β-type sialon phosphor particles and light-emitting device

By defining a specific Si concentration gradient in β-sialon phosphor particles through a two-stage firing process and acid treatment, brightness and stability are enhanced, addressing the need for improved β-sialon phosphors in light-emitting devices.

JP7588075B2Active Publication Date: 2024-11-21DENKA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021540766
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-20
Filing Date
2020-08-14
Publication Date
2024-11-21
Estimated Expiration
2040-08-14

Smart Images

  • Figure 0007588075000004
    Figure 0007588075000004
  • Figure 0007588075000005
    Figure 0007588075000005
  • Figure 0007588075000001
    Figure 0007588075000001
Patent Text Reader

Abstract

The β-sialon phosphor particles according to the present invention have europium incorporated in solid solution. If the element concentration of Si atoms in the surface portion of the phosphor particles found by analysis of a cross section of said particles with energy-dispersive X-ray spectroscopy is defined as Ps (at%), and the element concentration of Si atoms near the center of said particles found by analysis using the same method is defined as Pc (at%), the value of Pc − Ps is 3 at% or greater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to β-sialon phosphor particles and a light-emitting device.

[0002] A light-emitting device in which a light-emitting element that emits primary light and a phosphor that absorbs the primary light and emits secondary light are combined is known. In recent years, with the increase in the output of light-emitting devices, the requirements for the heat resistance and durability of phosphors have been increasing. For this reason, β-sialon phosphors with a stable crystal structure have attracted attention.

[0003] A phosphor in which Eu 2+ is dissolved in the crystal structure of β-sialon is a phosphor that is excited by ultraviolet to blue light and exhibits green light emission with a wavelength of 520 nm or more and 550 nm or less. β-sialon in which Eu 2+ is dissolved is also called Eu-doped β-sialon. This phosphor is used as a green light-emitting component of a light-emitting device such as a white light-emitting diode (white LED (Light Emitting Diode)). Eu-doped β-sialon has a very sharp emission spectrum among the phosphors in which Eu 2+ is dissolved. Therefore, Eu-doped β-sialon is a phosphor particularly suitable for the green light-emitting component of a backlight light source of a liquid crystal display panel that requires narrow-band light emission composed of the three primary colors of blue, green, and red light.

[0004] As a technique related to β-sialon phosphors, for example, those described in Patent Document 1 can be mentioned. Patent Document 1 describes a β-sialon represented by the general formula: Si 6-Z Al Z O Z N 8-Z (0 < Z ≦ 0.42), which is a β-sialon in which Eu is dissolved, and the 50% area average diameter of the primary particles of the β-sialon is 5 μm or more.

Prior Art Documents

Patent Documents

[0005] [Patent Document 1] International Publication No. 2012 / 011444 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, there has been a demand for further improvement in brightness of β-sialon phosphors and light emitting devices. The present invention has been made in view of the above circumstances and provides a β-sialon phosphor and a light emitting device with improved luminance. [Means for solving the problem]

[0007] The present inventors have carried out various studies to improve the brightness, and as a result of the studies, have completed the invention provided below.

[0008] According to the present invention, A β-type sialon phosphor particle having europium dissolved therein, When the elemental concentration of Si atoms in the surface portion of the phosphor particle, which is obtained by analyzing the cross section of the phosphor particle by energy dispersive X-ray analysis, is Ps [at%], and the elemental concentration of Si atoms near the center of the phosphor particle, which is obtained by analyzing the cross section by the same method, is Pc [at%], β-type sialon phosphor particles with a Pc-Ps value of 3 at% or more is provided.

[0009] Further, according to the present invention, A light emitting device including a light emitting source and a wavelength conversion member, The wavelength conversion member includes a phosphor, A light emitting device, wherein the phosphor contains the above-mentioned β-type SiAlON phosphor particles. is provided. Effect of the Invention

[0010] According to the present invention, there are provided β-sialon phosphor particles and a light emitting device with improved luminance. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic example of the structure of a light-emitting device. [Diagram 2] FIG. 2 is a diagram for explaining measurement points in energy dispersive X-ray analysis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The drawings are for illustrative purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.

[0013] In this specification, the term "approximately" means that a range taking into consideration manufacturing tolerances, assembly variations, and the like, is included, unless otherwise specified explicitly.

[0014] <β-type SiAlON phosphor particles> The β-sialon phosphor particles of this embodiment are β-sialon phosphor particles containing europium as a solid solution. When the elemental concentration of Si atoms on the surface of the phosphor particle, determined by analyzing the cross section of the phosphor particle using energy dispersive X-ray analysis (also abbreviated as EDX), is defined as Ps [at%], and the elemental concentration of Si atoms near the center of the phosphor particle, determined by analysis using the same method, is defined as Pc [at%], the value of Pc-Ps is 3 at% or more.

[0015] Just to be clear, in this embodiment, attention is focused on the relationship between Pc and Ps when a cut surface of a primary particle or a secondary particle (preferably a primary particle) is analyzed by an EDX method. A primary particle is a single particle that cannot be broken down even by a considerable mechanical stress. An aggregate of primary particles is called a secondary particle. Primary particles can be either single crystals or polycrystals.

