Polymer compositions containing basic additives, methods and articles containing said polymer compositions - Patents.com

Incorporating a basic additive with specific pH into polymer compositions enhances biodegradability, addressing environmental pollution by increasing the degradation rate of polymeric materials.

JP7586864B2Active Publication Date: 2024-11-19SOLVAY ACETOW GMBH(DE)
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022128105
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2014-12-11
Filing Date
2022-08-10
Publication Date
2024-11-19
Estimated Expiration
2035-12-10

AI Technical Summary

Technical Problem

Polymeric compositions, such as packaging materials and cigarette filters, have short life cycles and contribute to environmental pollution due to improper disposal, necessitating improved biodegradability to reduce their residence time in the environment.

Method used

Incorporating a basic additive with a pH of 7 to 13 in a 1% solution in water at 20°C into polymer compositions, which enhances biodegradability by creating a suitable habitat for degrading microorganisms and providing a slow, stable release of the additive.

Benefits of technology

The polymer compositions exhibit improved biodegradability, with increased weight loss in soil burial tests and aquatic aerobic biodegradation, up to 15% and 4 times higher than compositions without additives, respectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586864000001
    Figure 0007586864000001
  • Figure 0007586864000002
    Figure 0007586864000002
Patent Text Reader

Abstract

Fibers and methods for their manufacture are provided that include polymer compositions that exhibit enhanced biodegradability. The present invention provides a fiber comprising a polymer composition including at least one polymer and at least one basic additive, wherein the at least one basic additive has a pH of 13 or less and 7 or more when measured in a 1 wt % solution in water at 20° C. Preferably, at least one polymer in the polymer composition is selected from the group consisting of polysaccharide esters.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to European Patent Application No. 14197348.7, the entire contents of which are incorporated herein by reference for all purposes.

[0002] The present invention relates to a polymer composition comprising at least one basic additive and to a method comprising at least one process step for obtaining the polymer composition or an article comprising the polymer composition.

[0003] The articles comprising the polymer composition are present everywhere at the same time. In many cases, the articles comprising the polymer composition, such as packaging materials, binders and cigar filters, have a short life cycle and are discarded after use. Environmental pollution due to improper disposal has become a problem. It is desirable to provide the polymer composition with improved biodegradability in order to shorten the residence time of the polymer contaminants in the environment. It is further desirable to shorten the residence time of the polymer contaminants in landfills by increasing the biodegradability of the polymer composition.

[0004] WO 9410238 discloses a method for enhancing the biodegradability of cellulose esters by contacting the cellulose esters with certain basic hydrolysis enhancing agents.

[0005] It has been found that polymer compositions containing at least one basic additive, where the at least one basic additive has a pH of 13 or less and 7 or more when measured in a 1% by weight solution in water at 20°C, exhibit improved biodegradability over compositions that do not contain the at least one additive. This effect is particularly advantageous for polymer compositions containing a low solubility basic additive. The at least one additive creates a suitable habitat for the decomposition microorganisms rather than acting as a hydrolysis promoter; the low solubility is believed to be advantageous because the additive slowly leaches out of the polymer composition, thereby avoiding overly basic conditions that are potentially harmful to the decomposition microorganisms. Furthermore, the slow leaching of the low solubility basic additive provides a longer, steady release of the additive; therefore, the effect can be maintained for a long period of time.

