Highly adhesive polyamide film
A biaxially oriented polyamide film with biomass-derived resin and an adhesion-modifying layer addresses bending and friction pinhole resistance and adhesive strength issues, ensuring durable and tear-resistant packaging.
Patent Information
- Application Number
- JP2020555087
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-25
- Filing Date
- 2020-06-11
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-06-11
AI Technical Summary
Existing polyamide films face challenges in achieving both bending and friction pinhole resistance while maintaining excellent adhesive strength with sealant films, and conventional methods using polyamide elastomers lead to deterioration and production inefficiencies.
A biaxially oriented polyamide film containing 99 to 70% polyamide 6 resin and 1 to 30% biomass-derived polyamide resin, with an adhesion-modifying layer made of polyester, polyurethane, or polyacrylic resin, ensuring excellent impact resistance, bending and friction pinhole resistance, and high adhesive strength.
The film achieves long-term continuous production without die deterioration, provides high lamination strength, and prevents tearing, especially under water-resistant conditions, making it suitable for packaging applications.
Smart Images

Figure 0007581879000006 
Figure 0007581879000001 
Figure 0007581879000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon-neutral, easily adhesive polyamide film using a biomass-derived raw material, which has excellent impact resistance, resistance to pinholes due to bending, and resistance to pinholes due to friction, and also has excellent water-resistant adhesive strength with a sealant film. The easily adhesive polyamide film of the present invention is suitable for use as a food packaging film or the like. [Background technology]
[0002] Biaxially oriented films made of aliphatic polyamides, such as polyamide 6, have been widely used as various packaging film materials due to their excellent impact resistance and pinhole resistance.
[0003] Additionally, for liquid-filled packaging of soup, seasonings, and the like, biaxially oriented polyamide films that have been mixed with various elastomers (rubber components) to further improve resistance to pinholes caused by bending and impact resistance are widely used, making them more flexible and improving pinhole resistance.
[0004] As a means for improving the above-mentioned pinhole resistance due to bending, a film in which a polyamide-based elastomer is mixed with an aliphatic polyamide is known (see, for example, Patent Document 1). This film has good pinhole resistance due to bending and impact resistance in a low-temperature environment, and is less likely to develop pinholes due to bending fatigue even in a low-temperature environment.
[0005] However, pinholes are generated not only by bending but also by friction (abrasion). Methods for improving pinholes caused by bending and pinholes caused by friction are often contradictory. For example, increasing the flexibility of a film makes it less likely for pinholes to occur due to bending, but the softer the film is, the more likely it is that pinholes caused by friction will occur. In response to this, a packaging laminate has been proposed that has excellent resistance to bending and pinholes caused by friction by providing a surface coating agent on the outer surface of a biaxially oriented polyamide film (see, for example, Patent Document 2). However, this method is not very effective at preventing pinholes caused by friction. In addition, a coating process is required. Furthermore, in the case of a film made by mixing aliphatic polyamide with a polyamide-based elastomer, the polyamide-based elastomer added during film production is thermally degraded, and a degraded material called "pit jelly" is easily generated at the exit of the die lip. It was found that the degraded material causes a deterioration in the accuracy of the film thickness. In addition, the degraded material itself falls off, resulting in defective products, which reduces the production efficiency during continuous film production.
[0006] Furthermore, when a film obtained by laminating a polyamide film with a sealant film is used for liquid soup bags or water bags, the adhesive strength between the laminated films (also called lamination strength) must be sufficiently high.
[0007] Meanwhile, in recent years, the use of biomass as an alternative to fossil fuels as a raw material has been attracting attention in the field of materials in order to build a recycling-oriented society. Biomass is an organic compound that is photosynthesized from carbon dioxide and water, and by using it, it becomes carbon dioxide and water again, making it a so-called carbon-neutral raw material (the amount of carbon dioxide emitted and absorbed in the environment is the same, so the increase in carbon dioxide, a greenhouse gas, can be suppressed). Recently, the practical application of biomass plastics made from these biomass raw materials has progressed rapidly, and there are also attempts to produce polyester, a general-purpose polymer material, from these biomass raw materials.
[0008] For example, Patent Document 3 discloses, in the field of polyester films, a resin composition comprising a polyester composed of diol units and dicarboxylic acid units, the diol component unit being ethylene glycol derived from biomass and the dicarboxylic acid component unit being a dicarboxylic acid derived from petroleum, and the resin composition and film are characterized in that the resin composition contains 50 to 95 mass% of the polyester based on the total mass of the resin composition. According to this technology, even if a polyester is produced using ethylene glycol derived from biomass instead of ethylene glycol obtained from conventional fossil fuels, the polyester can have mechanical properties equivalent to those of a polyester produced using ethylene glycol derived from conventional fossil fuels. Against this background, there is a demand for carbon-neutral polyamide films made from raw materials derived from biomass. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 11-254615 [Patent Document 2] JP 2001-205761 A [Patent Document 3] JP 2012-097163 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in view of the problems of the conventional technology. An object of the present invention is to provide a carbon-neutral, easily adhesive biaxially oriented polyamide film using raw materials derived from biomass, which has excellent impact resistance, bending pinhole resistance, and abrasion pinhole resistance, and also has excellent water-resistant adhesive strength with a sealant film. [Means for solving the problem]
[0011] That is, the present invention comprises the following: [1] A biaxially oriented polyamide film containing 99 to 70% by mass of polyamide 6 resin and 1 to 30% by mass of polyamide resin at least partly derived from biomass, with a coating amount of 0.01 to 3 g / m2 as solid content on at least one side of the film. 2 1. An easily adhesive polyamide film, comprising an adhesion modifying layer made of any one of a polyester resin, a polyurethane resin, and / or a polyacrylic resin. [2] A coating amount of 0.01 to 3 g / m2 as a solid content is applied to at least one side of a biaxially oriented polyamide film having the following functional layer (B layer) laminated on at least one side of the following base layer (A layer). 2 1. An easily adhesive polyamide film, comprising an adhesion modifying layer made of any one of a polyester resin, a polyurethane resin, and / or a polyacrylic resin. The base layer (A layer) contains 99 to 70 mass % polyamide 6 resin and 1 to 30 mass % polyamide resin at least partly derived from biomass, and the functional layer (B layer) contains 70 mass % or more polyamide 6 resin. [3] The radioactive carbon (C) relative to the total carbon in the biaxially oriented polyamide film 14 ) is 1 to 15% by mass-derived carbon content. [4] The highly adhesive polyamide film according to any one of [1] to [3], wherein the polyamide resin, at least a part of which is derived from biomass as a raw material, is at least one polyamide resin selected from the group consisting of polyamide 11, polyamide 410, polyamide 610, and polyamide 1010. [5] The highly adhesive polyamide film according to any one of [1] to [4], which satisfies the following (a) and (b): (a) The number of Gelbo pinhole defects is 10 or less when a twisting and bending test using a Gelbo flex tester is performed 1,000 times at a temperature of 1°C. (b) In the abrasion pinhole resistance test, the distance until pinholes appear is 2,900 cm or more. [6] The highly adhesive polyamide film according to any one of [1] to [5], characterized in that the laminate strength after being attached to a polyethylene sealant film is 4.0 N / 15 mm or more. [7] A laminate film obtained by laminating a sealant film onto the highly adhesive polyamide film according to any one of [1] to [6]. [8] [7] A packaging bag using the laminated film described in [7]. Effect of the Invention
[0012] The highly adhesive polyamide film of the present invention is made primarily of polyamide 6 resin, and by blending it with a polyamide resin polymerized from a specific biomass-derived raw material and adopting specific film-forming conditions, it is possible to obtain a polyamide film that exhibits impact resistance, flexure pinhole resistance, abrasion pinhole resistance, and adhesion to sealant films, as well as being carbon-neutral. Furthermore, unlike conventional polyamide-based elastomers added to improve pinhole resistance, the polyamide-based elastomer in the present invention does not deteriorate inside the die, so adhesion of deteriorated materials to the inner surface of the die and adhesion of resin to the outlet of the die lip can be suppressed for a long period of time, thereby preventing the thickness unevenness of the film from worsening. In addition, if deteriorated materials adhere to the inner surface of the die or the outlet of the die lip, the thickness unevenness worsens, so production must be stopped and the die lip must be cleaned. The highly adhesive polyamide film of the present invention enables long-term continuous production. Furthermore, the coating amount as a solid content is 0.01 to 3 g / m on at least one side of the biaxially oriented polyamide film. 2By laminating an adhesive modifying layer made of any one of polyester resin, polyurethane resin, and / or polyacrylic resin, when the sealant film and the laminated film are used for liquid soup bags or liquid food bags, the adhesive strength (also called lamination strength) between the laminated films is high, so that a packaging bag with less tearing can be provided. In particular, since the water-resistant lamination strength (lamination strength under water adhesion conditions) is high, a packaging bag with less tearing can be provided even when used for boiling treatment or retort treatment. [Brief description of the drawings]
[0013] [Figure 1] Schematic diagram of a friction pinhole resistance evaluation device [Explanation of symbols]
[0014] 1: Head of fastness tester 2:Corrugated cardboard 3: Mount for holding samples 4: Film sample folded in four 5: Rubbing amplitude direction DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The highly adhesive polyamide film of the present invention will be described in detail below. The highly adhesive polyamide film of the present invention is a biaxially stretched polyamide film comprising 99 to 70 mass% polyamide 6 resin and 1 to 30 mass% polyamide resin at least part of which is derived from biomass, or a biaxially stretched polyamide film comprising a base layer (A layer) comprising 99 to 70 mass% polyamide 6 resin and 1 to 30 mass% polyamide resin at least part of which is derived from biomass, and a functional layer (B layer) described below laminated on at least one side of the base layer (A layer) comprising 99 to 70 mass% polyamide 6 resin and 1 to 30 mass% polyamide resin at least part of which is derived from biomass, with a coating amount of 0.01 to 3 g / m as a solid content on at least one side of the biaxially stretched polyamide film. 2 The highly adhesive polyamide film is characterized by having an adhesion modifying layer made of any one of polyester resin, polyurethane resin, and / or polyacrylic resin.
[0016] [Biaxially oriented polyamide film or base layer (A layer)] The biaxially oriented polyamide film or base layer (layer A) in the present invention contains 70% by mass or more of polyamide 6 resin, thereby obtaining the excellent mechanical strength such as impact strength and gas barrier properties such as oxygen that are inherent to biaxially oriented polyamide films made of polyamide 6 resin. The biaxially stretched polyamide film or base layer (A layer) in the present invention improves pinhole resistance by containing 1 to 30% by mass of polyamide resin, at least a part of which is derived from biomass. In the case of polyamide-based elastomers and polyolefin-based elastomers, which are conventionally used agents for improving pinhole resistance, pinhole resistance is improved but friction pinhole resistance is deteriorated. By containing 1 to 30% by mass of polyamide resin, at least a part of which is derived from biomass, a biaxially stretched polyamide film having excellent pinhole resistance for bending and pinhole resistance for friction can be obtained. In addition, a carbon-neutral film that is less affected by the increase or decrease in carbon dioxide on the ground can be obtained.
[0017] [Polyamide 6 resin] The polyamide 6 resin used in the present invention is usually produced by ring-opening polymerization of ε-caprolactam. The polyamide 6 resin obtained by ring-opening polymerization is usually subjected to removal of lactam monomer with hot water, followed by drying and melt extrusion in an extruder. The relative viscosity of the polyamide 6 resin is preferably 1.8 to 4.5, and more preferably 2.6 to 3.2. If the relative viscosity is less than 1.8, the impact strength of the film is insufficient. If the relative viscosity is more than 4.5, the load on the extruder increases, making it difficult to obtain an unstretched film before stretching.
[0018] [Polyamide resin made from at least part of biomass-derived raw materials] Examples of the polyamide resin used in the present invention, at least a part of which is derived from biomass, include polyamide 11, polyamide 410, polyamide 610, polyamide 1010, polyamide MXD10 resin, and polyamide 11·6T copolymer resin.
[0019] Polyamide 11 is a polyamide resin having a structure in which monomers having 11 carbon atoms are bonded via amide bonds. Polyamide 11 is usually obtained by using aminoundecanoic acid or undecane lactam as a monomer. In particular, aminoundecanoic acid is a monomer obtained from castor oil, and is therefore desirable from the viewpoint of carbon neutrality. The constituent units derived from these monomers having 11 carbon atoms preferably account for 50% or more of all the constituent units in polyamide 11, more preferably 80% or more, and may even be 100%.
[0020] The polyamide 11 is usually produced by polymerization of the above-mentioned aminoundecanoic acid. The polyamide 11 obtained by polymerization is optionally subjected to removal of lactam with hot water, dried, and then melt-extruded in an extruder. The relative viscosity of polyamide 11 is preferably 1.8 to 4.5, and more preferably 2.4 to 3.2. If the relative viscosity is less than 1.8, the impact strength of the film is insufficient. If the relative viscosity is more than 4.5, the load on the extruder increases, making it difficult to obtain an unstretched film before stretching.