[0016] The β-sialon phosphor of this embodiment is, for example, represented by the general formula Si 6-z Al z O z N 8-z :Eu 2+ (0 < Z ≤ 4.2), and is a phosphor composed of β-sialon in which Eu 2+ is dissolved. Hereinafter, β-sialon in which europium is dissolved is also simply referred to as β-sialon. In the general formula Si 6-z Al z O z N 8-z :Eu 2+ , the Z value and the europium content are not particularly limited. The Z value is, for example, more than 0 and 4.2 or less, and from the viewpoint of further improving the emission intensity of the β-sialon phosphor, it is preferably 0.005 or more and 1.0 or less. Also, the europium content is preferably 0.1 mass% or more and 2.0 mass% or less.

[0017] In the β-sialon phosphor particles of this embodiment, when the value of Pc - Ps is 3 at% or more, that is, when the Si concentration near the center is high and the Si concentration on the surface portion is low, the luminance is improved. The reason for this is not necessarily clear, but it is presumed as follows, for example. As the finding of the present inventors, Si tends to absorb light in a wide wavelength range from ultraviolet to visible. Therefore, it is presumed that when Si generated particularly by partial decomposition of β-sialon or a compound formed from Si is present on the surface of the phosphor particles, the luminance will be significantly reduced. Therefore, as in this embodiment, it is considered that the luminance is improved because the amount of Si that does not contribute to emission is small in the surface portion of the phosphor particles.

[0018] In order to obtain the β-SiAlON phosphor of this embodiment, it is preferable to select an appropriate manufacturing method in addition to the selection of appropriate raw materials. For example, a β-SiAlON phosphor having a Pc-Ps value of 3 at% or more can be obtained by performing two-stage firing, that is, a first firing step and a second firing step described later, and / or performing an acid treatment as a post-firing treatment.

[0019] The β-sialon phosphor particles of this embodiment will be described in more detail below.

[0020] (About Ps and Pc) The Ps content is preferably 20 at % or more and 35 at % or less, and more preferably 22 at % or more and 35 at % or less. Pc is preferably 23 at % or more and 50 at % or less, more preferably 30 at % or more and 50 at % or less, and further preferably 35 at % or more and 45 at % or less.

[0021] The difference between Pc and Ps (Pc-Ps) is at least 3 at%, more preferably at least 5 at%, and even more preferably at least 6.5 at%. By designing the difference between Pc and Ps to be sufficiently large, the brightness can be further increased. From the viewpoint of practical design etc., the difference between Pc and Ps is usually at most 20 at %, preferably at most 17.5 at %, and more preferably at most 15 at %.

[0022] (Abundance of elements other than Si) The β-SiAlON phosphor particles of this embodiment are "SiAlON", and therefore generally contain Al, O, and N in addition to Si. The β-SiAlON phosphor particles of this embodiment also contain Eu. The chemical composition according to the general formula is as described above. For the sake of completeness, the preferred ratios of each element other than Si in the surface and center of the phosphor particle are listed below. It is believed that brightness will be further improved if these ratios are within appropriate ranges. These ratios can also be determined by the EDX method.

[0023] - Ratio of each element on the surface of the phosphor particle Al: preferably 0.05 at % or more and 10 at % or less, more preferably 0.2 at % or more and 7.5 at % or less, and further preferably 0.3 at % or more and 5 at % or less Eu: preferably 0.01 at% or more and 1 at% or less, more preferably 0.02 at% or more and 0.75 at% or less, and further preferably 0.02 at% or more and 0.5 at% or less N: preferably 40 at % or more and 75 at % or less, more preferably 45 at % or more and 70 at % or less O: preferably 5 at% or more and 25 at% or less, preferably 10 at% or more and 20 at% or less, more preferably 12 at% or more and 18 at% or less, further preferably 12 at% or more and 17 at% or less

[0024] - Ratio of each element near the center of the phosphor particle Al: preferably 0.1 at% or more and 5 at% or less, more preferably 0.5 at% or more and 5 at% or less, further preferably 0.5 at% or more and 4 at% or less Eu: preferably 0.01 at% or more and 0.5 at% or less, more preferably 0.02 at% or more and 0.3 at% or less, and further preferably 0.02 at% or more and 0.2 at% or less. N: preferably 45 at % or more and 65 at % or less, more preferably 50 at % or more and 60 at % or less O: preferably 1 at% or more and 10 at% or less, more preferably 1 at% or more and 7.5 at% or less, further preferably 1 at% or more and 6 at% or less

[0025] (Supplementary information on the EDX method) In this embodiment, the "cross section" of the β-sialon phosphor particle is exposed and analyzed by the EDX method to determine Ps, Pc, and the like.

[0026] The cross-section of the phosphor particles can be exposed by applying a known ion milling method (more specifically, cross-section milling method). That is, the particle cross-section can be exposed by irradiating the sample with ions accelerated by an electric field to flick off atoms on the sample surface.

[0027] The EDX method is a technique for elemental and compositional analysis by detecting characteristic X-rays generated by electron beam irradiation and dispersing them by energy. Since characteristic X-rays have specific energies depending on the element, elemental analysis can be performed by measuring these. Energy dispersive X-ray analysis equipment is often attached to a scanning electron microscope (SEM) or a transmission electron microscope (TEM), so that the location (surface or core) for elemental analysis can be determined by viewing the SEM or TEM image.

