Release Film

A laminated polyester film with controlled dimensional changes and surface properties addresses the wrinkling and releasability issues of ethylene-tetrafluoroethylene copolymers, ensuring stable mold release in semiconductor encapsulation processes.

JP7589767B2Active Publication Date: 2024-11-26TORAY INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023085341
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-12-25
Filing Date
2023-05-24
Publication Date
2024-11-26
Estimated Expiration
2038-12-13

AI Technical Summary

Technical Problem

Existing mold release films, particularly those based on ethylene-tetrafluoroethylene copolymers, suffer from wrinkling and loss of mold releasability due to high dimensional instability and insufficient heat resistance during semiconductor encapsulation processes, especially in compression molding methods.

Method used

A laminated polyester film with specific dimensional change rates, surface free energy changes, and elastic modulus ranges, along with a release layer thickness and composition, is developed to maintain mold conformability and heat resistance, preventing wrinkles and ensuring stable mold releasability even after large deformations.

Benefits of technology

The film effectively suppresses wrinkles during heating and maintains excellent peelability after high-temperature molding, making it suitable for semiconductor encapsulation processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589767000001
    Figure 0007589767000001
  • Figure 0007589767000002
    Figure 0007589767000002
  • Figure 0007589767000003
    Figure 0007589767000003
Patent Text Reader

Abstract

To provide a release film that can be suitably used for process applications, especially for semiconductor encapsulation process applications, by having excellent mold followability and heat resistance, suppressing wrinkles that occur during heating, and having properties that prevent mold release from changing even after large deformation.SOLUTION: The maximum dimensional change rate from 30°C to 150°C when the temperature is increased from 30°C to 200°C at 10°C / minute measured by TMA is S1 (%), the temperature giving S1 is T1 (°C), and the dimensional change rate at 40°C is S0 (%), the following equations (I) and (II) are satisfied and the surface free energy at 25°C Sa (mN / mm), surface free energy Sb (mN / mm) after heat treatment at 180°C for 3 minutes, and surface free energy Sc (mN / mm) after 50% elongation at 180°C. On at least one side of the film, the following equations (III) and (IV) are satisfied. 0≤S1≤1.5...(I) 0≤|S1-S0| / (T1-40)≤0.050...(II) 0≤|Sa-Sb|≤15...(III) 0≤|Sa-Sc|≤15...(IV).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a release film, which can be suitably used in applications such as circuit manufacturing processes and semiconductor manufacturing processes, and can be particularly suitably used as a release film for semiconductor encapsulation processes. [Background technology]

[0002] Semiconductor chips are sealed with resin to protect them from disturbances such as light, heat, moisture, and physical shocks, and are mounted on a substrate as a molded product called a package. Hardening resins such as epoxy resins are used to seal semiconductor chips. The so-called transfer molding method and compression molding method are known as methods for sealing semiconductor chips, but in recent years, the introduction of compression molding has been progressing against the backdrop of trends such as larger semiconductor wafers and lower-profile packages with more pins.

[0003] In the compression molding method, the molten encapsulating resin is compressed and hardened by moving a mold up and down while it is heated. In this process, a release film is generally inserted between the mold and the encapsulating resin to ensure their releasability. Ethylene-tetrafluoroethylene copolymer films, which have excellent releasability, heat resistance, and conformability to the mold shape, are widely used as release films. However, there is an issue that wrinkles caused by expansion during heating are transferred to the package surface, and improvement is desired.

[0004] In order to solve this problem, the following films have been proposed: [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-92272 A [Patent Document 2] JP 2016-127091 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the polyester films laminated with a release layer described in Patent Documents 1 and 2 use polyester as a base material, which has high dimensional stability compared to ethylene-tetrafluoroethylene copolymer films, but the problem of wrinkles occurring when heated described above was not improved. Furthermore, there was a problem that the mold conformability or heat resistance was insufficient, and releasability was lost in areas where the film was significantly deformed, making it impossible to peel off in parts.

[0007] The object of the present invention is to solve the problems of the conventional techniques described above, that is, to provide a release film that is excellent in mold conformability and heat resistance, suppresses wrinkles that occur during heating, and has properties that make it difficult for releasability to change even after large deformation, and can therefore be suitably used for process applications, particularly for semiconductor encapsulation processes. [Means for solving the problem]

[0008] The gist of the present invention for solving the above problems is as follows. (1) A process release film which satisfies the following formulas (I) and (II) when the maximum dimensional change from 30°C to 150°C when heated from 30°C to 200°C at a rate of 10°C / min is S1 (%), the temperature at which S1 occurs is T1 (°C), and the dimensional change at 40°C is S0 (%), as measured by thermomechanical analysis (TMA); and the surface free energy Sa (mN / mm) at 25°C, the surface free energy Sb (mN / mm) after heat treatment at 180°C for 3 minutes, and the surface free energy Sc (mN / mm) after 50% elongation at 180°C satisfy the following formulas (III) and (IV) on at least one side of the film. 0≦S1≦1.5 (I) 0≦|S1−S0| / (T1−40)≦0.050···(II) 0≦|Sa-Sb|≦15 (III) 0≦|Sa-Sc|≦15 (IV) (2) The release film for process use according to (1), having a surface elastic modulus of 50 to 3000 MPa on at least one surface as measured using an atomic force microscope. (3) The release film for process use according to any one of (1) to (2), having a surface elastic modulus root mean square (Rq) of 50 to 500 MPa on at least one surface. (4) The release film for process use according to any one of (1) to (3), which has a maximum temperature (Tm) of a melting peak observed by a differential scanning calorimeter (DSC) of 240° C. or more and 265° C. or less. (5) The release film for process use according to any one of (1) to (4), wherein the polar strength of the film surface on at least one side is 0.1 mN / m or more and 5.0 mN / m or less. (6) The release film for process use according to any one of (1) to (5), which has a release layer having a thickness of 50 nm or more and 500 nm or less on at least one surface. (7) The release film for process use according to any one of (1) to (6), wherein the release layer has a thickness unevenness of 50 nm or less. (8) The release film for process use according to any one of (1) to (7), which has a surface breaking elongation at 180° C. of more than 0% and not more than 30%. (9) The release film for process use according to any one of (1) to (8), which has a piercing strength of 2 N or more and 10 N or less. (10) The release film for process use according to any one of (1) to (9) is a laminated polyester film having a polyester A layer and a polyester B layer having a melting point lower than that of the polyester A layer, and is formed by laminating 3 to 1,000 layers of the A layer and the B layer alternately. (11) The process release film according to any one of (1) to (10), wherein the polyester A layer contains a polyester containing at least one copolymer component selected from the group consisting of bisphenol A ethylene oxide, spiroglycol, cyclohexanedicarboxylic acid, and naphthalenedicarboxylic acid, and / or a polyetherimide. (12) The release film for process use according to any one of (1) to (11), which has a polyester A layer having a thickness of 3 μm or more and 10 μm or less within a thickness range of 10 μm or less from the outermost surface of the film. (13) The release film for process use according to any one of (1) to (12), which is used as a process film in semiconductor manufacturing. (14) The release film for process use according to any one of (1) to (13), which is used for semiconductor compression molding. Effect of the Invention

