Laminate and packaging using same

The laminate with a polyester resin heat-sealing layer and inorganic thin film layer addresses adsorption, sealing strength, and gas barrier issues, ensuring effective packaging for foods and pharmaceuticals.

JP7581881B2Active Publication Date: 2024-11-13TOYOBO CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020559972
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-06
Filing Date
2019-12-04
Publication Date
2024-11-13
Estimated Expiration
2039-12-04

AI Technical Summary

Technical Problem

Conventional packaging materials face issues with adsorption of organic compounds, low heat sealing strength at low temperatures, poor gas barrier properties, heat shrinkage, and inadequate concealment, making them unsuitable for certain products like foods and pharmaceuticals.

Method used

A laminate structure comprising a heat-sealing layer made of polyester resin, an inorganic thin film layer, and optionally a heat-resistant layer, with specific properties such as heat-sealing strength, gas barrier properties, and optical density to address these issues.

Benefits of technology

The laminate provides high heat-sealing strength, effective gas barrier properties, low heat shrinkage, and concealment, ensuring the contents remain intact and unaltered over time, even after heat treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581881000004
    Figure 0007581881000004
  • Figure 0007581881000001
    Figure 0007581881000001
  • Figure 0007581881000002
    Figure 0007581881000002
Patent Text Reader

Abstract

The present invention provides a laminate that exhibits low component adsorption of contents, high heat seal strength in a low temperature range, and excellent gas barrier properties, low heat shrinkage, heat resistance, and hiding properties. [Solution] A laminate having at least a heat seal layer and an inorganic thin film layer, characterized in that the laminate satisfies the following requirements (1) to (5). (1) At least one of the laminates has a heat seal layer on the outermost surface thereof, the heat seal layer is made of a polyester resin containing ethylene terephthalate as the main component, and the heat seal layer has a seal strength of 8N / 15mm or more and 30N / 15mm or less when sealed together at 140°C, 0.2MPa, and 2 seconds. (2) The water vapor permeability is 0.05 g / m under the condition of 40°C temperature and 90% relative humidity. 2 ·d] or more 4[g / m 2 ·d] or less (3) The oxygen permeability is 0.05 cc / m under the condition of 23°C temperature and 65% relative humidity. 2 ·d·atm] or more 4[cc / m 2 ·d·atm] or less (4) Optical density (OD value) is 1 or more and 5 or less (5) After immersion in 98°C hot water for 3 minutes, the thermal shrinkage rate is between -5% and 5% in both the longitudinal and transverse directions. [Selected Figure] Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate having a polyester resin layer that is excellent in gas barrier property, heat seal strength and hiding power, and a package using the same. [Background technology]

[0002] Conventionally, laminated films obtained by heat sealing or laminating sealant films have been used as packaging materials such as packages and lids for many of the distribution goods represented by food, medicines, and industrial products. The innermost surface of the packaging material (the surface that comes into contact with the contents) is provided with a sealant layer made of a polyolefin resin such as polyethylene or polypropylene, which exhibits high sealing strength, or a copolymer resin such as ionomer or EMMA. It is known that these resins can achieve high adhesion strength by heat sealing.

[0003] However, the non-stretched sealant film made of polyolefin resin as described in Patent Document 1 has the disadvantage that it is prone to adsorbing organic compounds such as fats and oils and fragrances, and therefore tends to change the scent and taste of the contents. Therefore, it is often not suitable to use a sealant layer made of polyolefin resin as the innermost layer in packaging for chemical products, medicines, food, etc.

[0004] On the other hand, a sealant made of an acrylonitrile resin as described in Patent Document 2 is suitable for use as the innermost layer of a packaging material because it does not easily adsorb organic compounds contained in chemical products, medicines, foods, etc. However, acrylonitrile films have a problem of low heat seal strength in the low temperature range (150°C or less). In the bag making process, if the heat seal temperature becomes high, the maintenance frequency of the seal bar increases, which is not preferable from the viewpoint of productivity. In addition, in order to improve the yield of bags, the speed of bag making lines is increasing, and a low sealing temperature is preferable for this requirement. A sealant made of an acrylonitrile resin does not satisfy these requirements.

[0005] In view of such problems, Patent Document 3 discloses a polyester-based sealant that is non-adsorbent of organic compounds and has low-temperature sealing properties. However, the sealant in Patent Document 3 has a problem that not only does it shrink due to heat during heat sealing, but the sealant melts and develops holes. For example, when producing a package using the sealant, if the sealant shrinks due to heat, not only will the shape of the bag be distorted, but if holes are developed, the bag will not be able to perform its preservation function, which is undesirable. Thus, the sealant in Patent Document 3 has room for improvement in heat resistance.

[0006] Therefore, Patent Document 4 discloses a sealant with improved heat resistance. The sealant of Patent Document 4 satisfies heat sealability and heat resistance by separating a layer having heat sealability from other layers and separately controlling the raw material composition of each of these layers. However, the sealant described in Patent Document 4 does not have the ability to block gases such as oxygen and water vapor (gas barrier properties), so there is a problem that the shelf life of the contents is short. In addition, although it has a certain degree of heat resistance as described above, its heat resistance against the heating treatment and heat history described below is insufficient.

[0007] Conventionally, a well-known method for improving the gas barrier properties of a film is to provide an inorganic thin film layer by vapor deposition. For example, Patent Document 5 discloses a lid material in which a gas barrier layer made of an inorganic oxide is provided on a polyester film substrate by vapor deposition, and a heat-sealable resin film is further laminated thereon. However, the material of the heat-sealable resin film used in Patent Document 5 is polyethylene, which has a problem with non-adsorption to the contents. In contrast, Patent Document 6 discloses a laminate in which an inorganic thin film layer is provided on a sealant made of a polyester material to improve the gas barrier properties. However, the present inventors have found that when a package is produced using the laminate described in Patent Document 6 and subjected to a heat treatment such as boiling treatment, not only does the package deform due to the heat shrinkage of the sealant, resulting in a poor appearance, but also cracks are generated in the inorganic thin film layer, resulting in a decrease in gas barrier properties. In other words, the production of a low-adsorption sealant having gas barrier properties and heat resistance was impossible at the conventional technical level. Furthermore, since the sealant film in Patent Document 6 is transparent, it also has the disadvantage of being poor in concealing the contents when used as a package. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 3817846 [Patent Document 2] Japanese Patent Application Publication No. 7-132946 [Patent Document 3] International Publication No. 2014-175313 [Patent Document 4] JP 2017-165059 A [Patent Document 5] JP 2006-27695 A [Patent Document 6] JP 2017-165060 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention aims to solve the problems of the conventional techniques as described above. That is, the object of the present invention is to provide a laminate which exhibits low component adsorption of the contents, high heat seal strength in a low temperature range, and excellent gas barrier properties, low heat shrinkage properties, heat resistance, and hiding properties. At the same time, the object of the present invention is to provide a package containing the above-mentioned laminate as at least one layer, and to provide the above-mentioned laminate having an overcoat layer laminated thereon, and a package containing the laminate as at least one layer. [Means for solving the problem]

[0010] The present invention comprises the following configurations. 1. A laminate having at least a heat seal layer and an inorganic thin film layer, characterized in that the laminate satisfies the following requirements (1) to (5). (1) At least one of the laminates has a heat seal layer on the outermost surface thereof, the heat seal layer is made of a polyester-based component mainly composed of ethylene terephthalate, and the heat seal layer has a seal strength of 8N / 15mm or more and 30N / 15mm or less when sealed together at 140°C, 0.2MPa, and 2 seconds. (2) The water vapor permeability at a temperature of 40°C and a relative humidity of 90% is 0.1 [g / m 2 ·d] or more and 2[g / m2·d] or less (3) The oxygen permeability is 0.3 [cc / (m 2 ·d·atm)] or more 3[cc / (m 2 ·d·atm)] or less (4) Optical density (OD value) is 1 to 5 (5) After immersing in 98°C hot water for 3 minutes, the thermal shrinkage rate is between -5% and 5% in both the longitudinal and transverse directions. 2. The laminate according to 1 above, wherein the maximum value of the molecular orientation angle measured in the width direction is from 0 degrees to 35 degrees. 3. The laminate according to any one of 1 or 2 above, wherein the main component of the inorganic material constituting the inorganic thin film layer is aluminum. 4. A laminate according to any one of 1 to 3 above, which has a heat-resistant layer in addition to the heat seal layer and the inorganic thin film layer, and which is made of a polyester resin containing ethylene terephthalate as a main component. 5. The laminate according to any one of 1 to 4 above, wherein the folded angle is 20 degrees or more and 70 degrees or less. 6. A laminate according to any one of 1 to 5 above, characterized in that the monomer components of the polyester resin constituting the heat seal layer contain a diol monomer component other than ethylene glycol and an acid component other than terephthalic acid, the diol monomer component contains one or more of neopentyl glycol, 1,4-cyclohexanedimethanol, 1,4-butanediol, and diethylene glycol, and the acid component contains isophthalic acid. 7. A packaging material comprising at least one layer of the laminate described in any one of 1 to 6 above. 8. The laminate according to any one of the above items 1 to 7, further comprising an overcoat layer laminated on the inorganic thin film layer. 9. A packaging material comprising at least one layer of the laminate described in 8 above. Effect of the Invention

