Image pickup element, stacked image pickup element, and image pickup device
The use of a carrier blocking layer with specific organic materials and thickness in organic image sensors addresses capacitance and dark current issues, enhancing image quality and sensitivity.
Patent Information
- Application Number
- JP2023094308
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-01-19
- Filing Date
- 2023-06-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2036-04-19
AI Technical Summary
Existing organic image sensors face challenges in reducing capacitance while maintaining high external quantum efficiency and preventing dark current increase, which affects image quality and sensitivity.
Incorporating a carrier blocking layer made of specific materials with structural formulas (1), (2), or (3) with a thickness of 5×10^-9 m to 1.5×10^-7 m, which absorbs minimal visible light and enhances carrier mobility, thereby reducing capacitance without interfering with photoelectric conversion.
The solution achieves improved external quantum efficiency, suppressed dark current, and enhanced dark current breakdown voltage characteristics, resulting in clearer images with reduced afterimages.
Smart Images

Figure 0007586230000026 
Figure 0007586230000027 
Figure 0007586230000028
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an imaging element, a stacked imaging element, and an imaging apparatus. [Background technology]
[0002] In recent years, imaging devices have been improved in performance and diversified in functions to meet various applications, and continue to evolve. One of the next-generation technologies is photoelectric conversion using organic semiconductor materials, rather than inorganic semiconductor materials. Such imaging devices are called "organic imaging devices." In addition, imaging devices that have spectral sensitivity corresponding to red, green, and blue by stacking multiple organic semiconductor layers (called "stacked imaging devices") are being developed and are attracting attention. Such stacked imaging devices do not require a color separation optical system, and three types of electrical signals (image signals) corresponding to red, green, and blue can be extracted from one pixel, so that the light utilization rate is high, the aperture is wide, and false signals such as moire are unlikely to occur. It is said that about 40% of the transmitted light is lost due to the transmission absorption of the color filters in imaging devices equipped with normal color filters.
[0003] Incidentally, currently, imaging devices using silicon (Si) as a photoelectric conversion material are mainstream. In order to improve recording density, pixels have been miniaturized, and the pixel size has reached approximately 1 μm. The optical absorption coefficient of Si is 10 3 〜10 4 cm -1 The photoelectric conversion layer in an image sensor is usually located at a depth of 3 μm or more in a silicon semiconductor substrate. As pixel sizes become smaller, the aspect ratio between the pixel size and the depth of the photoelectric conversion layer increases. This results in light leakage from adjacent pixels and limits on the angle of incidence of light, leading to a decrease in the performance of the image sensor. As a solution to these problems, organic materials with large absorption coefficients have been attracting attention. The absorption coefficient of organic materials in the visible light region is around 10 5 cm -1In the case of organic imaging elements or stacked-type imaging elements, it is possible to reduce the thickness of the photoelectric conversion layer, which is thought to enable improved sensitivity and an increase in the number of pixels while suppressing false colors, and development of these elements is currently underway.
[0004] Although organic imaging elements are believed to have many advantages, one of the challenges is to reduce the capacity of the imaging module. Here, an imaging module is a device that incorporates an organic imaging element and outputs an electrical signal obtained by photoelectric conversion as an image. The charge obtained in the photoelectric conversion layer that constitutes the imaging element by light irradiation is converted into a voltage and output as an electrical signal (image signal). At this time, if the total amount C of electrical capacity including the electrical capacity of the organic imaging element, the floating diffusion (hereinafter abbreviated as "FD"), the buffer amplifier connected to the FD, and the peripheral structures such as the reset gate and horizontal output gate adjacent to the FD, is large, the voltage change per charge becomes small, resulting in a small S / N ratio and deterioration of image quality. Here, the voltage V of the electrical signal is expressed as follows when the amount of charge is Q: V = Q / C Ultimately, if the capacitance of the organic imaging element increases, V decreases, resulting in a smaller electric signal. The capacitance of the organic imaging element (specifically, the capacitance of the organic layer, described next) accounts for about half of the total capacitance C. In addition, the capacitance C0 is generally expressed as follows, where ε is the dielectric constant, S0 is the area, and d0 is the thickness: C0=(ε·S0) / d0 Therefore, factors that influence the reduction in capacitance of an organic imaging element include the pixel area, the dielectric constant of the material that constitutes the organic imaging element, and the thickness of the organic layers in the organic imaging element. In order to reduce capacitance by the thickness, it is necessary to increase the total thickness of the organic layers in the organic imaging element.
[0005] As shown in the conceptual diagram of FIG. 1A, the organic layer has a laminated structure of a carrier blocking layer (first carrier blocking layer) 22, an organic photoelectric conversion layer 23, and a second carrier blocking layer 24 sandwiched between a first electrode 21 and a second electrode 25. It is possible to increase the thickness of the organic photoelectric conversion layer 23. However, since the organic photoelectric conversion layer 23 is a layer involved in the photoelectric conversion function, it is often difficult to achieve both a thicker film and a lower photoelectric conversion efficiency when converting light of a certain wavelength into an electric current. In addition, in a laminated imaging element, if the material constituting the organic photoelectric conversion layer 23 has a spectral characteristic that absorbs light other than the desired wavelength, there is a risk that the photoelectric conversion layer constituting the imaging element located below will block the light that should be absorbed if the organic photoelectric conversion layer 23 is made thick. The second carrier blocking layer 24 needs to have the function of transporting electrons. If the thickness of the second carrier blocking layer 24, which is made of an organic material with low electron mobility, is increased, it becomes a resistive component, making it difficult to maintain high photoelectric conversion efficiency.
[0006] Incidentally, the parent skeletons of the following structural formulas (1), (2), and (3) are well-known materials for organic thin film transistors (organic TFTs), and are called benzothienobenzothiophene (BTBT)-based materials. JP 2010-232413 A discloses the application of BTBT-based materials to organic TFTs, static induction transistors, and solar cells, but does not mention the application to imaging devices. This patent publication also discloses a wide range of applications, using BTBT-based materials as active layers with film thicknesses of 1 nm to 10 μm, preferably 5 nm to 5 μm, and more preferably 10 nm to 3 μm, but in the examples, the film thickness of the BTBT-based material is 250 nm. In addition, the active layer itself is not required to have spectral characteristics, and no mention is made of capacitance. International Publication WO2012 / 121393 discloses a technology for expressing liquid crystals using BTBT-based materials and applying them to organic TFTs. However, this international publication also makes no mention of imaging elements, makes no mention of spectral characteristics, and makes no mention of capacitance.
[0007] [ka] [ka] [ka] [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent Publication No. 2010-232413 [Patent Document 2] International Publication WO2012 / 121393 [Patent Document 3] Patent Publication 2011-176259 Summary of the Invention [Problem to be solved by the invention]
[0009] The first carrier blocking layer of an organic imaging element is often referred to as an electron blocking layer, and is generally made of, for example, a carbazole-based material or an aromatic amine-based material as disclosed in JP-A-2011-176259. However, when the capacitance is reduced by increasing the thickness of the first carrier blocking layer, it has been found that, for example, when the first carrier blocking layer is made of a carbazole-based material or an aromatic amine-based material, the external quantum efficiency is significantly decreased and the dark current is significantly increased when the thickness of the first carrier blocking layer is increased, as described below, making it unsuitable for practical use.
[0010] Therefore, an object of the present disclosure is to provide a stacked imaging element and an imaging device that are constituted by imaging elements that are less likely to cause problems such as a decrease in external quantum efficiency and an increase in dark current. [Means for solving the problem]
[0011] In order to achieve the above object, an imaging element according to a first aspect of the present disclosure includes at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer. The carrier blocking layer is made of a material having the following structural formula (1) and has a thickness of 5×10 -9 m to 1.5×10 -7 m, preferably 5 x 10 -9 m to 1.0×10 -7 m.
[0012] [ka]
[0013] Where: R1 and R2 are each independently a group selected from hydrogen, an aryl group, and an alkyl group, and the aryl group is a group selected from the group consisting of a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, a naphthylphenyl group, a tolyl group, a xylyl group, a phenyl group substituted with an alkyl group having 2 to 6 carbon atoms, an anthracenyl group, an anthracenylphenyl group, a phenanthryl group, a phenanthrylphenyl group, a pyrenyl group, a pyrenylphenyl group, a tetracenyl group, a tetracenylphenyl group, a fluoranthenyl group, a fluoranthenylphenyl group, a pyridinyl group, a pyridinylphenyl group, a quinolinyl group, a quinolinylphenyl group, an acridinyl group, an acridinylphenyl group, an indole group, an indolylphenyl group, an imidazole group, an imidazolylphenyl group, a benzimidazole group, a benzimidazolylphenyl group, a thienyl group, and a thienylphenyl group; The alkyl group is a group selected from the group consisting of a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and may be a linear alkyl group or a branched alkyl group.
[0014] In order to achieve the above object, an imaging element according to a second aspect of the present disclosure includes at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer. The carrier blocking layer is made of a material having the following structural formula (2) and has a thickness of 5×10 -9m to 1.5×10 -7 m, preferably 5 x 10 -9 m to 1.0×10 -7 m.
[0015] [ka]
[0016] Here, Ar1 and Ar2 are each independently an aryl group which may have a substituent, and are selected from the group consisting of a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, a naphthylphenyl group, a tolyl group, a xylyl group, a phenyl group substituted with an alkyl group having 2 to 6 carbon atoms, an anthracenyl group, an anthracenylphenyl group, a phenanthryl group, a phenanthrylphenyl group, a pyrenyl group, a pyrenylphenyl group, a tetracenyl group, a tetracenylphenyl group, a fluoranthenyl group, a fluoranthenylphenyl group, a pyridinyl group, a pyridinylphenyl group, a quinolinyl group, a quinolinylphenyl group, an acridinyl group, an acridinylphenyl group, an indole group, an indolylphenyl group, an imidazole group, an imidazolylphenyl group, a benzimidazole group, a benzimidazolylphenyl group, a thienyl group, and a thienylphenyl group.
