Packaging
A laminated packaging material with a cyclic polyolefin innermost layer, uniaxially stretched polyolefin intermediate layer, and metal oxide outermost layer addresses adsorption and cut straightness issues, enhancing usability and manufacturability while maintaining effective sealing.
Patent Information
- Application Number
- JP2021551402
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Existing packaging materials for pharmaceutical patches with volatile pharmacologically active ingredients face challenges in suppressing adsorption of these ingredients and ensuring straightness of the cut portion, while also being user-friendly and cost-effective.
A packaging material comprising a cyclic polyolefin film with 60% or more cyclic polyolefin resin as the innermost layer, a uniaxially stretched polyolefin film as the intermediate layer, and a metal or metal oxide vapor-deposited film as the outermost layer, providing a laminated structure that suppresses adsorption and improves cut straightness.
The packaging material effectively reduces adsorption of volatile active ingredients and enhances the straightness of the cut portion, offering improved usability, manufacturability, and heat-sealing properties.
Smart Images

Figure 0007582959000001 
Figure 0007582959000002 
Figure 0007582959000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a bag-shaped packaging material (hereinafter referred to as "packaging material") for primary packaging of pharmaceutical patches, and more specifically to a packaging material for patches which not only has excellent sealing properties, but also has low adsorption of volatile pharmacological ingredients and excellent linearity at the cut section when the packaging material is opened. [Background technology]
[0002] Pharmaceutical packaging materials must be suitable for ensuring the quality of pharmaceutical products, as well as for proper use and safety during administration. The General Provisions for Preparations in the 17th Revised Japanese Pharmacopoeia [2], General Provisions for Preparation Packaging, lists the qualifications required for pharmaceutical packaging, including "protection of the preparation" (such as suppressing drug adsorption into patches), "compatibility between the preparation and packaging" (to ensure that the quality of the preparation is not reduced), "safety of the materials used in the packaging" (to ensure that ingredients in the packaging do not migrate to the preparation and impair its safety), and "additional functions at the time of administration" (performance) regarding identification, usability, and disposal.
[0003] Among these, with regard to the suppression of volatile pharmacologically active ingredient adsorption, which is one of the performances of "protection of preparations," the composition of the sealant material (the innermost layer of the packaging material) to which volatile pharmacologically active ingredients such as l-menthol are not adsorbed is particularly important. For example, a low-adsorption sealant substrate (Patent Document 1) in which an inorganic vapor-deposited thin film layer is laminated on a heat-sealable thermoplastic resin, a polyacrylonitrile (PAN) substrate (Patent Document 2) or a substrate selected from the group consisting of polyacrylonitrile resin particles and polyester resin particles (Patent Document 3), a laminate characterized in that the innermost layer is a polyacrylonitrile resin, a polyester resin, or an ethylene-vinyl acetate copolymer saponification product that suppresses the sorption of l-menthol (Patent Document 4), a sealant film (Patent Document 5) containing one or more resins selected from polyester-based resins, polyamide-based resins, and ethylene-based copolymers with a solubility parameter (SP value) of 9 or more, and a sealant layer (Patent Document 6) containing a cyclic olefin-based resin with a glass transition temperature of 50°C to 190°C for contents containing a volatile low-molecular-weight compound with a molecular weight of 800 or less, etc. are known. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2005-144879 A [Patent Document 2] JP 2005-328928 A [Patent Document 3] JP 2012-184357 A [Patent Document 4] Japanese Patent Application Publication No. 8-143452 [Patent Document 5] JP 2016-198918 A [Patent Document 6] JP 2016-222332 A Summary of the Invention [Problem to be solved by the invention]
[0005] The low-adsorption sealant base material, in which an inorganic vapor-deposited thin film layer is laminated onto the above-mentioned heat-sealable thermoplastic resin, results in a packaging material that is hard and therefore has a poor feel to the touch and is difficult to insert and remove. In addition, polyacrylonitrile (PAN)-based base materials are expensive and have poor processability (manufacturability), ethylene-vinyl acetate copolymers have a low effect of suppressing the adsorption of volatile pharmacologically active ingredients, and cyclic polyolefin-based resins have a high effect of suppressing the adsorption of volatile pharmacologically active ingredients, but have a poor feel when used as a packaging material. Furthermore, all of the packaging materials using the above-mentioned sealant materials have the problem that the linearity of the cut portions is poor when the materials are cut by hand. [Means for solving the problem]
[0006] There is a demand for packaging materials for patches containing volatile pharmacologically active ingredients that have excellent sealing properties, suppress adsorption of the volatile pharmacologically active ingredient, and, when made into a bag, can simultaneously satisfy the problem of poor linearity at the cut section when first opened. The inventors have discovered that the above-mentioned problems can be solved by a packaging material in which the innermost layer, which will come into contact with the contents when the bag is made, is a cyclic polyolefin film containing 60% by mass or more of cyclic polyolefin resin based on the total resin components, or a film having a polyethylene resin layer on the innermost layer side of the film, and which is laminated with this film, a uniaxially oriented polyolefin film, and a film vapor-deposited with a metal or metal oxide, and have completed the present invention.
[0007] That is, the present invention provides: 1. A bag-shaped packaging material containing a patch containing a volatile pharmacologically active ingredient, the packaging material comprising: a cyclic polyolefin film containing 60% by mass or more of a cyclic polyolefin resin based on the total resin components as an innermost layer on the patch side; As an intermediate layer outside the innermost layer, a uniaxially oriented polyolefin film; a film selected from polyester, polyamide, and polypropylene, on which a metal or metal oxide is vapor-deposited, as an outermost layer outside the intermediate layer; The packaging material has a laminated structure in which the surface of the outermost layer on which the metal or metal oxide is vapor-deposited faces the intermediate layer.
