Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display element

A liquid crystal aligning agent with specific polymers forms a high refractive index alignment film that enhances light transmittance and vertical alignment, addressing the refractive index mismatch issue in liquid crystal displays to improve brightness in high-definition panels.

JP7582304B2Active Publication Date: 2024-11-13NISSAN CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022514318
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-10
Filing Date
2021-02-05
Publication Date
2024-11-13
Estimated Expiration
2041-02-05

AI Technical Summary

Technical Problem

The refractive index mismatch between transparent conductive films and liquid crystal alignment films in liquid crystal display elements leads to reduced light transmittance and display brightness, particularly in high-definition panels like 4K and 8K displays, due to light reflection at their interfaces, which affects the aperture ratio and overall brightness.

Method used

A liquid crystal aligning agent is developed containing specific polymers with a triazine ring terminal capped by an arylamino group having a crosslinking group, which forms a liquid crystal alignment film with a high refractive index and high vertical alignment, ensuring high light transmittance without coloring properties.

Benefits of technology

The solution achieves a liquid crystal alignment film with a high refractive index and high light transmittance, improving display brightness and maintaining vertical alignment, suitable for high-definition panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582304000064
    Figure 0007582304000064
  • Figure 0007582304000065
    Figure 0007582304000065
  • Figure 0007582304000001
    Figure 0007582304000001
Patent Text Reader

Abstract

The present invention provides: a liquid crystal aligning agent that forms a liquid crystal alignment film that, while having a high refractive index, has high light transmittance because of a lack of coloring properties; and a liquid crystal alignment agent that, in addition to the properties noted above, has high homeotropic alignment. This liquid crystal alignment agent contains a component (A) and a component (B), described below. Component (A) is a polymer (A) of at least one type chosen from the group consisting of polyimide precursors and polyimides that are imidated forms of such polyimide precursors; and component (B) is a polymer (B) characterized in that the polymer includes a repeated unit structure represented by formula (1) and has at least one triazine ring terminal, at least part of this triazine ring terminal being blocked by an arylamino group that comprises a cross-linking group.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid crystal aligning agent, a liquid crystal alignment film obtained from the liquid crystal aligning agent, and a liquid crystal display device having the liquid crystal alignment film. [Background technology]

[0002] Conventionally, various driving methods have been developed for liquid crystal display elements, which differ in electrode structure and physical properties of the liquid crystal molecules used, and various display elements such as TN (Twisted Nematic) type, STN (Super Twisted Nematic) type, VA (Vertical Alignment) type, IPS (In-Plane Switching) type, and FFS (fringe field switching) type are known. A liquid crystal display element is generally configured by arranging a pair of electrode substrates facing each other with a predetermined gap (several μm) and sealing liquid crystal between the electrode substrates. Display on the liquid crystal display element is performed by applying a voltage between the transparent conductive films constituting the electrodes of the electrode substrates. In addition, these liquid crystal display elements have a liquid crystal alignment film for orienting the liquid crystal molecules. Known materials for the liquid crystal alignment film include, for example, polyamic acid (polyamide acid), polyamic acid ester, polyimide, etc. (see Patent Document 1, etc.). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2016-080458 Summary of the Invention [Problem to be solved by the invention]

[0004] The transparent conductive film in the liquid crystal display element is usually formed of a composition (ITO) in which indium oxide is the main component and is doped with a few percent of tin oxide, but its refractive index is different from that of the liquid crystal alignment film and has a high value. Therefore, when light from a display light source is transmitted through the electrode substrate, the light is reflected at the interface between the transparent conductive film and the liquid crystal alignment film in each electrode substrate. As a result, the light transmittance of the electrode substrate cannot be sufficiently obtained, leading to a problem of reduced display brightness. In particular, ultra-high definition panels such as 4K and 8K have been developed in recent years, but these panels require a large occupancy rate of black matrix (BM) and TFT, etc., which reduces the aperture ratio of the panel, so improving the transmittance of the display area is becoming important.

[0005] Therefore, the present inventors have investigated various materials for forming the liquid crystal alignment film in order to increase the refractive index of the liquid crystal alignment film, from the viewpoint that the above-mentioned problems can be solved by reducing the difference between the refractive index of the transparent conductive film and the refractive index of the liquid crystal alignment film. Specifically, in order to increase the refractive index of the liquid crystal alignment film, various types of polymers to be contained in the liquid crystal alignment agent forming the liquid crystal alignment film have been searched for.

[0006] As a result, by selecting a specific polymer, it was possible to obtain a liquid crystal alignment film having a high refractive index close to that of the transparent conductive film, but on the other hand, it was revealed that the polymer forming the liquid crystal alignment film having a high refractive index is often colored. A liquid crystal alignment film formed from a liquid crystal alignment agent containing a colored polymer has a low light transmittance, which leads to a decrease in display brightness, and as a result, the above-mentioned object is not achieved. In addition, it was revealed that it is difficult to obtain a high refractive index for a liquid crystal alignment film with high vertical alignment due to the influence of the side chain structure, and a liquid crystal alignment film having both a high refractive index and vertical alignment was required.

[0007] In view of the above circumstances, the object of the present invention is to provide a liquid crystal aligning agent which forms a liquid crystal alignment film having a high refractive index but no coloring and therefore high light transmittance, a liquid crystal alignment film obtained from the liquid crystal aligning agent, and a liquid crystal display element having the liquid crystal alignment film.Furthermore, the object of the present invention is to provide a liquid crystal aligning agent which forms a liquid crystal alignment film having high vertical alignment property in addition to the above characteristics, a liquid crystal alignment film obtained from the liquid crystal aligning agent, and a liquid crystal display element having the liquid crystal alignment film. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted intensive research to achieve the above object, and as a result have found that a liquid crystal aligning agent containing a specific polymer is effective for achieving the above object, thereby completing the present invention.

[0009] The present invention includes the following aspects. [1] A liquid crystal aligning agent comprising the following components (A) and (B): Component (A): at least one polymer (A) selected from the group consisting of polyimide precursors and polyimides which are imidized products of the polyimide precursors Component (B): A polymer (B) comprising a repeating unit structure represented by the following formula (1), having at least one triazine ring terminal, at least a portion of which is blocked with an arylamino group having a crosslinking group: [ka] (R and R' each independently represent a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, or an aralkyl group; Ar represents at least one selected from the group represented by formulas (2) to (12). [ka] (Any hydrogen atom on the aromatic ring of formulas (2) to (12) may be substituted, R 12 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, W 1 and W 2 are, independently of each other, a single bond, -CR 95 R 96 -(R 95 and R 96 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms (which may be joined together to form a ring), -C(=O)-, -O-, -S-, -S(=O)-, -SO2-, or -NR 97 -(R 97 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a phenyl group; X 1 and X 2 each independently represents a single bond, an alkylene group having 1 to 10 carbon atoms, or a group represented by -Y1-Ph-Y2- (Ph represents a phenylene group, any hydrogen atom on the phenylene group may be substituted, and Y1 and Y2 each independently represent a single bond or an alkylene group having 1 to 10 carbon atoms). Effect of the Invention

[0010] According to the present invention, it is possible to provide a liquid crystal aligning agent that forms a liquid crystal alignment film having a high refractive index but no coloring and therefore a high light transmittance, a liquid crystal alignment film obtained from the liquid crystal aligning agent, and a liquid crystal display element having the liquid crystal alignment film.Furthermore, it is possible to provide a liquid crystal aligning agent that forms a liquid crystal alignment film having high vertical alignment property in addition to the above characteristics, a liquid crystal alignment film obtained from the liquid crystal aligning agent, and a liquid crystal display element having the liquid crystal alignment film. [Brief description of the drawings]

[0011] [Figure 1] 1 is a graph showing the results of measuring the 1H-NMR spectrum of compound T-1 synthesized in an example. [Diagram 2] 1 is a graph showing the results of measuring the 1H-NMR spectrum of compound T-2 synthesized in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the liquid crystal alignment agent of the present invention, the liquid crystal alignment film obtained from the liquid crystal alignment agent, and the liquid crystal display element having the liquid crystal alignment film will be described in detail. However, the explanation of the constituent elements described below is an example of one embodiment of the present invention, and the present invention is not limited to these contents.

[0013] (Liquid crystal alignment agent) The liquid crystal aligning agent of the present invention contains the following components (A) and (B): Component (A): at least one polymer (A) selected from the group consisting of polyimide precursors and polyimides which are imidized products of the polyimide precursors Component (B): A polymer (B) containing a repeating unit structure represented by the above formula (1), having at least one triazine ring terminal, at least a part of which is blocked with an arylamino group having a crosslinking group. The polymer (A) which is the component (A) and the polymer (B) which is the component (B) will each be described in detail below.

[0014] <Polymer (A)> The liquid crystal aligning agent of the present invention contains at least one polymer (A) selected from the group consisting of polyimide precursors and polyimides which are imidized products of the polyimide precursors. The polymer constituting component (A) may be composed of one type of polymer or two or more types of polymers. Examples of the polyimide precursor include polyamic acid, polyamic acid ester, and polyamic acid-polyamic acid ester copolymer, and the polyimide precursor is preferably obtained by polymerizing a diamine component and a tetracarboxylic acid component.

[0015] <<Diamine component>> The diamine component may be at least one diamine (a) selected from the group consisting of structures represented by the following formulas (S1) to (S3): p-phenylenediamine, m-phenylenediamine, 4-(2-(methylamino)ethyl)aniline, 2,4-diaminobenzoic acid, 2,5-diaminobenzoic acid, 3,5-diaminobenzoic acid, or diamine compounds represented by the following formulas (3b-1) to (3b-4), each of which has a carboxyl group; 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylamine, ter, 3,3'-diaminodiphenyl ether, 1,2-bis(4-aminophenyl)ethane, 1,3-bis(4-aminophenyl)propane, 1,4-bis(4-aminophenyl)butane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,2-bis(4-aminophenoxy)ethane, 1,2-bis(4-amino-2-methylphenoxy)ethane, 1,3-bis(4-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane Tan, 1,6-bis(4-aminophenoxy)hexane, 4-(2-(4-aminophenoxy)ethoxy)-3-fluoroaniline, di(2-(4-aminophenoxy)ethyl)ether, 4-amino-4'-(2-(4-aminophenoxy)ethoxy)biphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 1,4-diaminonaphthalene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2 diamines having a urea bond such as 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 2,2'-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis(4-aminophenyl)propane, and 1,3-bis(4-aminophenethyl)urea; diamines having a photopolymerizable group at the end such as 2-(2,4-diaminophenoxy)ethyl methacrylate and 2,4-diamino-N,N-diallylaniline; diamines having a radical initiation function such as those represented by the following formulas (R1) to (R5);Examples of the diamine include, but are not limited to, diamines having a photosensitizing function that exhibits a sensitizing effect upon irradiation with light, such as 4'-diaminobenzophenone, 3,3'-diaminobenzophenone, and 9,9-bis(4-aminophenyl)fluorene; 2,6-diaminopyridine, 3,4-diaminopyridine, 2,4-diaminopyrimidine, 3,6-diaminocarbazole, N-methyl-3,6-diaminocarbazole; diamines having a heterocycle, such as those shown in the following formulae (z-1) to (z-18); diamines having a diphenylamine skeleton, such as those shown in the following formulae (Dp-1) to (Dp-9); diamines having a group "-N(D)-" (D represents a protecting group that is eliminated by heating and replaced with a hydrogen atom, preferably a tert-butoxycarbonyl group), such as those shown in the following formulae (5-1) to (5-10); and aromatic diamines having an oxazoline structure, such as those shown in the following formulae (Ox-1) to (Ox-2). The diamine component may be composed of one or more diamines.

