(Binary) Metal Sulfide Polymer Composites and Their Use as Catalysts for Hydrogen Production - Patent application

By forming a composite of amorphous metal sulfide nanoparticles with sulfur-containing polymers, the stability and catalytic performance of amorphous metal sulfides are enhanced, addressing the issues of reductive corrosion and overvoltage in hydrogen generation, providing a cost-effective alternative to platinum-based catalysts.

JP7586926B2Active Publication Date: 2024-11-19TOYOTA MOTOR EUROPE NV SA +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022566276
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-29
Filing Date
2021-04-28
Publication Date
2024-11-19
Estimated Expiration
2041-04-28

AI Technical Summary

Technical Problem

Amorphous metal sulfide catalysts like molybdenum sulfide suffer from low stability due to reductive corrosion, leading to detachment and loss of catalytic activity, and require a higher overvoltage for hydrogen generation compared to platinum-based catalysts.

Method used

A composite material is formed by directly bonding amorphous metal sulfide nanoparticles, such as molybdenum sulfide, with sulfur-containing polymers through covalent bonds, which stabilizes the nanoparticles and maintains active sites, preventing detachment and enhancing catalytic performance.

Benefits of technology

The composite material exhibits improved stability against oxygen and maintains catalytic activity over time, reducing the overvoltage required for hydrogen generation, offering a cost-effective alternative to platinum-based catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586926000002
    Figure 0007586926000002
  • Figure 0007586926000003
    Figure 0007586926000003
  • Figure 0007586926000004
    Figure 0007586926000004
Patent Text Reader

Abstract

The present invention relates to a composite material formed of amorphous (binary) metal sulfide nanoparticles and a sulfur-containing polymer, wherein the amorphous (binary) metal sulfide nanoparticles are directly bonded to the sulfur-containing polymer by coordinate covalent bonds. The present invention also relates to a method for preparing the composite material according to the present invention. The use of the composite material according to the present invention as a catalyst for hydrogen production is also part of the present invention. Finally, the present invention relates to a proton exchange membrane (PEM) electrolyzer comprising the composite material according to the present invention, and a photoelectrochemical cell comprising the composite material according to the present invention.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THEINVENTION The present invention relates to a composite polymeric material formed of a sulfur-containing polymer and amorphous (binary) metal sulfide nanoparticles, which can be bonded to metal sites via sulfur atoms (or sulfur-based binding sites). The present invention also relates to a method for the preparation of the composite material according to the invention. The use of the composite material according to the invention as a catalyst for hydrogen production is also part of the present invention. Finally, the present invention relates to a proton-exchange membrane (PEM) electrolyser comprising the composite material according to the invention, and to a photoelectrochemical cell comprising the composite material according to the invention.

[0002] Research Support Information The project leading to this patent application has received funding from the European Research Council (ERC) under the European Union's Horizon 2020 research and innovation programme (grant agreement no. 836429). [Background technology]

[0003] Technical background Metal sulfides such as molybdenum sulfide are very attractive noble metal-free electrocatalysts for the hydrogen evolution reaction (HER). For example, amorphous molybdenum sulfide (a-MoS), prepared as nanoparticles or as films, x ) was detected by the separate [Mo3S7] 4+ The cluster (hereafter referred to as [Mo]3 cluster) is a disulfide (S2 2- ) anions bonded to other clusters. This molecular structure allows a-MoS x This explains some of the special properties of the cations, such as their catalytic activity, reductive activation and corrosion. In some clusters, disulfides (S2 2-) ligand, oxo(O 2- ) ligand, or sulfide (S 2- ) ligands remain unshared and are considered terminal ligands. Under reducing aqueous conditions, these terminal ligands are displaced, allowing the molybdenum hydride sites to become active sites for H2 evolution. Thus, such HER electrocatalysts are considered to be a possible alternative to platinum, and therefore have attracted great interest. Indeed, Pt-based catalysts have high performance and stability, but have the disadvantages of being scarce and expensive.

[0004] Scalable and renewable hydrogen production by solar-driven water splitting using viable and economical (photo)electrochemical devices or a combination of electrochemical and photovoltaic devices is a potential technology to address the global demand for renewable energy. To this end, highly efficient electrocatalysts based on non-precious metals for oxygen evolution reaction (OER) and HER have been explored. In particular, during the past few years, significant progress has been made in the search for platinum-based HER electrocatalysts based on transition metals such as Fe, Ni, Co, Mo, or W. Indeed, more abundantly available alternatives to Pt-based catalysts are needed to realize large-scale hydrogen production through scale-up. Molybdenum sulfide is one of the highly promising candidates to replace platinum due to its high performance, as well as other metal sulfides. In particular, crystalline molybdenum disulfide (c-MoS2), amorphous molybdenum sulfide (a-MoS2), and other metal sulfides have been developed. x ), and [Mo3S4] 4+ , [Mo3S 13 ] 2- , or [MoS 12 ] 2-Molybdenum sulfide clusters such as have recently attracted attention due to their scalable preparation methods, attractive catalytic activity, robustness, and ability to be integrated into H2-evolving photocathodes (Y. Latach et al., ACS Appl. Mater. Interfaces 2015, 7, 4476-4480; T. Bourgeteau et al. B. ACS Appl. Mater. Interfaces 2015, 7, 16395-16403; T. Bourgeteau et al., B. Energy Environ. Sci. 2013, 6, 2706-2713; T. Bourgeteau et al., BJ Mater. Chem. A 2016, 4, 4831-4839; A. Morozan et al., Nanotechnology 2016, 27, 355401). Also, other metal sulfides with linkers such as dithiolate ligands between clusters (Ji et al. J. Am. Chem. Soc. 2018, 140, 13618-13622), or mixtures of amorphous molybdenum / tungsten sulfides with other metal ions such as Co, Cu, Fe, and Ni (Staszak-Jirkovsky(yacute) et al. Nat. Mater. 2016, 15, 197; Tran et al. Energy Environ. Sci. 2012, 5, 8912-8916; Di Giovanni et al. ACS Catal. 2016, 6, 2626-2631; Tran et al. Energy. Environ. Sci. 2013, 6, 2452-2459; Shim et al. al. J. Am. Chem. Soc. 2013, 135, 2330-2337) is also attracting attention.

[0005] P.D.Tran et al. (Nature Materials, 2016, volume 15, pages 640-646) reported a-MoS x They investigated the structure and reactivity of [Mo3S 13 ] 2- Clusters (in other words, disulfides (S2 2-a-MoS, which can be formulated as a coordination polymer based on [Mo]3 clusters bound by ) anions x They report that the polymeric structure and molecular nature of [Mo]3 provide a catalytic center for proton reduction. By reducing and / or removing the terminal disulfide ligands, unsaturated Mo ions can be attached to the [Mo]3 cluster. IV Proton-coupled reduction of these sites then forms active centers for H2 evolution. Summary of the Invention [Problem to be solved by the invention]

[0006] However, metal sulfides such as molybdenum sulfide catalysts are not currently widely used in commercial electrolyzers due to their poor stability, especially towards oxygen. In the case of amorphous molybdenum sulfide, the lack of stability is due to the reductive dissociation of [Mo]3 clusters from the chain structure with the concomitant evolution of H2S, resulting in the reduction of many active sites. When these catalytic units dissociate and dissolve in the electrolyte solution, they lose activity, and the catalytic activity decreases over time.

[0007] Another drawback of amorphous metal sulfides, such as amorphous molybdenum sulfide, as catalysts is that the overpotential (or driving force) required to generate H2 at a significant rate is higher than that of platinum. This characteristic is evident when the catalyst is used at a current of 10 mA.cm -2 Overvoltage measured when operating at + OP, which is the difference between the working potential and the equilibrium potential of the / H2 bond 10mAcm-2 It can be quantified by the value.

