Protective cover and method for manufacturing the same
The ethylene-tetrafluoroethylene copolymer-based protective cover with specific thickness ratios in its bellows structure addresses the issue of repulsive stress in fluororesin bellows, enhancing durability and compressibility by reducing compressive stress and suppressing repulsive stress.
Patent Information
- Application Number
- JP2021032208
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-03-02
AI Technical Summary
Conventional fluororesin bellows used in protective covers experience repulsive stress during extension, leading to fatigue and performance deterioration due to long-term use, especially when applied in extended states.
A protective cover made of ethylene-tetrafluoroethylene copolymer with a bellows structure having alternating peaks and valleys, where the average thickness of the valley bottoms is greater than the peaks, and the ratio of these thicknesses is between 0.05 and 1.0, reducing compressive stress and improving durability.
The solution effectively reduces compressive stress, enhances durability, and suppresses repulsive stress, ensuring the cover maintains performance even with repeated expansion and contraction, while maintaining excellent compressibility and elasticity.
Smart Images

Figure 0007585566000003 
Figure 0007585566000004 
Figure 0007585566000005
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE The present disclosure relates to protective covers and methods of making protective covers. [Background technology]
[0002] Bellows are widely used in applications requiring elasticity, such as protective covers, joints, and pumps. In recent years, fluororesins such as polytetrafluoroethylene (PTFE) have come to be used as bellows materials because of their thermal stability, chemical resistance, non-stickiness, and lubricity.
[0003] As a method for producing such fluororesin bellows, in addition to cutting, bending molding has been proposed for the purpose of improving workability, precision, and the like (see Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 57-188320 Summary of the Invention
[0005] A protective cover according to one embodiment of the present disclosure is a stretchable cylindrical protective cover that is primarily composed of an ethylene-tetrafluoroethylene copolymer, that is arranged in an extended state, and that has a bellows portion that is compressible in the axial direction, where the bellows portion has peaks and valleys that are alternately continuous in the axial direction, where an average thickness H1 of the bottoms of the valleys is greater than an average thickness H2 of the tops of the peaks, and where a ratio H2 / H1 of the average thickness H1 of the bottoms of the valleys is 0.05 or greater and 1.0 or less.
[0006] A manufacturing method for a protective cover according to another embodiment of the present disclosure is a method for manufacturing an expandable cylindrical protective cover, the method comprising the step of blow molding a resin composition mainly composed of an ethylene-tetrafluoroethylene copolymer into a bellows shape, the bellows portion formed after the blow molding step has peaks and valleys that are alternately continuous in the axial direction, an average thickness H1 of the bottoms of the valleys is greater than an average thickness H2 of the tops of the peaks, and a ratio H2 / H1 of the average thickness H2 of the tops of the peaks to the average thickness H1 of the bottoms of the valleys is 0.05 or greater and 1.0 or less. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic front view showing a protective cover according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic side view illustrating a protective cover according to one embodiment of the present disclosure. [Diagram 3] FIG. 3 is a schematic cross-sectional view taken along line AA in FIG. 2, showing a protective cover according to one embodiment of the present disclosure. [Figure 4] FIG. 4 is a schematic partial cross-sectional view showing peaks and valleys of a protective cover according to one embodiment of the present disclosure. [Diagram 5] FIG. 5 is a graph showing the relationship between the compression ratio and the maximum compressive stress in the examples. [Figure 6] FIG. 6 is a graph showing the relationship between compression ratio and maximum compressive stress for some examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] [Problem to be solved by the invention] In the above-mentioned conventional technology, the bellows are sized in a contracted state, so in applications where the bellows are held in an extended state, repulsive stress is likely to occur during the holding (extension). As a result, the bellows itself may be continuously subjected to stress over a long period of use, leading to the accumulation of fatigue and elongation creep, which may result in deterioration of performance. Furthermore, when the bellows is used as a protective cover, the repulsive stress may also act on the components housed in the protective cover, causing a load to be applied.
[0009] The present disclosure has been made based on the above circumstances, and has an object to provide a protective cover that is excellent in the effect of reducing compressive stress and can improve durability.
[0010] [Effects of this disclosure] The protective cover of the present disclosure has an excellent effect of reducing compressive stress and can improve durability.