[0016] [ka] (X 1 and X 2 are each independently a single bond, -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -COO-, -OCO- or -((CH2) a1 -A1) m1 - (a1 is an integer of 1 to 15, A1 represents an oxygen atom or -COO-, and m1 is an integer of 1 to 2. When m1 is 2, a1 and A1 each independently have the above definition.) 1 and G 2each independently represents a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms and a divalent alicyclic group having 3 to 8 carbon atoms. Any hydrogen atom on the cyclic group may be substituted with an alkyl group having 1 to 3 carbon atoms, an alkoxyl group having 1 to 3 carbon atoms, a fluorine atom-containing alkyl group having 1 to 3 carbon atoms, a fluorine atom-containing alkoxy group having 1 to 3 carbon atoms, or a fluorine atom. m and n each independently represent an integer of 0 to 3, and m+n represents an integer of 1 to 6, preferably an integer of 1 to 4. R 1 represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms; R 1 Any hydrogen atom forming the formula (I) may be substituted with a fluorine atom.

[0017] [ka] (X 3 represents a single bond, -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CHO-, -COO- or -OCO-. 2 represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms; R 2 Any hydrogen atom forming the formula (I) may be substituted with a fluorine atom.

[0018] [ka] (X 4 represents -CONH-, -NHCO-, -O-, -CHO-, -COO- or -OCO-. 3 represents a structure having a steroid skeleton.)

[0019] [ka] (In formula (3b-1), A 1represents a single bond, -CH2-, -C2H4-, -C(CH3)2-, -CF2-, -C(CF3)2-, -O-, -CO-, -NH-, -N(CH3)-, -CONH-, -NHCO-, -CHO-, -OCH2-, -COO-, -OCO-, -CON(CH3)- or -N(CH3)CO-, m1 and m2 each independently represent an integer of 0 to 4, and m1+m2 represents an integer of 1 to 4. In formula (3b-2), m3 and m4 each independently represent an integer of 1 to 5. In formula (3b-3), A 2 represents a linear or branched alkyl group having 1 to 5 carbon atoms, and m5 is an integer of 1 to 5. 3 and A 4 each independently represents a single bond, -CH2-, -C2H4-, -C(CH3)2-, -CF2-, -C(CF3)2-, -O-, -CO-, -NH-, -N(CH3)-, -CONH-, -NHCO-, -CHO-, -OCH2-, -COO-, -OCO-, -CON(CH3)- or -N(CH3)CO-, and m6 is an integer of 1 to 4.

[0020] [ka]

[0021] [ka]

[0022] [ka] (In (R3) to (R5), n is an integer from 1 to 6.)

[0023] [ka]

[0024] [ka] (Boc represents a tert-butoxycarbonyl group.)

[0025] [ka]

[0026] The diamine (a) preferably has at least one benzene ring. More preferred specific examples include diamines represented by the following formula (d1) or formula (d2).

[0027] [ka] (X is a single bond, -O-, -C(CH3)2-, -NH-, -CO-, -(CH2) m -, -SO2-, -O-(CH2) m -O-, -OC(CH3)2-, -CO-(CH2) m -, -NH-(CH2) m -, -SO2-(CH2) m -, -CONH-(CH2) m -, -CONH-(CH2) m -NHCO- or -COO-(CH2) m represents --OCO--; m is an integer of 1 to 8; Y represents any of the structures of the above formulae (S1) to (S3); in formula (d2), the two Y's may be the same or different.

[0028] Preferred examples of the diamine represented by the above formula (d1) include the following formulas (d1-1) to (d1-7): Preferred examples of the diamine represented by the above formula (d2) include the following formulas (d2-1) to (d2-6):

[0029] [ka]

[0030] [ka] (X v1 ~X v4 , X p1~X p8 are each independently -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CHO-, -CH2-OCO-, -COO-, or -OCO-; X V5 ~X V6 , X s1 ~X s4 Each independently represents -O-, -CH2O-, -COO- or -OCO-. X v7 represents -O-, -CH2O-, -CH2-OCO-, -COO-, or -OCO-. X a ~X f is a single bond, -O-, -NH-, -O-(CH2) m -O- (m is an integer of 1 to 8), R v1 ~R v4 , R 1a ~R 1h are each independently: -C n H 2n+1 (n is an integer from 1 to 20), -OC n H 2n+1 (n is an integer from 2 to 20).

[0031] The above-mentioned diamines having a radical initiating function or diamines having a photosensitizing function that exhibit a sensitizing effect upon light irradiation may be used alone or in combination of two or more kinds when producing polymer (A) in order to increase the response speed of liquid crystal display elements such as PSA type liquid crystal display elements and SC-PVA mode liquid crystal display elements.

[0032] Of the above, from the viewpoint of suitably obtaining the effects of the present invention, the diamine component is preferably p-phenylenediamine, 3,5-diaminobenzoic acid, 4,4'-diaminodiphenylmethane, 4,4'-diaminobenzophenone, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2-(2,4-diaminophenoxy)ethyl methacrylate, 2,4-diamino-N,N-diallylaniline, diamines represented by the above formulae (R1) to (R5), diamines represented by the above formulae (z-1) to (z-18), diamines represented by the above formulae (Dp-1) to (Dp-9), or diamines represented by the above formulae (Ox-1) to (Ox-2).

[0033] In addition, examples of the diamine component include aliphatic diamines such as metaxylenediamine, alicyclic diamines such as 4,4-methylenebis(cyclohexylamine), and diamines described in WO 2016 / 125870.

[0034] <<Tetracarboxylic acid component>> The tetracarboxylic acid component refers to a component containing at least one selected from tetracarboxylic acids and tetracarboxylic acid derivatives. Examples of the tetracarboxylic acid derivatives include tetracarboxylic acid dihalides, tetracarboxylic acid dianhydrides, tetracarboxylic acid diester dichlorides, and tetracarboxylic acid diesters. The tetracarboxylic acid component may be composed of one or more types of tetracarboxylic acids and tetracarboxylic acid derivatives. The tetracarboxylic acid component for producing the polymer (A) may be an aromatic tetracarboxylic acid dianhydride, an aliphatic tetracarboxylic acid dianhydride, an alicyclic tetracarboxylic acid dianhydride, or a derivative thereof. Here, the aromatic tetracarboxylic acid dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups, including at least one carboxyl group bonded to an aromatic ring. The aliphatic tetracarboxylic acid dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups bonded to a chain hydrocarbon structure. However, it is not necessary to be composed of only a chain hydrocarbon structure, and it may have an alicyclic structure or an aromatic ring structure in part. The alicyclic tetracarboxylic acid dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups, including at least one carboxyl group bonded to an alicyclic structure. However, none of these four carboxyl groups are bonded to an aromatic ring. In addition, it is not necessary to be composed of only an alicyclic structure, and it may have a chain hydrocarbon structure or an aromatic ring structure in part.

[0035] The tetracarboxylic acid component preferably contains a tetracarboxylic dianhydride represented by the following formula (S4).

[0036] [ka] (X represents a structure selected from the group consisting of the following (x-1) to (x-13).)

[0037] [ka] (R 1 ~R 4 R each independently represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom, a monovalent organic group having 1 to 6 carbon atoms containing a fluorine atom, or a phenyl group. 5 and R 6 each independently represents a hydrogen atom or a methyl group; j and k are integers of 0 or 1; A1 and A2 each independently represent a single bond, -O-, -CO-, -COO-, phenylene, sulfonyl, or amide bond; *1 is a bond bonded to one acid anhydride group, and *2 is a bond bonded to the other acid anhydride group.

[0038] More preferred specific examples of the above formula (x-1) include the following formulae (X1-1) to (X1-6), in which * represents a bond.

[0039] [ka]

[0040] Preferred specific examples of the above (x-12) and (x-13) include the following formulae (x-14) to (x-29), in which "*" represents a bond.

[0041] [ka]

[0042] [ka]

[0043] Preferred examples of the tetracarboxylic dianhydride represented by the above formula (S4) or a derivative thereof include tetracarboxylic dianhydrides represented by formula (3) in which X is represented by the above formulae (x-1) to (x-7) and (x-11) to (x-13) or a derivative thereof.

[0044] <Method for producing polymer (A)> The polymer (A) used in the present invention can be synthesized by a known method such as that described in International Publication WO2013 / 157586.

[0045] A polyimide can be obtained by ring-closing (imidization) the polyimide precursor obtained in the polymer (A). Note that the imidization rate referred to in this specification refers to the ratio of imide groups to the total amount of imide groups derived from tetracarboxylic dianhydride or its derivatives and carboxyl groups (or their derivatives).

[0046] The molecular weight of the polymer (A) used in the present invention is preferably 5,000 to 1,000,000, more preferably 10,000 to 150,000, in terms of weight average molecular weight measured by GPC (Gel Permeation Chromatography), taking into consideration the strength of the liquid crystal alignment film obtained therefrom, workability during film formation, and coating properties.

[0047] <Polymer (B)> The liquid crystal aligning agent of the present invention contains a polymer (B) which includes a repeating unit structure represented by the following formula (1), has at least one triazine ring terminal, and at least a part of the triazine ring terminal is blocked with an arylamino group having a crosslinking group. The polymer constituting the component (B) may be composed of one kind of polymer or two or more kinds of polymers.

[0048] [ka] (R and R' each independently represent a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, or an aralkyl group; Ar represents at least one selected from the group represented by the formulas (2) to (12).

[0049] [ka] (Any hydrogen atom on the aromatic ring of formulas (2) to (12) may be substituted, R 12 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, W 1 and W 2 are, independently of each other, a single bond, -CR 95 R 96 -(R 95 and R 96 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms (which may be joined together to form a ring), -C(=O)-, -O-, -S-, -S(=O)-, -SO2-, or -NR 97 -(R 97 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a phenyl group; X 1 and X 2 each independently represents a single bond, an alkylene group having 1 to 10 carbon atoms, or a group represented by -Y1-Ph-Y2- (Ph represents a phenylene group, any hydrogen atom on the phenylene group may be substituted, and Y1 and Y2 each independently represent a single bond or an alkylene group having 1 to 10 carbon atoms).

[0050] In the above formula (1), R and R' each independently represent a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, or an aralkyl group, but from the viewpoint of further increasing the refractive index, it is preferable that both are hydrogen atoms. In the present invention, the number of carbon atoms in the alkyl groups R and R' in the above formula (1) is not particularly limited, but is preferably 1 to 20, and in consideration of further improving the heat resistance of the polymer, the number of carbon atoms is more preferably 1 to 10, and even more preferably 1 to 3. In addition, the structure may be any of linear, branched, and cyclic.