[0028] When measuring Pc, it is sufficient to measure the elemental concentration of Si atoms "near" the center of the phosphor particle, and it is not necessary to measure the elemental concentration at the exact "center" (geometric center of gravity, etc.). Common sense dictates that it is sufficient to measure the elemental concentration in a portion that is sufficiently inside the particle than the surface. Similarly, when measuring Ps, it is not necessary to measure the elemental concentration at the exact "particle surface". It is sufficient to measure the elemental concentration in a portion that is sufficiently close to the particle surface. Considering the presumed mechanism of action mentioned above, that "brightness is thought to be improved due to the small amount of Si that does not contribute to light emission on the surface of the phosphor particle," it is believed that a sufficient brightness improvement effect can be obtained even if the element concentrations at the "center" and "surface" are not measured precisely, by measuring the Si element concentration Pc 'near' the center and the Si element concentration Ps on the surface and confirming that Pc-Ps is 3 at% or more.

[0029] As for Ps, it is sufficient that Ps measured at at least one point on the surface of the phosphor particle satisfies the relationship Pc-Ps≧3at%. In other words, when the concentration of Si atoms is measured at several points on the surface of the phosphor particle and the smallest value among them is taken as Ps, it is sufficient that the value of Pc-Ps is 3at% or more. Although it is possible that the value of Ps is not uniform across the entire surface of a phosphor particle, if the elemental concentration of Si atoms in at least a part of the surface of the phosphor particle is sufficiently lower than that near the center, then the brightness improvement effect can be obtained at least in that part.

[0030] In this embodiment, Pc and Ps are measured for at least one randomly selected β-SiAlON phosphor particle, and it is sufficient that Pc and Ps satisfy a predetermined relationship. If one particle in an assembly of β-SiAlON phosphor particles manufactured using the same raw materials and manufacturing method satisfies the predetermined relationship between Pc and Ps, then the assembly should contain a considerable amount of particles (although not all other particles) that satisfy the predetermined relationship between Pc and Ps in addition to that one particle.

[0031] (particle size) The β-sialon phosphor particles of this embodiment have an appropriate particle size, so that the brightness can be further increased. Specifically, the 50% diameter D of the β-type SiAlON phosphor particles of this embodiment (more precisely, phosphor powder containing the β-type SiAlON phosphor particles of this embodiment) in terms of the volume-based cumulative fraction V50 (volume-based median diameter) is preferably 5 μm or more, more preferably 10 μm or more. V50 The upper limit is preferably 50 μm, more preferably 30 μm. D V50 can be determined by a laser diffraction scattering method in accordance with JIS R 1629:1997. V50 When measuring the particle size distribution, it is preferable to carry out pretreatment such as dispersion treatment using an ultrasonic homogenizer to minimize particle aggregation. For specific conditions of the pretreatment and details of the measuring device, please refer to the Examples given later. From another perspective, the primary particle diameter (equivalent circle diameter) of the β-sialon phosphor particles of this embodiment, as obtained by observing them with a scanning electron microscope, is preferably 5 μm or more and 50 μm or less, and more preferably 10 μm or more and 30 μm or less.

[0032] The β-sialon phosphor particles of this embodiment are excited by a wide wavelength range from ultraviolet light to visible light, and emit green light with a main wavelength in the range of 520 nm to 550 nm with high efficiency, making them excellent as green-emitting phosphors. In addition, the β-SiAlON phosphor particles of this embodiment can be suitably used as a material for a phosphor layer in a light-emitting element. The light-emitting element can be applied to a light-emitting device such as a backlight source for a display or a lighting device. The light-emitting element is not particularly limited, but includes an LED and a phosphor layer laminated on the light-emitting surface side of the LED. As the LED, an ultraviolet LED or a blue LED that emits light with a wavelength of 300 nm or more and 500 nm or less, particularly a blue LED that emits light with a wavelength of 440 nm or more and 480 nm or less, can be used. In particular, the β-SiAlON phosphor particles obtained by the manufacturing method described below are excited by a wide range of wavelengths from ultraviolet to blue light and exhibit high-luminance green light emission, and therefore can be suitably used as a phosphor for a white LED that uses blue or ultraviolet light as a light source.

[0033] (Manufacturing method) As briefly described above, the β-sialon phosphor particles of this embodiment are manufactured by selecting appropriate raw materials and an appropriate manufacturing method. Specifically, the β-type sialon phosphor particles of this embodiment can be obtained by adopting manufacturing process innovations such as adding one of the raw materials, a europium compound, in two or more batches and performing a firing process, adding a sufficiently large amount of europium compound in the second firing process, performing an annealing process, and performing an acid treatment after firing. However, on the premise that these manufacturing techniques are adopted, various other specific manufacturing conditions can be adopted for the β-sialon phosphor particles of this embodiment.

[0034] The method for producing the β-sialon phosphor particles will now be described in more detail. The method for producing β-SiAlON phosphor particles of this embodiment preferably includes two firing steps. That is, the method for producing β-SiAlON phosphor particles of this embodiment preferably includes the following steps: (i) a first firing step of firing a first raw powder containing a first europium compound to obtain a first fired powder containing β-sialon particles; (ii) a second firing step of firing the obtained first fired powder and a second raw material powder containing a second europium compound to obtain the β-sialon phosphor particles of the present embodiment; Includes. Here, in the second firing step, it is preferable to add the second europium compound in an amount larger than the conventional standard. Specifically, in the second firing step, it is preferable to add the second europium compound so that the amount of Eu is in excess of the amount of Eu that can be dissolved in the β-sialon.

[0035] Although the details are unclear, it is believed that by adding a second europium compound in the second firing step so that the amount of Eu is in excess of the amount that can be dissolved in β-SiAlON, the element distribution will be different between the surface layer and the interior of the phosphor particles, and this will enable the production of a β-SiAlON phosphor with a desired relationship between Pc and Ps.