[0011] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described.
[0012] A protective cover according to one embodiment of the present disclosure is a stretchable cylindrical protective cover that is primarily composed of an ethylene-tetrafluoroethylene copolymer, that is arranged in an extended state, and that has a bellows portion that is compressible in the axial direction, where the bellows portion has peaks and valleys that are alternately continuous in the axial direction, where an average thickness H1 of the bottoms of the valleys is greater than an average thickness H2 of the tops of the peaks, and where a ratio H2 / H1 of the average thickness H1 of the bottoms of the valleys is 0.05 or greater and 1.0 or less.
[0013] The protective cover is mainly composed of an ethylene-tetrafluoroethylene copolymer, and the ratio H2 / H1 of the average thickness H2 of the top of the peak to the average thickness H1 of the bottom of the valley is 0.05 or more and 1.0 or less, so that the protective cover has an excellent effect of reducing compressive stress and the load on the protective cover is reduced. Since the protective cover has excellent compressibility, the amount of displacement of the protective cover can be improved. Furthermore, since the average thickness H1 of the bottom of the valley is larger than the average thickness H2 of the top of the peak, deformation of the shape during compression can be suppressed, and the elasticity can be improved. Furthermore, since the bellows portion is arranged in an extended state, the generation of repulsive stress is suppressed, and the effect of suppressing deterioration of performance can be improved. Therefore, even in a state where expansion and contraction are repeated, excessive load is not applied, and the durability of the protective cover can be improved.
[0014] The maximum compressive stress [MPa] at a compression ratio of 0.6, which is the ratio of the average compression amount [mm] to the axial length [mm] of the bellows portion, is preferably 30 MPa or more and 70 MPa or less. When the maximum compressive stress at the ratio of the average compression amount to the axial length of the bellows portion is 0.6, the compressive stress reduction effect is further enhanced, and the load on the protective cover can be further reduced.
[0015] In a graph in which the compression ratio is plotted on the horizontal axis and the maximum compressive stress is plotted on the vertical axis, it is preferable that there is no inflection point where the gradient of the graph increases sharply in a range of the compression ratio of 0.55 or less. In the graph, the absence of an inflection point where the gradient of the graph increases sharply in a range of the compression ratio of 0.55 or less enhances the effect of reducing the compressive stress, thereby further reducing the load on the protective cover.
[0016] A manufacturing method for a protective cover according to another embodiment of the present disclosure is a method for manufacturing an expandable cylindrical protective cover, the method comprising the step of blow molding a resin composition mainly composed of an ethylene-tetrafluoroethylene copolymer into a bellows shape, the bellows portion formed after the blow molding step has peaks and valleys that are alternately continuous in the axial direction, an average thickness H1 of the bottoms of the valleys is greater than an average thickness H2 of the tops of the peaks, and a ratio H2 / H1 of the average thickness H2 of the tops of the peaks to the average thickness H1 of the bottoms of the valleys is 0.05 or greater and 1.0 or less.
[0017] The manufacturing method of the protective cover includes a step of blow molding a resin composition mainly composed of an ethylene-tetrafluoroethylene copolymer into a bellows shape, so that the protective cover in the stretched state can be easily and reliably manufactured. In particular, a protective cover that can follow a protection object having multiple movements such as expansion and contraction, rotation, etc., such as a semiconductor manufacturing device, can be integrally molded, so that the number of parts can be reduced. In addition, the average thickness H1 of the bottom of the valleys in the bellows portion formed after the blow molding step is larger than the average thickness H2 of the top of the peaks, and the ratio of the average thickness of the top of the peaks to the average thickness of the bottom of the valleys is 0.05 or more and 1 or less, so that a protective cover that has excellent compressive stress reduction effect and compressibility and can improve durability can be obtained.
[0018] In this disclosure, "main component" refers to the component with the highest content, for example, a component with a content of 50% by mass or more. "Compression amount" refers to the thickness compressed in the axial direction. "Average compression amount" refers to the average compression amount measured at 10 test pieces. "Average thickness" refers to the average thickness (wall thickness) measured at any 10 points. "Compressive stress" refers to the compressive stress per unit area, and is measured in accordance with JIS-K7181 (2011) "Plastics - Determination of compressive properties".