[0011] The laminate of the present invention exhibits low component adsorption of the contents, has high heat seal strength at low temperatures, and is excellent in gas barrier properties, low shrinkage, heat resistance, and concealment properties. Therefore, when used as a packaging material, it can exhibit high seal strength, conceal the contents, and not only does it prevent the components of the contents from decreasing over a long period of time even after heat treatment, but it can also suppress deterioration. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a schematic diagram of a method for measuring a folding holding angle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention relates to a laminate having at least a heat seal layer and an inorganic thin film layer, which is characterized by satisfying the following requirements (1) to (5). (1) At least one of the laminates has a heat seal layer on the outermost surface thereof, the heat seal layer is made of a polyester resin containing ethylene terephthalate as a main component, and the heat seal layer has a seal strength of 8N / 15mm or more and 30N / 15mm or less when sealed together at 140°C, 0.2MPa, and 2 seconds. (2) The water vapor permeability at a temperature of 40°C and a relative humidity of 90% is 0.1 [g / m 2 ·d] or more and 2[g / m2·d] or less (3) The oxygen permeability at a temperature of 23°C and a relative humidity of 65% is 0.3 [cc / (m 2 ·d·atm)] or more 3[cc / (m 2 ·d·atm)] or less (4) Optical density (OD value) is 1 to 5 (5) After immersing in 98°C hot water for 3 minutes, the thermal shrinkage rate is between -5% and 5% in both the longitudinal and transverse directions.

[0014] The laminate of the present invention will now be described. 1.Layer structure, thickness, and layer ratio of laminate The laminate of the present invention must have at least one heat seal layer and at least one inorganic thin film layer in order to achieve both heat sealability and gas barrier property. Furthermore, in order to achieve a predetermined heat seal strength, the heat seal layer must be provided on either one of the outermost layers of the laminate. The inorganic thin film layer may be located either on the outermost layer or as an intermediate layer (in the case of three or more layers) of the laminate. The laminate of the present invention preferably has a three-layer structure including the above-mentioned two layers and a heat-resistant layer. The heat-resistant layer is preferably made of a polyester resin containing ethylene terephthalate as a main component, and may be located either as the outermost layer or as an intermediate layer, but is preferably an intermediate layer. The constituent requirements for each layer will be described later, but in the case of a structure including a heat seal layer and a heat-resistant layer, the layer with the highest content of ethylene terephthalate components becomes the heat-resistant layer.

[0015] The layer structure of the laminate of the present invention is more preferably configured, from the outermost layer on either side, of a heat seal layer / a heat resistant layer / an inorganic thin film layer in that order. The laminate of the present invention may also have an overcoat layer on the outermost layer opposite to the heat seal layer. In this case, a structure in which four layers are laminated in the order of heat seal layer / heat-resistant layer / inorganic thin film layer / overcoat layer is preferable. By providing an overcoat layer, not only is the gas barrier property improved, but the laminate strength when laminated with other materials is improved, and the occurrence of cracks due to rubbing or bending can be suppressed, and other advantages are obtained.

[0016] The thickness of the laminate is not particularly limited, but is preferably 3 μm or more and 200 μm or less. If the thickness of the laminate is thinner than 3 μm, it is not preferable because there is a risk of insufficient heat seal strength and processing such as printing becoming difficult. The thickness of the laminate may be thicker than 200 μm, but it is not preferable because the weight of the laminate used increases and the cost increases. The thickness of the laminate is more preferably 5 μm or more and 160 μm or less, and even more preferably 7 μm or more and 120 μm or less.

[0017] The layer ratio of the heat seal layer to the total thickness of the laminate is preferably 20% or more and 80% or less. If the layer ratio of the heat seal layer is less than 20%, the heat seal strength of the laminate may decrease, which is not preferable. If the layer ratio of the heat seal layer is higher than 80%, the heat sealability of the laminate is improved, but the heat resistance may decrease, which is not preferable. The layer ratio of the heat seal layer is more preferably 30% or more and 70% or less.

[0018] Regarding the thickness of the inorganic thin film layer, when the inorganic thin film layer is a vapor-deposited metal layer, it is preferably 2 nm or more and 100 nm or less (details on the inorganic thin film layer will be described later). If the thickness of this layer is less than 2 nm, it is not preferable because it is difficult to satisfy the specified water vapor permeability, oxygen permeability (gas barrier property), and optical density (concealing property). On the other hand, even if the thickness of this layer exceeds 100 nm, it is not preferable because there is no corresponding improvement effect in gas barrier property and the manufacturing cost increases. The thickness of the inorganic thin film layer (vapor-deposited metal layer) is more preferably 5 nm or more and 97 nm or less, and even more preferably 8 nm or more and 94 nm or less. When the inorganic thin film layer is a metal foil, the thickness of the metal foil is preferably 3 μm or more and 200 μm or less. If the thickness of this layer is less than 3 μm, it is not preferable because it is difficult to satisfy the specified water vapor permeability, oxygen permeability (gas barrier property), and optical density (concealment property). On the other hand, even if the thickness of this layer exceeds 200 μm, it is not preferable because there is no corresponding improvement effect in gas barrier property and the manufacturing cost increases. The thickness of the inorganic thin film layer (metal foil) is more preferably 5 μm or more and 197 μm or less, and even more preferably 8 μm or more and 194 μm or less.

[0019] The layer ratio of the heat-resistant layer is preferably 20% or more and 80% or less. If the layer ratio of the heat-resistant layer is less than 20%, the heat resistance of the film may decrease, which is not preferable. If the layer ratio of the heat-resistant layer is higher than 80%, the ratio of the heat seal layer of the laminate decreases accordingly, which is not preferable because the heat sealability may be sacrificed and deteriorated. The layer ratio of the heat-resistant layer is more preferably 30% or more and 70% or less.

[0020] When an overcoat layer is provided, the thickness of this layer is preferably 0.1 μm or more and 3 μm or less. If the thickness of the overcoat layer is thinner than 0.1 μm, it may be difficult to satisfy the predetermined gas barrier property or the laminate strength may be reduced. On the other hand, even if the thickness of this layer exceeds 3 μm, the corresponding improvement effect of the gas barrier property and the laminate strength is reduced, and the manufacturing cost is increased, so it is not preferable. In addition, the outermost layer (including the heat seal layer) of the laminate of the present invention may be provided with a layer that has been subjected to corona treatment, coating treatment, flame treatment, or the like in order to improve the printability and slipperiness of the film surface, and may be provided as desired within the scope of the present invention. In the following description, layers made of polyester resins, such as a heat seal layer and a heat resistant layer, are collectively referred to as a "polyester resin layer" to be distinguished from an inorganic thin film layer and an overcoat layer.

[0021] 2. Properties of the laminate 2.1.Heat seal strength The heat seal strength when the heat seal layers of the laminate of the present invention are heat sealed at a temperature of 140° C., a seal bar pressure of 0.2 MPa, and a sealing time of 2 seconds must be 8 N / 15 mm or more and 30 N / 15 mm or less. If the heat seal strength is less than 8N / 15mm, the sealed portion is easily peeled off by boiling treatment, etc., and therefore the material cannot be used as a package. The heat seal strength is preferably 9N / 15mm or more, and more preferably 10N / 15mm or more. Although a high heat seal strength is preferable, the upper limit currently available is about 30N / 15mm.