[0036] The method for producing β-sialon phosphor particles may further include one or more third firing steps in which the second fired powder is further fired to obtain a third fired powder, and in this step, a europium compound may be further added.

[0037] Here, in this embodiment, the "first firing step" refers to the first firing step in which a raw material powder containing a first europium compound is heat-treated, the "second firing step" refers to the second firing step in which a second europium compound is added and heat-treated, and the "third firing step" refers to a firing step carried out after the second firing step. In addition, in this embodiment, the "first europium compound" means the europium compound added in the first firing step, and the "second europium compound" means the europium compound added in the second firing step. In the present embodiment, the term "first raw material powder" refers to the raw material powder used in the first firing step, and the term "second raw material powder" refers to the raw material powder used in the second firing step. It is preferable that the respective raw material powders are mixed. In addition, in this embodiment, "first calcined powder" means the product obtained in the first calcination process, "second calcined powder" means the product obtained in the second calcination process, and "third calcined powder" means the product obtained in the third calcination process.

[0038] In the present embodiment, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. When multiple substances corresponding to europium are present in the composition, the content of europium in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified.

[0039] The first raw material powder preferably contains silicon nitride and aluminum nitride in addition to the first europium compound. The silicon nitride and aluminum compounds are materials for forming the skeleton of the β-sialon, and the europium compound is a material for forming the luminescence center. The first raw material powder may further contain β-sialon. The β-sialon is a material that serves as an aggregate or a core. The form of each of the above components contained in the first raw powder is not particularly limited, but each is preferably in powder form.

[0040] The europium compound that can be used is not particularly limited. For example, there can be mentioned oxides containing europium, hydroxides containing europium, nitrides containing europium, oxynitrides containing europium, halides containing europium, etc. These can be used alone or in combination of two or more. Among these, it is preferable to use europium oxide, europium nitride, and europium fluoride alone, and it is more preferable to use europium oxide alone.

[0041] The europium compound is preferably added separately before each of the multiple firing steps, specifically, before each of the first and second firing steps.

[0042] In each firing step, europium is divided into those that dissolve in the β-sialon, those that volatilize, and those that remain as hetero-phase components. The hetero-phase components containing europium can be removed by acid treatment or the like. However, if too much is produced, insoluble components may be produced by acid treatment, which may reduce brightness. On the other hand, if the hetero-phase does not absorb excess light, such a hetero-phase may remain, and europium may be contained in this hetero-phase. When a europium compound is added before firing in multiple firing steps, a β-sialon phosphor raw material other than the europium compound may be added together with the europium compound.

[0043] In the method for producing β-sialon phosphor particles, when the total of the first fired powder and the second europium compound is 100 mass%, from the viewpoint of more effectively removing Eu that does not contribute to improving the brightness of the β-sialon phosphor particles and more effectively improving the brightness of the obtained β-sialon phosphor particles, the ratio of the second europium compound is preferably 1.0 mass% or more, more preferably 2.0 mass% or more, and even more preferably 3.0 mass% or more. Also, from the viewpoint of reducing the amount of insoluble hetero-phase components generated by the acid treatment and more effectively improving the brightness of the obtained β-sialon phosphor particles, the ratio of the second europium compound is preferably 18.0 mass% or less, more preferably 17.0 mass% or less, and even more preferably 15.0 mass% or less. In the manufacturing method of the β-sialon phosphor particles of this embodiment, when the ratio of the second europium compound is within the above range, Eu that does not contribute to improving the brightness of the β-sialon phosphor can be more effectively removed, and the generation of heterophase components that are insoluble in acid treatment can be suppressed. Therefore, the manufacturing process for removing the heterophase components can be simplified, and as a result, the manufacturing time of the β-sialon phosphor particles can be shortened.

[0044] The total amount of europium contained in the first raw powder and the second raw powder is not particularly limited, but is preferably at least three times, and more preferably at least four times, the amount of europium dissolved in the final β-sialon phosphor particles. Moreover, the total amount of europium contained in the first raw material powder and the second raw material powder is preferably 18 times or less the amount of europium dissolved in the finally obtained β-sialon phosphor, which can reduce the amount of insoluble heterogeneous phase components generated by the acid treatment and further improve the brightness of the obtained β-sialon phosphor.

[0045] The amount of europium contained in the first raw material powder is not particularly limited, but it is preferable that this amount is greater than the amount of europium dissolved in the final β-sialon phosphor. Moreover, the amount of europium contained in the first raw powder is preferably three times or less than the amount of europium dissolved in the finally obtained β-sialon phosphor particles, which can reduce the amount of insoluble hetero-phase components generated by the acid treatment and further improve the brightness of the obtained β-sialon phosphor particles.

[0046] In each firing step, the raw material powder containing the europium compound can be obtained by, for example, a dry mixing method, or a wet mixing method in an inert solvent that does not substantially react with each component of the raw material and then removing the solvent, etc. The mixing device is not particularly limited, but for example, a V-type mixer, a rocking mixer, a ball mill, a vibration mill, etc. can be used.