[0021] The polyamide 610 is a polyamide resin having a structure in which a diamine having 6 carbon atoms and a dicarboxylic acid having 10 carbon atoms are polymerized. Usually, hexamethylenediamine and sebacic acid are used. Of these, sebacic acid is a monomer obtained from castor oil, and is therefore desirable from the viewpoint of carbon neutrality. The total of the constituent units derived from these monomers having 6 carbon atoms and the constituent units derived from monomers having 10 carbon atoms in PA610 is preferably 50% or more, more preferably 80% or more, and may be 100% of all the constituent units.
[0022] The above-mentioned polyamide 1010 is a polyamide resin having a structure in which a diamine having 10 carbon atoms and a dicarboxylic acid having 10 carbon atoms are polymerized. Usually, 1,10-decanediamine (decamethylenediamine) and sebacic acid are used in polyamide 1010. Decamethylenediamine and sebacic acid are monomers obtained from castor oil, and are therefore desirable from the viewpoint of carbon neutrality. The total of the structural units derived from these diamines having 10 carbon atoms and the structural units derived from dicarboxylic acids having 10 carbon atoms in PA1010 is preferably 50% or more, more preferably 80% or more, and may be 100% of all the structural units.
[0023] The above-mentioned polyamide 410 is a polyamide resin having a structure in which a monomer having 4 carbon atoms is copolymerized with a diamine having 10 carbon atoms. Usually, sebacic acid and tetramethylenediamine are used for polyamide 410. From an environmental perspective, it is preferable that the sebacic acid is made from castor oil, a vegetable oil. The sebacic acid used here is preferably made from castor oil from the viewpoint of environmental protection (especially from the viewpoint of carbon neutrality).
[0024] In the biaxially stretched polyamide film or base layer (A layer) of the present invention, the upper limit of the content of the polyamide resin at least partly derived from biomass is 30% by mass, more preferably 20% by mass. If the content of the polyamide resin at least partly derived from biomass exceeds 30% by mass, the molten film becomes unstable when cast, making it difficult to obtain a homogeneous unstretched film.
[0025] [Secondary materials, additives] The biaxially oriented polyamide film or base layer (A layer) in the present invention may contain various additives such as other thermoplastic resins, lubricants, heat stabilizers, antioxidants, antistatic agents, antifogging agents, UV absorbers, dyes, pigments, etc., as necessary.
[0026] <Other thermoplastic resins> The biaxially stretched polyamide film or base layer (A layer) in the present invention may contain a thermoplastic resin in addition to the above-mentioned polyamide 6 and polyamide resin at least part of which is derived from biomass, provided that the object of the present invention is not impaired. Examples of such polyamide resins include polyamide 12 resin, polyamide 66 resin, polyamide 6·12 copolymer resin, polyamide 6·66 copolymer resin, and polyamide MXD6 resin. If necessary, thermoplastic resins other than polyamides, for example, polyester polymers such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene-2,6-naphthalate, and polyolefin polymers such as polyethylene and polypropylene, may be contained. It is preferable that the raw materials for these thermoplastic resins are derived from biomass, since they do not affect the increase or decrease in carbon dioxide on the ground and therefore the environmental load can be reduced.
[0027] <Lubricant> In the present invention, the biaxially oriented polyamide film or the base layer (A layer) preferably contains fine particles or an organic lubricant such as a fatty acid amide as a lubricant in order to improve the slipperiness and make it easy to handle. The biaxially oriented polyamide film of the present invention has an effect of reducing breakage of packaging bags due to friction by improving the slipperiness.
[0028] The fine particles can be appropriately selected from inorganic fine particles such as silica, kaolin, zeolite, etc., polymeric organic fine particles such as acrylic and polystyrene, etc. From the viewpoints of transparency and lubricity, it is preferable to use silica fine particles. The average particle size of the fine particles is preferably 0.5 to 5.0 μm, more preferably 1.0 to 3.0 μm. If the average particle size is less than 0.5 μm, a large amount of the fine particles is required to obtain good slip properties. On the other hand, if the average particle size is more than 5.0 μm, the surface roughness of the film tends to become too large, resulting in poor appearance.
[0029] When the silica fine particles are used, the pore volume of the silica is preferably in the range of 0.5 to 2.0 ml / g, more preferably 0.8 to 1.6 ml / g. If the pore volume is less than 0.5 ml / g, voids are likely to occur, resulting in poor transparency of the film, whereas if the pore volume exceeds 2.0 ml / g, the fine particles tend not to form surface protrusions.
[0030] In the present invention, the biaxially stretched polyamide film or the base layer (layer A) may contain fatty acid amide and / or fatty acid bisamide for the purpose of improving the slip property. Examples of fatty acid amide and / or fatty acid bisamide include erucic acid amide, stearic acid amide, ethylene bisstearic acid amide, ethylene bisbehenic acid amide, and ethylene bisoleic acid amide. The content of fatty acid amide and / or fatty acid bisamide in the biaxially stretched polyamide film of the present invention is preferably 0.01 to 0.40% by mass, more preferably 0.05 to 0.30% by mass. If the content of fatty acid amide and / or fatty acid bisamide is less than the above range, the slipping property tends to be deteriorated. On the other hand, if it exceeds the above range, the wettability tends to be deteriorated.
[0031] In the present invention, a polyamide resin such as polyamide MXD6 resin, polyamide 12 resin, polyamide 66 resin, polyamide 6·12 copolymer resin, polyamide 6·66 copolymer resin, etc. can be added to the biaxially stretched polyamide film or base layer (A layer) for the purpose of improving the slip property. In particular, polyamide MXD6 resin is preferred, and it is preferable to add it in an amount of 1 to 10 mass %.
[0032] <Antioxidants> The biaxially oriented polyamide film or the base layer (layer A) in the present invention may contain an antioxidant. The antioxidant is preferably a phenol-based antioxidant. The phenol-based antioxidant is preferably a completely hindered phenol-based compound or a partially hindered phenol-based compound. For example, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 3,9-bis[1,1-dimethyl-2-[β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]2,4,8,10-tetraoxaspiro[5,5]undecane, etc. may be mentioned. By adding the phenol-based antioxidant, the film-forming operability of the biaxially oriented polyamide film is improved. In particular, when using recycled film as a raw material, the resin is prone to thermal degradation, which tends to cause film-forming operational problems and increase production costs. In contrast, by adding an antioxidant, the thermal degradation of the resin is suppressed and the operability is improved.
[0033] [Functional layer (B layer)] In one embodiment of the present invention, a functional layer (layer B) can be laminated on at least one surface of the base layer (layer A) to improve the surface properties. The layer B is a layer containing 70% by mass or more of polyamide 6 resin. Layer B contains 70% by mass or more of polyamide 6 resin, thereby obtaining a biaxially oriented polyamide film having excellent mechanical strength such as impact strength and gas barrier properties such as oxygen. As the polyamide 6 resin, the same polyamide 6 resin as that used in the above-mentioned layer A can be used.
[0034] Layer B may contain various additives such as other thermoplastic resins, lubricants, heat stabilizers, antioxidants, antistatic agents, anti-fogging agents, UV absorbers, dyes, pigments, etc., depending on the functions to be imparted to the surface of layer B. When layer B is used on the outside of a packaging bag, it needs to be resistant to abrasion and pinholes, so it is undesirable to contain soft resins such as polyamide-based elastomers and polyolefin-based elastomers or substances that generate a large amount of voids.
[0035] Layer B may contain a thermoplastic resin other than the above-mentioned polyamide 6, provided that the object of the present invention is not impaired. Examples of such a polyamide resin include polyamide-MXD6 resin, polyamide 11 resin, polyamide 12 resin, polyamide 66 resin, polyamide 6·12 copolymer resin, and polyamide 6·66 copolymer resin. If necessary, thermoplastic resins other than polyamides, for example, polyester polymers such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene-2,6-naphthalate, and polyolefin polymers such as polyethylene and polypropylene, may be contained.
[0036] In order to improve the slipping property of the film, it is preferable that layer B contains fine particles or an organic lubricant as a lubricant. By improving the slipperiness, the film becomes easier to handle and the risk of packaging bags breaking due to friction is reduced.
[0037] The fine particles can be appropriately selected from inorganic fine particles such as silica, kaolin, zeolite, etc., polymeric organic fine particles such as acrylic and polystyrene, etc. From the viewpoints of transparency and lubricity, it is preferable to use silica fine particles.
[0038] The average particle size of the fine particles is preferably 0.5 to 5.0 μm, more preferably 1.0 to 3.0 μm. If the average particle size is less than 0.5 μm, a large amount of the fine particles is required to obtain good slip properties. On the other hand, if the average particle size is more than 5.0 μm, the surface roughness of the film tends to become too large, resulting in poor appearance.
[0039] When the silica fine particles are used, the pore volume of the silica is preferably in the range of 0.5 to 2.0 ml / g, more preferably 0.8 to 1.6 ml / g. If the pore volume is less than 0.5 ml / g, voids are likely to occur, and the transparency of the film is deteriorated. If the pore volume is more than 2.0 ml / g, the fine particles tend not to form surface protrusions.
[0040] The organic lubricant may contain a fatty acid amide and / or a fatty acid bisamide, such as erucic acid amide, stearic acid amide, ethylene bisstearic acid amide, ethylene bisbehenic acid amide, or ethylene bisoleic acid amide. The content of fatty acid amide and / or fatty acid bisamide added to layer B is preferably 0.01 to 0.40% by mass, more preferably 0.05 to 0.30% by mass. If the content of fatty acid amide and / or fatty acid bisamide is less than the above range, the slipping property tends to be deteriorated. On the other hand, if it exceeds the above range, the wettability tends to be deteriorated.
[0041] To improve the slipperiness of the film, polyamide resins other than polyamide 6, such as polyamide MXD6 resin, polyamide 11, polyamide 12 resin, polyamide 66 resin, polyamide 6·12 copolymer resin, polyamide 6·66 copolymer resin, etc., can be added to layer B. Polyamide MXD6 resin is particularly preferred, and it is preferable to add 1 to 10% by mass. If it is less than 1% by mass, the effect of improving the slipperiness of the film is small. If it is more than 10% by mass, the effect of improving the slipperiness of the film becomes saturated. Polyamide MXD6 resin is produced by the polycondensation of metaxylylenediamine and adipic acid. The relative viscosity of polyamide MXD6 is preferably 1.8 to 4.5, and more preferably 2.0 to 3.2. If the relative viscosity is less than 1.8 or more than 4.5, it may be difficult to knead it with the polyamide resin in the extruder.
[0042] When adding fine particles, an organic lubricant, or a polyamide resin such as polyamide-MXD6 resin to layer B for the purpose of improving the slipperiness of the film, it is preferable to reduce the amount of these added to the base layer (layer A), since this results in a film that is excellent in both transparency and slipperiness.
[0043] To improve adhesion, layer B may contain a polyamide resin other than polyamide 6. In this case, copolymer polyamide resins such as polyamide 6·12 copolymer resin and polyamide 6·66 copolymer resin are preferred.
[0044] The layer B of the biaxially oriented polyamide film of the present invention may contain an antioxidant, similar to the layer A.
[0045] In the present invention, the biaxially stretched polyamide film or the base layer (A layer) and the functional layer (B layer) can be added with sub-materials and additives such as lubricants and antioxidants during resin polymerization or melt extrusion in an extruder. A high-concentration master batch can be prepared and added to the polyamide resin during film production. Such known methods can be used.
[0046] [Thickness composition of biaxially oriented polyamide film] The thickness of the biaxially oriented polyamide film in the present invention is not particularly limited, but when used as a packaging material, it is usually 100 μm or less, and a thickness of 5 to 50 μm is generally used, and a thickness of 8 to 30 μm is particularly used.
[0047] In the thickness configuration of each layer of the biaxially stretched polyamide film of the present invention, when the thickness of Layer B accounts for most of the total thickness of the film, the bending pinhole resistance decreases. Therefore, in the present invention, the thickness of Layer A is preferably 50 to 93%, particularly 70 to 93%, of the total thickness of Layer A and Layer B.
[0048] [Adhesion modification layer] The highly adhesive polyamide film of the present invention has a coating amount of 0.01 to 3 g / m2 as a solid content on at least one surface. 2 The adhesive layer is made of any one of polyester resin, polyurethane resin, and / or polyacrylic resin. The adhesion modifying layer is preferably provided by applying a coating liquid to the film and drying it before the film is wound up as a mill roll in the film production process. The coating solution can be applied to an unstretched film, a uniaxially stretched film, and / or a biaxially stretched film. When a film is produced by a sequential biaxial stretching method, the coating solution is usually applied to a uniaxially stretched film and then dried. When a film is produced by a simultaneous biaxial stretching method, the coating solution is usually applied to an unstretched film and then dried.