[0006] The present invention therefore relates to a polymer composition comprising at least one polymer and at least one basic additive, the at least one basic additive having a pH of less than or equal to 13 and more than or equal to 7, measured in a 1% by weight solution in water at 20° C. The polymer composition generally exhibits improved biodegradability compared to a polymer composition not comprising the at least one additive. The additive is therefore an additive which enhances the biodegradability of the polymer composition. The polymer composition may further comprise at least one inhibitor of the autocondensation reaction (often occurring under acid or base catalysis) which takes place in a solvent having at least one carbonyl functional group and a C-H bond in the α-position of said carbonyl functional group. Another aspect of the present invention is a method for the manufacture of a polymer composition according to the invention or of an article comprising a polymer composition according to the invention, comprising at least one step: a) contacting at least one basic additive and optionally at least one inhibitor with at least one polymer in a liquid phase comprising at least one solvent, followed by separation of the at least one solvent to obtain a polymer composition according to the invention; b) contacting at least one basic additive and optionally at least one inhibitor with at least one polymer in a liquid phase comprising at least one solvent, and then spinning the resulting mixture to obtain a fiber comprising the polymer composition; c) contacting at least one basic additive and optionally at least one inhibitor with at least one polymer in a liquid phase comprising at least one solvent, followed by applying a film casting method to obtain a film comprising the polymer composition; d) contacting at least one basic additive with at least one polymer, at least a portion of which is in a molten state, and optionally cooling the mixture to obtain a polymer composition according to the invention; e) contacting at least one basic additive with at least one polymer, at least a part of which is in the molten state, and then extruding and / or film-blowing the mixture obtained to obtain molded parts, fibers, films, deep drawn films, injection molded articles, thick-walled molded parts, in particular flower pots, granules, microbeads, beads or containers comprising the polymer composition. The present invention relates to a method comprising at least one step selected from the group of steps consisting of:

[0007] In another aspect, the present invention relates to a filter tow comprising the polymer composition of the present invention or a filter tow comprising fibers produced by a process comprising at least one step b) according to the process described above.

[0008] At least one polymer contained in the polymer composition according to the invention is a biodegradable polymer. In many cases, the at least one polymer is a biopolymer. In particular, the at least one polymer is a polysaccharide, preferably a polymer based on cellulose or starch. Preferably, the at least one polymer is an ester of a polysaccharide. More preferably, the at least one polymer is a cellulose ester selected from the group consisting of cellulose acetate, cellulose propionate, cellulose butyrate, cellulose acetate propionate and cellulose acetate butyrate. Cellulose acetate is most preferred. The average degree of substitution (DS) of the cellulose ester is 1.5 to 3.0, in particular 2.2 to 2.7, which is especially the case for cellulose acetate. The optimal average degree of polymerization for the cellulose ester is 150 to 500, in particular 180 to 280. In another embodiment, the at least one polymer is selected from the group consisting of polylactic acid, polycaprolactone and polyhydroxybutyric acid.

[0009] According to the invention, "basic additive" is intended to mean an additive having a pH of 13 or less and 7 or more, measured in a 1% by weight solution in water at 20°C. Generally, basic additives have a pH of 13 or less, measured in a 1% by weight solution in water at 20°C; preferably a pH of 12 or less, measured in a 1% by weight solution in water at 20°C, most preferably a pH of 11 or less, measured in a 1% by weight solution in water at 20°C. Generally, basic additives have a pH of 7 or more, measured in a 1% by weight solution in water at 20°C; preferably a pH of 7.8 or more, measured in a 1% by weight solution in water at 20°C; most preferably a pH of 8.5 or more, measured in a 1% by weight solution in water at 20°C. Basic additives with a pH of 8.5 to 11, measured in a 1% by weight solution in water at 20°C, are particularly advantageous. The pH is measured according to standard procedures, for example with a glass pH electrode.

[0010] In general, the at least one basic additive is selected from the group consisting of alkaline earth metal oxides, alkaline earth metal hydroxides, alkaline earth metal carbonates, alkali metal carbonates, alkali metal bicarbonates, ZnO and basic Al2O3. Preferably, the at least one basic additive is selected from the group consisting of MgO, Mg(OH)2, MgCO3, CaO, Ca(OH)2, CaCO3, NaHCO3, Na2CO3, K2CO3, ZnO KHCO3 and basic Al2O3. In another preferred embodiment, the at least one basic additive is selected from the group consisting of MgO, Mg(OH)2, MgCO3, CaO, Ca(OH)2, NaHCO3, K2CO3, ZnO, KHCO3 and basic Al2O3. More preferably, the at least one basic additive is selected from the group consisting of MgO, Mg(OH)2, CaO, Ca(OH)2, ZnO and basic Al2O3. In one embodiment, alkaline earth metal oxides, ZnO and basic Al2O3 are particularly preferred as basic additives; therefore, the at least one basic additive is more preferably selected from the group consisting of MgO, ZnO, CaO and Al2O3, even more preferably from the group consisting of MgO, CaO and ZnO. MgO is the most preferred basic additive.

