Large-area copper nanofoams with hierarchical structures for use as electrodes
A novel pack cementation and dealloying process for copper foil produces hierarchical nanoporous copper electrodes with enhanced mechanical properties and capacity, significantly outperforming traditional graphite anodes in lithium-ion batteries.
Patent Information
- Application Number
- JP2021535178
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-18
- Filing Date
- 2019-12-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-12-18
AI Technical Summary
Existing methods for producing dealloyed nanoporous copper result in small size and poor mechanical properties, limiting their application in high-performance electrodes for energy devices.
A pack cementation process using copper foil to form a precursor alloy, followed by dealloying, produces hierarchical microporous or nanoporous copper with improved mechanical properties and large surface area, suitable for use as electrodes in lithium-ion batteries.
The method results in electrodes with four times higher areal capacity and stable performance over 20 cycles compared to traditional graphite anodes, effectively addressing the limitations of previous methods.
Smart Images

Figure 0007590327000002 
Figure 0007590327000003 
Figure 0007590327000004
Abstract
Description
[Technical field]
[0001] explanation CROSS-REFERENCE TO RELATED APPLICATIONS This patent application claims the benefit of U.S. Patent Application No. 62 / 781,579, filed December 18, 2018, and is incorporated by reference, along with all other references referenced in this application.
[0002] 2. Background of the Invention The present invention relates to the field of metal electrodes, and in particular to techniques for fabricating large area copper nanofoams with hierarchical structures for use as high performance electrodes in energy devices and energy storage cells, including batteries. [Background technology]
[0003] No technology is yet available for producing dealloyed nanoporous copper, because any results would involve the use of metal "powders" to create the precursor alloy prior to dealloying, resulting in small size and poor mechanical properties. Summary of the Invention [Problem to be solved by the invention]
[0004] Therefore, there is a need for improved electrode materials with carefully designed structures for lithium-ion batteries to improve capacity and power performance for use in modern mobile and electronic devices. [Means for solving the problem]
[0005] BRIEF SUMMARY OF THE INVETION The facile synthesis is based on a pack cementation process using copper foil instead of copper powder. Depending on the pack cementation time and the amount of aluminum, hierarchical microporous or nanoporous copper is produced, which can be coated with tin for use as a lithium-ion battery anode. Coin cell testing of the nanocopper foam anode showed a four-fold higher areal capacity (7.4 milliamp-hours per square centimeter without performance degradation up to 20 cycles) compared to conventional graphite anodes due to the extremely high surface area.
[0006] In the technique, a pack cementation process was used to fabricate precursor alloys in the form of foils, and a dealloying process was used to form nanoscale copper struts and pores across the specimens, resulting in hierarchical microporous or nanoporous or full nanoporous copper (NPC). Furthermore, this method can be used to fabricate large area nano copper foams based on a new foil-based process with high reproducibility and suitable mechanical properties. This method is a much simpler manufacturing process compared to the conventional methods.
[0007] As a representative example, an aluminum-copper alloy precursor foil was selected and processed with an aluminum concentration that can vary from about 20 atomic percent to about 85 atomic percent. When subsequently etched away, the aluminum concentration can indicate porosity. The alloy precursor can be reacted with a dealloying solution (HCl). The ligament size can be varied from about 50 nanometers to about 500 nanometers, and the pore size can be controlled from about 10 nanometers to about 10 microns due to different corrosion behavior for different aluminum-copper phases.
[0008] To form an aluminum-copper precursor alloy foil, the pack cementation temperature may vary from about 400° C. to about 900° C. The dealloying solution may be about 0.01 molar to about 20 molar hydrochloric acid (HCl) solution at about 20° C. to about 100° C. The pack cementation may include a mixed powder pack of one or more metal powders, fillers, and halide salt activators.
[0009] A dealloying process can be performed on the produced precursor alloy based on the chemical corrosion potential difference with respect to a standard hydrogen electrode, therefore aluminum can be replaced with other elements having higher corrosivity than copper. For example, the other elements can be magnesium (Mg), silicon (Si), chromium (Cr), niobium (Nb), zinc (Zn), titanium (Ti), molybdenum (Mo), tin (Sn), or manganese (Mn), or any combination. The halide salt can be sodium chloride (NaCl), sodium fluoride (NaF), or ammonium chloride (NH4Cl), or any combination.
