Photoresponsive Compounds
The azomethine compound with specific structural modifications addresses the coloration issue of azobenzene derivatives, providing reversible fluidization and non-fluidization for improved toner and adhesive performance.
Patent Information
- Application Number
- JP2020135375
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-08-07
AI Technical Summary
Azobenzene derivatives used in toners and adhesives exhibit significant coloration, making it difficult to achieve desired colors and are nearly colorless, limiting their industrial applications.
A photoresponsive azomethine compound with an aromatic hydrocarbon and aromatic heterocyclic structure at both ends of a C=N bond, where a hydrogen atom is bonded to an adjacent carbon atom, allowing for reversible fluidization and non-fluidization without significant coloring.
The compound ensures photoresponsiveness, improves fixing properties, and provides good color reproducibility in toners, enabling applications in image forming and adhesives that can be repeatedly attached and detached by light.
Smart Images

Figure 0007585651000027 
Figure 0007585651000028 
Figure 0007585651000029
Abstract
Description
[Technical field]
[0001] The present invention relates to a photoresponsive compound that becomes fluid and reversibly non-fluid upon irradiation with light. [Background technology]
[0002] Photoresponsive materials are known as materials whose fluidity changes when irradiated with light. For example, the azobenzene compounds (azobenzene derivatives) described in Patent Documents 1 and 2 undergo a phase change in association with an isomerization reaction caused by irradiation with light.
[0003] It is believed that the change in molecular structure caused by this induces a phase transition from a solid state to a fluid state. In addition, if the material is exposed to light of a different wavelength, heated, or left in the dark at room temperature, a reverse reaction occurs and the material solidifies again. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2011-256155 A [Patent Document 2] JP 2011-256291 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the azobenzene derivatives described in the above Patent Documents 1 and 2 are all colored yellow to orange, and there is a problem in that the desired color cannot be reproduced when applied to industrial products such as toners, adhesives, etc. Furthermore, according to the study by the present inventors, it was found that although the yellow to orange coloring can be adjusted to some extent by changing the substituent of the azobenzene derivative, it is fundamentally impossible to achieve a colorless or nearly colorless state.
[0006] It is therefore an object of the present invention to provide a compound which becomes fluid when irradiated with light, becomes non-fluid reversibly, and is free from significant coloration. [Means for solving the problem]
[0007] The present inventors have conducted extensive research in view of the above problems, and as a result have found that the above problems can be solved by providing an azomethine compound having an aromatic hydrocarbon structure and an aromatic heterocyclic structure at both ends of a C=N bond, in which a hydrogen atom is bonded to at least one carbon atom adjacent to the carbon atom bonded to the C=N in the aromatic heterocyclic structure, and have thus completed the present invention.
[0008] That is, the present invention relates to a photoresponsive compound which is fluidized and reversibly non-fluidized by irradiation with light and is represented by the following general formula (1):
[0009] [ka]
[0010] In the formula, Z1 and Z2 are N or CH, with the proviso that Z1 ≠ Z2; R1 contains an aromatic hydrocarbon structure; R2 contains an aromatic heterocyclic structure; A hydrogen atom is bonded to at least one carbon atom adjacent to the carbon atom in the aromatic heterocyclic structure bonded to Z2. Effect of the Invention
[0011] According to the present invention, it is possible to provide a photoresponsive compound that fully ensures the photoresponsiveness of being fluidized and reversibly non-fluidized upon irradiation with light, improves the fixing property when used in a toner, and further has good color reproducibility. [Brief description of the drawings]
[0012] [Figure 1]FIG. 1 is a schematic diagram showing an image forming apparatus 100 used in an image forming method according to an embodiment of the present invention. [Diagram 2] 2 is a schematic configuration diagram of an irradiation unit 40 in the image forming apparatus 100. FIG. [Diagram 3] FIG. 2 is a schematic diagram of an apparatus for measuring the change in adhesiveness of a compound due to light irradiation, used in the photoresponsive adhesion test of the Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Preferred embodiments of the present invention will be described below. In this specification, the range "X to Y" means "X or more and Y or less." Furthermore, in this specification, unless otherwise specified, operations and measurements of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.
[0014] <Photoresponsive compounds> One embodiment of the present invention is a photoresponsive compound that is fluidized and reversibly non-fluidized upon irradiation with light, and is represented by the following general formula (1):
[0015] [ka]
[0016] In the formula, Z1 and Z2 are N or CH, with the proviso that Z1 ≠ Z2; R1 contains an aromatic hydrocarbon structure; R2 contains an aromatic heterocyclic structure; A hydrogen atom is bonded to at least one carbon atom adjacent to the carbon atom in the aromatic heterocyclic structure bonded to Z2.
[0017] Here, the above general formula (1) will be explained using one of the following specific examples:
[0018] [ka]
[0019] As shown in the above, Z2 is bonded to a carbon atom in the aromatic heterocyclic structure, and at least one of the bonding sites adjacent to the carbon atom (i.e., the bonding site indicated by *) is a carbon atom (two carbon atoms in the above specific example), and a hydrogen atom (two hydrogen atoms in the above specific example) is bonded to the carbon atom (two carbon atoms in the above specific example). In this specification, the "photoresponsive compound" may also be simply referred to as a "compound". Such an azomethine compound can provide a photoresponsive compound that is sufficiently guaranteed to be fluidized and reversibly non-fluidized by irradiation with light, has improved fixability, and has good color reproducibility.
[0020] In this specification, the term "fluidized by light irradiation and reversibly non-fluidized" refers to a state in which the compound of the present invention changes from a non-fluid state to a fluid state by light irradiation and then returns to a non-fluid state. That is, the compound of the present invention is in a non-fluid solid state at room temperature and normal pressure when not irradiated with light, and softens and changes to a fluid state by light irradiation. When the light irradiation is stopped and the compound is left in a dark place at room temperature or under visible light irradiation, or is heated, the compound returns to a non-fluid solid state. In this specification, the term "fluid state" refers to a state in which the compound is deformed by a small external force.
[0021] The mechanism by which such technical effects are achieved is presumed to be as follows. However, the technical scope of the present invention is not limited to such a mechanism. In other words, azobenzene compounds are materials that absorb light and soften from a solid state (photochemical phase transition), and it is believed that this photochemical phase transition occurs when the crystal structure collapses due to cis-trans isomerization. The azobenzene compounds described in Patent Documents 1 and 2 undergo a phase change in association with an isomerization reaction due to light irradiation, but these compounds undergo n-π isomerization in the visible light region. * It has been found that, since it exhibits strong absorption due to transition and is colored orange, it is difficult to reproduce the desired color when applied to industrial products.
[0022] In the present invention, by using a specific azomethine compound, it has become possible to provide a compound that becomes fluid when irradiated with light, becomes non-fluid reversibly, and does not have a significant coloration. By introducing an azomethine moiety (C=N moiety) instead of an azobenzene moiety, the strong n-π * Because the absorption can be weakened, it is possible to realize a compound that does not have significant coloration.
[0023] In addition, when a non-fluid trans form of a compound is irradiated with light and isomerized to a cis form, many of the trans forms change to cis forms, which destroys the ordered structure and induces a phase transition, i.e., the fluidization phenomenon. In addition, when the cis forms return to the trans form, an ordered structure is formed again, which induces the non-fluidization phenomenon. Therefore, in order to induce the fluidization phenomenon, many of the trans forms must be isomerized to cis forms. However, it is generally known that azomethine compounds are faster in isomerization from cis to trans than azobenzene compounds, and it was expected that azomethine compounds with unsubstituted benzene rings at both ends of the C=N bond would be disadvantageous in inducing the reversible fluidization and non-fluidization phenomena.
[0024] Therefore, in the present invention, an azomethine compound is provided in which an aromatic hydrocarbon structure and an aromatic heterocyclic structure are provided at both ends of a C=N bond, and at least one of the two atoms adjacent to the carbon atom bonded to C=N in the aromatic heterocyclic structure is a carbon atom and has a hydrogen atom on the carbon atom. This is believed to increase the amount of cis isomers upon light irradiation, and induce fluidization associated with the photoisomerization reaction. This is believed to be due to the fact that the introduction of the aromatic heterocyclic structure reduces the cis-to-trans reaction rate, and furthermore, the hydrogen atom on the carbon atom adjacent to the carbon atom bonded to C=N of the aromatic heterocyclic group and the aromatic hydrocarbon group form an intramolecular CH-π interaction in the cis isomer, stabilizing the cis isomer and producing more cis isomers.
[0025] The compound represented by formula (1) will be further described below.
[0026] (Z1 and Z2) In one embodiment of the present invention, Z1 and Z2 are N or CH, as described above, with the proviso that Z1 ≠ Z2.
[0027] (R1 and R2) In one embodiment of the present invention, R1 comprises an aromatic hydrocarbon structure and R2 comprises an aromatic heterocyclic structure, as described above.
[0028] In one embodiment of the present invention, the aromatic hydrocarbon structure is not particularly limited, but may be, for example, a substituted or unsubstituted aromatic hydrocarbon group, preferably a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms. In a preferred embodiment of the present invention, the R1 is a substituted or unsubstituted phenyl group, naphthyl group, anthracenyl group, phenanthrenyl group, pyrenyl group, or biphenyl group. Such a compound can effectively cause fluidization and non-fluidization. Among them, R1 is preferably a substituted or unsubstituted phenyl group, naphthyl group, or phenanthrenyl group, from the viewpoint that intermolecular packing is easily developed, and when trans-cis isomerization occurs, it shows high thermal mobility and is easily induced to cause a fluidization phenomenon.
[0029] In one embodiment of the present invention, the aromatic heterocyclic structure is not particularly limited, but may be, for example, a substituted or unsubstituted aromatic heterocyclic group, preferably a substituted or unsubstituted aromatic heterocyclic group having 2 to 30 carbon atoms. The aromatic hydrocarbon structure is preferably one having high electron donating properties, and in a preferred embodiment of the present invention, the R2 may be a substituted or unsubstituted thienyl group, furanyl group, pyrrolyl group, pyrazolyl group, imidazolyl group, pyridyl group, pyrimidinyl group, pyrazinyl group, triazinyl group, benzothienyl group, benzimidazolyl group, indolyl group, isoindolyl group, quinolinyl group, isoquinolinyl group, quinazolinyl group, quinoxalinyl group, naphthyridinyl group, acridinyl group, carbazolyl group, or dibenzothienyl group. With such a compound, fluidization and non-fluidization can occur effectively.
[0030] The above aromatic hydrocarbon group or aromatic heterocyclic group may each have a substituent. The substituent is not particularly limited, but examples thereof include a halogen atom, a cyano group, a nitro group, an amino group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms. Preferred are a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0031] As described above, the photoinduced phase transition of the azomethine compound is considered to occur due to the collapse of the crystal structure caused by cis-trans isomerization, as in the case of the azobenzene compound. In general, since the π-π interaction between molecules of azomethine compounds is strong, the photoinduced phase transition occurs only at the very outermost surface of the crystal structure. Here, when the aromatic hydrocarbon group or aromatic heterocyclic group represented by R1 or R2 in the above general formula (1) respectively has a substituent, the azomethine compound of the present invention forms a specific crystal structure in which an isotropically disordered structure due to the thermal motion of these substituents coexists in a periodic structure in which the π-π interaction is dominant. Therefore, when the cis-trans isomerization reaction proceeds locally and the π-π interaction of the azomethine moiety is reduced, isotropic melting occurs in a chain reaction throughout the system. Therefore, it is considered that the cis-trans isomerization proceeds more easily, and fluidization is more likely to occur.
[0032] In this case, it is preferable that at least one of the above-mentioned substituents is a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 18 carbon atoms, or an alkoxycarbonyl group having 2 to 18 carbon atoms. That is, in one embodiment of the present invention, in the above general formula (1), at least one of the R1 and the R2 has at least one substituent selected from the group consisting of a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 18 carbon atoms, and an alkoxycarbonyl group having 2 to 18 carbon atoms. It is considered that such a structure makes it easier for cis-trans isomerization to proceed and makes it easier for fluidization to occur. Among these, due to their high thermal mobility, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms is more preferable, and an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, or a dialkylamino group having 2 to 10 carbon atoms is even more preferable.