[0008] Therefore, there remains a need for solutions to avoid or control the reductive corrosion of amorphous metal sulfide materials by synthetic modification of the cluster units and / or connecting ligands, and rational optimization of their catalytic performance. [Means for solving the problem]

[0009] Summary of the Invention This time, we focused on amorphous (binary) metal sulfides, especially amorphous molybdenum sulfide (a-MoS x It has been found that composites formed of sulfur-containing polymers directly bonded to Pt via coordinate covalent bonds can act as competitive hydrogen evolution catalysts and provide a low-cost and oxygen-stable alternative to current Pt-based electrocatalysts. The proposed composites of the present invention also show increased electrochemical performance for catalytic H2 evolution compared to pure amorphous metal sulfides.

[0010] Studies on photoelectrochemical cells combining non-precious metal-containing amorphous MoS3 particles with P3HT:PCBM have been carried out by T.Bourgeteau et al. (Energy Environ.Sci.2013,6,2706-2713; ACS Appl.Mater.Interfaces,2015,7,16395-16403; J.Mater.Chem.A 2016,4,4831-4839). In these studies, the P3HT and amorphous MoS3 particles are not homogeneously mixed. Importantly, the MoS3 particles, which are active for H2 evolution, are in contact with the PCBM n-type phase in P3HT:PCBM p / n solar cells. This point is demonstrated in a study investigating several different interfacial layers that can increase the charge transfer between P3HT:PCBM and amorphous MoS3 particles in photoelectrochemical cells. In such cells, the presence of an interfacial layer between the MoS3 metal and the P3HT:PCBM polymer prevents direct contact between MoS3 and P3HT:PCBM.

[0011] Two-dimensional nanosheets of crystalline MoS2 have also been used to assemble layers of P3HT to form highly ordered, long-fibrous structures of P3HT / MoS2 nanocomposites (Chaudhary et al. J. Phys. Chem. C 2020, 124, 8101-8109). The formation of this nanocomposite is due to the π-π stacking interactions between MoS2 and P3HT. Notably, all Mo ions present in the basal plane of c-MoS2 are saturated and cannot undergo coordinate covalent bonding.

[0012] In the composite material according to the invention, the inventors have observed that the direct contact of the sulfur-containing polymer with the amorphous (binary) metal sulfide nanoparticles through intimate bonds improves the stability of the resulting material, especially its stability against oxygen. This is due to the fact that the sulfur-containing polymer with sulfur-based coordination sites bonds the clusters of amorphous (binary) metal sulfides, such as the [Mo]3 clusters of amorphous molybdenum sulfide, and acts as an exoskeleton of the amorphous (binary) metal sulfide structure, thus preventing the separation of the clusters and their dissolution in the electrolyte and maintaining a constant number of active sites (as shown in FIG. 1 for the case of amorphous molybdenum sulfide). Moreover, the sulfur-containing polymer can keep the clusters in close proximity, so that even if the disulfide bonds between the clusters of the amorphous (binary) metal sulfide nanoparticles are broken, these bonds can be easily reformed. It is also believed that in the presence of oxygen (O2), the sulfur-containing polymer protects the clusters of amorphous (binary) metal sulfide nanoparticles from decomposition.

[0013] Summary of the Invention Thus, in a first aspect, the present invention contemplates a composite material comprising amorphous (binary) metal sulfide nanoparticles directly bonded to a sulfur-containing polymer by coordinate covalent bonds.

[0014] In another aspect, the present invention relates to a process for the preparation of a composite material according to the invention, comprising the steps of preparing amorphous (binary) metal sulfide nanoparticles, preferably by a redox reaction process, and then dispersing the obtained amorphous (binary) metal sulfide nanoparticles in and reacting with a sulfur-containing polymer.

[0015] The present invention also relates to the use of the composite material according to the invention as a catalyst for hydrogen production.

[0016] Finally, the present invention relates to electrochemical devices (such as, but not limited to, proton exchange membrane (PEM) electrolysers and photoelectrochemical cells) comprising a composite material according to the present invention in the (photo)cathode part. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 shows the composite structure of the catalyst according to the present invention, which shows amorphous molybdenum sulfide (a-MoSx) based on [Mo]3 clusters stabilized by sulfur-based coordination functional groups. [Diagram 2] FIG. 1 shows polarization curves for HER obtained with an amorphous a-MoSx catalyst (two different batches) (representative of the prior art) and with a composite a-MoSx-P3HT material (catalyst according to the invention), the surface used being the geometric surface of the electrode. [Diagram 3] FIG. 1 shows the polarization curves for HER obtained with composite a-MoSx-P3HT material (catalyst according to the invention) (washed and unwashed), the surface used being the geometric surface of the electrode. [Figure 4] The performance of a-MoSx-P3HT in an electrochemical device (electrolyzer) is investigated, and single cell polarization curves for proton exchange membrane (PEM) electrolysis (at 80° C.) using Ir black / Nafion® NRE-212 / a-MoSx-P3HT as the membrane-electrodes assembly (MEA) are shown. [Diagram 5] FIG. 1 shows the polarization curves for HER obtained with the composite materials WSx-P3HT(20:1) and WSx-P3HT(40:1) (catalyst according to the invention) and with the WSx catalyst, the surface used being the geometric surface of the electrode. [Figure 6] FIG. 1 shows the polarization curves for HER obtained with the composite materials CoWSx-P3HT(20:1) and CoWSx-P3HT(40:1) (catalyst according to the invention) and with the CoWSx catalyst, the surface used being the geometric surface of the electrode. [Figure 7] FIG. 1 shows the polarization curves for HER obtained with a composite FeMoSx-P3HT (20:1) material (catalyst according to the invention) and with a FeMoSx catalyst, the surface used being the geometric surface of the electrode. [Figure 8] FIG. 1 shows the polarization curves for HER obtained with a composite CoMoSx-P3HT (20:1) material (catalyst according to the invention) and with a CoMoSx catalyst, the surface used being the geometric surface of the electrode. [Figure 9a] Figure 1 shows the chronopotentiometry curves (stability test) of a-MoSx and a-MoSx-P3HT under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 9b] Figure 1 shows the chronopotentiometry curves (stability test) of a-MoSx and a-MoSx-P3HT under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 9c] Figure 1 shows the chronopotentiometry curves (stability test) of a-MoSx and a-MoSx-P3HT under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 9d] Figure 1 shows the chronopotentiometry curves (stability test) of a-MoSx and a-MoSx-P3HT under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 10]Figure 9 shows the evolution of overpotential (stability test) for a-MoSx during 24 hours of operation (ΔOP10mAcm-2 / mV=OP10mAcm-2(t) / mV-OP10mAcm-2(t0) / mV) (data extracted from Figure 9(a,c)). [Figure 11] Figure 9 shows the evolution of overpotential (stability test) for a-MoSx-P3HT during 24 h operation (ΔOP10mAcm-2HER / mV=OP10mAcm-2(t) / mV-OP10mAcm-2η(t0) / mV) (data extracted from Figure 9(b,d)). [Figure 12a] Figure 1 shows the chronopotentiometry curves (stability test) of FeMoSx and FeMoSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 12b] Figure 1 shows the chronopotentiometry curves (stability test) of FeMoSx and FeMoSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 12c] Figure 1 shows the chronopotentiometry curves (stability test) of FeMoSx and FeMoSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 12d] Figure 1 shows the chronopotentiometry curves (stability test) of FeMoSx and FeMoSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 13] Figure 12 shows the evolution of overpotential (stability test) for FeMoSx during 24 hours of operation (ΔOP10mAcm-2 / mV=OP10mAcm-2(t) / mV-OP10mAcm-2(t0) / mV) (data extracted from Figure 12(a,c)). [Figure 14] Figure 12 shows the evolution of overpotential (stability test) for FeMoSx-P3HT(20:1) during 24 hours of operation (ΔOP10mAcm-2 / mV=OP10mAcm-2(t) / mV-OP10mAcm-2(t0) / mV) (data extracted from Figure 12(b,d)). [Figure 15a] Figure 1 shows the chronopotentiometry curves (stability test) of WSx and WSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 15b] Figure 1 shows the chronopotentiometry curves (stability test) of WSx and WSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 15c] Figure 1 shows the chronopotentiometry curves (stability test) of WSx and WSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 15d] Figure 1 shows the chronopotentiometry curves (stability test) of WSx and WSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 16] Figure 15 shows the evolution of overpotential for WSx during 24 hours of operation (stability test) (ΔOP10mAcm-2 / mV=OP10mAcm-2(t) / mV-OP10mAcm-2(t0) / mV) (data extracted from Figure 15(a,c)). [Figure 17] Figure 15 shows the evolution of overpotential (stability test) for WSx-P3HT(20:1) during 24 hours of operation (ΔOP10mAcm-2 / mV=OP10mAcm-2(t) / mV-OP10mAcm-2(t0) / mV) (data extracted from Figure 15(b,d)). [Figure 18a] Figure 1 shows the chronopotentiometry curves (stability test) of CoMoSx and CoMoSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 18b] Figure 1 shows the chronopotentiometry curves (stability test) of CoMoSx and CoMoSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 18c]Figure 1 shows the chronopotentiometry curves (stability test) of CoMoSx and CoMoSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 18d] Figure 1 shows the chronopotentiometry curves (stability test) of CoMoSx and CoMoSx-P3HT (20:1) under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). [Figure 19] Figure 18 shows the evolution of overpotential (stability test) for CoMoSx during 24 hours of operation (ΔOP10mAcm-2 / mV=OP10mAcm-2(t) / mV-OP10mAcm-2(t0) / mV) (data extracted from Figure 18(a,c)). [Figure 20] Figure 18 shows the evolution of overpotential (stability test) for CoMoSx-P3HT(20:1) during 24 hours of operation (ΔOP10mAcm-2 / mV=OP10mAcm-2(t) / mV-OP10mAcm-2(t0) / mV) (data extracted from Figure 18(b,d)). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Detailed Description of the Invention The present invention relates to Amorphous (binary) metal sulfide nanoparticles based on amorphous (binary) metal sulfide clusters; The present invention relates to a composite material formed with a sulfur-containing polymer, in which amorphous (binary) metal sulfide nanoparticles are directly bonded to the sulfur-containing polymer by coordinate covalent bonds.