[0011] In most cases, at least one basic additive has a pH of 10 at 20°C. -5 ~70 g / 100 mL water solubility. Generally, at least one basic additive has a solubility of 10 -6 g / 100 mL of water. Preferably, at least one basic additive has a solubility of 10 -5 Most preferably, the at least one basic additive has a solubility of 10 g / 100 mL water at 20° C. -4Generally, the at least one basic additive has a solubility of 70 g or less / 100 mL water at 20° C. Preferably, the at least one basic additive has a solubility of 10 g or less / 100 mL water at 20° C. More preferably, the at least one basic additive has a solubility of 1 g or less / 100 mL water at 20° C. Most preferably, the at least one basic additive has a solubility of 0.1 g or less / 100 mL water at 20° C. In water, the at least one basic additive has a solubility of about 10 g or less / 100 mL water. -4 Examples of additives with a solubility of about 10 g / 100 mL (20°C) are MgO, ZnO and Mg(OH)2. -2 An example of an additive with a solubility of about 0.1 g / 100 mL (20° C.) in water is MgCO3. Examples of additives with a solubility of about 0.1 g / 100 mL (20° C.) in water are CaO and Ca(OH)2.

[0012] In another embodiment, the at least one basic additive is often selected from the group consisting of K2CO3 and basic Al2O3.

[0013] Generally, the at least one basic additive is present in the polymer composition in the form of finely distributed particles.

[0014] In one embodiment of the present invention, the at least one basic additive is present in the polymer composition in the form of finely distributed particles with a D90 particle size of 10 μm or less. More preferably, the finely distributed basic additive has a D90 particle size of 5 μm or less. More preferably, the finely distributed basic additive has a D90 particle size of 3 μm or less. A particle size of 2 μm or less is most preferred. In general, the lower limit of the D90 particle size of the at least one basic additive is not critical for the present invention. Particles of the stated particle size can be obtained by procedures known to the skilled person, for example by wet or dry grinding in a mill, for example a ball mill or a bead mill such as the WAB Dyno® Mill Multi Lab. The particles may also be obtained by grinding the additive in the presence of other additives, such as pigments, fillers or colorants. The D90 particle size can preferably be measured by laser diffraction, for example using a laser diffraction sensor such as the Helos® BR.

[0015] In one embodiment of the present invention, the at least one basic additive is present in the polymer composition in the form of finely distributed particles in an amount of 0.01 to 40% by weight. The term "wt.%" relates to the weight of the total polymer composition, including other additives such as pigments, fillers or colorants. In many cases, the at least one basic additive is present in the polymer composition in the form of finely distributed particles in an amount of 0.01% by weight or more. Preferably, the at least one basic additive is present in the polymer composition in the form of finely distributed particles in an amount of 0.05% by weight or more. Most preferably, the at least one basic additive is present in the polymer composition in the form of finely distributed particles in an amount of 0.1% by weight or more. In many cases, the at least one basic additive is present in the polymer composition in the form of finely distributed particles in an amount of 40% by weight or less. Preferably, the at least one basic additive is present in the polymer composition in the form of finely distributed particles in an amount of 30% by weight or less. More preferably, the at least one basic additive is present in the polymer composition in the form of finely distributed particles in an amount of 20% by weight or less. Even more preferably, the at least one basic additive is present in the polymer composition in the form of finely distributed particles in an amount of not more than 10% by weight. Most preferably, the at least one basic additive is present in the polymer composition in the form of finely distributed particles in an amount of not more than 8% by weight.