[0017] In order to achieve the above object, an imaging element according to a third aspect of the present disclosure includes at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer. The carrier blocking layer is made of a material having the following structural formula (3) and has a thickness of 5×10 -9 m to 1.5×10 -7 m, preferably 5 x 10 -9 m to 1.0×10 -7 m.
[0018] [ka]
[0019] In order to achieve the above object, a stacked type imaging element (a longitudinal spectroscopy imaging element) of the present disclosure is formed by stacking at least two imaging elements according to the first to third aspects of the present disclosure.
[0020] In order to achieve the above object, an imaging device according to a first aspect of the present disclosure includes a plurality of imaging elements according to the first to third aspects of the present disclosure. In such an imaging device according to the first aspect of the present disclosure, a blue imaging element, a green imaging element, and a red imaging element may be arranged on a plane such as a Bayer array. In addition, in order to achieve the above object, an imaging device according to a second aspect of the present disclosure includes a plurality of stacked imaging elements according to the present disclosure. Effect of the Invention
[0021] In the imaging element according to the first to third aspects of the present disclosure, the imaging element constituting the stacked imaging element of the present disclosure, and the imaging device constituting the imaging apparatus according to the first to second aspects of the present disclosure (hereinafter, these imaging elements are collectively referred to as "the imaging element, etc. of the present disclosure"), the carrier blocking layer is made of a material having structural formula (1), structural formula (2), or structural formula (3) that absorbs little visible light, so that it is possible to achieve both good external quantum efficiency and spectral characteristics without interfering with the photoelectric conversion of the imaging element including the carrier blocking layer or the imaging element located in the lower layer as viewed from the light incidence direction. Moreover, it is possible to suppress dark current and improve the withstand voltage characteristics of dark current. Furthermore, it is possible to reduce the capacitance of the electric capacitance. In addition, it is possible to improve the so-called afterimage characteristics. As a result of the above, it is possible to realize an imaging device that can output a beautiful image and is less likely to cause afterimages. Note that the effects described in this specification are merely examples and are not limited, and additional effects may be present. [Brief description of the drawings]
[0022] [Figure 1] 1A and 1B are conceptual diagrams of an image sensor according to a first embodiment. [Diagram 2]2A and 2B are a schematic partial cross-sectional view of an image sensor for evaluation in Example 1, and a schematic diagram showing the flow of holes and electrons generated by photoelectric conversion, respectively. [Diagram 3] FIG. 3 is a conceptual diagram of the imaging device of the first embodiment. [Figure 4] FIG. 4A shows the results of determining the external quantum efficiency when the imaging elements of Example 1, and Comparative Example 1A, Comparative Example 1B, and Comparative Example 1C were irradiated with light having a wavelength of 560 nm and 2 microwatts / cm2 and a voltage of -2.6 volts was applied between the second electrode and the first electrode. FIG. 4B shows the results of measuring the dark current in a dark place when the imaging elements of Example 1, Comparative Example 1A, Comparative Example 1B, and Comparative Example 1C have a first carrier blocking layer with a thickness of 100 nm and voltages from -1 volt to -10 volts were applied between the second electrode and the first electrode. [Diagram 5] FIG. 5 is a diagram showing the results of determining the optical absorption spectrum (optical absorption ratio) of a thin film made of a material having structural formula (3). [Figure 6] FIG. 6 is a graph showing the relationship between carrier mobility and the value of T0 in Example 2. [Figure 7] 7A and 7B are conceptual diagrams of a stack-type imaging element according to a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, the present disclosure will be described based on examples with reference to the drawings, but the present disclosure is not limited to the examples, and various numerical values and materials in the examples are merely examples. The description will be made in the following order. 1. General Description of the Imaging Device According to the First to Third Aspects of the Present Disclosure, the Stacked Imaging Device According to the Present Disclosure, and the Imaging Device According to the First and Second Aspects of the Present Disclosure 2. Example 1 (Imaging element according to the first to third aspects of the present disclosure, imaging device according to the first aspect of the present disclosure) 3. Example 2 (Modification of Example 1) 4. Example 3 (Modifications of Examples 1 and 2, Stacked Imaging Element of the Present Disclosure, and Imaging Device According to the Second Aspect of the Present Disclosure) 5.Other
[0024] <General Description of the Imaging Element According to the First to Third Aspects of the Present Disclosure, the Stacked Imaging Element According to the Present Disclosure, and the Imaging Device According to the First and Second Aspects of the Present Disclosure> Specifically, the stacked imaging element of the present disclosure may include an imaging element according to the first to third embodiments of the present disclosure having sensitivity to blue light (light of 425 nm to 495 nm) (for convenience, referred to as a "blue imaging element"), an imaging element according to the first to third embodiments of the present disclosure having sensitivity to green light (light of 495 nm to 570 nm) (for convenience, referred to as a "green imaging element"), and an imaging element according to the first to third embodiments of the present disclosure having sensitivity to red light (light of 620 nm to 750 nm) (for convenience, referred to as a "red imaging element"), which are stacked vertically. Note that the stacking order of these imaging elements is preferably the blue imaging element, the green imaging element, and the red imaging element from the light incidence direction, or the green imaging element, the blue imaging element, and the red imaging element from the light incidence direction. This is because light with a shorter wavelength is absorbed more efficiently on the incident surface side. Since red has the longest wavelength among the three colors, it is preferable to position the red imaging element at the bottom layer as viewed from the light incident surface. Alternatively, it is also possible to form an imaging element having sensitivity to red on a silicon semiconductor substrate, and form a green imaging element and a blue imaging element on the silicon semiconductor substrate, or to form two types of imaging elements on a silicon semiconductor substrate, and form one type of imaging element according to the first to third aspects of the present disclosure on the silicon semiconductor substrate. The imaging element formed on the silicon semiconductor substrate is preferably a back-illuminated type, but may also be a front-illuminated type.In addition, examples of inorganic materials constituting the photoelectric conversion layer include, in addition to crystalline silicon, amorphous silicon, microcrystalline silicon, crystalline selenium, amorphous selenium, and chalcopyrite compounds such as CIGS (CuInGaSe), CIS (CuInSe2), CuInS2, CuAlS2, CuAlSe2, CuGaS2, CuGaSe2, AgAlS2, AgAlSe2, AgInS2, and AgInSe2, as well as III-V group compounds such as GaAs, InP, AlGaAs, InGaP, AlGaInP, and InGaAsP, as well as compound semiconductors such as CdSe, CdS, In2Se3, In2S3, Bi2Se3, Bi2S3, ZnSe, ZnS, PbSe, and PbS. In addition, quantum dots made of these materials can also be used in the inorganic photoelectric conversion layer. Moreover, a single-chip color solid-state imaging device can be configured using the imaging devices according to the first and second aspects of the present disclosure.
[0025] In the imaging device according to the second aspect of the present disclosure, which includes a stacked imaging element, unlike an imaging device including an imaging element with a Bayer array (i.e., instead of using color filters to separate blue, green, and red light), imaging elements having sensitivity to light of a plurality of wavelengths are stacked in the direction of light incidence within the same pixel, so that it is possible to improve sensitivity and pixel density per unit volume. In addition, since organic materials have a high light absorption coefficient, the film thickness of the organic photoelectric conversion layer can be made thinner than that of a conventional Si-based photoelectric conversion layer, and light leakage from adjacent pixels and restrictions on the angle of incidence of light are alleviated. Furthermore, in the conventional Si-based imaging element, false colors occur because color signals are created by performing an interpolation process between three color pixels, but the occurrence of false colors is suppressed in the imaging device according to the second aspect of the present disclosure, which includes a stacked imaging element. On the other hand, in the imaging device according to the first aspect of the present disclosure, the use of color filters can alleviate the requirements for the spectral characteristics of blue, green, and red light, and the imaging device has high mass productivity.
[0026] In the imaging element etc. of the present disclosure, the first electrode may constitute an anode, the second electrode may constitute a cathode, and the carrier blocking layer may be provided between the first electrode and the organic photoelectric conversion layer, but is not limited to this configuration.
[0027] In the imaging element etc. of the present disclosure including the above preferred embodiment, the carrier blocking layer preferably has a small light absorption rate in the visible light region as much as possible so as not to hinder the photoelectric conversion function in the organic photoelectric conversion layer. In the imaging element etc. of the present disclosure, the light absorption rate of the carrier blocking layer can be 3% or less at a wavelength of 450 nm, 30% or less at a wavelength of 425 nm, and 80% or less at a wavelength of 400 nm when the thickness of the carrier blocking layer is converted to 150 nm. That is, the carrier blocking layer made of the material having the above structural formula (1), structural formula (2), or structural formula (3) also has excellent spectral characteristics. In general, many organic compounds have high light absorption intensity in the wavelength region shorter than 450 nm, and there is a problem that they absorb blue light that should be absorbed by the organic photoelectric conversion layer of the imaging element. However, in the imaging element etc. of the present disclosure, the material constituting the carrier blocking layer has excellent light absorption characteristics and does not hinder the photoelectric conversion function of the imaging element.
[0028] In the imaging device and the like of the present disclosure including the various preferred embodiments described above, the carrier mobility of the material constituting the carrier blocking layer is 9×10 -4 cm 2 / V s or more, preferably 9×10 -3 cm 2 / V s or more, preferably 6×10 -2 cm 2 / V s or more is desirable.