[0019] In the sense of the present invention, amorphous (binary) metal sulfide nanoparticles encompass amorphous single metal sulfide nanoparticles and amorphous double metal sulfide nanoparticles. Thus, according to a first embodiment, the amorphous (binary) metal sulfide nanoparticles are amorphous single metal sulfide nanoparticles. According to a second embodiment, the amorphous (binary) metal sulfide nanoparticles are amorphous double metal sulfide nanoparticles, and the metals of the amorphous double metal sulfides are different from each other.

[0020] The metal of the amorphous (binary) metal sulfide nanoparticles according to the invention may advantageously be selected in the group consisting of the metals of the fifth and sixth columns of the periodic table (Mendeleev's table), optionally combined with other elements selected in the group consisting of the fourth to eleventh columns of the periodic table (if the amorphous (binary) metal sulfide is an amorphous binary metal sulfide). In a preferred embodiment, the metal of the amorphous (binary) metal sulfide nanoparticles according to the invention is selected in the group consisting of Mo, V and W, optionally combined with other elements selected in the group consisting of Mo, V, W, Ti, Cr, Mn, Fe, Co, Ni, Cu, Nb, Ta, optionally combined with other elements selected in the group consisting of Mo, V, W, Ti, Cr, Mn, Fe, Co, Ni, Cu, Nb, Ta (if the amorphous (binary) metal sulfide is an amorphous binary metal sulfide). In a further preferred embodiment, the metal of the amorphous (binary) metal sulfide nanoparticles according to the invention is selected in the group consisting of Mo and W, optionally (when the amorphous (binary) metal sulfide is an amorphous binary metal sulfide) in combination with another element, preferably selected in the group consisting of Mo, W, Fe, Co.

[0021] The amorphous (binary) metal sulfide is an amorphous binary metal sulfide, and when the metals of the amorphous binary metal sulfide nanoparticles are different from each other, they are advantageously selected in the group consisting of Mo, V, and W, and are combined with another element selected in the group consisting of Mo, V, W, Ti, Cr, Mn, Fe, Co, Ni, Cu, Nb, Ta. In a preferred embodiment, they are advantageously selected in the group consisting of Mo and W, and when the metals of the amorphous binary metal sulfide nanoparticles are different from each other, they are combined with another element selected in the group consisting of Mo, W, Fe, Co. In a preferred embodiment, the amorphous binary metal sulfide nanoparticles are a-CoMoS x Nanoparticles, a-FeMoS x Nanoparticles, and a-CoWS x Nanoparticles are selected from the group consisting of:

[0022] In a particularly preferred embodiment, the metal of the amorphous (binary) metal sulfide of the present invention is Mo, and in such embodiment, the present invention provides Disulfide (S2 2- Amorphous molybdenum sulfide nanoparticles based on [Mo]3 clusters (as building blocks) linked by [Mo]3) anions; and a sulfur-containing polymer, wherein the [Mo]3 cluster is directly bonded to the sulfur-containing polymer by a coordinate covalent bond.

[0023] The composite material of the present invention has the major advantage that it is a hydrogen evolution catalyst with increased electrochemical performance and improved oxygen stability compared to amorphous metal sulfides.

[0024] In the composite material according to the present invention, the amorphous (binary) metal sulfide nanoparticles are in direct contact with the sulfur-containing polymer by coordinate covalent bonds between the sulfur atoms of the sulfur-containing polymer and the metal ions of the amorphous (binary) metal sulfide. In this way, the amorphous (binary) metal sulfide and the sulfur-containing polymer are intimately connected. In other words, the composite material according to the present invention does not have an intermediate layer between the amorphous (binary) metal sulfide and the sulfur-containing polymer.

[0025] In the sense of the present invention, a coordinate covalent bond is a covalent bond with two centers and two electrons originating from the same atom. A coordinate covalent bond is characterized in that it connects a metal ion with a ligand.

[0026] In the composite material according to the invention, the sulfur-containing polymer may be selected in the group consisting of polythiophenes such as poly(3-hexylthiophene-2,5-diyl) (P3HT), poly(ethylenedioxythiophenes) such as poly(3,4-ethylenedioxythiophene) (PEDOT), poly(arylene thioethers) such as polyphenylene sulfide, and mixtures thereof.

[0027] In one preferred embodiment, the sulfur-containing polymer is poly(3-hexylthiophene-2,5-diyl) (P3HT).

[0028] The sulfur-containing polymer according to the present invention has a molecular weight of 5,000 to 100,000 g.mol -1 The copolymer may have a number average molecular weight Mn in the range of

[0029] In the composite material according to the invention, the amorphous (binary) metal sulfide nanoparticles are based on (binary) metal sulfide clusters and can be considered as coordination polymers of (binary) metal sulfide clusters. The nanoparticles according to the invention are formed of several clusters, preferably a group of 2 to 40 clusters, which are linked together to form a molecular-based coordination polymer. The number of (binary) metal sulfide clusters in one chain of amorphous (binary) metal sulfide can therefore range from 2 to 40. In this particular embodiment of amorphous molybdenum sulfide, the latter is based on [Mo]3 clusters and can be considered as a polymer of [Mo]3 clusters. Typically, in this case, the number of [Mo]3 clusters in one chain of amorphous molybdenum sulfide can range from 2 to 30, preferably from 2 to 20, although longer [Mo]3 cluster polymers are not excluded.

