Steaming paper substrate
A paper substrate with a polyvinyl alcohol resin-based sealing layer addresses the challenge of maintaining oxygen and water vapor barrier properties under high humidity, enhancing performance and reducing manufacturing complexity.
Patent Information
- Application Number
- JP2020101231
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-10
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-06-10
AI Technical Summary
Conventional paper substrates for vapor deposition struggle to exhibit excellent oxygen barrier properties, especially under high humidity conditions, and increasing the coating amount of barrier layers leads to manufacturing challenges and equipment limitations.
A paper substrate for vapor deposition is developed with a sealing layer containing a polyvinyl alcohol resin, optionally with a water vapor barrier resin and pigments, to form a uniform vapor deposition layer that maintains oxygen and water vapor barrier properties under high humidity.
The substrate achieves excellent oxygen and water vapor barrier properties under high humidity by preventing gas permeation and maintaining layer integrity, while reducing manufacturing constraints.
Smart Images

Figure 0007582640000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a metallized paper substrate. [Background technology]
[0002] Conventionally, there have been provided products in which water vapor barrier properties have been imparted to paper substrates by vapor deposition processing (Patent Document 1). Also, there has been disclosed a product in which oxygen barrier properties and water vapor barrier properties have been imparted to paper substrates by a coating layer rather than vapor deposition processing (Patent Document 2). However, it has been difficult for these paper substrate-based barrier materials to exhibit excellent oxygen barrier properties, especially under high humidity conditions. On the other hand, Patent Document 3 discloses that a water vapor barrier layer, a gas barrier layer, and a protective layer such as a resin layer are provided on a paper substrate to provide good oxygen barrier properties under high humidity. However, in this case, in order to provide particularly good oxygen barrier properties under high humidity, it was necessary to increase the coating weight of the barrier layer or provide a protective layer with good barrier properties. Increasing the coating weight of the barrier layer poses a problem of a large coating drying load during production, limiting the manufacturing equipment. In addition, reducing the coating weight requires providing a vapor deposition film or the like with excellent barrier properties as a protective layer, which restricts the type of protective layer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 7-256811 [Patent Document 2] Patent No. 5331265 [Patent Document 3] WO 2018 / 62466 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a vapor-deposited paper substrate for vapor deposition processing, which has particularly oxygen barrier properties. [Means for solving the problem]
[0005] The means for solving the problems of the present invention are as follows. 1. A metallized paper substrate having a sealing layer containing a polyvinyl alcohol resin on a base paper. 2. The deposited paper substrate according to 1., further comprising a layer containing a water vapor barrier resin as the filling layer. 3. The deposited paper substrate according to 2., wherein the layer containing the water vapor barrier resin contains a flat pigment. Effect of the Invention
[0006] The vapor-deposited paper substrate of the present invention can form a uniform vapor-deposited layer. A vapor-deposited paper obtained by subjecting the vapor-deposited paper substrate of the present invention to vapor deposition processing has excellent oxygen barrier properties and water vapor barrier properties, and can exhibit both excellent oxygen barrier properties and water vapor barrier properties even under high humidity conditions. The metal-deposited paper obtained from the metal-deposited paper substrate of the present invention can maintain oxygen barrier properties even under high humidity conditions because the metal-deposited layer prevents high-humidity gas from passing through, thereby suppressing deterioration of the sealing layer. In addition, by preventing high-humidity gas from passing through, excellent water vapor barrier properties can also be achieved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The deposition paper substrate of the present invention has a sealing layer containing a polyvinyl alcohol resin on a base paper. The deposition paper substrate of the present invention has this sealing layer, so that a uniform deposition layer can be formed. The deposition paper substrate of the present invention can suppress the decrease in oxygen barrier property under high humidity and can be imparted with excellent water vapor barrier property by carrying out various deposition processes on this sealing layer. Furthermore, the deposition paper substrate of the present invention can add a layer having water vapor barrier property as a sealing layer.
[0008] (Base paper) In the present invention, the base paper is a sheet made of pulp, a filler, and various auxiliary agents. The pulp may be selected from chemical pulps such as bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), unbleached hardwood kraft pulp (LUKP), unbleached softwood pulp (NUKP), sulfite pulp, and other mechanical pulps, wood fibers such as deinked pulp and recycled paper pulp, and non-wood fibers obtained from kenaf, bamboo, hemp, and other materials, which may be used in appropriate combinations. Among these, it is preferable to use chemical pulp or mechanical pulp made from wood fibers, and it is more preferable to use chemical pulp, because it is difficult for foreign matter to be mixed into the base paper, it has a high whiteness, and therefore the surface texture during printing is good, and it is particularly valuable when used as a packaging material.
[0009] As the filler, known fillers such as white carbon, talc, kaolin, clay, heavy calcium carbonate, light calcium carbonate, titanium oxide, zeolite, synthetic resin filler, etc. Also, aluminum sulfate and various anionic, cationic, nonionic or amphoteric retention improvers, drainage improvers, paper strength enhancers, internal sizing agents, etc. may be used as necessary. Furthermore, dyes, fluorescent whitening agents, pH adjusters, defoamers, pitch control agents, slime control agents, etc. may also be added as necessary.