[0033] Further, a preferred embodiment of the present invention is a compound in which, in the general formula (1), the R1 and the R2 each independently have at least one substituent selected from the group consisting of a halogen group, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms, and at least one of the R1 and the R2 has at least one substituent selected from the group consisting of an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms. By adopting such a configuration, lattice defects that act favorably on cis-trans isomerization, free volume, reduction of π-π interaction, etc. occur. Therefore, it is considered that cis-trans isomerization is more likely to proceed and fluidization is more likely to occur.
[0034] As for the number of carbon atoms of the substituent, the alkyl group is more preferably an alkyl group having 1 to 12 carbon atoms, and even more preferably an alkyl group having 4 to 12 carbon atoms. The alkoxy group is more preferably an alkoxy group having 1 to 12 carbon atoms, and even more preferably an alkoxy group having 4 to 12 carbon atoms. The dialkylamino group is more preferably a dialkylamino group having 2 to 8 carbon atoms, and even more preferably a dialkylamino group having 4 to 6 carbon atoms. The acyl group is more preferably an acyl group having 2 to 13 carbon atoms, and even more preferably an acyl group having 5 to 13 carbon atoms. The alkoxycarbonyl group is more preferably an alkoxycarbonyl group having 2 to 13 carbon atoms, and even more preferably an alkoxycarbonyl group having 5 to 13 carbon atoms. In this way, by introducing a long-chain substituent, the crystal is easily collapsed, the light melting property is improved, and when used in a toner, the fixability is improved.
[0035] Examples of the alkyl group having 1 to 18 carbon atoms are not particularly limited, and include linear alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an isobutyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, and an n-hexadecyl group; an isopropyl group, a sec-butyl group, a t Examples of branched alkyl groups include t-butyl, 1-methylpentyl, 4-methyl-2-pentyl, 3,3-dimethylbutyl, 2-ethylbutyl, 1-methylhexyl, t-octyl, 1-methylheptyl, 2-ethylhexyl, 2-propylpentyl, 2,2-dimethylheptyl, 2,6-dimethyl-4-heptyl, 3,5,5-trimethylhexyl, 1-methyldecyl, and 1-hexylheptyl groups.
[0036] Examples of alkoxy groups having 1 to 18 carbon atoms include linear alkoxy groups such as methoxy group, ethoxy group, n-propoxy group, n-butoxy group, n-hexyloxy group, n-heptyloxy group, n-octyloxy group, n-nonyloxy group, n-decyloxy group, n-undecyloxy group, n-dodecyloxy group, n-tridecyloxy group, n-tetradecyloxy group, n-pentadecyloxy group, and n-hexadecyloxy group; 1-methylpentyloxy group, 4-methyl-2-methylpentyloxy group, and 5-methyl-2-methylpentyloxy group. Examples of branched alkoxy groups include t-pentyloxy group, 3,3-dimethylbutyloxy group, 2-ethylbutyloxy group, 1-methylhexyloxy group, t-octyloxy group, 1-methylheptyloxy group, 2-ethylhexyloxy group, 2-propylpentyloxy group, 2,2-dimethylheptyloxy group, 2,6-dimethyl-4-heptyloxy group, 3,5,5-trimethylhexyloxy group, 1-methyldecyloxy group, and 1-hexylheptyloxy group.
[0037] Examples of alkylamino groups having 1 to 10 carbon atoms include methylamino groups, ethylamino groups, n-propylamino groups, n-butylamino groups, isobutylamino groups, n-hexylamino groups, n-heptylamino groups, n-octylamino groups, n-nonylamino groups, and n-decylamino groups.
[0038] Examples of the dialkylamino group having 2 to 10 carbon atoms include a dimethylamino group, a diethylamino group, a di-n-propylamino group, a di-n-butylamino group, a di-isobutylamino group, and a methylethylamino group.
[0039] Examples of the acyl group having 2 to 19 carbon atoms include saturated or unsaturated straight-chain or branched-chain acyl groups, such as an acetyl group, a propanoyl group (propionyl group), a butanoyl group (butyryl group), an isobutanoyl group (isobutyryl group), a pentanoyl group (valeryl group), an isopentanoyl group (isovaleryl group), a sec-pentanoyl group (2-methylbutyryl group), a t-pentanoyl group (pivalyl group), and the like. Examples of such groups include hexanoyl, heptanoyl, octanoyl, t-octanoyl (2,2-dimethylhexanoyl), 2-ethylhexanoyl, nonanoyl, isononanoyl, decanoyl, isodecanoyl, undecanoyl, lauroyl, myristoyl, palmitoyl, stearoyl, behenoyl, undecylenoyl, and oleoyl groups.
[0040] Examples of the alkoxycarbonyl group having 2 to 19 carbon atoms include linear or branched alkoxycarbonyl groups such as a methoxycarbonyl group, an ethoxycarbonyl group, an n-butoxycarbonyl group, an n-hexyloxycarbonyl group, an n-heptyloxycarbonyl group, an n-octyloxycarbonyl group, an n-nonyloxycarbonyl group, an n-decyloxycarbonyl group, an n-undecyloxycarbonyl group, an n-dodecyloxycarbonyl group, an n-tridecyloxycarbonyl group, an n-tetradecyloxycarbonyl group, an n-pentadecyloxycarbonyl group, and an n-hexadecyloxycarbonyl group; Examples of branched alkoxycarbonyl groups include branched alkoxycarbonyl groups such as a 4-methyl-2-pentyloxycarbonyl group, a 3,3-dimethylbutyloxycarbonyl group, a 2-ethylbutyloxycarbonyl group, a 1-methylhexyloxycarbonyl group, a t-octyloxycarbonyl group, a 1-methylheptyloxycarbonyl group, a 2-ethylhexyloxycarbonyl group, a 2-propylpentyloxycarbonyl group, a 2,2-dimethylheptyloxycarbonyl group, a 2,6-dimethyl-4-heptyloxycarbonyl group, a 3,5,5-trimethylhexyloxycarbonyl group, a 1-methyldecyloxycarbonyl group, and a 1-hexylheptyloxycarbonyl group.
[0041] In one embodiment of the present invention, the compound represented by the general formula (1) is a compound in which the two atoms adjacent to and bonded to the carbon atom in the aromatic heterocyclic structure bonded to Z2 are both carbon atoms to which hydrogen atoms are bonded. This embodiment significantly improves the expected effects of the present invention, particularly fixability. In the aromatic heterocyclic structure, when two carbon atoms are adjacent to a carbon atom bonded to a carbon atom or nitrogen atom constituting a C=N bond and hydrogen atoms are bonded to each of the two carbon atoms, the probability of intramolecular CH-π interaction occurring between the cis isomer and the aromatic hydrocarbon ring increases. Therefore, it is considered that the cis isomer is more stabilized, and thus the fluidization accompanying photoisomerization can be more effectively expressed.
[0042] (R2) One embodiment of the present invention is a compound represented by the general formula (1), wherein R2 is represented by the following formula:
[0043] [ka]
[0044] wherein at least two of X, Y, P and Q are carbon atoms and the rest are nitrogen, sulfur or oxygen atoms, provided that at least one of X and Y is a carbon atom; R a , R b , R c and R d is R a , R b , R c and R d are present according to the valences of X, Y, P, and Q, each independently represents an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, or a hydrogen atom, provided that R a and R b At least one of the atoms bonded to the carbon atom is a hydrogen atom, and R b and R c , or R c and R d may form a condensed ring.
[0045] In one embodiment of the present invention, in the above formula, it is preferred that at least one of P and Q is a nitrogen atom, and it is more preferred that both of P and Q are nitrogen atoms.
[0046] In one embodiment of the present invention, X and Y are both carbon atoms, and R a and R b are preferably all hydrogen atoms.
[0047] In one embodiment of the present invention, R c and R dAt least one of the groups is a hydrogen atom or an alkyl group having 1 to 18 carbon atoms (for example, an alkyl group having 1 to 12 carbon atoms, preferably an alkyl group having 3 to 8 carbon atoms, and more preferably an alkyl group having 4 to 6 carbon atoms). In particular, by using an alkyl group having 4 or more carbon atoms, the desired effect of the present invention (particularly the effect of improving fixability when used in a toner) can be efficiently achieved.
[0048] Another embodiment of the present invention is a compound represented by the following formula (1), wherein R2 is:
[0049] [ka]
[0050] In the formula, R c is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or an alkoxy group having 1 to 18 carbon atoms. By adopting such an embodiment, the desired effect of the present invention (particularly the effect of improving fixability) can be efficiently achieved. Preferably, R c is a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 4 to 12 carbon atoms. By adopting such an embodiment, the desired effects of the present invention (particularly the effect of improving fixability) can be efficiently achieved.
[0051] <Method for producing photoresponsive compound> The synthesis method of the azomethine compound of the present invention is not particularly limited. For example, a compound represented by the general formula (1) in which Z1 is N, Z2 is CH, R1 is a 4-decyloxyphenyl group, and R2 is a 1-methyl-4-pyrazolyl group can be synthesized according to the following scheme 1.
[0052] In ethanol (EtOH), 4-decyloxybenzeneamine (4-decyloxyaniline) and 1-methyl-1H-pyrazole-4-carboxaldehyde are reacted with each other by heating and stirring, the reaction liquid is filtered, the resulting powder is washed with cooled ethanol, and recrystallized with methanol / ethanol to obtain the target azomethine compound (see Scheme 1 below). The temperature during heating and stirring is preferably within the range of 0°C to 100°C, more preferably within the range of 30°C to 70°C, and even more preferably within the range of 40°C to 60°C.
[0053] [ka]
[0054] Furthermore, for example, a compound in which Z1 is N, Z2 is CH, R1 is a 4-hexyloxyphenyl group, and R2 is a 5-methyl-2-thienyl group in general formula (1) can be synthesized according to the following scheme 2.
[0055] In ethanol (EtOH), 4-(hexyloxy)aniline and 5-methylthiophene-2-carboxaldehyde are reacted with each other by heating and stirring, the reaction liquid is filtered, the obtained powder is washed with cooled ethanol, and recrystallized with methanol / ethanol to obtain the target azomethine compound (see Scheme 2 below). The temperature during heating and stirring is not particularly limited, but is, for example, the same as that of the reaction in Scheme 1 above.
[0056] [ka]
[0057] Azomethine compounds other than those mentioned above can be synthesized in a similar manner by appropriately changing the raw materials with reference to the above schemes 1 and 2. For example, when preparing a compound in which Z1 and Z2 of the compound obtained by the reaction of the above scheme 2 are interchanged, that is, a compound in which Z1 is CH, Z2 is N, R1 is a 4-hexyloxyphenyl group, and R2 is a 5-methyl-2-thienyl group, the raw materials can be changed to 4-(hexyloxy)benzaldehyde and 5-methyl-2-thienylamine and the synthesis can be performed with reference to the above scheme 2.
[0058] The azomethine compounds of the present invention can be used alone or in combination of two or more kinds.
[0059] The molecular weight of the compound represented by the above general formula (1) of the present invention is not particularly limited, but is preferably 100 or more and less than 1000, and more preferably 100 or more and 800 or less. The compound represented by the above general formula (1) of the present invention does not include a polymer. In a preferred embodiment, the compound represented by the above general formula (1) is configured without including a repeating unit. In a preferred embodiment, the compound represented by the above general formula (1) is not obtained by polymerizing a monomer containing a polymerizable group.
[0060] One embodiment of the present invention relates to a photoresponsive compound that is fluidized and reversibly non-fluidized by light irradiation and is represented by the following general formula (1):
[0061] [ka]
[0062] (wherein Z1 and Z2 are N or CH, with the proviso that Z1≠Z2, R1 comprises an aromatic hydrocarbon structure, R2 comprises an aromatic heterocyclic structure, and a hydrogen atom is bonded to at least one carbon atom adjacent to the carbon atom in the aromatic heterocyclic structure bonded to Z2; However, this does not include the following compounds 1) and 2) (compounds specifically disclosed in Tables 1 and 2).