[0049] In the present invention, the coating solution for providing the adhesion modifying layer is applied and dried to provide a coating film before the film is wound up as a mill roll in the film production process. Therefore, in order to ensure safety and hygiene during production, it is preferable to use an aqueous dispersion of a resin.
[0050] <Polyester resin used in the adhesion modifying layer> When a polyester resin is provided as the adhesion modifying layer in the present invention, a copolymerized polyester resin can be selected as the polyester resin. A copolymerized polyester resin is a polycondensate of a dicarboxylic acid component, a diol component, and other ester forming components. Examples of dicarboxylic acid components contained as constituents in a copolymerized polyester resin include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenylenedicarboxylic acid, and 5-sodium sulfoisophthalic acid, aliphatic dicarboxylic acids such as succinic acid, adipic acid, azelaic acid, and sebacic acid, alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and 1,2-cyclohexanedicarboxylic acid, and unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and tetrahydrophthalic acid.
[0051] In addition to the above dicarboxylic acid components, salts of 5-sulfoisophthalic acid, sulfoterephthalic acid, 4-sulfoisophthalic acid, 4-sulfonaphthalene-2,6-dicarboxylic acid, and 5-(4-sulfophenoxy)isophthalic acid can be used to impart water dispersibility. Among these, it is preferable to use 5-sodium sulfoisophthalic acid in the range of 1 to 10 mol %.
[0052] Examples of the diol component contained in the copolymer polyester resin include aliphatic diols such as ethylene glycol, diethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, and polyethylene glycol; alicyclic diols such as 1,4-cyclohexanedimethal; aromatic diols such as 4,4'-bis(hydroxyethyl)bisphenol A; and bis(polyoxyethylene glycol) bisphenol ether. The polyester resin is preferably used as a coating liquid in the form of an aqueous dispersion.
[0053] In the present invention, when a polyester resin is provided as the adhesion modifying layer, the polyester resin is particularly preferably an acrylic graft copolymer polyester, which will be described later, since it can increase the water-resistant laminate strength.
[0054] <Polyurethane resin used in the adhesion modification layer> In the case where a polyurethane resin is provided as the adhesion modifying layer in the present invention, examples of the polyurethane resin include those obtained by reacting polyols having two or more active hydrogens with an organic polyisocyanate. Examples of polyols include polyols having unsaturated double bonds, such as saturated polyester polyols; polyether polyols (e.g., polyethylene glycol, polytetramethylene glycol, etc.); amino alcohols (e.g., ethanolamine, diethanolamine, triethanolamine, etc.); unsaturated polyester polyols (e.g., those obtained by polycondensation of an unsaturated polyvalent carboxylic acid alone or a mixture of an unsaturated polyvalent carboxylic acid with a mixture of a saturated polyhydric alcohol and an unsaturated polyhydric alcohol), polybutadiene polyols (e.g., 1,2-polybutadiene polyol, 1,4-polybutadiene polyol, etc.), and acrylic polyols (acrylic polyols having hydroxyl groups in the side chains obtained by copolymerizing various acrylic monomers with acrylic acid monomers having hydroxyl groups). Examples of organic polyisocyanates include aromatic polyisocyanates (such as diphenylmethane diisocyanate, toluene diisocyanate, etc.), aliphatic polyisocyanates (such as hexamethylene diisocyanate, etc.), alicyclic polyisocyanates (such as isophorone diisocyanate, etc.), aromatic / aliphatic polyisocyanates (such as xylene diisocyanate), and polyisocyanates obtained by previously reacting these isocyanates with low molecular weight polyols.
[0055] This polyurethane resin can be produced by a known method. During production, it is necessary to ensure that there are two or more unreacted isocyanate groups in the resulting prepolymer. It is preferable to block this isocyanate group, and this blocking is essential, particularly when preparing a water-based coating liquid. This blocking is well known as blocking of isocyanate, and free isocyanate groups can be regenerated by heating. Examples of blocking agents include bisulfites, alcohols, oximes, active methylene compounds, imidazoles, lactams, imine compounds, amide compounds, and imide compounds.
[0056] The reaction between these blocking agents and the isocyanate groups in the polyurethane prepolymer can be carried out at room temperature to 100°C, and a urethanization catalyst can be used as necessary. Here, in order to impart stable water dispersibility and water solubility to the polyurethane prepolymer, it is advisable to introduce a hydrophilic group into the molecule. Examples of the hydrophilic group include -SO3M (where M is an alkali metal or an alkaline earth metal), -OH, -COOR (where R is a residue of ammonia or a tertiary amine). Among these, a carboxyl group neutralized with ammonia or a tertiary amine is particularly preferred. To introduce a carboxyl group neutralized with ammonia or a tertiary amine into the polyurethane prepolymer, for example, there are a method of using a carboxyl group-containing polyhydroxy compound as one of the reaction raw materials during the synthesis of the polyurethane prepolymer, a method of reacting a hydroxyl group-containing carboxylic acid or an amino group-containing carboxylic acid with the isocyanate group of a polyurethane prepolymer having an unreacted isocyanate group, and then adding the reaction product to ammonia water or an aqueous tertiary amine solution under high speed stirring to neutralize it. The polyurethane resin is preferably used in the form of a coating liquid in the form of an aqueous dispersion.
[0057] <Polyacrylic resin used in adhesive modification layer> In the case where a polyacrylic resin is provided as the adhesion modifying layer in the present invention, the polyacrylic resin may be an acrylic polymer obtained by polymerizing acrylic acid or methacrylic acid, or salts or esters thereof. Examples of acrylic acid ester and methacrylic acid ester monomers include methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, glycidyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, 2-hydroxyethyl methacrylate, glycidyl methacrylate, etc. Examples of salts of acrylic acid and methacrylic acid include sodium acrylate, sodium methacrylate, potassium acrylate, potassium methacrylate, ammonium acrylate, ammonium methacrylate, etc. In addition to these essential components, acrylic acid monomers such as acrylamide, methacrylamide, aminoethyl methacrylate, aminomethyl methacrylate, N-methylolacrylamide, and N-methoxymethylacrylamide may be added. In addition, the polyacrylic resin may contain monomers such as vinyl chloride, vinyl acetate, styrene, vinyl ether, butadiene, isoprene, and sodium vinyl sulfonate as copolymerization components. It is preferable that the acrylic polymer contains hydrophilic components such as acrylate components, methacrylate components, acrylic acid components, acrylamide components, 2-hydroxyethyl acrylate components, and N-methylol acrylamide components as copolymerization components in order to enhance the functionality of the coating film. It may also be a copolymer having a functional group in the molecular side chain. The acrylic polymer may also be obtained by using a hard component such as methyl methacrylate or ethyl methacrylate as the main component and copolymerizing a soft component such as an acrylic ester as the copolymerization component. The polyacrylic resin is preferably used in the form of a coating liquid in the form of an aqueous dispersion.
[0058] <Acrylic graft copolymer polyester resin used in adhesion modification layer> In the present invention, when a polyester resin is provided as the adhesion modifying layer, a copolymer polyester obtained by graft-polymerizing a polyacrylic resin onto a polyester resin is particularly preferable, and will be described in detail below. As a coating liquid for forming an adhesion-modifying layer, a water-based dispersion of a copolymer polyester obtained by graft-polymerizing a polyacrylic resin onto a polyester resin is particularly preferred. The average particle size of the acrylic-grafted polyester particles in the aqueous dispersion of the acrylic-grafted polyester copolymer, as measured by a laser light scattering method, is 500 nm or less, preferably 10 nm to 500 nm, and more preferably 10 nm to 300 nm. If the average particle size exceeds 500 nm, the strength of the coating film after coating may decrease.
[0059] The content of the acrylic-grafted polyester particles in the acrylic-grafted polyester aqueous dispersion is usually 1% by mass to 50% by mass, and preferably 3% by mass to 30% by mass. The particles in the aqueous dispersion of the acrylic-grafted copolymerized polyester that can be used in the present invention have a core-shell structure in the aqueous dispersion medium, with the polyester main chain serving as the core.
[0060] The coating film obtained from the above-mentioned acrylic-grafted copolymerized polyester aqueous dispersion has excellent adhesion to polyamide films. Furthermore, since it has excellent blocking resistance, it can be used without problems even on film substrates with relatively low glass transition points. When it is used as a laminate, it also has excellent adhesion to the adhesive used when laminating printing inks or sealant layers. The obtained laminate film (also called laminate film) has significantly improved durability in retort treatment and boiling water treatment.
[0061] (Polyester main chain of acrylic graft copolymer polyester) The polyester that can be used as the main chain of the grafted polyester in the present invention is preferably a saturated or unsaturated polyester synthesized from at least a dicarboxylic acid component and a diol component, and the resulting polyester can be one type of polymer or a mixture of two or more types of polymers. And, a polyester that does not disperse or dissolve in water by itself is preferable. The weight average molecular weight of the polyester that can be used in the present invention is 5000 to 100000, preferably 5000 to 50000. If the weight average molecular weight is less than 5000, the coating film properties such as post-processability of the dried coating film are reduced. Furthermore, if the weight average molecular weight is less than 5000, the polyester that becomes the main chain itself is easily water-soluble, so that the grafted polyester formed cannot form a core-shell structure described later. If the weight average molecular weight of the polyester exceeds 100000, it becomes difficult to disperse in water. From the viewpoint of dispersing in water, it is preferable that it is 100000 or less. The glass transition point is 30°C or less, preferably 10°C or less.
[0062] The dicarboxylic acid component is preferably a dicarboxylic acid mixture containing at least one aromatic dicarboxylic acid, at least one aliphatic and / or alicyclic dicarboxylic acid, and at least one dicarboxylic acid having a radical polymerizable unsaturated double bond. The aromatic dicarboxylic acid contained in this dicarboxylic acid mixture is 30 to 99.5 mol%, preferably 40 to 99.5 mol%, the aliphatic and / or alicyclic dicarboxylic acid is 0 to 70 mol%, preferably 0 to 60 mol%, and the dicarboxylic acid having a radical polymerizable unsaturated double bond is 0.5 to 10 mol%, preferably 2 to 7 mol%, more preferably 3 to 6 mol%. If the content of the dicarboxylic acid containing a radical polymerizable unsaturated double bond is less than 0.5 mol%, it is difficult to effectively graft the radical polymerizable monomer to the polyester, and the dispersed particle size in the aqueous medium tends to increase, and the dispersion stability tends to decrease.
[0063] Examples of aromatic dicarboxylic acids that can be used include terephthalic acid, isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, biphenyldicarboxylic acid, etc. Furthermore, sodium 5-sulfoisophthalate can also be used if necessary. Examples of the aliphatic dicarboxylic acid that can be used include succinic acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, dimer acid, and acid anhydrides thereof. As the alicyclic dicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, and acid anhydrides thereof can be used.
[0064] As the dicarboxylic acid containing a radically polymerizable unsaturated double bond, α,β-unsaturated dicarboxylic acids such as fumaric acid, maleic acid, maleic anhydride, itaconic acid, and citraconic acid can be used, and as the alicyclic dicarboxylic acid containing an unsaturated double bond, 2,5-norbornene dicarboxylic anhydride, tetrahydrophthalic anhydride, etc. can be used. Among these, fumaric acid, maleic acid, and 2,5-norbornene dicarboxylic acid (endo-bicyclo-(2,2,1)-5-heptene-2,3-dicarboxylic acid) are preferred.
[0065] The diol component is at least one of an aliphatic glycol having 2 to 10 carbon atoms, an alicyclic glycol having 6 to 12 carbon atoms, and an ether bond-containing glycol. Examples of the aliphatic glycol having 2 to 10 carbon atoms include ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, and 1,6-hexanediol. As the alicyclic glycol having 6 to 12 carbon atoms, 1,4-cyclohexanedimethanol and the like can be used. Examples of the ether bond-containing glycol include diethylene glycol, triethylene glycol, dipropylene glycol, and glycols obtained by adding 1 to several moles of ethylene oxide or propylene oxide to two phenolic hydroxyl groups of bisphenols, such as 2,2-bis(4-hydroxyethoxyphenyl)propane, etc. Polyethylene glycol, polypropylene glycol, and polytetramethylene glycol can also be used as necessary.
[0066] In addition to the above dicarboxylic acid component and diol component, a tri- or higher functional polycarboxylic acid and / or polyol may be copolymerized. Examples of trifunctional or higher polycarboxylic acids that can be used include trimellitic acid (anhydride), pyromellitic acid (anhydride), benzophenone tetracarboxylic acid (anhydride), trimesic acid, ethylene glycol bis(anhydrotrimellitate), and glycerol tris(anhydrotrimellitate). As the tri- or higher functional polyol, glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, etc. can be used. Examples of tri- or higher functional polycarboxylic acids that can be used include trimellitic acid (anhydride), pyromellitic acid (anhydride), benzophenonetetracarboxylic acid (anhydride), and trimesic acid. As the tri- or higher functional polyol, glycerin, trimethylolethane, trimethylolpropane, etc. can be used. The tri- or higher functional polycarboxylic acid and / or polyol may be used in an amount of 0 to 5 mol %, preferably 0 to 3 mol %, based on the total polycarboxylic acid components including the dicarboxylic acid components or the total polyol components including the diol components.