[0030] The size of the amorphous (binary) metal sulfide clusters may advantageously range from 0.1 to 2 nm, preferably from 0.2 to 1.5 nm. The size of the amorphous (binary) metal sulfide clusters is the particle size Dn90 based on number (also referred to as particle diameter Dn90 based on number). The size of the amorphous (binary) metal sulfide clusters can be measured by scanning transmission electron microscopy (STEM), for example using a JEM-ARM200F NEOARM atomic resolution analytical electron microscope. More specifically, the size of the amorphous (binary) metal sulfide clusters can be measured by high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM). In a particularly preferred embodiment, when the amorphous (binary) metal sulfide clusters are [Mo]3 molybdenum sulfide clusters, the size of the [Mo]3 molybdenum sulfide clusters is about 0.3 nm. In this case, the structure of a-MoSx can be examined by scanning transmission electron microscopy (STEM) by using graphite flakes (GF) (Alfa Aesar) with a large surface area as a carbon support for the clusters to land gently, as described in Nature Materials, vol. 15, pages 640-646 (2016). GF was dissolved in H2SO4 solution (0.5 mol.L) before use. -1 ) at a potential of 1.0 V (vs. Ag / AgCl) for 3 min. -3 5 mL of the (wt%) a-MoSx suspension can be mixed with 50 mg of GF by continuous stirring. The methanol can then be evaporated under vacuum. The resulting sample, in which the GF surface is covered with a sub-monolayer of a-MoSx, can then be observed by high-angle annular dark-field (HAADF) imaging.

[0031] Concerning the size of the composite material according to the invention, this is advantageously in the range of 1 to 100 nm. The size of the composite material according to the invention is the particle size Dn90 based on number (also referred to as particle diameter Dn90 based on number). The size of the composite material can be measured by scanning electron microscopy (SEM) (for example using a ZEISS Ultra-55 scanning electron microscope) or transmission electron microscopy (TEM) (for example using a Cs-probe corrected FEI Titan Themis transmission electron microscope). More specifically, the size of the composite material can be measured by high angle annular dark field scanning transmission electron microscopy (HAADF-STEM). In this case, a catalyst suspension in ethanol can be prepared by ultrasonic homogenization and then drop cast onto an ultra-thin carbon film on a Cu grid as described in ACS Catalysis, 2020, 10, 14336-14348. The resulting sample can then be observed by HAADF-STEM and corresponding energy-dispersive spectroscopy (EDS) elemental mapping analysis (using an FEI-Osiris microscope (eg, operating at 200 kV)).

[0032] In the composite material according to the present invention, the amount of metal in the amorphous (binary) metal sulfide nanoparticles may be 20-75% by weight, preferably 30-60% by weight. In a particularly preferred embodiment, when the amorphous (binary) metal sulfide nanoparticles are amorphous molybdenum sulfide nanoparticles, the amount of Mo in the amorphous molybdenum sulfide nanoparticles may be 30-45% by weight, preferably 32-40% by weight, more preferably about 36% by weight.

[0033] In the composite material according to the present invention, the amount of S in the amorphous (binary) metal sulfide nanoparticles may be 25 to 80% by weight, preferably 40 to 60% by weight. In a particularly preferred embodiment, when the amorphous (binary) metal sulfide nanoparticles are amorphous molybdenum sulfide nanoparticles, the amount of S in the amorphous molybdenum sulfide nanoparticles may be 40 to 60% by weight, preferably 45 to 55% by weight, more preferably about 50% by weight.

[0034] In the composite material according to the present invention, the amorphous (binary) metal sulfide nanoparticles may further comprise oxygen, preferably in an amount ranging from 1 to 30% by weight, more preferably from 2 to 20% by weight. In a particularly preferred embodiment, when the amorphous (binary) metal sulfide nanoparticles are amorphous molybdenum sulfide nanoparticles, the amorphous molybdenum sulfide nanoparticles may further comprise oxygen, preferably in an amount ranging from 2 to 20% by weight, more preferably from 5 to 15% by weight, even more preferably about 14% by weight.

[0035] In the composite material according to the present invention, the mass ratio of the amorphous (binary) metal sulfide nanoparticles to the sulfur-containing polymer may be in the range of 1:1 to 100:1, preferably 1:1 to 50:1, more preferably 1:1 to 45:1, and even more preferably 25:1 to 45:1.

[0036] In the composite material according to the present invention, the mass ratio of the sulfur-containing polymer to the entire composite material according to the present invention may be in the range of 0.50 to 0.98, preferably 0.60 to 0.90.

[0037] In another aspect, the present invention relates to a process for the preparation of a composite material according to the present invention, comprising: (i) preparing amorphous (binary) metal sulfide nanoparticles, preferably by a redox reaction; (ii) dispersing the amorphous (binary) metal sulfide obtained in step (i) in a solution of a sulfur-containing polymer under stirring, thereby forming coordinate covalent bonds between the sulfur-containing polymer and the metal ions of the amorphous (binary) metal sulfide nanoparticles obtained in step (i).

[0038] The amorphous (binary) metal sulfide nanoparticles and the sulfur-containing polymer are as defined above for the composite material according to the invention.

[0039] Step (i) may be carried out by reacting the metal salt with a sulfur-containing compound, preferably with a compound having a thiourea group, more preferably with thiourea, ethylenethiourea, propylenethiourea, thioacetamide, thioacetic acid, or a mixture thereof, and then heating the resulting mixture. Heating is advantageously carried out in a microwave oven, having a radiation power capable of maintaining the temperature of the reaction medium at 200-300°C, preferably 230-270°C, and the pressure of the reaction medium at 6-10 bar, preferably 7-9 bar. For example, the radiation power may advantageously vary from 0 to 300 W in the synthesis of amorphous (binary) metal sulfides on a 100 mg scale. Heating by radiation may be carried out in a Discover Microwave Synthesizer (CEM).

[0040] Alternatively, step (i) can be carried out by a redox reaction of a thiometallate ion, even more preferably by a redox reaction of a thiometallate ion with an oxidizing agent, even more preferably by a redox reaction of an ammonium thiometallate with an oxidizing agent.

[0041] In step (i) of the process according to the invention, when the amorphous (binary) metal sulfide nanoparticles are prepared by a redox reaction between thiometallate ions and an oxidizing agent, the thiometallate ions may be oxidized by the addition of an oxidizing agent selected from the group consisting of sodium persulfate, potassium persulfate, sodium permanganate, potassium permanganate, sodium dichromate, potassium dichromate, ceric nitrate. In a preferred embodiment, the oxidizing agent used to prepare the amorphous (binary) metal sulfide nanoparticles in step (i) is sodium persulfate.

[0042] In one particularly preferred embodiment, when the amorphous (binary) metal sulfide nanoparticles are amorphous molybdenum sulfide nanoparticles, [MoS4](NH4)2 is advantageously used as the thiometallate salt which undergoes a redox reaction in step (i) to obtain amorphous molybdenum sulfide nanoparticles.

[0043] Step (i) according to the invention is advantageously carried out under argon with stirring for at least 30 minutes, more advantageously for 1 to 5 hours, even more advantageously for 2 hours.

[0044] At the end of step (i), the obtained amorphous (binary) metal sulfide nanoparticles may be washed with a solvent preferably selected in the group consisting of water, diethyl ether, C1-C6 alcohols such as methanol, ethanol, isopropanol, and mixtures thereof, and dried under vacuum until solvent-free prior to step (ii).