[0010] The method for producing the base paper (papermaking) is not particularly limited, and the base paper can be produced by acidic papermaking, neutral papermaking, or alkaline papermaking using a known Fourdrinier former, on-top hybrid former, gap former machine, etc. The base paper may be composed of one layer, or two or more layers.
[0011] Furthermore, the surface of the base paper can be treated with various chemicals. Examples of chemicals that can be used include oxidized starch, hydroxyethyl etherified starch, enzyme-modified starch, polyacrylamide, polyvinyl alcohol, surface sizing agents, water-resistant agents, water retention agents, thickeners, and lubricants, and these can be used alone or in combination of two or more. Furthermore, these various chemicals can be used in combination with pigments. Examples of pigments include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, and satin white, and organic pigments such as solid, hollow, and core-shell types can be used alone or in combination of two or more.
[0012] The method for surface treatment of the base paper is not particularly limited, but known coating devices such as a rod metering size press, a pond type size press, a gate roll coater, a spray coater, a blade coater, and a curtain coater can be used.
[0013] The basis weight of the base paper can be appropriately selected depending on the desired qualities and handling properties of the metallized paper base material or metallized paper, but is usually 20 g / m 2 More than 500g / m 2 For metallized paper used for packaging purposes such as food packaging, containers, cups, etc., the thickness should be 25 g / m 2 More than 400g / m 2 The following is more preferable, and in particular for metallized paper used for soft packaging applications described later, it is 30 g / m 2 More than 110g / m 2 The following is more preferred:
[0014] (Sealing layer) The filler layer of the present invention is provided in advance by coating on the surface of the base paper so that the deposition can be uniform when various deposition processes are performed on it. The filler layer of the present invention may be one layer or may be composed of multiple layers, for example, a layer having water vapor barrier properties can be added as the filler layer. In this specification, the filler layer means a layer provided on the base paper, and may be only one layer or multiple layers.
[0015] The filling layer of the present invention contains a polyvinyl alcohol-based resin and can have at least oxygen barrier properties and can also have other barrier properties, such as water vapor barrier properties. In the present invention, depending on the performance to be imparted to the deposition paper substrate, one filling layer may be imparted with a plurality of properties, or each of the plurality of filling layers may be imparted with different properties.
[0016] The filling layer of the present invention contains at least a polyvinyl alcohol-based resin. The filling layer containing a polyvinyl alcohol-based resin enables the deposition layer to be formed uniformly and can have oxygen barrier properties. In the present invention, examples of the polyvinyl alcohol-based resin contained in the filling layer include polyvinyl alcohols such as fully saponified polyvinyl alcohol, partially saponified polyvinyl alcohol, ethylene copolymer polyvinyl alcohol, etc. Among these, ethylene copolymer polyvinyl alcohol is preferred from the viewpoint of gas barrier properties.
[0017] In the present invention, it is preferable to include a pigment in the filling layer from the viewpoint of improving gas barrier properties (oxygen barrier properties, water vapor barrier properties). When a pigment is included in the filling layer, gases such as oxygen pass by bypassing the pigment. Therefore, compared with a filling layer that does not include a pigment, it has excellent gas barrier properties in a high humidity atmosphere. As the pigment used in the filling layer, inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, satin white, and organic pigments such as solid, hollow, or core-shell types can be used alone or in combination of two or more. Among these, it is preferable to use a flat inorganic pigment from the viewpoint of gas barrier properties, and it is more preferable to use an inorganic pigment having an average particle size of 3 μm or more and an aspect ratio of 10 or more, and it is even more preferable to use an inorganic pigment having an average particle size of 5 μm or more and an aspect ratio of 30 or more. Examples of flat inorganic pigments that fall into this category include kaolin, clay, engineered kaolin, delaminated clay, mica, talc, and bentonite.
[0018] In the present invention, when the pigment is contained in the filling layer, the blending ratio of the pigment to the polyvinyl alcohol-based resin is preferably 0.01 / 100 to 200 / 100 by dry weight. If the pigment ratio is outside the above range, the effect of improving the barrier property may be small. In addition, in order to maintain the strength of the filling layer and prevent a decrease in the oxygen barrier property due to folding cracks during processing, the blending ratio of the pigment to the polyvinyl alcohol-based resin is preferably 0.01 / 100 to 40 / 100. Furthermore, it is particularly preferably 0.01 / 100 to 20 / 100. In the present invention, when the pigment is blended into the polyvinyl alcohol resin, it is preferable to add and mix the pigment in a slurried form.