[0047] The firing temperature in each firing step is not particularly limited, but is preferably in the range of 1800° C. or higher and 2100° C. or lower. By setting the firing temperature at 1800° C. or higher, grain growth proceeds more effectively, and the light absorption rate, internal quantum efficiency, and external quantum efficiency can be further improved. By setting the firing temperature at 2100° C. or less, decomposition of the phosphor can be sufficiently suppressed, and the light absorptance, internal quantum efficiency, and external quantum efficiency can be further improved. Other conditions such as the temperature rise time, temperature rise rate, heating retention time, and pressure in each firing step are also not particularly limited. These conditions may be appropriately adjusted depending on the raw materials used, etc. Typically, the heating retention time is 3 hours or more and 30 hours or less, and the pressure is 0.6 MPa or more and 10 MPa or less.

[0048] In each firing step, the mixture can be fired, for example, by filling the mixture into a container made of a material that does not react with the mixture during firing (e.g., boron nitride) and heating it in a nitrogen atmosphere. By using such a method, crystal growth reactions and solid-solution reactions can be promoted to obtain β-SiAlON phosphor particles.

[0049] The first fired powder and the second fired powder are granular or agglomerated sintered bodies, which can be processed into β-sialon phosphor particles of a predetermined size by crushing, grinding, classifying, or other processes, either alone or in combination. A specific processing method is, for example, a method of pulverizing the sintered body to a predetermined particle size using a general pulverizer such as a ball mill, a vibration mill, or a jet mill. However, excessive pulverization may not only produce fine particles that easily scatter light, but may also cause crystal defects on the particle surface. In other words, it should be noted that excessive pulverization may cause a decrease in the luminous efficiency of the β-SiAlON phosphor particles. Incidentally, this processing may be performed after the acid treatment or alkali treatment described later.

[0050] The method for producing β-sialon phosphor particles may further include, after the second firing step, an annealing step of heating the second fired powder at a temperature lower than the firing temperature of the second firing step to obtain an annealed product. The annealing step is preferably carried out in a non-oxidizing atmosphere other than pure nitrogen, such as an inert gas, such as a rare gas or nitrogen gas, a reducing gas, such as hydrogen gas, carbon monoxide gas, hydrocarbon gas, or ammonia gas, or a mixture of these gases, or in a vacuum, etc. It is particularly preferably carried out in a hydrogen gas atmosphere or an argon atmosphere. The annealing step may be carried out either at atmospheric pressure or under elevated pressure. The heat treatment temperature in the annealing step is not particularly limited, but is preferably 1200° C. or higher and 1700° C. or lower, and more preferably 1300° C. or higher and 1600° C. or lower. By carrying out the annealing process, the luminous efficiency of the β-SiAlON phosphor particles can be further improved, and the transparency can also be improved since the rearrangement of the elements removes distortions and defects. Incidentally, a heterogeneous phase may be generated during the annealing process, but this can be removed by an acid treatment or the like, which will be described later.

[0051] Before the annealing step, a compound of an element constituting the β-SiAlON phosphor particles may be added and mixed in. The compound to be added is not particularly limited, but examples thereof include oxides, nitrides, oxynitrides, fluorides, chlorides, etc. of each element. In particular, the luminance of the β-sialon phosphor can be further improved by adding silica, aluminum oxide, europium oxide, europium fluoride, etc. to each heat-treated product. However, it is preferable that the undissolved residue of the added raw material can be removed by acid treatment or alkali treatment after the annealing step.

[0052] In the method for producing β-sialon phosphor particles, a step of treating the second fired powder or the annealed product of the second fired powder with an acid, an alkali and / or a fluorine may be further carried out. The acid treatment or alkali treatment is, for example, a treatment in which an acidic or alkaline liquid is brought into contact with the second fired powder or the annealed product of the second fired powder, and the fluorine treatment is, for example, a step in which a fluorine-containing gas is brought into contact with the second fired powder or the annealed product of the second fired powder. It is believed that by carrying out such a process, it is possible to dissolve and remove the heterogeneous phase components (luminescence inhibitors) that are generated during the firing process, annealing process, etc. Therefore, it is possible to further improve the light absorption rate, internal quantum efficiency, and external quantum efficiency of the β-SiAlON phosphor particles. In addition, it is believed that by appropriately removing the Si near the surface of the particles, it becomes easier to manufacture particles in which Pc and Ps have the desired relationship.

[0053] The acidic liquid may be, for example, an aqueous solution containing one or more acids selected from hydrofluoric acid, sulfuric acid, phosphoric acid, hydrochloric acid, and nitric acid. The alkaline liquid may be, for example, an aqueous solution containing one or more alkalis selected from potassium hydroxide, ammonia water, and sodium hydroxide, but an acidic aqueous solution is more preferable, and a mixed aqueous solution of hydrofluoric acid and nitric acid is particularly preferable.

[0054] The treatment method using an acidic or alkaline liquid is not particularly limited, but can be carried out by dispersing the second fired powder or the annealed product of the second fired powder in an aqueous solution containing an acid or an alkali, and stirring for several minutes to several hours (for example, 10 minutes to 6 hours). A known stirrer or the like can be used for stirring. The temperature during stirring is, for example, 50 to 100°C, preferably 65 to 85°C (the liquid is maintained at this temperature). The stirring time is, for example, 1 minute to 2 hours, preferably about 10 minutes to 1 hour. The stirring speed is, for example, 300 to 600 rpm, preferably 400 to 500 rpm. After this treatment, it is preferable to separate substances other than the β-sialon phosphor particles by filtration, and to wash away the substances adhering to the β-sialon phosphor with water.

[0055] <Light emitting device> The light emitting device of this embodiment is a light emitting device including a light source and a wavelength conversion member. The wavelength conversion member includes a phosphor. The phosphor includes the β-SiAlON phosphor particles of this embodiment (the β-SiAlON phosphor particles described above).