[0067] (Grafted portion of acrylic grafted polyester copolymer) The graft portion of the acrylic grafted copolyester that can be used in the present invention is an acrylic polymer derived from a monomer mixture containing at least one radical polymerizable monomer having a hydrophilic group or a group that can be later converted to a hydrophilic group.
[0068] The weight average molecular weight of the polymer constituting the graft portion is 500 to 50,000, preferably 4,000 to 50,000. When the weight average molecular weight is less than 500, the grafting rate decreases, so that the polyester is not sufficiently imparted with hydrophilicity, and it is generally difficult to control the weight average molecular weight of the graft portion to less than 500. The graft portion forms a hydration layer of the dispersed particles. In order to provide the particles with a hydration layer of sufficient thickness and obtain a stable dispersion, it is desirable that the weight average molecular weight of the graft portion derived from the radical polymerizable monomer is 500 or more. The upper limit of the weight average molecular weight of the graft portion of the radical polymerizable monomer is preferably 50,000 as described above in terms of the polymerizability in solution polymerization. The molecular weight can be controlled within this range by appropriately selecting the amount of polymerization initiator, monomer dropping time, polymerization time, reaction solvent, and monomer composition, and by appropriately combining a chain transfer agent or a polymerization inhibitor as necessary. The glass transition point is 30°C or less, preferably 10°C or less.
[0069] Examples of the hydrophilic group possessed by the radical polymerizable monomer include a carboxyl group, a hydroxyl group, a sulfonic acid group, an amide group, a quaternary ammonium salt, and a phosphate group. Examples of the group that can be converted into a hydrophilic group include an acid anhydride, a glycidyl group, and a chlorine group. The dispersibility of the grafted polyester in water can be controlled by the hydrophilic group introduced into the polyester by grafting. Among the above hydrophilic groups, the carboxyl group is preferable in terms of controlling the dispersibility of the grafted polyester in water, since the amount of the carboxyl group introduced into the grafted polyester can be accurately determined using an acid value known in the art.
[0070] Examples of the carboxyl group-containing radical polymerizable monomer include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, etc., and further, maleic anhydride, itaconic anhydride, methacrylic anhydride, etc., which easily generate carboxylic acid when in contact with water / amine, can be used. Preferred carboxyl group-containing radical polymerizable monomers are acrylic anhydride, methacrylic anhydride, and maleic anhydride.
[0071] In addition to the above-mentioned hydrophilic group-containing radical polymerizable monomer, it is preferable to copolymerize at least one kind of radical polymerizable monomer that does not contain hydrophilic groups. In the case of only hydrophilic group-containing monomer, grafting to polyester main chain does not occur smoothly, and it is difficult to obtain a good copolymerized polyester aqueous dispersion. Only by copolymerizing at least one kind of radical polymerizable monomer that does not contain hydrophilic groups can grafting be performed efficiently.
[0072] As the radical polymerizable monomer not containing a hydrophilic group, one or more of the above-mentioned monomers having an ethylenically unsaturated bond and not containing a hydrophilic group are used. Examples of such monomers include acrylic esters such as methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, and hydroxypropyl acrylate; methacrylic esters such as methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and hydroxypropyl methacrylate; acrylic acid or methacrylic acid derivatives such as acrylamide, N-methylolacrylamide, and diacetoneacrylamide; acrylonitrile, methacrylic acid derivatives such as ... Examples of suitable monomers include nitriles such as vinyl acetate, vinyl propionate, vinyl benzoate, and the like; vinyl ethers such as vinyl methyl ether, vinyl ethyl ether, vinyl isobutyl ether, and the like; vinyl ketones such as vinyl methyl ketone, vinyl hexyl ketone, and methyl isopropenyl ketone, and the like; N-vinyl compounds such as N-vinylpyrrole, N-vinylcarbazole, N-vinylindole, and N-vinylpyrrolidone, and the like; vinyl halides such as vinyl chloride, vinyl chloride, vinyl bromide, and vinyl fluoride, and the like; and aromatic vinyl compounds such as styrene, α-methylstyrene, t-butylstyrene, vinyltoluene, and vinylnaphthalenes, and the like. These monomers may be used alone or in combination of two or more.
[0073] The ratio of the hydrophilic group-containing monomer to the hydrophilic group-free monomer to be used is determined in consideration of the amount of hydrophilic groups to be introduced into the grafted polyester, and is usually in the range of 95:5 to 5:95, preferably 90:10 to 10:90, and more preferably 80:20 to 40:60, as a mass ratio (hydrophilic group-containing monomer:hydrophilic group-free monomer).
[0074] When a carboxyl group-containing monomer is used as the hydrophilic group-containing monomer, the total acid value of the grafted polyester is 600 to 4000 eq. / 10 6 g, preferably 700-3000eq. / 10 6 g, most preferably 800-2500eq. / 10 6 g. The acid value is 600eq. / 10 6 If the acid value is less than 4000 eq. / 10 g, it is difficult to obtain an aqueous dispersion of copolymerized polyester having a small particle size when the grafted polyester is dispersed in water, and the dispersion stability of the aqueous dispersion of copolymerized polyester is reduced. 6 If it is more than g, the water resistance of the adhesion-modifying layer formed from the aqueous dispersion of copolymerized polyester is reduced.
[0075] The mass ratio of the polyester main chain to the graft portion in the acrylic graft copolyester (polyester: radically polymerizable monomer) is in the range of 40:60 to 95:5, preferably 55:45 to 93:7, and more preferably 60:40 to 90:10.
[0076] If the mass ratio of the polyester main chain is 40% by mass or less, the excellent properties of the parent polyester already described, i.e., high processability, excellent water resistance, and excellent adhesion to various substrates, cannot be fully exhibited, and conversely, undesirable properties of the acrylic resin, i.e., poor processability, gloss, water resistance, etc., are imparted. If the mass ratio of the polyester is 95% by mass or more, the amount of hydrophilic groups in the grafted portion that imparts hydrophilicity to the grafted polyester becomes insufficient, making it impossible to obtain a good aqueous dispersion.
[0077] (Solvent for grafting reaction of acrylic graft copolymer polyester) The solvent for the grafting reaction is preferably composed of an aqueous organic solvent having a boiling point of 50 to 250°C. Here, the aqueous organic solvent refers to an organic solvent having a solubility in water at 20°C of at least 10 g / L or more, preferably 20 g / L or more. An aqueous organic solvent having a boiling point of more than 250°C is inappropriate because it has a slow evaporation rate and cannot be sufficiently removed even by high-temperature baking of the coating film after formation of the coating film. In addition, when an aqueous organic solvent having a boiling point of 50°C or less is used as a solvent for the grafting reaction, an initiator that decomposes into radicals at a temperature of 50°C or less must be used, which increases the danger of handling, and is therefore undesirable.
[0078] Examples of the aqueous organic solvents (first group) which dissolve polyesters well and also dissolve polymerizable monomers containing hydrophilic groups, particularly carboxyl group-containing polymerizable monomers, and polymers thereof relatively well include esters such as ethyl acetate; ketones such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; cyclic ethers such as tetrahydrofuran, dioxane, and 1,3-dioxolane; glycol ethers such as ethylene glycol dimethyl ether, propylene glycol methyl ether, propylene glycol propyl ether, ethylene glycol ethyl ether, and ethylene glycol butyl ether; carbitols such as methyl carbitol, ethyl carbitol, and butyl carbitol; lower esters of glycols or glycol ethers such as ethylene glycol diacetate and ethylene glycol ethyl ether acetate; ketone alcohols such as diacetone alcohol; N-substituted amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone;
[0079] On the other hand, examples of aqueous organic solvents (second group) that hardly dissolve polyester but relatively well dissolve polymerizable monomers containing hydrophilic groups, particularly carboxyl group-containing polymerizable monomers, and polymers thereof include water, lower alcohols, lower glycols, lower carboxylic acids, lower amines, etc. Alcohols and glycols having 1 to 4 carbon atoms are preferred.
[0080] If the grafting reaction is carried out in a single solvent, one of the aqueous organic solvents of the first group may be used, if it is carried out in a mixture of solvents, several of the aqueous organic solvents of the first group or at least one of the aqueous organic solvents of the first group and at least one of the aqueous organic solvents of the second group may be used.
[0081] The grafting reaction can be carried out either in a single solvent consisting of the first group of aqueous organic solvents or in a mixed solvent consisting of one each of the first and second groups of aqueous organic solvents. However, in terms of the progress behavior of the grafting reaction, the appearance and properties of the grafting reaction product and the aqueous dispersion derived therefrom, etc., it is preferable to use a mixed solvent consisting of one each of the first and second groups of aqueous organic solvents. The reason for this is that in the grafting reaction of polyester, gelation of the system is likely to occur due to crosslinking between polyester molecules, but gelation can be prevented by using a mixed solvent as described below.
[0082] It was confirmed by the viscosity measurement of the polyester in these solutions that in the first group of solvents, the polyester molecular chain is in a stretched state with a large spread, while in the first / second group mixed solvents, the polyester molecular chain is in a tangled state with a small spread. In the stretched state of the polyester molecular chain, all the reaction points in the polyester main chain can contribute to the grafting reaction, so the grafting rate of the polyester is high, but at the same time, the rate of intermolecular crosslinking is also high. On the other hand, when the polyester molecular chain is in a thread-like shape, the reaction points inside the thread-like shape cannot contribute to the grafting reaction, and at the same time, the rate of intermolecular crosslinking is also low. Therefore, the state of the polyester molecule can be adjusted by selecting the type of solvent, and thereby the grafting rate and the intermolecular crosslinking due to the grafting reaction can be adjusted.
[0083] Achieving both a high grafting rate and suppressing gelation can be achieved in a mixed solvent system. The optimal mixing ratio of the first group / second group mixed solvents may vary depending on the solubility of the polyester used, but the mass ratio of the first group / second group mixed solvents is usually in the range of 95:5 to 10:90, preferably 90:10 to 20:80, and more preferably 85:15 to 30:70.
[0084] (Radical polymerization initiator and chain transfer agent for acrylic graft polyester copolymer) As the radical polymerization initiator that can be used, organic peroxides and organic azo compounds known to those skilled in the art can be used. Examples of the organic peroxide include benzoyl peroxide and t-butyl peroxypivalate, and examples of the organic azo compounds include 2,2'-azobisisobutyronitrile and 2,2'-azobis(2,4-dimethylvaleronitrile). The amount of the radical polymerization initiator used for carrying out the grafting reaction is at least 0.2% by mass or more, and preferably 0.5% by mass or more, based on the radically polymerizable monomer. In addition to the polymerization initiator, a chain transfer agent for adjusting the chain length of the graft portion, such as octyl mercaptan, mercaptoethanol, 3-t-butyl-4-hydroxyanisole, etc., may be used as necessary. In this case, it is desirable to add the agent in an amount of 0 to 5% by mass relative to the radical polymerizable monomer.
[0085] (Grafting reaction of acrylic graft copolymer polyester) The formation of the grafted portion proceeds by polymerization of the radically polymerizable unsaturated double bond in the polyester with the radically polymerizable monomer and / or reaction of the radically polymerizable unsaturated double bond with the active end of the polymer of the radically polymerizable monomer. The reaction product after the grafting reaction contains, in addition to the desired grafted polyester, polyester having no grafted portion and a polymer of polyester and radically polymerizable monomer not grafted. If the production ratio of grafted polyester in the reaction product is low and the ratio of polyester having no grafted portion and polymer of radically polymerizable monomer not grafted is high, a dispersion with good stability cannot be obtained.
[0086] Usually, the grafting reaction can be carried out by adding the radical polymerizable monomer and the radical initiator at once to a solution containing the polyester under heating, or by dropping them separately over a certain period of time, and then continuing to heat with stirring for a certain period of time to allow the reaction to proceed. Alternatively, if necessary, a part of the radical polymerizable monomer can be added first, and then the remaining radical polymerizable monomer and the polymerization initiator can be dropped separately over a certain period of time, and then the grafting reaction can be carried out by continuing to heat with stirring for a certain period of time.
[0087] The mass ratio of polyester to solvent is selected so that the reaction proceeds uniformly during the polymerization step, taking into consideration the reactivity of polyester with radical polymerizable monomers and the solubility of polyester in the solvent, and is usually in the range of 70:30 to 10:90, preferably 50:50 to 15:85.