[0019] In the present invention, a crosslinking agent, such as a polyvalent metal salt, can be added to the filling layer. The crosslinking agent causes a crosslinking reaction with the polyvinyl alcohol resin contained in the filling layer, and the number of bonds (crosslinking points) in the filling layer increases. In other words, by adding a crosslinking agent, the filling layer has a dense structure and can exhibit good gas barrier properties. In the present invention, the type of crosslinking agent is not particularly limited, and it is possible to appropriately select and use polyvalent metal salts (compounds in which polyvalent metals such as copper, zinc, silver, iron, potassium, sodium, zirconium, aluminum, calcium, barium, magnesium, titanium, etc. are bonded to ionic substances such as carbonate ions, sulfate ions, nitrate ions, phosphate ions, silicate ions, nitrogen oxides, boron oxides, etc.), amine compounds, amide compounds, aldehyde compounds, hydroxy acids, etc. From the viewpoint of the expression of the crosslinking effect, it is preferable to use polyvalent metal salts, and it is more preferable to use potassium alum.
[0020] The amount of crosslinking agent is not particularly limited as long as it is within the range of paint concentration and paint viscosity that can be applied, but it is preferably 1 part by weight to 10 parts by weight, more preferably 3 parts by weight to 5 parts by weight, per 100 parts by weight of pigment. If it is less than 1 part by weight, the effect of adding the crosslinking agent may not be fully obtained. Also, if it is more than 10 parts by weight, the viscosity of the paint may increase significantly, making coating difficult.
[0021] In the present invention, as the filling layer, a filling layer containing a polyvinyl alcohol resin (hereinafter also referred to as filling layer [1]) and a filling layer having water vapor barrier properties (hereinafter also referred to as filling layer [2]) can be laminated, and it is preferable that the filling layer [2] is the lower layer of the filling layer [1]. In this case, it is preferable that the filling layer [1] contains a surfactant from the viewpoint of adhesion with the filling layer [2]. There is no limitation on the ionicity of the surfactant, and any type of anionic surfactant, cationic surfactant, amphoteric surfactant, or nonionic surfactant can be used alone or in combination of two or more types. In addition, specific types include silicone-based surfactants, fluorine-based surfactants, alcohol-based surfactants, acetylene-based surfactants having an acetylene group, acetylene diol-based surfactants having an acetylene group and two hydroxyl groups, alkylsulfonic acid-based surfactants having an alkyl group and a sulfonic acid, ester-based surfactants, amide-based surfactants, amine-based surfactants, alkyl ether-based surfactants, phenyl ether-based surfactants, sulfate ester-based surfactants, and phenol-based surfactants can be exemplified. Among these, it is preferable to use acetylene diol surfactants, which have a large effect of improving the leveling property of the paint. Furthermore, when the leveling property of the paint is improved, the uniformity of the filling layer [1] is improved, and therefore the gas barrier property is improved. In the present invention, in addition to the above-mentioned polyvinyl alcohol-based resin, any pigment, crosslinking agent, and surfactant, various commonly used auxiliaries such as dispersants, thickeners, water retention agents, defoamers, water-resistant agents, dyes, and fluorescent dyes can be blended into the filling layer.
[0022] In the present invention, from the viewpoint of adhesion with the filling layer [2], it is preferable to adjust the surface tension of the paint for the filling layer [1] to 10 mN / m or more and 60 mN / m or less, and it is preferable to adjust the surface tension to 15 mN / m or more and 50 mN / m or less. In addition, it is preferable to set the surface tension of the paint for the filling layer [1] within ±20 mN / m with respect to the wetting tension of the surface of the filling layer [2] from the viewpoint of adhesion between the filling layer [2] and the filling layer [1].
[0023] (Filling layer [2]) As the filling layer, a filling layer [1] containing a polyvinyl alcohol resin and a filling layer [2] containing a water vapor barrier resin and having water vapor barrier properties can be laminated. The filling layer [2] is preferably formed as a lower layer of the filling layer [1].
[0024] As the water vapor barrier resin to be contained in the sealing layer [2], various copolymers such as styrene-butadiene, styrene-acrylic, ethylene-vinyl acetate, paraffin (wax), butadiene-methyl methacrylate, vinyl acetate-butyl acrylate, etc., synthetic adhesives such as maleic anhydride copolymers, acrylic acid-methyl methacrylate copolymers, or paraffin (wax)-containing synthetic adhesives of these can be used alone or in combination of two or more. In addition, as long as there is no problem with the water vapor barrier property, it is also possible to use polyvinyl alcohols such as fully saponified polyvinyl alcohol, partially saponified polyvinyl alcohol, and ethylene copolymerized polyvinyl alcohol, proteins such as casein, soy protein, and synthetic protein, starches such as oxidized starch, cationic starch, urea phosphate esterified starch, and hydroxyethyl etherified starch, cellulose derivatives such as carboxymethyl cellulose, hydroxymethyl cellulose, and hydroxyethyl cellulose, and water-soluble polymers such as polyvinylpyrrolidone and sodium alginate in combination with the above water vapor barrier resins.