[0056] FIG. 1 is a cross-sectional view showing a schematic example of the structure of a light emitting device 10. As shown in FIG. 1 is formed of an LED chip as a light emitting source 12, a first lead frame 13 on which the light emitting source 12 is mounted, a second lead frame 14, a wavelength conversion member 15 that covers the light emitting source 12, a bonding wire 16 that electrically connects the light emitting source 12 and the second lead frame 14, and a synthetic resin cap 19 that covers these. The wavelength conversion member 15 has a phosphor 18 and a sealing resin 17 in which the phosphor 18 is dispersed.

[0057] A recess 13b is formed in the upper portion 13a of the first lead frame 13 for mounting a light emitting diode chip as the light emitting source 12. The recess 13b has a generally funnel shape with a hole diameter gradually increasing from the bottom surface toward the top, and the inner surface of the recess 13b serves as a reflective surface. An electrode on the lower surface of the light emitting source 12 is die-bonded to the bottom surface of this reflective surface. The other electrode formed on the upper surface of the light emitting source 12 is connected to the surface of the second lead frame 14 via a bonding wire 16.

[0058] Various LED chips can be used as the light emitting source 12. Particularly preferred is an LED chip that emits light with a wavelength of 300 nm or more and 500 nm or less, which is from near ultraviolet to blue light.

[0059] The phosphor 18 used in the wavelength conversion member 15 of the light emitting device 10 includes the β-sialon phosphor particles of this embodiment. From the viewpoint of controlling the light wavelength of the light emitting device 10, the phosphor 18 may further include phosphors such as an α-sialon phosphor, a KSF phosphor, CaAlSiN3, or a mixture of YAG, in addition to the β-sialon phosphor particles of this embodiment. Examples of elements that are dissolved in these phosphors include europium (Eu), cerium (Ce), strontium (Sr), calcium (Ca), and manganese (Mn). These phosphors may be used alone or in combination of two or more. Among these, the phosphor to be used in combination with the β-SiAlON phosphor particles of the present embodiment is preferably a KSF phosphor with manganese as a solid solution. By using the β-SiAlON phosphor of the present embodiment that shows green in combination with a KSF phosphor that shows red, it can be suitably used as a backlight LED suitable for high color rendering TVs, for example. By combining the light emitting source 12 and the wavelength conversion member 15, it is possible to emit light having a high emission intensity. Just to be clear, KSF phosphors containing manganese in solid solution have the general formula: A2M (1-n) F6:Mn 4+ n In this general formula, the element A is one or more alkali metal elements containing K, the element M is Si alone, Ge alone, or a combination of Si and one or more elements selected from the group consisting of Ge, Sn, Ti, Zr, and Hf, and 0 <n≦0.1である。

[0060] In the case of the light emitting device 10 using the β-SiAlON phosphor particles of this embodiment, by irradiating near-ultraviolet light or visible light containing a wavelength of 300 nm or more and 500 nm or less as an excitation source as the light emission source 12, the device has green light emission characteristics having a peak in a wavelength range of 520 nm or more and 550 nm or less. Therefore, by using a near-ultraviolet LED chip or a blue LED chip and the β-SiAlON phosphor of this embodiment as the light emission source 12, and further combining it with a single substance or a mixture of a red light emitting phosphor, a blue light emitting phosphor, a yellow light emitting phosphor, or an orange light emitting phosphor having a wavelength of 600 nm or more and 700 nm or less, it is possible to produce white light.

[0061] The light emitting device 10 has good brightness since it contains β-sialon phosphor particles with improved emission intensity.

[0062] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0063] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples.

[0064] Example 1 Using a V-type mixer (Tsutsui Rikagaku Kikai S-3), 95.80 mass% of α-type silicon nitride powder (SN-E10 grade, oxygen content 1.0 mass%) manufactured by Ube Industries, 2.74 mass% of aluminum nitride powder (F grade, oxygen content 0.8 mass%) manufactured by Tokuyama, 0.56 mass% of aluminum oxide powder (TM-DAR grade) manufactured by Taimei Chemical, and 0.90 mass% of europium oxide powder (RU grade) manufactured by Shin-Etsu Chemical were mixed, and then the resulting mixture was passed through a sieve with a mesh size of 250 μm to remove aggregates, thereby obtaining a first raw material mixed powder. The compounding ratio here (referred to as the first compounding composition (mass%)) is the general formula of β-type sialon: Si 6-Z Al Z O Z N 8-Z In this case, except for europium oxide, it was designed so that Z=0.22 was obtained by calculating from the Si / Al ratio.

[0065] 200 g of the resulting raw powder having the first composition was packed into a cylindrical boron nitride container with a lid, having an inner diameter of 10 cm and a height of 10 cm, and was subjected to a heat treatment (first firing step) at 1950°C for 10 hours in a nitrogen atmosphere pressurized at 0.8 MPa in an electric furnace with a carbon heater. The powder subjected to the heat treatment was pulverized with a supersonic jet pulverizer (Nippon Pneumatic Mfg. Co., Ltd., PJM-80SP), and the pulverized material was then passed through a nylon sieve with an opening of 45 μm to obtain a first fired powder. The first calcined powder was mixed with europium oxide powder (RU grade) manufactured by Shin-Etsu Chemical Co., Ltd. in a mixing ratio of 90:10 (referred to as the second blending composition (mass%)), and the first calcined powder and europium oxide powder were mixed using a V-type mixer (S-3 manufactured by Tsutsui Rikagaku Kikai Co., Ltd.) The mixture was then passed through a nylon sieve with a mesh size of 250 μm to remove aggregates, and a second raw material mixed powder was obtained.

