same manner as described above for the laminate film 1, except that this laminate 9 was used instead of the laminate 1.

[0170] (Example 10) Polymer solution 10 having a pH in the range of 4 to 5 at 25°C was prepared in the same manner as described above for polymer solution 1, except that polyacrylic acid having a number average molecular weight of 5,000 (polyacrylic acid 5,000 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the carboxy group-containing polymer (A) instead of polyacrylic acid having a number average molecular weight of 50,000 (AC-10LP manufactured by Toa Gosei Co., Ltd.).

[0171] Next, coating liquid 10 was prepared in the same manner as described above for coating liquid 2, except that polymer solution 10 was used instead of polymer solution 1. This coating liquid 10 had a pH of 4.8 at 25°C.

[0172] Next, a laminate 10 was obtained in the same manner as described above for the laminate 1, except that this coating liquid 10 was used instead of the coating liquid 1. Then, a laminate film 10 was obtained in the same manner as described above for the laminate film 1, except that this laminate 10 was used instead of the laminate 1.

[0173] [Rating 1] (1) Haze of coating liquid The haze of each coating solution immediately after preparation was measured using NDH2000 manufactured by Nippon Denshoku Industries Co., Ltd., which complies with JIS K7136:2000. Note that the haze of Coating Solutions 6 and 7 was not measured because precipitation occurred immediately after preparation. The results are shown in Tables 1 to 3 below.

[0174] (2) Stability of the coating solution Immediately after preparation, each coating solution was visually observed and its stability was evaluated according to the following criteria. The results are shown in Tables 1 to 3 below.

[0175] AA: No precipitation was observed one day after preparation. A: No precipitation occurred 8 hours after preparation, but precipitation occurred after 1 day. B: No precipitate was observed 2 hours after preparation, but a precipitate was observed 4 hours after preparation. C: Precipitation occurred immediately after preparation.

[0176] (2) Oxygen permeability of laminated film A film piece was cut out from each of the laminate films, and the oxygen permeability thereof was measured by the following procedure.

[0177] That is, the oxygen permeability of each laminate was measured under conditions of a temperature of 30° C. and a relative humidity of 70% using an oxygen permeability tester OXTRAN (registered trademark) 2 / 20 manufactured by Modern Control Co., Ltd. The measurement method was in accordance with JIS K-7126 B method (constant pressure method) and ASTM D3985, and the measurement value is in the unit of cm 3 / (m 2 The pressure is expressed in units of MPa.

[0178] Next, two pieces of film measuring 20 cm x 15 cm were cut out from each laminate film, and these were stacked with the unstretched polypropylene films facing each other, and three sides were sealed to create a pouch. 200 mL of water was poured into this pouch, and the remaining side was sealed.

[0179] The obtained water-filled pouch was subjected to a retort treatment at 120° C. for 30 minutes using a retort treatment machine (RCS-60 manufactured by Hisaka Works, Ltd.).

[0180] After the retort treatment, the water was removed, and the oxygen permeability of each laminate film was measured in the same manner as above. The results are shown in Tables 1 to 3.

[0181] [Table 1]

[0182] [Table 2]

[0183] [Table 3]

[0184] As shown in Tables 1 to 3, Coating Liquids 1 to 4, 9 and 10 were superior in stability to Coating Liquids 5 to 8. When a high molecular weight dispersant not containing an acidic group was used, the stability of the coating liquid was equivalent to that of Examples 5 and 6.

[0185] Furthermore, the laminate films 1 to 4, 9 and 10 obtained using the coating liquids 1 to 4, 9 and 10 had lower oxygen permeability and better gas barrier properties after retort treatment compared to the laminate films 7 and 8 obtained using the coating liquids 7 and 8.

[0186] [Rating 2] The first average particle diameter D1 of the coating liquid 2 was measured immediately after its preparation. Then, the coating liquid was left to stand for 8 hours at a temperature of 25°C, and the second average particle diameter D2 was measured. These average particle diameters were measured using Nanotrac UPA-EX150 manufactured by Microtrackbell. As a result, the ratio D2 / D1 of the second average particle diameter D2 to the first average particle diameter D1 was 0.9.