[0025] In the present invention, in a configuration having the filling layer [2] and the filling layer [1], it is preferable that the filling layer [2] contains a pigment from the viewpoint of adhesion between the two layers. As the pigment, inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, satin white, and organic pigments such as solid, hollow, and core-shell types can be used alone or in combination of two or more. Among these pigments, inorganic pigments such as kaolin, mica, and talc, which are flat in shape, are preferred from the viewpoints of both improving the water vapor barrier property and suppressing the penetration of the sealing layer [1] having oxygen barrier properties. In addition, it is preferred to use flat pigments with a volume 50% average particle size (D50) (hereinafter also referred to as "average particle size") of 5 μm or more and an aspect ratio of 10 or more alone or in combination of two or more. If the average particle size or aspect ratio of the pigment used is smaller than the above range, the number of detours that water vapor takes through the filling layer [2] will decrease, and the distance that it travels will be shorter, which may result in a smaller improvement in the water vapor barrier property.
[0026] The water vapor barrier properties can be further improved by adding a pigment with an average particle size of 5 μm or less to the filling layer [2] in addition to the flat pigment. This pigment with an average particle size of 5 μm or less does not need to be flat. By incorporating flat pigments and pigments with an average particle size of 5 μm or less in the filling layer [2], the structure is created in which the pigments with an average particle size of 5 μm or less penetrate between the flat pigments that exist in layers. The water vapor that is forced to move along the surface of the flat pigments is prevented from moving by these small pigment particles. In other words, when the filling layer [2] contains flat pigments and pigments with an average particle size of 5 μm or less, the gaps formed between adjacent flat pigments in the filling layer [2] are filled with small particle pigments, and water vapor passes through by bypassing the pigments, demonstrating high water vapor barrier properties.
[0027] In the present invention, when a flat pigment and a pigment having an average particle size of 5 μm or less are used in combination, the blending ratio of the flat pigment and the pigment having an average particle size of 5 μm or less is preferably 50 / 50 to 99 / 1 by dry weight. If the blending ratio of the flat pigment is less than the above range, the number of times that water vapor takes a detour through the filling layer [2] decreases, and the travel distance becomes shorter, so that the effect of improving the water vapor barrier property may be reduced.
[0028] In the present invention, examples of pigments having an average particle size of 5 μm or less that can be used in combination with the flat pigment include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicates, colloidal silica, and satin white, and organic pigments such as solid, hollow, and core-shell types, which can be used alone or in combination of two or more.
[0029] When a pigment is contained in the filling layer [2], the total amount of the water vapor barrier resin and the water-soluble polymer is preferably in the range of 5 parts by weight or more and 500 parts by weight or less, and more preferably 10 parts by weight or more and 300 parts by weight or less, per 100 parts by weight of the pigment, on a dry weight basis.
[0030] In the present invention, a crosslinking agent, such as a polyvalent metal salt, can be added to the filling layer [2]. The crosslinking agent causes a crosslinking reaction with the water vapor barrier resin or water-soluble polymer contained in the filling layer [2], and the number of bonds (crosslinking points) in the filling layer [2] increases. In other words, the filling layer [2] has a dense structure and can exhibit good water vapor barrier properties. In the present invention, the type of crosslinking agent is not particularly limited, and it is possible to appropriately select and use, depending on the type of water vapor barrier resin or water-soluble polymer contained in the filling layer [2], from polyvalent metal salts (compounds in which a polyvalent metal, such as copper, zinc, silver, iron, potassium, sodium, zirconium, aluminum, calcium, barium, magnesium, or titanium, is bonded to an ionic substance, such as carbonate ion, sulfate ion, nitrate ion, phosphate ion, silicate ion, nitrogen oxide, or boron oxide), amine compounds, amide compounds, aldehyde compounds, hydroxy acids, and the like.
[0031] When using styrene-based water vapor barrier resins such as styrene-butadiene and styrene-acrylic resins, which exhibit excellent water vapor barrier properties, it is preferable to use a polyvalent metal salt as a crosslinking agent from the viewpoint of exhibiting a crosslinking effect, and it is more preferable to use potassium alum. The amount of crosslinking agent is not particularly limited as long as it is within the range of paint concentration and paint viscosity that can be applied, but it is preferably 1 part by weight to 10 parts by weight, more preferably 3 parts by weight to 5 parts by weight, per 100 parts by weight of pigment. If it is less than 1 part by weight, the effect of adding the crosslinking agent may not be fully obtained. Also, if it is more than 10 parts by weight, the viscosity of the paint may increase significantly, making coating difficult. In the present invention, when a crosslinking agent is added to the coating material for the filling layer [2], it is preferable to dissolve the crosslinking agent in a polar solvent such as ammonia and then add it to the coating material. When the crosslinking agent is dissolved in a polar solvent, the crosslinking agent and the polar solvent form a bond, so that even if the crosslinking agent is added to the coating material, a crosslinking reaction with the water vapor barrier resin or the water-soluble polymer does not occur immediately, and therefore the thickening of the coating material can be suppressed. In that case, it is presumed that the polar solvent components volatilize when the coating material is dried after being applied to the base paper, and a crosslinking reaction with the water vapor barrier resin or the water-soluble polymer occurs, forming a dense filling layer [2].