[0063] 1) A compound represented by the following chemical formula 1, which is reversibly fluidized and non-fluidized by irradiation with light, wherein X, Y, Z1, Z2, R1 to R 10 is a compound represented by the following Table 1 (in Table 1, "group of formula 2" is a group represented by the following chemical formula 2):
[0064] [ka]
[0065] 2) A photoresponsive compound that is fluidized and reversibly non-fluidized by irradiation with light and is represented by the following general formula (1), in which Z1, Z2, A and B are compounds shown in Table 2 below.
[0066] [ka]
[0067] [Table 1-1]
[0068] [Table 1-2]
[0069] [Table 1-3]
[0070] [Table 2-1]
[0071] [Table 2-2]
[0072] [Table 2-3]
[0073] [Table 2-4]
[0074] [Table 2-5]
[0075] <Fluidization and reversible non-fluidization by light irradiation> The wavelength of the irradiated light when the compound of the present invention is fluidized by light irradiation is preferably in the range of 280 nm to 480 nm, more preferably in the range of 300 nm to 420 nm, and even more preferably in the range of 330 nm to 420 nm. Within the above range, the crystals are easily broken (improved light melting property), and the fixability is improved. In addition, when fluidizing, heat or pressure may be applied in addition to light irradiation to promote fluidization. By irradiating with light of the above wavelength, even when heat or pressure is applied, it is possible to fluidize with less heat or pressure. Therefore, by introducing the compound of the present invention into a toner, fixation at the above wavelength is possible, and a toner with excellent fixability and high color reproducibility can be obtained.
[0076] The above wavelength range includes a part of visible light. Therefore, it is desirable that the compound of the present invention is not fluidized by only receiving light from sunlight (natural light) or fluorescent lamps, and is more fluidized under low-cost conditions with the amount and time of irradiation kept as low as possible. From this viewpoint, the irradiation conditions for the light irradiation when the compound is fluidized are preferably an amount of irradiation of 0.1 J / cm. 2 More than 200J / cm 2 Within the range of 0.1 J / cm 2 More than 100J / cm 2 Within the range below, more preferably 0.1 J / cm 2More than 50J / cm 2 It is within the following range.
[0077] When the compound is fluidized, the compound may be heated together with the light irradiation. This allows the compound to be fluidized with a lower irradiation dose. The heating temperature in this case is, for example, in the range of 20°C to 200°C, preferably in the range of 20°C to 150°C.
[0078] On the other hand, the conditions for immobilizing (resolidifying) the compound of the present invention are preferably left at room temperature (within the range of 25±15° C.) (in a natural environment). In this case, it is preferable to leave it in a dark place, but it may be exposed to visible light such as natural light or fluorescent light. It is more preferable to apply heat during the immobilization process. Light may also be applied.
[0079] When the compound is heated to make it non-fluid, the heating temperature is preferably in the range of 0°C or higher and 200°C or lower, more preferably in the range of 20°C or higher and 150°C or lower.
[0080] [Toner composition] One embodiment of the present invention is a toner containing the compound of the present invention. By introducing the compound of the present invention into a toner, it is possible to obtain a toner that can be fixed by light irradiation, has excellent fixability, and has high color reproducibility. The term "toner" refers to toner base particles or an aggregate of toner particles. The toner particles are preferably toner base particles to which an external additive has been added, but the toner base particles can also be used as they are as toner particles. In the present invention, when there is no particular need to distinguish between the toner base particles, the toner particles, and the toner, they are also simply referred to as "toner".
[0081] (Binding resin) The toner of the present invention preferably further contains a binder resin in addition to the predetermined azomethine compound of the present invention. It is generally known that toner particles having a substantially uniform particle size and shape can be produced by utilizing the emulsion aggregation method described below as a method for producing a toner. It is possible to produce a toner by using the azomethine compound alone or by adding other additives such as a colorant or a release agent without using a binder resin. By using the azomethine compound in combination with a binder resin, toner particles having a substantially uniform particle size and shape can be produced by salting out in the emulsion aggregation method. Therefore, a toner containing the azomethine compound and a binder resin can be more easily applied to an electrophotographic toner.
[0082] The binder resin may be any resin that is generally used as a binder resin constituting a toner without any restrictions. For example, styrene resin, acrylic resin, styrene-acrylic resin, polyester resin, silicone resin, olefin resin, amide resin, and epoxy resin may be used. These binder resins may be used alone or in combination of two or more kinds.
[0083] Among these, from the viewpoint of having a low viscosity when melted and a high sharp melting property, the binder resin preferably contains at least one selected from the group consisting of styrene resin, acrylic resin, styrene-acrylic resin, and polyester resin, and more preferably contains at least one selected from the group consisting of styrene-acrylic resin and polyester resin. By adopting such an embodiment, the image strength can be increased.
[0084] (styrene acrylic resin) The styrene-acrylic resin in the present invention is a polymer containing at least a structural unit derived from a styrene monomer and a structural unit derived from a (meth)acrylic acid ester monomer. Here, the styrene monomer includes not only styrene represented by the structural formula CH2=CH-C6H5, but also structures having a known side chain or functional group in the styrene structure.
[0085] Examples of the styrene monomer include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-phenylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, pt-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene.
[0086] Moreover, the (meth)acrylic acid ester monomer has a functional group having an ester bond in the side chain. Specifically, in addition to the acrylic acid ester monomer represented by CH2=CHCOOR (R is an alkyl group), it includes vinyl ester compounds such as the methacrylic acid ester monomer represented by CH2=C(CH3)COOR (R is an alkyl group). Note that (meth)acrylic acid in the (meth)acrylic acid ester monomer means acrylic acid and methacrylic acid.
[0087] Examples of (meth)acrylic acid ester monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate.
[0088] The styrene monomer and the (meth)acrylic acid ester monomer can be used either alone or in combination of two or more kinds.
[0089] The content of the structural unit derived from the styrene monomer and the structural unit derived from the (meth)acrylic acid ester monomer in the styrene-acrylic resin is not particularly limited, and can be appropriately adjusted from the viewpoint of controlling the softening point and glass transition temperature of the binder resin. Specifically, the content of the structural unit derived from the styrene monomer is preferably 40 to 95 mass% and more preferably 50 to 90 mass% based on the total structural units constituting the styrene-acrylic resin. In addition, the content of the structural unit derived from the (meth)acrylic acid ester monomer is preferably 5 to 60 mass% and more preferably 10 to 50 mass% based on the total structural units.
[0090] The styrene-acrylic resin may further contain structural units derived from other monomers than the styrene monomer and the (meth)acrylic acid ester monomer, if necessary. Examples of other monomers include vinyl monomers. Below, examples of vinyl monomers that can be used in combination when forming the styrene-acrylic copolymer of the present invention are shown, but the vinyl monomers that can be used in combination are not limited to those shown below.
[0091] (1) Olefins Ethylene, propylene, isobutylene, etc. (2) Vinyl esters Vinyl propionate, vinyl acetate, vinyl benzoate, etc. (3) Vinyl ethers Vinyl methyl ether, vinyl ethyl ether, etc. (4) Vinyl ketones Vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc. (5) N-vinyl compounds N-vinylcarbazole, N-vinylindole, N-vinylpyrrolidone, etc. (6)Other Vinyl compounds such as vinylnaphthalene and vinylpyridine, acrylic acid or methacrylic acid derivatives such as acrylonitrile, methacrylonitrile and acrylamide, and the like.
[0092] It is also possible to prepare a resin having a crosslinked structure by using a polyfunctional vinyl monomer. Furthermore, it is also possible to use a vinyl monomer having an ionic dissociation group in the side chain. Specific examples of the ionic dissociation group include a carboxyl group, a sulfonic acid group, and a phosphoric acid group. Specific examples of the vinyl monomer having these ionic dissociation groups are shown below.
[0093] Specific examples of vinyl monomers having a carboxyl group include acrylic acid, methacrylic acid, maleic acid, itaconic acid, cinnamic acid, fumaric acid, maleic acid monoalkyl esters, and itaconic acid monoalkyl esters.
[0094] When forming the styrene-acrylic resin used in the present invention, the contents of the styrene monomer and the (meth)acrylic acid ester monomer are not particularly limited, and can be appropriately adjusted from the viewpoint of controlling the softening point temperature and the glass transition temperature of the binder resin. Specifically, the content of the styrene monomer is preferably 40 to 95 mass% and more preferably 50 to 90 mass% based on the total monomers constituting the styrene-acrylic resin. In addition, the content of the (meth)acrylic acid ester monomer is preferably 5 to 60 mass% and more preferably 10 to 50 mass% based on the total monomers constituting the styrene-acrylic resin.
[0095] The method for forming the styrene-acrylic resin is not particularly limited, and may be a method of polymerizing a monomer using a known oil-soluble or water-soluble polymerization initiator. If necessary, a known chain transfer agent such as n-octyl mercaptan may be used. As the oil-soluble polymerization initiator, for example, the following azo-based or diazo-based polymerization initiator or peroxide-based polymerization initiator may be used.
[0096] Examples of the azo or diazo polymerization initiator include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, and azobisisobutyronitrile.
[0097] Examples of the peroxide polymerization initiator include benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, 2,2-bis-(4,4-t-butylperoxycyclohexyl)propane, and tris-(t-butylperoxy)triazine.
[0098] In addition, when forming styrene-acrylic resin particles by emulsion polymerization, a water-soluble radical polymerization initiator can be used. Examples of the water-soluble radical polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate, azobisaminodipropane acetate, azobiscyanovaleric acid and its salts, and hydrogen peroxide.
[0099] The polymerization temperature varies depending on the types of monomers and polymerization initiators used, but is preferably 50 to 100° C., and more preferably 55 to 90° C. The polymerization time varies depending on the types of monomers and polymerization initiators used, but is preferably, for example, 2 to 12 hours.
[0100] The styrene-acrylic resin particles formed by emulsion polymerization can be made to have two or more layers made of resins with different compositions. In this case, the manufacturing method can be a multi-stage polymerization method in which a polymerization initiator and a polymerizable monomer are added to a dispersion of resin particles prepared by emulsion polymerization treatment (first stage polymerization) according to a conventional method, and this system is polymerized (second stage, third stage polymerization).
[0101] (polyester resin) The polyester resin is obtained by a polycondensation reaction between a divalent or higher carboxylic acid (a polyvalent carboxylic acid component) and a divalent or higher alcohol (a polyhydric alcohol component). The polyester resin may be amorphous or crystalline.
[0102] The valence of each of the polyvalent carboxylic acid component and the polyhydric alcohol component is preferably 2 to 3, and more preferably 2. That is, the polyvalent carboxylic acid component preferably contains a dicarboxylic acid component, and the polyhydric alcohol component preferably contains a dialcohol component.
[0103] Examples of the dicarboxylic acid component include saturated aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid (dodecanedioic acid), 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and methylenesuccinic acid. unsaturated aliphatic dicarboxylic acids such as fumaric acid, maleic acid, 3-hexenedioic acid, 3-octenedioic acid, and dodecenylsuccinic acid; unsaturated aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, t-butylisophthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-phenylenediacetic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, and anthracenedicarboxylic acid; and lower alkyl esters and acid anhydrides of these may also be used. The dicarboxylic acid component may be used alone or in combination of two or more.
[0104] In addition, trivalent or higher polyvalent carboxylic acids such as trimellitic acid and pyromellitic acid, and their anhydrides or alkyl esters having 1 to 3 carbon atoms can also be used.
[0105] Examples of the diol component include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,20-eicosanediol, and neopentanediol. Examples of the diol component include saturated aliphatic diols such as ethyl glycol; unsaturated aliphatic diols such as 2-butene-1,4-diol, 3-butene-1,4-diol, 2-butyne-1,4-diol, 3-butyne-1,4-diol, and 9-octadecene-7,12-diol; and aromatic diols such as bisphenols such as bisphenol A and bisphenol F, and alkylene oxide adducts of bisphenols such as ethylene oxide adducts and propylene oxide adducts thereof, and derivatives thereof can also be used. The diol component may be used alone or in combination of two or more kinds.
[0106] The method for producing the polyester resin is not particularly limited, and the polyester resin can be produced by polycondensing (esterifying) the polyvalent carboxylic acid component and the polyhydric alcohol component using a known esterification catalyst.