[0051] Specific examples of the alkyl groups R and R' in the above formula (1) include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, 1-methyl-cyclopropyl, 2-methyl-cyclopropyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, cyclopentyl, 1-methyl-cyclobutyl, 2-Methyl-cyclobutyl, 3-Methyl-cyclobutyl, 1,2-Dimethyl-cyclopropyl, 2,3-Dimethyl-cyclopropyl, 1-Ethyl-cyclopropyl, 2-Ethyl-cyclopropyl, n-Hexyl, 1-Methyl-n-pentyl, 2-Methyl-n-pentyl, 3-Methyl-n-pentyl, 4-Methyl-n-pentyl, 1,1-Dimethyl-n-butyl, 1,2-Dimethyl-n-butyl, 1,3-Dimethyl-n-butyl, 2,2-Dimethyl-n-butyl, 2,3-Dimethyl-n-butyl, 3,3-Dimethyl-n-butyl, 1-Ethyl-n-butyl ethyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl, 1,3-dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2,3-dimethyl-cyclobutyl, 2, Examples of such cyclopropyl groups include 4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-isopropyl-cyclopropyl, 2-isopropyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,3-trimethyl-cyclopropyl, 1-ethyl-2-methyl-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl, and 2-ethyl-3-methyl-cyclopropyl groups.

[0052] The number of carbon atoms in the alkoxy groups R and R' in the above formula (1) is not particularly limited, but is preferably 1 to 20, and in consideration of further improving the heat resistance of the polymer, the number of carbon atoms is more preferably 1 to 10, and even more preferably 1 to 3. In addition, the structure of the alkyl portion may be any of linear, branched, and cyclic.

[0053] Specific examples of the alkoxy groups R and R' in the above formula (1) include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, n-pentoxy, 1-methyl-n-butoxy, 2-methyl-n-butoxy, 3-methyl-n-butoxy, 1,1-dimethyl-n-propoxy, 1,2-dimethyl-n-propoxy, 2,2-dimethyl-n-propoxy, 1-ethyl-n-propoxy, n-hexyloxy, 1-methyl-n-pentyloxy, 2-methyl-n-pentyloxy, Examples of the alkyl group include 3-methyl-n-pentyloxy, 4-methyl-n-pentyloxy, 1,1-dimethyl-n-butoxy, 1,2-dimethyl-n-butoxy, 1,3-dimethyl-n-butoxy, 2,2-dimethyl-n-butoxy, 2,3-dimethyl-n-butoxy, 3,3-dimethyl-n-butoxy, 1-ethyl-n-butoxy, 2-ethyl-n-butoxy, 1,1,2-trimethyl-n-propoxy, 1,2,2-trimethyl-n-propoxy, 1-ethyl-1-methyl-n-propoxy, and 1-ethyl-2-methyl-n-propoxy groups.

[0054] The number of carbon atoms in the aryl group of R and R' in the above formula (1) is not particularly limited, but is preferably 6 to 40. In consideration of further improving the heat resistance of the polymer, the number of carbon atoms is more preferably 6 to 16, and even more preferably 6 to 13. Specific examples of the aryl group for R and R' in the above formula (1) include phenyl, o-chlorophenyl, m-chlorophenyl, p-chlorophenyl, o-fluorophenyl, p-fluorophenyl, o-methoxyphenyl, p-methoxyphenyl, p-nitrophenyl, p-cyanophenyl, α-naphthyl, β-naphthyl, o-biphenylyl, m-biphenylyl, p-biphenylyl, 1-anthryl, 2-anthryl, 9-anthryl, 1-phenanthryl, 2-phenanthryl, 3-phenanthryl, 4-phenanthryl, and 9-phenanthryl groups.

[0055] The number of carbon atoms in the aralkyl group of R and R' in the above formula (1) is not particularly limited, but it is preferably 7 to 20 carbon atoms, and the alkyl portion may be linear, branched, or cyclic. Specific examples thereof include benzyl, p-methylphenylmethyl, m-methylphenylmethyl, o-ethylphenylmethyl, m-ethylphenylmethyl, p-ethylphenylmethyl, 2-propylphenylmethyl, 4-isopropylphenylmethyl, 4-isobutylphenylmethyl, and α-naphthylmethyl groups.

[0056] Any hydrogen atom on the aromatic ring in the above formulas (2) to (12) may be substituted with a halogen atom, a carboxy group, a sulfo group, an alkyl group having 1 to 10 carbon atoms which may have a branched structure, a halogenated alkyl group having 1 to 10 carbon atoms which may have a branched structure, or an alkoxy group having 1 to 10 carbon atoms which may have a branched structure.

[0057] Examples of the halogen atom which is a substituent on the aromatic ring in the above formulas (2) to (12) include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. In addition, examples of the alkyl group and alkoxy group which are the substituents on the aromatic ring in the above formulas (2) to (12) include the same structures as those exemplified in the above formula (1).

[0058] The halogenated alkyl group having 1 to 10 carbon atoms which is a substituent on the aromatic ring in the above formulas (2) to (12) is one in which at least one hydrogen atom in the above alkyl group having 1 to 10 carbon atoms which may have a branched structure is substituted with a halogen atom. Specific examples thereof include trifluoromethyl, 2,2,2-trifluoroethyl, perfluoroethyl, 3,3,3-trifluoropropyl, 2,2,3,3,3-pentafluoropropyl, 2,2,3,3-tetrafluoropropyl, 2,2,2-trifluoro-1-(trifluoromethyl)ethyl, perfluoropropyl, 4, Examples of such groups include 4,4-trifluorobutyl, 3,3,4,4,4-pentafluorobutyl, 2,2,3,3,4,4,4-heptafluorobutyl, perfluorobutyl, 2,2,3,3,4,4,5,5,5-nonafluoropentyl, 2,2,3,3,4,4,5,5-octafluoropentyl, perfluoropentyl, 2,2,3,3,4,4,5,5,6,6,6-undecafluorohexyl, 2,2,3,3,4,4,5,5,6,6-decafluorohexyl, 3,3,4,4,5,5,6,6,6-nonafluorohexyl, and perfluorohexyl groups.

[0059] X in the above formula (11) 1 , X 2 Examples of the alkylene group having 1 to 10 carbon atoms include methylene, ethylene, propylene, trimethylene, tetramethylene, and pentamethylene groups.

[0060] Any hydrogen atom on the phenylene group in the above group "-Y1-Ph-Y2-" may be replaced with a halogen atom, a carboxyl group, a sulfo group, an alkyl group having 1 to 10 carbon atoms which may have a branched structure, a halogenated alkyl group having 1 to 10 carbon atoms which may have a branched structure, or an alkoxy group having 1 to 10 carbon atoms which may have a branched structure.

[0061] When any hydrogen atom on the aromatic ring in the above formulas (2) to (12) and any hydrogen atom on the phenylene group in the group "-Y1-Ph-Y2-" are substituted, among the above examples, a halogen atom, a sulfo group, an alkyl group having 1 to 5 carbon atoms which may have a branched structure, a halogenated alkyl group having 1 to 5 carbon atoms which may have a branched structure, or an alkoxy group having 1 to 5 carbon atoms which may have a branched structure is preferred.

[0062] As Ar in the above formula (1), at least one of the formulae (2), (5) to (12) is preferable, and at least one of the formulae (2), (5), (7), (8), (11) to (12) is more preferable. Specific examples of the aryl group represented by the above formulae (2) to (12) include, but are not limited to, those represented by the following formulae (1-1) to (1-25). In the formulae, Ph represents a phenyl group.

[0063] [ka]

[0064] [ka]

[0065] Among these, the aryl groups represented by the above formulas (1-1), (1-2), (1-5) to (1-15), (1-18) to (1-21), and (1-23) to (1-25) are more preferable since polymers having higher refractive indexes can be obtained.

[0066] In particular, in order to further increase the solubility of the polymer in organic solvents, Ar is preferably a m-phenylene group represented by formula (21-a).

[0067] [ka]

[0068] Furthermore, the polymer (B) of the present invention has at least one triazine ring terminal, and at least a portion of the triazine ring terminal is blocked with an arylamino group having a crosslinking group. The polymer (B) of the present invention has at least one triazine ring terminal, and this terminal triazine ring usually has two halogen atoms that can be substituted with the arylamino group having the crosslinking group. Therefore, the arylamino group having the crosslinking group may be bonded to the same triazine ring terminal, or when there are multiple triazine ring terminals, each may be bonded to a different triazine ring terminal.

[0069] Examples of the aryl group of the arylamino group having a crosslinking group include the same as those mentioned above, with a phenyl group being particularly preferred.

[0070] Examples of the crosslinking group include a hydroxy-containing group, a vinyl-containing group, an epoxy-containing group, an oxetane-containing group, a carboxy-containing group, a sulfo-containing group, a thiol-containing group, and a (meth)acryloyl-containing group. In consideration of improving the heat resistance of the polymer (B), the hydroxy-containing group and the (meth)acryloyl-containing group are preferred.

[0071] Examples of the hydroxy-containing group include a hydroxy group, a hydroxyalkyl group, etc. Both the hydroxy group and the hydroxyalkyl group are preferred, with a hydroxyalkyl group having 1 to 10 carbon atoms being more preferred. Examples of the hydroxyalkyl group having 1 to 10 carbon atoms include hydroxymethyl, 2-hydroxyethyl, 3-hydroxypropyl, 4-hydroxybutyl, 5-hydroxypentyl, 6-hydroxyhexyl, 7-hydroxyheptyl, 8-hydroxyoctyl, 9-hydroxynonyl, 10-hydroxydecyl, 2-hydroxy-1-methylethyl, 2-hydroxy-1,1-dimethylethyl, 3-hydroxy-1-methylpropyl, 3-hydroxy-2-methylpropyl, 3-hydroxy-1,1-dimethylpropyl, 3-hydroxy-1,2-dimethylpropyl, 3-hydroxy-2,2-dimethylpropyl, 4-hydroxypropyl, 5-hydroxypropyl, 6-hydroxypropyl, 7-hydroxypropyl, 8-hydroxypropyl, 9-hydroxypropyl, 10-hydroxypropyl, 2-hydroxypropyl, 3-hydroxypropyl, 4-hydroxypropyl, 5-hydroxypropyl, 6-hydroxypropyl, 7-hydroxypropyl, 8-hydroxypropyl, 9-hydroxypropyl, 10-hydroxypropyl, 2-hydroxypropyl, 2-hydroxypropyl, 3-hydroxypropyl, 3-hydroxypropyl, 4-hydroxypropyl, 5-hydroxypropyl, 6-hydroxypropyl, 7-hydroxypropyl, 8-hydroxypropyl, 9-hydroxypropyl, 10-hydroxypropyl, 1 ... -1-methylbutyl, 4-hydroxy-2-methylbutyl, 4-hydroxy-3-methylbutyl, and other groups in which the carbon atom to which the hydroxy group is bonded is a primary carbon atom; and 1-hydroxyethyl, 1-hydroxypropyl, 2-hydroxypropyl, 1-hydroxybutyl, 2-hydroxybutyl, 1-hydroxyhexyl, 2-hydroxyhexyl, 1-hydroxyoctyl, 2-hydroxyoctyl, 1-hydroxydecyl, 2-hydroxydecyl, 1-hydroxy-1-methylethyl, 2-hydroxy-2-methylpropyl, and other groups in which the carbon atom to which the hydroxy group is bonded is a secondary or tertiary carbon atom.

[0072] In particular, in consideration of improving heat resistance and resistance to high temperature and high humidity, it is preferable that the carbon atom to which the hydroxyl group is bonded is a primary carbon atom, and among these, a hydroxyalkyl group having 1 to 5 carbon atoms is more preferable, a hydroxyalkyl group having 1 to 3 carbon atoms is even more preferable, a hydroxymethyl group and a 2-hydroxyethyl group are further preferable, and a 2-hydroxyethyl group is most preferable.

