Airtight Terminal
The airtight terminal design with a curved ceramic substrate surface addresses easy wiring and airtightness issues by optimizing brazing contact area, enhancing bonding strength and airtightness.
Patent Information
- Application Number
- JP2023551627
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-29
- Filing Date
- 2022-09-28
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2042-09-28
AI Technical Summary
Existing airtight terminals face challenges in ensuring easy wiring connections and preventing gaps that compromise joint strength and airtightness due to variations in the distance between the inner and outer circumferential surfaces of the washer and lead pin.
The airtight terminal design incorporates a ceramic substrate with a curved inner surface on the annular member to increase the contact area for brazing, enhancing bonding strength and airtightness by optimizing the curvature and distribution of brazing material.
This design facilitates easy wiring connections and improves joint strength and airtightness by minimizing gaps and ensuring robust bonding between the annular member and conductive member, even under impact or thermal stress.
Smart Images

Figure 0007583954000001 
Figure 0007583954000002 
Figure 0007583954000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a hermetic terminal. [Background technology]
[0002] Conventionally, in vacuum pumps such as turbomolecular pumps, airtight terminals are used to supply electrical signals from the outside of the vacuum pump to the inside, which is a vacuum space. Such airtight terminals generally include a cylindrical metal sleeve, a disk-shaped insulating base having a through hole in the axial direction and brazed to the inner peripheral surface of the metal sleeve, and a lead pin (conductive member) having a washer (annular member) fixed in the through hole.
[0003] For example, Patent Document 1 describes an airtight terminal in which a metal layer (metallized layer) is formed on the periphery of a through hole in an insulating base and on the inner surface of the through hole to a depth of 200 μm to 5 mm from the opening of the through hole. A washer and a lead pin are fixed to this metal layer by brazing. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-16620 Summary of the Invention [Means for solving the problem]
[0005] The hermetic terminal according to the present disclosure includes a cylindrical metal sleeve, a ceramic substrate fixed to an inner peripheral surface of the metal sleeve and having a first through hole along the axial direction of the metal sleeve, an annular member having a second through hole coaxially positioned with the first through hole, and a columnar conductive member inserted into the first through hole and the second through hole and brazed to the ceramic substrate and the annular member. The inner peripheral surface of the annular member facing the conductive member has a first region that curves in a direction away from the conductive member. The vacuum pump according to the present disclosure includes this hermetic terminal. [Brief description of the drawings]
[0006] [Figure 1] FIG. 2 is a plan view showing a hermetic terminal according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is an explanatory diagram for illustrating a cross section taken along line XX shown in FIG. [Diagram 3] 3 is an enlarged explanatory view for explaining a region Y shown in FIG. 2. FIG. [Figure 4] 3 is an enlarged explanatory view for explaining another embodiment of the region Y shown in FIG. 2.
[0023] FIG. [Diagram 5] 3 is an enlarged explanatory view for explaining another embodiment of the region Y shown in FIG. 2.
[0023] FIG. [Figure 6] 3 is an enlarged explanatory view for explaining another embodiment of the region Y shown in FIG. 2.
[0023] FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] As described above, when the washer and the lead pin are fixed to the metal layer by brazing, if the straightness of the inner peripheral surface of the washer is small and the gap between the inner peripheral surface of the washer and the outer peripheral surface of the lead pin is wide, the lead pin may be fixed at an angle to the insulating base. In such a case, the wiring work to connect to the tip of the lead pin may be difficult. On the other hand, if the gap between the inner peripheral surface of the washer and the outer peripheral surface of the lead pin is narrow, it is not possible to flow a sufficient amount of brazing material between the inner peripheral surface of the washer and the outer peripheral surface of the lead pin. As a result, many gaps may remain between the inner peripheral surface of the washer and the outer peripheral surface of the lead pin, resulting in poor joint strength and airtightness.
[0008] An object of the present disclosure is to provide an airtight terminal that facilitates wiring work to be connected to the tip of a lead pin and that suppresses gaps that may occur between the inner and outer circumferential surfaces.
[0009] As described above, in the hermetic terminal according to the present disclosure, the inner peripheral surface of the annular member facing the conductive member has a first region that curves toward the outer peripheral surface. With this structure, the contact area of the brazing material with the inner peripheral surface of the annular member can be increased. Therefore, the hermetic terminal according to the present disclosure facilitates wiring to be connected to the tip of the lead pin, and suppresses voids that may occur between the inner peripheral surface and the outer peripheral surface.