[0088] <Water dispersion of acrylic graft polyester copolymer> The grafted polyester usable in the present invention can be dispersed in water by adding it in a solid state to an aqueous medium or by dissolving it in a hydrophilic solvent and then adding it to an aqueous medium. In particular, when a monomer having an acidic group such as a sulfonic acid group or a carboxyl group is used as the radical polymerizable monomer having a hydrophilic group, the grafted polyester can be easily dispersed in water as fine particles having an average particle size of 500 nm or less by neutralizing the grafted polyester with a basic compound, thereby preparing an aqueous dispersion of a copolymerized polyester.
[0089] The basic compound is preferably a compound that volatilizes during coating film formation or during bake curing when a curing agent described below is added. Such basic compounds are preferably ammonia, organic amines, etc. Examples of organic amines include triethylamine, N,N-diethylethanolamine, N,N-dimethylethanolamine, aminoethanolamine, N-methyl-N,N-diethanolamine, isopropylamine, iminobispropylamine, ethylamine, diethylamine, 3-ethoxypropylamine, etc. The amount of the basic compound used is preferably an amount that at least partially or completely neutralizes the carboxyl groups contained in the grafted portion and adjusts the pH value of the aqueous dispersion to the range of 5.0 to 9.0.
[0090] The method for preparing the aqueous dispersion of copolymerized polyester neutralized with a basic compound is to remove the solvent from the reaction solution after the grafting reaction under reduced pressure using an extruder or the like to obtain a melt or solid (pellets, powder, etc.), which is then added to an aqueous solution of a basic compound and stirred under heating, or to add an aqueous solution of a basic compound to the reaction solution immediately after the grafting reaction is completed, and continue to heat and stir (one-pot method) to prepare the aqueous dispersion. The one-pot method is preferred from the viewpoint of convenience. In this case, if the boiling point of the solvent used in the grafting reaction is 100°C or less, a part or all of it can be easily removed by distillation.
[0091] <Crosslinking agent added to coating solution> A crosslinking agent (curing resin) can be further blended into the coating solution of any of the above polyester resins, polyurethane resins, and / or polyacrylic resins to harden the coating solution, thereby imparting high water resistance to the adhesion modification layer. Examples of the crosslinking agent that can be used include phenol formaldehyde resins which are condensates of alkylated phenols, cresols, or the like with formaldehyde; amino resins such as adducts of urea, melamine, benzoguanamine, or the like with formaldehyde, and alkyl ether compounds which are made of such adducts and alcohols having 1 to 6 carbon atoms; polyfunctional epoxy compounds; polyfunctional isocyanate compounds; blocked isocyanate compounds; polyfunctional aziridine compounds; and oxazoline compounds. These crosslinking agents may be used alone or in combination of two or more. The amount of the crosslinking agent to be added is preferably 5% by mass to 40% by mass based on the grafted polyester.
[0092] The method of blending the crosslinking agent may be (1) a method in which the crosslinking agent is water-soluble, in which it is directly dissolved or dispersed in the aqueous dispersion, or (2) a method in which the crosslinking agent is oil-soluble, in which the crosslinking agent is added after the grafting reaction is completed, before or after the aqueous dispersion, so that the crosslinking agent coexists with the polyester in the core part. These methods may be appropriately selected depending on the type and properties of the crosslinking agent. Furthermore, the crosslinking agent may be used in combination with a curing agent or an accelerator.
[0093] The adhesion modification layer used in the present invention can further contain additives such as antistatic agents, inorganic lubricants, and organic lubricants in order to impart antistatic properties and slipping properties, within a range that does not impair the effects of the present invention. When antistatic agents, inorganic lubricants, organic lubricants, etc. are applied to the film surface, it is preferable to contain them in the adhesion modification layer to prevent the detachment of these additives.
[0094] [Method of manufacturing highly adhesive polyamide film] The highly adhesive polyamide film of the present invention is produced by forming an adhesion modifying layer on the biaxially oriented polyamide film of the present invention by the method described below. The biaxially stretched polyamide film of the present invention can be produced by a known production method. For example, a sequential biaxial stretching method or a simultaneous biaxial stretching method can be mentioned. The sequential biaxial stretching method is preferable because it can increase the film production speed and is advantageous in terms of production costs. The method for producing the biaxially stretched polyamide film of the present invention will now be described in further detail. First, the raw material resin is melt-extruded using an extruder, extruded from a T-die into a film, and cast onto a cooling roll and cooled to obtain an unstretched film. The melting temperature of the resin is preferably 200 to 300° C. If it is lower than the above, unmelted matter may occur, resulting in defects and other poor appearance, whereas if it exceeds the above, deterioration of the resin may be observed, resulting in a decrease in molecular weight and a deterioration in appearance.
[0095] The cooling roll temperature is preferably from -30 to 80°C, and more preferably from 0 to 50°C. To obtain an unstretched film by casting the film-like molten material extruded from a T-die onto a rotating cooling drum and cooling it, for example, a method using an air knife or an electrostatic adhesion method in which a static charge is applied can be preferably used. The latter method is particularly preferably used.
[0096] It is also preferable to cool the surface of the cast unstretched film opposite the cooling roll. For example, it is preferable to use a method of contacting the surface of the unstretched film opposite the cooling roll with a cooling liquid in a tank, a method of applying a liquid that evaporates with a spray nozzle, a method of spraying a high-speed fluid, or the like. The unstretched film thus obtained is stretched biaxially to obtain a biaxially stretched polyamide film.
[0097] As a method for stretching in the MD direction, multi-stage stretching such as one-stage stretching or two-stage stretching can be used. As described later, multi-stage MD stretching such as two-stage stretching is preferable in terms of physical properties and uniformity of physical properties in the MD direction and the TD direction (isotropy) rather than one-stage stretching. In the sequential biaxial stretching method, stretching in the MD direction is preferably performed by roll stretching.
[0098] The lower limit of the MD stretching temperature is preferably 50° C., more preferably 55° C., and further preferably 60° C. If the temperature is less than 50° C., the resin does not soften, and stretching may become difficult. The upper limit of the MD stretching temperature is preferably 120° C., more preferably 115° C., and further preferably 110° C. If the temperature exceeds 120° C., the resin becomes too soft and stable stretching may not be possible.
[0099] The lower limit of the stretching ratio in the MD direction (when stretching in multiple stages, the total stretching ratio multiplied by each stretching ratio) is preferably 2.2 times, more preferably 2.5 times, and further preferably 2.8 times. If it is less than 2.2 times, the thickness accuracy in the MD direction decreases, and the crystallinity becomes too low, which may reduce the impact strength. The upper limit of the stretching ratio in the MD direction is preferably 5.0 times, more preferably 4.5 times, and most preferably 4.0 times. If it exceeds 5.0 times, the subsequent stretching may become difficult.
[0100] In addition, when the MD stretching is performed in multiple stages, the above-mentioned stretching is possible in each stretching, but the stretching ratios must be adjusted so that the product of all MD stretching ratios is 5.0 or less. For example, in the case of two-stage stretching, the first stage stretching is preferably 1.5 to 2.1 times, and the second stage stretching is preferably 1.5 to 1.8 times.
[0101] The film stretched in the MD direction is stretched in the TD direction using a tenter, heat-set, and then subjected to a relaxation treatment (also called a relaxation treatment). The lower limit of the TD stretching temperature is preferably 50° C., more preferably 55° C., and further preferably 60° C. If the temperature is less than 50° C., the resin does not soften, and stretching may become difficult. The upper limit of the stretching temperature in the TD direction is preferably 190° C., more preferably 185° C., and further preferably 180° C. If the temperature exceeds 190° C., crystallization may occur, making stretching difficult.
[0102] The lower limit of the stretch ratio in the TD direction (when stretching in multiple stages, the total stretch ratio multiplied by each stretch ratio) is preferably 2.8, more preferably 3.2, even more preferably 3.5, and particularly preferably 3.8. If it is less than 2.8, the thickness accuracy in the TD direction decreases, and the crystallinity becomes too low, which may reduce the impact strength. The upper limit of the stretching ratio in the TD direction is preferably 5.5 times, more preferably 5.0 times, still more preferably 4.7 times, particularly preferably 4.5 times, and most preferably 4.3 times. If it exceeds 5.5 times, the productivity may decrease significantly.
[0103] Selection of the heat setting temperature is an important factor in the present invention. As the heat setting temperature is increased, the crystallization and orientation relaxation of the film progresses, improving the impact strength and reducing the heat shrinkage rate. On the other hand, when the heat setting temperature is low, the crystallization and orientation relaxation are insufficient, and the heat shrinkage rate cannot be reduced sufficiently.) Moreover, if the heat setting temperature is too high, the resin deteriorates and the film rapidly loses its toughness, such as its impact strength.
[0104] The lower limit of the heat setting temperature is preferably 180° C., more preferably 200° C. If the heat setting temperature is too low, the heat shrinkage rate becomes too large, which tends to deteriorate the appearance after lamination and to decrease the laminate strength. The upper limit of the heat setting temperature is preferably 230° C., more preferably 220° C. If the heat setting temperature is too high, the impact strength tends to decrease.
[0105] The heat setting time is preferably 0.5 to 20 seconds. More preferably, it is 1 to 15 seconds. The heat setting time can be set appropriately by taking into account the heat setting temperature and the wind speed in the heat setting zone. If the heat setting conditions are too weak, crystallization and orientation relaxation become insufficient, causing the above problems. If the heat setting conditions are too strong, the film toughness decreases.
[0106] Relaxation treatment after heat setting is effective for controlling the heat shrinkage rate. The temperature for relaxation treatment can be selected within the range from the heat setting temperature to the glass transition temperature (Tg) of the resin, but it is preferably from the heat setting temperature -10°C to Tg +10°C. If the relaxation temperature is too high, the shrinkage speed will be too fast, which is undesirable and may cause distortion. Conversely, if the relaxation temperature is too low, relaxation treatment will not occur and the film will simply slacken, the heat shrinkage rate will not decrease, and dimensional stability will deteriorate.
[0107] The lower limit of the relaxation rate in the relaxation treatment is preferably 0.5%, and more preferably 1%. If it is less than 0.5%, the heat shrinkage rate may not be reduced sufficiently. The upper limit of the relaxation rate is preferably 20%, more preferably 15%, and further preferably 10%. If it exceeds 20%, sagging may occur in the tenter, making production difficult.
[0108] In order to increase the adhesive strength with the sealant film or the printing layer, the surface of the laminated stretched polyamide film and / or the surface of the adhesive modification layer may be subjected to corona treatment, flame treatment, etc. In addition, in order to increase the adhesive strength between the laminated stretched polyamide film and the adhesive modification layer, the surface of the laminated stretched polyamide film on the adhesive modification layer side may be subjected to corona treatment, flame treatment, etc.
[0109] The method for forming the adhesion modification layer in the present invention can be a method of applying a coating agent containing any one of polyester resin, polyurethane resin, and / or polyacrylic resin to a laminated stretched polyamide film by a known coating method such as a gravure method, reverse method, die method, bar method, or dip method.
[0110] The coating amount of the coating agent is 0.01 to 3 g / m2 in terms of solid content relative to the polyamide film after biaxial stretching. 2 More preferably, the thickness is 0.04 to 0.5 g / m 2 The above coating amount can provide sufficient adhesive strength between the adhesion modifying layer and other layers, and can also prevent blocking between films.
[0111] The adhesion modifying layer in the present invention can be formed by applying a coating agent to a biaxially oriented polyamide film substrate, or by applying a coating agent to an unstretched or uniaxially oriented polyamide film substrate, drying the substrate, and, if necessary, further heat fixing after uniaxial or biaxial stretching. The drying temperature after coating the coating agent is 180°C or higher, preferably 200°C or higher, whereby the coating film becomes strong and the adhesion between the adhesion modifying layer and the polyamide film substrate is improved.
[0112] When stretching is performed after coating, the moisture content of the coated film must be controlled to within the range of 0.1 to 2% in order not to impair the stretchability of the coated film. After stretching, the coating film is strengthened by drying and heat fixing at 200°C or higher, and the adhesion between the adhesion modifying layer and the polyamide film substrate is dramatically improved.
[0113] The thus obtained highly adhesive polyamide film of the present invention can prevent the film from being scraped by friction with a transport package such as a cardboard during transport of the bag-made product, which would cause the bag to break. It can also prevent the bag from being broken by bending fatigue caused by contact between the bags. In addition, the high water-resistant adhesive strength between the polyamide film and the sealant film allows the film to exhibit high bag breakage prevention properties.
[0114] [Characteristics of highly adhesive polyamide film] The highly adhesive polyamide film of the present invention has 10 or less pinhole defects when a twist bending test is performed 1000 times at a temperature of 1° C. using a Gelbo flex tester according to the measurement method described in the Examples. More preferably, the number is 5 or less. The fewer the number of pinhole defects after the bending test, the better the bending pinhole resistance is. If the number of pinholes is 10 or less, a packaging bag that is less likely to develop pinholes even when the packaging bag is subjected to a load during transportation, etc. can be obtained.