[0010] The pack cementation temperature can be set below the melting temperature of the metal precursor. The dealloying solution is a mixture of hydrogen chloride (HCl), sodium hydroxide (NaOH), nitric acid ( HNO 3), phosphoric acid (H3PO4), or perchloric acid (HClO4), or a combination thereof.
[0011] The fabricated hierarchical microporous, nanoporous or full nanoporous copper (NPC) can be used in various energy devices due to its large surface area and unique three-dimensional structure. One example is as a lithium-ion battery anode current collector after coating with tin active material, which can react with and store lithium ions and absorb the volume expansion well during the charge and discharge cycling process.
[0012] The nano copper foam anode can be filled with additional anode active materials such as graphite-based materials, metal-based materials, or oxide-based materials, and the additional anode active materials can be selected from one of artificial graphite, natural graphite, soft carbon, hard carbon, tin-lithium based alloys, silicon-lithium based alloys, indium-lithium based alloys, antimony-lithium based alloys, germanium-lithium based alloys, bismuth-lithium based alloys, gallium-lithium based alloys, and oxide-based materials including tin dioxide (SnO2), cobalt oxide (Co3O4), copper oxide (CuO), nickel oxide (NiO), or iron oxide (Fe3O4), or a combination.
[0013] Other objects, features and advantages of the present invention will become apparent from consideration of the following detailed description and the accompanying drawings, in which like reference characters represent like features throughout. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic diagram showing a proposed new synthesis method for producing nanoporous or microporous or nanoporous copper using a pack cementation aluminum cladding process on copper foil to produce large area nanocopper foam, more specifically, depending on the size of the initial copper foil used, the area of the final nanocopper foam product can be relatively easily scaled up. [Diagram 2] 2A-2F show the x-ray diffraction patterns of the P3H and P6H samples after dealloying and the corresponding SEM images of the surface of the nanoporous copper foam samples. [Diagram 3] 3A-3F show the x-ray diffraction patterns of the dealloyed p12h and p15h samples and the corresponding SEM images of the surfaces of the hierarchical nanoporous copper foams. [Figure 4A] FIG. 13 shows the cycling performance of a SnO / CuSn / CuO / Cu lithium ion battery anode from about 0.01 to 3.0 volts and about 1 milliamp per square centimeter. [Figure 4B] FIG. 1 shows a comparison of the areal capacitance of a SnO / Cu3Sn / Cu2O / Cu anode with that of similar nanoscale anode materials. [Diagram 5] FIG. 1 shows a plot of the change in aluminum composition and coating thickness of an aluminum-copper alloy precursor foil with increasing time for a pack cementation process conducted at about 800 degrees Celsius. [Figure 6] 6A-6F show scanning electron microscope (SEM) cross-sectional images of copper foil samples during the pack cementation aluminum cladding process (a: p15m, b: p30m, c: p3h, d: p6h, e: p12h, and f: p15h) comparing the thickness increase of the copper foil samples. [Figure 7] 7A-7D show SEM images of the surfaces of the dealloyed packed cementation samples (a: P15M and b: P30M) and the corresponding X-ray diffraction patterns, showing that the X-ray diffraction patterns of both the P15M and P30M samples reveal the presence of only copper and Cu9Al4 phases. [Figure 8] Figure 1 shows a backscattered SEM image of the p15h sample showing a continuous network of solid-solution α-Al (dark areas: A) and Al2Cu (light areas: B) that, when unfolded, produced uniform three-dimensionally connected α-Al and Al2Cu phases that formed microporosity and nanoporosity, respectively. [Figure 9] FIG. 1 shows a comparative plot of strut size distribution within nanoporous and microporous or nanoporous copper samples using standard metallographic techniques. [Figure 10] FIG. 1 is a schematic diagram illustrating the dealloying mechanism of hierarchical microporous or nanoporous copper samples produced according to the techniques described in this patent, showing that upon dealloying, the intermetallic AlCu phase creates nanoporosity while the solute α-Al phase creates microporosity. [Figure 11]FIG. 1 shows the x-ray diffraction patterns of P15H microporous or nanoporous copper samples after tin coating using electroless plating method with heat treatment at about 150 degrees Celsius for about 1 hour. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Detailed Description of the Invention Nanoporous metal structures may provide beneficial properties such as significant specific surface area, low density, and efficient catalysis due to their unique three-dimensional structure. As such, nanoporous metal structures may be used in energy device applications such as electrocatalysis, actuators, and energy storage (e.g., batteries and secondary batteries). Various syntheses of nanoporous metals may be produced using different methods, such as chemical dealloying, metal dissolution dealloying, and oxygen plasma dealloying. Chemical dealloying is the most commonly used method for producing nanoporous metals, which are generally composed of pores with an average diameter of less than 100 nanometers. In this case, chemical dealloying selectively dissolves one or more elements (base metals) from the alloy using various acidic or base solutions.