[0029] In the imaging element and the like of the present disclosure including the various preferred embodiments described above, a wavelength of 560 nm and 2 microwatts / cm are applied while applying −3 volts between the second electrode and the first electrode. 2When light is irradiated to the second electrode and then the light irradiation is stopped, the amount of current flowing between the second electrode and the first electrode just before the light irradiation is stopped is defined as I0, and the time from the stop of light irradiation until the amount of current becomes (0.03×I0) is defined as T0. It is desirable that T0 be 10 milliseconds or less.
[0030] In the imaging element and the like of the present disclosure including the various preferred embodiments described above, when light is irradiated and photoelectric conversion is performed in the organic photoelectric conversion layer, holes and electrons are separated as carriers. The electrode from which the holes are extracted is the anode, and the electrode from which the electrons are extracted is the cathode. Here, when configuring a stacked type imaging element, the first electrode and the second electrode can be configured to be made of a transparent conductive material. Alternatively, when the imaging element or the like of the present disclosure is arranged on a plane, for example, as in a Bayer array, one of the first electrode and the second electrode can be made of a transparent conductive material and the other can be made of a metal material. In this case, the first electrode located on the light incident side can be made of a transparent conductive material, and the second electrode can be made of Al (aluminum), Al-Si-Cu (alloy of aluminum, silicon and copper) or Mg-Ag (alloy of magnesium and silver), or the second electrode located on the light incident side can be made of a transparent conductive material, and the first electrode can be made of Al-Nd (alloy of aluminum and neodymium) or ASC (alloy of aluminum, samarium and copper). Note that an electrode made of a transparent conductive material may be called a "transparent electrode".Here, examples of the transparent conductive material constituting the transparent electrode include conductive metal oxides. Specifically, examples of the transparent conductive material include indium oxide, indium tin oxide (ITO, Indium Tin Oxide, including Sn-doped In2O3, crystalline ITO, and amorphous ITO), and indium zinc oxide (IZO, Indium Zinc Oxide) in which indium is added as a dopant to zinc oxide. Examples of the oxide include indium-gallium oxide (IGO) in which indium is added as a dopant to gallium oxide, indium-gallium-zinc oxide (IGZO, In-GaZnO4) in which indium and gallium are added as dopants to zinc oxide, IFO (F-doped In2O3), tin oxide (SnO2), ATO (Sb-doped SnO2), FTO (F-doped SnO2), zinc oxide (including ZnO doped with other elements), aluminum-zinc oxide (AZO) in which aluminum is added as a dopant to zinc oxide, gallium-zinc oxide (GZO) in which gallium is added as a dopant to zinc oxide, titanium oxide (TiO2), antimony oxide, spinel-type oxide, and oxides having a YbFe2O4 structure. Alternatively, examples of the transparent electrode include a base layer of gallium oxide, titanium oxide, niobium oxide, nickel oxide, etc. The thickness of the transparent electrode is 2×10. -8 m to 2×10 -7 m, preferably 3 × 10 -8 m to 1×10 -7 m can be mentioned.
[0031] Alternatively, when transparency is not required, the conductive material constituting the anode having the function as an electrode for extracting holes is preferably composed of a conductive material having a high work function (for example, φ=4.5 eV to 5.5 eV). Specific examples of such a conductive material include gold (Au), silver (Ag), chromium (Cr), nickel (Ni), palladium (Pd), platinum (Pt), iron (Fe), iridium (Ir), germanium (Ge), osmium (Os), rhenium (Re), and tellurium (Te). On the other hand, the conductive material constituting the cathode having the function as an electrode for extracting electrons is preferably composed of a conductive material having a low work function (for example, φ=3.5 eV to 4.5 eV). Specific examples of the conductive material include alkali metals (for example, Li, Na, K, etc.) and their fluorides or oxides, alkaline earth metals (for example, Mg, Ca, etc.) and their fluorides or oxides, aluminum (Al), zinc (Zn), tin (Sn), thallium (Tl), sodium-potassium alloys, aluminum-lithium alloys, magnesium-silver alloys, indium, ytterbium, and other rare earth metals, and alloys thereof. Alternatively, the materials constituting the anode and cathode may include metals such as platinum (Pt), gold (Au), palladium (Pd), chromium (Cr), nickel (Ni), aluminum (Al), silver (Ag), tantalum (Ta), tungsten (W), copper (Cu), titanium (Ti), indium (In), tin (Sn), iron (Fe), cobalt (Co), and molybdenum (Mo), or alloys containing these metal elements, conductive particles made of these metals, conductive particles of alloys containing these metals, polysilicon containing impurities, carbon-based materials, oxide semiconductors, carbon nanotubes, graphene, and other conductive substances, or may have a laminated structure of layers containing these elements. Furthermore, the materials constituting the anode and cathode may include organic materials (conductive polymers) such as poly(3,4-ethylenedioxythiophene) / polystyrenesulfonic acid [PEDOT / PSS]. Moreover, these conductive materials may be mixed with a binder (polymer) to form a paste or ink, which may then be hardened and used as an electrode.
[0032] As a method for forming the first electrode and the second electrode (anode and cathode), a dry method or a wet method can be used. Examples of the dry method include physical vapor deposition (PVD) and chemical vapor deposition (CVD). Examples of the film formation method using the principle of the PVD method include vacuum deposition using resistance heating or high-frequency heating, EB (electron beam) deposition, various sputtering methods (magnetron sputtering, RF-DC coupled bias sputtering, ECR sputtering, facing target sputtering, and high-frequency sputtering), ion plating, laser ablation, molecular beam epitaxy, and laser transfer. Examples of the CVD method include plasma CVD, thermal CVD, metal organic (MO) CVD, and photo CVD. On the other hand, examples of the wet method include electrolytic plating, electroless plating, spin coating, inkjet printing, spray coating, stamping, microcontact printing, flexographic printing, offset printing, gravure printing, and dip printing. For patterning, chemical etching such as shadow masks, laser transfer, and photolithography, and physical etching using ultraviolet rays, lasers, etc. can be used. For planarization, laser planarization, reflow, CMP (Chemical Mechanical Polishing), etc. can be used.
[0033] The organic photoelectric conversion layer is (1) It is composed of a p-type organic semiconductor. (2) Consists of a laminated structure of a p-type organic semiconductor layer / n-type organic semiconductor layer. Consists of a laminated structure of a p-type organic semiconductor layer / mixed layer of p-type organic semiconductor and n-type organic semiconductor (bulk heterostructure) / n-type organic semiconductor layer. Consists of a laminated structure of a p-type organic semiconductor layer / mixed layer of p-type organic semiconductor and n-type organic semiconductor (bulk heterostructure). Consists of a laminated structure of an n-type organic semiconductor layer / mixed layer of p-type organic semiconductor and n-type organic semiconductor (bulk heterostructure). (3) It is composed of a mixture of p-type and n-type organic semiconductors (bulk heterostructure). The above three aspects can be adopted.
[0034] Examples of p-type organic semiconductors include naphthalene derivatives, anthracene derivatives, phenanthrene derivatives, pyrene derivatives, perylene derivatives, tetracene derivatives, pentacene derivatives, quinacridone derivatives, picene derivatives, chrysene derivatives, fluoranthene derivatives, phthalocyanine derivatives, subphthalocyanine derivatives, metal complexes having heterocyclic compounds as ligands, etc. Examples of n-type organic semiconductors include fullerenes and fullerene derivatives, organic semiconductors having larger (deeper) HOMO and LUMO than p-type organic semiconductors, and transparent inorganic metal oxides. Specific examples of n-type organic semiconductors include heterocyclic compounds containing nitrogen atoms, oxygen atoms, and sulfur atoms, such as pyridine, pyrazine, pyrimidine, triazine, quinoline, quinoxaline, isoquinoline, acridine, phenazine, phenanthroline, tetrazole, pyrazole, imidazole, thiazole, oxazole, imidazole, benzimidazole, benzotriazole, benzoxazole, carbazole, benzofuran, and dibenzofuran, as part of the molecular skeleton, organic metal complexes, and subphthalocyanine derivatives. The thickness of the organic photoelectric conversion layer is not limited, but may be, for example, 1×10 -8 m to 5×10 -7 m, preferably 2.5 × 10 -8 m to 3×10 -7 m, more preferably 2.5 × 10 -8 m to 2×10 -7 m, more preferably 1×10 -7 m to 1.8×10 -7 Examples of the organic semiconductor include p-type and n-type. Although organic semiconductors are often classified as p-type and n-type, the p-type means that they easily transport holes, and the n-type means that they easily transport electrons, and are not limited to the interpretation that they have holes or electrons as the majority carriers of thermal excitation like inorganic semiconductors.
[0035] Examples of the film formation method of various organic layers include a dry film formation method and a wet film formation method. Examples of the dry film formation method include a vacuum deposition method using resistance heating or high-frequency heating, an EB deposition method, various sputtering methods (magnetron sputtering method, RF-DC coupled bias sputtering method, ECR sputtering method, facing target sputtering method, high-frequency sputtering method), an ion plating method, a laser ablation method, a molecular beam epitaxy method, and a laser transfer method. Examples of the CVD method include a plasma CVD method, a thermal CVD method, an MOCVD method, and a photo-CVD method. On the other hand, examples of the wet method include a spin coat method, an inkjet method, a spray coat method, a stamp method, a microcontact printing method, a flexographic printing method, an offset printing method, a gravure printing method, and a dip method. For patterning, a shadow mask, a laser transfer method, chemical etching such as photolithography, and physical etching using ultraviolet rays or a laser can be used. Examples of the planarization technique include a laser planarization method and a reflow method.
[0036] When forming the carrier blocking layer, it is also possible to co-deposit the material having the structural formula (1), the structural formula (2), or the structural formula (3) and another organic semiconductor material (for example, a pentacene derivative).