[0045] The solution of sulfur-containing polymer used in step (ii) of the process according to the invention may then comprise a sulfur-containing polymer dissolved in a solvent selected from the group consisting of water, 1,2-dichlorobenzene, dichloromethane, chloroform, 1,1,2,2-tetrachloroethane, 1,2,3-trichloropropane, chlorobenzene, and mixtures thereof. In a preferred embodiment, the sulfur-containing polymer is dissolved in 1,2-dichlorobenzene.

[0046] The concentration of the solution of the sulfur-containing polymer in step (ii) is 0.05 to 1 mg.mL -1 may vary.

[0047] Step (ii) according to the invention is advantageously carried out under stirring for at least 10 hours, preferably between 24 and 72 hours, more preferably for 48 hours.

[0048] The process according to the invention may further comprise a step (iii) of washing the composite material obtained at the end of step (ii) with a solvent selected in the group consisting of water, diethyl ether, C1-C6 alcohols such as methanol, ethanol, isopropanol, and mixtures thereof, preferably ethanol.

[0049] The process according to the invention may further comprise a step (iv) of drying the composite material obtained at the end of step (i) or (iii) under vacuum until free of solvent.

[0050] In a third aspect, the present invention relates to the use of a composite material according to the present invention as a catalyst, preferably as an electrocatalyst, for hydrogen (H2) production. In particular, the composite material according to the present invention may be used for HER.

[0051] In a preferred embodiment, the composite material according to the invention is used in an electrochemical cell (Wang et al. Renewable and Sustainable Energy Reviews 2014, 29, 573), more preferably in In a proton exchange membrane (PEM) water electrolyser, which comprises an anode and a cathode that are electrically connected but separated by an ion-conducting membrane and an ion-conducting electrolyte (Sun et al. Catalysts 2018, 8, 657), or They are advantageously used as HER catalysts in photoelectrochemical cells (Walter et al. Chem. Rev. 2010, 110, 6446-6473), which may comprise a (photo)anode and / or a (photo)cathode electrically connected but separated by an ion-conducting membrane and an ion-conducting electrolyte, preferably for water splitting.

[0052] In one aspect, the present invention also relates to a proton exchange membrane (PEM) electrolyser comprising a composite material according to the present invention.

[0053] An electrolyser is an electrochemical device that uses an electric current to provide energy to split water (H2O) molecules into hydrogen (H2) and oxygen (O2). Electrolysers consist of an anode, a cathode, and an electrolyte. PEM electrolysers use a proton-conducting solid polymer (e.g., Nafion®).

[0054] The PEM electrolyzer according to the present invention consists of two external conductive plates and two grooved plates (cathode side made of carbon and anode side made of titanium). The grooved plates form a serpentine flow field over the working area, promoting the flow of water and the produced gases (H2 and O2). The membrane-electrode assembly (MEA) is sandwiched between the two grooved plates and clamped together with the conductive plates using nuts and bolts. The cell is assembled with a polytetrafluoroethylene (PTFE) gasket. The MEA may be prepared, for example, by forming the anode with a Nafion® NRE-212 membrane (50 μm thick) as the polymer electrolyte membrane, a water oxidation catalyst, and a titanium grid on one side, and forming the cathode on the other side with a hydrogen evolution catalyst (i.e., the composite material according to the present invention) deposited on the gas diffusion layer. The gas diffusion layer is a porous layer made of carbon fibers. The side on which the catalyst is deposited may be covered with a microporous layer, usually made of PTFE and carbon black. When a potential difference (voltage) is applied between two electrodes (anode and cathode) through a conductive plate, water is oxidized at the anode to produce protons, electrons, and O2, which are pumped out through the titanium grid. + ) migrates through the polymer electrolyte to the cathode where it is reduced to hydrogen using electrons provided by an external power source. The hydrogen is expelled through the diffusion layer.

[0055] In another aspect, the present invention relates to a photoelectrochemical cell, preferably for water splitting, comprising a composite material according to the invention. The photoelectrochemical cell advantageously comprises a (photo)anode and / or a (photo)cathode electrically connected but separated by an ion-conducting membrane and an ion-conducting electrolyte. In a preferred embodiment, the composite material according to the invention is in contact with the (photo)cathode of the photoelectrochemical cell.

[0056] Unless otherwise stated herein or clearly contradicted by context, the present invention encompasses all possible variations of the elements described above in any combination. Thus, all features and embodiments described herein (particularly as applicable, advantageous or preferred in the context of the present invention) should be construed as applicable in combination with each other in preferred embodiments of the present invention.

[0057] In addition to what has been described above, the present invention further comprises other features, the latter of which will become apparent from the following description, namely the examples in which the composite material (catalyst) according to the present invention is evaluated.

[0058] Working Example Amorphous molybdenum sulfide (a-MoS) was prepared by chemical oxidation of [MoS](NH) x Preparation of: Sodium persulfate (4 mmol, 960 mg) was added to a deep red solution of [MoS4](NH4)2 (2 mmol, 520 mg) dissolved in water (100 mL) and thoroughly degassed with Ar. The solution quickly turned into a dark brown suspension, which was stirred continuously for 2 h under Ar. After the reaction was completed, the dark brown powder was collected by centrifugation and washed thoroughly with water, ethanol, and diethyl ether. The product was dried under vacuum overnight and kept in air atmosphere. The obtained sample was named a-MoS x It was decided.

[0059] Amorphous tungsten sulfide (WS x ) and amorphous binary metal sulfides (CoWS x , FeMoS x , CoMoS x Preparation of: Appropriate amounts of metal salts (WCl6: 1 mmol, 396 mg) and thiourea (1.5 mmol, 114.2 mg) precursors were mixed in ethylene glycol (10 mL). After stirring for 5 min, the solution was placed in a special 30 mL vial in a Discover SP microwave synthesizer (CEM) and reacted under the following conditions: temperature was maintained at 255°C with radiation at 200 W for 20 min and pressure of 8 bar. The resulting viscous black precipitate was transferred into ethanol and centrifuged. The precipitate was then washed with ethanol and distilled water by centrifuging several times until the supernatant was clear. The final precipitate (approximately 150 mg) was vacuum dried overnight and then collected for characterization. The resulting sample was a-WS x It was decided.

[0060] Appropriate amounts of metal salts (WCl6: 0.5 mmol, 198 mg and CoCl2·6H2O: 0.5 mmol, 119 mg) and thiourea (1.5 mmol, 114.2 mg) precursors were mixed in ethylene glycol (10 mL). After stirring for 5 min, the solution was placed in a special 30 mL vial in a Discover SP microwave synthesizer (CEM) and reacted under the following conditions: temperature was maintained at 255 °C and pressure was 8 bar with radiation varying from 0 to 300 W for 20 min. The resulting viscous black precipitate was transferred into ethanol and centrifuged. The precipitate was then washed with ethanol and distilled water by centrifuging several times until the supernatant was clear. The final precipitate (approximately 120 mg) was vacuum dried overnight and then collected for characterization. The resulting sample was a-CoWS x It was decided.

[0061] Appropriate amounts of metal salts (MoCl3: 0.5 mmol, 101.1 mg and FeCl3·6H2O: 0.5 mmol, 135.2 mg) and thiourea (1.5 mmol, 114.2 mg) precursors were mixed in ethylene glycol (10 mL). After stirring for 5 min, the solution was placed in a special 30 mL vial in a Discover SP microwave synthesizer (CEM) and reacted under the following conditions: temperature was maintained at 255 °C and pressure was 8 bar with radiation varying from 0 to 300 W for 20 min. The resulting viscous black precipitate was transferred into ethanol and centrifuged. The precipitate was then washed with ethanol and distilled water by centrifuging several times until the supernatant was clear. The final precipitate (approximately 130 mg) was vacuum dried overnight and then collected for characterization. The resulting sample was named a-FeMoS x It was decided.