[0073] Examples of the (meth)acryloyl-containing group include a (meth)acryloyl group, a (meth)acryloyloxyalkyl group, and a group represented by the following formula (i). Of these, a (meth)acryloyloxyalkyl group having an alkyl group having 1 to 10 carbon atoms and a group represented by the following formula (i) are preferred, and a group represented by the following formula (i) is more preferred.

[0074] [ka] (In the formula, A 1 represents an alkylene group having 1 to 10 carbon atoms; 2 represents a single bond or a group represented by the following formula (j), 3 represents a divalent or trivalent aliphatic hydrocarbon group which may be substituted with a hydroxy group; A 4 represents a hydrogen atom or a methyl group, a represents 1 or 2, and * represents a bond.

[0075] [ka] (* represents a bond.)

[0076] Examples of the alkyl group contained in the (meth)acryloyloxyalkyl group having an alkyl group of 1 to 10 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl groups. In consideration of improving heat resistance and resistance to high temperature and high humidity, among these, those having an alkyl group of 1 to 5 carbon atoms are preferred, those having an alkyl group of 1 to 3 carbon atoms are preferred, and those having an alkyl group of 1 or 2 carbon atoms are more preferred.

[0077] Specific examples of the (meth)acryloyloxyalkyl group include a (meth)acryloyloxymethyl group, a 2-(meth)acryloyloxyethyl group, a 3-(meth)acryloyloxypropyl group, and a 4-(meth)acryloyloxybutyl group.

[0078] In formula (i), A 1 is an alkylene group having 1 to 10 carbon atoms, preferably an alkylene group having 1 to 5 carbon atoms, and more preferably a methylene group or an ethylene group. Examples of the alkylene group having 1 to 10 carbon atoms include methylene, ethylene, propylene, trimethylene, tetramethylene, and pentamethylene groups.

[0079] A 2 represents a single bond or a group represented by formula (j), and a group represented by formula (j) is preferred.

[0080] A 3 A is a divalent or trivalent aliphatic hydrocarbon group which may be substituted with a hydroxy group, and specific examples thereof include an alkylene group having 1 to 5 carbon atoms and groups represented by the following formulas (k-1) to (k-3), with an alkylene group having 1 to 5 carbon atoms being preferred, an alkylene group having 1 to 3 carbon atoms being more preferred, and a methylene group and an ethylene group being even more preferred. 3 As the alkylene group of A 1 Among the alkylene groups exemplified above, alkylene groups having 1 to 5 carbon atoms can be mentioned.

[0081] [ka] (In the formula, * is as defined above.)

[0082] In formula (i), a represents 1 or 2, with 1 being preferred.

[0083] A preferred embodiment of the group represented by formula (i) is one represented by the following formula (i-1).

[0084] [ka] (In the formula, A 1 , A 3 , A 4 and * are as above.)

[0085] More preferred embodiments of the group represented by formula (i) include those represented by the following formulas (i-2) to (i-3).

[0086] [ka] (In the formula, * is as defined above.)

[0087] Examples of the vinyl-containing group include alkenyl groups having 2 to 10 carbon atoms and having a vinyl group at the terminal thereof, etc. Specific examples include ethenyl, 1-propenyl, allyl, isopropenyl, 1-butenyl, 2-butenyl, and 2-pentenyl groups.

[0088] Examples of the epoxy-containing group include an epoxy group, a glycidyl group, a glycidylalkyl group, a glycidyloxy group, etc. Specific examples include a glycidylmethyl group, a 2-glycidylethyl group, a 3-glycidylpropyl group, and a 4-glycidylbutyl group.

[0089] Examples of oxetane-containing groups include oxetan-3-yl, (oxetan-3-yl)methyl, 2-(oxetan-3-yl)ethyl, 3-(oxetan-3-yl)propyl, 4-(oxetan-3-yl)butyl groups, and the like.

[0090] Examples of the carboxy-containing group include a carboxy group and a carboxyalkyl group having 1 to 10 carbon atoms. As the carboxyalkyl group having 1 to 10 carbon atoms, the carbon atom to which the carboxy group is bonded is preferably a primary carbon atom, and specific examples include a carboxymethyl group, a 2-carboxyethyl group, a 3-carboxypropyl group, and a 4-carboxybutyl group.

[0091] Examples of the sulfo-containing group include a sulfo group and a sulfoalkyl group having 1 to 10 carbon atoms. As the sulfoalkyl group having 1 to 10 carbon atoms, the carbon atom to which the sulfo group is bonded is preferably a primary carbon atom, and specific examples include a sulfomethyl group, a 2-sulfoethyl group, a 3-sulfopropyl group, and a 4-sulfobutyl group.

[0092] Examples of the thiol-containing group include a thiol group and a mercaptoalkyl group having 1 to 10 carbon atoms. As the mercaptoalkyl group having 1 to 10 carbon atoms, the carbon atom to which the thiol group is bonded is preferably a primary carbon atom, and specific examples include mercaptomethyl, 2-mercaptoethyl, 3-mercaptopropyl, and 4-mercaptobutyl groups.

[0093] The number of crosslinking groups is not particularly limited and can be any number that can be substituted on the aryl group, but 1 to 4 is preferable, 1 or 2 is more preferable, and 1 is even more preferable.

[0094] Suitable arylamino groups having a bridging group include those represented by formula (15), and in particular, those represented by formula (16) having a bridging group at the para position relative to the amino group are preferred.

[0095] [ka] (In the formula, R 15 represents a bridging group. * represents a bond.

[0096] [ka] (In the formula, R 15 has the same meaning as above. * represents a bond.)

[0097] Specific examples of the arylamino group having a crosslinking group include, but are not limited to, those represented by the following formulas (16-1) to (16-13), in which * represents a bond.

[0098] [ka]

[0099] An arylamino group having a hydroxyalkyl group can be introduced by using a corresponding hydroxyalkyl group-substituted arylamino compound in the production method described below. Specific examples of the hydroxyalkyl group-substituted arylamino compound include (4-aminophenyl)methanol and 2-(4-aminophenyl)ethanol.

[0100] The arylamino group having a (meth)acryloyloxyalkyl group can be introduced by a method using a corresponding (meth)acryloyloxyalkyl group-substituted arylamino compound, or by a method in which an arylamino group having a hydroxyalkyl group is introduced into the polymer (B) and then a (meth)acrylic acid halide or glycidyl (meth)acrylate is allowed to react with the hydroxy group contained in the hydroxyalkyl group.

[0101] The arylamino group having a group represented by formula (i) can be introduced by a method using an arylamino compound having the desired crosslinking group, or by a method in which an arylamino group having a hydroxyalkyl group is introduced into the polymer (B) and then a (meth)acrylic acid ester compound having an isocyanate group represented by the following formula (i') is allowed to react with the hydroxy group contained in the hydroxyalkyl group.

[0102] [ka] (In the formula, A 3 , A 4 and a are as above.)

[0103] Specific examples of the (meth)acryloyloxyalkyl group-substituted arylamino compound include ester compounds obtained by reacting the hydroxy group of the above-mentioned hydroxyalkyl group-substituted arylamino compound with (meth)acrylic acid halide or glycidyl (meth)acrylate. The (meth)acrylic acid halide may include (meth)acrylic acid chloride, (meth)acrylic acid bromide, and (meth)acrylic acid iodide. Specific examples of the (meth)acrylic acid ester compound having an isocyanate group represented by the above formula (i') include 2-isocyanatoethyl acrylate, 2-isocyanatoethyl methacrylate, and 1,1-(bisacryloyloxymethyl)ethyl isocyanate.

[0104] In the present invention, particularly preferred examples of the polymer (B) include those containing repeating units represented by formulas (18) to (21).

[0105] [ka] (Wherein, R, R′, and R 15 has the same meaning as above. R 1 ~R 4 represents a hydrogen atom, a halogen atom, a carboxy group, a sulfo group, an alkyl group having 1 to 10 carbon atoms which may have a branched structure, a halogenated alkyl group having 1 to 10 carbon atoms which may have a branched structure, or an alkoxy group having 1 to 10 carbon atoms which may have a branched structure, except when R and R' are both hydrogen atoms.

[0106] [ka] (In the formula, R 15 has the same meaning as above. R 1 ~R 4 is the same as the above formula (18). 1 ~R 4 Except when all are hydrogen atoms.)

[0107] [ka] (In the formula, R 15 has the same meaning as above.)

[0108] [ka] (In the formula, R 15 has the same meaning as above.)

[0109] The weight average molecular weight of the polymer (B) in the present invention is not particularly limited, but is preferably 500 to 500,000, more preferably 500 to 100,000. From the viewpoint of further improving heat resistance and reducing shrinkage, it is preferably 2,000 or more. From the viewpoint of further increasing solubility and reducing the viscosity of the obtained solution, it is preferably 50,000 or less, more preferably 30,000 or less, even more preferably 15,000 or less, and particularly preferably 10,000 or less. The weight average molecular weight in the present invention is an average molecular weight obtained by gel permeation chromatography (hereinafter, referred to as GPC) analysis in terms of standard polystyrene.

[0110] The polymer (B) (hyperbranched polymer) of the present invention can be produced in accordance with the method disclosed in the above-mentioned WO 2010 / 128661. That is, a trihalogenated triazine compound is reacted with an aryldiamino compound in an organic solvent, and then, for example, reacted with at least one arylamino compound selected from an arylamino compound having a hydroxyalkyl group (hydroxy-containing group), an arylamino compound having an acryloyloxyalkyl group (acryloyl-containing group), and an arylamino compound having a group represented by formula (i) (acryloyl-containing group), thereby obtaining the polymer (B) of the present invention.

[0111] For example, as shown in Scheme 1 below, polymer (B) (20') can be obtained by reacting a triazine compound (22) with an aryldiamino compound (23) in a suitable organic solvent, and then reacting the resulting mixture with at least one arylamino compound (24), which is an end-capping agent, selected from arylamino compounds having a hydroxyalkyl group and arylamino compounds having a group represented by formula (i).

[0112] [ka] (In the formula, X's each independently represent a halogen atom; R a represents a hydroxyalkyl group or a group represented by formula (i).

[0113] In the above reaction, the charging ratio of the aryldiamino compound (23) is arbitrary as long as the target polymer is obtained, but the charging ratio is preferably 0.01 to 10 equivalents, more preferably 1 to 5 equivalents, of the aryldiamino compound (23) relative to 1 equivalent of the triazine compound (22). The aryldiamino compound (23) may be added neat or in the form of a solution dissolved in an organic solvent. In view of ease of operation and control of the reaction, the latter method is preferred. The reaction temperature may be appropriately set within the range from the melting point to the boiling point of the solvent used, and is preferably about -30 to 150°C, more preferably -10 to 100°C.

[0114] Another embodiment is the method shown in Scheme 2 below. In this method, polymer (B) (20') can be obtained by reacting a triazine compound (22) with an aryldiamino compound (23) in a suitable organic solvent, followed by reacting with an arylamino compound (24') having a hydroxyalkyl group, which is an end-capping agent, to obtain polymer (B) (20'') (first step), and then reacting a (meth)acrylic acid ester compound having an isocyanate group represented by formula (i') with the hydroxy group of the hydroxyalkyl group contained in polymer (B) (20'') (second step). When the polymer (B) (20'') is the target product, the reaction may be completed in the first stage without carrying out the second stage reaction.