[0032] In the present invention, from the viewpoint of improving the water vapor barrier property, a water repellent can be contained in the sealing layer [2]. Examples of the water repellent include paraffin-based water repellents mainly composed of alkane compounds, natural oil-based water repellents derived from animals and plants such as carnauba and lanolin, silicone-containing water repellents containing silicone or silicone compounds, and fluorine-containing water repellents containing fluorine compounds. These water repellents can be used alone or in combination of two or more kinds. The filling layer [2] may contain, in addition to the water vapor barrier resin, water-soluble polymer, pigment, crosslinking agent, and water repellent agent, various commonly used auxiliary agents such as dispersants, thickeners, water retention agents, defoamers, water-resistant agents, dyes, and fluorescent dyes.
[0033] In addition, in the present invention, in order to improve the water vapor barrier property and the adhesion to the filling layer [1] having the above-mentioned oxygen barrier property, the wetting tension of the surface of the filling layer [2] is preferably 10 mN / m or more and 60 mN / m or less, and more preferably 15 mN / m or more and 50 mN / m or less.
[0034] (Coating of the sealing layer) In the present invention, the coating method of the sealing layer is not particularly limited, and coating can be performed using a known coating device and coating system. For example, the coating device may be a blade coater, a bar coater, a roll coater, an air knife coater, a reverse roll coater, a curtain coater, a spray coater, a size press coater, a gate roll coater, etc. In addition, the coating system may be an aqueous coating using a solvent such as water, or a solvent coating using a solvent such as an organic solvent, etc. The coating liquid for the sealing layer is preferably an aqueous one. The filling layer can be dried by a conventional method using, for example, a steam heater, a gas heater, an infrared heater, an electric heater, a hot air heater, a microwave, a cylinder dryer, or the like.
[0035] In the present invention, when a single layer of a filling layer containing a polyvinyl alcohol resin is provided, the coating amount is 0.2 g / m2 in terms of dry weight. 2More than 20g / m 2 The coating weight is preferably 0.2 g / m or less. 2 If the coating density is less than 20 g / m, a smooth layer cannot be formed during coating, and in extreme cases, pinholes may occur, making it difficult to form a uniform filling layer, and therefore making it difficult to obtain a uniform deposition layer. 2 If it is more than 20g / m, the drying load during coating will be large. 2 If the amount is larger, it becomes necessary to maintain the strength of the filling layer itself (to prevent cohesive failure or cracking of the coating layer).
[0036] In the present invention, when a filler layer [2] having water vapor barrier properties is further added as a filler layer, the coating amount of the filler layer [2] is 3 g / m2 in dry weight. 2 More than 50g / m 2 It is preferable that the density is 3.5 g / m or less. 2 More than 40g / m 2 More preferably, it should be 4 g / m or less. 2 More than 30g / m 2 It is more preferable that the coating weight of the filling layer [2] is 3 g / m or less. 2 If it is less than 50 g / m, it becomes difficult to completely cover the base paper with the coating liquid, and sufficient water vapor barrier properties cannot be obtained, or the filler layer [1] applied on the filler layer [2] may penetrate into the base paper, making it difficult to obtain a uniform filler layer. 2 If it is more than this amount, the drying load during coating increases.
[0037] (Paper base material for vapor deposition) In the present invention, the moisture content of the deposition paper substrate is not particularly limited, but when forming a deposition layer under vacuum conditions, a high moisture content leads to a low degree of vacuum, so a low moisture content is preferable. Specifically, it is preferably 8.0% by weight or less, more preferably 6.0% by weight or less, even more preferably 3.0% by weight or less, and most preferably 1.0% by weight or less. The lower limit of the moisture content is not particularly limited, but is about 0.1% by weight.
[0038] (deposited layer) A vapor deposition layer is provided on the sealing layer of the vapor deposition paper substrate to obtain a vapor deposition paper. The vapor deposition layer can contain metal, inorganic oxide, inorganic nitride, etc. Examples of the metal vapor deposition layer include aluminum, tin, nickel, copper, gold, platinum, silver, cobalt, chromium, etc., with aluminum being more preferred because it has high light shielding properties and is inexpensive. Examples of the inorganic oxide vapor deposition layer include oxides of silicon, aluminum, titanium, zirconium, tin, magnesium, lead, boron, sodium, etc., or mixtures thereof, and further, composites with inorganic nitrides, with silicon oxide or aluminum oxide being more preferred because they have high barrier properties and transparency and are inexpensive. The method of forming the vapor deposition layer is arbitrary, and known methods such as vacuum vapor deposition, ion plating, sputtering, and plasma vapor deposition (CVD) can be used. The vacuum vapor deposition method is relatively easy to form a vapor deposition layer, and is preferable in terms of productivity. The thickness of the deposition layer is preferably 5 to 300 nm, and more preferably 10 to 150 nm. If the thickness is less than 5 nm, a uniform deposition layer cannot be formed, and sufficient barrier properties may not be obtained. On the other hand, if the thickness exceeds 300 nm, it becomes difficult to maintain the flexibility of the deposition layer, and there is a risk of cracks occurring due to external factors such as bending and pulling after film formation.