[0066] 200 g of the raw powder having the second composition obtained was filled into a cylindrical boron nitride container with a lid having an inner diameter of 10 cm and a height of 10 cm, and heat-treated in an electric furnace with a carbon heater in a pressurized nitrogen atmosphere of 0.8 MPa at 2020°C for 12 hours (second firing step). The powder subjected to the heat treatment was pulverized with a supersonic jet pulverizer (Nippon Pneumatic Mfg. Co., Ltd., PJM-80SP), and the pulverized material obtained was passed through a nylon sieve with a mesh size of 45 μm to obtain a second fired powder. The sieve passing rate was 92%.

[0067] 20 g of the obtained second fired powder was filled into a cylindrical boron nitride container with a lid having an inner diameter of 5 cm and a height of 3.5 cm, and annealed for 8 hours at 1500 ° C. in an argon atmosphere at atmospheric pressure in an electric furnace with a carbon heater. The annealed powder was put into a 1:1 mixed acid of 50% hydrofluoric acid and 70% nitric acid kept at 75 ° C. Then, while keeping the temperature at 75 ° C., it was immersed in an acid treatment for 30 minutes at 75 ° C. while stirring at a rotation speed of 450 rpm using a magnetic stirrer. The powder after the acid treatment was precipitated as it was, and decantation to remove the supernatant and fine powder was repeated until the pH of the solution was 5 or more and the supernatant was transparent, and the precipitate finally obtained was filtered and dried to obtain the phosphor powder of Example 1. Powder X-ray diffraction measurements revealed that the crystal phase present was a single phase of β-sialon, and that a β-sialon phosphor was obtained. The first blend composition and the second blend composition in Example 1 are shown in Table 1 below.

[0068] <D V50 Measurements > The particle size distribution of the β-sialon phosphor particles of Example 1 was measured by the laser diffraction scattering method in accordance with JIS R1629:1997 using Microtrac MT3300EX II (Microtrac Bell Co., Ltd.). The pretreatment of the measurement sample was as follows. 0.5 g of β-sialon phosphor particles were put into 100 cc of ion-exchanged water, and dispersion treatment was performed thereon for 3 minutes with an Ultrasonic Homogenizer US-150E (Nippon Seiki Co., Ltd., chip size φ20 mm, Amplitude 100%, oscillation frequency 19.5 KHz, amplitude of about 31 μm). This was used as the measurement sample. The particle size distribution of the measurement sample was measured using the above device. From the obtained particle size distribution, D V50 was determined. D V50 is shown in Table 1 below.

[0069] <Analysis of Element Concentration by EDX Method> Analysis was performed as follows. (1) First, particles recognized as primary particles among the β-sialon phosphor particles of Example 1 were cut by an ion milling device. (2) Regarding the cut surface obtained in (1) above, EDX measurement was performed using JED-2300 manufactured by JEOL Ltd. under the conditions of an acceleration voltage of 15 kV and a measurement time of 50 sec. The measurement was performed at one point near the center of the cut surface and one point at the end of the cut surface (corresponding to the surface portion of the particle before cutting). For reference, the measurement points of the particles of Example 2 are shown in Fig. 2. The obtained data was analyzed by software to determine the concentration of each element.

[0070] The analysis results of the element concentrations are shown in Table 2 below.

[0071] <Evaluation of Fluorescence Characteristics> The fluorescence characteristics of the β-sialon phosphor particles were evaluated by the peak intensity and peak wavelength measured by the following method. As the device, a spectrofluorophotometer (F-7000, manufactured by Hitachi High-Technologies Corporation) calibrated by the rhodamine B method and a standard light source was used. The obtained phosphor powder was filled into a dedicated solid sample holder, and then, using the spectrofluorophotometer, the fluorescence spectrum when irradiated with excitation light spectrally split at a wavelength of 455 nm was measured, and the peak intensity and peak wavelength were determined from the obtained fluorescence spectrum. The obtained results are shown in Table 3.

[0072] For the sake of completeness, it should be noted that since the peak intensity varies depending on the measuring device and conditions, the unit is an arbitrary unit. It was measured under the same conditions in each example and comparative example, and the β-sialon phosphors in each example and comparative example were continuously measured and compared. Table 3 shows the peak intensity when the peak intensity of the β-sialon phosphor particles of Comparative Example 1 was normalized to 100%.

[0073] <CIE Chromaticity> The CIE (International Commission on Illumination) chromaticity of the fluorescence spectrum was determined by measuring the emission spectrum of the total luminous flux that collected the fluorescence for excitation at 455 nm using an integrating sphere with an instantaneous multi-photometry system (MCPD-7000, manufactured by Otsuka Electronics Co., Ltd.).

[0074] (Example 2) β-sialon phosphor particles were obtained by the same raw materials and method as in Example 1. As a result of performing powder X-ray diffraction measurement on the obtained β-sialon phosphor particles, the existing crystal phase was β-sialon single phase. Also, the same analysis and evaluation as in Example 1 were performed. The composition, D V50 , the analysis results of the element concentrations by the EDX method, and the evaluation results of the fluorescence characteristics are shown in Tables 1 to 3. As shown in Table 2, for example, even when manufactured by the same raw materials and method as in Example 1, the element concentrations in the surface part and near the center of the particles were different from those in Example 1. This is presumably due to subtle manufacturing errors.