[0115] [ka] (In the formula, R a1 represents a hydroxyalkyl group; X, A 3 , A 4 , R a and a have the same meaning as above.)

[0116] In the above reaction, the charging ratio and addition method of the aryldiamino compound (23) in the first step, and the reaction temperature in the reaction until the polymer (B) (20″) is obtained can be the same as those explained in Scheme 1. In the second step, the ratio of the (meth)acrylic acid ester compound having an isocyanate group represented by formula (i') to the polymer (B) (20'') can be arbitrarily set according to the ratio of the hydroxyalkyl group to the group represented by formula (i), and is preferably 0.1 to 10 equivalents, more preferably 0.5 to 5 equivalents, even more preferably 0.7 to 3 equivalents, and even more preferably 0.9 to 1.5 equivalents relative to 1 equivalent of the arylamino compound having a hydroxyalkyl group used. For example, when all of the hydroxyalkyl groups contained in the polymer (B) (20'') are groups represented by formula (i), the ratio of the (meth)acrylic acid ester compound to 1 equivalent of the arylamino compound having a hydroxyalkyl group used is preferably 1.0 to 10 equivalents, more preferably 1.0 to 5 equivalents, even more preferably 1.0 to 3 equivalents, and even more preferably 1.0 to 1.5 equivalents. The reaction temperature in this reaction is the same as the reaction temperature in the reaction to obtain the polymer (B) (20''); however, in consideration of preventing polymerization of the (meth)acryloyl group during the reaction, the reaction temperature is preferably 30 to 80°C, more preferably 40 to 70°C, and even more preferably 50 to 60°C.

[0117] As the organic solvent, various solvents commonly used in this type of reaction can be used, for example, tetrahydrofuran (THF), 1,4-dioxane, dimethyl sulfoxide; amide solvents such as N,N-dimethylformamide, N-methyl-2-pyrrolidone, tetramethylurea, hexamethylphosphoramide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N,N-dimethylethyleneurea, N,N,N',N'-tetramethylmalonic acid amide, N-methyl-ε-caprolactam, N-acetylpyrrolidine, N,N-diethylacetamide, N-ethyl-2-pyrrolidone, N,N-dimethylpropionic acid amide, N,N-dimethylisobutylamide, N-methylformamide, and N,N'-dimethylpropyleneurea, and mixed solvents thereof. Among these, N,N-dimethylformamide, dimethylsulfoxide, N-methyl-2-pyrrolidone, N,N-dimethylacetamide, and mixtures thereof are preferred, and N,N-dimethylacetamide and N-methyl-2-pyrrolidone are particularly suitable.

[0118] In the first step reaction of the above scheme 1, various bases that are commonly used may be added during or after the polymerization. Specific examples of the base include potassium carbonate, potassium hydroxide, sodium carbonate, sodium hydroxide, sodium bicarbonate, sodium ethoxide, sodium acetate, lithium carbonate, lithium hydroxide, lithium oxide, potassium acetate, magnesium oxide, calcium oxide, barium hydroxide, trilithium phosphate, trisodium phosphate, tripotassium phosphate, cesium fluoride, aluminum oxide, ammonia, n-propylamine, trimethylamine, triethylamine, diisopropylamine, diisopropylethylamine, N-methylpiperidine, 2,2,6,6-tetramethyl-N-methylpiperidine, pyridine, 4-dimethylaminopyridine, N-methylmorpholine, and the like. The amount of the base to be added is preferably 1 to 100 equivalents relative to 1 equivalent of the triazine compound (22), and more preferably 1 to 10 equivalents. These bases may be used in the form of an aqueous solution. It is preferred that no raw material components remain in the resulting polymer, but some raw materials may remain as long as the effects of the present invention are not impaired. After completion of the reaction, the product can be easily purified by a method such as reprecipitation.

[0119] As a method for blocking the terminals using an arylamino compound having a crosslinking group, a known method may be adopted. In this case, the amount of the end-capping agent used is preferably about 0.05 to 10 equivalents, more preferably 0.1 to 5 equivalents, and even more preferably 0.5 to 2 equivalents, per equivalent of halogen atoms derived from the excess triazine compound not used in the polymerization reaction. The reaction solvent and reaction temperature may be the same as those described in the first step of the above scheme 1, and the end-capping agent may be charged simultaneously with the aryldiamino compound (23). In addition, an unsubstituted arylamino compound having no crosslinking group may be used, and the terminals may be blocked with two or more groups. The aryl groups of this unsubstituted arylamino compound may be the same as those mentioned above.

[0120] Specific examples of the unsubstituted arylamino group include, but are not limited to, those represented by the following formula (26).

[0121] [ka]

[0122] The unsubstituted arylamino group can be introduced by using a corresponding unsubstituted arylamino compound in the production method described below. Specific examples of unsubstituted arylamino compounds include aniline.

[0123] In addition, when introducing an unsubstituted arylamino group, the ratio of the arylamino compound having a crosslinking group and the unsubstituted arylamino compound is preferably 0.1 to 1.0 mol, more preferably 0.1 to 0.5 mol, and even more preferably 0.1 to 0.3 mol of the unsubstituted arylamino compound per 1 mol of the arylamino compound having a crosslinking group, from the viewpoint of achieving a good balance between solubility in organic solvents and yellowing resistance.

[0124] (Liquid crystal alignment agent) The liquid crystal aligning agent is used to prepare a liquid crystal alignment film, and takes the form of a coating liquid from the viewpoint of forming a uniform thin film. The liquid crystal aligning agent of the present invention is also preferably a coating liquid containing the above-mentioned polymer component and an organic solvent. In this case, the concentration of the polymer component in the liquid crystal aligning agent can be appropriately changed depending on the thickness of the coating film to be formed. From the viewpoint of forming a uniform and defect-free coating film, it is preferably 0.5% by mass or more, and from the viewpoint of storage stability of the solution, it is preferably 15% by mass or less. A particularly preferable concentration of the polymer component is 1 to 10% by mass.

[0125] From the viewpoint of enhancing the liquid crystal alignment property, the content ratio of the (A) component and the (B) component contained in the liquid crystal aligning agent of the present invention may be 10 / 90 to 90 / 10, 20 / 80 to 90 / 10, or 20 / 80 to 80 / 20 in terms of the mass ratio of [(A) component] / [(B) component].

[0126] The liquid crystal alignment agent used for producing the liquid crystal alignment film may contain polymer (A) or polymer (B) as a polymer component, or other polymers may be mixed. In this case, the content of the other polymers is 0.5% by mass to 15% by mass, preferably 1% by mass to 10% by mass, of the total amount of the polymer components. Examples of other polymers include acrylic polymers, methacrylic polymers, polystyrene, polyamide, and polysiloxane.

[0127] The solvent contained in the liquid crystal alignment agent is not particularly limited as long as it can dissolve the polymer (A) and the polymer (B). For example, lactone solvents such as γ-valerolactone and γ-butyrolactone; γ-butyrolactam, N-(n-propyl)-2-pyrrolidone, N-isopropyl-2-pyrrolidone, N-(n-butyl)-2-pyrrolidone, N-(t-butyl)-2-pyrrolidone, N-(n-pentyl)-2-pyrrolidone, N-methoxypropyl-2-pyrrolidone, N-ethoxyethyl-2-pyrrolidone, N-methoxybutyl ... Lactam solvents such as pyrrolidone, N-cyclohexyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-methyl-2-pyrrolidone; amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethyllactamide, 3-butoxy-N,N-dimethylpropanamide, 3-methoxy-N,N-dimethylpropanamide, 3-hexyloxy-N,N-dimethylpropanamide, isopropoxy-N-isopropyl-propionamide, n-butoxy-N-isopropyl-propionamide;4-Hydroxy-4-methyl-2-pentanone, 2,6-dimethyl-4-heptanone (diisobutyl ketone), methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isoamyl lactate, n-butyl acetate, propylene glycol monoethyl ether acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-butyl ether (butyl cellosolve), ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol Monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monobutyl ether, propylene glycol diacetate, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, isoamyl propionate, isoamyl isobutyrate, diisopropyl ether, diisopentyl ether; carbonate solvents such as ethylene carbonate and propylene carbonate, 1-hexanol, cyclohexanol, 1,2-ethanediol, 2,6-dimethyl-4-heptanol (diisobutyl carbinol), propylene carbonate, etc. These can be used alone or in combination of two or more.;

[0128] Preferred solvent combinations include N-methyl-2-pyrrolidone and ethylene glycol monobutyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone and ethylene glycol monobutyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone and propylene glycol monobutyl ether, N-ethyl-2-pyrrolidone and propylene glycol monobutyl ether, and N-methyl-2-pyrrolidone, γ-butyrolactone and 4-hydroxy-4-methyl-2-pentanone. and diethylene glycol diethyl ether, N-ethyl-2-pyrrolidone and N-methyl-2-pyrrolidone and 4-hydroxy-4-methyl-2-pentanone, N-methyl-2-pyrrolidone and 4-hydroxy-4-methyl-2-pentanone and diisobutyl ketone, N-methyl-2-pyrrolidone and 4-hydroxy-4-methyl-2-pentanone and dipropylene glycol monomethyl ether, N-methyl-2-pyrrolidone and 4-hydroxy-4-methyl-2-pentanone and propylene glycol monobutyl ether, N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone, and propylene glycol diacetate, gamma-butyrolactone, 4-hydroxy-4-methyl-2-pentanone, and diisobutyl ketone, gamma-butyrolactone, 4-hydroxy-4-methyl-2-pentanone, and propylene glycol diacetate, N-methyl-2-pyrrolidone, gamma-butyrolactone, propylene glycol monobutyl ether, and diisobutyl ketone, N-methyl-2 N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether, and diisopropyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether, and diisobutyl carbinol, N-methyl-2-pyrrolidone, γ-butyrolactone, and dipropylene glycol dimethyl ether, N-methyl-2-pyrrolidone, propylene glycol monobutyl ether, and dipropylene glycol dimethyl ether, etc. The type and content of such a solvent are appropriately selected depending on the coating device, coating conditions, coating environment, etc. of the liquid crystal alignment agent.

[0129] <Other ingredients> The liquid crystal aligning agent of the present invention may contain other components other than those described above, such as a crosslinkable compound, a functional silane compound, a surfactant, a compound having a photopolymerizable group, etc., if necessary.

[0130] The crosslinkable compound can be used for the purpose of increasing the strength of the liquid crystal alignment film. Examples of such crosslinkable compounds include compounds having an isocyanate group or a cyclocarbonate group, or compounds having at least one group selected from the group consisting of lower alkoxyalkyl groups, as described in paragraphs

[0109] to

[0113] of International Publication WO2016 / 047771, as well as compounds having a blocked isocyanate group.

[0131] The blocked isocyanate compound is commercially available, and for example, Coronate AP Stable M, Coronate 2503, 2515, 2507, 2513, 2555, Millionate MS-50 (all manufactured by Tosoh Corporation), Takenate B-830, B-815N, B-820NSU, B-842N, B-846N, B-870N, B-874N, B-882N (all manufactured by Mitsui Chemicals, Inc.) and the like can be preferably used.

[0132] Specific examples of preferred crosslinkable compounds include compounds represented by the following formulas (CL-1) to (CL-11).

[0133] [ka]

[0134] The above are examples of the crosslinkable compound, and the present invention is not limited to these. The crosslinkable compound used in the liquid crystal aligning agent of the present invention may be one type or a combination of two or more types.