[0187] The same measurement was also carried out for the coating liquid 7. As a result, the ratio D2 / D1 of the second average particle diameter D2 to the first average particle diameter D1 was 4.8. Furthermore, the same measurement as above was also carried out for the coating liquid 9. As a result, the ratio D2 / D1 of the second average particle diameter D2 to the first average particle diameter D1 was 1.2.

[0188] Thus, the coating liquids evaluated as having excellent stability by visual observation were less likely to aggregate even when left for a long period of time, compared with the coating liquids evaluated as having insufficient stability by visual observation. The invention as originally claimed is set forth below. [1] A coating liquid for producing a gas barrier laminate, comprising a carboxyl group-containing polymer (A), polyvalent metal-containing particles (B), a high molecular weight dispersing agent having an acidic group (C), and an organic solvent (D), and having a pH at 25°C within the range of 4 to 6. [2] 2. The coating liquid according to item 1, wherein the polyvalent metal of the polyvalent metal-containing particles (B) is a divalent metal. [3] 3. The coating liquid according to item 1 or 2, wherein the polyvalent metal-containing particles (B) contain zinc oxide. [4] 4. The coating liquid according to any one of items 1 to 3, wherein the high molecular weight dispersant (C) contains a polyether phosphate ester. [5] 5. The coating liquid according to any one of items 1 to 4, wherein the amount of the high molecular weight dispersant (C) is in the range of 1 to 30 parts by mass relative to 100 parts by mass of the polyvalent metal-containing particles (B). [6] 6. The coating liquid according to any one of Items 1 to 5, wherein the carboxyl group-containing polymer (A) has a number average molecular weight in the range of 5,000 to 50,000. [7] 7. The coating liquid according to any one of items 1 to 6, wherein the water content is 50,000 ppm or less in terms of mass fraction. [8] 8. The coating liquid according to any one of items 1 to 7, wherein a ratio of a product (Bt) of a molar number and a valence of a polyvalent metal contained in the polyvalent metal-containing particle (B) to a molar number (At) of a carboxy group contained in the carboxy group-containing polymer (A) is 0.6 or more. [9] 9. The coating liquid according to any one of items 1 to 8, wherein, when a first average particle diameter D1 immediately after production and a second average particle diameter D2 are measured after 8 hours from production under a temperature condition of 25° C., a ratio D2 / D1 of the second average particle diameter D2 to the first average particle diameter D1 is within a range of 0.8 to 1.3.

[10] 10. A gas barrier laminate comprising a cured film of the coating liquid according to any one of items 1 to 9 as a coating layer.

[11] The thickness is within the range of 0.01 to 100 μm, and the oxygen permeability measured under the conditions of 30°C and 70% relative humidity is 1,000 cm 3 / (m 2 Item 11. The gas barrier laminate according to item 10, wherein the gas barrier layer is 0.1·day·MPa or less.

[12] Item 12. A packaging material comprising the gas barrier laminate according to item 10 or 11.

[13] Item 13. A package comprising the packaging material according to item 12.

[14] Item 13. A packaging body according to item 13, The contents contained in the package; A packaged article including:

[15] Mixing the polymer solution (I) and the polyvalent metal dispersion liquid (II) to obtain a mixed liquid having a pH in the range of 4 to 6 at 25°C; The polymer solution (I) contains a carboxy group-containing polymer (A) and an organic solvent (D), The polyvalent metal dispersion (II) contains polyvalent metal-containing particles (B), a high molecular weight dispersing agent having an acidic group (C), and an organic solvent (D), and the method for producing a coating liquid for producing a gas barrier laminate.

[16] Item 16. The method according to item 15, wherein the polymer solution (I) has a pH in the range of 3 to 7 at 25° C., and the polyvalent metal dispersion liquid (II) has a pH in the range of 3 to 7 at 25° C.

[17] Item 17. A method for producing a gas barrier laminate, comprising: producing the coating liquid by the method according to item 15 or 16; and forming a coating layer from the coating liquid.

