Multilayer film, packaging material and packaging body
A multilayer film with specific polymer compositions addresses the challenges of heat resistance, transparency, and cold impact resistance in retort processing, ensuring film integrity and visibility during high-temperature sterilization.
Patent Information
- Application Number
- JP2021000801
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-06
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-01-06
AI Technical Summary
Conventional polypropylene multilayer films face challenges in maintaining excellent heat resistance, transparency, and cold impact resistance, particularly during retort processing which involves high-temperature sterilization.
A multilayer film structure is developed with specific compositions for the outer and inner layers, including propylene homopolymer, propylene-ethylene random copolymer, and a nucleating agent in the outer layers, and a propylene-ethylene block copolymer and ethylene-propylene copolymer elastomer in the inner layer, to enhance heat resistance, transparency, and cold impact resistance.
The film achieves high heat resistance, transparency, and cold impact resistance, suitable for retort processing, by suppressing film deformation and maintaining flexibility and sealability.
Smart Images

Figure 0007581884000002 
Figure 0007581884000003 
Figure 0007581884000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer film, a packaging material, and a package. More specifically, the present invention relates to a polypropylene-based multilayer film that has excellent heat resistance and transparency and can be suitably used as a sealant film for packaging materials even in severe treatments such as boiling water treatment and retort treatment, and to a packaging material and a package obtained by using the polypropylene-based multilayer film. [Background technology]
[0002] Polypropylene-based films are sometimes used as sealant films in various packaging materials such as food packaging because they have excellent rigidity and heat resistance and are inexpensive.
[0003] Patent Document 1 proposes a polypropylene-based composite film consisting of three layers, characterized in that the middle layer is made of a propylene-ethylene block copolymer and both surface layers are made of a propylene-based random copolymer.
[0004] Patent Document 2 proposes a multilayer film comprising surface layers each containing an ethylene-α-olefin copolymer and a propylene-based polymer, and an intermediate layer containing a propylene polymer and an ethylene-propylene copolymer.
[0005] Patent Document 3 proposes a multilayer film comprising two surface layers made of polypropylene or an ethylene-propylene random copolymer, and an inner layer made of an ethylene-propylene block copolymer or a blend of an ethylene-propylene block copolymer and a polyolefin polymer having good compatibility with the rubber component in the block copolymer. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-132186 A [Patent Document 2] JP 2017-105174 A [Patent Document 3] Japanese Patent Application Publication No. 62-3950 Summary of the Invention [Problem to be solved by the invention]
[0007] Polypropylene-based multilayer films are now required to have heat resistance that can withstand retort treatment, which involves performing sterilization and pasteurization at high temperatures of, for example, 120 to 135° C., and transparency that can maintain the visibility of the contents. However, with conventional polypropylene-based films, it is currently difficult to maintain excellent heat resistance, transparency, and cold impact resistance at the same time.
[0008] The present invention has been made in view of the above circumstances, and aims to provide a polypropylene-based multilayer film having excellent heat resistance, transparency, and cold impact resistance. It is also an object of the present invention to provide a packaging material and a package obtained by using the multilayer film. [Means for solving the problem]
[0009] As a result of intensive research aimed at solving the above problems, the inventors discovered that it is important to mix different propylene-based polymers into the outer layer of a polypropylene-based multilayer film, and then to add a specified amount of a nucleating agent to adjust the crystallinity, which led to the completion of the present invention.
[0010] A multilayer film according to one aspect of the present invention is a multilayer film comprising, in this order, a first outer layer which is a heat seal layer containing a propylene homopolymer (A), a propylene-ethylene random copolymer (B) and a nucleating agent, an inner layer containing a propylene-ethylene block copolymer (C) and an ethylene-propylene copolymer elastomer (D), and a second outer layer containing the propylene homopolymer (A) and the propylene-ethylene random copolymer (B), wherein the content of the nucleating agent is 1 to 5 parts by mass per 100 parts by mass of the total amount of the propylene homopolymer (A) and the propylene-ethylene random copolymer (B).