[0135] The content of the other crosslinkable compounds in the liquid crystal aligning agent of the present invention is 0.1 to 150 parts by mass, or 0.1 to 100 parts by mass, or 1 to 50 parts by mass, based on 100 parts by mass of all polymer components.

[0136] The functional silane compound can be used for the purpose of improving the adhesion between the liquid crystal alignment film and the base substrate. Specific examples include the silane compounds described in paragraph

[0019] of International Publication No. 2014 / 119682. The content of the functional silane compound is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 20 parts by mass, based on 100 parts by mass of all polymer components.

[0137] The surfactant can be used for the purpose of improving the uniformity of the thickness and the surface smoothness of the liquid crystal alignment film. Examples of the surfactant include fluorine-based surfactants, silicone-based surfactants, and nonionic surfactants. Specific examples of these surfactants include those described in paragraph

[0117] of International Publication WO2016 / 047771. The amount of the surfactant used is preferably 0.01 to 2 parts by mass, more preferably 0.01 to 1 part by mass, based on 100 parts by mass of all polymer components contained in the liquid crystal alignment agent.

[0138] Examples of compounds having a photopolymerizable group include compounds having one or more polymerizable unsaturated groups, such as an acrylate group or a methacrylate group, in the molecule, such as compounds represented by the following formulas (M-1) to (M-7).

[0139] [ka]

[0140] Furthermore, the liquid crystal aligning agent of the present invention can be added with a nitrogen-containing heterocyclic amine compound represented by formula [M1] to formula [M156], more preferably 3-picolylamine and 4-picolylamine, as described in paragraphs

[0194] to

[0200] of International Publication WO2011 / 132751 (published on October 27, 2011), as a compound that promotes charge transfer in the liquid crystal alignment film and promotes charge escape from the element. This amine compound may be added directly to the liquid crystal aligning agent, but it is preferable to add it after making it into a solution with a concentration of 0.1 to 10% by mass, preferably 1 to 7% by mass. This solvent is not particularly limited as long as it dissolves the polymer component.

[0141] An imidization promoter or the like may be added to the liquid crystal aligning agent of the present invention for the purpose of efficiently promoting imidization by heating when baking the coating film.

[0142] The solid content concentration in the liquid crystal alignment agent (the ratio of the total mass of the components other than the solvent of the liquid crystal alignment agent to the total mass of the liquid crystal alignment agent) is appropriately selected taking into consideration viscosity, volatility, etc., but is preferably in the range of 0.5 to 15 mass%, more preferably 1 to 10 mass%. The particularly preferred range of solid content varies depending on the method used to apply the liquid crystal alignment agent to the substrate. For example, in the case of the spin coating method, the solid content is particularly preferably in the range of 1.5 to 4.5 mass%. In the case of the printing method, the solid content is particularly preferably in the range of 3 to 9 mass%, thereby making the solution viscosity in the range of 12 to 50 mPa·s. In the case of the inkjet method, the solid content is particularly preferably in the range of 1 to 5 mass%, thereby making the solution viscosity in the range of 3 to 15 mPa·s.

[0143] (Liquid crystal alignment film / Liquid crystal display element) The liquid crystal alignment film of the present invention is obtained from the above liquid crystal alignment agent. The liquid crystal alignment film of the present invention can be used for horizontal alignment type or vertical alignment type liquid crystal alignment film, and is particularly suitable for vertical alignment type liquid crystal display elements such as VA type liquid crystal display elements or PSA type liquid crystal display elements. The liquid crystal display element of the present invention is provided with the above liquid crystal alignment film. The liquid crystal display element of the present invention can be manufactured, for example, by a method including the following steps (1) to (3) or steps (1) to (4). The liquid crystal alignment film of the present invention can be preferably used for a liquid crystal display element obtained by a manufacturing method of a liquid crystal display element, which comprises applying a coating film onto a pair of substrates having a conductive film to form a coating film, arranging the coating films so as to face each other via a layer of liquid crystal molecules to form a liquid crystal cell, and irradiating the liquid crystal cell with light while applying a voltage between the conductive films of the pair of substrates. More specifically, it is a PSA type liquid crystal display element or a liquid crystal display element for SC-PVA mode, which will be described later.

[0144] (1) A process of applying a liquid crystal alignment agent onto a substrate The liquid crystal alignment agent of the present invention is applied to one side of a substrate on which a patterned transparent conductive film is provided by an appropriate application method such as a roll coater method, a spin coat method, a printing method, an inkjet method, etc. The substrate is not particularly limited as long as it is a highly transparent substrate, and plastic substrates such as acrylic substrates and polycarbonate substrates can be used in addition to glass substrates and silicon nitride substrates. In addition, in a reflective liquid crystal display element, an opaque material such as a silicon wafer can be used for only one substrate, and in this case, a light-reflecting material such as aluminum can be used for the electrode.

[0145] (2) The coating is baked After applying the liquid crystal alignment agent, it is preferable to first perform pre-heating (pre-baking) for the purpose of preventing dripping of the applied alignment agent. The pre-baking temperature is preferably 30 to 200° C., more preferably 40 to 150° C., and particularly preferably 40 to 100° C. The pre-baking time is preferably 0.25 to 10 minutes, more preferably 0.5 to 5 minutes. Then, in order to completely remove the solvent, it is preferable to perform a further heating (post-baking) step. The post-bake temperature is preferably 80 to 300° C., more preferably 120 to 250° C. The post-bake time is preferably 5 to 200 minutes, more preferably 10 to 100 minutes. The film thus formed has a thickness of preferably 5 to 300 nm, more preferably 10 to 200 nm.

[0146] The coating film formed in the above step (1) can be used as a liquid crystal alignment film as it is, but the coating film may be subjected to an alignment ability imparting treatment, such as a rubbing treatment in which the coating film is rubbed in a certain direction with a roll wrapped with a cloth made of fibers such as nylon, rayon, or cotton, or a photoalignment treatment in which the coating film is irradiated with polarized or non-polarized radiation.

[0147] In the photo-alignment treatment, the radiation to be irradiated to the coating film may be, for example, ultraviolet light and visible light containing light with a wavelength of 150 to 800 nm. When the radiation is polarized, it may be linearly polarized or partially polarized. When the radiation used is linearly polarized or partially polarized, the radiation may be applied from a direction perpendicular to the substrate surface, from an oblique direction, or a combination of these. When non-polarized radiation is applied, the radiation is applied in an oblique direction.

[0148] (3) Forming the liquid crystal layer (3-1) VA type LCD element Two substrates on which a liquid crystal alignment film is formed are prepared as described above, and liquid crystal is placed between the two substrates arranged opposite each other. Specifically, the following two methods can be mentioned. The first method is a conventionally known method. First, the two substrates are arranged opposite each other with a gap (cell gap) between them so that the liquid crystal alignment films face each other. Next, the peripheries of the two substrates are bonded together using a sealant, and a liquid crystal composition is injected and filled into the substrate surfaces and the cell gap partitioned by the sealant to come into contact with the film surface, and then the injection hole is sealed.

[0149] The second method is a method called ODF (One Drop Fill) method. For example, a UV-curable sealant is applied to a predetermined location on one of the two substrates on which a liquid crystal alignment film is formed, and a liquid crystal composition is dropped at a predetermined number of locations on the liquid crystal alignment film surface. Thereafter, the other substrate is bonded so that the liquid crystal alignment film faces the other substrate, and the liquid crystal composition is spread over the entire surface of the substrate and contacted with the film surface. Next, the entire surface of the substrate is irradiated with UV light to cure the sealant. In either method, it is preferable to further remove the flow alignment during liquid crystal filling by heating to a temperature at which the liquid crystal composition used has an isotropic phase and then slowly cooling to room temperature.

[0150] (3-2) Manufacturing of PSA type liquid crystal display elements The procedure is the same as that of (3-1) above, except that a liquid crystal composition containing a polymerizable compound is injected or dropped. Examples of the polymerizable compound include the polymerizable compounds represented by the above formulas (M-1) to (M-7).

[0151] (3-3) When a coating film is formed on a substrate using a liquid crystal alignment agent containing a compound having a polymerizable group (LCD element for SC-PVA mode) A method of manufacturing a liquid crystal display element may be adopted in which, after the same procedure as in the above (3-1), a step of irradiating ultraviolet light described later is carried out. According to this method, a liquid crystal display element having excellent response speed can be obtained with a small amount of light irradiation, as in the case of manufacturing the above PSA type liquid crystal display element. The compound having a polymerizable group may be a compound having one or more polymerizable unsaturated groups in the molecule, such as acrylate groups or methacrylate groups, as represented by the above formulas (M-1) to (M-7), and the content thereof is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, relative to 100 parts by mass of all polymer components. The polymerizable group may be contained in a polymer used for a liquid crystal alignment agent, and an example of such a polymer is a polymer obtained by using a diamine component containing a diamine having the above photopolymerizable group at its terminal in a reaction.

[0152] (4) UV irradiation process The liquid crystal cell is irradiated with light while a voltage is applied between the conductive films of the pair of substrates obtained in (3-2) or (3-3) above. The voltage applied here can be, for example, 5 to 50 V DC or AC. The light to be irradiated can be, for example, ultraviolet light and visible light containing light with a wavelength of 150 to 800 nm, but ultraviolet light containing light with a wavelength of 300 to 400 nm is preferred. The light source for the irradiation light can be, for example, a low-pressure mercury lamp, a high-pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, or the like. The light irradiation dose is preferably 1,000 to 200,000 J / m 2 and more preferably 1,000 to 100,000 J / m 2 It is.

[0153] A liquid crystal display element can be obtained by attaching a polarizing plate to the outer surface of the liquid crystal cell. Examples of the polarizing plate to be attached to the outer surface of the liquid crystal cell include a polarizing film called an "H film" made by absorbing iodine while stretching and aligning polyvinyl alcohol, sandwiched between cellulose acetate protective films, and a polarizing plate made of the H film itself.

[0154] The liquid crystal display element of the present invention can be effectively applied to various devices, and can be used in various display devices such as watches, portable games, word processors, notebook computers, car navigation systems, camcorders, PDAs, digital cameras, mobile phones, smartphones, various monitors, liquid crystal televisions, and information displays. EXAMPLES

[0155] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. The meanings of the abbreviations of the compounds used in the examples are as follows.

[0156] (Specific diamine) DA-1 to DA-5: Compounds represented by the following formulas [DA-1] to [DA-5], respectively.

[0157] [ka]

[0158] (Tetracarboxylic acid component) D1: 1,2,3,4-cyclobutanetetracarboxylic dianhydride D2: Bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic dianhydride D3: Benzene-1,2,4,5-tetracarboxylic anhydride

[0159] [ka]

[0160] (Additive ingredients) A-1: A compound represented by the following formula [A-1]

[0161] [ka]

[0162] (Triazine ring-containing polymer) T-1: A compound having a repeating unit structure represented by the following formula [T-1] T-2: A compound having a repeating unit structure represented by the following formula [T-2]

[0163] [ka]

[0164] (solvent) NMP: N-methyl-2-pyrrolidone BCS: Ethylene glycol monobutyl ether THF: tetrahydrofuran DMAc: N,N-dimethylacetamide

[0165] (Measurement of molecular weight of polymer (A)) The molecular weight of the polymer (A) in the synthesis examples was measured as follows using a room temperature gel permeation chromatography (GPC) apparatus (SSC-7200) manufactured by Senshu Scientific Co., Ltd. and columns (KD-803, KD-805) manufactured by Shodex Co., Ltd. Column temperature: 50℃ Eluent: N,N-dimethylformamide (additives: lithium bromide monohydrate (LiBr·H2O) 30mmol / L, phosphoric acid·anhydrous crystal (o-phosphoric acid) 30mmol / L, tetrahydrofuran (THF) 10ml / L) Flow rate: 1.0ml / min Standard samples for creating calibration curves: TSK standard polyethylene oxide (molecular weights: approximately 900,000, 150,000, 100,000, and 30,000) manufactured by Tosoh Corporation, and polyethylene glycol (molecular weights: approximately 12,000, 4,000, and 1,000) manufactured by Polymer Laboratory.