[0010] A hermetic terminal according to one embodiment of the present disclosure will be described with reference to Figures 1 to 3. The hermetic terminal 1 according to one embodiment shown in Figure 1 includes a metal sleeve 2, a ceramic substrate 3, and a conductive member 4. Figure 1 is a plan view showing the hermetic terminal 1 according to one embodiment.
[0011] The metal sleeve 2 has a tubular shape, and the shape is not limited, and may be a cylindrical shape or a rectangular shape (e.g., a triangular shape, a rectangular shape, a pentagonal shape, a hexagonal shape, etc.) as long as it is a cylindrical shape. The size of the metal sleeve 2 may be appropriately set according to the device equipped with the airtight terminal 1. The length of the metal sleeve 2 is, for example, 15 mm or more and 30 mm or less, and the outer diameter of the outermost circumference is 20 mm or more and 30 mm or less. In the case of a rectangular tube shape, the outer diameter means the length of the longest outer edge. The metal sleeve 2 is formed of a metal such as carbon steel, low alloy steel, tool steel, stainless steel, iron, copper, copper alloy, titanium, titanium alloy, molybdenum, molybdenum alloy, Fe-Ni alloy, Fe-Ni-Cr-Ti-Al alloy, Fe-Cr-Al alloy, Fe-Co-Cr alloy, Fe-Co-based alloy, Fe-Co-C-based alloy, Fe-Ni-based alloy, or Fe-Ni-Co-based alloy.
[0012] Carbon steel is an alloy of Fe and 0.02 to 2.14 mass% C, and contains Si, Mn, P, and S in addition to C. Examples of such carbon steel include S10C, S12C, S15C, S17C, S20C, S22C, S25C, S28C, S30C, S33C, S35C, S38C, S40C, S43C, S45C, S48C, S50C, S53C, S55C, S58C, S60C, S65C, S70C, and S75C, which are specified in JIS G 4051:2016.
[0013] Low alloy steel refers to carbon steel that contains at least one of Al, B, Co, Cr, Cu, La, Mo, Nb, Ni, Pb, Se, Te, Ti, V, W, and Zr, and the total content of these elements is 5 mass% or less.
[0014] Tool steel refers to carbon tool steel as specified in JIS G 4401:2009 and alloy tool steel as specified in JIS G 4404:2006.
[0015] Stainless steel is an alloy of Fe and 10.5 mass% or more of Cr with a C content of 1.2% or less, and other components are specified, for example, in ISO 15510: 2014. Examples of stainless steel include SUS304, SUS304L, SUS304ULC, SUS310ULC, and SUSXM15J1.
[0016] The ceramic substrate 3 is a member for fixing the conductive member 4, which will be described later, inside the metal sleeve 2. As shown in Figs. 1 and 2, the ceramic substrate 3 is fixed between the outer peripheral surface of the ceramic substrate 3 and the inner wall surface of the metal sleeve 2. That is, the ceramic substrate 3 is formed according to the inner diameter of the metal sleeve 2. The thickness of the ceramic substrate 3 may be any thickness that allows the conductive member 4 to be fixed, and is, for example, 4 mm or more and 10 mm or less. Fig. 2 is an explanatory diagram for explaining a cross section when cut along the XX line shown in Fig. 1.
[0017] There are no limitations on the ceramic substrate 3 as long as it is made of ceramics. Examples of such ceramics include ceramics containing aluminum oxide, aluminum nitride, silicon carbide, or silicon nitride as a main component.
[0018] In this specification, the term "main component" refers to a component that occupies 80% by mass or more of the total 100% by mass of the components that make up the ceramic. Each component contained in the ceramic can be identified by an X-ray diffraction device using CuKα radiation, and the content of each component can be determined, for example, by an ICP (Inductively Coupled Plasma) emission spectrometer or a fluorescent X-ray analyzer.
[0019] The ceramic substrate 3 has a first through hole 3a along the axial direction of the metal sleeve 2. The first through hole 3a is a through hole for inserting a conductive member 4, and the diameter of the first through hole 3a is set appropriately depending on the outer diameter of the conductive member 4. It is sufficient that at least one first through hole 3a is formed in the ceramic substrate 3, and the diameter is set appropriately depending on the number of conductive members 4 to be inserted.