[0009] The release film of the present invention has a small dimensional change rate and its fluctuation when heated from 30°C to 200°C, so that the occurrence of wrinkles during heating can be suppressed. In addition, since the change in surface free energy after heat treatment and after thermal elongation is small, it has excellent releasability after high-temperature molding, and is suitable as a release film for circuit manufacturing processes and semiconductor manufacturing processes, and can be particularly suitable for use as a release film for semiconductor encapsulation processes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The release film of the present invention is a laminated film in which a release layer is laminated on a base film, or is a film having releasability in the base film itself. The release film of the present invention must satisfy the following formulas (I) and (II), where S1 is the maximum dimensional change from 30° C. to 150° C. when the temperature is raised from 30° C. to 200° C. at a rate of 10° C. / min, T1 is the temperature at which S1 occurs, and S0 is the dimensional change at 40° C., as measured by TMA. 0≦S1≦1.5 (I) 0≦|S1−S0| / (T1−40)≦0.050···(II) In the compression molding method, in the process of contacting a release film from a room temperature state with a high-temperature mold and suctioning it with a vacuum to mold it into the shape of the mold, the release film may expand during the temperature rise process, and the wrinkles that occur may be transferred to the package. Even when a film with high dimensional stability such as a biaxially stretched film is used, the expansion in the low temperature range is not sufficiently suppressed, and wrinkles that occur during the temperature rise process may be similarly transferred. As a result of intensive research by the inventors, it was found that it is possible to suppress the occurrence of wrinkles during temperature rise and obtain a product with a good appearance by setting the dimensional change rate at 30°C to 150°C corresponding to the temperature change in the mold to a specific range shown in formula (I) and setting the change rate of the dimensional change in this temperature range to a specific range shown in formula (II). With regard to formula (I), it is more preferable that formula (I') is satisfied, and it is most preferable that formula (I") is satisfied. 0≦S1≦1.0 (I') 0≦S1≦0.7...(I") With respect to formula (II), it is more preferable that formula (II') is satisfied, and it is most preferable that formula (II") is satisfied. 0≦|S1−S0| / (T1−40)≦0.025···(II') 0≦|S1−S0| / (T1−40)≦0.010···(II”) The method for making the release film of the present invention satisfy the above formulas (I) and (II) is not particularly limited, but examples thereof include a method of continuously applying a step A of applying a tension of 0.5 MPa to 5 MPa in the film conveying direction at a temperature (Ta) of 70°C to 150°C and a step B of applying a tension of 0.5 MPa to 5 MPa in the film conveying direction at a temperature (Tb) of Ta+5°C to Ta+20°C in the release film manufacturing process. The molecular chains oriented by the application of tension in this temperature range may relax during the temperature rise process during molding, and the dimensional change may be in the shrinkage direction, thereby making it possible to suppress expansion. In addition, by applying tension under a stepwise temperature gradient, relaxation shrinkage may occur gradually, and the occurrence of wrinkles due to shrinkage deformation may be suppressed. In this method for producing a release film, when the stretching tension of the substrate film is high, the orientation of the molecular chains due to the application of tension may be insufficient, and it is preferable that the 150°C 10% stretching stress in the MD direction of the substrate film is 1 MPa to 30 MPa. More preferably, it is from 1 MPa to 25 MPa, and most preferably from 1 MPa to 20 MPa.

[0011] The release film of the present invention must have a surface free energy Sa at 25°C, a surface free energy Sb after heat treatment at 180°C for 3 minutes, and a surface free energy Sc after 50% elongation at 180°C that satisfy the following formulas (III) and (IV) on at least one side of the film. 0≦|Sa-Sb|≦15 (III) 0≦|Sa-Sc|≦15 (IV) Formulas (III) and (IV) mean that the change in the surface free energy before and after heat treatment at 180°C and after 50% elongation treatment at 180°C is small. In conventional release films, the release properties are impaired after molding due to denaturation at high temperatures and deformation of the release film surface due to molding, which can lead to poor peeling. In recent years, there has been a demand for conformity to the shape of a mold with a deeper package thickness, and poor release at acute corners can be an issue. The film of the present invention is characterized in that the change in surface free energy at high temperatures and large deformation is small, so that the release properties are less susceptible to the influence of the molded shape and are stable. It is more preferable that formula (III') is satisfied, and it is most preferable that formula (III") is satisfied. 0.5≦|Sa-Sb|≦13···(III') 0.5≦|Sa-Sb|≦11···(III”) With respect to formula (IV), it is more preferable that formula (IV') is satisfied, and it is most preferable that formula (IV") is satisfied. 1.0≦|Sa-Sc|≦13 (IV') 1.0≦|Sa-Sc|≦11···(IV”) As described above, it is preferable that the change in surface energy at high temperatures and large deformation is small, but it has been confirmed that when the surface energy increases or decreases slightly, the energy difference between the interfaces at the resulting peel interface becomes a distortion, which tends to improve the peelability. Therefore, as shown in formulas (III'), (III"), (IV'), and (IV"), the preferred range of the change in surface energy has a lower limit. There is no particular limitation on the method for making the release film of the present invention satisfy the above formulas (III) and (IV), but an example of such a method is a method of providing a release layer having a thickness of 50 nm to 500 nm on the base film. It is presumed that by thinning the release layer to 500 nm or less, the deformation stress of the release layer is reduced and the layer is deformed uniformly, which has the effect of suppressing the occurrence of cracks and thickness unevenness. On the other hand, if the release layer thickness is less than 50 nm, it is difficult to form a uniform release layer, and the change in surface energy due to heating or elongation tends to be large. The release film of the present invention preferably has a surface elastic modulus of 50 MPa or more and 3000 MPa or less, measured on at least one side using an atomic force microscope. If the surface elastic modulus of the release film is greater than 3000 MPa, cracks are likely to occur on the surface during molding, and the release property may be locally impaired. If it is less than 50 MPa, the flow marks of the resin may be transferred to the release film surface, and the quality of the package surface after transfer may be reduced. The surface elastic modulus is more preferably 300 MPa or more and 2500 MPa or less, and most preferably 500 MPa or more and 2000 MPa or less. There is no particular limitation on the method for making the surface elastic modulus 50 MPa or more and 3000 MPa or less, but examples thereof include a method of incorporating a crosslinking agent into the release layer composition. The release film of the present invention preferably has a surface modulus root mean square (Rq) of 50 MPa or more and 500 MPa or less on at least one side. When Rq is greater than 500 MPa, the variation in surface modulus is large and the molding stress distribution is non-uniform. Therefore, when a thin release layer is provided, the variation in layer thickness increases due to molding, and the release characteristics in the plane may become non-uniform. The lower the Rq, the better, but it is difficult to make it less than 50 MPa by a general manufacturing method. Rq is more preferably 50 MPa or more and 400 MPa or less, and most preferably 50 MPa or more and 300 MPa or less. As a method for making Rq in the above-mentioned specific range, a method of performing stepwise elongation of 0.1% or more and 10% or less in the drying process during processing of the release layer can be mentioned. Stepwise elongation means performing elongation in a plurality of different temperature zones, and the elongation ratio means the sum of the ratios in all zones. By performing a stretching process at a small ratio on the release layer, the variation in surface modulus can be reduced. In addition, by performing the stretching stepwise, the stress concentration on the release layer during curing can be reduced, and the breakage of the release layer and the decrease in adhesion can be suppressed. If the stretching rate is less than 0.1%, the effect of reducing the variation in the surface elastic modulus is small, and if it is more than 10%, the formability of the film may deteriorate, or the release property may deteriorate due to the breakage of the release layer. The stretching rate is preferably 0.4% or more and 8.5% or less, and most preferably 0.7% or more and 7.5% or less. The release film of the present invention preferably has a maximum melting peak temperature (Tm) of 240°C or more and 265°C or less as observed by a differential scanning calorimeter (DSC). In recent years, the use of resins for high-temperature molding has been increasing from the viewpoint of heat resistance of chips, and the heat resistance requirements for release films tend to be more stringent, so Tm is preferably 240°C or more. The higher the Tm, the more preferable, but from the viewpoint of compatibility with moldability, it is preferably 265°C or less. It is more preferably 243°C or more and 265°C or less, and most preferably 246°C or more and 265°C or less. The release film of the present invention preferably has a polar force of 0.1 mN / m or more and 5.0 mN / m or less on at least one side of the film surface. The polar force in the present invention refers to a value calculated by a measurement method described later. If the polar force of the film surface is less than 0.1 mN / m, the molten resin may be repelled by the film surface, resulting in insufficient leveling and poor transfer appearance. If the polar force of the film surface is greater than 5.0 mN / m, the adhesion with the release film may be excessive, and the film may not peel off during the peeling process, or the film may break or adhere, making it difficult to maintain process stability. The polar force of the film surface is more preferably 0.4 mN / m or more and 4 mN / m or less, and most preferably 0.8 mN / m or more and 3 mN / m or less. Methods for setting the polar strength of the film surface to 0.1 mN / m or more and 5 mN / m or less include a method of using the additives described below as the resin composition for forming the release layer. In particular, compounds containing long-chain alkyl groups are preferably used because they have good conformability during stretching during release layer processing. The release film of the present invention preferably has a release layer having a thickness of 50 nm to 500 nm on at least one surface. By having a thin release layer, the deformation stress of the release layer is reduced and the layer is deformed uniformly, and the occurrence of cracks and thickness unevenness is suppressed. The thickness of the release layer is more preferably 70 nm to 400 nm, and most preferably 90 nm to 300 nm. In the release film of the present invention, the thickness unevenness of the release layer is preferably 50 nm or less. The thickness unevenness of the release layer has a large effect on the release property when the release layer is designed to have a thickness of 200 nm or less. When the thickness unevenness is more than 50 nm, it is easy to generate peel marks due to heavy peeling at local thin film parts, cohesive failure of the release layer, and peeling force unevenness with thick film parts. In addition, when a release film is used in a semiconductor encapsulation process, the encapsulation resin to be peeled generally contains a large amount of large-diameter particles, and the surface is uneven and not uniform, so that the effect of the thickness unevenness of the release layer tends to be expanded and appears. By reducing the thickness unevenness of the release layer, it is possible to reduce the effect of these factors that deteriorate the release property and to impart properties that are particularly suitable for a release film for a semiconductor encapsulation process. The thickness unevenness of the release layer is more preferably 40 nm or less, and most preferably 30 nm or less. There is no particular limitation on the method for making the thickness unevenness of the release layer into a preferred range, but examples include a method of elongating the release layer by 1.0% to 5% in the drying process during the processing of the release layer. In this case, when the stretching is performed in a plurality of zones, the total stretching ratio is preferably within the above range. The thickness unevenness of the coating film is often larger in the MD direction than in the TD direction as a result of the influence of the MD thickness unevenness of the film itself due to casting, roll adhesion, and discharge fluctuation, and the coating unevenness due to the micro-vibration of the coater, etc., but by carrying out the above-mentioned process of conveying the release layer coating liquid under a specific speed condition before preheating and drying, the coating liquid becomes easy to spread in the MD direction along the accompanying air flow of the film conveyance, and the thickness unevenness may be reduced. The release film of the present invention preferably has a surface rupture elongation at 180°C of more than 0% and not more than 30%. The surface rupture elongation at 180°C means an elongation at which a rupture occurs in the outermost layer after stretching at 180°C. As a result of intensive research by the inventors, it was found that the appearance unevenness of the resin surface after encapsulation may be improved by causing a rupture due to stretching on the outermost surface of the release film. Although the principle is not clear, it is considered to be the result of the improvement of the leveling of the encapsulating resin due to the fine unevenness of the film and the improvement of the appearance due to the transfer of the fine unevenness to the resin surface. The surface rupture elongation at 180°C is more preferably 3% to 25% and most preferably 3% to 20%. If the surface rupture elongation exceeds 30%, the effect may not be exhibited in the semiconductor encapsulation process, and if the surface rupture elongation is 0%, that is, if a rupture occurs from the time of film formation, it is not preferable because the release layer is easily scraped during the conveying process. As a method for making the surface breaking elongation at 180°C within the above-mentioned preferred range, a method of making the maximum heating temperature in the coating, drying, and curing steps of the release layer 100°C or less can be mentioned. By applying the low temperature condition to the actual molding (stretching) step in a state where crosslinking is not completed, crosslinking is completed by heating in the molding step, causing breakage due to stretching, and it is possible to suppress the occurrence of breakage due to the tension of film transport during film formation. Examples of the configuration of the release film of the present invention include a base film having releasability, or a laminated film in which a release layer having releasability is laminated on a base film, but a configuration in which a release layer is laminated on a base film is preferred because of the advantage that the release property can be controlled in accordance with the encapsulating resin. The resin used in the base film of the present invention is not particularly limited as long as it does not impair the effects of the present invention, and examples thereof include polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polyarylates, polyethylene, polypropylene, polyamides, polyimides, polymethylpentene, polyvinyl chloride, polystyrene, polymethyl methacrylate, polycarbonates, polyether ether ketones, polysulfones, polyether sulfones, fluororesins, polyetherimides, polyphenylene sulfide, polyurethanes, and cyclic olefin resins, which can be used alone or in combination. Among these, polyesters such as polyethylene terephthalate and polybutylene terephthalate are preferably used from the viewpoints of film handling and dimensional stability, and economic efficiency during production.