[0022] 2.2.Water vapor permeability The laminate of the present invention has a water vapor permeability of 0.1 [g / m2·d] or more and 2 g / m2 or more when measured under an environment of a temperature of 40°C and a relative humidity of 90%. 2 It must be less than 2 [g / m2·d]. If it is used as a package containing contents, the shelf life of the contents will be shortened, which is not desirable. On the other hand, if the water vapor permeability is less than 0.1 [g / m 2 ·d] is preferable because it increases the gas barrier properties and extends the shelf life of the contents, but the current state of the art limits this to 0.1 [g / m 2 ·d] is the lower limit. The lower limit of water vapor permeability is 0.15 [g / m 2 ·d] is sufficient for practical use. The upper limit of water vapor permeability is 1.5 [g / m 2 ·d], and 1 [g / m 2·d] is more preferable.

[0023] 2.3.Oxygen permeability The laminate of the present invention has an oxygen permeability of 0.3 [cc / (m 2 ·d·atm)] or more 3[cc / (m 2 ·d·atm)] or less. Oxygen permeability is 3 [cc / (m 2 ·d·atm)] is undesirable because it shortens the shelf life of the contents. On the other hand, if the oxygen permeability is 0.3 [cc / (m 2 If the oxygen permeability is less than 0.3 [cc / (m 2 The lower limit of oxygen permeability is 0.35 [cc / (m 2 ·d·atm)] is sufficient for practical use. The upper limit of oxygen permeability is 2.5 [cc / (m 2 ·d·atm)], and 2 [cc / (m 2 It is more preferable that the sintering temperature is 100°C or less.

[0024] 2.4.Optical Density (OD value) The laminate of the present invention must have an optical density (OD value) of 1 or more and 5 or less. The OD value is a logarithmic representation of the attenuation rate of light measured by the method described below, and the larger the value, the less light is transmitted. If the OD value is below 1 (light transmittance exceeds 10%), the concealing property of the sealant decreases, and the contents are easily visible when the sealant is used as a package, which is not preferable. On the other hand, the higher the OD value, the better the concealing property, which is preferable, but the current technical level has an upper limit of OD value of 5. Even if the upper limit of the OD value is 4.8, it can be said that it is sufficient for practical use. The lower limit of the OD value is preferably 1.2, and more preferably 1.4.

[0025] 2.5. Molecular orientation angle in the width direction The laminate of the present invention preferably has a maximum molecular orientation angle of 35 degrees or less when measured over a predetermined length in the width direction (including a film slit into a small width after a film having the entire width is formed). The molecular orientation angle is an index showing how straight the molecular chains in the layer (film) made of polyester resin constituting the laminate are aligned over the entire width of the film. A large molecular orientation angle means that the molecular chains are aligned in a distorted manner. A phenomenon generally called bowing, in which the molecular orientation of a film is distorted in a bow shape over the width direction, tends to increase the molecular orientation angle at the end. The maximum molecular orientation angle is considered to be an index showing the magnitude of bowing. When the molecular orientation angle is 0 degrees, the bowing phenomenon does not occur, and the molecular orientation angle can be said to be aligned straight over the width direction. When the molecular orientation angle of the laminate exceeds 30 degrees, the distortion of the film tends to cause uneven lamination (vapor deposition) of the inorganic thin film layer, which may reduce the water vapor permeability and oxygen permeability. The maximum molecular orientation angle is more preferably 30 degrees or less, and even more preferably 25 degrees or less. The most preferable lower limit of the molecular orientation angle is 0 degree, as described above.

[0026] 2.6.Heat shrinkage rate The laminate of the present invention preferably has a hot water heat shrinkage rate of -5% or more and 5% or less in both the width direction and the length direction when treated in hot water at 98°C for 3 minutes. If the hot water heat shrinkage rate exceeds 5%, when a bag made using the laminate is subjected to a heat treatment such as a retort treatment, not only does the bag deform significantly and cannot maintain its original shape, but also cracks occur in the layer made of inorganic substances, which is undesirable because the gas barrier property is reduced. It is more preferable that the hot water heat shrinkage rate is 4% or less, and even more preferable that it is 3% or less. On the other hand, if the hot water heat shrinkage rate is less than -5%, it means that the laminate stretches, and it is undesirable because the bag is less able to maintain its original shape as in the case of a high shrinkage rate. It is more preferable that the hot water heat shrinkage rate of the laminate is -4% or more and 4% or less, and even more preferable that it is -3% or more and 3% or less.

[0027] 2.7.Folding angle The laminate of the present invention preferably has a folding angle of 20 degrees or more and 70 degrees or less, as measured by the method described below. If the folding angle exceeds 70 degrees, it is difficult to make a crease when the laminate is made into a bag, which is undesirable because it results in a poor appearance. On the other hand, the smaller the folding angle, the more preferable it is, but the range that can be covered by the present invention is 20 degrees as the lower limit, and even if the folding angle is 25 degrees or more, it can be said that it is practically preferable. The upper limit of the folding angle is more preferably 65 degrees, and even more preferably 60 degrees.

[0028] 2.8.Type of contents and adsorption amount The laminate of the present invention has a feature of being less likely to adsorb organic compounds contained in chemical products, medicines, foods, etc. When the laminate is used as a package, the heat seal layer is usually the innermost layer, and therefore the adsorption amount of the laminate of the present invention described in this section refers to the amount of the contents that the heat seal layer adsorbs. Examples of the organic compounds include aroma components and medicinal components such as d-limonene, citral, citronellal, p-menthane, pinene, terpinene, myrcene, carene, geraniol, nerol, citronellal, terpineol, l-menthol, nerolidol, borneol, dl-camphor, lycopene, carotene, trans-2-hexenal, cis-3-hexenol, β-ionone, selinene, 1-octen-3-ol, benzyl alcohol, octyltulobuterol hydrochloride, and tocopherol acetate. The amount of adsorption to the laminate varies depending on the adsorption conditions (concentration of the adsorbent, storage period, temperature, etc.), but the amount of adsorption after storage for one week according to the method shown in the examples below is 0 μg / cm 2 2μg / cm or more 2 It is preferable that the adsorption amount is 0 μg / cm 2 indicates that the contents were not adsorbed to the sealant at all. The amount of adsorption was 1.8 μg / cm 2 More preferably, it is 1.6 μg / cm or less. 2 It is even more preferable that the ratio is less than or equal to the above. Since the laminate of the present invention has a heat seal layer made of a polyester resin, there is a risk of increased adsorption of organic compounds with a similar chemical structure. Specifically, since the polyester resin constituting the sealant has four oxygen atoms in the repeating unit of the constituent components, the greater the number of oxygen atoms in the chemical structure of the organic compound (approaching four), the greater the solubility of the organic compound in the sealant and the greater the adsorptivity. For example, when packaging contents containing eugenol, which has two oxygen atoms, or methyl salicylate, which has three oxygen atoms, the amount of adsorption is 2 μg / cm. 2 This is not desirable because it is easy to exceed the limit.

[0029] 3. Raw materials for laminates 3.1. Raw material type of polyester resin layer The raw material type of the polyester-based resin layer constituting the laminate of the present invention is one that contains ethylene terephthalate units as a main component. Here, "containing ethylene terephthalate units as a main component" means that the content of ethylene terephthalate units is 50 mol % or more when the total amount of all components is 100 mol %. In addition, it is preferable that the polyester used in the polyester-based resin layer of the present invention contains at least one component other than ethylene terephthalate. This is because the presence of a component other than ethylene terephthalate improves the heat seal strength of the heat seal layer. In the heat-resistant layer, it is preferable that the amount of components other than ethylene terephthalate is small, but by containing a component other than ethylene terephthalate, the shrinkage difference with the heat seal layer can be reduced, and curling of the laminate can be reduced. The content of each component differs between the heat seal layer and the heat-resistant layer, and will be described later. Examples of dicarboxylic acid monomers that can be components other than terephthalic acid that constitute ethylene terephthalate include aromatic dicarboxylic acids such as isophthalic acid, 1,4-cyclohexanedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and orthophthalic acid, aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, and decanedicarboxylic acid, and alicyclic dicarboxylic acids. Among the above carboxylic acid components, isophthalic acid is preferable because it makes it easier to make the heat seal strength between the heat seal layers 8N / 15mm or more. However, it is preferable not to incorporate trivalent or higher polyvalent carboxylic acids (eg, trimellitic acid, pyromellitic acid, and anhydrides thereof) into the polyester.