[0020] As shown in Fig. 2, an annular member 5 is positioned on the surface of the ceramic substrate 3. The annular member 5 corresponds to a washer, and is formed of a metal such as carbon steel, low alloy steel, tool steel, stainless steel, iron, copper, copper alloy, titanium, titanium alloy, molybdenum, molybdenum alloy, Fe-Ni alloy, Fe-Ni-Cr-Ti-Al alloy, Fe-Cr-Al alloy, Fe-Co-Cr alloy, Fe-Co based alloy, Fe-Co-C based alloy, Fe-Ni based alloy, or Fe-Ni-Co based alloy. The definitions of carbon steel, low alloy steel, tool steel, and stainless steel are as described above.
[0021] There are no limitations on the size of the annular member 5 as long as it is smaller than the width and thickness of the ceramic substrate 3 and has a size that allows the conductive member 4 to be inserted therein. Regarding the size of the annular member 5, for example, the outer diameter of the annular member 5 is about 1.2 to 2 times, and particularly preferably 1.4 to 1.8 times, the outer diameter of the conductive member 4. The thickness of the annular member 5 is about 0.1 mm to 0.5 mm.
[0022] The annular member 5 has a second through hole 5a located coaxially with the first through hole 3a formed in the ceramic substrate 3. The second through hole 5a is a through hole for inserting the conductive member 4, and the diameter of the second through hole 5a is set appropriately depending on the outer diameter of the conductive member 4.
[0023] The conductive member 4 corresponds to a lead pin, and the shape is not limited as long as it has a columnar shape such as a cylindrical shape or a rectangular shape (e.g., a triangular prism, a square prism, a pentagonal prism, a hexagonal prism, etc.). The length and the outer diameter of the conductive member 4 are appropriately set according to, for example, the size of the metal sleeve 2. The conductive member 4 is formed of a metal such as copper or oxygen-free copper (e.g., alloy number C1020 specified in JIS H 3100:2012 or alloy number C1011 specified in JIS H 3510:2012). At least one conductive member 4 may be included, and may be appropriately set according to the use of the airtight terminal 1, etc.
[0024] The conductive member 4 is inserted into a first through hole 3a formed in the ceramic substrate 3 and a second through hole 5a formed in the annular member 5, and is fixed to the ceramic substrate 3. Specifically, the conductive member 4 is brazed to the surface of the ceramic substrate 3 using a brazing material 6 so as to cover the annular member 5. Examples of the brazing material 6 include Ag-Cu-Ti brazing material, BAg-8, BAg-8A, BAg-8B, and BAg-9. The Ag-Cu-Ti brazing material is, for example, 35 to 50 mass% Cu, 1 to 8 mass% Ti, and the remainder silver (Ag) out of a total of 100 mass% Ag, Cu, and Ti.
[0025] As shown in Fig. 3, the annular member 5 in the airtight terminal 1 has a first region 51 in which the inner peripheral surface facing the conductive member 4 curves toward the outer peripheral surface. Fig. 3 is an enlarged explanatory view for explaining the region Y shown in Fig. 2. By having the annular member 5 have such a first region 51, the contact area of the brazing material 6 with the inner peripheral surface of the annular member 5 can be increased. As a result, the airtightness and the bonding strength of the annular member 5 to the conductive member 4 can be improved.
[0026] The first region 51 may be present in only one location on the inner peripheral surface of the annular member 5, or may be present in multiple locations. By having multiple first regions 51 on the inner peripheral surface of the annular member 5, the contact area of the brazing material 6 with the inner peripheral surface of the annular member 5 can be increased. As a result, the airtightness and the bonding strength of the annular member 5 with the conductive member 4 can be further improved.
[0027] The curvature of the first region 51 is not limited, and may be, for example, 0.6 (1 / mm) or more. When there are multiple first regions 51, it is preferable that each of the first regions 51 has a curvature of 0.6 (1 / mm) or more. When the curvature of the first region 51 is 0.6 (1 / mm) or more, the contact area of the brazing material 6 with the inner peripheral surface of the annular member 5 can be further increased. As a result, the airtightness and the bonding strength of the annular member 5 with the conductive member 4 can be further improved. The upper limit of the curvature of the first region 51 may be, for example, 1.2 (1 / mm).
[0028] To find the curvature of the first region 51, first, a scanning electron microscope is used to photograph the entire annular member 5, focusing on a cross section including the axis of the conductive member 4. The curvature of the first region 51 can be found by tracing the inner peripheral surface of the annular member 5 displayed in the photographed image. The magnification of the image is, for example, 35 times, but the magnification can be adjusted appropriately so that the entire annular member 5 is photographed.