[0016] Recently, nanoporous copper (NPC) with interconnected nano-sized pore structure has been discussed. Few production methods have been developed to prepare alloy precursors before dealloying, such as powder metallurgy, electrolytic plating, and ingot casting. All of these precursor methods have problems to overcome for their use in practical applications due to their complexity and limitations in producing large-sized samples. In particular, common powder metallurgy methods require high pressure and high temperature to completely solidify two or more different powders. As a result, nanoporous copper produced using this method usually exhibits micro-sized defects that eventually lead to cracks during the dealloying process (or in the final nanoporous copper).
[0017] In order to improve the mechanical properties and enlarge the area of the final nanoporous copper samples, a new simple dealloying technique is described in combination with a pack cementation aluminum coating process for copper foils. That is, a uniform thin layer of aluminum is coated on the prepared copper foils using the pack cementation method to produce copper-aluminum alloy precursors in the subsequent heat treatment process, and this technique allows the production of large-area nanocopper foam samples by preparing large initial copper foils. Depending on the desired final porosity and pore structure, the thickness of the aluminum coating layer can be precisely controlled by controlling the pack cementation time and temperature.
[0018] By slightly manipulating the phases present in the aluminum-copper alloy precursor, it was possible to generate hierarchically structured microporous or nanoporous copper along with conventional nanoporous copper. More specifically, intrinsic hierarchical microporous or nanoporous copper was generated by optimizing the composition and heat treatment process. This was based on the phase diagram between aluminum and copper, where two phases consisting of solid solution α-Al and intermetallic Al2Cu can be formed. In this case, the solid solution phase of α-Al can be preferentially etched away in acidic solution to generate micropores between the intermetallic Al2Cu cellular phases, which are then also etched away to form nanopores. It is expected that the hierarchical organization with a combination of nanopores and micropores (due to its large surface area) can be promisingly applied for use in various electrocatalysts and other energy-related fields that require high electrochemical efficiency, such as lithium-ion batteries (LIBs).
[0019] To demonstrate the promising energy device applications of microporous or nanoporous copper produced by this technique, it was used as a high-performance anode of lithium-ion batteries after being coated with tin as the anode active material (by an electroless plating process), without any binder or conductive agent. Tin, which can form various alloys with lithium, has recently attracted much attention as a high-capacity anode active material for high-performance lithium-ion batteries because it has a higher theoretical capacity (e.g., 991 milliampere hours per gram) than graphite (e.g., 372 milliampere hours per gram). However, it remains a significant drawback when applied in conventional lithium-ion battery anodes. Tin undergoes severe volume expansion (up to 300%) during the insertion or extraction of lithium ions during the charge or discharge process, which ultimately leads to premature cycling failure for copper foil anode designs.
[0020] This study demonstrates that hierarchical microporous or nanoporous copper coated with tin can help to solve the problems caused by the use of tin during cycling. The structural properties were investigated and the lithium-ion battery anode performance of microporous or nanoporous structured three-dimensional (3-D or 3D) porous copper-tin anodes was compared with that of nanostructured tin-based anodes. Microstructural examination was performed using x-ray diffraction (XRD), scanning electron microscopy (SEM), and energy dispersive X-ray spectroscopy (EDS). Additionally, the capacity and cycling performance of the tin-coated microporous or nanoporous copper anodes were analyzed.