[0039] (Vapor deposition protective layer) A protective layer may be laminated on the deposition layer for the purpose of protecting the surface or improving suitability for post-processing such as lamination. In this case, for example, a water-soluble polymer is dissolved in water or a water / alcohol mixed solvent, and a metal alkoxide is mixed with the water-soluble polymer, either directly or after being hydrolyzed in advance, and the mixed solution is applied onto the deposition layer and dried to form the protective layer. In addition, an isocyanate compound, a silane coupling agent, a dispersant, a stabilizer, a viscosity modifier, a colorant, etc. may be added to the mixed solution as necessary.
[0040] (Resin layer) A resin layer can be provided on at least one side of the metallized paper, which can impart heat sealability. The resin layer can be provided on both sides of the metallized paper, but it is preferable to provide the resin layer at least on the side having the metallized layer. Resins for the resin layer can include resins derived from fossil resources such as polyester, polyvinyl alcohol, polypropylene, polyethylene, polystyrene, polyethylene terephthalate, polybutylene terephthalate, polymethylpentene, polyvinyl chloride, acrylonitrile-butadiene-styrene, acrylonitrile-styrene, polymethyl(meth)acrylic, polyvinylidene chloride, polyamide (nylon), polyacetal, and polycarbonate, as well as biologically derived resins such as polylactic acid (PLA), esterified starch, cellulose acetate, polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), biopolyethylene, biopolyethylene terephthalate, and biopolyurethane. Note that bioresin refers to a polymeric material with a number average molecular weight (Mn) of 1,000 or more that contains substances derived from renewable organic resources as raw materials and is obtained by chemical or biological synthesis.
[0041] In addition, as resins derived from fossil resources and biologically derived resins, any of the following can be used: biodegradable resins such as polylactic acid (PLA), esterified starch, cellulose acetate, polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), and non-biodegradable resins such as polyethylene, polypropylene, polyester, polyethylene terephthalate, polyamide (nylon), and biopolyethylene. A biodegradable resin is a resin that can be broken down to the molecular level by the action of microorganisms, and ultimately circulates back into nature as carbon dioxide and water.
[0042] In the present invention, the resin layer is preferably a resin laminate layer. Examples of the resin laminate layer include an extrusion laminate layer and a film attachment layer such as a barrier film. When the resin laminate layer is an extrusion laminate layer, the above-mentioned various resins are laminated as a resin laminate layer on at least one surface of the metal-deposited paper by an extrusion lamination method. When the resin laminate layer is a film attachment layer, the above-mentioned various resin films are attached as a resin laminate layer on at least one surface of the metal-deposited paper by a dry lamination method, a sand lamination method, etc. The resin layer can be provided on both sides of the metal-deposited paper, but it is preferable to have a resin layer at least on the surface having the metal-deposited layer. In the present invention, the film used for the film attachment layer may be any of the above-mentioned various resin films. Depending on the purpose, one or more of these films may be attached.
[0043] The metallized paper can be used as it is, or laminated with various resins, or pasted with various general-purpose films, barrier films, etc., to form a packaging material used for packaging applications such as food packaging, containers, cups, etc., or a laminate used for industrial materials, etc. Among these, the metallized paper can be suitably used as a packaging material used for packaging applications such as food packaging, containers, cups, etc., and can be particularly suitably used as a soft packaging material for food, etc. Note that the soft packaging material is a packaging material made of a highly flexible material, and generally refers to a packaging material made of thin, flexible materials such as paper, film, aluminum foil, etc., either alone or pasted together. In terms of shape, the soft packaging material refers to a packaging material such as a bag that maintains a three-dimensional shape by putting contents inside.
[0044] When the metallized paper is used as a packaging material for food and the like, particularly as a soft packaging material, laminating it with a resin having heat-sealing properties can enhance the airtightness of the packaging material, protect the contents from oxidation due to oxygen and deterioration due to moisture, and enable the shelf life to be extended. Furthermore, when used as a laminate for industrial materials, etc., it is possible to prevent putrefaction and deterioration by suppressing the intrusion of oxygen and moisture, and it is also expected to have effects such as flavor barrier properties that prevent the odor of solvents from leaking out. EXAMPLES
[0045] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, parts and % are by weight, respectively, unless otherwise specified. The obtained metallized paper substrate and metallized paper were subjected to tests based on the evaluation methods described below.