[0016] In one embodiment of the present invention, the polymer composition comprises, in addition to at least one additive, at least one inhibitor of the autocondensation reaction that occurs in a solvent having at least one carbonyl functional group and a C-H bond in the α-position of said carbonyl functional group. It has been observed that the beneficial effect of at least one basic additive on the improved biodegradability may involve the catalytic effect of at least one basic additive on a solvent having at least one carbonyl functional group and a C-H bond in the α-position of said carbonyl functional group that may undergo autocondensation in the presence of at least one basic additive that may be present in the further processing of the polymer composition. Autocondensation can be observed, for example, in a filter tow spinning process, where a polymer composition containing at least one basic additive is processed in the presence of acetone. Autocondensation products, such as diacetone alcohol from acetone, should advantageously be avoided in the processing of the polymer composition. Solvents often present in the processing of polymer compositions are solvents with at least one carbonyl functional group and a C-H bond in the α-position of said carbonyl functional group, such as ketones, more particularly C3-C6 ketones, most particularly acetone. Preferably, the at least one inhibitor is selected from the group consisting of carboxylic acids and alcohols. More preferably, the inhibitor is selected from the group consisting of citric acid, lactic acid, malic acid, tartaric acid and glycerol. Citric acid is the most preferred inhibitor. In one embodiment, the at least one inhibitor is present in the polymer composition in an amount of 0.001-10 wt. %. Generally, the at least one inhibitor is present in the polymer composition in an amount of 0.001 wt. % or more. The term "wt. %" relates to the weight of the total polymer composition. Preferably, the at least one inhibitor is present in the polymer composition in an amount of 0.01 wt. % or more. Most preferably, the at least one inhibitor is present in the polymer composition in an amount of 0.1 wt. % or more. Generally, the at least one inhibitor is present in the polymer composition in an amount of 10 wt. % or less. Preferably, the at least one inhibitor is present in the polymer composition in an amount of 5 wt% or less. More preferably, the at least one inhibitor is present in the polymer composition in an amount of 1 wt% or less. An inhibitor amount of 0.5 wt% or less is most preferred.In one embodiment, the at least one inhibitor is present in the polymer composition in the form of finely distributed particles with a D90 particle size of 10 μm or less. More preferably, the finely distributed inhibitor has a D90 particle size of 5 μm or less. More preferably, the finely distributed inhibitor has a D90 particle size of 3 μm or less. A particle size of 2 μm or less is most preferred. In general, the lower limit of the D90 particle size of the at least one inhibitor is not critical for the present invention. Particles of the appropriate size can be obtained by procedures known to the skilled artisan, for example by wet or dry grinding in a mill, for example a bead mill such as the WAB Dyno® Mill Multi Lab. The particles may also be obtained by grinding the inhibitor in the presence of other additives, such as at least one basic additive, pigment or colorant. The D90 particle size of the at least one inhibitor can preferably be measured by laser diffraction, for example by using a laser diffraction sensor such as the Helos® BR.

[0017] The particle size of any other additives, such as pigments or colorants, should be in the same range as the inhibitor and / or base additive. The 90 particle size of any other additives is preferably measured by laser diffraction as described above.

[0018] In another embodiment, the at least one inhibitor is present in a polymer composition mixture that includes at least one solvent in solution. The at least one inhibitor often precipitates when the solvent is removed and is then present in the polymer composition in the form of finely divided particles, also referred to as "domains" or "phases."

[0019] In yet another embodiment, the at least one inhibitor is a material that is soluble in the polymer composition mixture and / or the polymer composition that includes at least one solvent.

[0020] Polymer compositions containing at least one basic additive generally exhibit improved biodegradability. In one embodiment, the term "improved biodegradability" is intended to mean biodegradability evaluated by measuring the resistance of cellulose-containing textiles to microorganisms according to the procedure of DIN specification EN ISO11721-1. When evaluated according to DIN specification EN ISO11721-1, "improved biodegradability" means an increase in the average weight loss of the polymer composition in a soil burial test after 2 months of 10% absolute or more, preferably 13% absolute or more, most preferably 15% absolute or more, compared to the biodegradability of the polymer composition without basic additive. In another embodiment, the term "improved biodegradability" is intended to mean biodegradability evaluated by measuring the aquatic aerobic biodegradability by O2 consumption according to the procedure of specification ISO 14851. "Improved biodegradability" means an increased biodegradation as measured by the O2 consumption of the polymer composition after 28 days of aquatic aerobic biodegradation that is at least 2 times higher, preferably at least 3 times higher, most preferably at least 4 times higher than the biodegradability of the polymer composition without the basic additive, when evaluated according to specification ISO 14851. The polymer compositions according to the invention generally exhibit improved biodegradability compared to polymer compositions not comprising the basic additive according to the invention.