[0062] Appropriate amounts of metal salts (MoCl3: 0.5 mmol, 101.1 mg and CoCl2·6H2O: 0.5 mmol, 119 mg) and thiourea (1.5 mmol, 114.2 mg) precursors were mixed in ethylene glycol (10 mL). After stirring for 5 min, the solution was placed in a special 30 mL vial in a Discover SP microwave synthesizer (CEM) and reacted under the following conditions: temperature was maintained at 255 °C and pressure was 8 bar with radiation varying from 0 to 300 W for 20 min. The resulting viscous black precipitate was transferred into ethanol and centrifuged. The precipitate was then washed with ethanol and distilled water by centrifuging several times until the supernatant was clear. The final precipitate (approximately 130 mg) was vacuum dried overnight and then collected for characterization. The resulting sample was named a-CoMoS x It was decided.

[0063] The composite material a-MoS according to the present invention x Preparation of -P3HT: A solution of poly(3-hexylthiophene-2,5-diyl) (P3HT, M102 from Ossila 95.7% RR, Mw=65,200) in o-dichlorobenzene (o-DCB) was prepared at 0.25 mg.mL-1 Amorphous molybdenum sulfide (120 mg) was dissolved in a solution of P3HT (0.25 mg.mL) in o-DCB. -1 The a-MoS was dispersed in 25 mL of 100% NaCl and kept under stirring for 24 h. x The mass ratio of P3HT to SiO2 was 20:1. The composite material was then collected by centrifugation and washed with ethanol and water. Finally, the composite material was dried under vacuum overnight and kept in an air atmosphere.

[0064] Preparation of other composite materials according to the invention: A solution of poly(3-hexylthiophene-2,5-diyl) (P3HT, M102 from Ossila 95.7% RR, Mw=65,200) in o-dichlorobenzene (o-DCB) was prepared at 0.25 mg.mL -1 The (binary) metal sulfide (a-WS) prepared as described above was x , a-CoWS x , a-FeMoS x , a-CoMoS x ) (120 mg) in a solution of P3HT in o-DCB (0.25 mg mL -1 ) and kept under stirring for 24 hours. The mass ratio of each (binary) metal sulfide to P3HT is 20:1. The resulting composite material was then collected by centrifugation and washed with ethanol and water. Finally, the composite material was dried overnight under vacuum and kept in air atmosphere. This sample is hereafter and in the figures as "Composite Catalyst Name P3HT(20:1)".

[0065] Preparation of electrodes: The electrochemical activity of the catalysts towards HER was investigated using a gas diffusion electrode (GDE) as the working electrode. For each composite prepared as described above, a catalyst ink was prepared by sonication, containing 1 mg of composite (catalyst), 0.2 mg of CNTs (NANOCYL® NC7000™ multi-walled carbon nanotubes, Belgium), 160 μL of ethanol, 40 μL of water, and 10 μL of 5 wt % Nafion® perfluorinated resin solution. Four 10 μL aliquots of this catalyst ink were then transferred to a 0.196 cm sieve of the initial state. 2 The catalyst was deposited successively on a microporous layer of a gas diffusion layer (GDL (gas diffusion layer) with a microporous layer, SIGRACET® 39-BC (SGL Carbon, Germany)) with a catalyst content of 0.97 mg cm -2 (corresponding to 40 μL of catalyst ink). The working GDE with the catalyst layer deposited was used in a three-electrode cell configuration.

[0066] Varying P3HT concentration: The concentration of P3HT in o-DCB was reduced to 0.125 mg mL -1 The same protocol as above was followed, except that WS x and CoWS x A composite material consisting of two synthetic catalysts was prepared. In this case, the mass ratio of the catalyst to P3HT was 40:1. This sample will be referred to as "Composite Material Catalyst Name P3HT (40:1)" in the following and in the figures.

[0067] Electrochemical measurements: Electrochemical measurements were performed using a Bio-Logic SP300 potentiostat in a three-electrode cell configuration in an electrolyte that was continuously degassed by nitrogen bubbling. Electrocatalytic activity towards HER was evaluated in H2SO4 (0.5 M, pH 0.3) electrolyte used in a half-cell holder for the GDE configuration (Le Goff et al. Science 2009,326,1384-1387). The working electrode consisted of a GDL substrate with a deposited catalyst layer fixed in a half-cell holder. Gas was passed over the surface of the GDL to remove the generated H2. The pipe used to vent the gas was also used as the contact with the modified GDL. The counter electrode consisted of a Ti wire and the reference electrode was Ag / AgCl, KCl (3 M) (hereafter referred to as Ag / AgCl). Linear sweep voltammetry (LSV) technique was used to measure the electrocatalytic activity at a scan rate of 5 mV.s. -1 Polarization curves were recorded at 200 rpm and 25 °C. Stability tests were performed by chronopotentiometry (CP) measurements in N2-saturated or O2-saturated electrolyte for 24 h. The current density (cathodic current) was −10 mA cm -2 The constant applied current was related to the geometric area of ​​the working electrode to obtain the . Data extracted from the CP measurements were used to characterize the . x and a-MoS x The evolution of the overpotential for -P3HT was evaluated (ΔOP 10mAcm-2 / mV=OP 10mAcm-2 (t) / mV-OP 10mAcm-2 (t0) / mV).

[0068] All curves were IR-corrected by automatic ohmic drop compensation performed by Bio-Logic EC-Lab® software. The geometric area of ​​the electrodes (0.056 cm 2Current densities were normalized by matching to the Eq. (E = 1.0). All potentials were reported relative to the Reversible Hydrogen Electrode (RHE) potential using the following equation: E 対RHE =E 対Ag / AgCl -E Ag / AgCl対NHE +0.059×pH.

[0069] The electrochemically active surface area (ECSA) of the electrode is defined as the double layer capacitance (C DL ) was determined by electrochemical investigation (L(Lstrok)ukaszewski et al. Int. J. Electrochem. Sci., 11(2016)4442-4469). -1 Cyclic voltammograms were measured in a 300-mV LC-MS / MS (using Bio-Logic EC-Lab® software) at potentials in the range where faradaic processes are not observed to measure the capacitive current resulting from double layer charging. The capacitive current was plotted as a function of CV scan rate. These data were analyzed using a linear regression analysis with a slope of C DL Based on this value, the C of the electrode material was calculated. DL and specific capacitance C S The ECSA was calculated from the ratio (ECSA = C DL / C S ). C S Value 35μF cm -2 was used in the examples (McCrory et al. J. Am. Chem. Soc. 2015, 137, 4347-4357).

[0070] The roughness factor (RF) is the ratio of the electrochemically active surface area (ECSA) to the geometric area (RF = ECSA / S geom ).

[0071] FIG. 2 shows the results of two different batches of amorphous molybdenum sulfide catalysts (representative of the prior art) and a previously prepared composite material, a-MoS.x HER on .P3HT (a catalyst according to the invention) at a current density of 10 mA cm -2 The overvoltage (η 10 HER ) is a representative prior art a-MoS x 155 mV for the a-MoS catalyst, x The polarization curves in FIG. 2 show that for the composite material of the present invention, the polarization curves are 130 mV compared to the prior art a-MoS x The increase in potential is much smaller than with the catalyst, thus indicating improved stability.

[0072] Figure 3 shows the composite material a-MoS x 3 shows the polarization curves for HER on a-MoS-P3HT (a catalyst according to the present invention) (unwashed and washed with ethanol and water as described above). x -The overpotential η between the washed and unwashed forms of the P3HT catalyst 10 HER No significant difference was observed.

[0073] Figure 5 shows the tungsten sulfide catalyst and the composite material WS x -P3HT(20:1) and WS x Polarization curves for HER on -P3HT(40:1) at a current density of 10 mA cm per geometric area. -2 The overvoltage (η 10 HER ) is W.S. x 358mV for the catalyst, whereas WS x - 320 mV for P3HT(20:1) catalyst, WS x - 275 mV for P3HT (40:1) catalyst.