[0037] A second carrier blocking layer may be provided between the organic photoelectric conversion layer and the second electrode (cathode). The carrier blocking layer provided between the organic photoelectric conversion layer and the first electrode (anode) may be referred to as the "first carrier blocking layer" for convenience. The material used for the second carrier blocking layer (second carrier blocking material) is preferably a material having a larger (deeper) ionization potential than the material used for the first carrier blocking layer, and specifically, for example, organic molecules and organometallic complexes having a nitrogen (N)-containing heterocycle as a part of the molecular skeleton, such as pyridine, quinoline, acridine, indole, imidazole, benzimidazole, and phenanthroline, and materials with low optical absorption in the visible light region are preferred. In addition, when the second carrier blocking layer is formed as a thin film of about 5×10-9m to 2×10-8m, fullerenes such as C60 and C70 can also be used. However, the second carrier blocking layer is not limited to these.
[0038] An electron injection layer may be provided between the second carrier blocking layer and the second electrode. Examples of materials constituting the electron injection layer include alkali metals such as lithium (Li), sodium (Na), and potassium (K), and fluorides and oxides thereof, and alkaline earth metals such as magnesium (Mg) and calcium (Ca), and fluorides and oxides thereof.
[0039] In addition, the imaging element or imaging device may be provided with an on-chip microlens or a light-shielding layer as necessary, and may be provided with a driving circuit and wiring for driving the imaging element. If necessary, a shutter for controlling the incidence of light into the imaging element may be provided, and an optical cut filter may be provided depending on the purpose of the imaging device. Furthermore, examples of the arrangement of the imaging element in the imaging device according to the first aspect of the present disclosure include, in addition to the Bayer arrangement, an interline arrangement, a G-stripe RB checkered arrangement, a G-stripe RB complete checkered arrangement, a checkered complementary color arrangement, a stripe arrangement, a diagonal stripe arrangement, a primary color color difference arrangement, a field color difference sequential arrangement, a frame color difference sequential arrangement, a MOS type arrangement, an improved MOS type arrangement, a frame interleaved arrangement, and a field interleaved arrangement.
[0040] The imaging element of the present disclosure can be formed on a substrate. Here, examples of the substrate include organic polymers (having the form of polymeric materials such as flexible plastic films, plastic sheets, and plastic substrates made of polymeric materials) such as polymethyl methacrylate (polymethyl methacrylate, PMMA), polyvinyl alcohol (PVA), polyvinylphenol (PVP), polyethersulfone (PES), polyimide, polycarbonate (PC), polyethylene terephthalate (PET), and polyethylene naphthalate (PEN). If a substrate made of such a flexible polymeric material is used, it becomes possible to incorporate or integrate the imaging element into, for example, an electronic device having a curved surface. Alternatively, examples of the substrate include various glass substrates, various glass substrates having an insulating film formed on the surface, quartz substrates, quartz substrates having an insulating film formed on the surface, silicon semiconductor substrates, silicon semiconductor substrates having an insulating film formed on the surface, and metal substrates made of various alloys such as stainless steel and various metals. Note that examples of the insulating film include silicon oxide-based materials (e.g., SiO X and spin-on glass (SOG); silicon nitride (SiN Y); silicon oxynitride (SiON); aluminum oxide (Al2O3); metal oxides and metal salts. In addition, a conductive substrate (a substrate made of a metal such as gold or aluminum, or a substrate made of highly oriented graphite) on whose surface an insulating film is formed can also be used. The surface of the substrate is preferably smooth, but may be rough to a degree that does not adversely affect the characteristics of the organic photoelectric conversion layer. The adhesion between the electrode and the substrate can be improved by forming a silanol derivative on the surface of the substrate by the silane coupling method, forming a thin film made of a thiol derivative, a carboxylic acid derivative, a phosphoric acid derivative, or the like by the SAM method, or forming a thin film made of an insulating metal salt or metal complex by the CVD method.
[0041] In some cases, the electrodes may be covered with a coating layer. Examples of materials constituting the coating layer include silicon oxide-based materials; silicon nitride (SiN Y ); metal oxide high dielectric insulating film such as aluminum oxide (Al2O3) and the like; as well as inorganic insulating materials such as polymethyl methacrylate (PMMA); polyvinylphenol (PVP); polyvinyl alcohol (PVA); polyimide; polycarbonate (PC); polyethylene terephthalate (PET); polystyrene; silanol derivatives (silane coupling agents) such as N-2 (aminoethyl) 3-aminopropyltrimethoxysilane (AEAPTMS), 3-mercaptopropyltrimethoxysilane (MPTMS), octadecyltrichlorosilane (OTS), and the like; and straight-chain hydrocarbons having a functional group at one end capable of bonding to an electrode, such as octadecanethiol and dodecyl isocyanate, and combinations of these may also be used. Silicon oxide-based materials include silicon oxide (SiO X), BPSG, PSG, BSG, AsSG, PbSG, silicon oxynitride (SiON), SOG (spin-on glass), and low dielectric constant materials (e.g., polyaryl ether, cycloperfluorocarbon polymer and benzocyclobutene, cyclic fluororesin, polytetrafluoroethylene, fluorinated aryl ether, fluorinated polyimide, amorphous carbon, and organic SOG). As a method for forming the insulating layer, for example, the above-mentioned dry film formation method and wet film formation method can be used.
[0042] By forming a carrier blocking layer from materials having structural formula (1), structural formula (2), or structural formula (3), there is no deterioration in sensitivity even when the carrier blocking layer is made thick. The reason for this is thought to be that the thienoacene skeleton, which is the parent skeleton, overlaps in the carrier blocking layer, and efficiently transports carriers even when the layer is made thick. On the other hand, the dark current reduction and dark current withstand voltage characteristics are excellent, and this is presumed to be related to the energy levels of the p-type organic semiconductor and the carrier blocking layer in the organic photoelectric conversion layer, the thin film surface roughness when the carrier blocking layer made of materials having structural formula (1), structural formula (2), or structural formula (3) is made thick, the stress of the carrier blocking layer, etc.
[0043] The carrier blocking layer may have a laminated structure of a material layer having the structural formula (1), the structural formula (2), or the structural formula (3) and another material layer. Specifically, for example, in order to improve electrical connection, aromatic amine-based materials such as triarylamine compounds, benzidine compounds, and styrylamine compounds, carbazole derivatives, naphthalene derivatives, anthracene derivatives, phenanthrene derivatives, pyrene derivatives, perylene derivatives, tetracene derivatives, pentacene derivatives, picene derivatives, chrysene derivatives, fluoranthene derivatives, phthalocyanine derivatives, subphthalocyanine derivatives, hexaazatriphenylene derivatives, metal complexes having heterocyclic compounds as ligands, poly(3,4-ethylenedioxythiophene) / polystyrenesulfonic acid [PEDOT / PSS], polyaniline, molybdenum oxide (MoO x), ruthenium oxide (RuO x ), vanadium oxide (VOx), tungsten oxide (WO x ) or the like may be formed. EXAMPLES
[0044] A first embodiment relates to an imaging element according to the first to third aspects of the present disclosure, and an imaging device according to the first aspect of the present disclosure.
[0045] As shown in the conceptual diagrams of FIGS. 1A and 1B, the imaging element 11 of Example 1 includes at least a first electrode 21, a second electrode 25, an organic photoelectric conversion layer 23, and a carrier blocking layer 22. Specifically, the first electrode 21 constitutes an anode, the second electrode 25 constitutes a cathode, and the carrier blocking layer 22 is provided between the first electrode 21 and the organic photoelectric conversion layer 23. More specifically, the imaging element 11 of Example 1 includes at least a first electrode (anode) 21, a carrier blocking layer (first carrier blocking layer 22), an organic photoelectric conversion layer 23, and a second electrode (cathode) 25, which are sequentially laminated. Note that a second carrier blocking layer 24 is provided between the organic photoelectric conversion layer 23 and the second electrode 25. The first carrier blocking layer 22 is made of a material having the above structural formula (1), structural formula (2), or structural formula (3), and has a thickness of 5×10 -9 m to 1.5×10 -7 m, preferably 5 × 10 -9 m to 1.0×10 -7 m, more preferably 5×10 -8 m to 1.0×10 -7 m. In the image sensor shown in FIG. 1A, light is incident from the second electrode side (cathode side). On the other hand, in the image sensor shown in FIG. 1B, light is incident from the first electrode side (anode side). The flow of holes (indicated by "+" in a circle) and electrons (indicated by "-" in a circle) generated by photoelectric conversion is shown diagrammatically in FIG. 2B.
[0046] The imaging device 40 of the first embodiment includes a plurality of imaging elements 11 of the first embodiment. Specifically, a blue imaging element, a green imaging element, and a red imaging element are arranged on a plane like a Bayer array.
[0047] In the imaging element of Example 1, either the first electrode 21 or the second electrode 25 is made of a transparent conductive material, and the other is made of a metal material. In the imaging element shown in FIG. 1A, light is incident from the second electrode side (cathode side), so the second electrode 25 is made of a transparent conductive material (e.g., ITO), and the first electrode 21 is made of Al-Nd (alloy of aluminum and neodymium) or ASC (alloy of aluminum, samarium and copper). On the other hand, in the imaging element shown in FIG. 1B, light is incident from the first electrode side (anode side), so the first electrode 21 is made of a transparent conductive material (e.g., ITO), and the second electrode 25 is made of Al (aluminum), Al-Si-Cu (alloy of aluminum, silicon and copper), or Mg-Ag (alloy of magnesium and silver).