[0115] Furthermore, in the highly adhesive polyamide film of the present invention, the distance until pinholes appear in the friction pinhole resistance test is 2900 cm or more, more preferably 3100 cm or more, and even more preferably 3300 cm or more. The longer the distance at which pinholes appear, the better the friction pinhole resistance is, and if the distance at which pinholes appear is 2900 cm or more, a packaging bag that is less likely to have pinholes even if the packaging bag rubs against a cardboard box or the like during transportation can be obtained. The highly adhesive polyamide film of the present invention is characterized by having excellent properties in both bending pinhole resistance and friction pinhole resistance. The highly adhesive polyamide film of the present invention having these properties is highly useful as a packaging film because it is less likely to develop pinholes during transportation.
[0116] The heat shrinkage rate of the highly adhesive polyamide film of the present invention at 160°C for 10 minutes is in the range of 0.6 to 3.0% in both the machine direction (hereinafter abbreviated as MD direction) and the width direction (hereinafter abbreviated as TD direction), and is preferably 0.6 to 2.5%. If the heat shrinkage rate exceeds 3.0%, curling or shrinkage may occur when heat is applied in the next process such as lamination or printing. In addition, the lamination strength with the sealant film may be weakened. Although it is possible to make the heat shrinkage rate less than 0.6%, it may become mechanically fragile. In addition, it is not preferable because the productivity is deteriorated.
[0117] Since excellent impact resistance is a feature of biaxially oriented polyamide films, the impact strength of the highly adhesive polyamide film of the present invention is preferably 0.7 J / 15 μm or more, and more preferably 0.9 J / 15 μm or more.
[0118] The haze value of the highly adhesive polyamide film of the present invention is preferably 10% or less, more preferably 7% or less, and further preferably 5% or less. A small haze value means good transparency and gloss, so when used for packaging bags, beautiful printing is possible and the product value is increased. Adding fine particles to improve the slipperiness of the film increases the haze value, so the haze value can be reduced by adding fine particles only to the functional layer B.
[0119] The highly adhesive polyamide film of the present invention has a radioactive carbon (C 14 It is preferable that the content of carbon derived from biomass (also called biomass ratio) measured by the FT-IR spectrometer 200 is 1 to 15% based on the total carbon in the polyamide film. Carbon dioxide in the atmosphere contains 14 Since carbon dioxide is contained in the atmosphere at a constant rate (105.5pMC), plants that grow by absorbing carbon dioxide from the atmosphere, such as corn, contain 14 The content is known to be about 105.5 pMC. In addition, C in fossil fuels is 14 It is also known that polyamides contain almost no C. 14 By measuring the ratio of carbon derived from biomass, the ratio of carbon derived from biomass can be calculated.
[0120] The highly adhesive polyamide film of the present invention has a laminate strength of 4.0 N / 15 mm or more after being attached to the polyethylene sealant described in the Examples. The highly adhesive polyamide film of the present invention is usually laminated with a sealant film and then processed into a packaging bag. If the laminate strength is 4.0 N / 15 mm or more, when the highly adhesive polyamide film of the present invention is used to produce a packaging bag in various lamination configurations, the strength of the seal portion is sufficient, and a strong packaging bag that is difficult to tear can be obtained. In order to increase the lamination strength to 4.0 N / 15 mm or more, the highly adhesive polyamide film of the present invention can be subjected to corona treatment, coating treatment, flame treatment, or the like.
[0121] Furthermore, the highly adhesive polyamide film of the present invention can be subjected to heat treatment or humidity conditioning treatment to improve dimensional stability depending on the application. In addition, in order to improve the adhesion of the film surface, corona treatment, coating treatment, flame treatment, printing, deposition of metals, inorganic oxides, etc. can be performed. As the deposition film formed by deposition processing, a deposition film of aluminum, a deposition film of silicon oxide or aluminum oxide alone or a mixture thereof is preferably used. Furthermore, by coating a protective layer on these deposition films, oxygen and hydrogen barrier properties can be improved.
[0122] The highly adhesive polyamide film of the present invention is laminated with a sealant film or the like to form a laminate film, which is then processed into packaging bags such as bottom-sealed bags, side-sealed bags, three-side-sealed bags, pillow bags, standing pouches, gusseted bags, and square-bottom bags. Examples of the sealant film include an unstretched linear low-density polyethylene film, an unstretched polypropylene film, and an ethylene-vinyl alcohol copolymer resin film. The layer structure of the laminated film using the easy-adhesive polyamide film of the present invention is not particularly limited as long as the easy-adhesive polyamide film of the present invention is contained in the laminated film. The film used for the laminated film may be made of petrochemically derived raw materials or biomass-derived raw materials, but polylactic acid, polyethylene terephthalate, polybutylene succinate, polyethylene, polyethylene furanoate, etc. polymerized using biomass-derived raw materials are preferred in terms of reducing environmental load.
[0123] Examples of layer configurations of the laminated film of the present invention, where the boundary between layers is represented by / , include ONY / joint / LLDPE, ONY / joint / CPP, ONY / joint / Al / joint / CPP, ONY / joint / Al / joint / LLDPE, ONY / PE / Al / joint / LLDPE, ONY / joint / Al / PE / LLDPE, PET / joint / ONY / joint / LLDPE, PET / joint / ONY / PE / LLDPE, PET / joint / ONY / joint / Al / joint / LLDP. E, PET / Contact / Al / Contact / ONY / Contact / LLDPE, PET / Contact / Al / Contact / ONY / PE / LLDPE, PET / PE / Al / PE / ONY / PE / LLDPE, PET / Contact / ONY / Contact / CPP, P ET / Contact / ONY / Contact / Al / Contact / CPP, PET / Contact / Al / Contact / ONY / Contact / CPP, ONY / Contact / PET / Contact / LLDPE, ONY / Contact / PET / PE / LLDPE, ONY / Contact / PET / Contact / CPP , ONY / / Al / / PET / / LLDPE, ONY / bond / Al / bond / PET / PE / LLDPE, ONY / PE / LLDPE, ONY / PE / CPP, ONY / PE / Al / PE, ONY / PE / Al / PE / LLDPE, OPP / bond / ONY / bond / LLDPE, ONY / bond / EVOH / bond / LLDPE, ONY / bond / EVOH / bond / CPP, ONY / bond / aluminum or inorganic oxide vapor-deposited PET / bond / LLDPE, Examples include ONY / bond / aluminum-vapor-deposited PET / bond / ONY / bond / LLDPE, ONY / bond / aluminum-vapor-deposited PET / PE / LLDPE, ONY / PE / aluminum-vapor-deposited PET / PE / LLDPE, ONY / bond / aluminum-vapor-deposited PET / bond / CPP, PET / bond / aluminum-vapor-deposited PET / ONY / bond / LLDPE, CPP / bond / ONY / bond / LLDPE, ONY / bond / aluminum-vapor-deposited LLDPE, ONY / bond / aluminum-vapor-deposited CPP, etc. The abbreviations used in the above layer structure are as follows: ONY: highly adhesive polyamide film of the present invention, PET: stretched polyethylene terephthalate film, LLDPE: unstretched linear low-density polyethylene film, CPP: unstretched polypropylene film, OPP: stretched polypropylene film, PE: extrusion laminate or unstretched low-density polyethylene film, Al: aluminum foil, EVOH: ethylene-vinyl alcohol copolymer resin, Adhesive: adhesive layer for adhering films together, aluminum or inorganic oxide vapor deposition indicates that aluminum or inorganic oxide is vapor-deposited. EXAMPLES
[0124] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following examples. The films were evaluated by the following measurement methods. Unless otherwise specified, the measurements were performed in a measurement room with an environment of 23°C and a relative humidity of 65%. (1) Film haze value The measurement was performed using a direct reading haze meter manufactured by Toyo Seiki Seisakusho Co., Ltd. in accordance with JIS-K-7105. (2) Film thickness Divide the film into 10 equal parts in the TD direction (for narrow films, divide it so that the width is sufficient to measure the thickness), cut out 100mm films in the MD direction, and condition them for more than 2 hours in an environment with a temperature of 23℃ and a relative humidity of 65%. Using a thickness measuring device made by Tester Sangyo, measure the thickness at the center of each sample, and take the average value as the thickness.
[0125] (3) Biomass content of film The obtained film biomass degree was calculated based on the radiocarbon (C 14 ) measurements were performed. (4) Thermal shrinkage rate of film The heat shrinkage rate was measured according to the following formula in accordance with the dimensional change test method described in JIS C2318, except that the test temperature was 160° C. and the heating time was 10 minutes. Heat shrinkage rate = [(length before treatment - length after treatment) / length before treatment] x 100 (%) (5) Impact strength of film Measurements were performed using a film impact tester manufactured by Toyo Seiki Seisakusho Co., Ltd. The measured values were converted per 15 μm thickness and expressed as J (joules) / 15 μm. (6) Dynamic friction coefficient of film The coefficient of dynamic friction between the outer surfaces of the film rolls was evaluated under the following conditions in accordance with JIS-C2151. The test specimen size was 130 mm wide and 250 mm long, and the test speed was 150 mm / min.
[0126] (7) Pinhole resistance of film when bent The number of pinholes due to bending fatigue was measured by the following method using a Gelbo Flex Tester manufactured by Rigaku Kogyosha. After applying a polyester adhesive to the film prepared in the examples, a linear low-density polyethylene film (L-LDPE film: Toyobo Co., Ltd., L4102) having a thickness of 40 μm was dry laminated, and aged for 3 days in an environment at 40 ° C to obtain a laminate film. The obtained laminate film was cut into 12 inches × 8 inches and made into a cylindrical shape with a diameter of 3.5 inches. One end of the cylindrical film was fixed to the fixed head side of the Gelbo flex tester and the other end was fixed to the movable head side, and the initial gripping distance was set to 7 inches. A flex fatigue test was performed 1000 times at a speed of 40 times / min, in which a 440 degree twist was given in the first 3.5 inches of the stroke, and the entire stroke was completed in a linear horizontal motion for the next 2.5 inches, and the number of pinholes generated in the laminate film was counted. The measurement was performed in an environment at 1 ° C. The test film was placed on a filter paper (Advantec, No. 50) with the L-LDPE film side facing down, and the four corners were fixed with cellophane tape (registered trademark). Ink (Pilot ink (product number INK-350-Blue) diluted 5 times with pure water) was applied to the test film and spread over the entire surface using a rubber roller. After wiping off unnecessary ink, the test film was removed, and the number of ink dots on the filter paper was counted.
[0127] (8) Film abrasion and pinhole resistance A friction test was carried out using a fastness tester (manufactured by Toyo Seiki Seisakusho) according to the following method, and the distance at which pinholes occurred was measured. A test sample was made by folding the same laminate film as that produced in the pinhole resistance evaluation above in quarters to make sharp corners, and rubbing it against the inside of a cardboard box with a fastness tester at an amplitude of 25 cm, an amplitude speed of 30 times / min, and a weight of 100 g. The cardboard used was K280 x P180 x K210 (AF) = (surface liner x core material x backing liner (type of flute)). The pinhole occurrence distance was calculated according to the following procedure. The longer the pinhole occurrence distance, the better the abrasion pinhole resistance. First, a friction test was conducted with an amplitude of 100 times and a distance of 2500 cm. If no pinholes were found, the friction test was conducted with an amplitude of 20 times and a distance of 500 cm increased. If no pinholes were found, the friction test was conducted with an amplitude of 20 times and a distance of 500 cm increased again. This was repeated, and the distance at which a pinhole was found was marked with an X and set as level 1. If a pinhole was found with an amplitude of 100 times and a distance of 2500 cm, the friction test was conducted with an amplitude of 20 times and a distance reduced by 500 cm. If a pinhole was found, the friction test was conducted with an amplitude of 20 times and a distance reduced by 500 cm again. This was repeated, and the distance at which a pinhole was not found was marked with an O and set as level 1. Next, for level 2, if the final result in level 1 was ○, the number of amplitudes was increased by 20 and a friction test was conducted. If a pinhole did not appear, it was marked with an ○, and if a pinhole appeared, it was marked with an ×. If the final result in level 1 was ×, the number of amplitudes was decreased by 20 and a friction test was conducted. If a pinhole did not appear, it was marked with an ○, and if a pinhole appeared, it was marked with an ×. Further, for levels 3 to 20, if the previous level was rated as ○, increase the number of amplitudes by 20 and conduct a friction test; if no pinholes are created, mark it as ○, if a pinhole is created, mark it as ×. If the previous level was rated as ×, reduce the number of amplitudes by 20 and conduct a friction test; if no pinholes are created, mark it as ○, if a pinhole is created, mark it as ×. Repeat this process and mark levels 3 to 20 as ○ or ×. For example, the results shown in Table 1 were obtained. Using Table 1 as an example, we will explain how to find the pinhole occurrence distance. Count the number of O and X trials for each distance. The distance with the most tests was used as the median, and the coefficient was set to 0. For distances longer than that, the coefficient was set to +1, +2, +3... for every 500 cm, and for distances shorter than that, the coefficient was set to -1, -2, -3... for every 500 cm. For all tests from levels 1 to 20, the number of tests in which no holes occurred was compared with the number of tests in which holes occurred, and the friction pinhole occurrence distance was calculated using the following formula for each of the cases A and B. A: In all tests, the number of tests without holes is equal to or greater than the number of tests with holes. Distance at which pinholes occur due to friction = median + 500 x (Σ(coefficient x number of tests where no holes occurred) / number of tests where no holes occurred) + 1 / 2) B: In all tests, the number of tests without holes is less than the number of tests with holes. Distance at which friction pinholes occur = median + 500 x (Σ(coefficient x number of tests with holes) / number of tests with holes) - 1 / 2)
[0128] [Table 1]
[0129] (9) Lamination strength with polyethylene sealant The laminate film prepared in the same manner as described in the explanation of the pinhole resistance evaluation was cut into a strip of 15 mm width × 200 mm length, and one end of the laminate film was peeled off at the interface between the biaxially oriented polyamide film and the linear low-density polyethylene film. Using an autograph (manufactured by Shimadzu Corporation), the laminate strength was measured three times in each of the MD and TD directions under the conditions of a temperature of 23°C, a relative humidity of 50%, a tensile speed of 200 mm / min, and a peel angle of 90°, and the average value was used to evaluate the laminate strength.