[0166] (Synthesis of Polymer (A)) <Synthesis Example 1> Tetracarboxylic dianhydride D2 (15.01 g), diamine components DA-1 (15.65 g, molar ratio to all diamine components 0.3), DA-2 (8.33 g, molar ratio to all diamine components 0.35), DA-3 (5.95 g, molar ratio to all diamine components 0.2), and DA-4 (5.81 g, molar ratio to all diamine components 0.15) were mixed in NMP solvent (203.00 g) and reacted at 60 ° C for 3 hours, and then tetracarboxylic dianhydride D1 (11.30 g) and NMP (44.24 g) were added and mixed, and reacted at 40 ° C for 12 hours to obtain polyamic acid solution (A). The number average molecular weight of this polyamic acid polymer was 9,600 and the weight average molecular weight was 22,900.

[0167] <Synthesis Example 2> Tetracarboxylic dianhydride D1 (14.43g), diamine components DA-2 (9.12g, molar ratio 0.4 to the total diamine components), DA-3 (8.36g, molar ratio 0.3 to the total diamine components), and DA-5 (14.16g, molar ratio 0.3 to the total diamine components) were mixed in NMP solvent (221.94g) and reacted at room temperature for 1 hour, then tetracarboxylic dianhydride D3 (7.52g) and NMP (81.79g) were added and mixed, and reacted at room temperature for 12 hours to obtain polyamic acid solution (B). The number average molecular weight of this polyamic acid polymer was 10,800 and the weight average molecular weight was 32,500.

[0168] (Synthesis of Polymer (B)) <Preparation of triazine ring-containing polymer solution> <Synthesis Example 3>

[0169] [ka]

[0170] In a 1,000mL four-neck flask, 1,3-phenylenediamine [2] (42.22g, 0.390mol, Amino-Chem) and DMAc (672.62g, Kanto Chemical) were added, and the mixture was replaced with nitrogen. The mixture was then stirred to dissolve 1,3-phenylenediamine [2] in DMAc. The mixture was then cooled to -10°C in an ethanol-dry ice bath, and 2,4,6-trichloro-1,3,5-triazine [1] (60.00g, 0.325mol, Tokyo Chemical Industry Co., Ltd.) was added while making sure that the internal temperature did not exceed 0°C. After stirring for 30 minutes, the reaction solution was heated to 85±5°C in an oil bath set to 90-100°C. After stirring for 1 hour at an internal temperature of 85°C, aniline [6] (18.18g, 0.195mol, Tokyo Chemical Industry Co., Ltd.) and 2-(4-aminophenyl)ethanol [3] (26.78g, 0.195mol, Oakwood Co., Ltd.) were dissolved in DMAc (42.93g) in advance and added dropwise, followed by stirring for 3 hours. Then, 2-aminoethanol (59.62g, Tokyo Chemical Industry Co., Ltd.) was added dropwise, the temperature was lowered to room temperature, and stirring was continued for 30 minutes, after which the stirring was stopped. THF (369g), ammonium acetate (415g) and ion-exchanged water (415g) were added to the reaction solution, followed by stirring for 30 minutes. After stirring was stopped, the solution was transferred to a separatory funnel, separated into an organic layer and an aqueous layer, and the organic layer was collected. The collected organic layer was added dropwise to a mixture of methanol (461g) and ion-exchanged water (1,845g) to cause reprecipitation. The resulting precipitate was filtered and dried at 120°C for 8 hours using a vacuum dryer to obtain 89.3 g of the target polymer compound

[10] (hereinafter referred to as T-1). 1 The results of H-NMR spectrum measurement are shown in FIG. The weight average molecular weight Mw of compound T-1 measured by GPC in terms of polystyrene was 23,350, and the polydispersity Mw / Mn was 6.5. The triazine ring-containing polymer (T-1) (5.00 g) and NMP solvent (20.0 g) were stirred at 40° C. for 12 hours to dissolve the polymer, thereby obtaining a triazine ring-containing polymer solution (C).

[0171] <Synthesis Example 4>

[0172] [ka]

[0173] In a 1,000 mL four-neck flask, 1,3-phenylenediamine [2] (45.15 g, 0.418 mol) and DMAc (685.16 g) were added, and after replacing with nitrogen, 1,3-phenylenediamine [2] was dissolved in DMAc by stirring. Then, it was cooled to -10 ° C in an ethanol-dry ice bath, and 2,4,6-trichloro-1,3,5-triazine [1] (70.00 g, 0.380 mol) was added while making sure that the internal temperature did not exceed 0 ° C. After stirring for 30 minutes, the reaction vessel was transferred to an oil bath set at 90-110 ° C, and the reaction solution was heated until the internal temperature reached 85 ± 5 ° C. After stirring for 1 hour, 3-aminophenol [3] (49.71 g, 0.456 mol, Tokyo Chemical Industry Co., Ltd.) dissolved in DMAc (120.91 g) was added dropwise and stirred for 3 hours. Then, 2-aminoethanol (69.56 g, Tokyo Chemical Industry Co., Ltd.) was added dropwise, and the mixture was stirred for 30 minutes, after which the stirring was stopped. To the reaction solution, THF (416 g), ammonium acetate (468.2 g), and ion-exchanged water (468.2 g) were added, and the mixture was stirred for 30 minutes. After the stirring was stopped, the solution was transferred to a separatory funnel, separated into an organic layer and an aqueous layer, and the organic layer was collected. The collected organic layer was added dropwise to a mixture of methanol (1,040 g) and ion-exchanged water (1,561 g) to cause reprecipitation. The obtained precipitate was filtered and dried at 120°C for 8 hours using a vacuum dryer, and 95.1 g of the target polymer compound [5] (hereinafter referred to as T-2) was obtained. The weight average molecular weight Mw of compound T-2 measured by GPC in terms of polystyrene was 12,384, and the polydispersity Mw / Mn was 3.3. 1 The results of H-NMR spectrum measurement are shown in FIG. The triazine ring-containing polymer (T-2) (5.00 g) and NMP solvent (20.0 g) were dissolved by stirring at 40° C. for 12 hours to obtain a triazine ring-containing polymer solution (D).

[0174] <Preparation of Liquid Crystal Alignment Agent> <Example 1> NMP (3.88 g) and BCS (10.0 g) were added to the polyamic acid solution (A) (1.8 g) obtained in Synthesis Example 1, the triazine ring-containing polymer solution (C) (4.2 g) obtained in Synthesis Example 3, and the additive [A-1] (0.12 g), and the mixture was stirred for 5 hours to obtain a liquid crystal alignment agent [1] of Example 1. No abnormalities such as turbidity or precipitation were observed in this liquid crystal alignment agent, and it was confirmed that the resin components were uniformly dissolved.

[0175] <Examples 2 to 6, Comparative Examples 1 and 2> In Example 1, the liquid crystal alignment agents [2] to [6] of Examples 2 to 6 and the liquid crystal alignment agents [7] and [8] of Comparative Examples 1 and 2 were obtained in the same manner as in Example 1, except that the blending amounts were changed to those shown in Table 1 below. No abnormalities such as turbidity or precipitation were observed in these liquid crystal alignment agents, and it was confirmed that the resin components were uniformly dissolved.

[0176] [Table 1]

[0177] (Refractive index measurement) The liquid crystal alignment agents obtained in Examples 1 to 6 and Comparative Examples 1 and 2 were spin-coated onto a silicon substrate, baked on a hot plate at 70°C for 90 seconds, and then baked in an infrared heating furnace at 230°C for 20 minutes to prepare a liquid crystal alignment agent-coated Si substrate with a thickness of 100 nm.

[0178] Next, the refractive index was measured using an M-2000 manufactured by J.A. Woollam Japan, and the refractive index at 550 nm was compared. The measurement results of the refractive index in Examples 1 to 6 and Comparative Examples 1 and 2 are shown in Table 2 below.

[0179] (Transmittance measurement) The liquid crystal alignment agents of Examples 1 to 6 and Comparative Examples 1 and 2 obtained above were spin-coated onto a quartz substrate, baked on a hot plate at 70°C for 90 seconds, and then baked in an infrared heating furnace at 230°C for 20 minutes to prepare a quartz substrate coated with a liquid crystal alignment agent having a film thickness of 100 nm.

[0180] Next, the transmittance in the visible light region (380 nm to 780 nm) was measured using a quartz substrate before applying the liquid crystal alignment agent as a reference using a UV-2600 manufactured by Shimadzu Corporation. After that, the average transmittance Y in the XYZ color system defined by the CIE was calculated and used as the average luminous transmittance. The measurement results of the transmittance in Examples 1 to 6 and Comparative Examples 1 and 2 are shown in Table 2 below.

[0181] [Table 2]

[0182] As shown in Table 2, it was confirmed that the refractive index was 1.64 or less in Comparative Examples 1 and 2, whereas the refractive index was 1.66 or more, which is high, in Examples 1 to 6. It was also confirmed that Examples 1 to 6 exhibited a high average luminous transmittance of 95% or more while maintaining a high refractive index.

[0183] (Evaluation of voltage holding ratio) <Preparation of liquid crystal cells for evaluating voltage holding ratio> The liquid crystal alignment agents of Examples 1 to 6 and Comparative Examples 1 and 2 obtained above were spin-coated onto the ITO surface of a glass substrate (length 30 mm, width 40 mm, thickness 0.7 mm) with ITO that had been washed with pure water and IPA (isopropyl alcohol), baked on a hot plate at 70°C for 90 seconds, and then baked in an infrared heating furnace at 230°C for 20 minutes to prepare a polyimide-coated substrate with a film thickness of 100 nm.

[0184] Two substrates coated with a liquid crystal alignment agent were prepared by the above method, and 4 μm bead spacers were sprayed on the liquid crystal alignment film surface of one substrate, and then a thermosetting sealant (XN-1500T manufactured by Kyoritsu Chemical Industry Co., Ltd.) was printed on top of the bead spacers. Next, the other substrate was attached to the previous substrate with the side on which the liquid crystal alignment film was formed facing inward, and the sealant was cured to prepare an empty cell. PSA polymerizable compound-containing liquid crystal MLC-3023 (manufactured by Merck) was injected into this empty cell by the reduced pressure injection method to prepare a liquid crystal cell. The voltage retention rate of this liquid crystal cell was measured.

[0185] Next, with a DC voltage of 15 V applied to the liquid crystal cell, UV light was applied from the outside of the liquid crystal cell at 10 J / cm through a 325 nm cut filter. 2 The UV illuminance was measured using a UV-MO3A manufactured by ORC.

[0186] Thereafter, in order to inactivate the unreacted polymerizable compound remaining in the liquid crystal cell, the cell was irradiated with UV (UV lamp: FLR40SUV32 / A-1) for 30 minutes without applying voltage using a UV-FL irradiation device manufactured by Toshiba Lighting & Technology Corp. (referred to as secondary PSA treatment). Then, the voltage retention rate was measured.