[0011] In the above multilayer film, the outer layer contains a propylene homopolymer (A), a propylene-ethylene random copolymer (B), and a predetermined amount of a nucleating agent. This makes it possible to suppress surface irregularities, which are a factor in reducing the transparency of the film, maintain the flexibility of the film, and ensure excellent cold impact resistance, while maintaining heat resistance (high level of heat resistance that makes it difficult for the film to deform or fuse on the inner surface when used as a package). Such effects cannot be obtained when a propylene-based random copolymer is simply used in the outer layer (e.g., Patent Document 1 above), when an ethylene-α-olefin copolymer and a propylene-based polymer are used (e.g., Patent Document 2 above), or when either polypropylene or an ethylene-propylene random copolymer is used (e.g., Patent Document 3 above), and are particularly suitable for retort treatment (including high retort treatment) applications.
[0012] In one embodiment, the first outer layer and the second outer layer may contain 70 to 30 parts by mass of the propylene homopolymer (A) and 30 to 70 parts by mass of the propylene-ethylene random copolymer (B), which makes it easier to achieve both heat resistance and transparency.
[0013] In one embodiment, the propylene homopolymer (A) may satisfy the following requirement (a1), and the propylene-ethylene random copolymer (B) may satisfy the following requirement (b1), which makes it easier to achieve both heat resistance and transparency. Requirement (a1): When measured by differential scanning calorimetry (JIS K 7121), the melting onset temperature is 150°C or higher and the melting peak temperature is 155°C or higher. Requirement (b1): The ethylene content is 5% by mass or less.
[0014] In one embodiment, the inner layer may contain 90 to 50% by mass of the propylene-ethylene block copolymer (C) and 10 to 50% by mass of the ethylene-propylene copolymer elastomer (D), which maintains the flexibility of the film and makes it easier to obtain excellent cold impact resistance.
[0015] A packaging material according to one aspect of the present invention includes the multilayer film described above and a substrate.
[0016] A package according to one aspect of the present invention is produced from the above-described packaging material. Effect of the Invention
[0017] According to the present invention, a polypropylene-based multilayer film having excellent heat resistance, transparency, and cold impact resistance can be provided. The present invention also provides a packaging material and a package obtained by using the multilayer film. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a cross-sectional view of a multilayer film according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of a packaging material according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] <Polypropylene-based multi-layer film> Fig. 1 is a cross-sectional view of a multilayer film according to one embodiment of the present invention. The multilayer film 10 includes a first outer layer 1a, an inner layer 2, and a second outer layer 1b in this order. The multilayer film can be used as a polypropylene-based non-stretch sealant film.
[0020] [First outer layer and second outer layer] The first outer layer contains a propylene homopolymer (A), a propylene-ethylene random copolymer (B), and a nucleating agent. The first outer layer can be said to be a layer formed from a resin composition containing a propylene homopolymer (A), a propylene-ethylene random copolymer (B), and a nucleating agent. When used as a packaging material, the first outer layer plays a role as a heat seal layer (has heat sealability) and is disposed so as to contact the contents. For this reason, the first outer layer has a heat resistance to such an extent that the first outer layers do not fuse together during retort treatment.
[0021] The second outer layer contains a propylene homopolymer (A) and a propylene-ethylene random copolymer (B). The second outer layer can be said to be a layer formed from a resin composition containing the propylene homopolymer (A) and the propylene-ethylene random copolymer (B).
[0022] When the first outer layer and the second outer layer have the above-mentioned configuration, it is possible to impart heat resistance and transparency to the multilayer film. The first outer layer and the second outer layer may be collectively referred to simply as the outer layer.
[0023] (Propylene homopolymer (A)) The propylene homopolymer (A) is not particularly limited in its production method, but can be obtained by, for example, a method of homopolymerizing propylene using a Ziegler-Natta type catalyst, a metallocene catalyst, or a half metallocene catalyst. By including the propylene homopolymer (A) in the outer layer, excellent heat resistance can be imparted to the outer layer.
