Resin composition, method for producing same, rubber composition containing said resin composition, gas barrier film containing said rubber composition, and tire containing said gas barrier film

The resin composition with a molecular weight modifier improves air permeability and processability in tire inner liners, addressing the trade-off between these factors and enhancing tire performance.

JP7590542B2Active Publication Date: 2024-11-26KOLON INDUSTRIES INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023503458
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-20
Filing Date
2021-10-28
Publication Date
2024-11-26
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

Existing tire inner liners face a trade-off between air permeability resistance and manufacturing process efficiency, with increasing the thickness of the rubber layer or using halogenated butyl rubber alone leading to increased tire weight and manufacturing costs, respectively.

Method used

A resin composition is developed using a hydrogenated or non-hydrogenated petroleum resin with a molecular weight modifier, blended with raw rubber, to improve air permeability and processability, replacing process oil in tire inner liners.

Benefits of technology

The resin composition enhances air permeation resistance and manufacturing processability, reducing compounding time and costs while maintaining excellent compatibility with rubber, resulting in improved tire performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590542000009
    Figure 0007590542000009
  • Figure 0007590542000001
    Figure 0007590542000001
  • Figure 0007590542000002
    Figure 0007590542000002
Patent Text Reader

Abstract

The present invention relates to a resin composition comprising a base resin, at least a portion of which contains a hydrogenated or non-hydrogenated petroleum resin, and an additive comprising a modified C9 polymer having a structure in which a molecular weight regulator is bonded to at least one of both ends of the at least a portion of the hydrogenated or non-hydrogenated petroleum resin, as well as a gas barrier film and a tire each containing the resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition having a novel composition, a method for producing the same, a rubber composition containing the resin composition, a gas barrier film containing the same, and a tire containing the gas barrier film. [Background technology]

[0002] The tire inner liner is the innermost rubber layer in the tire structure and must maintain the air pressure inside the tire, be resistant to bending, and have excellent adhesion to adjacent supporting parts (e.g., carcass). Of these, research related to tire inner liners that maintain the durability of bending resistance while maintaining the tire's air pressure is being continuously conducted.

[0003] So far, methods of increasing the thickness of the rubber layer or increasing the content of halogenated butyl rubber have been utilized as techniques for improving the air permeability resistance of tire innerliners. However, when the thickness of the innerliner is increased, the weight of the entire tire increases, causing a decrease in fuel efficiency. In addition, when the content of halogenated butyl rubber, which has excellent air permeability resistance, is increased or when halogenated butyl rubber is used alone as a raw rubber, there still remains a problem that the tire manufacturing process is deteriorated and the manufacturing cost increases.

[0004] In order to solve such problems, research has been conducted into a technique for producing a rubber composition for an inner liner by compounding a halogenated butyl rubber together with natural rubber and adding a process oil, a processing aid, and a filler (organic filler and / or inorganic filler). However, the compounding of materials other than the halogenated butyl rubber causes a problem in that the air permeability resistance of the halogenated butyl rubber decreases.

[0005] In other words, there is a trade-off between manufacturing processability and air permeability resistance, and research is being continuously conducted to simultaneously improve both.

[0006] Therefore, there is a demand for a resin composition for producing rubber for an inner liner having improved air permeability resistance and manufacturing processability.

[0007] Also, since it is difficult to compound butyl rubber alone, the ratio of natural rubber is increased during compounding, and other materials such as process oil, processing aids, and fillers (organic and inorganic fillers) are used to compound the rubber for the inner liner. If materials other than butyl rubber are added, it will be disadvantageous in terms of air permeability resistance. Therefore, in order to reduce gas permeability, a semi-solid hydrocarbon resin that is non-polar, has a small molecular weight, is easy to process, and is non-crystalline and has high viscosity is used, which is compatible with the amorphous region of the polymer and has the effect of forming a film. By applying it to the inner liner, it is possible to improve processability and air permeability resistance. Summary of the Invention [Problem to be solved by the invention]

[0008] The problem to be solved by the present invention is to provide a resin composition having improved rubber air permeability resistance and manufacturing processability, a method for producing the same, a rubber composition and a gas barrier film containing the same, and a tire containing the same. [Means for solving the problem]

[0009] According to one embodiment, there is provided a resin composition comprising: a base resin, at least a portion of which comprises a hydrogenated or non-hydrogenated petroleum resin; and an additive, at least a portion of which comprises a modified petroleum resin having a structure in which a molecular weight regulator is bound to at least one end of the hydrogenated or non-hydrogenated petroleum resin.