[0008] Furthermore, the present invention further provides the following embodiments. 2. The packaging material, wherein the cyclic polyolefin film containing 60% by mass or more of the cyclic polyolefin resin based on the total resin components is a film having a polyethylene resin layer on the innermost layer side. 3. The packaging material, wherein the volatile pharmacologically active ingredient is one or more selected from the group consisting of methyl salicylate, glycol salicylate, l-menthol and dl-camphor. 4. The packaging material as described above, wherein the cyclic polyolefin film-based resin is at least one selected from the group consisting of norbornene-based polymers, vinyl alicyclic hydrocarbon polymers, and cyclic conjugated diene polymers. 5. The packaging material, wherein the uniaxially oriented polyolefin film is a uniaxially oriented polyethylene film or a uniaxially oriented polypropylene film. 6. The packaging material as described above, wherein the polyethylene resin layer is a resin layer containing at least one resin selected from the group consisting of low density polyethylene, linear low density polyethylene, medium density polyethylene, and high density polyethylene. 7. The packaging material, wherein the polyester film onto which a metal or metal oxide is vapor-deposited is a film of at least one polyester selected from the group consisting of polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate, onto which a metal or metal oxide is vapor-deposited. 8. The packaging material is the innermost layer being a cyclic polyolefin-based film containing 60% by mass or more of a cyclic polyolefin-based resin based on the total resin components; an intermediate layer that is adjacent to the outer side of the innermost layer and is a uniaxially oriented polyolefin film; a film selected from polyester, polyamide and polypropylene, on which a metal or metal oxide is vapor-deposited, the metal or metal oxide being the outermost layer adjacent to the outer side of the intermediate layer; It is a three-layer laminate. The packaging material. 9. The packaging material, wherein the uniaxially oriented polyolefin film is a uniaxially oriented polypropylene film. Effect of the Invention
[0009] According to the present invention, a packaging material for a patch containing a volatile pharmacologically active ingredient is used, which comprises a laminate having a cyclic polyolefin film containing 60% by mass or more of a cyclic polyolefin resin based on the total resin components as the innermost layer on the patch side when made into a bag, or a film having a polyethylene resin layer on the innermost layer side of said film, a uniaxially oriented polyolefin film as an intermediate layer outside the innermost layer, and a film vapor-deposited with a metal or metal oxide as the outermost layer outside the intermediate layer, thereby simultaneously achieving 1) suppression of adsorption of the volatile pharmacologically active ingredient and 2) improvement in the linearity of the cut portion when the packaging material is cut. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The packaging material of the present invention is composed of at least a specific cyclic polyolefin film, i.e., a cyclic polyolefin film containing 60% by mass or more of cyclic polyolefin resin based on the total resin components, or a film having a polyethylene resin layer on the innermost layer side of the film, a uniaxially stretched polyolefin film, and a film selected from polyester, polyamide, and polypropylene vapor-deposited with metal or metal oxide, laminated in this order (laminated film). Here, when the packaging material is made into a bag shape, the specific cyclic polyolefin film constitutes the innermost layer on the patch side, which is the content, and the film of polyester or the like vapor-deposited with metal or metal oxide constitutes the outermost layer.
[0011] [Innermost layer: cyclic polyolefin film] In the packaging material of the present invention, the specific cyclic polyolefin film constituting the innermost layer on the patch side when made into a bag is a film containing cyclic polyolefin resin at 60% by mass or more based on the total resin components.Specifically, as described below, it can be a monolayer film containing cyclic polyolefin resin at 60% by mass or more based on the total resin components, or a multilayer film containing cyclic polyolefin resin at 60% by mass or more based on the total resin components, and the innermost layer side (innermost surface) when made into a packaging material, which is the surface that contacts the contents, can be a polyethylene resin layer. Examples of the cyclic polyolefin resin include norbornene polymers, vinyl alicyclic hydrocarbon polymers, and cyclic conjugated diene polymers. Among these, norbornene polymers are preferred. Examples of norbornene polymers include ring-opening polymers of norbornene monomers (hereinafter referred to as "COP") and norbornene copolymers (hereinafter referred to as "COC") obtained by copolymerizing norbornene monomers with olefins such as ethylene. Hydrogenated products of COP and COC are particularly preferred. The glass transition point (Tg) of the cyclic olefin resin is preferably 100°C or higher. The weight average molecular weight of the cyclic olefin resin is preferably 5,000 to 500,000, and more preferably 7,000 to 300,000. The glass transition point and melting point in the present invention are measured by differential scanning calorimetry (DSC).
[0012] The norbornene monomer used as the raw material for the norbornene polymer is an alicyclic monomer having a norbornene ring. Examples of such norbornene monomers include norbornene, tetracyclododecene, ethylidenenorbornene, vinylnorbornene, ethylidetetracyclododecene, dicyclopentadiene, dimethanotetrahydrofluorene, phenylnorbornene, methoxycarbonylnorbornene, and methoxycarbonyltetracyclododecene. These norbornene monomers may be used alone or in combination of two or more.
[0013] The norbornene copolymer is a copolymer of the norbornene monomer and a copolymerizable olefin, and examples of such olefins include olefins having 2 to 20 carbon atoms such as ethylene, propylene, and 1-butene, cycloolefins such as cyclobutene, cyclopentene, and cyclohexene, and non-conjugated dienes such as 1,4-hexadiene, etc. These olefins can be used alone or in combination of two or more kinds.