[0024] The propylene homopolymer (A) may have a melting onset temperature of 150° C. or higher and a melting peak temperature of 155° C. or higher as measured by differential scanning calorimetry (JIS K 7121). A polymer having both a melting onset temperature and a melting peak temperature within this range has excellent heat resistance, and is unlikely to fuse on the inner surface of a package after, for example, a retort treatment at a high temperature.
[0025] As the propylene homopolymer (A), those having a melt flow rate (MFR: ISO 1133) (temperature 230°C, load 2.16 kg) in the range of 2.0 to 7.0 g / 10 min can be used. The melt flow rate is a parameter indicating the fluidity of a polymeric material when melted, and is also a parameter indicating the molecular weight. Therefore, if the melt flow rate is too high, the impact resistance of the polymeric material is likely to decrease, and if it is too low, the load on the extruder during molding processing increases, the processing speed decreases, and the productivity is likely to decrease. From these viewpoints, the melt flow rate can be 2.0 to 7.0 g / 10 min, and may be 2.0 to 5.0 g / 10 min.
[0026] (Propylene-ethylene random copolymer (B)) The method for producing the propylene-ethylene random copolymer (B) is not particularly limited, but it can be obtained, for example, by copolymerizing ethylene as a comonomer into the main monomer consisting of propylene using a Ziegler-Natta type catalyst, a metallocene catalyst, or a half metallocene catalyst. By containing the propylene-ethylene random copolymer (B) in the outer layer, a multilayer film with excellent transparency can be obtained.
[0027] The propylene-ethylene random copolymer (B) may have a melting onset temperature of 140°C or higher and a melting peak temperature of 145°C or higher when measured by differential scanning calorimetry (JIS K 7121). A copolymer having both a melting onset temperature and a melting peak temperature within this range has excellent heat resistance, and is unlikely to fuse on the inner surface of a package after, for example, a severe retort treatment at 135°C for 40 minutes.
[0028] The propylene-ethylene random copolymer (B) may have a ratio ΔHh / ΔHl of the heat of fusion ΔHh on the higher side than 135°C to the heat of fusion ΔHl on the lower side in differential scanning calorimetry (JIS K 7121) of 1.5 to 2.5. By keeping the ratio below the upper limit, the flexibility of the film is maintained, edge tearing of the heat-sealed portion after retort treatment can be suppressed, and the heat-seal strength is less likely to decrease. The lower limit of the ratio may be 1.5, from the viewpoint of preventing fusion on the inner surface of the package after retort treatment.
[0029] The ethylene content of the propylene-ethylene random copolymer (B) can be 5% by mass or less. By having the ethylene content be equal to or less than the upper limit, the heat resistance is not excessively decreased while maintaining the transparency, and it becomes easier to suppress fusion on the inner surface of the package after retort treatment. From this viewpoint, the ethylene content may be 4.5% by mass or less, or may be 4% by mass or less. The lower limit of the ethylene content is not particularly limited, but from the viewpoints of maintaining the flexibility of the film, suppressing edge tearing at the heat-sealed portion after retort treatment, and making it difficult for the heat-seal strength to decrease, it can be 2% by mass.
[0030] The ethylene content of the propylene-ethylene random copolymer (B) can be measured according to the quantitative method for ethylene content (IR method) described on pages 412-413 of the Polymer Analysis Handbook (May 10, 2013, 3rd printing) edited by the Polymer Analysis Roundtable of the Japan Analytical Society.