[0010] According to another embodiment, there is provided a rubber composition comprising a raw rubber and the resin composition, the resin composition being contained in an amount of 1 to 50 parts by weight based on 100 parts by weight of the raw rubber.

[0011] According to yet another aspect, there is provided a gas barrier film comprising the rubber composition.

[0012] According to yet another aspect, there is provided a tire comprising the gas barrier film.

[0013] According to yet another embodiment, there is provided a method for producing a resin composition, comprising blending, at a temperature of 100° C. to 180° C., a base resin at least partially containing a hydrogenated or non-hydrogenated petroleum resin and an additive at least partially containing a modified petroleum resin having a structure in which a molecular weight regulator is bound to at least one of both ends of the hydrogenated or non-hydrogenated petroleum resin, to obtain a semi-solid resin. Effect of the Invention

[0014] The resin composition according to one embodiment of the present invention contains additives including a petroleum resin modified with a molecular weight modifier, despite the absence of process oil, which facilitates dispersion of raw materials during the raw material blending process and shortens the blending time, thereby providing economic benefits. In addition, the resin composition has excellent compatibility with rubber, and the gas barrier film produced therefrom has improved air permeability resistance. [Brief description of the drawings]

[0015] [Figure 1] 1 is a diagram illustrating a basic structure of a tire. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present inventive concept described below may have various embodiments that can be modified in various ways, but specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, they do not limit the present inventive concept to specific embodiments, and should be understood to include all modifications, equivalents, or alternatives that fall within the technical scope of the present inventive concept.

[0017] The terms used below are merely used to describe specific embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In the following, terms such as "comprise" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. In the following, " / " may be interpreted as "and" or "or" depending on the context.

[0018] In the drawings, thicknesses are exaggerated or reduced to clearly depict the various layers and regions. Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part, such as a layer, film, region, plate, etc., is referred to as being "on" or "above" another part, this includes not only when it is directly on top of the other part, but also when there is another part between them. Throughout the specification, terms such as first, second, etc. may be used to describe various components, but the components are not limited by these terms. These terms are used only to distinguish one component from another.

[0019] Scientific terms used herein may be understood in the same manner as commonly understood by one of ordinary skill in the art to which the present invention pertains, unless otherwise defined.

[0020] In the present specification, the term "petroleum resin" includes a polymer obtained by polymerizing one or more of a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer. For example, the petroleum resin includes a homopolymer, a copolymer, etc. Examples of the homopolymer petroleum resin include a polymer obtained by polymerizing a C5 monomer, a polymer obtained by polymerizing a C5 mixed fraction, a polymer obtained by polymerizing a C9 monomer, a polymer obtained by polymerizing a C9 mixed fraction, a polymer obtained by polymerizing a cyclic diolefin monomer, and a polymer obtained by polymerizing a linear olefin monomer. Examples of the copolymer petroleum resin include copolymers of two different C5 monomers, copolymers of two different C9 monomers, copolymers of two different cyclic diolefin monomers, copolymers of two different linear olefin monomers, copolymers of a C5 fraction and a C5 monomer, copolymers of a C5 fraction and a C9 monomer, copolymers of a C9 fraction and a C5 monomer, copolymers of a C5 monomer and a C9 monomer, copolymers of a C9 fraction and a C5 monomer, copolymers of a C5 monomer and a C9 monomer, copolymers of a C9 fraction and a C9 monomer, copolymers of a C5 fraction and a linear olefin monomer, copolymers of a C9 fraction and a linear olefin monomer. Copolymers of a C5 fraction and a cyclic diolefin monomer, copolymers of a C9 fraction and a cyclic diolefin monomer, copolymers of a C5 monomer and a cyclic diolefin monomer, copolymers of a C9 monomer and a linear olefin monomer, and copolymers of a cyclic diolefin monomer and a linear olefin monomer can be mentioned.

[0021] In this specification, the term "hydrogenated petroleum resin" refers to a petroleum resin in which at least a portion of the unsaturated moieties, such as ethylene, in the above-mentioned petroleum resin has been modified to saturated hydrocarbons by a hydrogenation reaction.