[0130] (10) Water-resistant laminate strength (lamination strength under water adhesion conditions) When measuring the laminate strength in (9), water was dropped onto the peeling interface of the strip-shaped laminate film with a dropper, and the laminate strength was measured. Measurements were made three times in each of the MD and TD directions, and the average value was used to evaluate.
[0131] (11) Film formation stability during casting The molten resin was extruded from a T-die into a film, cast onto a cooling roll and cooled to obtain an unstretched film. The process was visually observed, and the film formation stability was evaluated as follows. ◯: The film formation was stable and a homogeneous unstretched film was obtained. △: Film formation was a little unstable, and fluctuations were observed in the width of the unstretched film, but biaxial stretching was possible. ×: The film formation was unstable and the unstretched film was inhomogeneous, so that a biaxially stretched film could not be obtained. (12) Period of occurrence of thermal degradation products at the die lip exit After cleaning the lip of the die, film production was started, and the time until thermally deteriorated products appeared on the lip of the die was observed.
[0132] (13) Relative viscosity of raw polyamide 0.25 g of polyamide was dissolved in 96% sulfuric acid in a 25 ml measuring flask to a concentration of 1.0 g / dl, and the relative viscosity of the polyamide solution was measured at 20°C. (14) Melting point of raw polyamide In accordance with JIS K7121, a differential scanning calorimeter SSC5200 manufactured by Seiko Instruments Inc. was used to measure in a nitrogen atmosphere at a sample weight of 10 mg, a heating start temperature of 30°C, and a heating rate of 20°C / min, and the endothermic peak temperature (Tmp) was determined as the melting point. (15) Coating amount of adhesive modification layer A biaxially oriented polyamide film was cut into a piece measuring 10 cm x 10 cm, and the adhesive modification layer of the film was wiped with a cloth soaked in a mixed organic solvent of methyl ethyl ketone / toluene = 1 / 1. The weight before and after wiping was measured with a precision balance (Shimadzu Corporation AUW120D). The difference in weight was converted to a value per square meter, and the coating amount (g / m 2 ) was calculated.
[0133] (Example 1-1) Using an apparatus consisting of an extruder and a 380 mm wide T-die, the following molten resin composition was extruded from the T-die into a film, which was then cast onto a cooling roll whose temperature was controlled at 20°C and electrostatically adhered to obtain an unstretched film having a thickness of 200 μm. Resin composition: A resin composition consisting of 97 parts by mass of polyamide 6 (manufactured by Toyobo Co., Ltd., relative viscosity 2.8, melting point 220°C), 3.0 parts by mass of polyamide 11 (manufactured by Arkema, relative viscosity 2.5, melting point 186°C, biomass degree 100%), 0.45 parts by mass of porous silica microparticles (manufactured by Fuji Silysia Chemical Ltd., average particle size 2.0 μm, pore volume 1.6 ml / g), and 0.15 parts by mass of fatty acid bisamide (ethylene bisstearamide, manufactured by Kyoeisha Chemical Co., Ltd.). The obtained unstretched film was introduced into a roll-type stretching machine, and using the difference in peripheral speed of the rolls, it was stretched 1.73 times in the MD direction at 80 ° C., and then further stretched 1.85 times at 70 ° C. Subsequently, the following coating solution (A) was applied to this uniaxially stretched film with a roll coater, and then it was continuously introduced into a tenter-type stretching machine while drying with hot air at 70 ° C., and after preheating at 110 ° C., it was stretched 1.2 times at 120 ° C., 1.7 times at 130 ° C., and 2.0 times at 160 ° C. in the TD direction, and then heat-set at 215 ° C., and then relaxed by 7% at 215 ° C., and wound up to obtain a biaxially stretched polyamide film laminated with an adhesive modification layer (AEG). The evaluation results of the obtained easy-adhesion polyamide film are shown in Table 2.
[0134] [Coating solution (A): Water-based dispersion of acrylic grafted polyester copolymer] A stainless steel autoclave equipped with a stirrer, a thermometer and a partial reflux condenser was charged with 466 parts by mass of dimethyl terephthalate, 466 parts by mass of dimethyl isophthalate, 401 parts by mass of neopentyl glycol, 443 parts by mass of ethylene glycol and 0.52 parts by mass of tetra-n-butyl titanate, and an ester exchange reaction was carried out at 160 to 220°C for 4 hours. Then, 23 parts by mass of fumaric acid was added, and the temperature was raised from 200°C to 220°C for 1 hour, and an esterification reaction was carried out. The temperature was then raised to 255°C, and the reaction system was gradually reduced in pressure, and then the reaction was carried out under reduced pressure of 0.2 mmHg for 1 hour and 30 minutes with stirring to obtain a polyester. The obtained polyester was pale yellow and transparent, had a glass transition temperature of 60°C and a weight average molecular weight of 12000. The composition obtained by NMR measurement etc. was as follows. Dicarboxylic acid component Terephthalic acid 48 mol% Isophthalic acid 48 mol% Fumaric acid 4 mol% Diol component Neopentyl glycol 50 mol% Ethylene glycol 50 mol% In a reactor equipped with a stirrer, a thermometer, a reflux device and a quantitative dropping device, 75 parts by mass of the polyester resin, 56 parts by mass of methyl ethyl ketone and 19 parts by mass of isopropyl alcohol were placed and heated at 65 ° C., stirred and dissolved to dissolve the resin. After the resin was completely dissolved, a mixture of 17.5 parts by mass of methacrylic acid and 7.5 parts by mass of ethyl acrylate and a solution of 1.2 parts by mass of azobisdimethylvaleronitrile dissolved in 25 parts by mass of methyl ethyl ketone were dropped into the polyester solution at 0.2 ml / min, and stirring was continued for another 2 hours after the end of the dropping. After sampling (5 g) for analysis from the reaction solution, 300 parts by mass of water and 25 parts by mass of triethylamine were added to the reaction solution and stirred for 1 hour to prepare a dispersion of grafted polyester. Thereafter, the temperature of the obtained dispersion was raised to 100 ° C., and methyl ethyl ketone, isopropyl alcohol and excess triethylamine were distilled off to obtain a copolymerized polyester aqueous dispersion.
[0135] The resulting dispersion was white, with an average particle size of 300 nm and a B-type viscosity of 50 centipoise at 25°C. 1.25 g of heavy water was added to 5 g of this dispersion to adjust the solid concentration to 20% by mass, and then DSS was added and 125 MHz 13C-NMR was measured. The half-width of the signal (160-175 ppm) of the carbonyl carbon of the polyester main chain was ∞ (no signal was detected), and the half-width of the signal (181-186 ppm) of the carbonyl carbon of the methacrylic acid in the grafted portion was 110 Hz. The solution sampled at the end of the grafting reaction was dried under vacuum at 100°C for 8 hours, and the acid value of the solid content was measured, the graft efficiency of the polyester was measured (NMR measurement), and the molecular weight of the grafted portion due to hydrolysis was measured. The acid value of the solid content was 2300 eq. / 10 6 It was g. 1 In the H-NMR measurement, no signal (δ=6.8-6.9 ppm, doublet) derived from fumaric acid was detected, confirming that the grafting efficiency of the polyester was 100%. The molecular weight of the grafted portion was a weight-average molecular weight of 10,000. Thereafter, the aqueous dispersion obtained as above was diluted with water to a solid content concentration of 5% by mass to obtain a coating liquid (A).
[0136] (Examples 1-2 to 1-9) A biaxially stretched polyamide film having an adhesion-modifying layer (AEG) was obtained in the same manner as in Example 1-1, except that the raw resin composition was changed as shown in Table 2. The evaluation results of the obtained highly adhesive polyamide film are shown in Table 2. However, in Examples 1-6 and 1-7, the coating liquid used was the coating liquid (B): an aqueous dispersion of polyurethane resin, and an easily adhesive polyamide film having an adhesiveness-modifying layer (PU) laminated thereon was obtained. [Coating liquid (B): Water-based dispersion of polyurethane resin] (A) Preparation of polyurethane and aqueous dispersion: A polyester (polyester polyol) with a Tg of -5°C was obtained using adipic acid as the dicarboxylic acid component, 60 mol% (of the glycol component) of 1,4-butanediol, and 40 mol% of a propylene oxide (1 mol) adduct of bisphenol A as the glycol component. Toluene diisocyanate was reacted with this polyester to obtain a urethane polymer. This was made into a prepolymer, and 1,6-hexanediol was reacted to extend the chain and react an aminocarboxylate at the end to obtain a water-insoluble and water-dispersible polyurethane. This was dispersed in hot water with stirring to obtain a 25% aqueous dispersion. The aqueous dispersion of polyurethane was diluted with an equal amount of a mixture of ion-exchanged water and isopropyl alcohol so that the solid content became 5% by mass, thereby obtaining a coating liquid (B).
[0137] (Comparative Examples 1-1 to 1-6) A biaxially stretched polyamide film was obtained in the same manner as in Example 1-1, except that the adhesiveness-modifying layer was not formed, using the resin composition of the raw material shown in Table 2. In order to improve the adhesion with the sealant film, the film surface was subjected to a corona discharge treatment after heat setting and relaxation treatment. The evaluation results are shown in Table 2. However, in Comparative Example 1-4, the molten resin could not be stably extruded into a film from the T-die, and a homogeneous unstretched film could not be obtained, so that biaxial stretching was not possible.
[0138] [Table 2]
[0139] As shown in Table 2, the films of the examples had good resistance to pinholes caused by bending and pinholes caused by friction. They also had low haze and good transparency, high impact strength, and high lamination strength with a sealant film, making them excellent as packaging films. In addition, due to the presence of the adhesive modification layer, the lamination strength, especially the water-resistant lamination strength, was excellent. The biaxially oriented polyamide films of Comparative Examples 1-1 and 1-2, which did not contain a material that improved pinhole resistance during bending, and the biaxially oriented polyamide film of Comparative Example 1-3, which had too little polyamide 11 content, had poor pinhole resistance during bending. In Comparative Example 1-4, the content of polyamide 11 was too high, so the molten resin could not be stably extruded into a film from the T-die, and therefore a homogeneous unstretched film could not be obtained, and a biaxially stretched polyamide film could not be obtained. In Comparative Example 1-5, a polyamide elastomer (Arkema nylon 12 / polytetramethylene glycol copolymer, product name "Pebax SA01") that has been conventionally used as a material for improving pinhole resistance was used, and although the pinhole resistance was good, the pinhole resistance at friction was poor. In addition, there was a drawback that deterioration materials were easily attached to the die during long-term production, making it impossible to carry out long-term continuous production. In Comparative Example 1-6, the biaxially oriented polyamide film of the present invention was not provided with an adhesiveness-modifying layer, but instead was subjected to corona treatment to improve adhesiveness. The bending pinhole resistance and friction pinhole resistance were good, but the laminate strength and water-resistant laminate strength were low.
[0140] (Example 2-1) An adhesive biaxially stretched polyamide film having an adhesive modification layer (AEG) was obtained in the same manner as in Example 1-1, except that the heat setting temperature and relaxation temperature were set to 218° C. The evaluation results of the obtained adhesive polyamide film are shown in Table 3.