[0030] Examples of diol monomers that can be components other than ethylene glycol constituting ethylene terephthalate include long-chain diols such as neopentyl glycol, 1,4-cyclohexanedimethanol, diethylene glycol, 2,2-diethyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-isopropyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, hexanediol, and 1,4-butanediol, aliphatic diols such as hexanediol, and aromatic diols such as bisphenol A. However, it is preferable that the polyester does not contain a diol having 8 or more carbon atoms (e.g., octanediol, etc.) or a polyhydric alcohol having a valence of 3 or more (e.g., trimethylolpropane, trimethylolethane, glycerin, diglycerin, etc.). Furthermore, the polyester may contain a polyester elastomer containing ε-caprolactone, tetramethylene glycol, etc. The polyester elastomer has the effect of lowering the melting point of the polyester resin layer, and therefore can be suitably used in particular for the heat seal layer.

[0031] Among these, it is preferable to use one or more of neopentyl glycol, 1,4-cyclohexanedimethanol, 1,4-butanediol, and diethylene glycol, since this facilitates achieving a heat seal strength of 8 N / 15 mm or more between the heat seal layers. It is more preferable to use one or more of neopentyl glycol and 1,4-cyclohexanedimethanol, and it is particularly preferable to use neopentyl glycol.

[0032] In the polyester resin layer constituting the laminate of the present invention, various additives such as waxes, antioxidants, antistatic agents, crystal nucleating agents, viscosity reducing agents, heat stabilizers, coloring pigments, coloring inhibitors, ultraviolet absorbers, etc. can be added as necessary. In addition, it is preferable to add fine particles as a lubricant to improve the slipperiness of the film to at least the outermost layer of the film. As the fine particles, any particles can be selected. For example, inorganic fine particles can include silica, alumina, titanium dioxide, calcium carbonate, kaolin, barium sulfate, etc., and organic fine particles can include acrylic resin particles, melamine resin particles, silicone resin particles, crosslinked polystyrene particles, etc. The average particle size of the fine particles can be appropriately selected as necessary within the range of 0.05 to 3.0 μm when measured with a Coulter counter.

[0033] As a method for blending particles into the polyester resin layer constituting the laminate of the present invention, for example, they can be added at any stage of manufacturing the polyester resin, but it is preferable to add them as a slurry dispersed in ethylene glycol or the like at the stage of esterification or after the completion of the transesterification reaction and before the start of the polycondensation reaction, and proceed with the polycondensation reaction. In addition, there is also a method of blending a slurry of particles dispersed in ethylene glycol, water, or other solvent with a polyester resin raw material using a vented kneading extruder, or a method of blending dried particles with a polyester resin raw material using a kneading extruder.

[0034] Preferred components contained in the heat seal layer and the heat resistant layer will be described below.

[0035] 3.2. Amount of polyester raw material contained in heat seal layer The polyester used in the heat seal layer constituting the laminate of the present invention preferably has a content of dicarboxylic acid monomers and / or diol monomers other than terephthalic acid and ethylene glycol constituting ethylene terephthalate of 25 mol % or more, more preferably 27 mol % or more, particularly preferably 29 mol % or more. The upper limit of the content of monomers other than ethylene terephthalate is 50 mol %. If the content of monomers other than the ethylene terephthalate in the heat seal layer is less than 25 mol%, even if the molten resin is rapidly cooled and solidified after being extruded from the die, it will crystallize in the subsequent stretching and heat setting steps, making it difficult to achieve a heat seal strength of 8 N / 15 mm or more, which is not preferable. On the other hand, if the content of the monomer other than the ethylene terephthalate in the heat seal layer is 50 mol % or more, the heat seal strength of the film can be increased, but the heat resistance of the heat seal layer is extremely low, so that the periphery of the sealed portion is blocked during heat sealing (a phenomenon in which a wider area than the intended area is sealed due to heat conduction from the heating member), making it difficult to perform proper heat sealing. The content of the monomer other than the ethylene terephthalate is more preferably 48 mol % or less, and particularly preferably 46 mol % or less.

[0036] 3.3. Amount of polyester raw material contained in heat-resistant layer The polyester used in the heat-resistant layer that can constitute the laminate of the present invention preferably has a content of dicarboxylic acid monomers and / or diol monomers other than terephthalic acid and ethylene glycol that constitute ethylene terephthalate of 9 mol % or more, more preferably 10 mol % or more, and particularly preferably 11 mol % or more. The upper limit of the content of the monomers other than ethylene terephthalate is 20 mol %. If the content of the monomer other than the ethylene terephthalate contained in the heat-resistant layer is less than 9 mol%, the difference in heat shrinkage rate between the heat-sealing layer and the heat-resistant layer becomes large, and the laminate curls more, which is not preferable. If the difference in the content of the monomer other than the ethylene terephthalate contained in the heat-resistant layer and the heat-sealing layer becomes large, the difference in heat shrinkage rate between the layers during heat setting becomes large, and even if cooling after heat setting is strengthened, shrinkage toward the heat-sealing layer becomes large, and curling becomes large. On the other hand, if the content of the monomer other than the ethylene terephthalate in the heat-resistant layer is 20 mol % or more, the heat resistance of the sealant is reduced, such as holes being generated by the heat applied during heat sealing, which is not preferable. The content of the monomer other than the ethylene terephthalate is more preferably 19 mol % or less, and particularly preferably 18 mol % or less. In addition, the content of the monomer other than the ethylene terephthalate for controlling curl is preferably, in addition to the amount in each layer, a difference between the heat seal layer and the heat resistant layer of 20 mol % or more and 35 mol % or less, and more preferably, 21 mol % or more and 34 mol % or less.

[0037] 3.4. Raw material type and composition of inorganic thin film layer The raw material species of the inorganic thin film layer constituting the laminate of the present invention can be a conventionally known material, and can be appropriately selected according to the purpose to satisfy the desired gas barrier properties, etc. Examples of raw material species of the inorganic thin film layer include metals such as silicon, aluminum, tin, zinc, iron, manganese, etc., and inorganic compounds containing one or more of these metals, and examples of the corresponding inorganic compounds include oxides, nitrides, carbides, fluorides, etc. These inorganic substances or inorganic compounds may be used alone or in combination. Among these, aluminum is particularly preferable because it can improve the OD value of the laminate. The metal material for the inorganic thin film layer may be vapor-deposited onto the film by the method described below, or a metal foil may be laminated onto the film.

[0038] 3.5.Types of overcoat layers The type of the overcoat layer that can constitute the laminate of the present invention is not particularly limited, but conventionally known materials such as a composition consisting of a urethane resin and a silane coupling agent, a compound consisting of an organosilicon and its hydrolyzate, a water-soluble polymer having a hydroxyl group or a carboxyl group, etc. can be used, and can be appropriately selected according to the purpose to satisfy the desired gas barrier properties, etc. Among these, a composition consisting of a urethane resin and a silane coupling agent is preferred because it can improve the gas barrier properties while maintaining the flexibility of the laminate. In addition, the overcoat layer may contain one or more additives for the purpose of imparting antistatic properties, UV absorbency, coloring, thermal stability, slip properties, etc., within the scope of the present invention, and the types and amounts of the additives can be appropriately selected depending on the desired purpose.

[0039] 4. Manufacturing conditions of laminate 4.1. Film-forming conditions for polyester resin layer 4.1.1.Melt extrusion The polyester-based resin layer (hereinafter, sometimes simply referred to as a film) constituting the laminate of the present invention can be obtained by melt-extruding the polyester raw material described in 3.1. "Raw material type of polyester-based resin layer" above with an extruder to form an unstretched laminated film, and stretching it by a predetermined method described below. When the film includes a heat seal layer and a heat-resistant layer, or other layers, the timing of laminating each layer may be either before or after stretching. When laminating before stretching, it is preferable to adopt a method in which the resins that are the raw materials for each layer are melt-extruded by separate extruders and joined using a feed block or the like in the middle of the resin flow path. When laminating after stretching, it is preferable to adopt a lamination method in which films formed separately are bonded together with an adhesive, or an extrusion lamination method in which a molten polyester resin is poured on the surface layer of a single or laminated film to laminate it. Among these, the method in which each layer is laminated before stretching is preferable.