[0021] Another embodiment of the present invention is a method for producing a polymer composition comprising at least one basic additive and optionally an inhibitor, or an article comprising such a polymer composition, comprising at least one step: a) contacting at least one basic additive and optionally at least one inhibitor with at least one polymer in a liquid phase comprising at least one solvent, followed by separation of the at least one solvent to obtain a polymer composition according to the invention; b) contacting at least one basic additive and optionally at least one inhibitor with at least one polymer in a liquid phase comprising at least one solvent, and then spinning the resulting mixture to obtain a fiber comprising the polymer composition; c) contacting at least one basic additive and optionally at least one inhibitor with at least one polymer in a liquid phase comprising at least one solvent, and wherein the resulting mixture is then processed in a film-making process, preferably a film casting process, to obtain a film comprising the polymer composition; d) contacting at least one basic additive with at least one polymer, at least a portion of which is in a molten state, and optionally cooling the mixture to obtain a polymer composition according to the invention; and e) contacting at least one basic additive with at least one polymer, at least a portion of which is in a molten state, and then extruding and / or film-blowing the mixture to obtain a molded part, fiber, film, deep drawn film, injection molded part, thick-walled molded part, granules, microbeads, beads, containers or flower pots comprising the polymer composition. The present invention relates to a method comprising at least one step selected from the group of steps consisting of:

[0022] One embodiment of the present invention relates to a method for the preparation of a polymer composition comprising at least one basic additive and optionally at least one inhibitor, or a method for the preparation of an article comprising such a polymer composition, the method comprising one step in which at least one basic additive and optionally at least one inhibitor are contacted with at least one polymer in a liquid phase comprising at least one solvent, followed by separation of the at least one solvent to obtain a polymer composition according to the invention. In one aspect, the at least one solvent is a solvent having at least one carbonyl functional group and a C-H bond in the α-position of said carbonyl functional group. Often, the at least one solvent is a ketone, more particularly a C3-C6 ketone, most particularly acetone. In one aspect of this embodiment, the at least one polymer is dissolved in the at least one solvent, preferably at a temperature between 10 and 60° C., and the at least one inhibitor and optionally at least one inhibitor are added. In another aspect of the invention, the at least one solvent is selected from the group consisting of ethers, alcohols and carboxylic acid esters, such as ethyl acetate, isopropanol, ethyl alcohol and ether ethers. In the absence of any solvent having at least one carbonyl functional group and a C-H bond at the α-position of said carbonyl functional group, the optional inhibitor is generally absent. In a preferred aspect of this embodiment, 5-90 parts by weight of a polymer, preferably cellulose acetate, is dissolved in 10-95 parts by weight of a solvent, preferably acetone, and the mixture is then contacted with 0.01-40% by weight of a basic additive, where "% by weight" relates to the weight of the polymer and additive. When the polymer is a cellulose ester, particularly cellulose acetate, it is preferred that the cellulose ester has a DS of 1.5-3.0, especially 2.2-2.7. Optionally, the mixture is further contacted with 0.001-10% by weight of an inhibitor, where "% by weight" relates to the combined weight of the polymer, inhibitor and basic additive. In another aspect, the mixture can be further contacted with other ingredients, such as pigments and colorants. A preferred pigment that can be present is TiO2.In general, the basic additive can be treated by wet or dry milling, preferably wet milling, in the presence of at least one solvent and optionally in the presence of other additives, such as inhibitors and / or pigments and / or colorants, before being contacted with the polymer in the solvent. Often, the milling is carried out in a ball mill. In another embodiment, the basic additive is ground in the presence of the polymer, optionally in the presence of at least one inhibitor, pigment and / or colorant, preferably in a wet milling procedure. This makes it possible to avoid re-agglomeration of the basic additive. The mixture of at least one polymer, at least one solvent, at least one basic additive, optionally at least one inhibitor, colorant, pigment and other additives is then subjected to a step of separating the solvent to obtain the polymer composition according to the invention. The step of separating the solvent is often carried out by applying at least one procedure selected from the group consisting of heating, applying a vacuum and applying an air flow to the mixture.