[0014] In the film constituting the innermost layer of the packaging material of the present invention, the content of the cyclic polyolefin resin based on the total resin components must be 60% by mass or more from the viewpoint of heat resistance and high rigidity when made into a laminate (packaging material). If the content is lower than this, it is difficult to obtain a laminate with excellent rigidity and heat resistance. A content of 65% by mass or more is particularly preferable. Examples of cyclic polyolefin-based films having a cyclic polyolefin-based resin content of 60% by mass or more based on the total resin components include films (hereinafter simply referred to as "COC") that are 100% by mass of cyclic polyolefin-based resin, films (single layer film form) made of a mixed resin containing cyclic polyolefin-based resin and other resins, such as polyolefin-based resins, or forms in which a cyclic polyolefin-based resin layer and other resin layers, such as a polyethylene resin layer, are laminated (such as a laminated film in which a polyethylene film is laminated on a cyclic polyolefin-based film) (hereinafter referred to as "special COC"). Of these, in the case of a special COC laminated film, the resin content may be adjusted by adjusting the thickness of the film, etc., so that the cyclic polyolefin-based resin is contained in an amount of 60% by mass or more based on the total resin components constituting the laminated film, and the cyclic polyolefin-based resin layer in the laminated film may be a resin layer containing 100% by mass of cyclic polyolefin-based resin, or a resin layer containing polyolefin-based resin, etc. Furthermore, among these, when using a special COC laminated film, it is preferable to use it so that the polyolefin resin layer is the innermost layer when made into a packaging material (i.e. the side facing the patch contained therein), as this provides a good feel when made into a packaging material, such as ease of use in terms of touch and ease of insertion and removal, excellent processability (manufacturability) in that the packaging material does not wrinkle when passing through the guide rolls of the packaging machine and slides smoothly, and excellent heat sealability in that high heat seal strength can be achieved.
[0015] The glass transition point (Tg) of the cyclic polyolefin resin is preferably 100°C or higher from the viewpoint of heat resistance and high rigidity of the resulting laminate (packaging material). From the viewpoint of co-extrusion in the production of the laminate and industrial availability of raw materials, the Tg is preferably 200°C or lower. Particularly preferably, it is 105°C to 180°C. As a cyclic polyolefin resin having such a Tg, the content ratio of the norbornene monomer is preferably in the range of 40 to 90% by mass, more preferably 50 to 90% by mass, and further preferably 60 to 85% by mass. If the content ratio is in this range, the heat resistance, rigidity, tearability, and processing stability of the laminate (packaging material) are improved. On the other hand, norbornene copolymers with a high glass transition point (Tg) have low tensile strength and can be extremely fragile or easily torn. Therefore, when taking into consideration the suitability for taking up and winding during film formation and slitting, it is possible to blend a high Tg product with a low Tg product having a glass transition point of less than 100°C. Furthermore, if the rigidity is too high and there are problems such as easy tearing or rupture when dropped during transportation, the drop strength can be improved by blending a cyclic polyolefin resin with a Tg of less than 100° C. It is also effective to blend other polyolefin resins that do not contain a cyclic structure, such as polypropylene resins or polyethylene resins, which have good compatibility with the cyclic polyolefin resins.
[0016] As commercially available products that can be used as the cyclic polyolefin resin, examples of ring-opening polymers (COP) of norbornene monomers include "ZEONOR" manufactured by Zeon Corporation, and examples of norbornene copolymers (COC) include "Apel" manufactured by Mitsui Chemicals, Inc. and "TOPAS" manufactured by Polyplastics Co., Ltd. Examples of cyclic polyolefin resin films (COC) include "COZEC" (registered trademark) manufactured by Kurabo Industries, Ltd., and examples of special COC films having a cyclic polyolefin resin layer and a polyolefin resin layer such as polyethylene include "DIFAREN" (registered trademark) MP film manufactured by DIC Corporation.
[0017] The thickness of the cyclic polyolefin resin film in the present invention is not particularly limited, but may be selected from the range of 5 μm to 50 μm, which is suitable for use as a packaging material, and for example, the range of 10 μm to 40 μm is used. In addition, when the cyclic polyolefin film containing 60% by mass or more of the cyclic polyolefin resin based on the total resin components is a film having a polyethylene resin layer on the innermost layer side, the polyethylene resin layer may be a layer containing a resin such as low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), etc., and LLDPE is preferred from the viewpoints of usability, manufacturability, heat sealability, etc. The thickness of the polyethylene resin layer in the laminated film is preferably 2 to 10 μm. This range is because it is excellent in usability, manufacturability, and heat sealability, and can suppress an increase in the amount of volatile drugs adsorbed due to an increase in thickness.
[0018] [Middle layer] <Uniaxially oriented polyolefin film> In the packaging material of the present invention, the intermediate layer (intermediate film) on the outer side of the innermost layer is provided with a uniaxially oriented polyolefin film. By using a uniaxially oriented polyolefin film as the intermediate layer, the packaging material can be given straight-line cutting properties. As the uniaxially stretched polyolefin-based film, a uniaxially stretched polyolefin-based film such as a uniaxially stretched polyethylene film (hereinafter sometimes abbreviated as "uniaxially stretched PE") or a uniaxially stretched polypropylene film (hereinafter sometimes abbreviated as "uniaxially stretched PP") can be used. Among them, the use of a uniaxially stretched polypropylene film as the uniaxially stretched polyolefin-based film is preferable because it improves tearability. The thickness of the uniaxially stretched polyolefin film of the present invention is not particularly limited, but can be selected from the range of 5 μm to 50 μm, which is suitable for use as a packaging material, for example, in the range of 10 μm to 40 μm or 15 μm to 30 μm.
[0019] <Other middle classes> In addition to the uniaxially stretched polyolefin film, one or more intermediate layers may be provided as necessary. The additional intermediate layer may be provided on either the outer layer side or the inner layer side of the uniaxially stretched polyolefin film. As the additional intermediate layer, metal foils such as aluminum, copper, magnesium, etc. can be used to provide gas barrier properties, and stretched films such as polyester, polyamide, polypropylene, etc. can be used to provide toughness. The thickness is preferably in the range of about 5 μm to 50 μm, for example.
[0020] [Outermost layer: a film selected from polyester, polyamide and polypropylene vapor-deposited with a metal or metal oxide] In the packaging material of the present invention, the film that is outside the intermediate layer and that constitutes the outermost layer (outermost layer) when the material is made into a bag is a film selected from polyester, polyamide, and polypropylene, on which a metal or metal oxide is vapor-deposited. By vapor-depositing the metal or metal oxide, it is possible to impart sealing properties such as water vapor barrier properties, oxygen barrier properties, and aroma barrier properties. In order to protect the deposition surface and prevent a decrease in the barrier properties, it is preferable to laminate the metal or metal oxide deposited surface facing the intermediate layer.