[0048] The second carrier blocking layer 24 is made of, for example, the second carrier blocking material described above, but if the second electrode (cathode) is made of a metal material, using a material containing an element that coordinates with the metal is expected to improve the electrical connection with the second electrode and reduce the resistance component. For example, organic molecules and organometallic complexes that have a nitrogen (N)-containing heterocycle as part of their molecular skeleton, such as pyridine, quinoline, acridine, indole, imidazole, benzimidazole, and phenanthroline, and that have low optical absorption in the visible light region are preferred. In addition, in the organic photoelectric conversion layer 23 of a blue imaging element having sensitivity to blue light and including an organic photoelectric conversion layer that absorbs blue light (light of 425 nm to 495 nm), examples of p-type organic semiconductors include naphthalene derivatives, anthracene derivatives, phenanthrene derivatives, pyrene derivatives, tetracene derivatives, picene derivatives, chrysene derivatives, fluoranthene derivatives, and metal complexes having heterocyclic compounds as ligands, and examples of n-type organic semiconductors include fullerene and fullerene derivatives, organic semiconductors having larger (deeper) HOMO and LUMO than p-type organic semiconductors, and transparent inorganic metal oxides. Specific examples of n-type organic semiconductors include heterocyclic compounds containing nitrogen atoms, oxygen atoms, and sulfur atoms, such as organic molecules and organometallic complexes having pyridine, pyrazine, pyrimidine, triazine, quinoline, quinoxaline, isoquinoline, acridine, phenazine, phenanthroline, tetrazole, pyrazole, imidazole, thiazole, oxazole, imidazole, benzimidazole, benzotriazole, benzoxazole, carbazole, benzofuran, and dibenzofuran as part of the molecular skeleton. The thickness of the organic photoelectric conversion layer is not limited, but may be, for example, 1×10 -8 m to 5×10 -7 m, preferably 2.5 × 10 -8 m to 3×10 -7 m, more preferably 2.5 × 10 -8 m to 2×10 -7 m, more preferably 1×10 -7 m to 1.8×10 -7m can be exemplified. In the organic photoelectric conversion layer 23 in the green imaging element having sensitivity to green light and including an organic photoelectric conversion layer that absorbs green light (light of 495 nm to 570 nm), examples of the p-type organic semiconductor include anthracene derivatives, phenanthrene derivatives, pyrene derivatives, perylene derivatives, tetracene derivatives, quinacridone derivatives, fluoranthene derivatives, subphthalocyanine derivatives, and metal complexes having a heterocyclic compound as a ligand, and examples of the n-type organic semiconductor include fullerene and fullerene derivatives, organic semiconductors having larger (deeper) HOMO and LUMO than p-type organic semiconductors, and transparent inorganic metal oxides. Specific examples of n-type organic semiconductors include heterocyclic compounds containing nitrogen atoms, oxygen atoms, and sulfur atoms, such as pyridine, pyrazine, pyrimidine, triazine, quinoline, quinoxaline, isoquinoline, acridine, phenazine, phenanthroline, tetrazole, pyrazole, imidazole, thiazole, oxazole, imidazole, benzimidazole, benzotriazole, benzoxazole, carbazole, benzofuran, and dibenzofuran, as part of the molecular skeleton, organic metal complexes, and subphthalocyanine derivatives. The thickness of the organic photoelectric conversion layer is not limited, but may be, for example, 1×10 -8 m to 5×10 -7 m, preferably 2.5 × 10 -8 m to 3×10 -7 m, more preferably 2.5 × 10 -8 m to 2×10 -7 m, more preferably 1×10 -7 m to 1.8×10 -7m can be exemplified. In the organic photoelectric conversion layer 23 in the red imaging element having sensitivity to red light and including an organic photoelectric conversion layer that absorbs red light (light of 620 nm to 750 nm), examples of the p-type organic semiconductor include pentacene derivatives, quinacridone derivatives, perylene derivatives, fluoranthene derivatives, phthalocyanine derivatives, subphthalocyanine derivatives, and metal complexes having a heterocyclic compound as a ligand, and examples of the n-type organic semiconductor include fullerene and fullerene derivatives, organic semiconductors having larger (deeper) HOMO and LUMO than p-type organic semiconductors, and transparent inorganic metal oxides. Specific examples of n-type organic semiconductors include heterocyclic compounds containing nitrogen atoms, oxygen atoms, and sulfur atoms, such as pyridine, pyrazine, pyrimidine, triazine, quinoline, quinoxaline, isoquinoline, acridine, phenazine, phenanthroline, tetrazole, pyrazole, imidazole, thiazole, oxazole, imidazole, benzimidazole, benzotriazole, benzoxazole, carbazole, benzofuran, and dibenzofuran, as part of the molecular skeleton, organic metal complexes, and subphthalocyanine derivatives. The thickness of the organic photoelectric conversion layer is not limited, but may be, for example, 1×10 -8 m to 5×10 -7 m, preferably 2.5 × 10 -8 m to 3×10 -7 m, more preferably 2.5 × 10 -8 m to 2×10 -7 m can be exemplified.
[0049] An imaging element for evaluation, the partial cross-sectional view of which is shown in Fig. 2A, was fabricated by the following method. The imaging element for evaluation was a green imaging element.
[0050] A sputtering device was used to form an ITO film having a thickness of 120 nm on a substrate 20 made of quartz, and a first electrode (anode) 21 made of the ITO film was obtained based on photolithography and etching techniques. Next, an insulating layer 31 was formed on the substrate 20 and the first electrode 21, and the insulating layer 31 was patterned based on photolithography and etching techniques to expose the first electrode 21 having a size of 1 mm square, followed by ultrasonic cleaning using detergent, acetone, and ethanol. The substrate was then dried, and further subjected to ultraviolet / ozone treatment for 10 minutes. Next, the substrate 20 was fixed to a substrate holder in a vacuum deposition device, and the deposition chamber was filled with 5.5×10 -5 The pressure was reduced to 10 Pa.
[0051] Then, based on the vacuum deposition method using a shadow mask, a first carrier blocking layer 22 made of a material having the structural formula (3) was formed on the first electrode 21 with five levels of film thickness, 5 nm, 50 nm, 100 nm, 150 nm, and 200 nm. Subsequently, in a vacuum deposition apparatus, quinacridone (QD) and subphthalocyanine chloride (SubPc-Cl) were co-deposited to a thickness of 120 nm at a deposition rate ratio of 1:1 to form an organic photoelectric conversion layer 23. The organic photoelectric conversion layer 23 is composed of a mixed layer (bulk heterostructure) of a p-type organic semiconductor and an n-type organic semiconductor. Furthermore, subsequently, NBphen was vacuum-deposited to a thickness of 5 nm to form a second carrier blocking layer 24. Thereafter, the substrate was carried into another sputtering apparatus under an inert atmosphere, and a second electrode (cathode) 25 made of ITO to a thickness of 60 nm was formed on the second carrier blocking layer 24. Thereafter, annealing treatment was performed for 2 hours and 30 minutes in a nitrogen atmosphere at 150° C., to obtain an imaging element for evaluation of Example 1, the partial cross-sectional view of which is shown in FIG. 2A.
[0052] Quinacridone (QD) [ka]
[0053] <Subphthalocyanine chloride (SubPc-Cl)> [ka]
[0054] <NBphen> [ka]
[0055] Comparative Example 1A An imaging element of Comparative Example 1A was produced in the same manner as in Example 1, except that the first carrier blocking layer was formed using the following compound-A at three different thicknesses, 5 nm, 50 nm, and 100 nm.
[0056] <Compound-A> [ka]
[0057] <Comparative example 1B> An imaging element of Comparative Example 1B was produced in the same manner as in Example 1, except that the first carrier blocking layer was formed to three different thicknesses, 5 nm, 50 nm, and 100 nm, using the following Compound-B.
[0058] <Compound-B> [ka]
[0059] <Comparative example 1C> An imaging element of Comparative Example 1C was produced in the same manner as in Example 1, except that the first carrier blocking layer was formed using the following Compound-C at three different thicknesses, 5 nm, 50 nm, and 100 nm.
[0060] <Compound-C> [ka]
[0061] The imaging devices of Example 1, Comparative Example 1A, Comparative Example 1B, and Comparative Example 1C were exposed to a wavelength of 560 nm and 2 microwatts / cm 2 While irradiating the sample with light of 1000 nm, a voltage of -2.6 volts (so-called reverse bias voltage of 2.6 volts) was applied between the second electrode (cathode) and the first electrode (anode), and the external quantum efficiency (EQE) was determined. The results are shown in Table 1 and FIG. 4A below. Note that FIG. 4A shows data for film thicknesses of 5 nm, 50 nm, and 100 nm for Example 1, Comparative Example 1A, Comparative Example 1B, and Comparative Example 1C, with the data for Example 1 indicated as "A", the data for Comparative Example 1A as "B", the data for Comparative Example 1B as "C", and the data for Comparative Example 1C as "D". The same is true for FIG. 4B described later.
[0062] [Table 1]
[0063] In Comparative Example 1A, Comparative Example 1B, and Comparative Example 1C, in which an aromatic amine compound and a carbazole derivative used in an organic EL element and an organic thin-film solar cell were used in the first carrier blocking layer, the external quantum efficiency was significantly reduced as the thickness of the first carrier blocking layer was increased to 50 nm and 100 nm, and improvement in the conversion efficiency of the organic module due to reduction in capacity could not be achieved. On the other hand, in the imaging element of Example 1, in which a material having structural formula (3) was used in the first carrier blocking layer, it was found that when the thickness of the first carrier blocking layer was in the range of 5 nm to 200 nm, there was no reduction in external quantum efficiency, the imaging element could be made thick, and it was effective in reducing capacity.
[0064] The results of measuring the dark current by applying a voltage of -2.6 volts in a dark place between the second electrode (cathode) and the first electrode (anode) of the imaging elements of Example 1, and Comparative Examples 1A, 1B, and 1C are shown in the following Table 2. Table 3 shows the relative values of the dark current of Comparative Examples 1A, 1B, and 1C when the dark current value of Example 1 at each film thickness of the first carrier blocking layer is used as a reference.