[0107] Examples of catalysts that can be used in the production of polyester resins include alkali metal compounds such as sodium and lithium; compounds containing group 2 elements such as magnesium and calcium; compounds of metals such as aluminum, zinc, manganese, antimony, titanium, tin, zirconium, and germanium; phosphorous compounds; phosphoric acid compounds; and amine compounds. Specifically, examples of tin compounds include dibutyltin oxide (dibutyltin oxide), tin octoate, tin dioctoate, and salts thereof. Examples of titanium compounds include titanium alkoxides such as tetra-normal-butyl titanate (Ti(On-Bu)4), tetraisopropyl titanate, tetramethyl titanate, and tetrastearyl titanate; titanium acylates such as polyhydroxytitanium stearate; and titanium chelates such as titanium tetraacetylacetonate, titanium lactate, and titanium triethanolamine. Examples of germanium compounds include germanium dioxide. Examples of aluminum compounds include polyaluminum hydroxide, aluminum alkoxide, and tributylaluminate. These may be used alone or in combination of two or more.
[0108] The polymerization temperature is not particularly limited, but is preferably 70 to 250° C. The polymerization time is also not particularly limited, but is preferably 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.
[0109] When the toner of the present invention contains a binder resin, the content of the azomethine compound depends on the type of compound and the type of resin, but from the viewpoint of fixability and color reproducibility, the azomethine compound:binder resin is preferably in the range of 5:95 to 95:5 (mass ratio), more preferably in the range of 10:90 to 90:10 (mass ratio), more preferably in the range of 10:90 to 80:20 (mass ratio), and even more preferably in the range of 10:90 to 70:30 (mass ratio). Within this range, the photo-induced phase transition of the compound having the azomethine moiety is easily caused, and the toner has a sufficient softening speed due to light irradiation. When two or more kinds of azomethine compounds are used, the total amount thereof is preferably in the above range. When two or more kinds of binder resins are used, the total amount thereof is preferably in the above range.
[0110] From the viewpoints of fixability, heat-resistant storage stability, etc., the glass transition temperature (Tg) of the toner is preferably 25 to 100° C., and more preferably 30 to 80° C. When the toner contains a binder resin, the glass transition temperature (Tg) of the toner can be adjusted by the content, type, molecular weight, etc. of the binder resin.
[0111] The toner of the present invention may be particles having a single layer structure or particles having a core-shell structure. The types of binder resins used for the core particles and shell part of the core-shell structure are not particularly limited.
[0112] <Coloring agent> The toner of the present invention may further contain a colorant. Since the compound of the present invention does not cause significant coloring, a toner having high color reproducibility of the colorant can be obtained. As the colorant, generally known dyes and pigments can be used.
[0113] Examples of colorants for obtaining black toner include carbon black, magnetic materials, iron-titanium composite oxide black, etc. Examples of carbon black include channel black, furnace black, acetylene black, thermal black, and lamp black, and examples of magnetic materials include ferrite and magnetite.
[0114] Colorants for obtaining yellow toners include dyes such as CI Solvent Yellow 19, 44, 77, 79, 81, 82, 93, 98, 103, 104, 112, and 162; and pigments such as CI Pigment Yellow 14, 17, 74, 93, 94, 138, 155, 180, and 185.
[0115] Colorants for obtaining magenta toner include dyes such as CI Solvent Red 1, 49, 52, 58, 63, 111, and 122; and pigments such as CI Pigment Red 5, 48:1, 53:1, 57:1, 122, 139, 144, 149, 166, 177, 178, and 222.
[0116] Colorants for obtaining cyan toner include dyes such as CI Solvent Blue 25, 36, 60, 70, 93, and 95; and pigments such as CI Pigment Blue 1, 7, 15, 15:3, 60, 62, 66, and 76.
[0117] The colorants for obtaining the toner of each color may be used alone or in combination of two or more kinds for each color.
[0118] The content of the colorant in the toner particles (toner base particles) before addition of external additives is preferably 0.5 to 20% by mass, and more preferably 2 to 10% by mass.
[0119] <Release agent> The toner according to the present invention may further contain a release agent. By incorporating a release agent into the toner, a toner having superior fixability and color reproducibility can be obtained when thermal fixing is performed together with light irradiation.
[0120] The release agent used is not particularly limited, and various known waxes can be used. Examples of the wax include polyolefins such as low molecular weight polypropylene, polyethylene, or oxidized low molecular weight polypropylene, polyethylene, paraffin wax, and synthetic ester wax. Among them, it is preferable to use paraffin wax from the viewpoint of improving the storage stability of the toner.
[0121] The content of the release agent in the toner base particles is preferably 1 to 30% by mass, and more preferably 3 to 15% by mass.
[0122] <Charge control agent> The toner according to the present invention may contain a charge control agent. The charge control agent used is a substance capable of imparting positive or negative charge by frictional charging, and is colorless, and is not particularly limited. Any of various known positively and negatively chargeable charge control agents can be used.
[0123] The content of the charge control agent in the toner base particles is preferably 0.01 to 30% by mass, and more preferably 0.1 to 10% by mass.
[0124] The amount of the compound of the present invention in the toner is not particularly limited, but from the viewpoint of efficient fluidization and image strength, it is, for example, in the range of 5 to 95 mass % based on the total amount of the binder resin, colorant, release agent, and compound of the present invention that constitute the toner.
[0125] <External additives> In order to improve the fluidity, chargeability, cleaning properties, etc. of the toner, external additives such as a fluidizing agent, a cleaning aid, etc., which are so-called post-treatment agents, may be added to the toner base particles to form the toner according to the present invention.
[0126] Examples of the external additive include inorganic oxide particles such as silica particles, alumina particles, and titanium oxide particles, inorganic stearic acid compound particles such as aluminum stearate particles and zinc stearate particles, and inorganic titanic acid compound particles such as strontium titanate particles and zinc titanate particles. If necessary, these inorganic particles may be hydrophobized. These may be used alone or in combination of two or more.
[0127] Among these, preferred external additives are, for example, sol-gel silica particles, silica particles whose surfaces have been hydrophobized (hydrophobic silica particles), or titanium oxide particles (hydrophobic titanium oxide particles), and it is more preferred to use at least two or more types of external additives among these.
[0128] The number average primary particle size of the external additive is preferably within the range of 1 to 200 nm, and more preferably 10 to 180 nm.
[0129] The amount of these external additives added is preferably 0.05 to 5% by mass, and more preferably 0.1 to 3% by mass, in the toner.
[0130] In one embodiment of the present invention, the amount of these external additives added is preferably 0.5 to 5% by mass, and more preferably 0.1 to 3% by mass, based on the toner base particles.
[0131] <Average particle size of toner> The average particle size of the toner (and the average particle size of the toner base particles) is preferably 4 to 20 μm, more preferably 5 to 15 μm, in terms of volume-based median diameter (D50). When the volume-based median diameter (D50) is within the above range, the transfer efficiency is increased, and the image quality of halftones and fine lines, dots, etc. is improved.
[0132] The volume-based median diameter (D50) can be measured and calculated using a measuring device consisting of a "Coulter Counter 3" (Beckman Coulter, Inc.) connected to a computer system (Beckman Coulter, Inc.) equipped with the data processing software "Software V3.51."
[0133] Specifically, 0.02 g of the measurement sample (toner or toner base particles) is added to 20 mL of surfactant solution (a surfactant solution prepared by diluting, for example, a neutral detergent containing surfactant components 10 times with pure water in order to disperse toner particles), and after mixing, ultrasonic dispersion is performed for 1 minute to prepare a dispersion liquid. This dispersion liquid is then pipetted into a beaker containing an "ISOTON II" (manufactured by Beckman Coulter, Inc.) in the sample stand until the concentration indicated on the measuring device reaches 8%.
[0134] Here, by setting the display concentration within the above range, it is possible to obtain reproducible measurement values. In the measurement device, the number of measured particles is set to 25,000, the aperture diameter is set to 50 μm, the measurement range of 1 to 30 μm is divided into 256 parts to calculate the frequency value, and the particle size with the largest volume cumulative fraction of 50% is set as the volume-based median diameter (D50).
[0135] [Toner manufacturing method] The method for producing the toner of the present invention is not particularly limited. For example, when the toner is made from only the compound of the present invention, a production method including pulverizing the compound using a device such as a hammer mill, feather mill, or counter jet mill, and then classifying the particles to a desired particle size using a dry classifier such as a spin air sieve, a classifier, or a micron classifier can be used. When a toner further containing a colorant is produced, the compound and the colorant are dissolved in a solvent in which both the compound of the present invention and the colorant are soluble to obtain a solution, the solvent is removed, and the solution is pulverized and classified in the same manner as above.
[0136] In particular, a toner containing the compound of the present invention, a binder resin, and, if necessary, additives such as a colorant, is preferably produced by a production method utilizing an emulsion aggregation method, which allows easy control of particle size and shape.
[0137] Such a manufacturing method is as follows: (1A) Binder resin particle dispersion preparation step of preparing a binder resin particle dispersion (1B) A compound particle dispersion preparation step for preparing a dispersion of particles of the compound of the present invention (1C) A colorant particle dispersion preparation step of preparing a colorant particle dispersion as required. (2) An association step in which a flocculant is added to an aqueous medium in which compound particles, binder resin particles, and, if necessary, colorant particles are present, and salting out is promoted while simultaneously flocculation and fusion are carried out to form associated particles. (3) Aging process to form toner base particles by controlling the shape of aggregated particles (4) A filtering and washing process for filtering the toner base particles from the aqueous medium and removing surfactants and the like from the toner base particles. (5) A drying process for drying the washed toner base particles. (6) Additive addition step of adding additives to the dried toner base particles It is preferable that the method includes each of the steps of:
[0138] The steps (1A) to (1C) are described below.
[0139] (1A) Binder resin particle dispersion preparation process In this process, resin particles are formed by a conventional emulsion polymerization or the like, and the resin particles are aggregated and fused to form binder resin particles. As an example, polymerizable monomers constituting the binder resin are introduced into an aqueous medium, dispersed therein, and polymerized by a polymerization initiator to prepare a dispersion of binder resin particles.
[0140] As a method for obtaining a binder resin particle dispersion, in addition to the above-mentioned method of polymerizing a polymerizable monomer in an aqueous medium by a polymerization initiator, for example, a method of performing a dispersion treatment in an aqueous medium without using a solvent, or a method of dissolving a crystalline resin in a solvent such as ethyl acetate to prepare a solution, emulsifying and dispersing the solution in an aqueous medium using a disperser, and then performing a solvent removal treatment, can be mentioned.
[0141] In this case, if necessary, a release agent may be added to the binder resin in advance. For dispersion, it is also preferable to carry out the polymerization in the presence of a known surfactant (for example, an anionic surfactant such as polyoxyethylene (2) dodecyl ether sodium sulfate, sodium dodecyl sulfate, or dodecylbenzenesulfonic acid).
[0142] The volume-based median diameter of the binder resin particles in the dispersion is preferably 50 to 300 nm. The volume-based median diameter of the binder resin particles in the dispersion can be measured by a dynamic light scattering method using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.).
[0143] (1B) Compound particle dispersion preparation process The compound particle dispersion preparation step is a step of dispersing the compound of the present invention in the form of fine particles in an aqueous medium to prepare a dispersion of particles of the compound.
[0144] In preparing a dispersion of particles of the compound, first, an emulsion of the compound is prepared. For example, the emulsion of the compound can be prepared by dissolving the compound in an organic solvent and then emulsifying the obtained solution in an aqueous medium.
[0145] The method of dissolving the compound in the organic solvent is not particularly limited, and examples thereof include a method of adding the compound to the organic solvent and stirring and mixing the compound so that the compound is dissolved. The amount of the compound added is preferably 5 parts by mass or more and 100 parts by mass or less, more preferably 10 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the organic solvent.
[0146] Next, the obtained solution of the compound is mixed with an aqueous medium and stirred using a known dispersing machine such as a homogenizer, whereby the compound becomes droplets and is emulsified in the aqueous medium, thereby preparing an emulsion of the compound.