[0019] [Details of the embodiment of the present disclosure] Preferred embodiments of the present disclosure will now be described with reference to the drawings.
[0020] <Protective cover> The protective cover is a protective cover for suppressing damage, breakage, deterioration, etc. of the elastic member to be protected, and the elastic member to be protected is housed in the protective cover. In other words, the protective cover is provided so as to cover the elastic member to be protected. FIG. 1 is a schematic front view of the protective cover, FIG. 2 is a schematic side view, and FIG. 3 is a schematic cross-sectional view along the line AA in FIG. 2. As shown in FIG. 1 to FIG. 3, the protective cover 1 is a cylindrical protective cover that is stretchable and mainly composed of ethylene-tetrafluoroethylene copolymer. The protective cover 1 is cylindrical as shown in FIG. 2, and is formed in a hollow shape. The protective cover 1 is arranged in an extended state and has a bellows portion 2 that is compressible in the axial direction. Therefore, the protective cover 1 can expand and contract in response to the movement of the elastic member to be protected. The protective cover 1 has a base portion 4 formed continuously at both ends of the bellows portion 2. Note that L in FIG. 1 indicates the length in the axial direction, that is, the length of the bellows portion 2.
[0021] In the protective cover 1, the bellows portion 2 has peaks 22 and valleys 21 that are alternately continuous in the axial direction of the protective cover 1. The bellows portion 2 is formed by alternately continuing valleys 21 having a small diameter and peaks 22 having a larger diameter than the valleys 21 in the axial direction. FIG. 4 is a schematic partial cross-sectional view showing the peaks 22 and valleys 21 of the protective cover 1. As shown in FIG. 4, the peaks 22 have peaks 26 on the outer periphery, and the valleys 21 have bottoms 25 on the outer periphery, and the peaks 26 and bottoms 25 are continuously formed by inclined surfaces. In the present disclosure, the average thickness of the bottoms 25 of the valleys 21 is represented by H1, and the average thickness of the peaks 26 of the peaks 22 is represented by H2.
[0022] By closely contacting the base 4 formed continuously at both ends of the bellows portion 2 with the telescopic member to be protected, it is possible to suppress adhesion of chemicals, solvents, dust, etc. from the outside and intrusion of foreign matter to the telescopic member to be protected. The structure of the base 4 is not particularly limited, and can be designed according to the structure of the telescopic member to be protected. The base 4 may have a function as a fastening member for fixing to the object to be protected. Furthermore, the protective cover 1 does not need to have a base 4. Furthermore, the protective cover 1 may be used in combination with an engaging member for attaching to the telescopic member to be protected.
[0023] The object to be protected by the protective cover 1 is not particularly limited, but examples include a power cylinder that is driven to expand and contract by hydraulic pressure, air pressure, water pressure, electricity, etc., a valve member such as a piston valve, a piston part of a cleaning device that performs reciprocating motion, etc. The protective cover 1 has a bellows part 2, and thus can expand and contract in response to movements at various operating angles due to the expansion and contraction motion, reciprocating motion, etc. of these objects to be protected.
[0024] The protective cover is a blow molded product mainly composed of ethylene-tetrafluoroethylene copolymer. The ethylene-tetrafluoroethylene copolymer (ETFE) is a fluororesin formed by polymerizing ethylene (C2H4) and tetrafluoroethylene (C2F4). The protective cover can be molded as a single piece and has excellent compressibility because it is mainly composed of ethylene-tetrafluoroethylene copolymer. Therefore, the protective cover has an excellent effect of reducing compressive stress and can improve durability. Furthermore, it has corrosion resistance and chemical resistance.
[0025] The lower limit of the average thickness of the protective cover 1 is 0.05 mm, preferably 0.075 mm, and more preferably 0.1 mm. Meanwhile, the upper limit of the average thickness is 10 mm, preferably 5 mm, and more preferably 1 mm. When the average thickness of the protective cover 1 is equal to or greater than the lower limit, the strength of the protective cover 1 can be improved. Meanwhile, when the average thickness of the protective cover 1 is equal to or less than the upper limit, the effect of reducing the compressive stress is excellent.