[0065] [Table 2]
[0066] [Table 3]
[0067] From the results of Tables 2 and 3, in Comparative Example 1A, Comparative Example 1B, and Comparative Example 1C, the dark current tends to increase as the thickness of the first carrier blocking layer increases. In particular, at thicknesses of 50 nm and 100 nm, the dark current value is more than twice as high as that of Example 1. On the other hand, in the imaging element of Example 1 in which the material having the structural formula (3) is used as the first carrier blocking layer, the dark current value tends to increase slightly when the thickness of the first carrier blocking layer is in the range of 5 nm to 100 nm, but is kept at a sufficiently low value. However, as the thickness increases to 150 nm and 200 nm, the dark current value increases. Therefore, from these results, it was found that the thickness of the first carrier blocking layer is desirably 5 nm to 150 nm or less, preferably 5 nm to 100 nm. Although the reason why the dark current value increases when the thickness exceeds a certain level is not understood, it is believed that the increase in roughness of the surface of the first carrier blocking layer due to the thickening of the film and the change in stress cause a change in the interface state between the first carrier blocking layer and the organic photoelectric conversion layer, etc. From the above results, when the thickness of the first carrier blocking layer is in the range of 5 nm to 150 nm, a large S / N ratio can be obtained when the material having structural formula (3) is used for the first carrier blocking layer, and it is possible to provide an imaging element suitable for low capacitance. It is possible to provide.
[0068] Furthermore, voltages from -1 volts to -10 volts (so-called reverse bias voltages of 1 volt to 10 volts) were applied between the second electrode (cathode) and the first electrode (anode) of an image sensor having a first carrier blocking layer with a thickness of 100 nm, and the dark current was measured in a dark place. The results are shown in Table 4, and the graphed results are shown in Figure 4B.
[0069] [Table 4]
[0070] In comparison with Comparative Example 1A, Comparative Example 1B, and Comparative Example 1C, it is found that Example 1 has excellent dark current withstand voltage characteristics, since the increase in dark current is small even when the absolute value of the applied voltage increases. In other words, it is found that when the material having structural formula (3) is used for the first carrier blocking layer, not only can a large S / N ratio be obtained, but also the dark current withstand voltage characteristics that enable high-voltage operation of the image sensor are excellent.
[0071] The first carrier blocking layer is required to absorb as little light in the visible light region as possible, not only in terms of electrical characteristics, but also in terms of not interfering with the photoelectric conversion of the organic photoelectric conversion layer or inorganic photoelectric conversion layer constituting another imaging element located below, even when the first carrier blocking layer is made thick. As mentioned above, organic compounds generally have high absorption intensity in the wavelength region shorter than 450 nm, and there is a problem that they absorb blue light that should be absorbed by the organic photoelectric conversion layer of the imaging element. Therefore, in a spectroscopic simulation, it is calculated that the light absorption rate of the carrier blocking layer is preferably 3% or less at a wavelength of 450 nm, 30% or less at a wavelength of 425 nm, and 80% or less at a wavelength of 400 nm.
[0072] Spectroscopic measurements were performed to measure the light absorption in the visible light region when the material having structural formula (3) was made into a thin film. Specifically, a thin film of 50 nm thick made of the material having structural formula (3) was formed on a quartz substrate by vacuum deposition, and the light absorption spectrum (light absorption ratio) was calculated for a film thickness of 150 nm from light transmittance and light reflectance measurements. The results are shown in Figure 5. The light absorption ratios of the material having structural formula (3) at 450 nm, 425 nm, and 400 nm were 1.1%, 25.5%, and 77.7%, respectively, and it was found that the target values of the light absorption ratios at the three wavelengths could be achieved. In other words, it can be seen that the material having structural formula (3) can be made into a thick film up to 150 nm in terms of spectroscopic characteristics as well. In other words, it was found that the material having structural formula (3) has excellent light absorption characteristics and does not interfere with the photoelectric conversion function of the image sensor.
[0073] 3 shows a conceptual diagram of the imaging device of Example 1. The imaging device 40 of Example 1 is composed of an imaging region 41 in which the above-mentioned imaging elements 11 are arranged in a two-dimensional array on a semiconductor substrate (e.g., a silicon semiconductor substrate), and a vertical drive circuit 42, a column signal processing circuit 43, a horizontal drive circuit 44, an output circuit 45, a control circuit 46, and the like as peripheral circuits. It goes without saying that these circuits can be composed of well-known circuits, and can also be composed using other circuit configurations (e.g., various circuits used in conventional CCD imaging devices and CMOS imaging devices).
[0074] The control circuit 46 generates clock signals and control signals that serve as references for the operations of the vertical drive circuit 42, the column signal processing circuit 43, and the horizontal drive circuit 44, based on the vertical synchronizing signal, the horizontal synchronizing signal, and the master clock. The generated clock signals and control signals are then input to the vertical drive circuit 42, the column signal processing circuit 43, and the horizontal drive circuit 44.
[0075] The vertical drive circuit 42 is configured with, for example, a shift register, and sequentially selects and scans each imaging element 11 in the imaging area 41 in the vertical direction on a row-by-row basis. Then, pixel signals based on currents (signals) generated in accordance with the amount of light received in each imaging element 11 are sent to a column signal processing circuit 43 via vertical signal lines 47.
[0076] The column signal processing circuit 43 is arranged, for example, for each column of the image sensor 11, and performs signal processing such as noise removal and signal amplification on signals output from one row of the image sensor 11 using signals from black reference pixels (not shown, but formed around the effective pixel area) for each image sensor. A horizontal selection switch (not shown) is provided at the output stage of the column signal processing circuit 43 and connected between the horizontal signal line 48.
[0077] The horizontal drive circuit 44 is configured by, for example, a shift register, and sequentially outputs horizontal scanning pulses to sequentially select each of the column signal processing circuits 43 and output signals from each of the column signal processing circuits 43 to a horizontal signal line 48.
[0078] The output circuit 45 processes the signals sequentially supplied from each of the column signal processing circuits 43 via the horizontal signal line 48 and outputs the processed signals.
[0079] Here, since the organic photoelectric conversion layer itself functions as a color filter, color separation is possible without providing a color filter.
[0080] As described above, in the imaging element of Example 1, the carrier blocking layer disposed between the organic photoelectric conversion layer and the first electrode is made of a material having structural formula (1), structural formula (2), or structural formula (3) that absorbs little visible light, so that the photoelectric conversion of the imaging element including the carrier blocking layer or the imaging element below it when viewed from the light incidence direction is not hindered, and good external quantum efficiency and spectral characteristics can be achieved at the same time. Moreover, the dark current can be suppressed, and the withstand voltage characteristics of the dark current can be improved. That is, the carrier blocking layer is considered to function as a carrier transport layer for the photocurrent, while functioning as a carrier blocking layer for the dark current. Furthermore, by setting the film thickness of the carrier blocking layer to 5 nm to 150 nm, preferably 5 nm to 100 nm, it is possible to reduce the electric capacitance, which was one of the problems of the conventional imaging element, and good spectral characteristics can be secured at the same time. As a result of the above, an imaging device capable of producing a beautiful image can be realized. EXAMPLES
[0081] Example 2 is a modification of Example 1. In Example 2, similarly to Example 1, a first carrier blocking layer 22 made of a material having structural formula (3) and having a thickness of 5 nm was formed on the first electrode 21 based on a vacuum deposition method using a shadow mask. Then, in a vacuum deposition apparatus, unlike Example 1, 2,9-dimethylquinacridone (see the structural formula below) and subphthalocyanine chloride (SubPc-Cl) were co-deposited at a deposition rate ratio of 1:1 to a thickness of 120 nm to form an organic photoelectric conversion layer 23. The organic photoelectric conversion layer 23 is composed of a mixed layer (bulk heterostructure) of a p-type organic semiconductor and an n-type organic semiconductor. Thereafter, an imaging element for evaluation of Example 2 was obtained in the same manner as Example 1. The cross-sectional structure of the imaging element for evaluation of Example 2 is the same as that shown in FIG. 2A.
[0082] 2,9-Dimethylquinacridone [ka]
[0083] Comparative Example 2B An imaging element of Comparative Example 2B was produced in the same manner as in Example 2, except that a first carrier blocking layer having a thickness of 5 nm was formed using the above-mentioned Compound-B.
[0084] Comparative Example 2C An imaging element of Comparative Example 2C was produced in the same manner as in Example 2, except that a first carrier blocking layer having a thickness of 5 nm was formed using the above-mentioned Compound-C.
[0085] <Comparative example 2D> An imaging element of Comparative Example 2D was produced in the same manner as in Example 2, except that a first carrier blocking layer having a thickness of 5 nm was formed using the following Compound-D.
[0086] <Compound-D> [ka]
[0087] In the imaging devices of Example 2, Comparative Example 2B, Comparative Example 2C, and Comparative Example 2D, a voltage of −3 volts (a so-called reverse bias voltage of 3 volts) was applied between the second electrode (cathode) 25 and the first electrode (anode) 21, and a wavelength of 560 nm and 2 microwatts / cm were applied. 2 The light was then irradiated at 100 nm, and then the light irradiation was stopped (specifically, the shutter was closed). The amount of current flowing between the second electrode and the first electrode immediately before the light irradiation was stopped was defined as I0, and the time from the cessation of light irradiation until the amount of current became (0.03×I0), i.e., the time until the value of I0 became 3%, was defined as T0. The value of T0 (unit: milliseconds) was measured. The results are shown in Table 5 below. In Table 5, the "afterimage ratio" is the relative value of T0 for each comparative example when the value of T0 for Example 2 was set to "1".