[0029] In order to fix the annular member 5 for a long period of time, it is preferable that the brazing portion sandwiched between the inner peripheral surface of the annular member 5 and the outer peripheral surface of the conductive member 4 has few voids. Specifically, the porosity of the brazing portion sandwiched between the inner peripheral surface of the annular member 5 and the outer peripheral surface of the conductive member 4 is preferably 1% or less in a cross-sectional view including the axis of the conductive member 4. Here, the area of the brazing portion refers to the area of only the portion sandwiched between the inner peripheral surface of the annular member 5 and the outer peripheral surface of the conductive member 4 (i.e., does not include the brazing material 6 located above the upper surface of the annular member 5 and the brazing material 6 located below the lower surface of the annular member 5) in the above image. The porosity is the percentage of voids present in the brazing portion when the area of the brazing portion is 100%.
[0030] 3, a second region 52 curved toward the inner circumferential surface may be further formed on the outer circumferential surface of the annular member 5. By providing the annular member 5 with such a second region 52, the contact area of the brazing material 6 with the outer circumferential surface of the annular member 5 can be increased. As a result, the annular member 5 can be fixed for a long period of time even if an impact is applied from the outer circumferential side.
[0031] The second region 52 may be present in only one location or in multiple locations on the outer peripheral surface of the annular member 5. By having multiple second regions 52 on the outer peripheral surface of the annular member 5, the contact area of the brazing material 6 with the outer peripheral surface of the annular member 5 can be increased. As a result, even if an impact is applied from the outer peripheral side, the annular member 5 can be fixed for a longer period of time.
[0032] The curvature of the second region 52 is not limited, and may be, for example, 0.6 (1 / mm) or more. When there are a plurality of second regions 52, each of the second regions 52 may have a curvature of 0.6 (1 / mm) or more. When the curvature of the second region 52 is 0.6 (1 / mm) or more, the contact area of the brazing material 6 with the outer peripheral surface of the annular member 5 can be enlarged. As a result, even if an impact is applied from the outer peripheral side, the annular member 5 can be fixed for a longer period of time. The upper limit of the curvature of the second region 52 may be, for example, 1.2 (1 / mm). The curvature of the second region 52 can be obtained by the same method as that used to obtain the curvature of the first region 51.
[0033] As shown in FIG. 3, the first through hole 3a formed in the ceramic substrate 3 may have a first opening 3a' that opens in an inverted frustum shape on the side where the annular member 5 is installed. When the first opening 3a' has a shape that opens in an inverted frustum shape, the stress of the ceramic substrate 3 near the first opening 3a' is dispersed more than when the first opening 3a' has a shape other than an inverted frustum shape. As a result, even if heating and cooling are repeated, cracks and the like are less likely to occur in the ceramic substrate 3, and the substrate can be used for a long period of time. The inverted frustum shape may be an inverted truncated cone shape, an inverted truncated pyramid shape, or the like, depending on the shape of the conductive member 4 (the shape of the first through hole 3a). As shown in FIG. 1, when the conductive member 4 is cylindrical, the inverted frustum shape is an inverted truncated cone shape.
[0034] Although not shown, the first through hole 3a formed in the ceramic substrate 3 may have a second opening that opens in an inverted frustum shape on the side opposite to the side where the annular member 5 is installed. When the second opening has a shape that opens in an inverted frustum shape, the stress of the ceramic substrate 3 near the second opening is dispersed more than when the second opening has a shape other than an inverted frustum shape. As a result, even if heating and cooling are repeated, cracks and the like are less likely to occur in the ceramic substrate 3, and the substrate can be used for a long period of time. The inverted frustum shape may be an inverted truncated cone shape, an inverted truncated pyramid shape, or the like, depending on the shape of the conductive member 4 (the shape of the first through hole 3a). As shown in FIG. 1, when the conductive member 4 is cylindrical, the inverted frustum shape is an inverted truncated cone shape.
[0035] In the first through hole 3a formed in the ceramic substrate 3, the first opening 3a' and the second opening are preferably symmetrical with respect to an imaginary plane that is perpendicular to the axial direction of the first through hole 3a and passes through the center of the thickness of the ceramic substrate 3. This configuration suppresses uneven distribution of stress in the thickness direction (axial direction) of the ceramic substrate 3. As a result, cracks and the like are less likely to occur in the ceramic substrate 3, and the ceramic substrate 3 can be used for a long period of time.