[0147] The amount of the solution of the compound added is preferably 10 parts by mass or more and 110 parts by mass or less with respect to 100 parts by mass of the aqueous medium.
[0148] The temperatures of the compound solution and the aqueous medium when the compound solution and the aqueous medium are in a temperature range below the boiling point of the organic solvent, and are preferably from 20° C. to 80° C., more preferably from 30° C. to 75° C. When the compound solution and the aqueous medium are mixed, the temperatures of the compound solution and the aqueous medium may be the same or different, and are preferably the same.
[0149] Regarding the stirring conditions of the dispersing machine, when the capacity of the stirring vessel is 1 to 3 L, for example, the rotation speed is preferably 7000 rpm or more and 20000 rpm or less, and the stirring time is preferably 10 minutes or more and 30 minutes or less.
[0150] The dispersion of the compound particles is prepared by removing the organic solvent from the emulsion of the compound. Examples of the method for removing the organic solvent from the emulsion of the compound include known methods such as blowing air, heating, reducing pressure, or a combination of these.
[0151] As an example, the emulsion of the compound is heated, for example, in an inert gas atmosphere such as nitrogen, preferably at 25° C. to 90° C., more preferably at 30° C. to 80° C., until, for example, about 80% by mass to 95% by mass of the initial amount of organic solvent is removed (for example, for 20 to 150 minutes), thereby removing the organic solvent. As a result, the organic solvent is removed from the aqueous medium, and a dispersion of the compound particles in which the particles of the compound are dispersed in the aqueous medium is prepared.
[0152] The mass average particle diameter of the compound particles in the dispersion of the compound particles is preferably 90 nm or more and 1200 nm or less. The mass average particle diameter can be set within the above range by appropriately adjusting the viscosity when the compound is mixed with an organic solvent, the mixing ratio of the solution of the compound to the aqueous medium, the stirring speed of the dispersing machine when preparing the emulsion of the compound, etc. The mass average particle diameter of the compound particles in the dispersion of the compound particles can be measured using Microtrac UPA-150 (manufactured by Nikkiso Co., Ltd.) or an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).
[0153] <Organic solvent> The organic solvent used in this step is not particularly limited as long as it can dissolve the compound.Specific examples of the organic solvent include esters such as ethyl acetate and butyl acetate, ethers such as diethyl ether, diisopropyl ether, and tetrahydrofuran, ketones such as acetone and methyl ethyl ketone, saturated hydrocarbons such as hexane and heptane, and halogenated hydrocarbons such as dichloromethane, dichloroethane, and carbon tetrachloride.
[0154] Such organic solvents can be used alone or in combination of two or more kinds. Among these organic solvents, ketones and halogenated hydrocarbons are preferred, and methyl ethyl ketone and dichloromethane are more preferred.
[0155] <Aqueous medium> The aqueous medium used in this step may be water, or an aqueous medium containing water as the main component and water-soluble solvents such as alcohols and glycols, and optional components such as surfactants and dispersants. The aqueous medium used is preferably a mixture of water and a surfactant.
[0156] Examples of the surfactant include cationic surfactants, anionic surfactants, and nonionic surfactants. Examples of the cationic surfactant include dodecyl ammonium chloride, dodecyl ammonium bromide, dodecyl trimethyl ammonium bromide, dodecyl pyridinium chloride, dodecyl pyridinium bromide, and hexadecyl trimethyl ammonium bromide. Examples of the anionic surfactant include fatty acid soaps such as sodium stearate and sodium dodecanoate, sodium dodecyl benzene sulfonate, and sodium dodecyl sulfate. Examples of the nonionic surfactant include polyoxyethylene dodecyl ether, polyoxyethylene hexadecyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene dodecyl ether, polyoxyethylene sorbitan monooleate ether, and monodecanoyl sucrose.
[0157] Such surfactants can be used alone or in combination of two or more. Among the surfactants, anionic surfactants are preferred, and sodium dodecylbenzenesulfonate is more preferred.
[0158] The amount of the surfactant added is preferably 0.01 to 10 parts by mass, more preferably 0.04 to 1 part by mass, in terms of solid content, relative to 100 parts by mass of the aqueous medium.
[0159] (1C) Colorant particle dispersion preparation process The colorant particle dispersion preparation step is a step of dispersing a colorant in the form of fine particles in an aqueous medium to prepare a colorant particle dispersion.
[0160] The colorant can be dispersed by utilizing mechanical energy. The median diameter based on the number of colorant particles in the dispersion is preferably 10 to 300 nm, and more preferably 50 to 200 nm. The median diameter based on the number of colorant particles can be measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).
[0161] The steps from (2) association step to (6) external additive addition step can be carried out according to various conventionally known methods.
[0162] The flocculant used in the (2) association step is not particularly limited, but is preferably selected from metal salts. Examples of metal salts include monovalent metal salts such as salts of alkali metals such as sodium, potassium, and lithium; divalent metal salts such as calcium, magnesium, manganese, and copper; and trivalent metal salts such as iron and aluminum. Specific examples of metal salts include sodium chloride, potassium chloride, lithium chloride, calcium chloride, magnesium chloride, zinc chloride, copper sulfate, magnesium sulfate, and manganese sulfate. Among these, it is particularly preferable to use divalent metal salts because they can promote flocculation with a smaller amount. These can be used alone or in combination of two or more.
[0163] [Developer] The toner according to the present invention may be used, for example, as a one-component magnetic toner by incorporating a magnetic material, as a two-component developer by mixing with a so-called carrier, or as a non-magnetic toner by itself, and any of these may be suitably used.
[0164] As the magnetic material, for example, magnetite, γ-hematite, or various ferrites can be used.
[0165] The carrier contained in the two-component developer may be magnetic particles made of conventionally known materials such as metals such as iron, steel, nickel, cobalt, ferrite, and magnetite, and alloys of these metals with metals such as aluminum and lead.
[0166] The carrier may be a coated carrier in which the surface of the magnetic particles is coated with a coating agent such as a resin, or a resin-dispersed carrier in which magnetic powder is dispersed in a binder resin. The resin for coating is not particularly limited, but for example, olefin resin, acrylic resin, styrene resin, styrene-acrylic resin, silicone resin, polyester resin, or fluororesin is used. The resin for constituting the resin-dispersed carrier particles is not particularly limited, and known resins can be used, for example, acrylic resin, styrene-acrylic resin, polyester resin, fluororesin, phenolic resin, etc. can be used.
[0167] The volume-based median diameter of the carrier is preferably 20 to 100 μm, and more preferably 25 to 80 μm. The volume-based median diameter of the carrier can be measured typically by a laser diffraction particle size distribution measuring device "HELOS" (manufactured by SYMPATEC) equipped with a wet disperser.
[0168] The mixed amount of the toner is preferably 2 to 10% by mass, with the total mass of the toner and carrier being 100% by mass.
[0169] [Image forming method] The toner of the present invention can be used in various known electrophotographic image forming methods. For example, it can be used in monochrome image forming methods and full-color image forming methods. In the full-color image forming method, it can be applied to any image forming method, such as a four-cycle image forming method that is composed of four types of color developing devices for yellow, magenta, cyan, and black, and one photoconductor, and a tandem image forming method that is equipped with image forming units having color developing devices and photoconductors for each color, respectively.
[0170] That is, an image forming method according to one embodiment of the present invention includes the steps of 1) forming a toner image made of the toner of the present invention on a recording medium, and 2) irradiating the toner image with light to soften the toner image. This embodiment provides excellent fixability and high image quality.
[0171] Regarding step 1) In this process, a toner image made of the toner of the present invention is formed on a recording medium.
[0172] (Recording medium) The recording medium is a member for holding a toner image. Examples of the recording medium include plain paper, high-quality paper, art paper, coated printing paper such as coated paper, commercially available Japanese paper and postcard paper, resin films for overhead projectors or packaging materials, and cloth.
[0173] The recording medium may be in the form of a sheet (foliage) having a predetermined size, or may be in the form of a long piece that is wound up in a roll after the toner image is fixed thereon.
[0174] As described later, the toner image can be formed, for example, by transferring the toner image on the photoconductor onto a recording medium.
[0175] Regarding step 2) In this process, the formed toner image is irradiated with light to soften the toner image, which allows the toner image to adhere to a recording medium.
[0176] The wavelength of the irradiated light is not particularly limited as long as it can sufficiently soften the toner image by photothermal conversion by the compound in the toner, but is preferably 280 nm or more and 480 nm or less. If it is in the above range, the toner image can be softened more efficiently. From the same viewpoint, the amount of light irradiation is preferably 0.1 to 200 J / cm. 2 , more preferably 0.1 to 100 J / cm 2 , and more preferably 0.1 to 50 J / cm 2 It is.
[0177] As described later, the light irradiation can be performed using a light source such as a light emitting diode (LED) or a laser light source. In addition, as described later, heating may be further performed in addition to the light irradiation.
[0178] After the step 2), if necessary, a step 3) of pressing the softened toner image may be further carried out. This embodiment improves the fixing property.
[0179] Regarding step 3) In this process, the softened toner image is pressed.
[0180] The pressure when pressing the toner image on the recording medium is not particularly limited, but is preferably 0.01 to 5.0 MPa, and more preferably 0.05 to 1.0 MPa. By setting the pressure to 0.01 MPa or more, the deformation amount of the toner image can be increased, so that the contact area between the toner image and the recording paper S increases, and it is easy to further improve the fixability of the image. In addition, by setting the pressure to 5.0 MPa or less, shock noise during pressing can be suppressed.
[0181] The pressurizing step may be carried out before or simultaneously with the step of irradiating light and softening the toner image (step 2) described above), but it is preferable to carry it out after the light irradiation, since this allows pressure to be applied to the toner image that has already been softened, thereby further improving the fixability of the image.
[0182] In addition, in the pressurizing step, the softened toner image may be further heated. That is, the pressurizing step may be performed while heating the toner image. The temperature at that time (for example, the temperature of the pressing member) is preferably 15°C or higher, more preferably 20°C or higher, even more preferably more than 20°C, even more preferably 30°C or higher, and even more preferably 40°C or higher. This embodiment significantly improves the fixability. There is no particular upper limit, but it is, for example, 200°C or lower, 150°C or lower, or 100°C or lower.
[0183] The heating temperature of the toner image (the surface temperature of the toner image during heating) is preferably (Tg+20) to (Tg+100)° C., and more preferably (Tg+25) to (Tg+80)° C., where Tg is the glass transition temperature of the toner. If the surface temperature of the toner image is (Tg+20)° C. or higher, the toner image is easily deformed by pressure, and if it is (Tg+100)° C. or lower, hot offset is easily suppressed. Note that hot offset refers to a phenomenon in which part of the toner is transferred to a pressure member such as a roller during the fixing process, causing the toner layer to break up.
[0184] In addition, before the step 2), a step 4) of heating the toner image in advance may be further carried out as necessary. In this way, by further carrying out the step 4) of heating the toner image in advance before the step 2), the sensitivity of the compound of the present invention to light can be further increased. As a result, even if the compound is a polymer, the sensitivity to light is unlikely to be impaired, and therefore, the melting or softening of the toner image by light irradiation can be easily promoted.
[0185] The image forming method of the present invention can be carried out by using, for example, the following image forming apparatus.
[0186] Fig. 1 is a schematic diagram showing an image forming apparatus 100 used in an image forming method according to an embodiment of the present invention. However, the image forming apparatus used in the present invention is not limited to the following form and illustrated example. Fig. 1 shows an example of a monochrome image forming apparatus 100, but the present invention can also be applied to a color image forming apparatus.
[0187] The image forming apparatus 100 is an apparatus for forming an image on a recording paper S as a recording medium, and is equipped with an image reading device 71 and an automatic document feeder 72, and performs image formation on the recording paper S transported by a paper transport system 7 using an image forming unit 10, an irradiation unit 40, and a pressing unit 9.
[0188] Furthermore, while image forming apparatus 100 uses recording paper S as a recording medium, the medium on which an image is formed may be something other than paper.
[0189] An original d placed on the platen of the automatic document feeder 72 is scanned and exposed by the optical system of the scanning exposure device of the image reading device 71 and read into the image sensor CCD. An analog signal photoelectrically converted by the image sensor CCD is subjected to analog processing, A / D conversion, shading correction, image compression processing, etc. in the image processing unit 20, and then input to the exposure device 3 of the image forming unit 10.