[0141] (Examples 2-2 to 2-10 and Comparative Examples 2-1 to 2-5) An adhesive polyamide film having an adhesive modified layer was obtained in the same manner as in Example 2-1, except that the raw resin composition was changed as shown in Table 3. The evaluation results of the obtained adhesive polyamide film are shown in Table 3. The polyamide resins at least partly made from biomass-derived raw materials, namely polyamide 410, polyamide 610, and polyamide 1010, were as follows: Polyamide 410: (DSM, ECOPaXX Q150-E, melting point 250°C, biomass content 71%) Polyamide 610: (Arkema, RilsanS SMNO, melting point 222°C, biomass content 62.5%) Polyamide 1010: (Arkema, RilsanT TMNO, melting point 202°C, biomass content 50%) However, in Example 2-7, the coating liquid used was the coating liquid (B): an aqueous dispersion of a polyurethane resin, and an easily adhesive polyamide film having an adhesion-modifying layer (PU) laminated thereon was obtained. The heat setting and relaxation treatments in Example 2-6 and Comparative Example 2-2 were carried out at 210°C. In Comparative Example 2-4, the molten resin could not be stably extruded from the T-die into a film, and a homogeneous unstretched film could not be obtained, so that biaxial stretching was not possible.
[0142] [Table 3]
[0143] As shown in Table 3, the films obtained in the examples had both good pinhole resistance due to bending and good pinhole resistance due to friction. In addition, the films had low haze and good transparency, high impact strength, and high lamination strength with the sealant film, making them excellent as packaging films. The biaxially oriented polyamide films of Comparative Examples 2-1 and 2-2, which do not contain a polyamide resin, at least part of whose raw materials is derived from biomass and which has the effect of improving pinhole resistance due to bending, and the biaxially oriented polyamide film of Comparative Example 2-3, which has too little polyamide 11 content, had poor pinhole resistance due to bending. In Comparative Example 2-4, the content of polyamide 11 was too high, so the molten resin could not be stably extruded into a film from the T-die, and a homogeneous unstretched film was not obtained, and a biaxially stretched polyamide film was not obtained. In Comparative Example 2-5, the polyamide elastomer conventionally used as a material for improving pinhole resistance was used, and the pinhole resistance was good but the pinhole resistance due to friction was poor. In addition, there was a drawback that deterioration materials were easily attached to the die during long-term production, making it impossible to carry out long-term continuous production.
[0144] (Example 3-1) Using an apparatus consisting of two extruders and a 380 mm wide co-extrusion T-die, the layers were laminated in a B layer / A layer / B layer configuration using the feed block method, and the molten resin was extruded from the T-die into a film. The film was then cast onto a cooling roll controlled at 20°C and electrostatically adhered to obtain an unstretched film with a thickness of 200 μm. The resin compositions of layers A and B are as follows. Resin composition constituting layer A: a polyamide resin composition consisting of 97 parts by mass of polyamide 6 (manufactured by Toyobo Co., Ltd., relative viscosity 2.8, melting point 220°C) and 3.0 parts by mass of polyamide 11 (manufactured by Shuseisha, relative viscosity 2.5, melting point 186°C, biomass content 100%). Resin composition constituting layer B: A resin composition consisting of 95 parts by mass of polyamide 6 (manufactured by Toyobo Co., Ltd., relative viscosity 2.8, melting point 220°C), 5.0 parts by mass of polyamide MXD6 (manufactured by Mitsubishi Gas Chemical Co., Ltd., relative viscosity 2.1, melting point 237°C), 0.54 parts by mass of porous silica microparticles (manufactured by Fuji Silysia Chemical Ltd., average particle diameter 2.0 μm, pore volume 1.6 ml / g), and 0.15 parts by mass of fatty acid bisamide (ethylene bisstearic acid amide, manufactured by Kyoeisha Chemical Co., Ltd.). The feed block configuration and extrusion volume were adjusted so that the biaxially oriented polyamide film had a total thickness of 15 μm, with the base layer (layer A) having a thickness of 12 μm and the front and back functional layers (layer B) each having a thickness of 1.5 μm. The obtained unstretched film was introduced into a roll-type stretching machine, and using the difference in peripheral speed of the rolls, it was stretched 1.73 times in the MD direction at 80 ° C., and then further stretched 1.85 times at 70 ° C. Subsequently, the coating liquid (A) was applied to this uniaxially stretched film with a roll coater, and then it was continuously introduced into a tenter-type stretching machine while drying with hot air at 70 ° C., and after preheating at 110 ° C., it was stretched 1.2 times at 120 ° C., 1.7 times at 130 ° C., and 2.0 times at 160 ° C. in the TD direction, and then heat-set at 215 ° C., and then relaxed by 7% at 215 ° C., and wound up to obtain a biaxially stretched polyamide film laminated with an adhesive modification layer (AEG). The evaluation results of the obtained easy-adhesion polyamide film are shown in Table 4.
[0145] (Examples 3-2 to 3-9) A biaxially stretched polyamide film having an adhesion-modifying layer was obtained in the same manner as in Example 3-1, except that the resin compositions of the A layer and B layer were changed as shown in Table 4. The evaluation results of the obtained highly adhesive polyamide film are shown in Table 4. However, in Examples 3-8 and 3-9, the coating liquid (B): an aqueous dispersion of polyurethane resin was used as the coating liquid to obtain an easily adhesive polyamide film laminated with an adhesion-modifying layer (PU). (Comparative Examples 3-1 to 3-5) The resin composition of the raw material shown in Table 4 was used, and instead of forming an adhesiveness-modifying layer in order to increase the adhesiveness, heat setting and relaxation treatments were performed, and then the film surface on the side to be dry-laminated with the linear low-density polyethylene film was subjected to corona discharge treatment. The evaluation results are shown in Table 4. However, in Comparative Example 3-3, the content of polyamide 11 was too high, so the molten resin could not be stably extruded into a film from the T-die, and a homogeneous unstretched film could not be obtained, so biaxial stretching was not possible.
[0146] [Table 4]
[0147] As shown in Table 4, the films of the examples had good resistance to pinholes due to bending and pinholes due to friction. They also had low haze, good transparency, and good slipperiness. They also had high impact strength and high lamination strength with the sealant film, making them excellent as packaging films. In addition, due to the presence of the adhesive modification layer, they had excellent water-resistant lamination strength. In addition, from the haze and dynamic friction coefficient values of the films obtained in Examples 3-2, 3-6, and 3-7, it can be seen that by incorporating fine particles, an organic lubricant, and polyamide MXD6 in layer B (functional layer), a biaxially oriented polyamide film with excellent properties in both transparency and slipperiness can be obtained. The biaxially oriented polyamide film of Comparative Example 3-1 that does not contain polyamide 11 and the biaxially oriented polyamide film of Comparative Example 3-2 that has a low content of polyamide 11 were inferior in bending pinhole resistance. In addition, since there was no adhesiveness-modifying layer, the water-resistant laminate strength was also low. In Comparative Example 3-3, the content of polyamide 11 was too high, so the molten resin could not be stably extruded into a film from the T-die, and therefore a homogeneous unstretched film could not be obtained, and a biaxially stretched polyamide film could not be obtained. In Comparative Example 3-4, the polyamide elastomer conventionally used as a material for improving pinhole resistance was used, and the pinhole resistance was good but the pinhole resistance at friction was poor. In addition, there was a drawback that deterioration materials were easily attached to the die during long-term production, making it impossible to carry out long-term continuous production. In Comparative Example 3-5, the biaxially oriented polyamide film of the present invention was not provided with an adhesiveness-modifying layer, but instead was corona-treated to improve adhesiveness. The bending pinhole resistance and friction pinhole resistance were good, but the water-resistant laminate strength was low.
[0148] (Example 4-1) An adhesive biaxially stretched polyamide film having an adhesive modification layer (AEG) was obtained in the same manner as in Example 3-1, except that the heat setting temperature and relaxation temperature were set to 218° C. The evaluation results of the obtained adhesive polyamide film are shown in Table 5.
[0149] (Examples 4-2 to 4-11 and Comparative Examples 4-1 to 4-7) An easily adhesive polyamide film was obtained in the same manner as in Example 4-1, except that the resin compositions of the A layer and the B layer, the heat setting temperature, and other film-forming conditions were changed as shown in Table 5. The evaluation results of the obtained easily adhesive polyamide film are shown in Table 5. However, in Example 4-8, the coating liquid (B): an aqueous dispersion of polyurethane resin was used as the coating liquid, and an easily adhesive polyamide film having an adhesion-modifying layer (PU) laminated thereon was obtained. The heat setting and relaxation treatments in Example 4-6 and Comparative Example 4-2 were carried out at 210°C. In addition, in Comparative Example 4-4, the content of polyamide 11 in the base layer was too high, so the molten resin could not be stably extruded into a film from the T-die, and a homogeneous unstretched film could not be obtained, so biaxial stretching was not possible.
[0150] [Table 5]
[0151] As shown in Table 5, the films obtained in the examples had both good bending pinhole resistance and good abrasion pinhole resistance. In addition, the films had low haze and good transparency, high impact strength, and high laminate strength with the sealant film and water-resistant laminate strength, making them excellent as packaging films. In Comparative Examples 4-1 and 4-2, the polyamide films that did not contain polyamide resin, at least part of whose raw materials are derived from biomass, which has the effect of improving pinhole resistance due to bending, and the polyamide film in Comparative Example 4-3, which had too little polyamide 11 content, had poor pinhole resistance due to bending. In Comparative Example 4-4, since the content of polyamide 11 was too high, the molten resin could not be stably extruded into a film from the T-die, and a homogeneous unstretched film was not obtained, and neither a biaxially stretched polyamide film was obtained. In Comparative Example 4-5, since the thickness and thickness ratio of layer A were small, the film had poor pinhole resistance due to bending. In Comparative Example 4-6, the amount of polyamide 6 resin in layer B was small, so that the film was inferior in bending pinhole resistance and abrasion pinhole resistance. In Comparative Example 4-7, the polyamide elastomer conventionally used as a material for improving pinhole resistance was used, and the pinhole resistance was good but the pinhole resistance due to friction was poor. In addition, there was a drawback that deterioration materials were easily attached to the die during long-term production, making it impossible to carry out long-term continuous production. [Industrial Applicability]
[0152] The highly adhesive polyamide film of the present invention is excellent in impact resistance, bending pinhole resistance, and friction pinhole resistance at the same time, and therefore can be suitably used as a packaging material for food packaging, etc. In addition, since the film has high laminate strength and water-resistant laminate strength, it is possible to provide various packaging bags that are difficult to tear during transportation, boiling treatment, etc. Furthermore, since the film uses a resin polymerized from raw materials derived from biomass that is originally on the ground, it is a carbon-neutral film, and can reduce the environmental load by having little effect on the increase or decrease of carbon dioxide on the ground.
Claims
1. A coating amount of 0.01 to 3 g / m2 as a solid content is applied to at least one side of a biaxially oriented polyamide film having a functional layer (B layer) as described below laminated on at least one side of the substrate layer (A layer) as described below. 2 1. An easily adhesive polyamide film, comprising an adhesion modifying layer made of any one of a polyester resin, a polyurethane resin, and / or a polyacrylic resin. The base layer (A layer) contains 99 to 70 mass% polyamide 6 resin and 1 to 30 mass% polyamide resin at least part of which is derived from biomass as a raw material, and does not contain a polyamide-based elastomer, and the functional layer (B layer) contains 70 mass% or more polyamide 6 resin.
2. The radioactive carbon (C 14 2. The highly adhesive polyamide film according to claim 1, characterized in that the content of carbon derived from biomass as measured by a carbon dioxide gas saturation test is 1 to 15%.
3. The highly adhesive polyamide film according to claim 1 or 2, characterized in that the polyamide resin, at least a part of which is derived from biomass as a raw material, is at least one polyamide resin selected from the group consisting of polyamide 11, polyamide 410, polyamide 610, and polyamide 1010.
4. 4. The highly adhesive polyamide film according to claim 1, which satisfies the following (a) and (b): (a) the number of Gelbo pinhole defects is 10 or less when a twisting and bending test using a Gelbo flex tester is performed 1,000 times at a temperature of 1° C.; (b) In the abrasion pinhole resistance test, the distance until pinholes appear is 2,900 cm or more.
5. 5. The highly adhesive polyamide film according to claim 1, wherein the laminate strength after being attached to a polyethylene sealant film is 4.0 N / 15 mm or more.
6. A laminated film comprising the highly adhesive polyamide film according to any one of claims 1 to 5 and a sealant film laminated thereon.
7. A packaging bag using the laminated film according to claim 6.
Citation Information
Patent Citations
Biaxially oriented polyamide film and production thereof
JP1996047972A
Magnetic recording medium
JP1997007163A
Polyamide laminated film
JP1999254615A
Laminate having excellent pinhole resistance and packaging bag using it