[0036] 3, the brazing material 6 may form a fillet from above the top surface of the annular member 5 toward the outside of the outer circumferential surface of the annular member 5. The brazing material 6 forming a fillet can increase the contact area of the brazing material 6 with the ceramic substrate 3, the conductive member 4, and the annular member 5. When the surface of the ceramic substrate 3 is provided with a metallized layer (not shown) and a plating layer (not shown) covering the metallized layer, the contact area of the brazing material 6 with the plating layer can be increased instead of the ceramic substrate 3. As a result, peeling is less likely to occur even when a force pulling outward is applied, and the brazing material 6 can be used for a long period of time.
[0037] When the surface of the ceramic substrate 3 is provided with a metallized layer and a plating layer covering the metallized layer so as to surround the conductive member 4, the average value of the cut level difference Rδc1 representing the difference between the cut level at a load length ratio of 25% on the roughness curve of the surface of the plating layer and the cut level at a load length ratio of 75% on the roughness curve may be greater than the average value of the cut level difference Rδc2 representing the difference between the cut level at a load length ratio of 25% on the roughness curve of the exposed portion of the surface of the ceramic substrate 3 and the cut level at a load length ratio of 75% on the roughness curve.
[0038] When the average value of the cut level difference Rδc1 is larger than the average value of the cut level difference Rδc2, the anchor effect of the brazed portion is increased, and the bonding strength of the brazed portion to the plating layer can be increased. In this case, the average value of the cut level difference Rδc2 is smaller than the average value of the cut level difference Rδc1. As a result, gaps are less likely to occur between the surface of the ceramic substrate 3 and the metallized layer, improving the adhesion of the metallized layer to the ceramic substrate 3. Furthermore, the variation in thickness of the metallized layer is also suppressed.
[0039] The cut level differences Rδc1 and Rδc2 can be measured using a shape analysis laser microscope (Keyence Corporation, Ultra-Deep Color 3D Shape Measuring Microscope (VK-X1100 or its successor model)). The measurement conditions are as follows: coaxial illumination, 60x magnification, no cutoff value λs, 0.8mm cutoff value λc, no cutoff value λf, and end effect correction. The measurement targets the surface of the plating layer around the conductive member 4 and the exposed portion of the surface of the ceramic substrate 3, and the measurement range per location is, for example, 5657μm×4232m. When determining the cut level difference Rδc1, a circumference C1 to be measured is drawn on the surface of the plating layer, with the axis of the conductive member 4 as the center. The length of each circumference is, for example, 6.2mm or more and 6.6mm or less. When determining the cut level difference Rδc2, a circumference C2 is drawn on the exposed portion of the surface of the ceramic substrate 3, coaxially with the circumference C1. The length per circumference is, for example, 7.8 mm or more and 8.3 mm or less. The measured values of the cut level differences Rδc1 and Rδc2 are obtained so that the number of measurements is the same as the number of conductive members 4, and the respective average values are calculated. When there is one conductive member 4, the measured value of the cut level difference Rδc1 and the measured value of the cut level difference Rδc2 can be compared.
[0040] For example, the average value of the cut level difference Rδc1 is 4 μm or more and 7 μm or less, and the average value of the cut level difference Rδc2 is 1 μm or more and 2 μm or less. In particular, it is preferable that the difference between the average value of the cut level difference Rδc1 and the average value of the cut level difference Rδc2 is 2 μm or more and 5 μm or less.
[0041] The metallization layer is, for example, composed mainly of molybdenum and contains manganese. In this case, of 100% by mass of the components constituting the metallization layer, for example, the content of manganese is 10% by mass or more and 30% by mass or less, and the remainder is molybdenum. The thickness of the metallization layer is, for example, several tens of μm. The plating layer is, for example, composed mainly of nickel and may contain phosphorus and boron. The thickness of the plating layer is, for example, several μm.
[0042] Another embodiment of the region Y shown in FIG. This will be explained with reference to FIG. FIG. 4 is an enlarged explanatory view for explaining another embodiment of the region Y shown in FIG. 2. As shown in Fig. 4, the cross-sectional outline of the brazing material 6 may have concave surfaces 7a, 7b. Because the brazing material 6 has the concave surfaces 7a, 7b, the volume of the brazing material 6 can be reduced compared to a case in which the concave surfaces 7a, 7b are not present. This reduces the stress applied to the ceramic substrate 3, and particularly prevents the occurrence of cracks in the ceramic substrate 3. In particular, because the brazing material 6 has the concave surface 7a, the stress applied to the ceramic substrate 3 is reduced.
[0043] A convex surface 8 is formed at the boundary between the concave surfaces 7a and 7b. The apex of the convex surface 8 may be close to the intersection line between the upper surface and the outer circumferential surface of the annular member 5. When the apex of the convex surface 8 is close to the intersection line between the upper surface and the outer circumferential surface of the annular member 5, the thickness of the brazing material is thin in the area close to the convex surface 8. This reduces the stress applied to the ceramic substrate 3, and makes it possible to particularly suppress the occurrence of cracks in the ceramic substrate 3.