[0021] The polyester in the polyester film is a general term for polymers having ester bonds in the molecular chain obtained by condensation polymerization of polycarboxylic acid monomers and polyol monomers, and among these, linear polyesters obtained by condensation polymerization of dicarboxylic acids and diols are common. Dicarboxylic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid, alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, and aliphatic dicarboxylic acids such as adipic acid and sebacic acid. Diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,4-cyclohexanedimethanol. Specific examples of polyesters that can be used include polyethylene terephthalate, polytrimethylene terephthalate, polypropylene terephthalate, polyethylene isophthalate, polybutylene terephthalate, poly-1,4-cyclohexylene dimethylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate. Of these, polyethylene terephthalate (PET) is preferably used because of its balance of mechanical properties and heat resistance. As the polyamide of the polyamide film, polyamide (nylon) containing an aliphatic skeleton, such as nylon 6, can be used.
[0022] The polyester film used in the present invention may be biaxially stretched. The biaxially stretched polyester film is obtained by stretching an unstretched polyester coating about 2.5 to 5 times in each of the longitudinal and transverse directions, and then subjecting the film to heat treatment, thereby obtaining a film excellent in dimensional stability, mechanical strength, and flatness. Furthermore, when a biaxially oriented polyamide film or a biaxially oriented polypropylene film is used as the polyamide film or the polypropylene film, the unstretched polyamide coating or the polypropylene coating can be stretched about 3 to 5 times (polyamide) or 5 to 10 times (polypropylene) in the longitudinal and transverse directions, respectively, and then heat-treated to produce a film with excellent dimensional stability, mechanical strength, and flatness. In addition, various additives such as antioxidants, heat stabilizers, weather stabilizers, ultraviolet absorbers, organic lubricants, pigments, dyes, organic or inorganic particles, fillers, antistatic agents, nucleating agents, etc. may be added to the polyester film, polyamide film, and polypropylene film to the extent that they do not deteriorate the properties of the film.
[0023] The thickness of the polyester film, polyamide film and polypropylene film in the present invention is not particularly limited, but may be selected from the range of 1 μm to 100 μm, which is suitable for use as a packaging material, preferably from 2.5 μm to 75 μm, and more preferably from 5 to 50 μm.
[0024] The polyester film, polyamide film and polypropylene film in the present invention may be a composite film produced by coextrusion, and may have a coating layer provided on the surface according to various purposes. The coating layer may be, for example, a so-called in-line coating in which the biaxially oriented polyester film, polyamide film and polypropylene film are stretched in the longitudinal direction during film formation and then stretched in the width direction, or may be an off-line coating on the biaxially oriented polyester film, polyamide film and polypropylene film. Furthermore, the surface of the polyester film, polyamide film and polypropylene film may be subjected to a surface modification treatment such as corona discharge treatment, low pressure plasma treatment, normal pressure plasma treatment, flame treatment, ultraviolet irradiation, matte finish, etc.
[0025] In the present invention, a layer formed of a metal such as aluminum, copper, magnesium, etc. or a metal oxide such as silicon oxide (silica) or aluminum oxide (alumina), etc. is provided on a polyester film, a polyamide film, or a polypropylene film. When the contents are to be protected from light (when light-shielding properties are required as a packaging material) and gas barrier properties are required, a metal-deposited film is used, whereas when light-shielding properties are not particularly required but gas barrier properties are required, a metal-oxide-deposited film is used. The deposition of metal or metal oxide can be carried out by known methods such as vacuum deposition (resistance heating, high-frequency induction heating, electron beam heating), ion plating, sputtering, etc. Among them, the vacuum deposition is preferably used from the viewpoint of productivity. For example, a film deposited with metal or metal oxide can be produced by a continuous vacuum deposition method in which a long film such as polyester is continuously unwound from a roll on a feeding shaft in a vacuum device, metal or metal oxide is continuously deposited in a deposition area, and the film is taken up on a take-up shaft.
[0026] The thickness of the metal or metal oxide vapor-deposited layer of the film vapor-deposited with a metal or metal oxide in the present invention is determined by the film transport speed and the amount of evaporation. For example, the thickness of the layer vapor-deposited with a metal or metal oxide can be in the range of 10 nm to 80 nm, 15 nm to 70 nm, or 20 nm to 60 nm.
[0027] The method for producing the packaging material of the present invention is not particularly limited, and for example, a dry lamination method in which the films constituting each layer are laminated together using an adhesive, or an extrusion lamination method in which a molten resin is extruded from a T-die in the form of a film and laminated on a substrate, etc., can be used depending on the purpose. The packaging material of the present invention can have a three-layer laminate structure consisting of an innermost layer (a cyclic polyolefin film containing 60% or more by mass of cyclic polyolefin resin based on the total resin components), an intermediate layer (a uniaxially oriented polyolefin film), and an outermost layer (a film vapor-deposited with a metal or metal oxide and selected from polyester, polyamide, and polypropylene). As described above, in addition to the uniaxially stretched polyolefin film, one or more layers may be provided as the intermediate layer, i.e., a laminate structure such as innermost layer / intermediate layer A (uniaxially stretched polyolefin film) / intermediate layer B (other) / outermost layer, innermost layer / intermediate layer B (other) / intermediate layer A (uniaxially stretched polyolefin film) / outermost layer, or innermost layer / intermediate layer B (other) / intermediate layer A (uniaxially stretched polyolefin film) / intermediate layer B (other) / outermost layer can be used. Here, the intermediate layer B (other) can be a metal foil or stretched film listed in the above <other intermediate layers>, and the intermediate layer B can be composed of one layer or two or more layers.
[0028] [Patches] The patch containing a volatile pharmacologically active ingredient (hereinafter, simply referred to as a patch) contained in the packaging material of the present invention will be described in detail below. The configuration of the patch is not particularly limited, and an example of the configuration includes a support, an adhesive layer containing a volatile pharmacologically active ingredient provided on at least one surface of the support, and a release liner (also referred to as a release sheet) provided on the adhesive layer.