[0026] In the protective cover 1, the average thickness H1 of the bottoms 25 of the valleys 21 is greater than the average thickness H2 of the tops 26 of the peaks 22. Since the average thickness H1 of the bottoms of the valleys is greater than the average thickness H2 of the tops of the peaks, deformation of the shape during compression can be suppressed, thereby improving stretchability.
[0027] The lower limit of the ratio H2 / H1 of the average thickness H2 of the tops 26 of the peaks 22 to the average thickness H1 of the bottoms 25 of the valleys 21 is 0.05, preferably 0.2. On the other hand, the upper limit of the ratio H2 / H1 of the average thickness H2 of the tops 26 of the peaks 22 to the average thickness H1 of the bottoms 25 of the valleys 21 is 1, preferably 0.6. If the ratio H2 / H1 is less than the lower limit, there is a risk of buckling or breakage due to insufficient thickness of the peaks. On the other hand, if the ratio H2 / H1 exceeds the upper limit, there is a risk of the compressive stress becoming too large, which increases the load on the protective cover.
[0028] The lower limit of the axial length L [mm] of the bellows portion is preferably 50 mm, more preferably 100 mm. Meanwhile, the upper limit of the axial length L of the bellows portion is preferably 1000 mm, more preferably 500 mm. When the axial length L is within the above range, it becomes easier to more appropriately form the valleys of the bellows portion.
[0029] The lower limit of the maximum compressive stress when the ratio of the average compression amount [mm] to the axial length [mm] of the bellows portion is 0.6 is preferably 30 MPa, more preferably 40 MPa. On the other hand, the upper limit of the maximum compressive stress is preferably 70 MPa, more preferably 60 MPa. If the maximum compressive stress is less than the lower limit, the strength of the protective cover 1 may be insufficient and buckling may easily occur. On the other hand, if the maximum compressive stress exceeds the upper limit, the load on the protective cover 1 may be too high, and the durability and the amount of displacement may not be sufficient.
[0030] In a graph in which the compression ratio is plotted on the horizontal axis and the maximum compressive stress is plotted on the vertical axis, the range of compression ratios in which there is no inflection point where the gradient of the graph increases sharply is preferably 0.55 or less, and more preferably 0.65 or less. The absence of an inflection point where the gradient of the graph increases sharply in the range of compression ratios enhances the effect of reducing compressive stress, thereby further reducing the load on the protective cover.
[0031] The lower limit of the content of the ethylene-tetrafluoroethylene copolymer in the protective cover is preferably 50% by mass, more preferably 75% by mass, even more preferably 98% by mass, and particularly preferably 100% by mass, that is, the molded product after molding is composed of only the ethylene-tetrafluoroethylene copolymer. If the content of the ethylene-tetrafluoroethylene copolymer is less than the lower limit, the protective cover may not be properly molded.
[0032] The resin component of the protective cover may contain polymerization units derived from other copolymerizable monomers than the ethylene-tetrafluoroethylene copolymer, as long as the effect of the present invention is not impaired. For example, it may contain polymerization units of copolymerizable monomers such as perfluoro(alkyl vinyl ether), hexafluoropropylene, (perfluoroalkyl)ethylene, and chlorotrifluoroethylene. The upper limit of the content of the polymerization units derived from the other copolymerizable monomers is, for example, 3 mol% with respect to the total polymerization units constituting the ethylene-tetrafluoroethylene copolymer.
[0033] The protective cover may contain components other than the ethylene-tetrafluoroethylene copolymer as long as the object of the present disclosure is not impaired.
[0034] (Sliding agent) The addition of a sliding agent reduces the coefficient of friction and improves slidability. Examples of the sliding agent include oils such as lubricating oil (machine oil) and solid lubricants. The amount of the sliding agent is preferably in the range of 1 part by mass to 10 parts by mass per 100 parts by mass of the resin.
[0035] Examples of the lubricating oil include paraffinic and naphthenic mineral oils such as spindle oil, refrigeration oil, dynamo oil, turbine oil, machine oil, cylinder oil, and gear oil, as well as synthetic oils such as grease, hydrocarbon, ester, polyglycol, polyphenylene ether, silicone, and halocarbon.
[0036] Examples of the solid lubricant include polytetrafluoroethylene particles, molybdenum disulfide, graphite, silicone rubber, polyethylene, etc. As the polyethylene, ultra-high molecular weight polyethylene having a molecular weight of 2 million or more and a particle size of about 3 μm to 40 μm is preferable.