[0031] The outer layer may contain 70 to 30 parts by mass of the propylene homopolymer (A) and 30 to 70 parts by mass of the propylene-ethylene random copolymer (B). When the content of the propylene homopolymer (A) is 30 parts by mass or more, excellent heat resistance is easily maintained. Furthermore, when the content of the propylene homopolymer (A) is 70 parts by mass or less, that is, when the content of the propylene-ethylene random copolymer (B) is at least 30 parts by mass or more, excellent transparency and heat sealability are easily exhibited. From these viewpoints, the outer layer may contain 60 to 40 parts by mass of the propylene homopolymer (A) and 40 to 60 parts by mass of the propylene-ethylene random copolymer (B). From a similar viewpoint, in particular the second outer layer may contain 70 to 30 mass% of the propylene homopolymer (A) and 30 to 70 mass% of the propylene-ethylene random copolymer (B), or may contain 60 to 40 mass% of the propylene homopolymer (A) and 40 to 60 mass% of the propylene-ethylene random copolymer (B).
[0032] (Nucleating agent) A nucleating agent (or nucleating agent, crystal nucleating agent) is an additive for promoting the crystallization of a polymer compound, and is an agent for adjusting the physical properties of a polymer compound by adding a small amount to the polymer compound. The nucleating agent is not particularly limited as long as it exhibits such an action, and examples of the nucleating agent include α crystal nucleating agents such as sorbitol-based compounds, organic phosphate metal salt-based compounds, organic carboxylate metal salt-based compounds, and rosin-based compounds, β crystal nucleating agents such as amide-based compounds and quinanacridone-based compounds, benzoic acid metal salts, alkyl fatty acid salts, and talc.
[0033] It is believed that by blending a nucleating agent in the first outer layer, which is the heat seal layer, the crystalline region in the first outer layer increases, improving heat resistance. This makes it possible to suppress fusion on the inner surface of the package after retort treatment. It is also believed that the nucleating agent refines the crystals in the first outer layer. This makes the size of the crystals smaller and more uniform than the wavelength of visible light, suppresses diffuse reflection of visible light, and provides excellent heat resistance while maintaining transparency.
[0034] The content of the nucleating agent may be 1 to 5 parts by mass relative to 100 parts by mass of the total amount of the propylene homopolymer (A) and the propylene-ethylene random copolymer (B). When the content is equal to or greater than the lower limit, the heat resistance is improved. On the other hand, when the content is equal to or less than the upper limit, the flexibility of the film is maintained, edge tearing of the heat-sealed portion after retort treatment can be suppressed, and excellent heat sealability can be obtained. In addition, costs can be suppressed. From this viewpoint, the content of the nucleating agent may be 1.5 to 4.5 parts by mass.
[0035] [Inner layer] The inner layer contains a propylene-ethylene block copolymer (C) and an ethylene-propylene copolymer elastomer (D). It is desirable for the inner layer to be flexible in order to obtain the impact resistance required to prevent the bag from breaking in a low-temperature environment.
[0036] (Propylene-ethylene block copolymer (C)) Propylene-ethylene block copolymer (C) is a copolymer that can be obtained by producing a propylene polymer (C1) in the first step, and then producing an ethylene-propylene copolymer (C2) by gas phase polymerization in the second step. Propylene-ethylene block copolymer (C) is not a block copolymer in which a propylene polymer end and an ethylene-propylene copolymer end are bonded, but a type of blend copolymer. By containing propylene-ethylene block copolymer (C) in the inner layer, the flexibility of the film is maintained, making it easy to obtain excellent cold impact resistance.
[0037] The propylene-ethylene block copolymer (C) may have a melt flow rate (MFR: ISO 1133) (temperature 230°C, load 2.16 kg) in the range of 0.5 to 2.5 g / 10 min. If the melt flow rate is too high, the impact resistance of the film is likely to decrease, and if it is too low, the load on the extruder during molding increases, the processing speed decreases, and the productivity is likely to decrease. From these viewpoints, the melt flow rate may be 0.5 to 2.5 g / 10 min., or may be 1.0 to 2.0 g / 10 min.
[0038] The propylene-ethylene block copolymer (C) may contain 90 to 60% by mass of the propylene polymer (C1) and 10 to 40% by mass of the ethylene-propylene copolymer (C2). When the respective components are in these ranges, excellent cold impact resistance is easily obtained.