[0012] In the present invention, polyester is a general term for polymers in which the main bond in the main chain is an ester bond. Polyesters can usually be obtained by polycondensation reaction of a dicarboxylic acid component and a glycol component.

[0013] The dicarboxylic acid component for obtaining the polyester is not particularly limited as long as it does not impair the effects of the present invention, and examples of components that can be used include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, diphenyldicarboxylic acid, diphenylsulfonedicarboxylic acid, diphenoxyethanedicarboxylic acid, 5-sodiumsulfonedicarboxylic acid, and 9,9'-bis(4-carboxyphenyl)fluorene acid, aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, dimer acid, maleic acid, and fumaric acid, alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, and oxycarboxylic acids such as paraoxybenzoic acid. The dicarboxylic acid component may be a dicarboxylic acid ester derivative component, and esters of the above dicarboxylic acid compounds, such as dimethyl terephthalate, diethyl terephthalate, 2-hydroxyethyl methyl terephthalate, dimethyl 2,6-naphthalenedicarboxylate, dimethyl isophthalate, dimethyl adipate, diethyl maleate, and dimethyl dimerate, may also be used.

[0014] The glycol component for obtaining the polyester is not particularly limited as long as it does not impair the effects of the present invention. For example, aliphatic dihydroxy compounds such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 2,2-dimethyl-1,3-propanediol; polyoxyalkylene glycols such as diethylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; alicyclic dihydroxy compounds such as 1,4-cyclohexanedimethanol, isosorbate, 9,9'-bis(4-carboxyphenyl)fluorene, and spiroglycol; and aromatic dihydroxy compounds such as bisphenol A and bisphenol S can be used. Among these, in terms of compatibility between flexibility and heat resistance, and ease of handling, it is preferable to use ethylene glycol, 1,4-butanediol, 2,2-dimethyl-1,3-propanediol, 1,4-cyclohexanedimethanol, and polytetramethylene glycol.

[0015] These dicarboxylic acid components and glycol components may be used in combination of two or more kinds as long as the effect of the present invention is not impaired.