[0187] <Measurement of voltage holding ratio> Using the liquid crystal cell prepared above, a voltage of 1V was applied for 60μs in a hot air circulating oven at 60℃, and the voltage was measured 1667msec later, and the voltage retention rate (VHR) was calculated to determine how long the voltage was retained. A VHR-1 manufactured by Toyo Corporation was used to measure the voltage retention rate. The measurement results of the voltage holding ratio in Examples 1 to 6 and Comparative Examples 1 and 2 are shown in Table 3 below.

[0188] [Table 3]

[0189] As shown in Table 3, in Examples 1 to 6, the VHR after the second PSA treatment was all around 90%, which was confirmed to be equivalent to that of the comparative example. It was confirmed that the liquid crystal elements of Examples 1 to 6 exhibited a voltage holding ratio that was good for practical use.

[0190] (Evaluation of pretilt angle) <Preparation of liquid crystal cell for evaluating pretilt angle> The liquid crystal alignment agents of Examples 1 to 6 and Comparative Examples 1 and 2 obtained above were spin-coated on the ITO surfaces of an ITO electrode substrate (length 35 mm, width 30 mm, thickness 0.5 mm) having an ITO electrode pattern with a pixel size of 200 μm × 600 μm and a line / space of 3 μm each, which had been washed with pure water and IPA (isopropyl alcohol), and a glass substrate (length 35 mm, width 30 mm, thickness 0.7 mm) with an ITO electrode patterned with a photospacer having a height of 3.2 μm, respectively, and baked on a hot plate at 70°C for 90 seconds, and then baked in an infrared heating furnace at 230°C for 20 minutes or 60 minutes to prepare polyimide-coated substrates with a film thickness of 100 nm. The ITO electrode substrate on which this ITO electrode pattern is formed is divided into four areas in a cross-checkered pattern, so that each of the four areas can be driven separately.

[0191] Two polyimide-coated substrates were prepared using the above method, and a thermosetting sealant (XN-1500T manufactured by Kyoritsu Chemical Industry Co., Ltd.) was printed on them. Next, the other substrate was attached to the previous substrate with the side on which the liquid crystal alignment film was formed facing inward, and the sealant was cured to prepare an empty cell. PSA polymerizable compound-containing liquid crystal MLC-3023 (manufactured by Merck) was injected into this empty cell by the reduced pressure injection method to prepare a liquid crystal cell. The voltage retention rate of this liquid crystal cell was measured.

[0192] Next, with a DC voltage of 15 V applied to the liquid crystal cell, UV light was applied from the outside of the liquid crystal cell at 10 J / cm through a 325 nm cut filter. 2The UV illuminance was measured using a UV-MO3A manufactured by ORC.

[0193] Thereafter, in order to inactivate the unreacted polymerizable compound remaining in the liquid crystal cell, the cell was irradiated with UV (UV lamp: FLR40SUV32 / A-1) for 30 minutes without applying voltage using a UV-FL irradiation device manufactured by Toshiba Lighting & Technology Corp. (referred to as secondary PSA treatment). Then, the pretilt angle was measured.

[0194] <Measurement of pretilt angle> The pretilt angle of the liquid crystal cell for evaluating the pretilt angle prepared above was measured using an LCD analyzer (LCA-LUV42A manufactured by Meiryo Technica Co., Ltd.) The pretilt angle difference was calculated by subtracting the pretilt angle measured using the polyimide-coated substrate baked for 60 minutes from the pretilt angle measured using the polyimide-coated substrate baked for 20 minutes in an infrared heating furnace at 230°C. The measurement results of the pretilt angles in Examples 1 to 6 and Comparative Examples 1 and 2 are shown in Table 4 below.

[0195] [Table 4]

[0196] As shown in Table 4, it was confirmed that Examples 1 to 6 exhibited tilt angle characteristics equivalent to those of Comparative Examples 1 and 2, and exhibited good vertical alignment properties.

Claims

1. A liquid crystal aligning agent comprising the following components (A) and (B): the component (A) is at least one polymer (A) selected from the group consisting of polyimide precursors and polyimides which are imidized products of the polyimide precursors, The component (B) is a polymer (B) that contains a repeating unit structure represented by the following formula (1), has at least one triazine ring terminal, and at least a part of the triazine ring terminal is blocked with an arylamino group having a crosslinking group: The polymer (A) is obtained by using a diamine component containing an aromatic diamine and a tetracarboxylic acid component containing a tetracarboxylic acid dianhydride represented by the following formula (S4) or a derivative thereof: Liquid crystal alignment agent. 【Chemistry 1】 (R and R′ each independently represent a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, or an aralkyl group; Ar represents at least one selected from the group represented by formulas (2) to (12). 【Chemistry 2】 (Any hydrogen atom on the aromatic ring of formulas (2) to (12) may be substituted, R 12 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, W 1 and W. 2 are each independently a single bond, -CR 95 R 96 - (R 95 and R 96 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms (which may be joined together to form a ring). ), -C(=O)-, -O-, -S-, -S(=O)-, -SO 2 - or -NR 97 - (R 97 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a phenyl group; X 1 and X 2 are each independently a single bond, an alkylene group having 1 to 10 carbon atoms, or -Y 1 -Ph-Y 2 -(Ph represents a phenylene group, any hydrogen atom on the phenylene group may be substituted; Y 1 and Y 2 each independently represents a single bond or an alkylene group having 1 to 10 carbon atoms. 【Chemistry 3】 (X represents a structure selected from the group consisting of the following (x-1) to (x-13).) 【Chemistry 4】 (R 1 to R 4 each independently represent a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom, a monovalent organic group containing 1 to 6 carbon atoms and a fluorine atom, or a phenyl group. R 5 and R 6 each represent a hydrogen atom or a methyl group. j and k each represent an integer of 0 or 1. A 1 and A 2 each independently represent a single bond, -O-, -CO-, -COO-, phenylene, sulfonyl, or an amide bond. *1 represents a bond bonding to one of the acid anhydride groups, and *2 represents a bond bonding to the other acid anhydride group.)

2. The liquid crystal aligning agent according to claim 1 , wherein the arylamino group having a crosslinking group of the polymer (B) is represented by formula (15): 【Chemistry 5】 (In the formula, R 15 represents a bridging group.)

3. The liquid crystal aligning agent according to any one of claims 1 to 2, wherein the crosslinking group of the polymer (B) is a hydroxy-containing group or a (meth)acryloyl-containing group.

4. The crosslinking group of the polymer (B) is one or more selected from a hydroxy group, a hydroxymethyl group, a 2-hydroxyethyl group, a (meth)acryloyloxymethyl group, a (meth)acryloyloxyethyl group, and a group represented by the following formula (i-2) to formula (i-3). The liquid crystal aligning agent according to any one of claims 1 to 3. 【Chemistry 6】

5. The liquid crystal aligning agent according to any one of claims 1 to 4, wherein a part of the terminals of the triazine ring of the polymer (B) is further blocked with an unsubstituted arylamino group.

6. The polymer (A) is obtained using a diamine component containing at least one diamine (a) selected from the group consisting of structures represented by the following formulas (S1) to (S3): The liquid crystal aligning agent according to any one of claims 1 to 5. 【Chemistry 7】 (X 1 and X 2 each independently represents a single bond, -(CH 2 ) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH 3 )-, -NH-, -O-, -COO-, -OCO- or -((CH 2 ) a1 -A 1 ) m1 - (a1 is an integer from 1 to 15, A 1 represents an oxygen atom or -COO-; m 1 is an integer from 1 to 2. 1 When is 2, a plurality of a1 and A 1 Each of the groups independently has the same definition as above. 1 and G 2 each independently represents a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms and a divalent alicyclic group having 3 to 8 carbon atoms. Any hydrogen atom on the cyclic group may be substituted with an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorine atom-containing alkyl group having 1 to 3 carbon atoms, a fluorine atom-containing alkoxy group having 1 to 3 carbon atoms, or a fluorine atom. m and n are each independently an integer of 0 to 3, and m+n is an integer of 1 to 6. R 1 represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms; R 1 Any hydrogen atom forming the formula (I) may be substituted with a fluorine atom. 【Chemistry 8】 (X 3 represents a single bond, -CONH-, -NHCO-, -CON(CH 3 )-, -NH-, -O-, -CH 2 represents -O-, -COO- or -OCO-. 2 represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms; R 2 Any hydrogen atom forming the formula (I) may be substituted with a fluorine atom. 【Chemistry 9】 (X 4 is -CONH-, -NHCO-, -O-, -CH 2 represents -O-, -COO- or -OCO-. 3 represents a structure having a steroid skeleton.)

7. The liquid crystal aligning agent according to claim 6, wherein the diamine (a) is a diamine represented by the following formula (d1) or formula (d2): 【Chemistry 10】 (X is a single bond, —O—, —C(CH 3 ) 2 -, -NH-, -CO-, -(CH 2 ) m -, -SO 2 -, -O-(CH 2 ) m -O-, -OC(CH 3 ) 2 --, --CO-(CH 2 ) m -, -NH-(CH 2 ) m -, -SO 2 - (CH 2 ) m -, -CONH-(CH 2 ) m -, -CONH-(CH 2 ) m -NHCO- or -COO-(CH 2 ) m represents a divalent organic group of -OCO-. m is an integer of 1 to 8. Y represents any of the structures of the above formulae (S1) to (S3). In formula (d2), the two Y's may be the same or different.

8. The tetracarboxylic dianhydride or its derivative represented by the formula (S4) is a tetracarboxylic dianhydride or its derivative represented by the formula (x-1) to (x-7), (x-11) to (x-13), wherein X is a tetracarboxylic dianhydride or its derivative represented by the formula (x-1) to (x-7), (x-11) to (x-13). The liquid crystal aligning agent according to claim 1.

9. The content ratio of the (A) component and the (B) component is 10 / 90 to 90 / 10 in terms of a mass ratio of [(A) component] / [(B) component]. The liquid crystal aligning agent according to any one of claims 1 to 8.

10. A liquid crystal alignment film formed by using the liquid crystal aligning agent according to any one of claims 1 to 9.

11. A liquid crystal display element having a liquid crystal alignment film according to claim 10.

12. A method for producing a liquid crystal display element, comprising a step of applying the liquid crystal aligning agent according to any one of claims 1 to 9 onto a substrate.

13. The method for producing a liquid crystal display element according to claim 12, comprising applying the liquid crystal aligning agent according to any one of claims 1 to 9 onto a pair of substrates having conductive films to form coating films, arranging the coating films so as to face each other via a layer of liquid crystal molecules to form a liquid crystal cell, and irradiating the liquid crystal cell with light while applying a voltage between the conductive films of the pair of substrates.

Citation Information

Patent Citations

  • Alignment layer, polymer, retardation plate using it, its preparing method and liquid crystal display device

    JP2005097377A

  • Diamine, liquid crystal aligning agent and liquid crystal display element

    JP2011257731A

  • Film-forming composition

    WO2012026451A1

  • Liquid crystal aligning agent, liquid crystal alignment film, liquid crystal display element using same, and compound

    WO2013094618A1

  • Liquid crystal aligning agent containing polyamic acid or derivative thereof, liquid crystal alignment film and liquid crystal display element

    WO2016080458A1