[0046] (Evaluation method) <Moisture percentage> Measurement was performed in accordance with JIS P8203:2010. The deposition paper substrate was cut into A4 size (210 mm x 297 mm) and the weight before drying was measured. Next, it was dried in a 105±2°C air dryer until it reached a constant weight, and then the weight after drying was measured. The moisture content was calculated using the following formula. Moisture percentage (weight %) = 100 × (weight before drying - weight after drying) / weight before drying <Appearance evaluation> The surface appearance of the metallized layer of the metallized paper was visually evaluated on a three-point scale: ◯ for a strong metallic luster, △ for a little luster and partial unevenness, and × for no luster.
[0047] <Oxygen permeability (gas barrier properties)> The metallized paper was measured using OX-TRAN2 / 21 manufactured by MOCON under conditions of 23°C and 0% RH (dry conditions) and 23°C and 85% RH (high humidity conditions). <Water vapor permeability (water vapor barrier properties)> The vapor-deposited paper was measured using a moisture permeability meter (L80-4000, manufactured by Dr. Lyssy) in accordance with JIS K7129A:2008 under conditions of a temperature of 40±0.5° C. and a relative humidity difference of 90±2%.
[0048] [Example 1] (Preparation of base paper) A hardwood bleached kraft pulp (LBKP) with a Canadian standard freeness (CSF) of 500 ml and a softwood bleached kraft pulp (NBKP) with a CSF of 530 ml were mixed in a weight ratio of 80 / 20 to prepare the raw pulp. To the raw pulp slurry, 0.1% of polyacrylamide (PAM) with a molecular weight of 2.5 million was added as a dry strength agent, 0.35% of alkyl ketene dimer (AKD) as a sizing agent, 0.15% of polyamide epichlorohydrin (PAEH) resin as a wet strength agent, and 0.08% of polyacrylamide (PAM) with a molecular weight of 10 million was added as a retention agent. The mixture was then made into paper at a speed of 300 m / min on a Duoformer FM papermaking machine to produce a paper with a basis weight of 50 g / m. 2 The obtained base paper was smoothed using a chilled calender at a speed of 300 min / m, a linear pressure of 50 kgf / cm, and one pass to obtain a base paper.
[0049] (Preparation of coating solution for filling layer [1]) Polyvinyl alcohol (PVA117 manufactured by Kuraray Co., Ltd.) was prepared so that the solid content concentration was 10%, and a coating solution [1] was obtained.
[0050] (Preparation of vapor-deposited paper substrate) On the obtained base paper, the coating solution for the filling layer [1] was applied in an amount (dry) of 5.0 g / m 2 The coating was applied to one side using a roll coater at a coating speed of 300 m / min so as to obtain a moisture content of 1.0% by weight, thereby obtaining a deposition paper substrate.
[0051] (Preparation of metallized paper) An aluminum vapor deposition layer having a thickness of 45 nm was formed on the sealing layer of the obtained vapor deposition paper substrate using a batch type vacuum deposition device. Furthermore, a resin layer made of low density polyethylene (manufactured by Japan Polyethylene Corporation, LC602A) was laminated to a thickness of 30 μm on both sides of the obtained vapor deposition paper by extrusion lamination.
[0052] [Example 2] A large particle size engineered kaolin (Imeris, Barisurf HX, particle size 9.0 μm, aspect ratio 80-100) was mixed with sodium polyacrylate as a dispersant (0.2 parts relative to inorganic pigment) and dispersed in a Serie mixer to prepare a large particle size kaolin slurry with a solid content concentration of 55%. A deposition paper substrate was produced in the same manner as in Example 1, except that the obtained kaolin slurry and the coating liquid for the filling layer [1] were mixed in a ratio of pigment: coating liquid for the filling layer [1] = 100:100 in solid content to give a solid content concentration of 10%. Further, a deposition process was performed in the same manner as in Example 1 to obtain a deposition paper.
[0053] [Example 3] (Preparation of coating solution for filling layer [2]) A large particle size engineered kaolin (Imerys Corporation, Barisurf HX, particle size 9.0μm, aspect ratio 80-100) was mixed with sodium polyacrylate as a dispersant (0.2 parts per inorganic pigment) in a Serie mixer to prepare a large particle size kaolin slurry with a solid content of 55%. Styrene-butadiene latex (Zeon Corporation, PNT7868) was mixed with the resulting kaolin slurry at 100 parts (solids) per 100 parts inorganic pigment to obtain a coating solution with a solid content of 50% [2].
[0054] On the base paper, apply the coating solution for the filling layer [2] at a coating amount (dry) of 12 g / m 2 The coating was applied to one side of the substrate at a coating speed of 300 m / min using a blade coater, and then dried. A coating liquid was applied on top of the substrate, which was a mixture of the kaolin slurry prepared in Example 2 and the coating liquid for the filling layer [1], with a solid content ratio of pigment:coating liquid for the filling layer [1] = 100:100, so that the solid content concentration was 10%, at a coating amount (dry) of 2 g / m 2 Except for the above, a deposition paper substrate was produced in the same manner as in Example 1. Further, a deposition treatment was carried out in the same manner as in Example 1 to obtain a deposition paper.