[0075] (Example 3) β-SiAlON phosphor particles were obtained by the same method as in Example 1, except that the second blend composition was changed to the blend ratio shown in Table 1. Powder X-ray diffraction measurement was performed on the obtained β-SiAlON phosphor particles, and the crystal phase present was found to be a single β-SiAlON phase. In addition, the same analysis and evaluation as in Example 1 were performed. V50 The analysis results of element concentrations by EDX method and the evaluation results of fluorescent properties are shown in Tables 1 to 3.

[0076] Example 4 β-SiAlON phosphor particles were obtained using the same raw materials and method as in Example 3. Powder X-ray diffraction measurement was performed on the obtained β-SiAlON phosphor particles, and the crystal phase present was found to be a single β-SiAlON phase. In addition, the same analysis and evaluation as in Example 1 were performed. V50 The analysis results of element concentrations by EDX method and the evaluation results of fluorescent properties are shown in Tables 1 to 3. For example, as shown in Table 2, even when produced using the same raw materials and method as in Example 3, the element concentrations in the surface and center areas of the particles were different from those in Example 3. This is presumably due to subtle manufacturing errors.

[0077] Comparative Example 1 β-SiAlON phosphor particles were obtained in the same manner as in Example 1, except that a step corresponding to the second firing step in Example 1 was not performed. Powder X-ray diffraction measurement was performed on the obtained β-SiAlON phosphor particles, and the crystal phase present was a single β-SiAlON phase. In addition, the same analysis and evaluation as in Example 1 were performed. V50 The analysis results of element concentrations by EDX method and the evaluation results of fluorescent properties are shown in Tables 1 to 3.

[0078] Comparative Example 2 β-SiAlON phosphor particles were obtained using the same raw materials and method as in Example 3. Powder X-ray diffraction measurement was performed on the obtained β-SiAlON phosphor particles, and the crystal phase present was found to be a single β-SiAlON phase. In addition, the same analysis and evaluation as in Example 1 were performed. V50 The analysis results of element concentrations by EDX method and the evaluation results of fluorescent properties are shown in Tables 1 to 3. For example, as shown in Table 2, even when produced using the same raw materials and method as in Comparative Example 1, the element concentrations in the surface and center areas of the particles were different from those in Comparative Example 1. This is presumably due to subtle manufacturing errors.

[0079] [Table 1]

[0080] [Table 2]

[0081] [Table 3]

[0082] As shown in Table 3 etc., the emission peak intensities of the β-SiAlON phosphor particles of Examples 1 to 4, in which the Pc-Ps value is 3 at% or more, were 10% or more higher than the emission peak intensities of the β-SiAlON phosphor particles of Comparative Examples 1 and 2, in which the Pc and Ps values ​​were approximately the same. In other words, it was demonstrated that luminance can be improved by using β-SiAlON phosphor particles in which the Pc-Ps value is 3 at% or more.

[0083] This application claims priority based on Japanese Patent Application No. 2019-150280, filed on August 20, 2019, the disclosure of which is incorporated herein in its entirety. [Explanation of symbols]

[0084] 10 Light emitting device 12 Light emitting source (LED chip) 13 First lead frame 13a Upper 13b Recess 14 Second Lead Frame 15 Wavelength conversion material 16 Bonding Wire 17 Sealing resin 18 Phosphor (β-type SiAlON phosphor particles) 19 Cap

Claims

1. β-sialon phosphor particles containing europium as a solid solution, When the elemental concentration of Si atoms in the surface portion of the phosphor particle, which is determined by analyzing the cross section of the phosphor particle using energy dispersive X-ray analysis, is defined as Ps [at %], and the elemental concentration of Si atoms in the vicinity of the center of the phosphor particle, which is determined by analyzing the cross section using the same method, is defined as Pc [at %], The value of Pc-Ps is 3 at% or more, β-type sialon phosphor particles represented by the general formula Si 6-z Al z O z N 8-z :Eu 2+ (0<Z≦4.2).

2. β-sialon phosphor particles according to claim 1, β-sialon phosphor particles having a Pc-Ps value of 5 at % or more and 20 at % or less.

3. 3. The β-sialon phosphor particle according to claim 1 or 2, β-sialon phosphor particles, in which Ps is 20 at % or more and 35 at % or less.

4. β-sialon phosphor particles according to any one of claims 1 to 3, 50% diameter D in volume-based cumulative fraction V50 β-sialon phosphor particles having a particle size of 5 μm or more and 50 μm or less.

5. A light emitting device including a light emitting source and a wavelength conversion member, the wavelength conversion member includes a phosphor, A light emitting device, wherein the phosphor comprises the β-sialon phosphor particles according to claim 1 .

6. 6. The light emitting device according to claim 5, The light emitting device, wherein the light source includes an LED chip that emits light having a wavelength of 300 nm or more and 500 nm or less.

7. 7. The light emitting device according to claim 5, The light emitting device, wherein the phosphor further comprises a KSF-based phosphor in which manganese is solid-solved.

Citation Information

Patent Citations

  • Method for producing β-sialon phosphor

    JP2017036430A

  • Method for producing β-sialon phosphor

    JP2017110206A

  • Β type sialon phosphor and method for producing the same and light emitting device using the same

    JP2018002870A

  • Manufacturing method of β type sialon phosphor

    JP2019199531A

  • JPP6572373B