[0021] Experimental example 1: Preparation of nanoporous copper samples Prior to dealloying, the aluminum-copper alloy precursor was synthesized using the pack cementation method. Figure 1 is a schematic diagram showing the overall processing route. The first step shows the mixing of powders used in the pack cementation process. The powders consisted of 3 wt% NH4Cl powder (100 micron, Alfa Aesar, USA) as the activator, 15 wt% pure aluminum powder (99.8%, +325 mesh, Alfa Aesar, USA) as the coating metal source, and 82 wt% Al2O3 powder (60 μm, Alfa Aesar, USA) as the filler. Mechanical mixing (8000-D Mixer Mill, SPEX SamplePrep, USA) was performed for 30 min to obtain a homogeneously mixed powder. After mixing, packing and sealing (Fig. 1b) was carried out with a stainless steel container for the next heat treatment step, followed by pack cementation (Fig. 1c) at a constant 800°C for 15 min, 30 min, 3 h, 6 h, 12 h, or 15 h to form different aluminum copper alloy precursor foils for comparison in an air tube furnace. The pack cemented aluminum copper alloy precursor foils are hereafter referred to as P15M, P30M, P3H, P6H, P12H, and P15H. At the end of the pack cementation process, the sealed container was immersed in water. Then, a further heat treatment process (Fig. 1d) was carried out in a tube furnace with an argon atmosphere at 500°C for 9 h or 700°C for 6 h for homogenization. Then, a dealloying process (Fig. 1e) of the aluminum copper alloy precursor was carried out at 50°C with 3 wt% HCl solution to etch away the aluminum atoms from the aluminum copper alloy. The final nanoporous copper was washed with absolute alcohol. The microstructures of the pack-cemented aluminum-copper alloy precursor foil and the dealloyed nanoporous copper samples were characterized and analyzed using a SEM (JSM7401F, JEOL) coupled with an EDS analyzer. XRD (Rigaku Ultima III X-ray diffractometer) with copper K-alpha radiation (wavelength of 1.5406 Å) was also used to determine the alloy phase between aluminum and copper.
[0022] Experimental example 2: Electroless tin coating process To demonstrate the performance of the synthesized nanoporous copper as a lithium-ion battery anode, a high-capacity anode active material (tin) was coated onto the nanoporous copper by electroless plating. The nanoporous copper was immersed in a tin plating solution at 60 degrees Celsius for 1 minute. The tin plating solution consisted of 200 milliliters of deionized water containing 2 grams of tin(II) chloride dihydrate (SnCl2·2H2O), 2 grams of sodium phosphate monohydrate (NaH2PO2·2H2O), 10.5 grams of thiourea (CS(NH2)2), and 0.84 milliliters of concentrated acid salt. The tin-coated nanoporous copper anode sample was then heat-treated in a tube furnace in a nitrogen atmosphere at 150 degrees Celsius for 1 hour.
[0023] Experimental example 3: Lithium-ion coin battery cycle test A copper disk with dimensions of 11 millimeter diameter and 250 microns thickness was prepared. CR2032 type coin cells were assembled in a glove box with a dry argon atmosphere using the tin-coated nanoporous copper anode coupon as the working electrode and lithium metal foil for both the counter and reference electrodes. The electrolyte was a conventional 1.3 molar LiPF6 solution in ethylene carbonate (EC) and diethylene carbonate (DEC) at a volume ratio of 3:7. Galvanostatic tests were performed on the assembled coin cells containing the tin-coated nanoporous copper anode coupon at a current density of 1 milliamp per square centimeter at a voltage range of 3.0 volts to 0.01 volts (vs. Li-ion / Li) at 25 degrees Celsius.
[0024] Example results: Processing of aluminum-copper precursors based on pack cementation Different aluminum-copper alloy precursor foils with compositions ranging from 9.7 atomic percent aluminum to 79.6 atomic percent aluminum were obtained by varying the pack cementation time from 15 minutes to 15 hours. The thickness of the foil samples increased from 255.0 ± 0.5 to 1139.6 ± 26.6 microns as the pack cementation time increased up to 15 hours (Table S1, Figure 5, and Figures 6A-6F).