[0029] The shape of the above-mentioned patch, particularly the preparation portion consisting of the support and the adhesive layer provided on the support, is not particularly limited, and various shapes can be selected according to the application site, such as a rectangle (square, rectangle, etc.), quadrilateral (trapezoid, rhombus, etc.), polygon, circle, ellipse, semicircle, triangle, crescent, and combinations of these. The area of the patch (particularly the above-mentioned preparation portion) can be appropriately determined, for example, in consideration of the amount of active ingredient to be blended in the adhesive layer, and is, for example, 2 to 300 cm. 2 The range may be:
[0030] [Support] Examples of the backing used in the above-mentioned patch include flexible backings such as films, nonwoven fabrics, Japanese paper, cotton fabrics, knitted fabrics, woven fabrics, and laminated composites of nonwoven fabrics and films. These supports are preferably made of a material that can adhere closely to the skin, is flexible enough to follow the movement of the skin, and can suppress the occurrence of skin rashes, etc. after long-term application. Examples of the material for these supports include polyethylene, polypropylene, polyethylene terephthalate, etc. The size of the support is not particularly limited and can be appropriately selected depending on the purpose.
[0031] [Adhesive layer] In the above patch, the adhesive constituting the adhesive layer is not particularly limited, and examples thereof include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, hydrocolloid-based adhesives, etc. These adhesives may be used alone or in combination of two or more. The adhesive layer may have a single-layer structure or a multi-layer structure. When the adhesive layer has a multi-layer structure, the volatile pharmacologically active ingredient may be contained in at least one of the layers. As a preferred embodiment, the adhesive layer may be made of a rubber-based adhesive. The rubber-based adhesive generally contains a rubber-based elastomer, a tackifier, and a softener, and may contain other components as necessary. An example of a patch using a rubber-based adhesive is shown below.
[0032] The volatile pharmacologically active ingredients include, for example, methyl salicylate, glycol salicylate, l-menthol and dl-camphor. These may be used alone or in combination of two or more. The content of the volatile pharmacologically active ingredient in the adhesive layer can be, for example, 0.1% by mass to 30% by mass, 0.2% by mass to 20% by mass, or 0.5% by mass to 15% by mass, when the total mass of the adhesive layer is 100% by mass.
[0033] The rubber-based elastomer is not particularly limited and can be appropriately selected according to the purpose. For example, various thermoplastic elastomers can be applied, such as styrene-isoprene-styrene copolymer (hereinafter sometimes referred to as "SIS"), styrene-butadiene-styrene copolymer (hereinafter sometimes referred to as "SBS"), or hydrogenated products thereof, thermoplastic block copolymers such as styrene-ethylene-propylene-styrene copolymer (hereinafter sometimes referred to as "SEPS"), and styrene-ethylene-butylene-styrene copolymer (hereinafter sometimes referred to as "SEBS"); ethylene-vinyl acetate copolymer; and ethylene-α-olefin copolymer. Among these, styrene-based thermoplastic elastomers, which are thermoplastic block copolymers such as SIS, SBS, SEPS, and SEBS, are preferably used because of their excellent adhesion and cohesiveness. Among these, SIS is particularly preferred from the viewpoints of adhesion to human skin and compatibility with other components, and examples thereof include commercially available products such as SIS5002 (manufactured by JSR Corporation) and Quintac 3520 (manufactured by Zeon Corporation). The elastomers may be used alone or in combination of two or more kinds. The content of the elastomer in the pressure-sensitive adhesive layer can be appropriately selected depending on the purpose, and can be, for example, 10% by mass to 60% by mass, 15% by mass to 50% by mass, 15% by mass to 40% by mass, etc., when the total mass of the pressure-sensitive adhesive layer is 100% by mass.
[0034] The tackifier is not particularly limited as long as it improves adhesion, and examples thereof include rosin resins, terpene resins, coumarone-indene resins, petroleum resins (C5 petroleum resins, C9 petroleum resins), alicyclic petroleum resins, alicyclic hydrogenated petroleum resins, styrene resins, dicyclopentadiene resins, etc. Among these, it is preferable to contain one or more tackifiers selected from terpene resins and rosin resins. Examples of the terpene resin include β-pinene resin, α-pinene resin, terpene-phenol resin, aromatic modified terpene resin, and hydrogenated terpene resin. Examples of the rosin resin include rosins such as gum rosin, tall oil rosin, and wood rosin; modified rosins such as hydrogenated rosin, disproportionated rosin, polymerized rosin, and maleated rosin; and rosin esters such as rosin glycerin ester, hydrogenated rosin ester, and hydrogenated rosin glycerin ester. Examples of the tackifier include YS Resin PX1150N (manufactured by Yasuhara Chemical Co., Ltd.), which is a terpene resin, and Pine Crystal KE-311 (manufactured by Arakawa Chemical Industries, Ltd.), which is a hydrogenated rosin glycerin ester. The tackifier may be used alone or in combination of two or more kinds. Also, a tackifier selected from the terpene resin and the rosin resin may be used in combination. The content of the tackifier in the adhesive layer is not particularly limited and can be selected appropriately depending on the purpose, but can be, for example, 10% by mass to 60% by mass, or 15% by mass to 50% by mass, when the total mass of the adhesive layer is 100% by mass.
[0035] Examples of the softener (plasticizer) include petroleum-based softeners such as liquid paraffin; liquid rubber-based softeners such as liquid polyisoprene, polybutene, and polyisobutylene; dibasic acid ester-based plasticizers such as phthalates and adipates; and other plasticizers such as polyethylene glycol and citrates. Among them, liquid paraffin is preferably used because it has excellent compatibility with rubber-based elastomers and does not reduce the cohesive force. For example, commercially available products include Hicol (registered trademark, liquid paraffin manufactured by Kaneda Co., Ltd.) M series. From the viewpoint of adhesiveness, the content of these softeners is preferably in the range of 25% by mass to 55% by mass, and more preferably 30% by mass to 50% by mass, when the total mass of the adhesive layer is 100% by mass.