[0040] As described above, the polyester resin can be obtained by polycondensation of a dicarboxylic acid component and a diol component selected in type and amount so as to contain an appropriate amount of a monomer that can be a component other than ethylene terephthalate. In addition, two or more kinds of chip-like polyesters can be mixed and used as a raw material for the polyester-based resin layer. When the raw resin is melt-extruded, it is preferable to dry the polyester raw material of each layer using a dryer such as a hopper dryer or a paddle dryer, or a vacuum dryer. After drying the polyester raw material of each layer in this way, it is melted at a temperature of 200 to 300 ° C. using an extruder and extruded as a laminated film. For extrusion, any existing method such as a T-die method or a tubular method can be adopted.

[0041] Thereafter, the film melted by extrusion is quenched to obtain an unstretched film. As a method for quenching the molten resin, a method in which the molten resin is cast from a die onto a rotating drum and quenched and solidified to obtain a substantially unoriented resin sheet can be suitably adopted.

[0042] The film may be produced by any of the following methods: non-stretching, uniaxial stretching (stretching in at least one of the longitudinal (length) direction and the transverse (width) direction), and biaxial stretching. From the viewpoint of the mechanical strength and productivity of the laminate of the present invention, uniaxial stretching is preferred, and biaxial stretching is more preferred. In the following, a sequential biaxial stretching method by longitudinal stretching and transverse stretching, in which longitudinal stretching is carried out first and transverse stretching is then carried out, will be described. However, the order may be reversed (transverse stretching first and longitudinal stretching) since only the main orientation direction is changed. Also, simultaneous biaxial stretching may be used.

[0043] 4.1.2. Longitudinal stretching For longitudinal (longitudinal) stretching, the unstretched film may be introduced into a longitudinal stretching machine in which a plurality of roll groups are arranged in series. For longitudinal stretching, it is preferable to preheat the film with a preheating roll until the film temperature reaches 65°C to 90°C. If the film temperature is lower than 65°C, the film is difficult to stretch when stretched in the longitudinal direction, and breakage is likely to occur, which is not preferable. Also, if the film temperature is higher than 90°C, the film is likely to stick to the roll, and the film may wrap around the roll or the roll may become dirty due to continuous production, which is not preferable. When the film temperature reaches 65°C to 90°C, longitudinal stretching is performed. The longitudinal stretching ratio should be between 1 and 5 times. Since 1 times means that no longitudinal stretching is performed, the longitudinal stretching ratio should be 1 to obtain a uniaxially stretched film, and longitudinal stretching of 1.1 times or more should be performed to obtain a biaxially stretched film. The upper limit of the longitudinal stretching ratio can be any number of times, but if the longitudinal stretching ratio is too high, not only will it be difficult to stretch transversely and breakage will occur, but the molecular orientation angle (bowing) will also become large, so it is preferable that the upper limit is 5 times or less.

[0044] In addition, by relaxing the film in the longitudinal direction after the longitudinal stretching (relaxation in the longitudinal direction), the shrinkage rate in the longitudinal direction of the film caused by the longitudinal stretching can be reduced. Furthermore, by relaxing in the longitudinal direction, the bowing phenomenon (distortion) occurring in the tenter can be reduced. This is because in the later process of transverse stretching and final heat treatment, both ends in the width direction of the film are heated while being held, and only the center part of the film shrinks in the longitudinal direction. The relaxation rate in the longitudinal direction is preferably 0% or more and 70% or less (relaxation rate of 0% means that relaxation is not performed). The upper limit of the relaxation rate in the longitudinal direction is determined by the raw material used and the longitudinal stretching conditions, so relaxation cannot be performed beyond this limit. In the polyester-based sealant of the present invention, the relaxation rate in the longitudinal direction is an upper limit of 70%. Relaxation in the longitudinal direction can be performed by heating the film after the longitudinal stretching at a temperature of 65°C to 100°C or less and adjusting the speed difference of the rolls. Any of rolls, near infrared rays, far infrared rays, hot air heaters, etc. can be used as the heating means. In addition, relaxation in the longitudinal direction does not have to be performed immediately after longitudinal stretching; for example, it can be performed during transverse stretching (including the preheating zone) or final heat treatment by narrowing the clip spacing in the longitudinal direction (in this case, both ends of the film width direction are also relaxed in the longitudinal direction, reducing bowing distortion), and can be performed at any time. After relaxation in the machine direction (longitudinal stretching when relaxation is not performed), the film is preferably cooled once, preferably with a cooling roll having a surface temperature of 20 to 40°C.

[0045] 4.1.3. Lateral stretching After the longitudinal stretching, the film is preferably transversely stretched at a stretch ratio of about 3 to 5 times at 65°C to 110°C in a tenter while both ends in the width direction (direction perpendicular to the longitudinal direction) of the film are held by clips. Before the transverse stretching, it is preferable to preheat the film, and the preheating is preferably performed until the film surface temperature reaches 75°C to 120°C. After the transverse stretching, it is preferable to pass the film through an intermediate zone where no active heating operation is performed. Since the temperature in the next final heat treatment zone is higher than that in the transverse stretching zone of the tenter, if an intermediate zone is not provided, the heat (hot air itself or radiant heat) from the final heat treatment zone will flow into the transverse stretching process. In this case, the temperature in the transverse stretching zone is not stable, and not only does the film thickness precision deteriorate, but physical properties such as heat seal strength and shrinkage rate also vary. Therefore, it is preferable to pass the film after the transverse stretching through the intermediate zone for a predetermined time and then perform the final heat treatment. In this intermediate zone, it is important to block the accompanying flow caused by the running of the film and the hot air from the transverse stretching zone and the final heat treatment zone so that when a strip of paper is hung down without the film passing through it, the paper hangs down almost completely in the vertical direction. The passing time through the intermediate zone is sufficient for about 1 to 5 seconds. If it is shorter than 1 second, the length of the intermediate zone is insufficient and the heat blocking effect is insufficient. On the other hand, it is preferable for the intermediate zone to be long, but if it is too long the equipment will become large, so about 5 seconds is sufficient.

[0046] 4.1.4. Final heat treatment After passing through the intermediate zone, it is preferable to perform heat treatment at a temperature of more than 180°C and not more than 250°C in the final heat treatment zone. If the heat treatment temperature is 180°C or less, the 98°C hot water shrinkage rate of the laminate will be more than 5%, which is not preferable. The higher the heat treatment temperature, the lower the shrinkage rate of the film, but if the heat treatment temperature is higher than 250°C, problems such as the haze of the film becoming more than 15%, the molecular orientation angle of the film becoming more than 30°C, and the film melting during the final heat treatment step and dropping into the tenter are likely to occur, which is not preferable. During the final heat treatment, the shrinkage rate in the width direction can be reduced by shortening the clip distance in the width direction of the tenter by any ratio (relaxation in the width direction). Therefore, in the final heat treatment, it is preferable to perform relaxation in the width direction in the range of 0% to 10% (a relaxation rate of 0% means that no relaxation is performed). Although the higher the relaxation rate in the width direction, the lower the shrinkage rate in the width direction, the upper limit of the relaxation rate (shrinkage rate in the width direction of the film immediately after transverse stretching) is determined by the raw material used, the stretching conditions in the width direction, and the heat treatment temperature, so relaxation cannot be performed beyond this limit. In the polyester sealant of the present invention, the relaxation rate in the width direction is an upper limit of 10%. Furthermore, during the final heat treatment, not only can the shrinkage rate in the longitudinal direction be reduced by shortening the distance between the clips in the longitudinal direction of the tenter by any factor (relaxation in the longitudinal direction), but also the molecular orientation angle can be reduced. Therefore, relaxation in the longitudinal direction during the final heat treatment is a preferred embodiment. Although the higher the relaxation rate in the longitudinal direction, the lower the shrinkage rate in the longitudinal direction and the lower the molecular orientation angle, the upper limit of the relaxation rate (shrinkage rate in the longitudinal direction of the film immediately after transverse stretching) is determined by the raw material used, the stretching and relaxation conditions in the longitudinal direction, and the heat treatment temperature, so that relaxation cannot be performed beyond this limit. In the polyester sealant of the present invention, the relaxation rate in the longitudinal direction is an upper limit of 10%.

[0047] In addition, the time for passing through the final heat treatment zone is preferably 2 to 20 seconds. If the time for passing through is less than 2 seconds, the film passes through the heat treatment zone before the surface temperature of the film reaches the set temperature, making the heat treatment meaningless. The longer the time for passing through, the more effective the heat treatment becomes, so a time of 2 seconds or more is preferable, and a time of 5 seconds or more is even more preferable. However, if the time for passing through is increased, the equipment will become larger, so for practical purposes, a time of 20 seconds or less is sufficient.