[0190] The paper transport system 7 includes a plurality of trays 16, a plurality of paper feed units 11, transport rollers 12, a transport belt 13, etc. The trays 16 each store recording paper S of a predetermined size, and operate the paper feed unit 11 of the specified tray 16 in response to an instruction from the control unit 90 to supply the recording paper S. The transport rollers 12 transport the recording paper S sent out from the tray 16 by the paper feed unit 11 or the recording paper S brought in from the manual paper feed unit 15 to the image forming unit 10.
[0191] The image forming unit 10 is configured by arranging a charger 2, an exposure unit 3, a developing unit 4, a transfer unit 5 and a cleaning unit 8 in this order around the photoreceptor 1 along the direction of rotation of the photoreceptor 1.
[0192] The photoconductor 1, which is an image carrier, is an image carrier having a photoconductive layer formed on its surface, and is configured to be rotatable in the direction of the arrow in Fig. 1 by a driving device (not shown). A thermo-hygrometer 17 that detects the temperature and humidity inside the image forming apparatus 100 is provided near the photoconductor 1.
[0193] The charger 2 uniformly charges the surface of the photoreceptor 1, thereby uniformly charging the surface of the photoreceptor 1. The exposure unit 3 is equipped with a beam emission source such as a laser diode, and irradiates the charged surface of the photoreceptor 1 with a beam of light, thereby dissipating the charge in the irradiated area and forming an electrostatic latent image on the photoreceptor 1 according to the image data. The development unit 4 supplies the toner contained therein to the photoreceptor 1, and creates a toner image on the surface of the photoreceptor 1 based on the electrostatic latent image.
[0194] The transfer unit 5 faces the photoreceptor 1 via the recording paper S, and transfers the toner image onto the recording paper S. The cleaning unit 8 includes a blade 85. The blade 85 cleans the surface of the photoreceptor 1 to remove developer remaining on the surface of the photoreceptor 1.
[0195] The recording paper S onto which the toner image has been transferred is transported by a transport belt 13 to a pressing unit 9. The pressing unit 9 may be installed arbitrarily, and performs a fixing process on the recording paper S onto which the toner image has been transferred by applying pressure alone or heat and pressure with pressure members 91 and 92, thereby fixing the image onto the recording paper S. The recording paper S onto which the image has been fixed is transported by transport rollers to a paper discharge unit 14, and is discharged from the paper discharge unit 14 to the outside of the machine.
[0196] In addition, the image forming apparatus 100 is equipped with a paper inversion section 24, so that the recording paper S that has been subjected to the heat fixing process is transported to the paper inversion section 24 just before the paper discharge section 14, and the recording paper S is either inverted and discharged, or the inverted recording paper S is transported again to the image forming section 10, so that images can be formed on both sides of the recording paper S.
[0197] <Irradiation unit> FIG. 2 is a schematic diagram of the irradiation unit 40 in the image forming apparatus 100. As shown in FIG.
[0198] An image forming apparatus 100 according to an embodiment of the present invention includes an irradiation section 40. The irradiation section 40 includes a light source 41 and a heating member 93. Examples of devices constituting the light source 41 include a light emitting diode (LED) and a laser light source.
[0199] The light source 41 irradiates the toner image formed on the recording medium with light to soften the toner image. The conditions of the light irradiation are not particularly limited as long as they melt and fluidize the compound of the present invention contained in the toner of the developer. The wavelength of the light irradiated to the toner image may be sufficient to sufficiently fluidize the compound, and is preferably in the range of 280 nm to 480 nm, more preferably in the range of 300 nm to 420 nm, and even more preferably in the range of 330 nm to 420 nm. The amount of light irradiated by the light source 41 may also be sufficient to sufficiently fluidize the compound, and is, for example, 0.1 J / cm. 2 More than 200J / cm 2 Within the following range, preferably 0.1 J / cm 2 More than 100J / cm 2 Within the range of 0.1 J / cm 2 More than 50J / cm 2 It is within the following range.
[0200] When the toner image is softened by irradiating the toner image with light from the light source 41, the toner image may be heated by the heating member 93 in addition to the light irradiation. This allows the toner image to be softened and melted more efficiently. The heating temperature at this time is, for example, in the range of 20° C. to 200° C., and preferably in the range of 20° C. to 150° C.
[0201] The softened toner image can be solidified and fixed to the recording medium by leaving it at room temperature (within the range of 25±15° C.), heating it, or irradiating it with visible light. As described below, the fixing step preferably further includes a step of applying pressure to the softened toner image. In the pressurizing step, it is preferable to further heat the softened toner image.
[0202] The light source 41 irradiates light toward the first surface of the recording paper S carrying the toner image, the first surface being the photoreceptor side. The recording paper S is nipped between the photoconductor 1 and the transfer roller 5 which is the transfer section. The light source 41 is disposed on the opposite side to the recording paper S side. A heating member 93 is disposed on the side of the recording paper S. The light source 41 and the heating member 93 are disposed therebetween.
[0203] The light source 41 and the heating member 93 are arranged at a nip position between the photoconductor 1 and the transfer roller 5. It is disposed on the downstream side in the paper transport direction and on the upstream side in the paper transport direction with respect to the pressure bonding unit 9.
[0204] According to an image forming method according to an embodiment of the present invention, the photoconductor 1 is charged by applying a uniform potential to it using the charger 2, and then the photoconductor 1 is scanned with a light beam irradiated by the exposure device 3 based on original image data to form an electrostatic latent image. Next, the developing unit 4 supplies a developer containing the toner of the present invention onto the photoconductor 1.
[0205] When recording paper S is transported from tray 16 to image forming unit 10 in time with the rotation of photoconductor 1 causing the toner image carried on the surface of photoconductor 1 to reach the position of transfer unit 5, the toner image on photoconductor 1 is transferred onto recording paper S nipped between transfer unit 5 and photoconductor 1 by a transfer bias applied to transfer unit 5.
[0206] The transfer unit 5 also functions as a pressure member, and can transfer the toner image from the photoreceptor 1 to the recording paper S while reliably bringing the compound contained in the toner image into close contact with the recording paper S.
[0207] After the toner image is transferred onto the recording paper S, the blade 85 of the cleaning unit 8 removes the developer remaining on the surface of the photoconductor 1 .
[0208] In the process in which the recording paper S onto which the toner image has been transferred is transported by the transport belt 13 to the pressing unit 9, the light source 41 irradiates light onto the toner image transferred onto the recording paper S. By irradiating light onto the toner image on the first side of the recording paper S from the light source 41, the toner image can be melted more reliably, and the fixability of the toner image to the recording paper S can be improved.
[0209] When the recording paper S carrying the toner image reaches the pressing unit 9 by the conveyor belt 13, the pressure members 91 and 92 press the toner image onto the first side of the recording paper S. Before the toner image is fixed by the pressing unit 9, the toner image is softened by being irradiated with light by the light source 41, so that it is possible to save energy in pressing the image onto the recording paper S. Furthermore, in the process of solidifying the toner image and fixing it to the recording medium, the toner image is pressed by the pressure members 91 and 92, so that the fixability of the toner image onto the recording paper S is further improved.
[0210] The pressure when pressing the toner image is as described above. The pressing step may be performed before, simultaneously with, or after the step of softening the toner image by irradiating light. From the viewpoint of being able to pressurize the toner image in a pre-softened state and facilitating the enhancement of image strength, it is preferable to perform the pressing step after the light irradiation.
[0211] In addition, the pressure member 91 can heat the toner image on the recording paper S when the recording paper S passes between the pressure members 91 and 92. The toner image softened by the light irradiation is further softened by this heating, and as a result, the fixability of the toner image to the recording paper S is further improved.
[0212] The heating temperature of the toner image is as described above. The heating temperature of the toner image (surface temperature of the toner image) can be measured by a non-contact temperature sensor. Specifically, for example, a non-contact temperature sensor may be installed at a position where the recording medium is discharged from the pressure member, and the surface temperature of the toner image on the recording medium may be measured.
[0213] The toner image pressed by the pressure members 91 and 92 is solidified and fixed onto the recording paper S.
[0214] In one embodiment of the present invention, the fixing device has a pressing section equipped with a pressure member.
[0215] In one embodiment of the present invention, the pressure member includes a heating means.
[0216] In one embodiment of the present invention, the temperature of the pressure member is preferably 15° C. or higher, more preferably 20° C. or higher, even more preferably more than 20° C., even more preferably 30° C. or higher, and even more preferably 40° C. or higher. There is no particular upper limit, but it is, for example, 200° C. or lower, 150° C. or lower, or 100° C. or lower.
[0217] <Photoresponsive adhesive> The compound of the present invention becomes fluid when irradiated with light and becomes non-fluid reversibly, so that a photoresponsive adhesive (photosensitive adhesive) that can be used repeatedly can be produced using the compound of the present invention. For example, it can be applied to various adhesion techniques as a photoresponsive adhesive that can be repeatedly attached and detached by light in response to changes in viscosity (friction coefficient). That is, one embodiment of the present invention is a photoresponsive adhesive that includes the compound of the present invention.
[0218] The light-responsive adhesive of the present invention can be used for temporary fixing that allows repeated use, and is also suitable for recycling, but is not limited thereto.
[0219] <Photoswitching materials> The compound of the present invention is fluidized by light irradiation and reversibly non-fluidized, so that a light-switching material can be prepared using the compound of the present invention. For example, a light-switching material can be prepared by utilizing the change in color or polarity, mass transfer, change in orientation, change in viscosity, and change in surface tension that accompanies photoisomerization. For example, in liquid crystal materials, it is possible to apply the compound to patterning drawings that can be repeatedly rewritten in response to the change in molecular orientation that accompanies photoisomerization. In addition, for example, the change in surface tension that accompanies light irradiation and the resulting mass transfer can be used to perform microfabrication of the surface of a polymer film. That is, one embodiment of the present invention is a light-switching material that includes the compound of the present invention.
[0220] The optical switching material of the present invention can be used for liquid crystal display materials and surface processing of polymer films, but is not limited thereto. EXAMPLES
[0221] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.
[0222] <Example 14: Synthesis of compound 14> 4-Decyloxybenzeneamine (4-decyloxyaniline) (5mmol), 1-methyl-1H-pyrazole-4-carboxaldehyde (5mmol), and 20ml of ethanol were added to a 100ml four-neck flask equipped with a cooling tube, nitrogen inlet tube, and thermometer, and heated and stirred. The reaction solution was suction filtered, and the resulting powder was washed with cooled ethanol. Further, recrystallization was performed with methanol / ethanol to obtain the target compound 14 in a yield of 63%.
[0223] [ka]
[0224] 1 The formation of compound 14 was confirmed by 1 H NMR. 1H NMR (400MHz, CDCl3); 8.34ppm(s,1H,CH=N), 7.89ppm(s,1H,pyrazol), 7.84ppm(2,1H,pyrazol), 7.12ppm(d,2H,aryl), 6.89ppm(d,2H,aryl), 4.10ppm(t ,2H,methylene), 3.94ppm(s,3H,methyl), 1.77ppm(m,2H,methylene), 1.43ppm(m,2H,methylene), 1.33ppm(m,4H,methylene), 0.89ppm(t,3H,methyl).
[0225] <Examples 1 to 13, 15, and 16, and Comparative Example 1> The synthesis of compounds 1 to 13, 15, 16, and the compound of Comparative Example 1 was carried out in the same manner as in the synthesis of compound 14, except that 4-decyloxybenzeneamine and 1-methyl-1H-pyrazole-4-carboxaldehyde were replaced with the corresponding raw materials shown below, and the target products were obtained. 1 The formation of each compound was confirmed by 1 H NMR.