[0036] If necessary, the rubber-based adhesive may further contain additives that are usually blended in the adhesive layer of a transdermal preparation, such as antioxidants, fillers, percutaneous absorption promoters, pigments, stabilizers, solubility enhancers, solubility inhibitors, etc. These additives may be used alone or in combination of two or more.
[0037] The average thickness of the pressure-sensitive adhesive layer can be appropriately selected depending on the purpose, but is preferably from 5 μm to 500 μm, more preferably from 10 μm to 300 μm, and even more preferably from 20 μm to 200 μm.
[0038] [Release liner] The release liner used in the above-mentioned patch is preferably made of a material that is unlikely to absorb or adsorb volatile pharmacologically active ingredients in the adhesive layer, and any material commonly used in the technical field of patches can be used. Examples of the material include plastic films such as polyester (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polypropylene (unstretched, stretched, etc.), polyethylene, polyurethane, polyvinyl chloride, polystyrene, etc.; paper and synthetic paper such as fine paper, glassine paper, parchment paper, and craft paper; release-processed paper obtained by coating the above-mentioned plastic films, paper, synthetic paper, synthetic fibers, etc. with a release agent having release properties such as silicone resin or fluororesin; aluminum foil; laminated paper obtained by laminating these films and sheets in various layers, and laminated release-processed paper obtained by coating the laminated paper with a release agent, etc., and other colorless or colored sheets. The release liner can also be provided with irregularities to make it easier to remove from the packaging material. The thickness of these release liners is not particularly limited, but is usually in the range of 10 μm to 1 mm, for example, 20 μm to 500 μm, and preferably 40 μm to 200 μm. The shape of the release liner can be square, rectangular, circular, etc., and can be rounded if desired. Its size can be the same as the size of the support in the patch or slightly larger. The release liner can be composed of one sheet or multiple sheets divided into two or more sheets, and the cuts can be straight, wavy, or perforated, and the release liners can be partially overlapped with each other.
[0039] [Method of manufacturing patch] The method for producing the above-mentioned patch is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method include a method in which a pressure-sensitive adhesive composition containing an elastomer, a tackifier, a volatile pharmacologically active ingredient, and optionally other ingredients is prepared and then coated onto a support, and a method in which a release liner is coated and then a support is attached.
[0040] According to the present invention, by adopting a cyclic polyolefin resin film containing 60% by mass or more of cyclic polyolefin resin based on the total resin components as the innermost layer of the packaging material when made into a bag shape, or a film having a polyethylene resin layer on the innermost layer side of the film [COC or special COC], the adsorption of volatile pharmacologically active ingredients (methyl salicylate, l-menthol, dl-camphor) can be suppressed. Furthermore, when the special COC is used as the cyclic polyolefin resin film to make a bag shape, not only is the usability (touch, ease of putting contents in and taking them out, occurrence of wrinkles and folds) improved, but manufacturability (sealability, stiffness, slippage) can also be improved. Furthermore, by laminating a uniaxially oriented polyolefin film as an intermediate layer, the linearity of the cut portion when the sheet is cut by hand can be improved. In addition, by laminating a film such as polyester on which a metal or metal oxide is vapor-deposited as the outermost layer, excellent airtightness can be achieved. EXAMPLES
[0041] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0042] Using the formulation shown in Table 1, the patches used in the Examples and Comparative Examples were manufactured according to the following procedures. <Paste stirring process> Styrene-isoprene-styrene block copolymer, terpene resin, hydrogenated rosin glycerin ester, dibutylhydroxytoluene and liquid paraffin were added to a Henschel mixer and stirred at 160℃ and 100-300 rpm for 80 minutes to obtain a uniform paste.The active ingredients methyl salicylate, l-menthol and dl-camphor were then added and stirred at 160℃ and 200 rpm for 10 minutes to obtain a uniform paste containing the active ingredients.
[0043] [Table 1]
[0044] <Coating process> The active ingredient-containing paste obtained in the mixing process was applied in a coating amount of 150 g / m using a die coater (head temperature 165°C, coating speed 15 m / min). 2 The mixture was applied to a polyethylene terephthalate liner (thickness 75 μm) and then to a polyester support (basis weight 120 g / m 2 ) was attached to obtain a coated product in which the active ingredient-containing paste was evenly coated between the support and the liner.
[0045] <Cutting process> The coated product obtained in the coating step was cut into a predetermined shape using a die roll cutter to obtain a patch.
[0046] Six of the obtained patches were piled up to form a pile, which was then packaged in the packaging material shown in the following Examples or Comparative Examples using a packaging machine to obtain a packaged product.
[0047] [Example 1] When the bag was formed, the cyclic polyolefin film (special COC) (DIC Corporation's "DIFAREN" (registered trademark) MP film M3400MP, thickness 30 μm (cross-sectional observation showed that the cyclic polyolefin resin layer was 21 μm and the polyethylene resin layer was 9 μm)) was arranged as the innermost layer so that the polyethylene resin layer of the cyclic polyolefin film was the innermost layer (innermost layer side), and the intermediate layer was a uniaxially oriented polypropylene film (uniaxially oriented PP, Tokyo Ink Co., Ltd.'s "Noblen", thickness 20 μm), and the outermost layer was a polyethylene terephthalate film vapor-deposited with aluminum oxide (AL2O3 vapor-deposited PET, Toray Film Processing Co., Ltd.'s "Barrierox", thickness 12 μm, the vapor-deposited surface facing the intermediate layer side (same below)) in that order, and a laminate was obtained. Each layer was laminated by the dry lamination (DL) method using an adhesive. The obtained laminate was used as a packaging material and the above-mentioned accumulation was packaged as the contents to obtain a package.