[0048] 4.1.5. Cooling After passing through the final heat treatment, the film is preferably cooled in the cooling zone with cooling air at 10°C to 30°C. At this time, it is preferable to improve the cooling efficiency by lowering the temperature of the cooling air or increasing the wind speed so that the actual temperature of the film at the tenter outlet is lower than the glass transition temperature of either the heat seal layer or the heat resistant layer, whichever is lower. The actual temperature refers to the film surface temperature measured with a non-contact radiation thermometer. If the actual temperature of the film at the tenter outlet exceeds the glass transition temperature, the film will thermally shrink when both ends of the film held by the clips are released. At this time, the film will curl toward the heat seal layer, which has a large thermal shrinkage rate, which is not preferable. The time for passing through the cooling zone is preferably 2 to 20 seconds. If the time for passing through is 2 seconds or less, the film passes through the cooling zone before the surface temperature of the film reaches the glass transition temperature, resulting in a small radius of curvature. The longer the time for passing through, the greater the cooling effect, so the time for passing through is preferably 2 seconds or more, and more preferably 5 seconds or more. However, if the time for passing through is increased, the equipment will become larger, so for practical purposes, a time for passing through through the zone of 20 seconds or less is sufficient. Then, both ends of the film are cut and removed while being wound up to obtain a film roll.

[0049] 4.2.Layering method of inorganic thin film layers The lamination method of the inorganic thin film layer in the laminate of the present invention is not particularly limited, and known manufacturing methods can be adopted as long as the object of the present invention is not impaired. For example, a method of depositing a metal material by a PVD method (physical vapor deposition method) such as a vacuum deposition method, a sputtering method, or an ion plating method, or a CVD method (chemical vapor deposition method) can be mentioned. Furthermore, a method of laminating a metal foil such as an aluminum foil onto a film may be adopted. Among these, the vacuum deposition method is particularly preferred from the viewpoint of production speed and stability. As a heating method in the vacuum deposition method, resistance heating, high-frequency induction heating, electron beam heating, etc. can be used. In addition, oxygen, nitrogen, water vapor, etc. may be introduced as a reactive gas, or reactive deposition using means such as ozone addition or ion assist may be used. In addition, the conditions may be changed as long as the object of the present invention is not impaired, such as applying a bias to the substrate, raising or cooling the substrate temperature, etc.

[0050] 4.3. Method for forming overcoat layer The method for laminating the overcoat in the laminate of the present invention is not particularly limited, and any conventionally known coating method can be used, such as gravure coating, reverse coating, dipping, low coating, air knife coating, comma coating, screen printing, spray coating, gravure offset, die coating, or bar coating, and can be appropriately selected depending on the desired purpose. The drying method may be one or a combination of two or more heat application methods such as hot air drying, hot roll drying, high frequency irradiation, infrared irradiation, and UV irradiation. In the drying method, the heating temperature is preferably in the range of about 60°C to 200°C, more preferably in the range of about 80°C to 180°C. When the drying temperature is 60°C or higher, the desired barrier properties are satisfactorily expressed. When the drying temperature is 180°C or lower, it is preferable because the substrate does not deform or the vapor deposition film does not crack if the vapor deposition is performed for a short period of time.

[0051] 5. Packaging structure and bag making method The laminate having the above-mentioned characteristics can be suitably used as a package. The laminate of the present invention can be made into a bag by itself, but other materials may be laminated. Examples of other layers constituting the laminate include, but are not limited to, a non-stretched film containing polyethylene terephthalate as a constituent component, a non-stretched, uniaxially or biaxially stretched film containing other amorphous polyester as a constituent component, a non-stretched, uniaxially or biaxially stretched film containing nylon as a constituent component, and a non-stretched, uniaxially or biaxially stretched film containing polypropylene as a constituent component. The method of using the laminate in the package is not particularly limited, and a conventionally known manufacturing method such as a coating forming method, a lamination method, or a heat sealing method can be adopted. The package may be at least partially composed of the laminate according to the present invention, but a configuration in which the above-mentioned laminate is present in the entire package is preferred because the gas barrier properties of the package are improved. In addition, the package may have the laminate of the present invention in any layer, but considering the non-adsorption properties of the contents and the seal strength when making a bag, it is preferred that the heat seal layer of the laminate of the present invention be the innermost layer of the bag. The method for producing a package having the laminate of the present invention is not particularly limited, and any conventional manufacturing method such as heat sealing using a heat bar (heat jaw), adhesion using a hot melt, or center sealing using a solvent can be used. A package having the laminate of the present invention can be suitably used as a packaging material for various items such as food, medicines, and industrial products. EXAMPLES

[0052] The present invention will now be described in detail using examples and comparative examples. However, the present invention is not limited to the embodiments of the examples, and can be modified as appropriate without departing from the spirit of the present invention. The laminate is evaluated as follows. If the longitudinal and transverse directions cannot be immediately determined because the area of ​​the laminate is small, etc., the longitudinal and transverse directions can be provisionally determined and then measured. There is no particular problem even if the provisionally determined longitudinal and transverse directions are 90 degrees different from the true directions.

[0053] <Laminate evaluation method> [Thickness of inorganic thin film layer] A sample cut to 1 mm x 10 mm was embedded in epoxy resin for electron microscopes, then fixed to the specimen holder of an ultramicrotome, and a thin cross-sectional section parallel to the short side of the embedded sample was prepared. Next, a transmission electron microscope (JEM2010, manufactured by JEOL Ltd.) was used to observe the thin section at a site that was not significantly damaged. The accelerating voltage was 200 kV, 2000 After observation at 0x, the film thickness of each layer was measured at 100 points, and the average was taken as the film thickness. [Heat seal strength] The heat seal strength was measured in accordance with JIS Z1707. The specific procedure is as follows. The heat-sealed surfaces of the samples were bonded together using a heat sealer. The heat-sealing conditions were upper bar temperature 140°C, lower bar temperature 30°C, pressure 0.2MPa, and time 2 seconds. The bonded samples were cut out to have a seal width of 15mm. The peel strength was measured using a universal tensile tester "DSS-100" (Shimadzu Corporation) at a tensile speed of 200mm / min. The peel strength is expressed as the strength per 15mm (N / 15mm).

[0054] [Water vapor permeability] The water vapor permeability was measured according to JIS K7126 B method. Using a water vapor permeability measuring device (PERMATRAN-W3 / 33MG manufactured by MOCON), the water vapor permeability was measured in a direction in which the moisture-conditioning gas permeated from the heat seal layer side of the laminate to the inorganic thin film layer side under an atmosphere of temperature 40°C and humidity 90% RH. Before the measurement, the sample was left to stand for 4 hours in a humidity 65% ​​RH environment to condition the moisture.

[0055] [Oxygen permeability] The oxygen permeability was measured according to JIS K7126-2. Using an oxygen permeability measuring device (OX-TRAN 2 / 20 manufactured by MOCOM), the oxygen permeability was measured in the direction in which oxygen permeates from the heat seal layer side of the laminate to the inorganic thin film layer side under an atmosphere of 23 degrees Celsius and 65% RH. Before the measurement, the sample was left in an environment of 65% RH for 4 hours to condition the humidity.

[0056] [Optical density (OD value)] The optical density (OD value) under white light was measured using a black and white transmission densitometer (Ihac-T5, manufactured by Ihara Electronics). The measurement was carried out in a dark room where external light was blocked. For five 50 mm square samples cut from five random points on the measurement sample, the ratio of the incident light incident on the sample to the transmitted light after transmission was expressed in common logarithm, and the OD value was calculated according to the following formula 1. The measurement was carried out five times, and the average value was calculated to be the OD value. OD value = log(incident light / transmitted light) = log(1 / transmittance) Equation 1

[0057] [Molecular orientation angle] The molecular orientation angle of the laminate in the width direction was measured using a molecular orientation angle measuring device (MOA-6004 manufactured by Oji Measurement Co., Ltd.). Samples were cut into 10 cm x 10 cm squares from both ends (L end, R end) of the laminate (width 1000 mm). The molecular orientation angles of the L end and R end were each measured twice in the longitudinal direction, and the larger measurement result was used as the molecular orientation angle of the laminate.