[0074] Figure 6 shows the cobalt-tungsten sulfide catalyst and the composite material CoWS. x -P3HT(20:1) and CoWS x Polarization curves for HER on -P3HT(40:1) at a current density of 10 mA cm per geometric area.-2 The overvoltage (η 10 HER ) is CoWS x 273mV for the catalyst, whereas CoS x - 236 mV for P3HT(20:1) catalyst, and 236 mV for CoWS x - 223 mV for P3HT (40:1) catalyst.

[0075] Figure 7 shows the iron-molybdenum sulfide catalyst and the composite material FeMoS x Polarization curves for HER on -P3HT(20:1) at a current density of 10 mA cm -2 The overvoltage (η 10 HER ) is 136 mV in both cases. Improvement of HER activity (relatively low η 10 HER Overvoltage equivalent to -10mA.cm -2 However, the composite FeMoS x At higher current densities, the composite FeMoS x Improved HER activity of Zn-P3HT(20:1) was observed, e.g., at a current density per geometric area of ​​50 mA cm -2 The overvoltage (η 50 HER ) is FeMoS x 206 mV for the FeMoS catalyst, x -For P3HT(20:1), it is 192mV.

[0076] Figure 8 shows the cobalt-molybdenum sulfide catalyst and the composite material CoMoS x Polarization curves for HER on -P3HT(20:1) at a current density of 10 mA cm -2 The overvoltage (η 10 HER ) is CoWS x 162 mV for the CoMoS catalyst x - 145 mV for P3HT (20:1) catalyst.

[0077] More features:

[0078] [Table 1]

[0079] The ECSA represents the surface area of ​​the electrode material that is accessible to the electrolyte and available for faradaic charge transfer. Dividing the ECSA by the geometric surface area of ​​the electrode gives the roughness factor, which is an intrinsic parameter of the electrode material.

[0080] Prior Art Amorphous a-MoS x In comparison with the catalyst, the composite material a-MoS x The roughness factor of -P3HT is three times higher at the same loading, which highlights that the higher organization and more catalytic sites accessible to the electrolyte can achieve catalysis and improved HER activity for the composite of the present invention.

[0081] Figure 9 shows the thermal expansion of a-MoS under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). x and a-MoS x The chronopotentiometry (CP) curves (stability test) of -P3HT are shown. 10mA.cm-2 To assess the evolution of the CP curves, data extracted from the CP curves are presented as bar graphs in Figures 10 and 11.

[0082] Figure 9a shows the a-MoS measured during continuous electrochemical H2 evolution for 24 h. x The performance of the catalyst is shown (potentiometry at 10 mA.cm -2 After 24 hours of electrolysis under suitable conditions, -2 (OP is an arbitrary unit for recording performance. 10mA.cm-2Using a-MoS, the potential E (V vs RHE) required to reach a solar-to-hydrogen conversion efficiency of 10% in the photoelectrochemical cell is increased by up to 20 mV. This increase in potential is also observed upon addition of O2 to the electrolyte and is found to be even higher (up to 35 mV after 24 h) (Figure 9c), which models the O2 crossover through the membrane of the electrolyzer during operation and the ingress of air while the electrolyzer is off in an accelerated test regime. x Overvoltage (stability test) vs. time (ΔOP 10mAcm-2 / mV=OP 10mAcm-2 (t) / mV-OP 10mAcm-2 (t0) / mV) (data extracted from Fig. 9(a,c)) are shown in Fig. 10. Fig. 9b and Fig. 9d show the same measurements carried out on a material according to the invention. Fig. 11 shows the change in the thermal conductivity of a-MoS during 24 hours of operation. x -P3HT overpotential (stability test) versus time (ΔOP 10mAcm-2 / mV=OP 10mAcm-2 (t) / mV-OP 10mAcm-2 (t0) / mV) (data extracted from Figure 9(b, d)). a-MoS x and a-MoS x a-MoS-P3HT shows almost the same stability in N2 saturated electrolyte. x a-MoS-P3HT shows improved stability in the presence of O2. The increase in potential in the presence of O2 indicates that a-MoS x 35 mV at 100 Hz, whereas it is significantly reduced (max. 20 mV) for the material according to the invention, indicating an improved stability of the composite material according to the invention.

[0083] Catalyst FeMoS x , W.S. x , and CoMoS x and the corresponding composite material FeMoS x -P3HT(20:1), WS x -P3HT(20:1), and CoMoS xA similar stability test was also performed with -P3HT(20:1).

[0084] FIG. 12 shows the thermal expansion of FeMoS under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). x and FeMoS x The chronopotentiometry (CP) curves (stability test) of -P3HT(20:1) are shown. 10mA.cm-2 To evaluate the evolution of the 10 mA cm -2 The potential E (V vs. RHE) required to reach x and FeMoS x -For P3HT(20:1), the maximum increase is 23 mV. -2 The potential E (V vs. RHE) required to reach x The increase was only up to 40 mV for FeMoS. x The increase in the charge transfer coefficient for FeMoS-P3HT(20:1) is only up to 25 mV. Thus, increased stability is observed for FeMoS-P3HT(20:1) in oxygen atmosphere. x Overvoltage (stability test) vs. time (ΔOP 10mAcm-2 / mV=OP 10mAcm-2 (t) / mV-OP 10mAcm-2 (t0) / mV) (data extracted from Fig. 12(a,c)) are shown in Fig. 13. x - Overpotential (stability test) vs. time (ΔOP 10mAcm-2 / mV=OP 10mAcm-2 (t) / mV-OP 10mAcm-2 (t0) / mV) (data extracted from Figure 12(b, d)) are shown in Figure 14.

[0085] FIG. 15 shows the WS2–O2–O3–O4–O4–O5–O6–O7–O8–O9–O10–O11–O12–O13–O14–O15–O16–O17–O18–O19–O20–O21–O22–O16–O17–O18–O19.x and W.S. x The chronopotentiometry (CP) curves (stability test) of -P3HT are shown. 10mA.cm-2 To evaluate the evolution of the CP curves, data extracted from the CP curves are shown as bar graphs in Figures 16 and 17. After electrolysis for 24 h under N2 saturated electrolyte, the CP curves were analyzed using a 10 mA cm -2 The potential E (V vs. RHE) required to reach WS x and W.S. x A similar increase (up to 33 mV) was observed for -P3HT(20:1). After 24 h of electrolysis in an O2-saturated electrolyte at 10 mA cm -2 The potential E (V vs. RHE) required to reach WS x The WS x The increase in stability is only 15 mV for WS-P3HT(20:1). x -P3HT(20:1). x Overvoltage (stability test) vs. time (ΔOP 10mAcm-2 / mV=OP 10mAcm-2 (t) / mV-OP 10mAcm-2 (t0) / mV) (data extracted from Fig. 15(a,c)) are shown in Fig. 16. x - Overpotential (stability test) vs. time (ΔOP 10mAcm-2 / mV=OP 10mAcm-2 (t) / mV-OP 10mAcm-2 (t0) / mV) (data extracted from Figures 15(b, d)) are shown in Figure 17.