[0088] T0 afterimage ratio Example 2 8 1.0 Comparative Example 2B 28 3.4 Comparative Example 2C 27 3.3 Comparative example 2D 30 3.7
[0089] From Table 5, it was found that the image lag times of Comparative Example 2B, Comparative Example 2C, and Comparative Example 2D were three times or more longer than that of Example 2, and that excellent image lag characteristics could be obtained when a material having structural formula (3) was used in the first carrier blocking layer. In addition, as shown in Table 6, Example 2 also exhibited a superior external quantum efficiency (EQE) when a reverse bias voltage of 3 volts was applied. In other words, the material having structural formula (3) is a material that can improve image lag characteristics while maintaining sensitivity.
[0090] External quantum efficiency Example 2 57.0% Comparative Example 2B 56.7% Comparative Example 2C 54.7% Comparative example 2D 56.4%
[0091] Table 7 shows the external quantum efficiency (EQE) and T0 (unit: milliseconds) values when the thickness of the first carrier blocking layer made of the material having structural formula (3) is changed to 5 nm, 50 nm, and 100 nm. Table 7 shows that there is no significant change in the image lag time T0 when the thickness of the first carrier blocking layer is up to 100 nm, and that by using a material having structural formula (3) as the first carrier blocking layer, it is possible to ensure the desired electrical capacitance in addition to improving the image lag characteristics and quantum efficiency.
[0092] Thickness of the first carrier blocking layer in Example 1 EQE T0 5nm 69.6% 8 50nm 67.9% 4 100nm 69.7% 6
[0093] Furthermore, a test laminate structure was prepared in which a first carrier blocking layer made of a material having structural formula (3) with a thickness of 200 nm was formed between a first electrode (specifically, a first electrode having a laminate structure of platinum with a thickness of 100 nm / molybdenum oxide with a thickness of 0.8 nm) and a second electrode (specifically, a second electrode having a laminate structure of molybdenum oxide with a thickness of 3 nm / gold with a thickness of 100 nm). The carrier mobility (unit: × 10) was measured when a voltage of −1 volt to −10 volts (so-called reverse bias voltage of 1 volt to 10 volts) was applied between the second electrode (cathode) and the first electrode (anode). -2 cm 2 / V s) are shown in Table 8 below. The carrier mobility was independent of the reverse bias voltage value, and was approximately three orders of magnitude higher than those of aromatic amine-based materials and carbazole-based materials.
[0094] Reverse bias voltage Carrier mobility 1 volt 6.07 3V 6.23 5V 6.33 10V 6.53
[0095] In addition, a test laminate structure was prepared in which a first carrier blocking layer made of a material having structural formula (3) and an aromatic amine-based material and having a thickness of 200 nm was formed between a first electrode (specifically, a first electrode having a laminate structure of platinum having a thickness of 100 nm / molybdenum oxide having a thickness of 0.8 nm) and a second electrode (specifically, a second electrode having a laminate structure of molybdenum oxide having a thickness of 3 nm / gold having a thickness of 100 nm). The carrier mobility (unit: cm) was measured when a voltage of up to -1 volt (so-called reverse bias voltage of 1 volt) was applied between the second electrode (cathode) and the first electrode (anode). 2 / V s) and the T0 values (unit: milliseconds) for imagers using these materials as a 5-nm-thick first carrier blocking layer are shown in Table 9 below. Furthermore, the relationship between carrier mobility and T0 value is shown in Figure 6.
[0096] Carrier mobility T0 Structural formula (3) 6.07×10 -2 8 Aromatic amine material (A) 1.00×10 -6 28 Aromatic amine material (B) 7.43×10 -7 30 Aromatic amine material (C) 1.00×10 -5 27
[0097] From Table 9, it can be seen that the material having structural formula (3) exhibits carrier mobility three orders of magnitude higher than that of aromatic amine-based materials, and also has significantly better image retention properties. EXAMPLES
[0098] Example 3 is a modification of the imaging element of Examples 1 and 2, but relates to the stacked imaging element of the present disclosure and the imaging device according to the second aspect of the present disclosure. That is, the stacked imaging element of Example 3 (vertical spectroscopy imaging element) is formed by stacking at least two imaging elements described in Examples 1 and 2. Also, the imaging device of Example 3 includes a plurality of such stacked imaging elements. Specifically, as shown in the conceptual diagram of FIG. 7A, the stacked imaging element of Example 3 has a configuration in which three imaging elements (three sub-pixels), namely, a blue imaging element, a green imaging element, and a red imaging element described in Examples 1 and 2, are stacked in the vertical direction. That is, a stacked imaging element having a structure in which the sub-pixels are stacked to form one pixel can be obtained. The blue imaging element is located in the top layer, the green imaging element is located in the middle, and the red imaging element is located in the bottom layer. However, the stacking order is not limited to this.
[0099] Alternatively, as shown in the conceptual diagram of FIG. 7B, the imaging elements described in the first and second embodiments (in the illustrated example, the blue imaging element and the green imaging element) are provided on a silicon semiconductor substrate, and one or more imaging elements (in the illustrated example, the imaging element having sensitivity to red) are provided inside the silicon semiconductor substrate located below the imaging elements, thereby obtaining a stacked imaging element having a structure in which imaging elements are stacked, that is, a structure in which sub-pixels are stacked to form one pixel. The imaging element formed on the silicon semiconductor substrate is preferably a back-illuminated type, but may also be a front-illuminated type. Instead of providing a photoelectric conversion layer inside the silicon semiconductor substrate, the imaging element may be formed on a semiconductor substrate by epitaxial growth, or may be formed on a silicon layer in a so-called SOI structure.
[0100] In the stacked imaging element of Example 3, in order not to interfere with the light reception of the imaging element located below, the first electrode (anode) of the imaging element located above is made of a transparent conductive material such as ITO, and the second electrode (cathode) is also made of a transparent conductive material such as ITO.
[0101] In the imaging device of Example 3 equipped with a stacked imaging element, instead of using color filters to separate blue, green, and red light, imaging elements having sensitivity to light of a plurality of wavelengths are stacked in the direction of light incidence within the same pixel, so that it is possible to improve sensitivity and pixel density per unit volume. In addition, since organic materials have a high light absorption coefficient, the film thickness of the organic photoelectric conversion layer can be made thinner than that of a conventional Si-based photoelectric conversion layer, and light leakage from adjacent pixels and restrictions on the angle of incidence of light are alleviated. Furthermore, in the conventional Si-based imaging element, false colors occur because color signals are created by performing an interpolation process between three color pixels, but the occurrence of false colors is suppressed in the imaging device of Example 3 equipped with a stacked imaging element.
[0102] Although the present disclosure has been described above based on preferred embodiments, the present disclosure is not limited to these embodiments. The structures and configurations, manufacturing conditions, manufacturing methods, and materials used of the imaging element, stacked imaging element, and imaging device described in the embodiments are merely examples and may be changed as appropriate.
[0103] In terms of the external quantum efficiency and the thickness of the carrier blocking layer, the imaging element of the present disclosure is an imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, and the carrier blocking layer has a thickness of 5×10 -9 m to 1.0×10 -7 m, preferably 5 x 10 -8 m to 1.0×10 -7 m, wavelength 560 nm, 2 microwatts / cm 2 When a voltage of −2.6 volts (a so-called reverse bias voltage of 2.6 volts) is applied between the second electrode (cathode) and the first electrode (anode) while irradiating the device with light, the external quantum efficiency is 0.6 or more.
[0104] Alternatively, when expressing an imaging element from the viewpoint of dark current and the thickness of a carrier blocking layer, the imaging element of the present disclosure is an imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, and the carrier blocking layer has a thickness of 5×10 -9 m to 1.0×10 -7 m, preferably 5 x 10 -8 m to 1.0×10 -7 m, and the value of the dark current when a voltage of −1 V to −10 V (a so-called reverse bias voltage of 1 V to 10 V) is applied between the second electrode (cathode) and the first electrode (anode) is 2.5×10 -10 Ampere / cm 2 The following is the result.
[0105] Alternatively, when expressing an imaging element from the viewpoint of afterimage characteristics and the thickness of a carrier blocking layer, the imaging element of the present disclosure is an imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, and the carrier blocking layer has a thickness of 5×10-9 m to 1.0×10 -7 m, preferably 5 x 10 -8 m to 1.0×10 -7 m, and a wavelength of 560 nm and 2 microwatts / cm were used while applying -3 volts (a so-called reverse bias voltage of 3 volts) between the second electrode and the first electrode. 2 When light irradiation is stopped, the amount of current flowing between the second electrode and the first electrode just before the light irradiation is stopped is I0, and the time from the stop of light irradiation to the amount of current becoming (0.03×I0) is T0, T0 is 10 milliseconds or less.
[0106] Alternatively, when expressing the imaging element from the viewpoint of the light absorption ratio and the thickness of the carrier blocking layer, the imaging element of the present disclosure is an imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, and the carrier blocking layer has a thickness of 5×10 -9 m to 1.0×10 -7 m, preferably 5 x 10 -8 m to 1.0×10 -7 m, and the light absorption rate of the carrier blocking layer is 3% or less at a wavelength of 450 nm, 30% or less at a wavelength of 425 nm, and 80% or less at a wavelength of 400 nm.
[0107] Alternatively, when expressing an imaging element from the viewpoint of carrier mobility and the thickness of a carrier blocking layer, the imaging element of the present disclosure is an imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, and the carrier blocking layer has a thickness of 5×10 -9 m to 1.0×10 -7 m, preferably 5 x 10 -8 m to 1.0×10 -7 m, and the carrier mobility of the material that constitutes the carrier blocking layer is 9 × 10 -4 cm 2 / V s or more, preferably 9×10 -3 cm 2 / V s or more, preferably 6×10 -2 cm 2 / V s or more.