[0016] Examples of polyolefins that can be preferably used in the present invention include propylene homopolymers exhibiting isotactic or syndiotactic stereoregularity, propylene-α-olefin copolymers, etc. Specific examples of the α-olefins include ethylene, butene-1, hexene-1, and heptene-1,4-methylpentene-1. The propylene-α-olefin copolymer preferably contains more than 50 mol% of propylene units when the total structural units constituting the polymer are taken as 100 mol%. The propylene-α-olefin copolymer may be any of a binary, ternary, and quaternary copolymers, and may be any of a random copolymer and a block copolymer, as long as the effects of the present invention are not impaired. The base film of the release film of the present invention may be a single layer film or a laminated film of two or more layers. In the case of a three-layer structure, it is preferable that the compositions of both surface layers are the same from the viewpoint of productivity. Furthermore, in order to improve productivity, it is preferable that the laminate thicknesses of both surface layers are equal. Furthermore, in order to improve the heat resistance of the base film, it is preferable that the maximum temperature (Tms) of the melting peak observed by a differential scanning calorimeter (DSC) of both surface layers is 248°C or more and 265°C or less. More preferably, it is 250°C or more and 265°C or less, and most preferably, it is 253°C or more and 265°C or less. The release film of the present invention preferably has a piercing strength of 2N or more and 10N or less. In the semiconductor sealing process, the release film may be used with holes for vacuum adsorption of the wafer, and a piercing strength of 10N or less is preferable because it is easy to open uniform holes. On the other hand, if the piercing strength is less than 2N, holes may be opened at unintended positions due to the mold protrusions being pressed against the release film, and sufficient vacuum may not be maintained, which is not preferable. There is no particular limitation on the method for making the piercing strength within the above preferred range, but for example, in the manufacturing process of a biaxially oriented polyester film, a method in which the magnification in each stretching direction is 2.8 times or more and 3.8 times or less, and a difference in stretching magnification is set to 0.7 times or more and 1.0 times or less in each stretching direction can be mentioned. In general, the piercing strength of a polymer film correlates with the degree of molecular orientation, but by forming a low orientation direction in the film plane by unbalancing the stretching magnification, it is possible to control the piercing strength to a good range while maintaining suitable mechanical properties as a process film. It is more preferable that the piercing strength is 3N or more and 7N or less. The release film of the present invention is preferably a laminated polyester film having a polyester A layer and a polyester B layer having a melting point lower than that of the polyester A layer, and is preferably configured by laminating at least 3 layers and 1000 layers of the A layer and the B layer alternately. The A layer having a high melting point functions as a heat-resistant layer, and contributes to suppressing film deformation caused by shear heat generated by the flow of the encapsulating resin, and suppressing release defects caused by deformation of the surface layer due to shear, particularly in the semiconductor encapsulation process. In addition, the B layer having a low melting point functions as a flexible layer, and can improve the moldability of the film. The polyester A layer preferably contains a polyester containing at least one copolymer component selected from spiroglycol, isosorbide, fluorene, cyclohexanedicarboxylic acid, and naphthalenedicarboxylic acid components, and / or a polyetherimide. By containing these specific polyesters or polyetherimides, it is possible to effectively suppress film deformation caused by shear heat generated by the resin flow in the semiconductor encapsulation process. In addition, although the specific polyester or polyetherimide has a high glass transition temperature or high melting point, even when laminated with a flexible polyester B layer, interfacial peeling is unlikely to occur during biaxial stretching, and productivity reduction due to tearing, unevenness in the film appearance, etc. can be improved in some cases. The release film of the present invention preferably has a polyester A layer having a thickness of 3 μm to 10 μm within a thickness range of 10 μm or less from the outermost surface of the film. By positioning the polyester A layer in a specific thickness range near the outermost surface of the film, it is possible to more effectively suppress film deformation due to shear heat caused by resin flow in the semiconductor encapsulation process. The thickness of the polyester A layer is more preferably 4 μm to 9 μm, and most preferably 5 μm to 8 μm. If the thickness of the polyester A layer is less than 3 μm, the effect of suppressing the film deformation is likely to be insufficient, and if it is greater than 10 μm, it is not preferable because the moldability may be insufficient. When a plurality of polyester A layers are present within a range of 10 μm or less from the outermost surface of the film, it is preferable that the total thickness is within the above range. In addition, from the viewpoint of achieving both the suppression of film deformation and moldability, it is also a more preferable embodiment that two or more polyester A layers are positioned within a range of 10 μm or less from the outermost surface of the film. By being divided into multiple layers, the effect of suppressing film deformation can be expressed without impairing moldability. The substrate film of the present invention is preferably a biaxially oriented film from the viewpoint of controlling dimensional changes in a mold. The biaxially oriented film can be obtained by stretching an unstretched film in the longitudinal direction and then in the width direction, or in the width direction and then in the longitudinal direction, using a sequential biaxial stretching method, or by stretching the film in the longitudinal direction and the width direction at approximately the same time, using a simultaneous biaxial stretching method, or the like.

[0017] In such a stretching method, the stretching ratio in the longitudinal direction is preferably 2.8 to 3.4 times, more preferably 2.9 to 3.3 times. The stretching speed is preferably 1,000% / min to 200,000% / min. The stretching temperature in the longitudinal direction is preferably 70°C to 90°C. The stretching ratio in the transverse direction is preferably 2.8 to 3.8 times, more preferably 3 to 3.6 times. The stretching speed in the transverse direction is preferably 1,000% / min to 200,000% / min.

[0018] Furthermore, the film is heat-treated after the biaxial stretching. The heat treatment can be performed by any conventional method such as in an oven or on a heated roll. This heat treatment is preferably performed at a temperature of -40°C to -5°C from the crystal melting peak temperature (Tm) of the film. If the heat treatment temperature is lower than Tm-40°C, the degree of molecular orientation becomes too high, and the conformability to the mold shape may be insufficient, or the shrinkage during heating may be large, causing wrinkles in the mold and transferring them to the package surface. If the heat treatment temperature is higher than Tm-5°C, crystallization may proceed excessively and the conformability to the mold may be insufficient. More preferably, Tm-34°C to -8°C, and most preferably Tm-32°C to -12°C. The heat treatment time can be any time within a range that does not deteriorate the properties, and is preferably performed for 5 seconds to 60 seconds, more preferably 10 seconds to 40 seconds, and most preferably 15 seconds to 30 seconds. Next, a method for providing a release layer on a substrate film will be described, but the present invention is not limited to this example. The release layer of the present invention can be laminated on one side or both sides of the substrate film. When the release layer is laminated on one side, an antistatic layer may be laminated on the opposite side. The antistatic layer can contain an antistatic agent such as carbon black, tin oxide, tin oxide antimony doped, polythiophene and polyaniline. In consideration of transparency, tin oxide-based antistatic agents are preferred. The release layer of the present invention preferably contains a binder resin, since the adhesiveness to the base film is improved and the peeling force to the object to be peeled can be adjusted. Specific examples of the binder resin include polyester resin, acrylic resin, urethane resin, polyvinyl, polyalkylene glycol, polyalkyleneimine, cellulose, starch, etc., and acrylic resin is preferably used from the viewpoint of mold followability and peeling force control.

[0019] Examples of the acrylic resin include homopolymers or copolymers of (meth)acrylic acid alkyl esters, and (meth)acrylic acid ester copolymers having a curable functional group at the side chain and / or main chain end, and the curable functional group includes a hydroxyl group, a carboxyl group, an epoxy group, an amino group, etc. Among them, an acrylic monomer copolymer in which an acrylic monomer is copolymerized with an acrylic acid ester having a curable functional group at the side chain and / or main chain end is preferred.

[0020] In addition, it is preferable to add a crosslinking agent as a component constituting the release layer. By using various crosslinking agents in combination with the above-mentioned resin, the heat resistance can be dramatically improved. The crosslinking agent is preferably an oxazoline resin, a melamine resin, an epoxy resin, a carbodiimide resin, or an isocyanate resin. From the viewpoint of the durability of the release layer to the solvent, a melamine resin is more preferably used. The crosslinking agents can be mixed and used in any ratio, but it is preferable to add 5 to 50 parts by weight of the crosslinking agent to 100 parts by weight of the binder resin in terms of improving heat resistance, and more preferably, 10 to 40 parts by weight of the crosslinking agent. If the amount of the crosslinking agent added is less than 5 parts by weight, the effect of improving heat resistance may be insufficient, or scratches may occur during roll transport. If the amount exceeds 50 parts by weight, it is not preferable because spots are likely to occur during application.

[0021] In the present invention, it is preferable that the resin composition forming the release layer contains an additive suitable for the purpose of imparting releasability in addition to the binder resin and the crosslinking agent. The additive is preferably 3 parts by mass or more and 50 parts by mass or less when the sum of the masses of the binder resin and the crosslinking agent is 100 parts by mass. By making the mass of the additive 3 parts by mass or more, releasability can be imparted, and by making it 50 parts by mass or less, sufficient heat resistance can be imparted. It is preferably 10 parts by mass or more and 42 parts by mass or less, and most preferably 20 parts by mass or more and 34 parts by mass or less.

[0022] The additive in the present invention refers to a compound that, when added to a resin, imparts releasability to the surface of the resin (i.e., reduces the surface free energy of the resin or reduces the static friction coefficient of the resin).

[0023] The additives that can be used in the present invention include silicone-containing compounds, fluorine compounds, waxes such as paraffin wax, polyethylene wax, and carnauba wax, compounds containing long-chain alkyl groups, and resins.Among them, compounds containing long-chain alkyl groups are preferred because they can achieve both peelability and heat resistance.The long-chain alkyl compound in the present invention refers to a compound having a long-chain alkyl group, and is not particularly limited as long as it contains a long-chain alkyl group, but includes compounds having a long-chain alkyl group on the side chain of the main chain polymer.