[0039] The ethylene content of the ethylene-propylene copolymer (C2) contained in the propylene-ethylene block copolymer (C) is not particularly limited, but may be 20 to 40 mass%. When the ethylene content is equal to or less than the upper limit, the tackiness of the product can be suppressed, and contamination due to the tackiness of the product during production is unlikely to occur, making it easier to maintain excellent productivity. When the ethylene content is equal to or more than the lower limit, the flexibility of the film is maintained, making it easier to obtain excellent cold impact resistance.
[0040] (Ethylene-propylene copolymer elastomer (D)) The ethylene-propylene copolymer elastomer (D) can be obtained by, for example, a slurry polymerization method carried out in the presence of an inert hydrocarbon such as hexane, heptane, kerosene, or a liquefied α-olefin solvent such as propylene, or a gas phase polymerization method without a solvent. Specifically, the ethylene-propylene copolymer elastomer (D) can be obtained by a known multi-stage polymerization method. That is, it is a polymerized polypropylene-based resin with high rubber content, which can be obtained by polymerizing propylene and / or propylene-α-olefin polymer in the first reaction stage and then copolymerizing propylene with α-olefin in the second reaction stage. By containing the ethylene-propylene copolymer elastomer (D) in the inner layer, it is easy to impart flexibility to the film and to obtain excellent cold impact resistance.
[0041] The ethylene-propylene copolymer elastomer (D) may have a melt flow rate (MFR: ISO 1133) (temperature 230°C, load 2.16 kg) in the range of 0.5 to 3.5 g / 10 min. When the melt flow rate is equal to or higher than the lower limit, the load on the extruder during molding is small, the processing speed is unlikely to decrease, and it is easy to maintain excellent productivity. When the melt flow rate is equal to or lower than the upper limit, the compatibility between the propylene-ethylene block copolymer (C) and the ethylene-propylene copolymer elastomer (D) is good, and transparency is unlikely to decrease.
[0042] The ethylene-propylene copolymer elastomer (D) may have a ratio of propylene content to ethylene content (propylene content / ethylene content) in the range of 1.5 to 4. When the ratio is equal to or higher than the lower limit, the flexibility of the film is maintained and excellent cold impact resistance is easily obtained. When the ratio is equal to or lower than the upper limit, the compatibility between the propylene-ethylene block copolymer (C) and the ethylene-propylene copolymer elastomer (D) is good and transparency is less likely to decrease.
[0043] The inner layer may contain 90 to 50% by mass of the propylene-ethylene block copolymer (C) and 10 to 50% by mass of the ethylene-propylene copolymer elastomer (D). When the content of the propylene-ethylene block copolymer (C) is 50% by mass or more, excellent cold impact resistance is easily maintained. Furthermore, when the content of the propylene-ethylene block copolymer (C) is 90% by mass or less, that is, when the content of the ethylene-propylene copolymer elastomer (D) is at least 10% by mass or more, even better heat sealability can be exhibited. From these viewpoints, the inner layer may contain 80 to 60% by mass of the propylene-ethylene block copolymer (C) and 20 to 40% by mass of the ethylene-propylene copolymer elastomer (D).
[0044] The thickness of the multilayer film is not particularly limited as long as it can be used as a film for packaging materials, but if the film is too thick, it will be cost-intensive. Therefore, the thickness of the multilayer film can be 100 μm or less, and may be 50 to 70 μm.
[0045] The thickness of the outer layer (i.e., the total thickness of the first outer layer and the second outer layer) may be 16 to 42% or 25 to 42% based on the thickness of the multilayer film. When the ratio of the thickness of the outer layer is equal to or more than the lower limit, excellent transparency is easily obtained, and when it is equal to or less than the upper limit, deterioration of the impact resistance and heat sealability of the film can be suppressed, making it easy to obtain practical use.
[0046] The thickness of the inner layer can be 20 μm or more, and may be 30 μm or more, which maintains the flexibility of the film, makes the film less likely to break after retort treatment, and makes the heat seal strength less likely to decrease.