[0025] Table S1 provides a list of aluminum-copper alloy precursor samples with different pack cementation times ranging from 15 min to 15 h. The relative compositions of aluminum and copper were estimated as atomic percentages based on weight measurements before and after the pack cementation process. The main phases present after the homogenization process were identified by x-ray diffraction.
[0026] [Table 1]
[0027] Only if the aluminum composition is high enough, three-dimensionally connected nanoporous copper can be obtained by dealloying. The p15m and p30m samples contain only copper and Cu9Al4 phases. These samples have a low aluminum content, which cannot penetrate the inside of the sample and react with the dealloying solution (Figures 7A-7D). The type of dealloying solution (e.g., hydrochloric acid or sodium hydroxide) also affects the corrosion behavior of each constituent phase present in the alloy precursor. For example, the aluminum-copper phase has good stability in hydrochloric acid (HCl) solution, while the aluminum and Al2Cu phases do not. Thus, the Al2Cu and α-Al phases become unstable and tend to produce nanoporous copper only when hydrochloric acid solutions are used.
[0028] Figures 2A-2F show the XRD patterns of the P3H and P6H samples, where all peaks correspond only to the Al2Cu phase, which can generate uniform three-dimensional nanopores when dealloyed. As a result, both the P3H (Figures 2D-2E) and P6H (Figures 2F-2F) samples were able to dissolve the entire aluminum in hydrochloric acid solution and form pure nanoporous copper ligaments throughout the thickness of the samples. The average ligament sizes of the P3H (Figures 2D-2E) and P6H (Figures 2F-2F) samples (after dealloying) were estimated to be 150±64 nanometers and 125±26 nanometers, respectively. The ligament size of the nanoporous copper after dealloying decreased as the aluminum content increased due to the formation of finer Al2Cu phases.
[0029] Also, Figures 3A-3F show the x-ray diffraction patterns of the p12h (Figures 3C-3D) and p15h (Figures 3E-3F) samples, which contain only solute α-Al and Al2Cu phases. It is interesting to note that both the p12h and p15h samples are composed of hierarchically structured micropores or nanopores throughout the entire sample. The average micropore diameters of the p12h and p15h samples are calculated to be 5.5 ± 2.2 microns and 6.5 ± 2.4 microns, respectively. The average micropore diameter of the p15h sample is 18% larger compared to the p12h sample. This is because the amount of solute α-Al is larger compared to the p15h sample, generating larger micropores between the copper struts.
[0030] Along the micropores, each copper strut consists of nanoscale pores between randomly structured nano-sized ligaments. The average thickness of the nano-sized ligaments is estimated to be 209.8 ± 100.7 nm and 98.7 ± 46.7 nm for the p12h and p15h samples, respectively (Figure 9). Furthermore, the backscattered SEM image of the p15h sample clearly shows a uniform and continuous network of α-Al (dark areas) and Al2Cu (light areas) phases (Figure 8). During the dealloying process, the α-Al phase dissolves first to generate the micropores. The Al2Cu phase subsequently dissolves to generate nanopores in each of the microscale Al2Cu struts, as shown diagrammatically in Figure 10.
[0031] Lithium-ion battery cycling performance of hierarchical porous copper as anode For potential use as high-performance lithium-ion battery anodes, hierarchical microporous or nanoporous copper samples (P15H) were applied as both anode current collectors and porous substrates for tin coating. The hierarchical electrode structure with well-developed porosity could be a rational design to mitigate the large volume change of tin during repeated charge or discharge processes.
[0032] FIG. 11 shows the x-ray diffraction pattern of microporous or nanoporous copper coated with tin with additional heat treatment at 150° C. for 1 hour. The heat treated tin coated copper foam anode shows diffraction peaks of SnO / Cu3Sn / Cu2O / Cu phases. The Cu2O phase typically forms at temperatures between 70° C. and 130° C. Furthermore, the intermetallic phase of Cu3Sn is known to be inert towards reaction with lithium ions, and the homogeneous presence of such inert material (as in the composite) favorably buffers volume changes during charge or discharge processes.