[0044] The average radius of curvature of the convex surface 8 may be 60 μm or more and 190 μm or less. When the average radius of curvature of the convex surface 8 is 60 μm or more and 190 μm or less, the bonding strength of the conductive member 4 to the ceramic substrate 3 is improved. Furthermore, when a plurality of conductive members 4 are arranged along the axial direction of the metal sleeve 2, it is possible to prevent adjacent conductive members 4 from being short-circuited by the brazing material 6. Here, if the conductive member 4 is cylindrical, the convex surface 8 will be annular and will surround the conductive member 4.
[0045] The average radius of curvature of the convex surface 8 can be measured using a shape analysis laser microscope (Keyence Corporation, ultra-deep color 3D shape measuring microscope (VK-X1100 or its successor model)). The measurement conditions are set as follows: coaxial illumination, 120x magnification, and a measurement range including the convex surface 8 of, for example, 2792 μm × 2093 μm per location, and profile measurement can be performed. Specifically, first, in one measurement range, four lines to be measured are drawn from the conductive member 4 side toward the ceramic substrate 3 side so as to include the convex surface 8.
[0046] The length of each line is, for example, 200 μm or more and 300 μm or less. At least three measurement ranges are set, and at least 12 lines are measured. The average value of the measurement values obtained from the 12 lines measured is set as the average radius of curvature of the convex surface 8.
[0047] Further embodiment of region Y shown in FIG. This will be explained with reference to FIG. FIG. 5 is an enlarged explanatory view for explaining another embodiment of the region Y shown in FIG. 2. As shown in FIG. 5, a part of the annular member 5 may be located inside the first opening 3a' of the ceramic substrate 3. In other words, the lower surface of the annular member 5 may be located at a distance D in the axial direction of the first through hole 3a from the surface of the ceramic substrate 3 toward the first opening 3a'. With the structure as shown in FIG. 5, the volume of the brazing material 6 in the through hole 3a is reduced by the annular member 5. This reduces the stress applied to the ceramic substrate 3 adjacent to the through hole 3a, and makes it possible to particularly suppress the occurrence of cracks in the ceramic substrate 3.
[0048] Further embodiment of region Y shown in FIG. This will be explained with reference to FIG. FIG. 6 is an enlarged explanatory view for explaining another embodiment of the region Y shown in FIG. As shown in FIG. 6, the distance between the outer peripheral surface of the conductive member 4 and the inner peripheral surface of the annular member 5 does not have to be uniform. In FIG. 6, the distance between the outer peripheral surface of the conductive member 4 and the inner peripheral surface of the annular member 5 is W1 on the left side of the page, and W2 on the right side of the page, where W1>W2. It is preferable to have such a structure. The reason for this is presumed to be as follows. When W1 is larger than W2, the volume of the brazing material 6 between the first region 51 and the conductive member 4 increases in the region on the left side of the page. When W1 is larger than W2, the distance between the intersection line between the upper surface and the outer peripheral surface of the annular member 5 and the convex surface 8 can be reduced in the region on the left side of the page.
[0049] On the other hand, in the region on the right side of the page, the volume of the brazing material 6 between the first region 51 and the conductive member 4 increases. In the region on the right side of the page, the volume of the brazing material 6 between the first region 51 and the conductive member 4 decreases. By distributing the brazing material 6 non-uniformly in this manner, localized stress concentration in a portion of the first opening 3a' of the ceramic substrate 3 is suppressed. As a result, the occurrence of cracks in the ceramic substrate 3 can be particularly suppressed.
[0050] The airtight terminal 1 according to one embodiment is manufactured, for example, by the following procedure. First, a metal sleeve 2 is prepared. Next, a ceramic substrate 3 is fixed to the inner peripheral surface of the metal sleeve 2. The annular member 5 is placed on the ceramic substrate 3 so that a first through hole 3a formed in the ceramic substrate 3 and a second through hole 5a formed in the annular member 5 overlap with each other. Next, a conductive member 4 is inserted into the first through hole 3a and the second through hole 5a, and the ceramic substrate 3, the conductive member 4, and the annular member 5 are fixed with a brazing material 6 so as to cover the annular member 5. By adjusting the mass of the brazing material 6 and the brazing temperature, the porosity of the brazing portion sandwiched between the inner peripheral surface of the annular member 5 and the outer peripheral surface of the conductive member 4 and the shape of the fillet formed can be controlled.