[0047] <Manufacturing method of multilayer film> The method for producing the multilayer film is not particularly limited, and known methods can be used. For example, examples of the thermoforming process include a melt-kneading method using a general mixer such as a single-screw extruder, a twin-screw extruder, or a multi-screw extruder, and a method in which the components are dissolved or dispersed and mixed, and then the solvent is removed by heating. In consideration of workability, a single-screw extruder or a twin-screw extruder can be used. When a single-screw extruder is used, the screw can be a full-flight screw, a screw with a mixing element, a barrier flight screw, a fluted screw, or the like, which can be used without any particular restrictions. As the twin-screw kneading device, a co-rotating twin-screw extruder, a counter-rotating twin-screw extruder, or the like can be used, and the screw shape can be a full-flight screw, a kneading disk type, or the like, which can be used without any particular restrictions.
[0048] In the above method, it is possible to use a method in which the multilayer film is melted using a single screw extruder or twin screw extruder, etc., and then formed into a film using a T-die via a feed block or a multi-manifold.
[0049] The obtained multilayer film may be subjected to a surface modification treatment to improve suitability for subsequent processes as necessary. For example, in order to improve printability when used as a single film or lamination suitability when used in a laminated form, a surface modification treatment may be performed on the printing surface or the surface that comes into contact with the substrate. Examples of the surface modification treatment include treatments such as corona discharge treatment, plasma treatment, and frame treatment that oxidize the film surface to generate functional groups, and modification treatments by a wet process that forms an easy-adhesion layer by coating.
[0050] <Packaging material> The multilayer film may be used as a single film or may be laminated with a substrate, and the method of use as a packaging material is not particularly limited.
[0051] When the multilayer film is laminated with a substrate, the packaging material can include the multilayer film and the substrate. Specifically, such a packaging material can be obtained by laminating at least one layer of a substrate such as a biaxially oriented polyamide film (ONy), a biaxially oriented polyester film (PET), a printed paper, a metal foil (AL foil), or a transparent vapor deposition film onto the multilayer film 10 to form a laminate. FIG. 2 is a cross-sectional view of a packaging material according to one embodiment of the present invention. The packaging material 100 shown in the figure includes a multilayer film 10, an adhesive layer 3, a substrate film 4, an adhesive layer 5, and a transparent vapor deposition film 6 in this order. The laminate can be produced by a normal dry lamination method in which the films constituting the laminate are bonded together using an adhesive, but if necessary, a method in which the multilayer film is directly extrusion laminated onto the substrate can also be used.
[0052] The laminate structure of the laminate can be adjusted appropriately according to the required properties of the packaging material, such as barrier properties that meet the shelf life of the packaged food, size and impact resistance to accommodate the weight of the contents, visibility of the contents, etc.
[0053] <Package> The packaging body may be made from the above packaging material, and there is no particular restriction on the form of the bag. For example, the above packaging material (laminate) can be used for a flat bag, a three-sided bag, a palm-shaped bag, a gusseted bag, a standing pouch, a pouch with a spout, a pouch with a beak, etc., using a multilayer film as a sealing material. EXAMPLES
[0054] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples.
[0055] <Preparation of various materials> The following propylene homopolymer (A), propylene-ethylene random copolymer (B), propylene-ethylene block copolymer (C), ethylene-propylene copolymer elastomer (D), and nucleating agent were prepared.
[0056] (Propylene homopolymer (A)) A propylene homopolymer having a melting onset temperature of 153°C, a melting peak temperature of 159°C, and a melt flow rate (MFR: ISO 1133) (temperature 230°C, load 2.16 kg) of 3.0 g / 10 min when measured by differential scanning calorimetry (JIS K 7121).
[0057] (Propylene-ethylene random copolymer (B)) When measured by differential scanning calorimetry (JIS K 7121), the melting start temperature was 142°C, the melting peak temperature was 147°C, and ΔH h / ΔH l A propylene-ethylene random copolymer having a molecular weight of 1.84 and an ethylene content of 3.4 mass%.