[0033] Figure 4A shows the cycling performance of a tin-coated microporous or nanoporous copper anode at 1 milliamp per square centimeter in the range of 0.01 to 3 volts. The first discharge capacity of this sample is up to 10.9 milliamp hours per square centimeter. The second and third discharge capacities are 8.3 and 8.0 milliamp hours per square centimeter, respectively. The slightly reduced capacity in the initial cycle is due to irreversible reactions associated with the SnO and Cu2O oxide active materials. In addition to this, the discharge capacity was stable at 7.4 milliamp hours per square centimeter at the 12th cycle without any performance degradation being observed. In contrast, previous reports have revealed severe capacity degradation and premature failure of tin-based anodes during the initial cycles.
[0034] Figure 4B shows a comparison of the performance of tin-coated microporous or nanoporous copper anodes with similar nanoscale anode materials such as nanoparticles, nanosheets, and nanowires that have been developed in recent years. The tin-coated microporous or nanoporous copper anodes (fabricated in this approach using a novel copper foil-based pack cementation process) show superior areal capacitance performance compared to other similar nanostructured anode materials under similar current density conditions. For example, they show approximately four times higher areal capacitance than conventional graphite anodes.
[0035] In this patent, it is shown that by effectively reducing the stress caused by the large volume expansion of the tin active material during the charge / discharge process, the tin-coated hierarchical microporous or nanoporous copper anode is stable and capable of improving capacity. More specifically, without the addition of binders and conductive agents, the microporous or nanoporous copper or tin anode integrated as both the current collector and the active anode material delivered an outstanding reversible capacity of 7.4 milliamp-hours per square centimeter after 20 cycles. The practical applications of hierarchical microporous or nanoporous copper are not limited to the application of lithium-ion battery anodes, but can also be applied to other energy fields where the extremely large surface area and unique pore structure can be utilized.
[0036] FIG. 5 shows a plot of the aluminum composition change and coating thickness of an aluminum-copper alloy precursor foil with increasing time of the pack cementation process carried out at 800 degrees Celsius.
[0037] Figures 6A-6F show SEM cross-sectional images of copper foil samples during the pack cementation aluminum cladding process (a: P15M, b: P30M, c: P3H, d: P6H, e: P12H, and f: P15H), where the thickness increase of the copper foil samples is compared.
[0038] Figure 7 shows the SEM images and corresponding x-ray diffraction patterns of the surfaces of the packed cementation samples (a: P15M and b: P30M) after dealloying. The x-ray diffraction patterns of both the P15M and P30M samples show the presence of only copper and Cu9Al4 phases. Note that the presence of only two phases does not allow complete dealloying throughout the interior of the samples due to the low aluminum content. However, only the outer surface of the samples was dealloyed, producing multiple irregular surface pores (as shown in the SEM images).
[0039] Figure 8 shows a backscattered SEM image of the p15h sample, which shows a continuous network of solid-solution α-Al (dark areas: A) and Al2Cu (light areas: B). When unfolded, the uniform three-dimensionally connected α-Al and Al2Cu phases generated micropores and nanopores, respectively.
[0040] FIG. 9 shows a comparative plot of strut size distribution in nanoporous and microporous or nanoporous copper samples using standard metallographic techniques.
[0041] Figure 10 is a schematic diagram showing the dealloying mechanism of the hierarchical microporous or nanoporous copper samples fabricated as described above. Upon dealloying, the solute α-Al phase generates micropores, while the intermetallic Al2Cu phase generates nanopores.
[0042] FIG. 11 shows the X-ray diffraction patterns of P15H microporous or nanoporous copper samples after tin coating using electroless plating method with heat treatment at 150 degrees Celsius for 1 hour.