[0024] In the compound having a long-chain alkyl group in the side chain of the main chain polymer, examples of the main chain polymer include acrylate polymers or copolymers, polyvinyl alcohol (including partially saponified polyvinyl acetate), ethylene-vinyl alcohol copolymers (including partially saponified ethylene-vinyl acetate copolymers), vinyl alcohol-acrylic acid copolymers (including partially saponified vinyl acetate-acrylic acid copolymers), polyethylimine, polyvinylamine, styrene-maleic anhydride copolymers, polyurethanes, and the like.

[0025] The fluorine compound in the present invention is a compound that contains fluorine atoms in the compound. For example, perfluoroalkyl group-containing compounds, polymers of olefin compounds that contain fluorine atoms, aromatic fluorine compounds such as fluorobenzene, etc. can be mentioned. In the compression molding method, since a high heat load is applied to the release film, in consideration of heat resistance and contamination, it is preferable that the fluorine compound is a polymer compound.

[0026] The wax in the present invention is a wax selected from natural wax, synthetic wax, and waxes blended therewith. Natural waxes are vegetable wax, animal wax, mineral wax, and petroleum wax. Examples of vegetable waxes include candelilla wax, carnauba wax, rice wax, wood wax, and jojoba oil. Examples of animal waxes include beeswax, lanolin, and whale wax. Examples of mineral waxes include montan wax, ozokerite, and ceresin. Examples of petroleum waxes include paraffin wax, microcrystalline wax, and petrolatum. Examples of synthetic waxes include synthetic hydrocarbons, modified waxes, hydrogenated waxes, fatty acids, acid amides, amines, imides, esters, and ketones. Examples of synthetic hydrocarbons include Fischer-Tropsch wax (also known as Sazowar wax) and polyethylene wax, but also include the following polymers, which are low molecular weight polymers (specifically, polymers with a viscosity average molecular weight of 500 to 20,000). These include polypropylene, ethylene-acrylic acid copolymer, polyethylene glycol, polypropylene glycol, and block or grafted combinations of polyethylene glycol and polypropylene glycol. Modified waxes include montan wax derivatives, paraffin wax derivatives, and microcrystalline wax derivatives. Derivatives here are compounds obtained by any of the following processes, or a combination of them: refining, oxidation, esterification, and saponification. Hydrogenated waxes include hydrogenated castor oil and hydrogenated castor oil derivatives.

[0027] The resin constituting the release layer of the present invention may contain inert particles for the purpose of improving the adhesion and slippage of the release layer. Specific examples of inert particles include silica, alumina, kaolin, calcium carbonate, titanium oxide, organic particles, etc.

[0028] Furthermore, within the scope of the present invention, antifoaming agents, coatability improvers, thickeners, organic lubricants, antistatic agents, antioxidants, ultraviolet absorbers, foaming agents, dyes, etc. may be contained as necessary.

[0029] When the resin composition forming the release layer is provided on the substrate film, a solvent may be used. That is, the resin composition may be dissolved or dispersed in a solvent to form a coating liquid, which may be applied to the substrate film. After application, the solvent is dried and heating is performed to obtain a laminated film on which the release layer is laminated. A preferred method for forming a release layer on a substrate film is to apply the release layer uniformly using a metalling bar or gravure roll, and then dry the layer in an oven. When applying the release layer using a coating method such as gravure coating, it is preferred to apply the release layer so as not to impede the flow and leveling of the coating layer. The oven temperature is preferably 70 to 245°C, more preferably 80 to 235°C, and most preferably 90 to 225°C. If the drying temperature is lower than 70°C, the release layer may not be cured sufficiently, and the substrate film and the release layer may not adhere to each other. If the temperature is higher than 245°C, the coating thickness accuracy may decrease due to thermal deformation of the film. The heat treatment time is preferably 1 to 60 seconds, more preferably 5 to 40 seconds, and most preferably 10 to 30 seconds. In the release film of the present invention, from the viewpoint of controlling the dimensional change during the temperature rise process during compression molding, it is preferred that the drying process of the release layer is performed at a temperature of 70 to 150°C under a tension of 0.5 MPa or more and 5 MPa or less. In the drying step of the release layer, which is the final step of the thermal history of the release film of the present invention, the strain of the molecular chain due to the microtension is allowed to remain, so that the expansion deformation during the temperature rise during compression molding can be suppressed. The tension in the drying step is preferably 0.8 MPa or more and 3 MPa or less, and most preferably 1.2 MPa or more and 3 MPa or less. If the tension in the drying step is less than 0.5 MPa, the effect of suppressing the expansion deformation may not be exhibited, and if it is more than 5 MPa, the shrinkage during heating in compression molding may be large, causing wrinkles in the release film or reducing the ability to follow the shape of the mold. In the release film of the present invention, in order to ensure stable releasability, the release layer can also be provided by in-line coating. As a method for providing the coating layer in-line in the film production process, a method is preferred in which a coating layer composition dispersed in water is uniformly applied onto a film that has been at least uniaxially stretched using a metering ring bar or gravure roll, and the coating agent is dried while being stretched, and in this case, the thickness of the release layer after drying is preferably 50 nm or more and 200 nm or less. By performing a stretching process after application of the coating composition, the thickness of the release layer can be made more uniform. In addition, the heat treatment at a higher temperature than that of offline coating increases the degree of hardening of the coating film, improving heat resistance and chemical resistance, and at the same time, there is an advantage that aging treatment after production is unnecessary or can be shortened. Various additives, such as antioxidants, heat stabilizers, ultraviolet absorbers, infrared absorbers, pigments, dyes, organic or inorganic particles, antistatic agents, nucleating agents, etc. may be added to the release layer. The release film of the present invention has a small dimensional change rate and its fluctuation when heated from room temperature to 180°C, so that the occurrence of wrinkles during heating can be suppressed. In addition, since the change in surface free energy at 150°C after heat treatment and after heat stretching is small, it has excellent releasability after high-temperature molding, and is suitable as a release film for circuit manufacturing processes and semiconductor manufacturing processes, and can be particularly suitable for use as a release film for semiconductor encapsulation processes. EXAMPLES

[0030] (1) Polyester composition The polyester resin and film were dissolved in hexafluoroisopropanol (HFIP), 1 H-NMR and 13 The content of each monomer residue component and by-product diethylene glycol can be quantified using C-NMR. In the case of a laminated film, each layer of the film can be scraped off according to the laminate thickness to sample and evaluate the components constituting each layer alone. For the film of the present invention, the composition was calculated by calculation from the mixing ratio at the time of film production.

[0031] (2) Intrinsic viscosity of polyester The intrinsic viscosity of polyester resin and film was measured by dissolving polyester in orthochlorophenol and using an Ostwald viscometer at 25° C. In the case of a laminated film, the intrinsic viscosity of each layer alone can be evaluated by scraping off each layer of the film according to the laminate thickness.

[0032] (3) Film thickness, layer thickness The film was embedded in epoxy resin, and the cross section of the film was cut out with a microtome. The cross section was observed at a magnification of 5000 times with a transmission electron microscope (TEM H7100 manufactured by Hitachi, Ltd.) to determine the thickness of the film and the thickness of the polyester layer.

[0033] (4) Melting point (Tm), melting point of the surface layer (Tms) Measurements and analysis were performed using a differential scanning calorimeter (Seiko Denshi Kogyo, RDC220) in accordance with JIS K7121-1987 and JIS K7122-1987. 5 mg of polyester film was used as a sample, and the temperature at the apex of the endothermic peak obtained from the DSC curve when the temperature was raised from 25°C to 300°C at 20°C / min was taken as the melting point. When multiple endothermic peaks exist, the peak temperature of the endothermic peak on the highest temperature side was taken as the melting point. In the case of a laminated film, the melting point of each layer alone can be measured by scraping off each layer of the film according to the laminate thickness.