[0037] (Reinforcement material) The addition of a reinforcing material can improve mechanical strength, creep resistance, etc. Examples of the reinforcing material include glass fillers such as glass fiber (glass fiber) and spherical glass, carbon fiber, calcium carbonate, talc, silica, alumina, aluminum hydroxide, inorganic whiskers such as basic magnesium sulfate whiskers, zinc oxide whiskers, and potassium titanate whiskers, and inorganic fillers such as montmorillonite and synthetic smectite. The amount of the reinforcing material to be added is preferably 5 parts by mass to 100 parts by mass relative to 100 parts by mass of the resin.
[0038] Generally, as inorganic fillers, short fiber fillers are most effective in increasing the elastic modulus, but chopped strand glass fibers with an average fiber length of about 1 mm to 3 mm are preferred. Also, since glass fibers are made of glass, they can increase the transparency of the molded product. Furthermore, when the glass fibers are surface-treated with a surface treatment agent, the affinity between the polyolefin resin and the glass fibers increases, further improving the transparency.
[0039] Examples of the surface treatment agent include silane coupling agents and titanium coupling agents having alkyl chains with amino, glycidyl, mercapto, vinyl, acryloxy, and methacryloxy groups. Examples of crosslinking assistants having functional groups that react with the surface treatment agent include those having amino, glycidyl, hydroxyl, isocyanate, carboxyl, and carbodiimide groups.
[0040] (Antioxidants) The stability can be improved by adding an antioxidant. The amount of the antioxidant to be added is preferably 0.0005 parts by mass to 0.5 parts by mass, and more preferably 0.001 parts by mass to 0.1 parts by mass, per 100 parts by mass of the resin.
[0041] Examples of the antioxidant include one or a combination of two or more selected from the group consisting of 2,2'-methylene-bis[6-(1-methylcyclohexyl-p-cresol)], 2,2'-methylene-bis(4-ethyl-6-tert-butylphenol), 2,2'-methylene-bis(4-methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol) and 2,6-di-tert-butyl-p-cresol.
[0042] (Crosslinking aid) The crosslinking aid is blended to promote crosslinking of the resin by irradiation with ionizing radiation. The blending amount of the crosslinking aid varies depending on the type of the crosslinking aid, but is usually preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, per 100 parts by mass of the resin.
[0043] Examples of the crosslinking aid include oximes such as p-quinone dioxime and p,p'-dibenzoylquinone dioxime; acrylates or methacrylates such as ethylene dimethacrylate, polyethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, cyclohexyl methacrylate, acrylic acid / zinc oxide mixture, allyl methacrylate, and trimethacrylic isocyanurate (hereinafter also referred to as TMIC); vinyl monomers such as divinylbenzene, vinyl toluene, and vinyl pyridine; allyl compounds such as hexamethylene diallyl nadimide, diaryl itaconate, diallyl phthalate, diallyl isophthalate, diallyl monoglycidyl isocyanurate, triallyl cyanurate, and triallyl isocyanurate (hereinafter also referred to as TAIC); and maleimide compounds such as N,N'-m-phenylene bismaleimide and N,N'-(4,4'-methylene diphenylene) dimaleimide. These crosslinking aids may be used alone or in combination.
[0044] (Polyfunctional Monomer) A polyfunctional monomer is a monomer having a molecular weight of 1000 or less and having at least two carbon-carbon double bonds in the molecule. By using a polyfunctional monomer having a molecular weight of 1000 or less, a molded product having excellent heat resistance while maintaining transparency can be obtained, and these properties can be achieved simultaneously. In addition, by using a polyfunctional monomer having a molecular weight of 1000 or less, the monomer has a viscosity that allows easy kneading with a resin, and is preferably in many cases where the polyfunctional monomer itself is less colored.