[0108] The present disclosure may also be configured as follows. [A01] Imaging element: First aspect An imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, The carrier blocking layer is made of a material having the following structural formula (1) and has a thickness of 5×10 -9 m to 1.5×10 -7 m, preferably 5 x 10 -9 m to 1.0×10 -7 m imaging element. [ka] Where: R1 and R2 are each independently a group selected from hydrogen, an aryl group, and an alkyl group, and the aryl group is a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, a naphthylphenyl group, a tolyl group, a xylyl group, a phenyl group substituted with an alkyl group having 2 to 6 carbon atoms, an anthracenyl group, an anthracenylphenyl group, a phenanthryl group, a phenanthrylphenyl group, a pyrenyl group, a pyrenylphenyl group, a tetracenyl group, a tetracenylphenyl group, a fluoranthenyl group, a fluoranthenylphenyl group, a pyridinyl group, a pyridylphenyl group, a fluoranthenylphenyl group, a pyrid ... and the alkyl group is a group selected from the group consisting of a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and may be a linear alkyl group or a branched alkyl group. [A02] Imaging element: second aspect An imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, The carrier blocking layer is made of a material having the following structural formula (2) and has a thickness of 5×10-9 m to 1.5×10 -7 m, preferably 5 x 10 -9 m to 1.0×10 -7 m imaging element. [ka] Here, Ar1 and Ar2 are each independently an aryl group which may have a substituent, and are selected from the group consisting of a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, a naphthylphenyl group, a tolyl group, a xylyl group, a phenyl group substituted with an alkyl group having 2 to 6 carbon atoms, an anthracenyl group, an anthracenylphenyl group, a phenanthryl group, a phenanthrylphenyl group, a pyrenyl group, a pyrenylphenyl group, a tetracenyl group, a tetracenylphenyl group, a fluoranthenyl group, a fluoranthenylphenyl group, a pyridinyl group, a pyridinylphenyl group, a quinolinyl group, a quinolinylphenyl group, an acridinyl group, an acridinylphenyl group, an indole group, an indolylphenyl group, an imidazole group, an imidazolylphenyl group, a benzimidazole group, a benzimidazolylphenyl group, a thienyl group, and a thienylphenyl group. [A03] 《Imaging element: third aspect》 An imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, The carrier blocking layer is made of a material having the following structural formula (3) and has a thickness of 5×10 -9 m to 1.5×10 -7 m, preferably 5 x 10 -9 m to 1.0×10 -7 m imaging element. [ka] [A04] An imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, The carrier blocking layer has a thickness of 5×10 -9 m to 1.0×10 -7 m, preferably 5 x 10 -8m to 1.0×10 -7 m, Wavelength 560nm, 2 microwatts / cm 2 An imaging element having an external quantum efficiency of 0.6 or more when a voltage of -2.6 volts is applied between the second electrode (cathode) and the first electrode (anode) while being irradiated with light. [A05] An imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, The carrier blocking layer is 5×10 -9 m to 1.0×10 -7 m, preferably 5 x 10 -8 m to 1.0×10 -7 m, The value of the dark current when a voltage of -1 V to -10 V is applied between the second electrode (cathode) and the first electrode (anode) is 2.5 × 10 -10 Ampere / cm 2 The imaging element is as follows. [A06] An imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, The carrier blocking layer is 5×10 -9 m to 1.0×10 -7 m, preferably 5 x 10 -8 m to 1.0×10 -7 m, A wavelength of 560 nm and 2 microwatts / cm were used while applying -3 volts between the second and first electrodes. 2 an imaging element in which, when light irradiation is irradiated to the second electrode and the first electrode and then the light irradiation is stopped, the amount of current flowing between the second electrode and the first electrode just before the light irradiation is stopped is I0, and the time from the stop of light irradiation to the time when the amount of current becomes (0.03 x I0) is T0, T0 is 10 milliseconds or less. [A07] An imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, The carrier blocking layer is 5×10 -9 m to 1.0×10 -7 m, preferably 5 x 10 -8m to 1.0×10 -7 m, An imaging element in which the light absorption rate of the carrier blocking layer is 3% or less at a wavelength of 450 nm, 30% or less at a wavelength of 425 nm, and 80% or less at a wavelength of 400 nm. [A08] An imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, The carrier blocking layer is 5×10 -9 m to 1.0×10 -7 m, preferably 5 x 10 -8 m to 1.0×10 -7 m, The carrier mobility of the material that constitutes the carrier blocking layer is 9×10 -4 cm 2 / V s or more, preferably 9×10 -3 cm 2 / V s or more, preferably 6×10 -2 cm 2 / V s or higher. [A09] The first electrode constitutes an anode and the second electrode constitutes a cathode; The imaging element according to any one of [A01] to [A08], wherein the carrier blocking layer is provided between the first electrode and the organic photoelectric conversion layer. [A10] The imaging element according to any one of [A01] to [A09], wherein the light absorption rate of the carrier blocking layer is 3% or less at a wavelength of 450 nm, 30% or less at a wavelength of 425 nm, and 80% or less at a wavelength of 400 nm. [A11] The carrier mobility of the material that constitutes the carrier blocking layer is 9×10 -4 cm 2 / V s or more, preferably 9×10 -3 cm 2 / V s or more, preferably 6×10 -2 cm 2 The imaging element according to any one of [A01] to [A10], wherein the refractive index is 1.0 / V·s or more. [A12] Apply -3 volts between the second electrode and the first electrode, and use a wavelength of 560 nm and 2 microwatts / cm2 The imaging element according to any one of [A01] to [A11], wherein when light irradiation is irradiated to the second electrode and the first electrode and then the light irradiation is stopped, the amount of current flowing between the second electrode and the first electrode just before the light irradiation is stopped is I0, and the time from the stop of light irradiation to the time when the amount of current becomes (0.03×I0) is T0, T0 is 10 milliseconds or less. [A13] The imaging element according to any one of [A01] to [A12], wherein the first electrode and the second electrode are made of a transparent conductive material. [A14] The imaging element according to any one of [A01] to [A12], wherein one of the first electrode and the second electrode is made of a transparent conductive material, and the other is made of a metal material. [A15] The imaging element according to [A14], wherein the first electrode is made of a transparent conductive material, and the second electrode is made of Al, Al-Si-Cu, or Mg-Ag. [A16] The imaging element according to [A14], wherein the second electrode is made of a transparent conductive material, and the first electrode is made of Al-Nd or ASC. [B01] 《Stacked image sensor》 A stacked type imaging element comprising at least two imaging elements according to any one of [A01] to [A16] stacked together. [C01] Imaging device: First aspect An imaging device comprising a plurality of imaging elements according to any one of [A01] to [A16]. [C02] Imaging device: second aspect An imaging device comprising a plurality of the stacked imaging elements according to [B01]. [Explanation of symbols]
[0109] REFERENCE SIGNS LIST 11 imaging element, 20 substrate, 21 first electrode (anode), 22 carrier blocking layer (first carrier blocking layer), 23 organic photoelectric conversion layer, 24 second carrier blocking layer, 25 second electrode (cathode), 31 insulating layer, 40 imaging device, 41 imaging area, 42 vertical drive circuit, 43 column signal processing circuit, 44 horizontal drive circuit, 45 output circuit, 46 control circuit, 47 vertical signal line, 48 horizontal signal line
Claims
1. An imaging element including at least a first electrode, a second electrode, an organic photoelectric conversion layer, and a carrier blocking layer, The carrier blocking layer is made of a material having the structural formula (3) shown in Chemical Formula 1 below, and has a thickness of 5×10 -9 m to 1.5×10 -7 m, The organic photoelectric conversion layer absorbs at least light having a wavelength of 495 nm to 570 nm, and the organic photoelectric conversion layer includes at least a p-type organic semiconductor and an n-type organic semiconductor, and is formed by co-depositing quinacridone (QD) shown in Chemical formula 2 below and subphthalocyanine chloride (SubPc-Cl) shown in Chemical formula 3 below at a deposition rate ratio of 1:1, or by co-depositing 2,9-dimethylquinacridone shown in Chemical formula 4 below and subphthalocyanine chloride (SubPc-Cl) shown in Chemical formula 3 below at a deposition rate ratio of 1:1, When the thickness of the carrier blocking layer is converted to 150 nm, the light absorption rate of the carrier blocking layer is 3% or less at a wavelength of 450 nm, 30% or less at a wavelength of 425 nm, and 80% or less at a wavelength of 400 nm. Image sensor. 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】
2. The first electrode constitutes an anode and the second electrode constitutes a cathode; The image sensor according to claim 1 , wherein the carrier blocking layer is provided between the first electrode and the organic photoelectric conversion layer.
3. 3. The image sensor according to claim 1, wherein the first electrode and the second electrode are made of a transparent conductive material.
4. 3. The image sensor according to claim 1, wherein one of the first electrode and the second electrode is made of a transparent conductive material, and the other is made of a metal material.
5. 5. The image sensor according to claim 4, wherein the first electrode is made of a transparent conductive material, and the second electrode is made of Al, Al--Si--Cu, or Mg--Ag.
6. 5. The image sensor according to claim 4, wherein the second electrode is made of a transparent conductive material, and the first electrode is made of Al--Nd or ASC.
7. 7. A stacked type imaging element comprising at least two imaging elements according to claim 1 stacked together.
8. An imaging device comprising a plurality of the imaging elements according to claim 1 .
9. An imaging device comprising a plurality of the stack-type imaging elements according to claim 7.
10. 3. The image sensor according to claim 1, wherein the organic photoelectric conversion layer is a mixed layer of a p-type semiconductor and an n-type semiconductor.
Citation Information
Patent Citations
Image sensor made of organic semiconductor
JP2002502120A
Radiation imaging element
JP2009032854A
Vertical organic semiconductor device
JP2010232413A
Photoelectric conversion device and imaging device
JP2011176259A
Photoelectric conversion element, photoelectric conversion apparatus and solid-state imaging apparatus
JP2011192966A