[0034] (5) Dimensional change rate (TMA) The film was cut into rectangular samples of 50 mm length x 4 mm width in the MD and TD directions, and heated under the following conditions using a thermomechanical analyzer (Seiko Instruments, TMA EXSTAR6000) to measure the maximum dimensional change rate S1 from 30°C to 150°C, the temperature T1 giving S1, and the dimensional change rate S0 at 40°C. Test length: 15 mm, Load: 19.6 mN, Heating rate: 10°C / min. Measurement temperature range: 30~200℃ Dimensional change rate (%) at temperature T (℃) = [{film length at temperature T (mm) - film length at 30℃ (mm)} / film length at 30℃ (mm)] × 100 The measurements were carried out five times in each of the MD and TD directions, with the sampling positions changed, and the average values ​​of S1, T1, and S0 obtained from the measurements in each direction were used to calculate the values ​​of formula (I) and formula (II). (6) Surface free energy Sa, polarity The surface free energy of the film and the polar component of the surface free energy were calculated as follows: First, the following formula (i) was derived from the extended Fowkes equation and Young's equation. [Extended Fowkes formula] γSL=γS +γL -2(γsd ·γLd )1 / 2 -2(γsD ·γLD )1 / 2 -2(γsh ·γLh )1 / 2 [Young's equation] γS = γSL + γL cosθ γS: Surface free energy of a solid γL: Surface tension of the liquid γSL: Interfacial tension between solid and liquid θ: Contact angle with liquid γsd, γLd: Dispersion force components of γS, γL γsD, γLD: Polar force components of γS and γL γsh, γhL: Hydrogen bond components of γS, γL (γsd ·γLd )1 / 2 +(γsD ·γLD )1 / 2 +(γsh ·γLh )1 / 2=γL (1+cosθ) / 2 (i) Next, the contact angles of the film with four types of liquids, each of which has a known component of surface tension, were measured, and substituted into equation (i). The polar component of the surface free energy of the film was calculated by solving the three-dimensional linear simultaneous equation for each liquid. The numerical calculation software "Mathematica" was used to solve the simultaneous equations. The contact angles were measured using water, ethylene glycol, formamide, and methylene iodide as the measurement liquids, and a contact angle meter CA-D model manufactured by Kyowa Interface Science Co., Ltd. The measurement was performed on both sides of the film (side I / side II) with N=3 each in an environment of 25°C and 65% humidity, and the average value was adopted as the value for each side.

[0035] (7) Surface free energy Sb after heat treatment at 180°C for 3 minutes The film was left to stand for 3 minutes in an oven set at 180° C. The heat-treated film was then removed from the oven, and the surface free energy was measured by the method described in (6). The measurements were performed on both sides of the film (side I / side II) in an environment of 25° C. and 65% humidity, with N=3 for each, and the average values ​​were used as the value for each side. (8) Surface free energy Sc after 50% elongation at 180°C The direction of the main orientation axis at any position of the film was defined as the TD direction, and the direction perpendicular to the TD direction was defined as the MD direction. The film was cut into a rectangular shape of 150 mm long x 30 mm wide in the MD and TD directions to obtain a sample. Using a tensile tester (Orientec Tensilon UCT-100), the film sample was stretched by 50% in the longitudinal direction with an initial tensile chuck distance of 50 mm and a tensile speed of 300 mm / min. The film sample was set in a thermostatic chamber previously set at 180°C and preheated for 90 seconds before stretching. The stretched film sample was then removed from the thermostatic chamber, and the surface free energy was measured by the method described in (6). The measurement was performed on both sides of the film (side I / side II) with N=3 each in an environment of 25°C and 65% humidity, and the average value was adopted as the value for each side.

[0036] (9) Surface elastic modulus Measurements were performed using an AFM (DimensionIcon, manufactured by Burker Corporation) in PeakForceQNM mode, and the obtained force curves were analyzed using the accompanying analysis software "NanoScopeAnalysis V1.40" based on the JKR contact theory to determine the elastic modulus distribution.

[0037] Specifically, following the PeakForceQNM mode manual, the cantilever's warpage sensitivity, spring constant, and tip curvature were configured, and measurements were performed under the following conditions, and the data obtained from the DMT Modulus channel was used as the surface elastic modulus. Note that the spring constant and tip curvature vary depending on the individual cantilever, but we used cantilevers that met the conditions of a spring constant of 0.3 (N / m) to 0.5 (N / m) and a tip curvature radius of 15 (nm) or less, within the range that does not affect the measurement, for use in the measurements.

[0038] The measurement conditions are shown below. Measurement equipment: Atomic force microscope (AFM) manufactured by Burker Corporation Measurement mode: PeakForceQNM (force curve method) Cantilever: Bruker AXS SCANASYST-AIR (Material: Si, spring constant K: 0.4 (N / m), tip curvature radius R: 2 (nm)) Measurement atmosphere: 23℃ in air Measurement range: 3 (μm) square Resolution: 512×512 Cantilever movement speed: 10(μm / s) Maximum pressing load: 10(nN) The data from the DMT Modulus channel was then analyzed using the analysis software "NanoScopeAnalysis V1.40", and the Image Raw Mean and Image Rq values ​​in the Results tab were processed using Roughness to calculate the number average for five randomly selected samples, which were then used as the "surface elastic modulus" and "root mean square of elastic modulus (Rq)". Measurements were performed on both sides of the film (side I / side II) with N=3 each, and the average values ​​were used as the values ​​for each side. (10) Stress at 10% elongation in film MD direction at 150℃ The film was cut into a rectangular sample of 150 mm long x 10 mm wide in the MD direction at an arbitrary position. Using a tensile tester (Orientec Tensilon UCT-100), the film was subjected to a tensile test in the MD direction with an initial tensile chuck distance of 50 mm and a tensile speed of 300 mm / min. The film sample was set in a thermostatic chamber set at 150°C in advance, and the tensile test was performed after preheating for 90 seconds. The load applied to the film when the sample was stretched by 10% (when the chuck distance became 55 mm) was read, and the value divided by the cross-sectional area of ​​the sample before the test (film thickness x 10 mm) was used as the stress at 10% stretch. The measurement was performed with the main orientation axis direction at an arbitrary position of the film as the TD direction, and the direction perpendicular to the TD direction as the MD direction. Sampling was performed at five arbitrary positions, and the average value of the values ​​obtained by measuring each sample was used.

[0039] (11) Uneven thickness of release layer Using the method described in (3), cross-sectional photographs of the film were taken at 10 different positions in each of the MD and TD directions, and the maximum and minimum values ​​of the release layer thickness were calculated from the cross-sectional photographs obtained in each direction and at each position.

[0040] (12) Surface rupture elongation at 180℃ The film sample was cut into a rectangular shape of 150 mm long x 30 mm wide in the MD and TD directions. Using a tensile tester (Orientec Tensilon UCT-100), the film sample was stretched in the longitudinal direction at 5%, 10%, 15%, 20%, 25%, and 30% elongation with an initial tensile chuck distance of 50 mm and a tensile speed of 300 mm / min. The surface of the stretched sample was then observed with an SEM to confirm the presence or absence of surface fracture. Samples were again prepared with the elongation increased by 1% from the highest elongation condition among the samples in which fracture was observed, and the presence or absence of fracture was confirmed in the same manner. The maximum elongation at which fracture occurred was adopted as the surface fracture elongation at 180 °C for that sample. In addition, if no fracture occurred at an elongation of 30%, it was noted as over 30%.

[0041] (13)Puncture strength The film was cut into a square sample measuring 50 mm in length and 50 mm in width in the longitudinal and transverse directions. A puncture test was performed using a tensile tester (Orientec Tensilon UCT-100) with a 0.5 mm diameter needle at a crosshead speed of 5 mm / min to measure the puncture load and puncture displacement. Each measurement was performed five times, and the average of the maximum puncture loads was used as the puncture strength of the sample. The room temperature was controlled to 25°C and 63% Rh. The puncture strength obtained was evaluated according to the following criteria. S: The piercing strength is 4N or more and 7N or less. The average molding depth is 4.5mm or more, and the corner at the center position of the mold recess on the bottom side of the mold is sharply formed. A: The average molding depth is 4.5 mm or more, and the corners on the bottom side of the mold are rounded, but molded. B: The average molding depth is 4.5 mm or more, but there are whitened areas. C: The average forming depth is less than 4.5 mm. A grade of B or above was considered a pass.