[0045] Examples of the polyfunctional monomer include 1,6-hexanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, ethylene oxide modified bisphenol A di(meth)acrylate, diethylene glycol di(meth)acrylate, dipentaerythritol hexaacrylate, dipentaerythritol monohydroxypentaacrylate, caprolactone modified dipentaerythritol hexaacrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, polyethylene glycol di(meth)acrylate, tris(acryloxyethyl)isocyanurate, and tris(methacryloxyethyl)isocyanurate. Among these, tris(acryloxyethyl)isocyanurate, tris(methacryloxyethyl)isocyanurate, trimethylolpropane tri(meth)acrylate, and the like can be mentioned.
[0046] As the polyfunctional monomer, a commercially available polyfunctional monomer can also be used. However, since the commercially available polyfunctional monomer may contain a stabilizer or the like to such an extent that it affects the effects of the present disclosure, it is preferable to perform a simple preliminary test on the effects of the present disclosure before use to confirm that it does not affect the effects of the present disclosure. As the polyfunctional monomer, one containing a stabilizer amount of 1000 ppm or less is usually used, and in order to prevent the effects of the present disclosure from being affected, the smaller the amount of stabilizer, the more preferable it is.
[0047] The amount of the polyfunctional monomer is preferably 0.05 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the resin. If it is less than 0.05 parts by mass, the efficiency of radiation crosslinking of the resin may be low, and sufficient heat resistance and light resistance may not be obtained. On the other hand, if it exceeds 20 parts by mass, handling during kneading may become difficult, and the additive may bleed out from the molded product. In addition, the transparency may decrease due to self-polymerization of the additive itself.
[0048] In addition to the above components, other components that can be added as long as they do not impair the objectives of the present disclosure include, for example, ultraviolet absorbers, weather stabilizers, copper damage inhibitors, flame retardants, colorants, etc.
[0049] The protective cover has an excellent effect of reducing compressive stress, and the load on the protective cover is reduced. Furthermore, the excellent compressibility allows the amount of displacement of the protective cover to be improved. Furthermore, the bellows portion is arranged in an extended state, so the generation of repulsive stress is suppressed, and the effect of suppressing deterioration of performance can be improved. Therefore, even in a state where expansion and contraction are repeated, excessive load is not applied, and the durability of the protective cover can be improved.
[0050] <Protective cover manufacturing method> The method for producing a protective cover is a method for producing a stretchable cylindrical protective cover, and includes a step of blow molding a resin composition containing an ethylene-tetrafluoroethylene copolymer as a main component into a bellows shape. The method for producing a protective cover may further include a step of irradiating with an electron beam.
[0051] (Blow molding process) In the blow molding step, as described above, a resin composition mainly composed of an ethylene-tetrafluoroethylene copolymer is blow molded into a bellows shape. Since the manufacturing method for the protective cover includes a blow molding step, a protective cover in an extended state can be easily and reliably manufactured. In particular, since a protective cover that can follow multiple movements such as expansion / contraction and rotation, such as a semiconductor manufacturing device that is an expandable member to be protected, can be integrally molded, the number of parts can be reduced. In addition, since the manufacturing method for the protective cover uses an ethylene-tetrafluoroethylene copolymer as a main component, a protective cover that is excellent in the effect of reducing compressive stress and can improve durability can be manufactured.
[0052] (Electron beam irradiation process) In the electron beam irradiation step, the molded body obtained in the blow molding step as described above is irradiated with an electron beam.
[0053] The ethylene-tetrafluoroethylene copolymer constituting the molded body is irradiated with electron beams. The irradiation with electron beams promotes crosslinking of the ethylene-tetrafluoroethylene copolymer, thereby improving the heat resistance, shape memory effect, chemical resistance, creep resistance and abrasion resistance of the resulting protective cover.
[0054] The atmospheric temperature in the step of irradiating the electron beam can be set to be equal to or higher than room temperature and equal to or lower than the melting point, which can further increase the manufacturing efficiency of the method for manufacturing the protective cover.
[0055] In addition, the electron beam irradiation step can be performed in the atmosphere, which does not require any equipment or energy for adjusting the atmosphere, thereby further improving the production efficiency.
[0056] The lower limit of the electron beam irradiation dose in the step of irradiating with electron beams is preferably 220 kGy, more preferably 240 kGy. On the other hand, the upper limit of the electron beam irradiation dose is not particularly limited, but is preferably 480 kGy. If the electron beam irradiation dose is less than the lower limit, the creep resistance and abrasion resistance of the obtained protective cover may not be sufficiently improved. On the other hand, if the electron beam irradiation dose exceeds the upper limit, the cost-effectiveness of the electron beam irradiation may not be sufficiently obtained.