[0023] Another embodiment of the present invention relates to a method for producing a polymer composition comprising at least one basic additive and optionally at least one inhibitor, or a method for producing an article comprising such a polymer composition, the method comprising one step in which at least one basic additive and optionally at least one inhibitor are contacted with at least one polymer in a liquid phase comprising at least one solvent, and then the resulting mixture is spun to obtain a fiber comprising the polymer composition. The preferred conditions for obtaining a mixture comprising at least one polymer, at least one basic additive and other optional additives and at least one solvent are shown in the previous embodiment. The mixture is then subjected to a spinning process, preferably a dry spinning process, to obtain a fiber comprising the polymer composition according to the present invention. Details of the dry spinning process are known to those skilled in the art and are described, for example, in "Bio-Based Polymer: Materials and Applications", S. Kabasci (Ed.), p. 49ff, Wiley 2014, and "Cellulose Acetates: Properties and Applications", Macromolecular Symposia, Volume 208, Issue 1, p. 267-292, Wiley, 2004. Both references are hereby incorporated by reference in their entirety.

[0024] A further embodiment of the present invention relates to a method for the preparation of a polymer composition comprising at least one basic additive and optionally at least one inhibitor, or a method for the preparation of an article comprising such a polymer composition, the method comprising one step in which at least one basic additive and optionally at least one inhibitor are contacted with at least one polymer in a liquid phase comprising at least one solvent, and the resulting mixture is then processed in a film-making process, preferably a film-casting process, to obtain a film comprising the polymer composition. In one aspect, the at least one solvent is a solvent having at least one carbonyl functional group and a C-H bond in the α-position of said carbonyl functional group. Often, the at least one solvent is a ketone, more particularly a C3-C6 ketone, most particularly acetone. In one aspect of this embodiment, at least one polymer is dissolved in at least one solvent, preferably at a temperature between 10 and 60° C., and at least one basic additive and optionally at least one inhibitor are added. In another aspect of the invention, the at least one solvent is selected from the group consisting of ethers, alcohols and carboxylic acid esters, such as ethyl acetate, isopropanol, ethyl alcohol and ether ethers. In the absence of any solvent having at least one carbonyl functional group and a C-H bond in the α-position of said carbonyl functional group, the optional inhibitor is generally not present. The resulting mixture is subjected to a film casting procedure to obtain a film comprising the polymer composition. In a preferred aspect of this embodiment, 5-30 parts by weight of a polymer, preferably cellulose acetate, is dissolved in 70-95 parts by weight of a solvent, preferably acetone, and the solution is then contacted with 0.01-40% by weight of a basic additive, where "% by weight" relates to the weight of the polymer and additive. When the polymer is a cellulose ester, especially cellulose acetate, the cellulose ester preferably has a DS of 1.5-3.0, especially 2.2-2.7. Optionally, the mixture is further contacted with 0.001 to 10 weight percent of an inhibitor, where "weight percent" relates to the combined weight of the polymer, inhibitor and basic additive.In another embodiment, the mixture can be further contacted with at least one other component, which can be selected, for example, from the group including plasticizers, pigments and colorants. A preferred pigment that can be present is TiO2. In general, the basic additive can be processed by wet or dry milling, preferably wet milling, in the presence of at least one solvent and optionally in the presence of other additives, such as inhibitors and / or plasticizers and / or pigments and / or colorants, before being contacted with the polymer in a solvent. In many cases, milling is carried out in a ball mill. In another embodiment, the basic additive is ground in a wet or dry grinding procedure, preferably a wet milling procedure, in the presence of the polymer, optionally in the presence of at least one inhibitor, pigment and / or colorant. This can avoid re-agglomeration of the basic additive. Technical details of various casting procedures are known to those skilled in the art and can be applied to the film casting method according to the present invention, for example, in "Industrial Plastics: Theory and Applications", E. Lokensgard, 5th Ed., 2010, Delmar, which reference is hereby incorporated by reference in its entirety.