[0042] (14) Mold shape conformity The evaluation was carried out using a mold with a concave shape of 150 mm square and 5 mm deep. The release film cut to A4 size was vacuum-sucked into the mold and allowed to follow. The vacuum was then released, and the depth of the removed release film was measured at the corner positions, and the average value for the four corners was taken as the molding depth. Based on the average value of the obtained molding depth and the reproducibility of the mold shape, the mold followability was evaluated as follows: S: The average molding depth is 4.5 mm or more, and the corners at the center position of the mold recess on the bottom side of the mold are sharply formed. A: The average molding depth is 4.5 mm or more, and the corners on the bottom side of the mold are rounded, but molded. B: The average molding depth is 4.5 mm or more, but there are whitened areas. C: The average forming depth is less than 4.5 mm. A grade of B or above was considered a pass.

[0043] (15) Mold releasability An encapsulant (Nagase ChemteX Corporation: product name "R4212-2C") was placed on a 6-inch dummy wafer and placed on the lower die of a compression mold. A release film was vacuum-sucked and fixed to the concave upper die, and then molded to obtain an encapsulation test sample. The die temperature was 130°C, the resin pressure was 3 MPa, and the curing time was 15 minutes. The releasability between the encapsulant and the release film of the obtained encapsulation test sample was evaluated by measuring the peel force when a peel test was performed at a peel angle of 180° and a peel speed of 300 mm / min, and the peel force was measured according to the following criteria. S: Less than 0.3N / 50mm A: 0.3N / 50mm or more, less than 3.0N / 50mm B: 3.0N / 50mm or more and less than 5.0N / 50mm C:5.0N / 50mm or more A grade of B or above was considered a pass.

[0044] (16) Molding appearance 1 For the encapsulation test sample obtained by the method described in (15), the release film was peeled off and the encapsulation material surface was observed visually and under a microscope (100x), and evaluated according to the following criteria. S: No wrinkles are observed visually or by microscopic observation. A: No wrinkles are observed with the naked eye, but wrinkles are observed under a microscope. B: Wrinkles are observed on part of the encapsulant surface both visually and under a microscope. C: Wrinkles are observed over the entire surface of the encapsulant both visually and by microscopic observation. A grade of B or above was considered a pass.

[0045] (17) Molding appearance 2 A dummy epoxy board was set in the lower mold, and a release film was vacuum-sucked and fixed to the upper mold, then the molds were clamped and an encapsulant (HC-300B, Nitto Denko Corporation) was transfer molded under the following conditions: mold temperature 180°C, injection pressure 7.7MPa, and curing time 5 minutes. The encapsulant surface and the release film after peeling off the release film of the obtained encapsulation test sample were observed visually and with a microscope (100x magnification), and judged according to the following criteria. S: No wrinkles are observed visually or by microscopic observation. A: No wrinkles are observed with the naked eye, but wrinkles are observed under a microscope. B: Wrinkles are observed on part of the encapsulant surface both visually and by microscopic observation, or whitening is observed on the release film. C: Wrinkles are observed over the entire surface of the encapsulant both visually and by microscopic observation, or the release film cannot be peeled off. A grade of B or higher was deemed to be acceptable. (18) Hole opening Using a hot needle type perforation machine, holes were made in the release film cut to A4 size with a hole diameter of 0.8 mm and a hole interval of 5 mm x 5 mm (MD x TD). The state of the holes in the obtained release film was observed under a microscope (100x) and judged according to the following criteria. A: There are less than two areas on the A4 size sheet that are not perforated. B: There are 3 to 10 areas on the A4 size sheet that are not perforated. C: There are 10 or more places on the A4 size sheet where no holes are drilled, or the film is torn. A grade of B or above was considered a pass.

[0046] (Production of polyester) The polyester resin used for film formation was prepared as follows.

[0047] (Polyester A) A polyethylene terephthalate resin (intrinsic viscosity 0.65) having 100 mol % terephthalic acid as the dicarboxylic acid component and 100 mol % ethylene glycol as the glycol component.

[0048] (Polyester B) A copolymer polyester (GN001 manufactured by Eastman Chemical Co.) in which 1,4-cyclohexanedimethanol was copolymerized at 33 mol% relative to the glycol component was used as cyclohexanedimethanol-copolymerized polyethylene terephthalate (intrinsic viscosity 0.75).

[0049] (Polyester C) An isophthalic acid copolymerized polyethylene terephthalate resin (intrinsic viscosity 0.7) having, as the dicarboxylic acid component, 82.5 mol % of a terephthalic acid component, 17.5 mol % of an isophthalic acid component, and as the glycol component, 100 mol % of an ethylene glycol component. (Polyester D) Ethoxylated bisphenol A diacrylate 30% copolymerized polyethylene terephthalate. (Polyester E) Polyethylene terephthalate copolymerized with 20 mol% naphthalenedicarboxylic acid. (Polyester F) Polyethylene terephthalate copolymerized with 20 mol% spiroglycol. (Polyester G) Polyethylene terephthalate copolymerized with 30% cyclohexanedicarboxylic acid. (Polyetherimide) Polyetherimide-containing polyethylene terephthalate obtained by compounding 50 parts by mass of Polyester A and 50 parts by mass of PEI “Ultem 1010” manufactured by SABIC Innovative Plastics.

[0050] (Particle Master) Polyethylene terephthalate particle master (intrinsic viscosity 0.65) containing aggregated silica particles with a number average particle diameter of 2.2 μm at a particle concentration of 2 mass% in polyester A. (Release layer 1 forming solution) 20 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd. 1 part by weight of acrylic resin (product name: Aron A-1017) manufactured by Toagosei Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 2 forming solution) 20 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd. 15 parts by weight of acrylic resin (product name: Aron A-1017) manufactured by Toagosei Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 3 forming solution) 10 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd. 15 parts by weight of acrylic resin (product name: Aron A-1017) manufactured by Toagosei Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 4 forming solution) 5 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd. 15 parts by weight of acrylic resin (product name: Aron A-1017) manufactured by Toagosei Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 5 forming solution) 1 part by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd. 15 parts by weight of acrylic resin (product name: Aron A-1017) manufactured by Toagosei Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 6 forming solution) 20 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd.; 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd.; 5 parts by weight of acrylic resin (product name: Aron A-1017) manufactured by Toagosei Co., Ltd.; 20 parts by weight of long-chain alkyl chain-containing compound (product name: Piroil 1010S) manufactured by Ichijo Oil Industries Co., Ltd.; 8 parts by weight of toluene; 8 parts by weight of methyl ethyl ketone (Release layer 7 forming solution) 20 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd.; 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd.; 5 parts by weight of acrylic resin (product name: Aron A-1017) manufactured by Toagosei Co., Ltd.; 10 parts by weight of long-chain alkyl chain-containing compound (product name: Piroil 1010S) manufactured by Ichijo Oil Industries Co., Ltd.; 8 parts by weight of toluene; 8 parts by weight of methyl ethyl ketone (Release layer 8 forming solution) 20 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd. 5 parts by weight of polyester resin (product name: Byron UR-1350) manufactured by Toyobo Co., Ltd. 10 parts by weight of long-chain alkyl chain-containing compound (product name: Piroil 1010S) manufactured by Ipposha Oil Industries Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 9 forming solution) 20 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd. 10 parts by weight of polyester resin (product name: Byron UR-1350) manufactured by Toyobo Co., Ltd. 10 parts by weight of long-chain alkyl chain-containing compound (product name: Piroil 1010S) manufactured by Ichijo Oil Industries Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 10 forming solution) 30 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd. 15 parts by weight of acrylic resin (product name: Aron A-1017) manufactured by Toagosei Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 11 forming solution) 40 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd. 15 parts by weight of acrylic resin (product name: Aron A-1017) manufactured by Toagosei Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 12 forming solution) 50 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Miwa Laboratory Co., Ltd. 15 parts by weight of acrylic resin (product name: Aron A-1017) manufactured by Toagosei Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 13 forming solution) 20 parts by weight of methylated melamine formaldehyde (product name: Nikalac MX-706) manufactured by Sanwa Chemical Co., Ltd. 0.4 parts by weight of paratoluenesulfonic acid amine manufactured by Sanwa Laboratory Co., Ltd. 8 parts by weight of toluene 8 parts by weight of methyl ethyl ketone (Release layer 14 forming solution) Kyoeisha Chemical Co., Ltd. acrylic resin "Product name: SMP-250AP" 50 parts by mass: Chukyo Yushi Co., Ltd. "Product name: Rezem N-137" 40 parts by mass: BASF Japan Ltd. "Product name "Irgacure" (registered trademark) 184" 3.0 parts by mass: Ethylene glycol monobutyl ether 20 parts by mass Example 1 The composition is as shown in the table, and the raw materials are fed to separate vented co-rotating twin screw extruders with an oxygen concentration of 0.2% by volume, and melted at a cylinder temperature of 270°C for the A layer extruder and a cylinder temperature of 277°C for the B layer extruder. The short pipe temperature after the A layer and B layer are joined is 277°C, the die temperature is 280°C, and the T die is discharged in the form of a sheet onto a cooling drum whose temperature is controlled at 25°C. At that time, electrostatic charge is applied using a wire electrode with a diameter of 0.1 mm, and the sheet is adhered to the cooling drum to obtain an unstretched sheet. Next, the film temperature is increased with a heating roll before stretching in the longitudinal direction, and the film is stretched 3.1 times in the longitudinal direction at a stretching temperature of 85°C, and immediately cooled with a metal roll whose temperature is controlled at 40°C.