[0057] As described above, the bellows portion formed after the blow molding process has peaks and valleys alternately arranged in the axial direction, and the average thickness H1 of the bottoms of the valleys is greater than the average thickness H2 of the tops of the peaks. This makes it possible to suppress deformation of the shape during compression, thereby improving stretchability.
[0058] In addition, the ratio H2 / H1 of the average thickness H2 of the tops of the peaks to the average thickness H1 of the bottoms of the valleys is 0.05 or more and 1 or less. Therefore, a protective cover can be obtained that is excellent in the effect of reducing compressive stress and in compressibility, and that can improve durability.
[0059] According to the manufacturing method of the protective cover, the protective cover in the extended state can be easily and reliably manufactured. In addition, since a protective cover with a complex structure that can expand and contract in response to various movements of a protected object having multiple movements such as expansion and contraction, reciprocation, etc. can be integrally molded, the number of parts can be reduced.
[0060] [Other embodiments] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present disclosure is not limited to the configurations of the above-described embodiments, but is indicated by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims. EXAMPLES
[0061] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.
[0062] [Bellows No.1~No.10] The bellows portions No. 1 to No. 10 were blow molded from a resin composition made of ethylene-tetrafluoroethylene copolymer (ETFE). The bellows portions No. 1 to No. 6, No. 9, and No. 10 had 12 peaks and 11 valleys, and the length in the axial direction was 111 mm. The bellows portion No. 7 had 12 peaks and 11 valleys, and the length in the axial direction was 3.33 mm. The bellows portion No. 8 had 12 peaks and 11 valleys, and the length in the axial direction was 1332 mm. The bellows portion No. 5 was blow molded from a resin composition made of polytetrafluoroethylene (PTFE). Table 1 shows the length L of the bellows portions, the average thickness H1 of the bottoms of the valleys, the average thickness H2 of the tops of the peaks, and the ratio H2 / H1 of the average thickness H2 to the average thickness H1.
[0063] [evaluation] (Maximum compressive stress at compression ratio of 0.6) The relationship between the average compression amount and the maximum compressive stress relative to the axial length of the obtained bellows portions No. 1 to No. 10 was obtained by simulation. Table 2 shows specific data on the relationship between the average compression amount and the maximum compressive stress relative to the axial length of the bellows portions No. 1 to No. 10. Table 1 shows the maximum compressive stress [MPa] at a compression ratio of 0.6, which is the ratio of the average compression amount [mm] to the axial length [mm] of the bellows portions No. 1 to No. 10. FIG. 5 shows a graph showing the relationship when the compression ratios of No. 1 to No. 10 are taken on the horizontal axis and the maximum compressive stresses are taken on the vertical axis. Of the graphs shown in FIG. 5, a graph showing the relationship between the compression ratio and the maximum compressive stress of No. 1 and No. 9 is shown in FIG. 6.
[0064] (The inflection point of the graph with the above compression ratio on the horizontal axis and the above maximum compressive stress on the vertical axis) The compression ratios at which the inflection points at which the gradient suddenly increases were found were evaluated from the graph in Figure 5, which shows the relationship between the compression ratio and the maximum compressive stress for No. 1 to No. 10. The compression ratios at the inflection points for No. 1 to No. 10 shown in the graph in Figure 5 are shown in Table 1.
[0065] [Table 1]
[0066] [Table 2]
[0067] From the results of Tables 1, 2 and FIG. 5, No. 1 to No. 3, No. 7 and No. 8, which are mainly composed of ETFE, have an average thickness H1 of the bottom of the valleys in the bellows portion that is greater than the average thickness H2 of the top of the peaks, and have a ratio H2 / H1 of the average thickness H2 of the top of the peaks to the average thickness H1 of the bottom of the valleys that is 0.05 or more and 1.0 or less, do not show a significant increase in maximum compressive stress even when the compression ratio is increased, and are excellent in the effect of reducing compressive stress and can improve elasticity. In addition, the evaluation of the maximum compressive stress at a compression ratio of 0.6 in No. 1 to No. 3, No. 7 and No. 8 was all in the range of 30 MPa to 70 MPa. Furthermore, as shown in the graph of FIG. 5, No. 1 to No. 3, No. 7 and No. 8 did not show an inflection point where the gradient of the graph suddenly increases in the range of compression ratios of 0.55 or less. From this, it is considered that Nos. 1 to 3, 7 and 8 can improve durability because the load on the protective cover is reduced.