[0051] When the surface of the ceramic substrate 3 includes a metallized layer and a plated layer covering the metallized layer so as to surround the conductive member 4, the average value of the cut level difference Rδc1 representing the difference between the cut level at a load length ratio of 25% on the roughness curve of the surface of the plated layer and the cut level at a load length ratio of 75% on the roughness curve can be made larger than the average value of the cut level difference Rδc2 representing the difference between the cut level at a load length ratio of 25% on the roughness curve of the exposed portion of the surface of the ceramic substrate 3 and the cut level at a load length ratio of 75% on the roughness curve by grinding or polishing the surface of the ceramic substrate 3 in advance. In this manner, an airtight terminal 1 according to one embodiment is obtained.
[0052] Next, an airtight end portion according to another embodiment having recesses 7a, 7b and a protrusion 8 shown in FIG. Child The manufacturing process can be carried out, for example, as follows. First, the metal sleeve 2 is prepared. Next, the ceramic substrate 3 is fixed to the inner peripheral surface of the metal sleeve 2. Separately, the annular member 5 is coated with the brazing material 6 in advance. The annular member 5 coated with the brazing material 6 can be produced, for example, by applying a paste consisting of fine powder of the brazing material 6 and an organic solvent, etc., to the entire periphery of the annular member 5, i.e., the upper surface, lower surface, inner peripheral surface, and outer peripheral surface, and then heating and cooling the paste.
[0053] The annular member 5 is placed on the ceramic substrate 3 so that the first through hole 3a formed in the ceramic substrate 3 overlaps with the second through hole 5a (previously coated with brazing material 6) formed in the annular member 5. Next, the conductive member 4 is inserted into the first through hole 3a and the second through hole 5a, and the ceramic substrate 3, the conductive member 4 and the annular member 5 are fixed together with the brazing material 6 so as to coat the annular member 5. In this manner, an airtight terminal according to another embodiment is formed. Child Obtained.
[0054] A part of the annular member 5 is located inside the first opening 3a' of the ceramic substrate 3 shown in FIG. moreover Another embodiment of the airtight end Child The manufacturing process may be carried out, for example, in the following manner. First, the metal sleeve 2 is prepared. Next, the ceramic substrate 3 is fixed to the inner peripheral surface of the metal sleeve 2. The annular member 5 is placed on the ceramic substrate 3 so that the first through hole 3a formed in the ceramic substrate 3 and the second through hole 5a formed in the annular member 5 overlap. When placing the annular member 5, the lower surface of the annular member 5 is positioned inside the first opening 3a' of the first through hole 3a, and then the annular member 5 is fixed. Next, the conductive member 4 is inserted into the first through hole 3a and the second through hole 5a, and the ceramic substrate 3, the conductive member 4, and the annular member 5 are fixed with the brazing material 6 so as to cover the annular member 5. In this manner, moreover Another embodiment of the airtight end Child Obtained.
[0055] The distances W1 and W2 shown in Fig. 6 are different from each other. Child The manufacturing process may be carried out, for example, in the following order. In the first manufacturing method, first, a metal sleeve 2 is prepared. Next, a ceramic substrate 3 is fixed to the inner peripheral surface of the metal sleeve 2. The annular member 5 is placed on the ceramic substrate 3 so that a first through hole 3a formed in the ceramic substrate 3 and a second through hole 5a formed in the annular member 5 overlap. Next, the conductive member 4 is inserted into the first through hole 3a and the second through hole 5a so that the gap between the conductive member 4 and the annular member 5 is not uniform. After that, the annular member 4 and the conductive member 5 are fixed together with a brazing material 6.
[0056] In the second manufacturing method, first, the metal sleeve 2 is prepared. Then, the ceramic substrate 3 is fixed to the inner peripheral surface of the metal sleeve 2. The annular member 5 is placed on the ceramic substrate 3 so that the first through hole 3a formed in the ceramic substrate 3 and the second through hole 5a formed in the annular member 5 overlap. Then, the conductive member 4 is inserted into the first through hole 3a and the second through hole 5a. Before fixing with the brazing material 6, the ceramic substrate 3 is tilted so that the axial direction of the annular member 5 is inclined at 10 to 30 degrees with respect to the vertical direction. Then, while the annular member 5 and the ceramic substrate 3 are kept in the tilted state, the brazing material 6 is heated and cooled to fix the conductive member 4 and the annular member 5. In this manner, Distances W1 and W2 are different Airtight End Child Obtained.