[0051] Next, the film was stretched 3.5 times in the width direction in a tenter-type transverse stretching machine with a preheating temperature of 100°C and a stretching temperature of 120°C, and then heat-treated at a constant length in the tenter at a temperature of 240°C for 15 seconds. After that, a 3% relaxation treatment was performed at the same temperature, and then a 2% relaxation treatment was performed at a temperature of 200°C to obtain a substrate film with a thickness of 55 μm. The release layer 1 forming solution was then applied to the substrate film by gravure coating, and the substrate was then transported to an oven, where the temperature was 100°C, the transport tension was 0.6 MPa, and the draw setting was 0.40% in the first half of the drying (step A), and the temperature was 110°C, the transport tension was 0.6 MPa, and the draw setting was 0.40% in the second half of the drying (step B), to dry the solution and obtain a release film with a release layer thickness of 135 nm. The evaluation results of each characteristic are shown in Table 2.

[0052] (Examples 2 to 46, Comparative Examples 1 to 5) A release film having a thickness of 55 μm was obtained in the same manner as in Example 1, except that the film configuration, the formulation of the release layer, and the drying conditions were changed as shown in Tables 1, 3, 5, 7, 9, and 11. The evaluation results of each property are shown in Tables 2, 4, 6, 8, 10, and 12. (Example 47) The composition was as shown in the table, and the raw materials were fed to separate vented co-rotating twin-screw extruders with an oxygen concentration of 0.2% by volume, and kneaded at a cylinder temperature of 270°C for the A layer extruder and a cylinder temperature of 277°C for the B layer extruder. Next, after passing through five FSS-type leaf disc filters, the materials were merged in a feed block with 387 slits while being metered with a gear pump, to obtain a laminate in which 387 layers were alternately laminated in the thickness direction with a lamination ratio of 4.0 (B layer / A layer). Here, the slit length and interval were all constant. The obtained laminate had 194 layers of polyester A and 193 layers of polyester B, which were alternately laminated in the thickness direction. The laminate was fed to a T-die and formed into a sheet, and then quenched and solidified on a casting drum whose surface temperature was kept at 25°C while applying an electrostatic voltage of 8 kV with a wire, to obtain an unstretched cast film. Thereafter, a release film with a film thickness of 55 μm was obtained in the same manner as in Example 1. The evaluation results of each property are shown in Table 16. In the above examples, Examples 1 to 4 2 , and 46 are Reference Examples 1 to 4, respectively. 2 , and 46 shall be read as follows.

[0053] [Table 1]

[0054] [Table 2]

[0055] [Table 3]

[0056] [Table 4]

[0057] [Table 5]

[0058]

Table 6

[0059]

Table 7

[0060]

Table 8

[0061]

Table 9

[0062]

Table 10

[0063]

Table 11

[0064]

Table 12

[0065]

Table 13

[0066]

Table 14

[0067]

Table 15

[0068] [Table 16] [Industrial Applicability]

[0069] The release film of the present invention has a small dimensional change rate and its fluctuation when heated from room temperature to 200°C, so that the occurrence of wrinkles during heating can be suppressed. In addition, since the change in surface free energy after heat treatment and after thermal elongation is small, it has excellent releasability after high-temperature molding, and is suitable as a release film for circuit manufacturing processes and semiconductor manufacturing processes, and can be particularly suitable for use as a release film for semiconductor encapsulation processes.

Claims

1. When the maximum dimensional change rate from 30°C to 150°C when the temperature is raised from 30°C to 200°C at a rate of 10°C / min, as measured by thermomechanical analysis (TMA), is S1 (%), the temperature giving S1 is T1 (°C), and the dimensional change rate at 40°C is S0 (%), the film satisfies the following formulas (I) and (II); and the surface free energy Sa (mN / mm) at 25°C, the surface free energy Sb (mN / mm) after heat treatment at 180°C for 3 minutes, and the surface free energy Sc (mN / mm) after 50% elongation at 180°C satisfy the following formulas (III) and (IV) on at least one side of the film, A laminated polyester film having a polyester A layer and a polyester B layer having a melting point lower than that of the polyester A layer, the A layer and the B layer being laminated alternately in 3 to 1000 layers, the polyester A layer containing a polyester containing at least one copolymer component selected from bisphenol A ethylene oxide, spiroglycol, cyclohexane dicarboxylic acid, and naphthalene dicarboxylic acid, and / or a polyetherimide, When the following formulae (III) and (IV) are satisfied on one side of the film, |Sa-Sb| is 0.1 or more and Sb is 47.5 or more on the side opposite to the side satisfying the formulae (III) and (IV), and when the following formulae (III) and (IV) are satisfied on both sides of the film, |Sa-Sb| is 0.1 or more and Sb is 47.5 or more on one side of the film. Release film for processing. 0≦S1≦1.5...(I) 0≦|S1-S0| / (T1-40)≦0.050...(II) 0≦|Sa-Sb|≦15...(III) 0≦|Sa-Sc|≦15...(IV)

2. 2. The process release film according to claim 1, wherein the surface elastic modulus of at least one surface is 50 to 3000 MPa as measured using an atomic force microscope.

3. The release film for process use according to claim 1 or 2, wherein the root mean square (Rq) of the surface elastic modulus on at least one side is 50 to 500 MPa.

4. The process release film according to any one of claims 1 to 3, wherein the maximum temperature (Tm) of the melting peak observed by a differential scanning calorimeter (DSC) is 240°C or higher and 265°C or lower.

5. The release film for process use according to any one of claims 1 to 4, wherein the polar strength of the film surface on at least one side is 0.1 mN / m or more and 5.0 mN / m or less.

6. The release film for process use according to any one of claims 1 to 5, having a release layer having a thickness of 50 nm or more and 500 nm or less on at least one surface.

7. The release film for manufacturing processes according to claim 6 , wherein the thickness unevenness of the release layer is 50 nm or less.

8. The release film for process use according to any one of claims 1 to 7, having a surface breaking elongation at 180 ° C. of more than 0% and not more than 30%.

9. The release film for process use according to any one of claims 1 to 8, having a puncture strength of 2 N or more and 10 N or less.

10. The process release film according to any one of claims 1 to 9, which has a polyester A layer having a thickness of 3 µm or more and 10 µm or less within a thickness range of 10 µm or less from the outermost surface of the film.

11. The release film for process use according to any one of claims 1 to 10, which is used as a process film in semiconductor manufacturing.

12. The release film for process use according to any one of claims 1 to 11, which is used for semiconductor compression molding (compression molding).

Citation Information

Patent Citations

  • Laminated film for molding simultaneous transfer

    JP2012224082A

  • Release sheet for semiconductor compression molding, and semiconductor package molded by use thereof

    JP2016092272A

  • Mold releasing film for semiconductor mold

    JP2016127091A

  • Method for producing fiber-reinforced composite material

    JP2017013455A

  • Processing release film excellent in appearance of molding, use thereof, and method for producing resin sealed semiconductor using the same

    JP2017177463A