[0068] On the other hand, in No. 4, No. 6 and No. 10, in which the average thickness H1 of the bottom of the valleys is equal to the average thickness H2 of the top of the peaks, or the average thickness H1 of the bottom of the valleys is equal to the average thickness H2 of the top of the peaks, and in No. 5, in which the main component is PTFE and the average thickness H1 of the bottom of the valleys is equal to the average thickness H2 of the top of the peaks, a significant increase in the maximum compressive stress was observed as the compression ratio increased. In particular, in No. 6 and No. 10, in which the ratio H2 / H1 of the average thickness H2 of the top of the peaks to the average thickness H1 of the bottom of the valleys is greater than 1.0, a very significant increase in the maximum compressive stress was observed as the compression ratio increased. That is, as shown in the graph of FIG. 5, in No. 4 to No. 6 and No. 10, an inflection point where the gradient of the graph increases sharply appears in the range of compression ratios of 0.55 or less. In addition, as shown in Fig. 6, in No. 9, in which the ratio H2 / H1 of the average thickness H2 of the tops of the peaks to the average thickness H1 of the bottoms of the valleys is less than 0.05, no increase in the maximum compressive stress was observed even when the compression ratio was increased, but buckling occurred in the valleys and peaks of the bellows section during compression. This is thought to be because, in No. 9, a phenomenon was observed in which compression progressed while buckling occurred, and because the load was released during buckling, the maximum compressive stress did not increase even when the compression ratio was increased, and compression progressed at a constant maximum compressive stress.
[0069] From the above results, it can be seen that the protective cover has an excellent effect of reducing compressive stress and can improve durability. [Explanation of symbols]
[0070] 1 Protective cover 2 Bellows 4 base 21 Valley 22 Yamabe 25 Bottom of valley 26 Top of the mountain L Axial length H1 Average thickness at the bottom of the valley H2 Average thickness of the peak
Claims
1. A flexible cylindrical protective cover, The main component is an ethylene-tetrafluoroethylene copolymer, a bellows portion disposed in a tensioned state and axially compressible; The bellows portion has peaks and valleys that are alternately arranged in the axial direction, the average thickness H1 of the bottom of the valley is greater than the average thickness H2 of the top of the peak, A protective cover in which a ratio H2 / H1 of an average thickness H2 of the tops of the peaks to an average thickness H1 of the bottoms of the valleys is 0.20 or greater and 0.40 or less.
2. The protective cover according to claim 1, wherein the maximum compressive stress [MPa] until the compression ratio, which is the ratio of the average compression amount [mm] to the axial length [mm] of the bellows portion, reaches 0.6, is 30 MPa or more and 70 MPa or less.
3. 3. The protective cover according to claim 2, wherein in a graph in which the compression ratio is plotted on the horizontal axis and the maximum compressive stress is plotted on the vertical axis, there is no inflection point where the gradient of the graph suddenly increases in a range of the compression ratio of 0.55 or less.
4. A method for manufacturing a stretchable tubular protective cover, comprising the steps of: The method includes a step of blow molding a resin composition containing an ethylene-tetrafluoroethylene copolymer as a main component into a bellows shape, The bellows portion formed after the blow molding step has peaks and valleys alternately arranged in an axial direction, the average thickness H1 of the bottom of the valley is greater than the average thickness H2 of the top of the peak, A method for manufacturing a protective cover, wherein a ratio H2 / H1 of an average thickness H2 of the tops of the peaks to an average thickness H1 of the bottoms of the valleys is 0.20 or greater and 0.40 or less.
Citation Information
Patent Citations
Corrugated tube and method for manufacturing same
CN111886435A
Corrugated pipe and electrical system
CN203760964U
Manufacture of fluorine resin bellows
JP1982188320A
Hose with bellows
JP1991194282A
Metal compounded corrugated hose and method for manufacturing the same
JP2001341230A