[0048] [Example 2] A package was obtained in the same manner as in Example 1, except that the innermost cyclic polyolefin film (special COC) in Example 1 was changed to a COC film (COC) (Kuraray Industries, Inc.'s "COZEC" (registered trademark), thickness 30 μm).
[0049] [Example 3] A package was obtained in the same manner as in Example 2, except that the intermediate layer in Example 2 was changed to a uniaxially oriented polyethylene film (uniaxially oriented PE, thickness 20 μm).
[0050] [Comparative Example 1] A package was obtained in the same manner as in Example 1, except that when the packaging material was made into a bag shape, the innermost layer was changed to a linear low-density polyethylene film (LLDPE, thickness 40 μm) and the middle layer was changed to a biaxially oriented PET film (PET, "Toyobo Ester" (registered trademark) manufactured by Toyobo Co., Ltd., thickness 12 μm).
[0051] [Comparative Example 2] A package was obtained in the same manner as in Example 2, except that the uniaxially oriented polypropylene film in the middle layer in Example 2 was changed to a biaxially oriented PET film (PET, Toyobo Ester (registered trademark) manufactured by Toyobo Co., Ltd., thickness 12 μm).
[0052] [Comparative Example 3] A package was obtained in the same manner as in Example 1, except that the uniaxially oriented polypropylene film in the middle layer in Example 1 was changed to a biaxially oriented PET film (PET, Toyobo Ester (registered trademark) manufactured by Toyobo Co., Ltd., thickness 12 μm).
[0053] The configurations of the packaging materials used in the Examples and Comparative Examples are shown below. [Table 2]
[0054] <Test Example 1 Drug Adsorption> The packages produced in Examples 1 and 2, Comparative Example 1, and Comparative Example 3 were stored at 60°C. Immediately after storage at room temperature and after a certain period of time (1 week (1W), 1 month (1M)), the packaging material was cut after removing the contents from the package, and the three active ingredients were extracted with tetrahydrofuran, and the content of the active ingredients was measured using the liquid chromatography method (HPLC method) of the general test method of the 17th revised Japanese Pharmacopoeia. In addition, the same test was performed on the packaging material immediately after storage (24 hours later), and the initial drug adsorption amount was recorded. Note that, since the innermost layer of Example 3 and Comparative Example 2 is a COC film like Example 2, it can be evaluated that the drug adsorption amount in these packages is equivalent to that of Example 2. The results obtained are shown in Table 3.
[0055] [Table 3]
[0056] As shown in Table 3, the adsorption amounts of the three active ingredients (l-menthol, dl-camphor and methyl salicylate) were almost the same in Example 1 (innermost layer: special COC film), Example 2 (innermost layer: COC film) and Comparative Example 3 (innermost layer: special COC film), but were more than twice as high in Comparative Example 1 (innermost layer: LLDPE film). From the above results, it was confirmed that by using a special COC film or COC film as the innermost layer, the adsorption of three volatile active ingredients (l-menthol, dl-camphor, and methyl salicylate) to the packaging material can be suppressed. In the "Overall Evaluation" described below, the results of this test were evaluated as "drug adsorption" according to the following criteria, and are shown in Table 5. A: The total amount of drug adsorption (3 types) after 1 month at 60℃ is less than 20mg C: The total amount of drug adsorption (3 types) after 1 month at 60℃ is 20mg or more
[0057] <Test Example 2 Heat sealability> The packaging materials used in the packages of Example 1, Example 2, Comparative Example 1, and Comparative Example 3 were overlapped with the innermost layer (special COC film or COC film) on the inside, and each sample was heat-sealed at a sealing pressure of 0.2 MPa, a sealing time of 1 second, and a heat-sealing temperature of 110°C to 200°C, and then the heat-seal strength was measured in accordance with JIS Z 0238. The results are shown in Table 4. Note that, since the innermost layer of Example 3 and Comparative Example 2 is a COC film like Example 2, the heat-sealability of these packages can be evaluated to be equivalent to that of Example 2.
[0058] [Table 4]
[0059] As shown in Table 4, the heat seal strengths of the packaging materials of Example 1 and Comparative Example 3, in which the innermost layer was a special COC film, and the packaging material of Comparative Example 1, in which the innermost layer was an LLDPE film, were 15 N / 15 mm or more at a heat seal temperature of 130°C or more, and the heat seal strength of Example 2, in which a COC film was used, was 8 N / 15 mm or more at a heat seal temperature of 130°C or more. In the case of general packaging bags, etc., when the mass of the contents is large and a somewhat strong heat seal strength is required, and in the case of general packaging bags, etc., when the mass of the contents is small and an ordinary heat seal strength is required, the reference heat seal strength guidelines are described as 15N / 15mm or more and 6N / 15mm or more (JIS Z 0238: Test method for heat-sealed flexible packaging bags and semi-rigid containers), respectively. From the above results, it was found that Example 1 (special COC), Example 2 (COC), Comparative Example 1 (LLDPE), and Comparative Example 3 (special COC) had ordinary heat seal strength or higher. Furthermore, Example 1, Comparative Example 1, and Comparative Example 3 had somewhat strong heat seal strength. In the later-described "Overall Evaluation", the results of this test were evaluated as "heat sealability" according to the following criteria. The evaluation results are also shown in Table 5. A: Maximum heat seal strength is 15N / 15mm or more B: Maximum heat seal strength is 6N / 15mm or more - less than 15N / 15mm C: Maximum heat seal strength is less than 6N / 15mm
[0060] <Test Example 3: Usability> The packages of Examples 1 to 3 and Comparative Examples 1 to 3 were visually observed for feel when held in the hand and when the contents were taken in and out of each package 10 times, and for change in appearance (creases and folds) after taking in and out the contents 10 times, and were evaluated as usability according to the following criteria. The results are shown in Table 5. A: It feels great to the touch when you hold it or insert or remove it (it doesn't feel hard), and there are almost no wrinkles or creases on the exterior after inserting or removing it. B: It feels slightly better to the touch when you hold it or insert or remove it (it feels a little stiff), and there are fewer wrinkles or creases on the appearance after inserting or removing it. C: The touch is bad when held (it feels hard), and wrinkles and creases are noticeable on the exterior after insertion and removal.