[0058] The ethylene content was measured according to the ethylene content determination method (IR method) described on pages 412-413 of the Polymer Analysis Handbook (May 10, 2013, 3rd printing) edited by the Polymer Analysis Roundtable of the Japan Analytical Society. ΔH h / ΔH l is the heat of fusion ΔH on the higher side of the measurement temperature 135°C when differential scanning calorimetry (JIS K 7121) is performed. h and the heat of fusion on the low temperature side ΔH l This is the ratio of
[0059] (Propylene-ethylene block copolymer (C)) A propylene-ethylene block copolymer having a melt flow rate (MFR: ISO 1133) of 2.0 g / 10 min (temperature 230°C, load 2.16 kg), which contains 77.1 mass % propylene polymer and 22.9 mass % ethylene-propylene copolymer, with the ethylene content of the ethylene-propylene copolymer being 28.7 wt %.
[0060] (Ethylene-propylene copolymer elastomer (D)) An ethylene-propylene copolymer elastomer with a melt flow rate (MFR: ISO 1133) (temperature 230°C, load 2.16 kg) of 0.6 g / 10 min and a propylene content / ethylene content of 2.7.
[0061] (Nucleating agent) Clearmaster H8020 (sorbitol-based crystal nucleating agent) manufactured by Dainichi Seikagaku Kogyo Co., Ltd. Clearmaster R8020 (sorbitol-based crystal nucleating agent) manufactured by Dainichi Seikagaku Kogyo Co., Ltd.
[0062] <Preparation of laminated film> Example 1 To form the first outer layer, a resin mixture was prepared by mixing 50 parts by mass of propylene homopolymer (A), 50 parts by mass of propylene-ethylene random copolymer (B) and nucleating agent Clearmaster H8020 in pellet form. The amount of nucleating agent added was 2.0 parts by mass per 100 parts by mass of the total amount of propylene homopolymer (A) and propylene-ethylene random copolymer (B). For forming the second outer layer, a resin mixture was prepared by mixing 50 parts by mass of a propylene homopolymer (A) and 50 parts by mass of a propylene-ethylene random copolymer (B) in a pellet state. For forming the inner layer, a resin mixture was prepared by mixing 67.8 parts by mass of a propylene-ethylene block copolymer (C) and 32.2 parts by mass of an ethylene-propylene copolymer (D) in a pellet state. Each resin mixture was fed to an extruder whose temperature was controlled at 250°C, kneaded in a molten state, and laminated in a T-die extruder equipped with a feed block so that the first outer layer and second outer layer were each 10 μm thick, and the inner layer was 40 μm thick, to produce the film of Example 1.
[0063] Example 2 A film of Example 2 was produced in the same manner as in Example 1, except that the blending ratio of the nucleating agent was changed as shown in Table 1.
[0064] Example 3 A film of Example 3 was produced in the same manner as in Example 1, except that Clear Master R8020 was used instead of Clear Master H8020.
[0065] Example 4 The film of Example 4 was produced in the same manner as in Example 3, except that the blending ratio of the nucleating agent was changed as shown in Table 1.
[0066] Comparative Example 1 A film of Comparative Example 1 was produced in the same manner as in Example 1, except that only the propylene homopolymer (A) was used to form the outer layer.
[0067] Comparative Example 2 A film of Comparative Example 2 was prepared in the same manner as in Example 1, except that only the propylene-ethylene random copolymer (B) was used to form the outer layer.
[0068] Comparative Example 3 A film of Comparative Example 3 was produced in the same manner as in Example 1, except that no nucleating agent was used.
[0069] Comparative Example 4 A resin mixture obtained by mixing 67.8 parts by mass of the propylene-ethylene block copolymer (C) and 32.2 parts by mass of the ethylene-propylene copolymer (D) in a pellet state was used to prepare a film of Comparative Example 4 having a thickness of 60 μm.