[0043] conclusion A simple dealloying method was successfully developed in combination with a pack cementation aluminum cladding process for copper foil to prepare copper-aluminum alloy precursors with about 10-80 atomic percent aluminum. A pack cementation time of 15 hours at 800 degrees Celsius resulted in two phases, solute α-Al and intermetallic Al2Cu, which could be dealloyed to produce hierarchically structured microporous or nanoporous copper. In this case, the solute α-Al phase could be preferentially etched away in acidic solution, leaving behind micropores. The Al2Cu phase could then generate nanopores in the Al2Cu microscale struts.
[0044] To demonstrate the promising energy applications of microporous or nanoporous copper, it was applied as a high-performance anode in lithium-ion batteries after being coated with metallic tin as the anode active material (by electroless plating process), which resulted in a SnO / Cu3Sn / Cu2O / Cu phase combination. In addition to this, the tin-coated hierarchical microporous or nanoporous copper anode exhibited four times higher capacity compared to conventional graphite. This was obtained by the favorable adoption of tin active material coating by effectively reducing the stress caused by the large volume expansion during the charging or discharging process.
[0045] The description of the invention has been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form described, and many modifications and variations are possible in light of the above teachings. The embodiments were chosen and described in order to best explain the principles of the invention and its practical application. This specification will enable those skilled in the art to better utilize and practice the invention in various embodiments and with various modifications to adapt it to a particular use. The scope of the invention is defined by the following claims.
Claims
1. producing a precursor alloy in the form of a foil consisting of two phases of solid solution α-Al and intermetallic Al 2 Cu using a pack cementation process; Dealloying the precursor alloy; and forming nanoscale copper struts and pores throughout the sample using the dealloyed precursor alloy; obtaining said sample of hierarchical micro / nanoporous copper or full nanoporous copper.
2. The foil of the precursor alloy comprises an aluminum-copper alloy resulting from the pack cementation process of copper foil, the aluminum concentration being between about 20 atomic percent and about 85 atomic percent, and the method further comprises: treating the precursor alloy with a dealloying solution of hydrochloric acid, the ligament size being variable between about 50 nanometers and about 500 nanometers, the method further comprising:
10. The method of claim 1, comprising controlling the pore size from about 10 nanometers to about 10 microns due to different corrosion behavior for different aluminum-copper phases.
3. The method of claim 2 comprising selecting a pack cementation temperature between about 400 degrees Celsius and about 900 degrees Celsius when forming the precursor alloy.
4. The method of claim 2, wherein the dealloying solution is about 0.01 molar to about 20 molar hydrochloric acid solution at about 20 degrees Celsius to about 100 degrees Celsius.
5. 10. The method of claim 1, wherein the pack cementation process includes using a mixed powder pack of one or more metal powders, a filler, and a halide salt activator.
6. The dealloying process can be performed on the precursor alloy produced based on a chemical corrosion potential difference with respect to a standard hydrogen electrode; 3. The method of claim 2, wherein aluminum can be replaced with other elements having a higher corrosiveness compared to copper, which can include materials selected from the group consisting of magnesium (Mg), silicon (Si), chromium (Cr), niobium (Nb), zinc (Zn), titanium (Ti), molybdenum (Mo), tin (Sn), and manganese (Mn).
7. The halide salt activators include sodium chloride (NaCl), sodium fluoride (NaF), and ammonium chloride (NH 4 6. The method of claim 5, wherein the material is selected from the group consisting of:
8. The method of claim 7 , wherein the pack cementation temperature can be set below the melting temperature of the metal precursor.
9. The dealloying solution is a mixture of hydrogen chloride (HCl), sodium hydroxide (NaOH), nitric acid (HNO 3 ), phosphoric acid (H 3 P.O. 4 ), and perchloric acid (HClO 4 3. The method of claim 2, wherein the compound is selected from the group consisting of:
10. 13. The method of claim 1, wherein the fabricated hierarchical micro / nanoporous copper or full nanoporous copper (NPC) has a large surface area and unique three-dimensional structure for use in various energy devices.
Citation Information
Patent Citations
Method for preparing nano porous copper thin film material by magnetron sputtering
CN105543796A
Independent coagulation structure
JP1980073346A
Nano-porous metal and production method therefor
JP2008184671A
Negative electrode for lithium ion secondary battery
JP2010009856A
Porous current collector and electrode for electrochemical battery
JP2017162812A