[0061] <Test Example 4: Straightness during cutting> The packages of Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to a cutting test in which a cut was made in a part of the package and the package was torn from the cut, and the package was evaluated according to the following criteria. The obtained results are shown in Table 5. A: When it was cut, it was straight. B: When cut, it was straight, but the appearance was slightly poor. C: When cut, the linearity was slightly poor. D: When cut, the linearity was clearly poor.
[0062] <Test Example 5: Manufacturability> In order to evaluate the operability (ease of handling) of the packaging material during packaging for the packages of Examples 1 to 3 and Comparative Examples 1 to 3, the presence or absence of wrinkles in the packaging material that occurred when passing through the guide rolls of the packaging machine was visually observed and evaluated according to the following criteria. The results are shown in Table 5. A: When packaging, the packaging material was smooth and there were almost no wrinkles. B: When packaging, the packaging material was slightly difficult to slide and some wrinkles occurred. C: When packaging, the packaging material did not slide well and wrinkles occurred.
[0063] [Table 5]
[0064] <Results and Discussion> As described above, the drug adsorption properties were good for the innermost layers of the special COC (Example 1 and Comparative Example 3) film and the COC (Example 2) film, but were clearly poor for the LLDPE (Comparative Example 1). The linearity at the time of cutting was good when uniaxially oriented PP (Example 1, Example 2) film was used for the intermediate layer. However, when uniaxially oriented PE (Example 3) or PET (Comparative Example 1, Comparative Example 2, Comparative Example 3) film was used for the intermediate layer, the linearity at the time of cutting was poor. Furthermore, in the cut part of the package using uniaxially oriented PE (Example 3) film for the intermediate layer, thin thread-like film pieces that were not observed when uniaxially oriented PP (Example 1, Example 2) film was used for the intermediate layer were slightly observed, and the appearance of the cut part was somewhat poor. In addition, the usability evaluated by the feel and appearance such as wrinkles after repeated use was rated as good in the packaging materials in which the innermost layer was a special COC (Example 1, Comparative Example 3) film and LLDPE (Comparative Example 1) film, even when the middle layer was a PET film. Note that, Examples 2 and 3, in which the innermost layer was a COC film, were somewhat inferior in usability compared to Example 1, but were able to ensure a usability that was fully applicable for practical use. On the other hand, Comparative Example 2, in which the innermost layer was a COC film and the middle layer was a PET film, was clearly inferior in usability. Regarding manufacturability, packaging materials in which the innermost layer was special COC (Example 1, Comparative Example 3) and LLDPE (Comparative Example 1) showed good results regardless of the type of intermediate layer, and while Examples 2 and 3, in which the innermost layer was COC film, were somewhat inferior in manufacturability compared to Example 1, they were able to ensure manufacturability that was hardly a problem in actual manufacturing sites. On the other hand, Comparative Example 2, in which the innermost layer was COC film and the intermediate layer was PET film, showed clearly inferior manufacturability. As for heat sealability, Example 1 (special COC), Example 2 (COC), Comparative Example 1 (LLDPE) and Comparative Example 3 (special COC) all had a strength equal to or greater than normal heat seal strength. Furthermore, Example 1, Comparative Example 1 and Comparative Example 3 had slightly strong heat seal strength. From the above results, it was confirmed that the packaging material which suppresses drug adsorption and has excellent straightness when cut is a laminate (Example 1, Example 2) which uses special COC or COC as the innermost layer, uniaxially oriented PP as the middle layer, and PET on which metal or metal oxide is vapor-deposited as the outermost layer. Furthermore, it was confirmed that the packaging material which suppresses drug adsorption, has excellent straightness when cut, and also has high usability, manufacturability, heat seal strength, and excellent sealability is a laminate (Example 1) which uses special COC as the innermost layer, uniaxially oriented PP as the middle layer, and PET on which metal or metal oxide is vapor-deposited as the outermost layer.
Claims
1. A bag-shaped packaging material containing a patch containing a volatile pharmacologically active ingredient as a content, The packaging material is a laminated film having an innermost layer on the patch side, the innermost layer being a cyclic polyolefin resin layer made of 100% by mass of a cyclic polyolefin resin, and a polyethylene resin layer made of 100% by mass of a polyethylene resin on the surface of the innermost layer that comes into contact with the contents, the laminated film containing 60% by mass or more of a cyclic polyolefin resin based on the total resin content of the laminated film; a uniaxially oriented polypropylene film which is an intermediate layer adjacent to the outer side of the innermost layer; and a polyethylene terephthalate film having a metal oxide vapor-deposited thereon, which is an outermost layer adjacent to the outer side of the intermediate layer. The surface of the outermost layer on which the metal oxide is deposited faces the intermediate layer. packaging material.
2. 2. The packaging material according to claim 1, wherein the volatile pharmacologically active ingredient is one or more selected from the group consisting of methyl salicylate, glycol salicylate, l-menthol, and dl-camphor.
3. 3. The packaging material according to claim 1, wherein the cyclic polyolefin resin is at least one resin selected from the group consisting of norbornene polymers, vinyl alicyclic hydrocarbon polymers, and cyclic conjugated diene polymers.
4. The packaging material according to claim 1 , wherein the polyethylene resin layer is at least one resin layer selected from the group consisting of low density polyethylene, linear low density polyethylene, medium density polyethylene, and high density polyethylene.
Citation Information
Patent Citations
Laminate for suppressing adhesion of 1-menthol
JP1996143452A
Transparent moistureproof package having cleanness
JP2001171045A
Low adsorption sealant substrate and low adsorption package using the substrate
JP2005144879A
Packaging pouch for accommodating adhesive preparation and package for adhesive preparation
JP2005328928A
Unadsorbable heat-sealing composition, unadsorbable packing material, and unadsorbable packaging bag
JP2012184357A