[18] Item 10. A method for producing a gas barrier laminate, comprising forming a coating layer from the coating liquid according to any one of items 1 to 9.

Claims

1. A coating liquid for producing a gas barrier laminate, comprising: a carboxyl group-containing polymer (A); polyvalent metal-containing particles (B) containing an oxide of a polyvalent metal; a high molecular weight dispersing agent having a phosphate group (C); and an organic solvent (D); and having a pH at 25°C in the range of 4 to 6.

2. 2. The coating liquid according to claim 1, wherein the polyvalent metal of the polyvalent metal-containing particles (B) is a divalent metal.

3. The coating liquid according to claim 1 or 2, wherein the polyvalent metal-containing particles (B) contain zinc oxide.

4. The coating liquid according to claim 1 , wherein the high molecular weight dispersant (C) contains a polyether phosphate ester.

5. 5. The coating liquid according to claim 1, wherein the amount of the high molecular weight dispersant (C) is in the range of 1 to 30 parts by mass when the amount of the polyvalent metal-containing particles (B) is 100 parts by mass.

6. 6. The coating liquid according to claim 1, wherein the carboxyl group-containing polymer (A) has a number average molecular weight in the range of 5,000 to 50,000.

7. 7. The coating liquid according to claim 1, which has a water content of 50,000 ppm or less in terms of mass fraction.

8. 8. The coating liquid according to claim 1, wherein a ratio of a product (Bt) of the number of moles and a valence of the polyvalent metal contained in the polyvalent metal-containing particles (B) to a number of moles (At) of the carboxy groups contained in the carboxy group-containing polymer (A) is 0.6 or more.

9. 9. The coating liquid according to claim 1, wherein, when a first average particle diameter D1 immediately after production and a second average particle diameter D2 are measured at a time when 8 hours have passed since production under a temperature condition of 25° C., a ratio D2 / D1 of the second average particle diameter D2 to the first average particle diameter D1 is within a range of 0.8 to 1.

3.

10. A gas barrier laminate comprising a cured film of the coating liquid according to claim 1 as a coating layer.

11. The thickness is within the range of 0.01 to 100 μm, and the oxygen permeability measured under the conditions of 30° C. and 70% relative humidity is 1,000 cm 3 / (m 2 11. The gas barrier laminate according to claim 10, wherein the gas barrier strength is 100% or less.

12. A packaging material comprising the gas barrier laminate according to claim 10 or 11.

13. A package comprising the packaging material of claim 12.

14. A packaging body according to claim 13; The contents contained in the package; A packaged article including:

15. The method includes mixing the polymer solution (I) and the polyvalent metal dispersion liquid (II) to obtain a mixed liquid having a pH of 4 to 6 at 25° C., The polymer solution (I) contains a carboxy group-containing polymer (A) and an organic solvent (D), The polyvalent metal dispersion (II) is a method for producing a coating liquid for producing a gas barrier laminate, the coating liquid comprising polyvalent metal-containing particles (B) containing an oxide of a polyvalent metal, a high molecular weight dispersing agent (C) having a phosphate group, and an organic solvent (D).

16. 16. The method according to claim 15, wherein the polymer solution (I) has a pH in the range of 3 to 7 at 25° C., and the polyvalent metal dispersion liquid (II) has a pH in the range of 3 to 7 at 25° C.

17. A method for producing a gas barrier laminate, comprising: producing the coating liquid by the method according to claim 15 or 16; and forming a coating layer from the coating liquid.

18. A method for producing a gas barrier laminate, comprising forming a coating layer from the coating liquid according to claim 1 .

Citation Information

Patent Citations

  • Gas-barrier resin composition and film

    JP1994093133A

  • Film with gas barrier property and manufacture thereof

    JP2000289154A

  • Gas barrier film and its production

    JP2000336195A

  • Coating agent having gas barrierness and film

    JP2001323204A

  • Gas barrier coating agent, gas barrier film prepared therefrom, and method for preparing same

    JP2002020677A