[0025] A further embodiment of the present invention relates to a method for the preparation of a polymer composition comprising at least one basic additive or an article comprising such a polymer composition, the method comprising one step in which at least one basic additive is contacted with at least one polymer, at least a part of which is in a molten state, and optionally cooling the mixture to obtain a polymer composition according to the present invention. In one aspect of the present invention, wet grinding of at least one basic additive and optionally an inhibitor and other optional additives is first carried out in a water-free solvent in a ball mill. The first part of the polymer can be present throughout the grinding. The polymer part then increases slightly and the suspension is dried, for example, in a roller dryer or spray dryer. If the polymer is poorly soluble in common solvents, such as acetone, ethyl acetate, butyl acetate, etc., the solids to be ground can be ground, for example, in acetone and stabilized with 1-5% cellulose acetate to obtain a dope mixture containing the basic additive. In another embodiment, at least one basic additive is dry milled with a portion of a polymer, optionally in a portion containing a different polymer, and further optionally in the presence of another additive, such as an anti-agglomeration additive, to obtain a dope mixture containing the basic additive. In yet another embodiment, the basic additive is milled in the presence of at least one plasticizer to obtain a dope mixture. The obtained dope mixture can then be homogeneously distributed as a masterbatch with at least one polymer in a molten state, optionally after cooling, to obtain the polymer composition of the present invention. Alternatively, the completely ground suspension can be incorporated into a matrix polymer in a kneader, then dried and molded again like a normal granule in a melt state.

[0026] A further embodiment of the present invention relates to a method for the preparation of a polymer composition comprising at least one basic additive and optionally an inhibitor, or a method for the preparation of an article comprising such a polymer composition, the method comprising one step in which at least one basic additive and optionally at least one inhibitor are contacted with at least one polymer, at least a part of which is in a molten state, and then extruding and / or molding and / or film-blowing the mixture to obtain a molded part, fiber, film, deep-drawn film, injection molded article, thick-walled molded part, granules, microbeads, beads, containers or flower pots comprising the polymer composition. The technical details of the various extrusion, molding and film-blowing procedures are known to the skilled person and are described, for example, in "Industrial Plastics: Theory and Applications", E. Lokensgard, 5th Ed., 2010, Delmar, and can be applied to the method according to the present invention. In one aspect of the present invention, wet grinding of at least one basic additive and optionally an inhibitor and other optional additives is first carried out in a water-free solvent in a ball mill. The first portion of the polymer can be present throughout the grinding. The polymer portion then increases slightly and the suspension is dried, for example, in a roller dryer or spray dryer. If the polymer is poorly soluble in common solvents, such as acetone, ethyl acetate, butyl acetate, etc., the solids to be ground can be ground, for example, in acetone and stabilized with 1-5% cellulose acetate to obtain a dope mixture containing a basic additive. In another embodiment, at least one basic additive is dry-milled, optionally with a portion of the polymer, optionally in a portion containing a different polymer, and further optionally in the presence of another additive, such as an anti-agglomeration additive, to obtain a dope mixture containing the basic additive. In yet another embodiment, the basic additive is milled in the presence of at least one plasticizer to obtain a dope mixture. The resulting dope mixture can then be uniformly distributed as a masterbatch with the polymer in the mixing zone of the extruder.Alternatively, the completely ground suspension can be incorporated into a matrix polymer in a kneader, then dried if the dope mixture contains a solvent, and molded again like a normal granule in the melt state. The molten polymer composition obtained by contacting at least one polymer, at least one basic additive, optionally an inhibitor and further additives at elevated temperature can be subjected to molding, extrusion and / or film blowing according to process details known to those skilled in the art and described, for example, in "Industrial Plastics: Theory and Applications", E. Lokensgard, 5th Ed., 2010, Delmar.

[0027] Another embodiment of the present invention relates to a filter tow comprising the polymer composition according to the present invention as shown above, in particular a filter tow in which the polymer composition comprises at least one basic additive, at least one inhibitor and a pigment. A polymer composition comprising MgO, citric acid and TiO2 is preferred. Another preferred polymer composition comprises MgO and does not comprise any inhibitor. Another aspect of the present invention is a filter tow comprising fibers produced by a method comprising at least one step b) as described above.

[0028] To the extent that the disclosure of a publication incorporated herein by reference conflicts with the description of this application to the extent that it may render a term unclear, this description shall control.

[0029] The following examples are intended to illustrate the invention but not to limit its scope.