[0226] Synthesis of compound 1: 4-decyloxybenzenamine and 5-methylthiophene-2-carboxaldehyde; 1 The formation of compound 1 was confirmed by 1 H NMR. 1 H NMR (400MHz, CDCl3); 8.37ppm(s,1H,CH=N), 7.39ppm(d,2H,aryl), 7.06ppm(d,1H,thiophene), 6.97ppm(d,2H,aryl), 6.67ppm(d,2H,thiophene), 4.11ppm(t,2H,methyle ne), 2.43ppm(s,3H,methyl), 1.74ppm(m,2H,methylene), 1.43ppm(m,2H,methylene), 1.29ppm(m,2H,methylene), 1.26ppm(m,10H,methylene), 0.89ppm(t,3H,methyl).
[0227] Synthesis of compound 2: 4-hexyloxy-3-methyl-benzenamine and 5-hexylthiophene-2-carboxaldehyde; Synthesis of compound 3: 4-butoxybenzenamine, 5-methylfuran-2-carboxaldehyde; Synthesis of compound 4: 4-hexylbenzenamine, 1-methyl-1H-pyrrole-2-carboxaldehyde; Synthesis of compound 5: 4-decyloxy-3-methyl-benzenamine, 1-methyl-1H-pyrazole-3-carboxaldehyde; Synthesis of compound 6: 4-decyloxybenzenamine, 1-methyl-1H-pyrazole-5-carboxaldehyde; Synthesis of compound 7: 4-decyloxybenzenamine, 1-methyl-1H-imidazole-4-carboxaldehyde; Synthesis of compound 8: 4-decyloxybenzenamine, 1-methyl-1H-imidazole-5-carboxaldehyde; Synthesis of compound 9: 6-hexyloxy-2-naphthalenamine (2-amino-6-hexyloxynaphthalene), 5-butylthiophene-2-carboxaldehyde: Synthesis of compound 10: 4-butoxy-1,1'-biphenyl-4'-amine (4-amino-4'-butoxybiphenyl), 1-methyl-1H-pyrazole-3-carboxaldehyde; Synthesis of compound 11: 4-octyloxybenzenamine, 1H-indole-3-carboxaldehyde; Synthesis of compound 12: 5-methyl-2-thienylamine, 2,6-dimethyl-4-(hexyloxy)-benzaldehyde; Synthesis of compound 13: 4-octyloxybenzenamine, 1-methyl-1H-pyrrole-3-carboxaldehyde; Synthesis of compound 15: 4-hexyloxybenzenamine, 1-butyl-1H-pyrazole-4-carboxaldehyde; Synthesis of compound 15: 4-hexyloxybenzenamine, 1-butyl-1H-pyrazole-4-carboxaldehyde; Synthesis of compound 16: 4-hexyloxy-3-methyl-benzenamine, 1-hexyl-1H-pyrazole-4-carboxaldehyde; Synthesis of comparative compound 1 (Comparative 1): 4-hexyloxybenzaldehyde, 1,3-dimethyl-1-pyrrol-2-amine.
[0228] Table 3 shows the structures of compounds 1 to 16 and comparative compound 1.
[0229] Synthesis of Comparative Compound 2 (Comparative 2) The following comparative compound 1 (number average molecular weight Mn: 2870) was obtained by the method described in paragraphs 0217 to 0227 of JP2014-191078A.
[0230] [ka]
[0231] [Toner production] (Preparation of Toner 1) <Preparation of styrene acrylic resin particle dispersion 1> (First stage polymerization) A solution of 8 parts by mass of sodium dodecyl sulfate dissolved in 3000 parts by mass of ion-exchanged water was charged into a reaction vessel equipped with a stirring device, a temperature sensor, a cooling tube, and a nitrogen introduction device, and the internal temperature was raised to 80 ° C. while stirring at a stirring speed of 230 rpm under a nitrogen gas flow. After the temperature was raised, a solution of 10 parts by mass of potassium persulfate dissolved in 200 parts by mass of ion-exchanged water was added, the liquid temperature was again raised to 80 ° C., and a polymerizable monomer solution consisting of 480 parts by mass of styrene, 250 parts by mass of n-butyl acrylate, 68.0 parts by mass of methacrylic acid, and 16.0 parts by mass of n-octyl-3-mercaptopropionate was dropped over 1 hour, and the mixture was heated and stirred at 80 ° C. for 2 hours to polymerize, thereby preparing a styrene acrylic resin particle dispersion liquid (1A) containing styrene acrylic resin particles (1a).
[0232] (Second stage polymerization) A solution of 7 parts by mass of sodium polyoxyethylene (2) dodecyl ether sulfate dissolved in 800 parts by mass of ion-exchanged water was charged into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device, and heated to 98°C. After that, a polymerizable monomer solution of 260 parts by mass of the styrene acrylic resin particle dispersion (1A) obtained above, 245 parts by mass of styrene, 120 parts by mass of n-butyl acrylate, 1.5 parts by mass of n-octyl-3-mercaptopropionate, and 67 parts by mass of paraffin wax "HNP-11" (manufactured by Nippon Seiro Co., Ltd.) as a release agent was added at 90°C, and the mixture was mixed and dispersed for 1 hour using a mechanical disperser "CREARMIX (registered trademark)" (manufactured by M Technique Co., Ltd.) with a circulation path to prepare a dispersion containing emulsified particles (oil droplets). Next, an initiator solution prepared by dissolving 6 parts by mass of potassium persulfate in 200 parts by mass of ion-exchanged water was added to this dispersion, and the system was heated and stirred at 82°C for 1 hour to carry out polymerization, thereby preparing a styrene-acrylic resin particle dispersion (1B) containing styrene-acrylic resin particles (1b).
[0233] (Third stage polymerization) A solution of 11 parts by mass of potassium persulfate dissolved in 400 parts by mass of ion-exchanged water was added to the obtained styrene-acrylic resin particle dispersion liquid (1B), and then a polymerizable monomer solution consisting of 435 parts by mass of styrene, 130 parts by mass of n-butyl acrylate, 33 parts by mass of methacrylic acid, and 8 parts by mass of n-octyl-3-mercaptopropionate was added dropwise over 1 hour under a temperature condition of 82°C. After the dropwise addition, polymerization was carried out by heating and stirring for 2 hours, and then the mixture was cooled to 28°C to obtain a styrene-acrylic resin particle dispersion liquid 1 containing a styrene-acrylic resin 1. The glass transition temperature (Tg) of the styrene-acrylic resin 1 was measured and found to be 45°C.
[0234] <Preparation of azomethine compound particle dispersion 1> 80 parts by mass of dichloromethane and 20 parts by mass of compound 1 prepared above were mixed and stirred while being heated at 50°C to obtain a liquid containing compound 1. A mixed liquid of 99.5 parts by mass of distilled water heated to 50°C and 0.5 parts by mass of a 20% by mass aqueous solution of sodium dodecylbenzenesulfonate was added to 100 parts by mass of this liquid. Thereafter, the mixture was emulsified by stirring at 16000 rpm for 20 minutes using a homogenizer (manufactured by Heidolph) equipped with a shaft generator 18F, to obtain emulsion liquid 1 of an azomethine compound.
[0235] The obtained azomethine compound emulsion 1 was placed in a separable flask, and the organic solvent was removed by heating and stirring at 40° C. for 90 minutes while blowing nitrogen into the gas phase, to obtain an azomethine compound particle dispersion 1.
[0236] (Preparation of Black Colorant Particle Dispersion (Bk-1)) 11.5 parts by mass of sodium n-dodecyl sulfate was dissolved in 160 parts by mass of pure water, 25 parts by mass of carbon black "Mogul L (manufactured by Cabot Corporation)" was gradually added, and then the mixture was dispersed using "Clearmix (registered trademark) W Motion CLM-0.8 (manufactured by M Technique Co., Ltd.)" to prepare a black colorant particle dispersion (Bk-1). The volume-based median diameter of the colorant particles in the black colorant particle dispersion (Bk-1) was 110 nm.
[0237] (Agglomeration, fusion) The above-prepared styrene acrylic resin particle dispersion 1 (504 parts by mass, calculated as solid content), azomethine compound particle dispersion 1 (216 parts by mass, calculated as solid content), ion-exchanged water (900 parts by mass), and black colorant particle dispersion (70 parts by mass, calculated as solid content) were charged into a reaction apparatus equipped with a stirrer, a temperature sensor, and a cooling tube. The temperature inside the vessel was kept at 30°C, and a 5 mol / L aqueous sodium hydroxide solution was added to adjust the pH to 10.
[0238] Next, an aqueous solution of 2 parts by mass of magnesium chloride hexahydrate dissolved in 1000 parts by mass of ion-exchanged water was added dropwise under stirring over a period of 10 minutes, and then heating was started. The temperature of this system was raised to 70°C over a period of 60 minutes, and the particle growth reaction was continued while maintaining the temperature at 70°C. In this state, the particle size of the associated particles was measured using a "Multisizer 3" (manufactured by Beckman Coulter, Inc.), and when the median diameter (D50) on a volume basis reached 6.5 μm, an aqueous solution of 190 parts by mass of sodium chloride dissolved in 760 parts by mass of ion-exchanged water was added to stop the particle growth. After stirring at 70°C for 1 hour, the temperature was further raised, and the particles were heated and stirred at 75°C to promote fusion of the particles. The mixture was then cooled to 30°C to obtain a dispersion of toner base particles.
[0239] The dispersion liquid of the toner base particles obtained above was subjected to solid-liquid separation using a centrifuge to form a wet cake of the toner base particles. The wet cake was washed with ion-exchanged water at 35°C until the electrical conductivity of the filtrate from the centrifuge reached 5 μS / cm, and then transferred to a "Flash Jet Dryer (manufactured by Seishin Enterprise Co., Ltd.)" and dried until the moisture content reached 0.5% by mass to form toner base particles.
[0240] To 100% by mass of the obtained toner base particles, 1% by mass of hydrophobic silica (number average primary particle size: 12 nm) and 0.3% by mass of hydrophobic titania (number average primary particle size: 20 nm) were added and mixed using a Henschel mixer (registered trademark), thereby obtaining toner 1.
[0241] (Preparation of Toners 2 to 20 and Comparative Examples 1 and 2) Toners 2 to 16 and Comparative Examples 1 and 2 were prepared in the same manner as in the preparation of Toner 1, except that in the preparation of Toner 1, Compound 1 was changed to Compound 14, and the mass ratio of Compound 14 to the styrene acrylic resin was changed as shown in Table 5 below. Toners 17 to 20 were prepared in the same manner as in the preparation of Toner 1, except that in the preparation of Toner 1, Compound 1 was changed to Compound 14, and the mass ratio of Compound 14 to the styrene acrylic resin was changed as shown in Table 5 below.
[0242] (Preparation of Toner 21) Toner 21 was prepared in the same manner as in the preparation of toner 1 above, except that in the preparation of toner 1 above, compound 1 was changed to compound 14, and in the (aggregation and fusion) process, styrene acrylic resin particle dispersion 1 (504 parts by mass in terms of solid content) was changed to polyester resin particle dispersion 2 (504 parts by mass in terms of solid content) prepared as follows.
[0243] <Preparation of polyester resin particle dispersion 2 containing polyester resin 1) In a 10-liter four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, 524 parts by mass of bisphenol A propylene oxide 2-mol adduct, 105 parts by mass of terephthalic acid, 69 parts by mass of fumaric acid, and 2 parts by mass of tin octylate (esterification catalyst) were added, and a polycondensation reaction was carried out at a temperature of 230°C for 8 hours. The polycondensation reaction was further continued for 1 hour at 8 kPa, and then cooled to 160°C to obtain polyester resin 1. 100 parts by mass of polyester resin 1 were pulverized with a "Landermill Type: RM" (manufactured by Tokuju Machinery Co., Ltd.), mixed with 638 parts by mass of a 0.26% by mass aqueous solution of sodium lauryl sulfate prepared in advance, and ultrasonically dispersed for 30 minutes at V-LEVEL and 300 μA using an ultrasonic homogenizer "US-150T" (manufactured by Nippon Seiki Co., Ltd.) while stirring, to obtain polyester resin particle dispersion liquid 2. The glass transition point Tg of this polyester resin 1 was measured and found to be 42°C.
[0244] (Preparation of developer) For the toners 1 to 21 and the toners of Comparative Examples 1 and 2 prepared above, ferrite carrier particles having a volume average particle size of 30 μm coated with a copolymer resin of cyclohexane methacrylate and methyl methacrylate (monomer mass ratio 1:1) were mixed so that the toner particle concentration was 6 mass%, thereby obtaining developers 1 to 21 and the developers of Comparative Examples 1 and 2. Mixing was performed for 30 minutes using a V-type mixer.