[0057] Alternatively, the conductive member 4 and the annular member 5 may be fixed to the ceramic substrate 3 in advance with the brazing material 6, and then the ceramic substrate 3 may be fixed to the inner circumferential surface of the metal sleeve 2. The annular member 5, whose inner circumferential surface facing the conductive member 4 has a first region 51 that curves in a direction away from the conductive member 4, can be obtained by preparing a metal plate in advance, and sequentially carrying out resist coating, mask exposure, development, etching, and resist peeling.
[0058] The airtight terminal 1 according to one embodiment is used in various devices, such as a vacuum pump, a plasma processing device such as a plasma film forming device, a plasma etching device, or a plasma ashing device. [Explanation of symbols]
[0059] 1 Airtight Terminal 2 Metal sleeve 3. Ceramic Substrate 3a 1st through hole 3a' 1st opening 4 Conductive materials 5 Annular member 5a 2nd through hole 51 First area 52 Second area 6 Brazing material 7a, 7b Concave 8 Convex
Claims
1. A cylindrical metal sleeve; a ceramic substrate fixed to an inner peripheral surface of the metal sleeve and having a first through hole along an axial direction of the metal sleeve; an annular member having a second through hole positioned coaxially with the first through hole; a columnar conductive member inserted into the first through hole and the second through hole and brazed to the ceramic substrate and the annular member; Including, an inner circumferential surface of the annular member facing the conductive member has a first region that is curved in a direction away from the conductive member; Airtight terminal.
2. The hermetic terminal according to claim 1 , wherein an inner circumferential surface of the annular member facing the conductive member has a plurality of the first regions.
3. The hermetic terminal according to claim 1 , wherein the curvature of the first region is 0.6 (1 / mm) or more.
4. The airtight terminal as described in claim 1, wherein the porosity of the brazing portion located between the inner surface of the annular member facing the conductive member and the outer surface of the conductive member is 1% or less when viewed in a cross-section including the axis of the conductive member.
5. The hermetic terminal according to claim 1 , wherein the outer circumferential surface of the annular member has a second region that curves toward an inner circumferential surface of the annular member that faces the conductive member.
6. The hermetic terminal according to claim 5 , wherein the outer peripheral surface of the annular member has a plurality of the second regions.
7. The hermetic terminal according to claim 5 , wherein the curvature of the second region is 0.6 (1 / mm) or more.
8. The hermetic terminal according to claim 1 , wherein the first through hole has a first opening portion that opens in an inverted frustum shape on a side where the annular member is disposed.
9. The airtight terminal according to claim 1 , wherein the first through hole has a second opening portion that opens in an inverted frustum shape on a side opposite to the side on which the annular member is disposed.
10. The hermetic terminal according to claim 8 , wherein the first through hole has a second opening portion that opens in an inverted frustum shape on a side opposite to a side on which the annular member is disposed.
11. The hermetic terminal according to claim 10 , wherein the first opening and the second opening are symmetrical with respect to an imaginary plane that is perpendicular to an axial direction of the first through hole and passes through a center of a thickness of the ceramic substrate.
12. The hermetic terminal according to claim 1 , wherein the brazing material is provided with a fillet extending from above the upper surface of the annular member toward the outside of the outer circumferential surface of the annular member.
13. The hermetic terminal according to claim 8 , wherein a portion of the annular member is located inside the first opening.
14. The hermetic terminal according to claim 12, wherein the fillet has a convex surface, and the mean radius of curvature of the convex surface is not less than 60 μm and not more than 190 μm.
15. 2. The hermetic terminal according to claim 1, comprising a metallized layer on a surface of the ceramic substrate, the metallized layer being disposed so as to surround the conductive member, and a plating layer covering the metallized layer, and an average value of a cut level difference Rδc1 representing a difference between a cut level at a load length ratio of 25% on a roughness curve of the surface of the plating layer and a cut level at a load length ratio of 75% on the roughness curve is greater than an average value of a cut level difference Rδc2 representing a difference between a cut level at a load length ratio of 25% on a roughness curve of an exposed portion of the surface of the ceramic substrate and a cut level at a load length ratio of 75% on the roughness curve.
16. A vacuum pump comprising the hermetic terminal according to any one of claims 1 to 15.
Citation Information
Patent Citations
JP1966-022350Y
JP1978053580U
Airtight terminal
JP1999016620A
Airtight vacuum terminal and electric pot
JP2002110265A
Sealed terminal
JP2019149304A