[0058] [Hot water heat shrinkage rate] The sample was cut into a 10cm x 10cm square and immersed in warm water at 98±0.5°C for 3 minutes without load to allow it to shrink, then immersed in water at 25°C±0.5°C for 10 seconds and removed from the water. The longitudinal and lateral dimensions of the sample were then measured, and the thermal shrinkage rate in each direction was calculated according to the following formula 2. The measurement was performed twice, and the average value was calculated. Shrinkage rate = {(length before shrinkage - length after shrinkage) / length before shrinkage} x 100 (%) Formula 2 The thermal shrinkage rates in the longitudinal and transverse directions were evaluated according to the following criteria. Judgment: Good Heat shrinkage rate: 5% or less Evaluation: × Heat shrinkage rate 5% or more

[0059] [Folding holding angle] The sample was left in a constant temperature room at 28°C and 50% RH for 24 hours. Immediately afterwards, the sample was cut into a 10cm x 10cm square at 20°C and 65% RH and folded in four (5cm x 5cm square). When folding the sample, the short side of the rectangle formed by the first 2 folds was in the longitudinal direction, and the heat seal layer was made to form a mountain fold. The sample folded in four was then sandwiched between two pieces of glass measuring 10cm x 15cm and 2mm thick, and a 5kg weight was placed on the glass and pressed for 10 seconds. After removing the weight from the sample folded in four, the angle at which the sample was opened was measured using the last fold as the base point, as shown in Figure 1. The angle when the sample was completely folded was 0 degrees, and when it was completely opened, it was 180 degrees.

[0060] [Heat resistance evaluation] The heat seal layer (surface) of the sample was placed facing an unstretched polyethylene terephthalate sheet (200 μm, no surface treatment such as coating or corona treatment) and heat sealed with the bar of a heat sealer. The heat sealing conditions were upper bar temperature 230°C, lower bar temperature 30°C, pressure 0.6 MPa, and time 1 second. The heat resistance was evaluated visually from the seal line of the bonded sample. Heat resistance was evaluated based on the presence or absence of holes in the sample. The evaluation criteria are as follows: Judgment: No holes Verdict: × Holes present

[0061] [Adsorption] The film was cut into a 10cm x 10cm square, two pieces were stacked with the heat-sealed side facing inward, and a bag was made by heat-sealing a position 1 cm from the edge of the film. An aluminum cup containing 0.5 ml of contents was placed in the bag, and the bag was closed and hermetically sealed by heat-sealing a position 1 cm from the edge of the film. The contents used were D-limonene (manufactured by Tokyo Chemical Industry Co., Ltd.) and L-menthol (manufactured by Nacalai Tesque, Inc.). The bag was kept in a 30°C environment for 20 hours. After that, a 5cm x 5cm square was cut from the surface of the film bag that contacted the mouth of the aluminum cup, and the cut film was immersed in 4ml of extraction solvent and extracted with ultrasound for 30 minutes. 99.8% ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the extraction solvent. The concentration of the contents in the extraction solution was quantified using a Shimadzu gas chromatograph "GC-14B." The gas chromatograph used a "GC-14A Glass ID2.6φx1.1m PET-HT 5% Uniport HP 80 / 100 (manufactured by GL Sciences Inc.)" column, an FID detector, and N2 carrier gas, and quantification was performed using the area percentage method with a carrier gas flow rate of 35ml / min and an injection volume of 1μl. The amount of adsorption was 1cm2 of the heat seal surface. 2 Adsorption amount per unit (μg / cm 2 ) and the low adsorption was judged as follows: Judgment ○ 0μg / cm 2 More than 2μg / cm 2 less than Judgment × 2μg / cm 2 End

[0062] <Preparation of polyester raw materials> [Synthesis Example 1] In a stainless steel autoclave equipped with a stirrer, a thermometer, and a partial reflux condenser, 100 mol % of dimethyl terephthalate (DMT) as a dicarboxylic acid component and 100 mol % of ethylene glycol (EG) as a polyhydric alcohol component were charged so that the molar ratio of ethylene glycol was 2.2 times that of dimethyl terephthalate, and 0.05 mol % (relative to the acid component) of zinc acetate was used as an ester exchange catalyst to carry out an ester exchange reaction while distilling off the produced methanol outside the system. Then, 0.225 mol % (relative to the acid component) of antimony trioxide was added as a polycondensation catalyst, and a polycondensation reaction was carried out at 280°C under reduced pressure of 26.7 Pa to obtain polyester (A) with an intrinsic viscosity of 0.75 dl / g. This polyester (A) is polyethylene terephthalate. The composition of polyester (A) is shown in Table 1.

[0063] [Synthesis Example 2] Polyesters (B) to (G) were obtained by changing the monomers in the same manner as in Synthesis Example 1. The composition of each polyester is shown in Table 1. In Table 1, TPA is terephthalic acid, IPA is isophthalic acid, BD is 1,4-butanediol, NPG is neopentyl glycol, CHDM is 1,4-cyclohexanedimethanol, and DEG is diethylene glycol. When producing polyester (G), SiO2 (Silysia 266 manufactured by Fuji Silysia) was added as a lubricant at a ratio of 7,000 ppm to the polyester. Each polyester was appropriately formed into chips. The composition of polyesters (B) to (G) is shown in Table 1. The intrinsic viscosity of each polyester was (B) 0.73 dl / g, (C) 0.72 dl / g, (D) 0.73 dl / g, (E) 0.8 dl / g, (F) 0.7 dl / g, and (G) 0.75 dl / g.

[0064] [Table 1]

[0065] [Film 1] The raw materials for the heat seal layer were polyester B, polyester E and polyester G mixed in a mass ratio of 67:24:8, and the raw materials for the heat resistant layer were polyester A, polyester B, polyester E and polyester G mixed in a mass ratio of 48:38:6:8. The mixed raw materials for the heat seal layer and the heat resistant layer were fed into separate twin screw extruders, and both were melted at 270°C. The molten resins were joined by a feed block midway through the flow path, extruded from a T-die, and cooled on a chill roll set at a surface temperature of 30°C to obtain an unstretched laminated film. The flow path of the molten resin was set so that one side of the laminated film was the heat seal layer and the other side was the heat resistant layer (a two-layer structure of heat seal layer / heat resistant layer), and the extrusion rate was adjusted so that the thickness ratio of the heat seal layer and the heat resistant layer was 50 / 50. The unstretched laminated film obtained by cooling and solidifying was introduced into a longitudinal stretching machine with multiple rolls arranged in series, preheated on the preheating roll until the film temperature reached 78°C, and then stretched 4.1 times. The film immediately after longitudinal stretching was passed through a heating furnace set at 100°C with a hot air heater, and a 20% relaxation treatment was performed in the longitudinal direction using the speed difference between the rolls at the entrance and exit of the heating furnace. The longitudinally stretched film was then forcibly cooled by a cooling roll set at a surface temperature of 25°C.

[0066] The film after the relaxation treatment was introduced into a transverse stretching machine (tenter) and preheated for 5 seconds until the surface temperature reached 105°C, after which it was stretched 4.0 times in the width direction (transverse direction). The film after the transverse stretching was introduced directly into the intermediate zone and passed through in 1.0 second. In the intermediate zone of the tenter, the hot air from the final heat treatment zone and the hot air from the transverse stretching zone were blocked so that when a rectangular piece of paper was hung down without the film passing through, the piece of paper would hang down almost completely in the vertical direction. After that, the film that passed through the intermediate zone was guided to the final heat treatment zone and heat-treated at 190°C for 5 seconds. At this time, the clip interval in the film width direction was narrowed at the same time as the heat treatment, so that a 3% relaxation treatment was performed in the width direction. After passing through the final heat treatment zone, the film was cooled with 30°C cooling air for 5 seconds. At this time, the actual film temperature at the tenter outlet was 45°C. By cutting and removing both edges and winding it into a roll with a width of 5000 mm, a biaxially stretched film with a thickness of 30 μm was continuously produced over a predetermined length. From this 5000 mm wide film roll (mill roll), five film rolls were obtained by slitting to a width of 1000 mm. Of the five slit film rolls, the roll corresponding to the right end (R end) in the flow direction when manufacturing the mill roll was used as a film sample. The properties of the obtained film were evaluated by the above method. The production conditions are shown in Table 2.