[0245] [Evaluation: Photoresponsive adhesion test of compounds] The change in adhesiveness of the compounds 1 to 16 prepared in each example and the comparative compounds 1 and 2 with light irradiation was evaluated by the following photoresponsive adhesive test using the apparatus shown in FIG. 3. As shown in FIG. 3, 2 mg of the compound was placed on a 18 mm square cover glass 1 within a radius of 6 mm from the center of the glass, and a cover glass 2 of the same size was placed at a position shifted about 4 mm in a parallel direction to the cover glass 1 so as to completely cover the compound. This was heated to melt the sample, and the cover glass 1 and the cover glass 2 were bonded together. Each of the obtained samples was subjected to the following non-fluidity → fluidity test, and then the following fluidity → non-fluidity (return) test.
[0246] <Testing for non-liquidity → liquidity> Part (A) shown in Figure 3 was fixed to the stand with cellophane tape, and a 30 cm long vinyl string with a 100 g weight attached was fixed to part (C) with cellophane tape. Part (B) was irradiated with 365 nm light at a dose of 30 J / cm. 2 It was confirmed whether cover glass 2 peeled off from cover glass 1, and the peeling was judged according to the following evaluation criteria.
[0247] - Evaluation criteria for non-liquidity to liquidity testing - ○: Cover glass 2 was completely peeled off from cover glass 1 △: Cover glass 2 is displaced ×: The cover glass 2 did not move.
[0248] <Test for fluidity → non-fluidity (return)> After the non-fluidity → fluidity test was completed, the following experiment was performed on the samples in which the cover glass 2 had been completely peeled off and on the samples in which it had shifted. For the shifted samples, the cover glasses 1 and 2 were peeled off by hand. Five minutes after the end of the light irradiation in the non-fluidity → fluidity test (the sample was left in a natural environment, i.e., in a dark room at room temperature, for five minutes), a cover glass 3 (same size as cover glasses 1 and 2) was placed so as to cover the sample portion (part (B)) of the cover glass 1 used in the above test, and it was confirmed whether the cover glass 1 and cover glass 3 were adhered to each other, and a judgment was made according to the following evaluation criteria.
[0249] -Evaluation criteria for fluidity to non-fluidity (return) tests- 〇: Did not adhere (had become non-fluid) △: Partially adhered (partially maintained in a fluid state) ×: Adhered (fluid state was maintained).
[0250] It was confirmed that all of the compounds prepared in the examples that were evaluated as ○ in the above-mentioned fluidity → non-fluidity (reversion) test re-solidified after the non-fluidity → fluidity test. The results are shown in Table 4 below.
[0251] [Evaluation: Fixation test] Fixing tests were carried out under normal temperature and humidity conditions (temperature 20°C, relative humidity 50% RH) using the above-obtained developers 1 to 21 and the developers of Comparative Examples 1 and 2. The developer was placed on one side, and paper (gloss coated paper, basis weight: 128 g / m2) was placed on the other side as a recording medium. 2 The developer is placed between a pair of parallel flat plate (aluminum) electrodes with a magnetic force, and the gap between the electrodes is 0.5 mm. The DC bias and AC bias are used to control the toner adhesion amount to 6 g / m. 2 The toner was developed under the above conditions to form a toner layer on the surface of the gloss coated paper, and the toner was fixed by each fixing device to obtain a printed matter (image formation).
[0252] A 1 cm square toner image on this print was rubbed 10 times with a "JK Wiper (registered trademark)" (manufactured by Nippon Paper Crecia Co., Ltd.) at a pressure of 50 kPa, and the image fixation rate was evaluated. A fixation rate of 60% or more was considered to be acceptable. The results are shown in Table 5. The image fixation rate is a numerical value obtained by measuring the reflection density of the image after printing and the image after rubbing with a fluorescent spectrodensitometer "FD-7" (manufactured by Konica Minolta, Inc.), and dividing the reflection density of the solid image after rubbing by the reflection density of the solid image after printing, expressed as a percentage.
[0253] The fixing devices used were the following four types of fixing devices configured by appropriately modifying the device shown in FIG. 2: No. 1: There is no pressure bonding portion 9 in FIG. 2, the temperature of the heating member 93 is 20° C., the wavelength of the ultraviolet light irradiated from the light source 41 is 365 nm (light source: LED light source with an emission wavelength of 365 nm±10 nm), and the irradiation amount is 15 J / cm 2 is; No. 2: The pressing unit 9 in FIG. 2 is included, the temperature of the heating member 93 is 20° C., the temperature of the pressure member 91 is 20° C., and the pressure during pressing is 0.2 MPa. The wavelength and irradiation amount of the light source 41 are the same as those of No. 1; No. 3: The pressing unit 9 in FIG. 2 is included, the temperature of the heating member 93 is 20° C., the temperature of the pressure member 91 is 80° C., and the pressure during pressing is 0.2 MPa. The wavelength and irradiation amount of the light source 41 are the same as those of No. 1; No. 4: There is no pressure bonding portion 9 in FIG. 2, the temperature of the heating member 93 is 80° C., and the wavelength and irradiation amount of the light source 41 are the same as those of No. 1.
[0254] - Evaluation criteria for fixation - ◎: Retention rate is 90% or higher ○: Retention rate is between 75% and 90% △: Retention rate is between 60% and 75% ×: Fixation rate is less than 60%.
[0255] [Color reproducibility evaluation] The color reproducibility of the images obtained in the above examples and comparative examples was evaluated by visual evaluation by 10 monitors according to the following evaluation criteria. Specifically, as a sample for evaluation comparison, a toner was prepared by removing the photoresponsive compound from the toner of each example. Using this, a developer was prepared in the same manner as above, and development was performed in the same manner as the image formation in the fixing property test above, and fixing was performed using the fixing device No. 5 described below.
[0256] Fixing device No. 5: The pressing unit 9 in FIG. 2 was included, the temperature of the heating member 93 was 20° C., the temperature of the pressure member 91 was 150° C., the pressure during pressing was 0.2 MPa, and no light irradiation was performed.
[0257] The 10 monitors were shown the sample for evaluation and the images obtained in the above-mentioned Examples and Comparative Examples in turn, and asked whether the colors of the two images were clearly different. The results of the evaluation based on the following color reproducibility evaluation criteria are shown in Table 5 below.
[0258] -Evaluation criteria for color reproducibility- ◎: Less than 2 people answered that it was clearly different ○: 3 to 4 people answered that it was clearly different △: 5 to 7 people answered that it was clearly different ×: Eight or more people answered that it was clearly different.
[0259] [Table 3]
[0260] [Table 4]
[0261] [Table 5]
[0262] "Compound" in Table 5 refers to the azomethine compound of each Example and Comparative Example. In Table 5, the ratio of compound and binder resin is the ratio (mass %) of the azomethine compound and binder resin to the total amount of the azomethine compound and binder resin in the toner.
[0263] As is clear from Table 4 above, it was found that all of the compounds 1 to 16 of the examples were fluidized and reversibly immobilized by light irradiation. In contrast, it was found that the compound of Comparative Example 1, in which there is no hydrogen atom on the carbon atom bonded adjacent to the carbon atom bonded to the nitrogen atom of the C=N bond in the aromatic heterocyclic structure constituting the azomethine compound, was not fluidized or immobilized by light irradiation. Moreover, reversible immobilization after fluidization was not confirmed in the azobenzene compound of Comparative Example 2.
[0264] As is clear from Table 5 above, all of the toners 1 to 21 of the examples exhibited high fixability and excellent color reproducibility. On the other hand, the toner of Comparative Example 1, which uses a compound that does not have a hydrogen atom on the carbon atom bonded adjacent to the carbon atom bonded to the nitrogen atom of the C=N bond, does not obtain sufficient fixability by light irradiation. In addition, the toner of Comparative Example 2, which uses an azobenzene compound, does not have sufficient fixability and low color reproducibility. Since the ultraviolet light source and ultraviolet irradiation conditions used in the fixability test are constant throughout the examples and comparative examples, it can be said that the toner of the examples fully exhibits the effect of the azomethine compound that is fluidized by light irradiation, reversibly non-fluidized, and does not significantly color, compared to the toner of the comparative example.
[0265] In particular, in Examples 13 to 16, which used compounds 13 to 16 in which, in an aromatic heterocyclic structure, hydrogen atoms are present on both of the two carbon atoms bonded adjacent to a carbon atom bonded to a nitrogen atom or carbon atom of a C=N bond, the fixability was further improved.
[0266] Comparing the fixing devices, it was found that the same toner 14 was used, ultraviolet rays were irradiated under the same conditions, and fixing device No. 2, which applied pressure with a pressure member, and fixing device No. 3, which applied pressure while heating with a pressure member, provided higher fixing properties than fixing device No. 1, which did not use a pressure member (comparison of Examples 14, 22, and 23). Also, the same toner 14 was used, ultraviolet rays were irradiated under the same conditions, and fixing device No. 4, which heated with a heating member 93, provided higher fixing properties than fixing device No. 1, which did not heat during ultraviolet irradiation (comparison of Examples 1 and 24). [Explanation of symbols]
[0267] 1 photoreceptor, 2 Charger, 3 Exposure device, 4 Development section, 5 Transcription unit, 7 Paper transport system, 8 Cleaning section, 9 Crimping part, 10 Image forming unit, 11 Paper feed section, 12 Transport roller, 13 conveyor belt, 14 Paper ejection section, 15 Manual feed unit, 16 trays, 17 Thermohygrometer, 20 Image processing unit, 24 Paper reversing section, 40 Irradiation unit, 41 light source, 71 Image reading device, 72 Automatic document feeder, 85 blades, 90 control section, 91, 92 Pressurizing member, 93 Heating element, 100 Image forming apparatus, d manuscript, S Recording paper.
Claims
1. A photoresponsive compound represented by the following general formula (1): [Formula 1] During the ceremony, Z 1 and Z 2 is N or CH, with the proviso that Z 1 ≠Z 2 and R 1 is an aromatic hydrocarbon structure, R 2 is expressed by the following formula, [chemical 2] In the formula, R c is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms, except for the following compounds 1, 2, and 4 to 6. [C3]
2. The R 1 The compound of claim 1 , wherein is a substituted or unsubstituted phenyl, naphthyl, anthracenyl, phenanthrenyl, pyrenyl, or biphenyl group.
3. The compound according to claim 1 or 2, wherein R 1 has at least one substituent selected from the group consisting of a halogen group, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms.
4. The compound according to claim 3, wherein R 1 has at least one substituent selected from the group consisting of an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms.
5. A toner comprising the compound according to any one of claims 1 to 4.
6. The toner according to claim 5 , further comprising a binder resin.
7. The toner according to claim 6 , wherein the binder resin comprises at least one selected from the group consisting of a styrene-acrylic resin and a polyester resin.
8. forming a toner image on a recording medium, the toner image being made of the toner according to any one of claims 5 to 7; irradiating the toner image with light to soften the toner image; An image forming method comprising:
9. The image forming method according to claim 8 , wherein the wavelength of the light is from 280 nm to 480 nm.
10. 10. The image forming method according to claim 8, further comprising a step of pressing the toner image.
11. The image forming method according to claim 10 , wherein the toner image is further heated in the pressurizing step.
12. 12. The image forming method according to claim 8, wherein in the step of irradiating the toner image with light to soften the toner image, the toner image is heated in addition to being irradiated with light.
13. A light-responsive adhesive comprising the compound according to any one of claims 1 to 4.
14. A light switching material comprising the compound according to any one of claims 1 to 4.
Citation Information
Patent Citations
Alphaatrichloromethylthenyl anilines * phenylethers * sulfides and sulphones as biodegradable pesticide and killing agent for mollusks
JP1976122062A
Photoresponsive liquid crystal compound
JP2011256155A
Method for fluidizing / non-fluidizing compound with light
JP2011256291A
Photoresponsive compound, and adhesive, toner and image formation method using the same
JP2021070673A
JPP7243259B