[0086] FIG. 18 shows the thermal quenching properties of CoMoS under N2 saturated electrolyte (a, b) or O2 saturated electrolyte (c, d). x and CoMoS x The chronopotentiometry (CP) curves (stability test) of -P3HT(20:1) are shown. 10mA.cm-2To evaluate the evolution of the CP curves, data extracted from the CP curves are shown as bar graphs in Figures 19 and 20. After 24 h of electrolysis in N2-saturated electrolyte, the CP curves were analyzed using a 10 mA cm -2 The potential E (V vs. RHE) required to reach CoMoS x The increase is only up to 60 mV for CoMoS x -P3HT(20:1) increased by a maximum of 50 mV. After 24 h of electrolysis in an O2-saturated electrolyte, the -2 The potential E (V vs. RHE) required to reach CoMoS x The maximum increase is 55 mV for CoMoS. x The increase in the charge transfer coefficient for CoMoS-P3HT(20:1) is only up to 40 mV. Thus, increased stability is observed for CoMoS-P3HT(20:1) in oxygen atmosphere. x Overvoltage (stability test) vs. time (ΔOP 10mAcm-2 / mV=OP 10mAcm-2 (t) / mV-OP 10mAcm-2 (t0) / mV) (data extracted from Fig. 18(a,c)) are shown in Fig. 19. x - Overpotential (stability test) vs. time (ΔOP 10mAcm-2 / mV=OP 10mAcm-2 (t) / mV-OP 10mAcm-2 (t0) / mV) (data extracted from Figure 18(b, d)) are shown in Figure 20.

[0087] Fabrication of membrane-electrode assembly (MEA) for PEM electrolysis: A membrane-electrode assembly (MEA) was prepared using a Nafion® 212 membrane (50 μm thick) as the polymer electrolyte membrane and iridium black as the anode catalyst. x-P3HT was used as the cathode catalyst. For the preparation of the cathode, the catalyst was mixed with carbon Vulcan XC72R (Cabot). A catalyst ink was prepared using an ethanol / water solution and a Nafion® perfluorinated resin solution (5 wt% solution, Sigma-Aldrich). The catalyst ink solution was sonicated for 1 h using an ultrasonic bath before deposition.

[0088] The anode catalyst ink was deposited on a transfer substrate (PTFE-coated fiberglass cloth, Plastic Elastomer) until a predefined catalyst content was reached. The cathode catalyst ink was deposited on a non-catalyzed gas diffusion layer (GDL, Sigracet 39BC, SGL Group-The Carbon Company) until a predefined catalyst content was reached. The as-prepared electrode and the coated transfer substrate were assembled with a Nafion® 212 membrane between them and subjected to hot welding at 120° C. and 5 MPa for 1 min 30 s. After the hot welding was stopped, the transfer substrate was peeled off to transfer the anode catalyst to one side of the Nafion® 212 membrane.

[0089] The as-prepared MEA was further incorporated into a single cell proton exchange membrane (PEM) electrolyzer. The measured polarization curve of the MEA is shown in Figure 4. At 80 °C, a remarkable electrochemical performance was obtained, with a current of 0.5 mA cm -2 It takes 1.75 V to reach 1 mA cm -2 It took 1.83V to reach this.

Claims

1. Amorphous (binary) metal sulfide nanoparticles; Sulfur-containing polymers and wherein the amorphous (binary) metal sulfide nanoparticles are directly bonded to the sulfur-containing polymer by coordinate covalent bonds; A composite material, wherein the metal of said amorphous (binary) metal sulfide nanoparticles is selected in the group consisting of Mo, V, and W.

2. 2. The composite material of claim 1, wherein the metal of the amorphous (binary) metal sulfide nanoparticles is combined with another element selected in the group consisting of Mo, V, W, Ti, Cr, Mn, Fe, Co, Ni, Cu, Nb, Ta, Co, Cu, Fe, Ni, V, Nb, Ta.

3. 2. The composite material of claim 1, wherein the amorphous (binary) metal sulfide nanoparticles are amorphous single metal sulfide nanoparticles, and the metal is selected from the group consisting of Mo, V, and W.

4. 3. The composite material of claim 1 or claim 2, wherein the amorphous (binary) metal sulfide nanoparticles are amorphous binary metal sulfide nanoparticles, the metals of the amorphous binary metal sulfide nanoparticles being different from each other and selected in the group consisting of Mo, V, and W in combination with another element selected in the group consisting of Mo, V, W, Ti, Cr, Mn, Fe, Co, Ni, Cu, Nb, Ta, Co, Cu, Fe, Ni, V, Nb, Ta.

5. The amorphous (binary) metal sulfide nanoparticles are a-CoMoS x Nanoparticles, a-FeMoS x Nanoparticles and a-CoWS x 5. The composite material of claim 4, which is an amorphous bimetallic sulfide nanoparticle selected from the group consisting of nanoparticles.

6. 6. The composite material of claim 1, wherein the sulfur-containing polymer is selected from the group consisting of polythiophene, poly(ethylenedioxythiophene), polyphenylene sulfide, and mixtures thereof.

7. The composite material according to any one of claims 1 to 6, wherein the sulfur-containing polymer is poly(3-hexylthiophene-2,5-diyl) (P3HT).

8. The sulfur-containing polymer has a molecular weight of 5,000 to 100,000 g.mol -1 The composite material according to any one of claims 1 to 7, having a number average molecular weight in the range of

9. 9. The composite material according to any one of claims 1 to 8, wherein said amorphous (binary) metal sulphide nanoparticles are formed of (binary) metal sulphide clusters, the number of said (binary) metal sulphide clusters being in the range of 2 to 40.

10. 10. The composite material of claim 9, wherein the amorphous (binary) metal sulfide clusters have a particle size based on number Dn90 in the range of 0.1 to 2 nm.

11. The composite material according to any one of claims 1 to 10, wherein the composite material has a number-based size Dn90 in the range of 1 to 100 nm.

12. 12. A composite material according to any one of claims 1 to 11, wherein the amount of metal in the amorphous (binary) metal sulphide nanoparticles is between 20 and 75% by weight.

13. 13. The composite material according to any one of claims 1 to 12, wherein the amount of S in the amorphous (binary) metal sulfide nanoparticles is 25 to 80 wt.%.

14. 14. The composite material according to any one of claims 1 to 13, wherein the mass ratio of the amorphous (binary) metal sulfide nanoparticles to the sulfur-containing polymer is in the range of 1:1 to 100:

1.

15. A process for the preparation of a composite material according to any one of claims 1 to 14, comprising the steps of: (i) preparing amorphous (binary) metal sulfide nanoparticles; (ii) dispersing the amorphous (binary) metal sulfide nanoparticles obtained in step (i) in a solution of a sulfur-containing polymer under stirring, thereby forming coordinate covalent bonds between the sulfur-containing polymer and the metal ions of the amorphous (binary) metal sulfide nanoparticles obtained in step (i).

16. 16. The process of claim 15, wherein the amorphous (binary) metal sulfide nanoparticles are prepared in step (i) by reacting a metal salt with a sulfur-containing compound and then heating the resulting mixture.

17. 16. The process of claim 15, wherein the amorphous (binary) metal sulfide nanoparticles are prepared in step (i) by redox reaction of thiometallate ions with an oxidant selected from the group consisting of sodium persulfate, potassium persulfate, sodium permanganate, potassium permanganate, sodium percarbonate, sodium dichromate, potassium dichromate, cerium nitrate.

18. The concentration of the sulfur-containing polymer in the solution in step (ii) is 0.05 to 1 g.mol -1 The process according to any one of claims 15 to 17, wherein

19. 19. The process according to any one of claims 15 to 18, further comprising a step (iii) of washing the composite material obtained in step (ii) with a solvent selected in the group consisting of water, diethyl ether, C1-C6 alcohols, and mixtures thereof.

20. Use of a composite material according to any one of claims 1 to 14 as a catalyst for hydrogen production in a proton exchange membrane (PEM) electrolyser or in a photoelectrochemical cell.

21. A proton exchange membrane (PEM) electrolyser comprising the composite material according to any one of claims 1 to 14.

22. A photoelectrochemical cell comprising the composite material according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Sliding material in oil and oil sealing ring

    JP1997291297A

  • Method of manufacturing electrode

    JP2011077044A

  • Photoelectrochemical cells

    US20190017184A1