[0067] [Film 2] The raw materials for the heat seal layer were polyester B, polyester C, and polyester G mixed in a mass ratio of 40:42:8, and the raw materials for the heat resistant layer were polyester A, polyester C, polyester D, and polyester G mixed in a mass ratio of 64:8:22:6. The mixed raw materials for the heat seal layer and the heat resistant layer were fed into separate twin screw extruders, melted and laminated in the same manner as in Film 1 above, extruded, and cooled to solidify, to obtain an unstretched laminated film. This unstretched laminated film was introduced into a simultaneous biaxial stretching machine and preheated for 5 seconds until the surface temperature reached 100°C, after which it was simultaneously biaxially stretched to 3.5 times its length (machine direction) and 4.0 times its width (transverse direction). After simultaneous biaxial stretching, the film was introduced directly into the intermediate zone and passed through in 1.0 second. In the intermediate zone, the hot air from the final heat treatment zone and the hot air from the transverse stretching zone were blocked so that when a strip of paper was hung down without the film passing through, the paper would hang down almost completely in the vertical direction. The film then passed through the intermediate zone and was guided to the final heat treatment zone, where it was heat-treated at 200°C for 10 seconds. At this time, the clip intervals in the longitudinal direction and the width direction of the film were narrowed simultaneously while the heat treatment was being performed, so that a relaxation treatment was performed by 15% in the longitudinal direction and 3% in the width direction. After passing through the final heat treatment zone, the film was cooled for 5 seconds with cooling air at 30°C. At this time, the actual film temperature at the tenter outlet was 45°C. Both edges were cut and removed, and the film was wound into a roll with a width of 5000 mm, thereby continuously producing a biaxially stretched film with a thickness of 30 μm over a predetermined length. The obtained film was slit to a width of 1000 mm in the same manner as film 1. The properties of this film were evaluated by the above-mentioned method. The production conditions are shown in Table 2.

[0068] [Films 3-6] Films 3 to 6 were also produced in the same manner as Film 1 and Film 2, but with various changes to the raw material blend ratio, layer structure, longitudinal stretching, relaxation in the longitudinal direction, transverse stretching, final heat treatment, and cooling conditions. The production conditions for each film are shown in Table 2. Film 3 is a laminate film similar to Film 1, and is produced using the sequential biaxial stretching method; Films 4 and 5 are single-layer films with a heat seal layer or heat-resistant layer, and are produced using the simultaneous biaxial stretching method; and Film 6 is a two-kind, three-layer film with heat seal layers on both sides of the heat-resistant layer, and is produced using the sequential biaxial stretching method. [Film 7] Film 7 was Rixfilm (registered trademark) L4102-25 μm manufactured by Toyobo Co., Ltd. The results are shown in Table 2 together with Films 1 to 6.

[0069] [Table 2]

[0070] [Example 1] A laminate was produced by forming an aluminum (AL) thin film on the heat-resistant layer side of Film 1 by vacuum deposition using aluminum as a deposition source. The properties of the obtained laminate were evaluated by the above-mentioned methods. The layer structure and the evaluation results are shown in Table 3.

[0071] [Examples 2 to 4, Comparative Examples 1 to 5] A laminate was produced in the same manner as in Example 1, except that the film was changed. The properties of the obtained laminate were evaluated by the above-mentioned methods. The layer structure and the evaluation results are shown in Table 3.

[0072] [Table 3]

[0073] [Film evaluation results] As shown in Table 3, all of the laminates of Examples 1 to 4 were excellent in heat seal strength, water vapor permeability, oxygen permeability, optical density, heat shrinkage rate, folding angle, heat resistance, and non-adsorption, and good evaluation results were obtained. On the other hand, the laminate of Comparative Example 1 had excellent heat seal strength, heat shrinkage rate, folding angle, heat resistance, and adsorption, but since it did not have a metal thin film layer, the water vapor permeability and oxygen permeability were higher than the specified range, and the optical density was low. The sealant of Comparative Example 2 was excellent in heat seal strength, water vapor permeability, oxygen permeability, optical density, folding angle, and non-adsorption. However, because Film 4, which has a final heat treatment temperature of 100°C, was used alone, the thermal shrinkage rate was large and the heat resistance was evaluated as ×. The sealant of Comparative Example 3 was excellent in heat shrinkage, heat resistance, and non-adsorption, but was inferior in heat seal strength, water vapor permeability, oxygen permeability, optical density, and folding angle. The sealant of Comparative Example 4 was excellent in heat seal strength, water vapor permeability, oxygen permeability, optical density, folding angle, and non-adsorption, but because Film 6, which has a final heat treatment temperature of 115°C, was used alone, the thermal shrinkage rate was large and the heat resistance evaluation was poor. The sealant of Comparative Example 5 was excellent in heat seal strength, water vapor permeability, oxygen permeability, optical density, thermal shrinkage rate, and heat resistance, but the folding angle exceeded 70 degrees and an olefin-based material was used in the heat seal layer, resulting in poor non-adsorption properties. [Industrial Applicability]

[0074] The present invention relates to a laminate that exhibits low adsorption of ingredients of contents, has excellent heat seal strength, gas barrier properties, and concealment properties at low temperatures, and is suitable for use as a packaging material because it is free from holes caused by heat sealing and has excellent foldability. In addition, the laminate of the present invention can be used as at least one layer to form a laminate with other films, and a package can be provided from the laminate.

Claims

1. A laminate having at least a heat seal layer made of a stretched film, a heat resistant layer, and an inorganic thin film layer, the inorganic thin film layer being directly laminated on an untreated surface of the heat resistant layer, and the laminate is characterized by satisfying the following requirements (1) to (6): (1) At least one of the laminates has a heat seal layer on the outermost surface thereof, the heat seal layer is made of a polyester resin mainly composed of ethylene terephthalate, and the content of dicarboxylic acid monomers and / or diol monomers other than terephthalic acid and ethylene glycol constituting ethylene terephthalate is 25 mol % or more, and the heat seal layers have a seal strength of 8 N / 15 mm or more and 30 N / 15 mm or less when sealed together at 140° C., 0.2 MPa, and 2 seconds. (2) The water vapor permeability in an environment of 40° C. and 90% RH is 0.1 [g / (m 2 ・d)] or more 2[g / (m 2 ・d)] Below (3) The oxygen permeability is 0.3 [cc / (m 2 ・d・atm)] or more 3 [cc / (m 2 ・d・atm)] and below (4) Optical density (OD value) is 1 or more and 5 or less (5) After immersing in 98°C hot water for 3 minutes, the thermal shrinkage rate is between -5% and 5% in both the longitudinal and transverse directions. (6) The heat-resistant layer is made of a polyester resin mainly composed of ethylene terephthalate, and the content of dicarboxylic acid monomers and / or diol monomers other than terephthalic acid and ethylene glycol constituting ethylene terephthalate is 20 mol % or less.

2. 2. The laminate according to claim 1, wherein the maximum value of the molecular orientation angle measured in the width direction is 0 degrees or more and 35 degrees or less.

3. 3. The laminate according to claim 1, wherein the main component of the inorganic material constituting the inorganic thin film layer is aluminum.

4. The laminate according to any one of claims 1 to 3, further comprising a heat-resistant layer in addition to the heat seal layer and the inorganic thin film layer, the heat-resistant layer being made of a polyester-based resin having ethylene terephthalate as a main component.

5. 5. The laminate according to claim 1, wherein the folded angle is 20 degrees or more and 70 degrees or less.

6. The laminate according to any one of claims 1 to 5, characterized in that the polyester-based resin constituting the heat seal layer contains a diol component other than ethylene glycol and / or an acid component other than terephthalic acid as a monomer component, the diol component being at least one selected from the group consisting of neopentyl glycol, 1,4-cyclohexanedimethanol, 1,4-butanediol, and diethylene glycol, and the acid component being isophthalic acid.

7. A packaging material comprising at least one layer of the laminate according to any one of claims 1 to 6.

8. 8. The laminate according to claim 1, further comprising an overcoat layer laminated on the inorganic thin film layer.

9. A packaging material comprising at least one layer of the laminate according to claim 8.

Citation Information

Patent Citations

  • Packing bag with fastener for object including volatile constituent

    JP1995132946A

  • Lid material

    JP2006027695A

  • Method for producing metal deposition film

    JP2012097331A

  • Polyester film for sealant, laminate and package

    JP2017165059A

  • Laminate film, laminate and package

    JP2017165060A