[0070] Comparative Example 5 A film of Comparative Example 5 was produced in the same manner as in Example 1, except that the blending ratio of the nucleating agent was changed as shown in Table 1.
[0071] Comparative Example 6 A film of Comparative Example 6 was produced in the same manner as in Example 1, except that the blending ratio of the nucleating agent was changed as shown in Table 1.
[0072] <Various evaluations> The films obtained in each example were subjected to the following evaluations, and the results are shown in Table 1.
[0073] [Haze measurement] A bag measuring 297 mm x 420 mm was made using the film obtained in each example, 800 g of water was placed inside, and retorted for 40 minutes at 135° C. A film sample measuring 50 mm x 50 mm was cut out from the bag after retort treatment, and evaluated using a haze meter (model number COH7700) manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with the haze measurement method described in JIS K7136.
[0074] [Cold impact resistance evaluation] Using a film impact tester manufactured by Toyo Seiki Co., Ltd., the cold impact resistance of the films obtained in each example was evaluated under conditions of a temperature of -5°C, a weight of 1.5 J, and a bullet size of 1 / 2 inch.
[0075] [Fusion strength measurement] The films obtained in each example were heat-sealed together using a heat sealer manufactured by Tester Sangyo Co., Ltd. under the conditions of a sealing pressure of 0.03 MPa, a sealing time of 30 seconds, a sealing width of 10 mm, and a sealing temperature of 135° C. The heat-sealed film was then cut into a piece of 15 mm width x 80 mm, and a tensile tester manufactured by Shimadzu Corporation was used to perform a T-peel test at a tensile speed of 300 mm / min to measure the fusion strength of the heat-sealed portion.
[0076] [Table 1] [Industrial Applicability]
[0077] The polypropylene-based multi-layer film of the present invention has high levels of heat resistance, transparency and cold impact resistance, and can be suitably used as a sealant film for retort packaging. [Explanation of symbols]
[0078] 10...multilayer film, 100...packaging material, 1a...first outer layer, 1b...second outer layer, 2...inner layer, 3...adhesive layer, 4...base film, 5...adhesive layer, 6...transparent vapor deposition film.
Claims
1. a first outer layer which is a heat seal layer containing a propylene homopolymer (A), a propylene-ethylene random copolymer (B) and a nucleating agent; an inner layer containing a propylene-ethylene block copolymer (C) and an ethylene-propylene copolymer elastomer (D); a second outer layer containing a propylene homopolymer (A) and a propylene-ethylene random copolymer (B) in this order, and not containing a nucleating agent; a content of the nucleating agent in the first outer layer is 1 to 5 parts by mass relative to 100 parts by mass of the total amount of the propylene homopolymer (A) and the propylene-ethylene random copolymer (B).
2. The multilayer film according to claim 1, wherein the first outer layer and the second outer layer contain 70 to 30 parts by mass of the propylene homopolymer (A) and 30 to 70 parts by mass of the propylene-ethylene random copolymer (B).
3. The multilayer film according to claim 1 or 2, wherein the propylene homopolymer (A) satisfies the following requirement (a1), and the propylene-ethylene random copolymer (B) satisfies the following requirement (b1): Requirement (a1): The melting onset temperature is 150° C. or higher and the melting peak temperature is 155° C. or higher, as measured by differential scanning calorimetry (JIS K 7121). Requirement (b1): The ethylene content is 5% by mass or less.
4. The multilayer film according to any one of claims 1 to 3, wherein the inner layer contains 90 to 50% by mass of the propylene-ethylene block copolymer (C) and 10 to 50% by mass of the ethylene-propylene copolymer elastomer (D).
5. A packaging material comprising the multilayer film according to any one of claims 1 to 4 and a substrate.
6. A package produced from the packaging material according to claim 5.
Citation Information
Patent Citations
Composite film and laminate thereof
JP1987003950A
Laminated film
JP1997150488A
Laminated polypropylene film
JP1998138419A
Polypropylene composite film
JP1999138716A
Polypropylene composite non-stretched film
JP2007045049A