[0055] [Example 4] A deposition paper substrate was prepared in the same manner as in Example 3, except that a coating liquid was used in which the kaolin slurry prepared in Example 2 and the coating liquid for filling layer [1] were mixed at a solid content ratio of pigment:coating liquid for filling layer [1] = 20:100 so that the solid content concentration was 10%. Further, a deposition treatment was performed in the same manner as in Example 1 to obtain a deposition paper. [Example 5] A deposition paper substrate was prepared in the same manner as in Example 3, except that a coating liquid was used in which the kaolin slurry prepared in Example 2 and the coating liquid for filling layer [1] were mixed at a solid content ratio of pigment:coating liquid for filling layer [1] = 1:100 to give a solid content concentration of 10%. Further, a deposition treatment was performed in the same manner as in Example 1 to obtain a deposition paper.
[0056] [Example 6] A deposited paper substrate was prepared in the same manner as in Example 3, except that the moisture content was adjusted from 1.0% by weight to 3.0% by weight. Further, a deposition treatment was carried out in the same manner as in Example 1 to obtain a deposited paper. [Example 7] A deposited paper substrate was prepared in the same manner as in Example 3, except that the moisture content was adjusted from 1.0% by weight to 6.0% by weight. Further, a deposition treatment was carried out in the same manner as in Example 1 to obtain a deposited paper. [Example 8] A deposited paper substrate was prepared in the same manner as in Example 3, except that the moisture content was adjusted from 1.0% by weight to 7.0% by weight. Further, a deposition treatment was carried out in the same manner as in Example 1 to obtain a deposited paper.
[0057] [Comparative Example 1] Except for not coating the base paper with the coating liquids [1] and [2] for the filling layer, a deposition paper substrate was prepared in the same manner as in Example 1. Further, a deposition treatment was performed in the same manner as in Example 1 to obtain a deposition paper. [Comparative Example 2] A deposition paper substrate was prepared in the same manner as in Example 3, except that the kaolin slurry and the coating liquid for filling layer [1] prepared in Example 2 were not coated with the coating liquid in which the ratio of pigment to coating liquid for filling layer [1] was 100:100 in terms of solid content. Further, deposition treatment was performed in the same manner as in Example 1 to obtain a deposition paper.
[0058] [Comparative Example 3] A deposition paper substrate was prepared in the same manner as in Comparative Example 2, except that in the coating solution for the filling layer [2], a styrene-butadiene latex (PNT7868 manufactured by Zeon Corporation) was used instead of a styrene-acrylic copolymer emulsion (X-511-374E manufactured by Saiden Chemical Industry Co., Ltd.). A deposition treatment was then carried out in the same manner as in Example 1 to obtain a deposition paper. [Comparative Example 4] A deposition paper substrate was prepared in the same manner as in Comparative Example 3, except that in the coating solution for the filling layer [2] in Comparative Example 3, 100 parts (solid content) of a styrene-acrylic copolymer emulsion (X-511-374E, manufactured by Saiden Chemical Industry Co., Ltd.) and 100 parts (solid content) of a paraffin-based water repellent (MYE-35G, wax-containing polyethylene emulsion, manufactured by Maruyoshi Chemical Industry Co., Ltd.) were mixed per 100 parts of pigment. Then, deposition treatment was carried out in the same manner as in Example 1 to obtain a deposition paper.
[0059] [Table 1]
[0060] From the vapor-deposited paper substrate having the polyvinyl alcohol-based resin-containing filling layer [1] obtained in Examples 1 to 8 of the present invention, vapor-deposited paper having excellent oxygen barrier properties not only under dry conditions but also under high humidity conditions was obtained. The obtained vapor-deposited paper had a metallic luster. The vapor-deposited paper obtained from the vapor-deposited paper substrate having the filling layer [1] and the filling layer [2] had excellent oxygen barrier properties and water vapor barrier properties under high humidity conditions. It was also confirmed that the lower the moisture content of the vapor-deposited paper substrate, the more excellent the vapor-deposited paper having excellent barrier properties was obtained. In Comparative Example 1, the base paper was used as it was as the metallized paper substrate, but the resulting metallized paper had poor barrier properties, poor metallic luster, and the paper fibers were visible through the surface of the metallized layer. The metal-deposited paper substrates having a filling layer containing a resin other than a polyvinyl alcohol-based resin obtained in Comparative Examples 2 to 4 were inferior in oxygen barrier property and water vapor barrier property to the metal-deposited paper substrate of the present invention. In addition, the metal-deposited paper obtained had a strong matte feel and no metallic luster.
Claims
[Claim 1] A sealing layer containing a polyvinyl alcohol-based resin is provided on a base paper, The deposition paper substrate further comprises a layer containing a water vapor barrier resin and a flat pigment as the filling layer.
Citation Information
Patent Citations
Filter type dust collector
JP1978031265A
Metallic vapor deposited paper and its manufacture
JP1982134556A
Mirror surface metal vapor deposition paper
JP1984015595A
Method for controlling exhaust gas recirculation in internal-combustion engine
JP1984049359A
JP1991120600U