[0030] Example 1 - Degradability of cast film The films were prepared by dissolving cellulose acetate DS 2.45 in acetone, adding a basic additive and optionally an inhibitor. The resulting mixture was subjected to a film casting procedure using an automatic film applicator. The films were dried and cut into pieces (6.5 cm x 6.5 cm), the pieces were mounted on frames and buried in soil according to EN ISO 11721-1. After one and two months, specimens were retrieved from the soil, carefully cleaned from coarse sediments and checked for weight and visually for area loss. Each reported weight loss and area loss, respectively, is the average of six films and relates to the part of the film that was in contact with the soil. Film A: from 15 parts cellulose acetate and 85 parts acetone (comparative example) Film B: 15 parts cellulose acetate, 85 parts acetone, 0.79 parts MgO (yielding 5% MgO by weight in the final product) Film C: 15 parts cellulose acetate, 85 parts acetone, 0.38 parts MgO (yielding 2.5% MgO by weight in the final product) Film D: 15 parts cellulose acetate, 85 parts acetone, 0.79 parts MgO (yielding 5 wt. % MgO in the final product) and 0.08 parts citric acid (yielding 0.5 wt. % citric acid in the final product).

[0031] JPEG0007586864000001.jpg55164

[0032] Example 2 - Degradability of spun fibers A spinning solution was prepared by mixing cellulose acetate (DS 2.45) with acetone and spun into 1.9 denier filaments of Y cross section using a dry spinning process. The filaments were milled and subjected to aquatic aerobic biodegradation according to ISO 14851. Biodegradation was determined by measuring O2 consumption. Filament A (comparison): spinning solution of 26.9 parts cellulose acetate and 0.1 parts TiO2 in 73 parts acetone. Filament B: spinning solution from 25.6 parts cellulose acetate, 1.35 parts MgO (yielding 5% by weight in the final product), 0.07 parts citric acid (yielding 0.25% by weight in the final product) and 0.1 parts TiO2 in 73 parts acetone.

[0033] JPEG0007586864000002.jpg47164

Claims

1. A fiber comprising a polymer composition comprising at least one polymer and at least one basic additive, said at least one basic additive having a pH of 13 or less and 7 or more when measured in a 1 wt % solution in water at 20° C., said at least one basic additive in said polymer composition being selected from the group consisting of MgO, ZnO, CaO, and Al 2 O 3 , and every polymer in said polymer composition being cellulose acetate.

2. The at least one basic additive in the polymer composition has a viscosity of 10° C. -6 10. The fiber of claim 1 having a solubility of ∼70 g / 100 mL water.

3. 3. The fiber of claim 1 or 2, wherein the at least one basic additive is MgO.

4. The fibre according to any one of claims 1 to 3, wherein said at least one basic additive is present in said polymer composition in the form of finely distributed particles, with a D90 particle size of less than or equal to 10 μm.

5. The fibre according to any one of the preceding claims, wherein said at least one basic additive is present in said polymer composition in the form of finely distributed particles in an amount ranging from 0.01 to 40% by weight.

6. The fiber according to any one of claims 1 to 5, wherein the polymer composition further comprises at least one inhibitor of the autocondensation reaction that occurs in a solvent having at least one carbonyl functional group and a C-H bond in the α-position of the carbonyl functional group.

7. 7. The fiber of claim 6, wherein the at least one suppressor in the polymer composition is selected from the group consisting of carboxylic acids and alcohols.

8. 8. The fiber of claim 7, wherein the at least one inhibitor in the polymer composition is selected from the group consisting of citric acid, lactic acid, malic acid, tartaric acid, and glycerol.

9. The fiber according to any one of claims 6 to 8, wherein said at least one inhibitor is present in said polymer composition in an amount of 0.001 to 10% by weight.

10. A method for producing the fiber of any one of claims 1 to 9 or an article comprising the fiber of any one of claims 1 to 9, comprising at least one step selected from the group comprising: a) contacting at least one basic additive and optionally at least one inhibitor with at least one polymer in a liquid phase comprising at least one solvent, and then spinning the resulting mixture to obtain a fiber comprising said polymer composition; b) contacting at least one basic additive with at least one polymer, at least partially in a molten state, and then extruding the mixture to obtain a fiber comprising said polymer composition.

11. A filter tow comprising the fibers according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Biodegradable plastic molding

    JP1992146952A

  • Tobacco smoke filter material and method of making same

    JP1993505106A

  • Filter material and filter for cigarette

    JP1999057343A

  • Far infrared radiation particle-containing rayon-based fiber, method for producing the same and underwear containing the fiber

    JP2002161429A

  • Biodegradable composition comprising starch and polysaccharide ester

    JP2002523598A