[0022] As used herein, the term "C5 (mixed) fraction" includes aliphatic C5 paraffins and aliphatic C6 paraffins, olefins, and diolefins derived from naphtha cracking. For example, the C5 fraction may include, but is not limited to, pentene, isoprene, 2-methyl-2-butene, 2-methyl-2-pentene, cyclopentadiene, and piperylene, including any mixture of two or more of the C5 monomers. The C5 fraction may also be selectively alkylated.

[0023] As used herein, "C5 monomer" refers to any one of the components contained in the aforementioned C5 (mixed) fraction.

[0024] As used herein, "C9 (mixed) fraction" refers to a composition derived from petroleum processing, e.g., cracking, and includes C8, C9 and / or C10 fractions boiling at atmospheric pressure and between about 100° C. and 300° C., as is commonly understood in the art to which the present invention pertains. 10 The C9 fraction may include, but is not limited to, any mixture of two or more of the C9 monomers. The C9 fraction may also be selectively alkylated. For example, the C9 fraction in the present invention may include vinyltoluene, indene, styrene, dicyclopentadiene, indene, trans-beta-methylstyrene, and methylindene, as well as alkylated derivatives of these components, such as alpha-methylstyrene, methylindene, etc.

[0025] As used herein, the term "C9 monomer" refers to any one of the components contained in the C9 fraction.

[0026] As used herein, "olefin" includes unsaturated compounds that contain at least one ethylenically unsaturated (C=C) bond. For example, the olefin can include, but is not limited to, linear olefins, cyclic olefins, α-olefins, and the like.

[0027] As used herein, "cyclic diolefin" includes cyclic unsaturated compounds containing two C=C bonds. For example, the cyclic diolefin can include, but is not limited to, dicyclopentadiene, tricyclopentadiene, and the like.

[0028] The resin composition of the present invention, a rubber composition and a gas barrier film containing the same, a tire containing the gas barrier film, and a method for producing the resin composition will be specifically described below.

[0029] [Resin composition] A resin composition according to one embodiment includes a base resin, at least a portion of which includes a hydrogenated or non-hydrogenated petroleum resin, and an additive, at least a portion of which includes a modified petroleum resin having a structure in which a molecular weight regulator is bound to at least one end of the hydrogenated or non-hydrogenated petroleum resin.

[0030] By including the additive in the base resin, processability is improved, and a gas barrier film produced therefrom has improved air permeability resistance.

[0031] According to an embodiment, the petroleum resin may include at least one repeating unit derived from a C9 mixed fraction. For example, the petroleum resin may be composed of a repeating unit derived from a C9 mixed fraction.

[0032] According to an embodiment, in the resin composition, the weight ratio of the base resin to the additive may be 12:1 to 1:12. For example, in the resin composition, the weight ratio of the base resin to the additive may be 11:1 to 1:11, 10:1 to 1:10, or 9:1 to 1:9.

[0033] According to an embodiment, the content of the base resin in the resin composition may be equal to or greater than the content of the additive. For example, the weight ratio of the base resin to the additive in the resin composition may be 12:1 to 1:1. For example, the weight ratio of the base resin to the additive in the resin composition may be 11:1 to 1:1, 10:1 to 1:1, or 9:1 to 1:1.

[0034] By satisfying the content ratio of the base resin and the additives, a resin composition having excellent compatibility and blendability with the raw rubber can be obtained, and by forming a film so as to be compatible with the amorphous region of the raw rubber for tire inner liners, air permeability resistance can be improved.

[0035] According to one embodiment, the base resin may have a weight average molecular weight (Mw) of 200 to 2,000, a softening point of 80°C to 150°C, a viscosity measured at 160°C of 250 to 2,000 cps, and a glass transition temperature of 30°C to 100°C.

[0036] For example, the base resin may have a weight average molecular weight (Mw) of 400 to 1,000, a softening point of 90°C to 120°C, a viscosity measured at 160°C of 500 to 1,000 cps, and a glass transition temperature of 40°C to 70°C.

[0037] According to an embodiment, the base resin may be a petroleum resin including a polymer of one or more selected from the group consisting of a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer.

[0038] According to an embodiment, the base resin may be a petroleum resin including a copolymer of two selected from a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer. For example, the base resin may include a copolymer of a C9 mixed fraction and a cyclic diolefin.

[0039] According to an embodiment, the base resin may include a C9 dicyclopentadiene (DCPD) copolymer. For example, the petroleum resin may be a C9 dicyclopentadiene (DCPD) copolymer resin.

[0040] According to an embodiment, the base resin may be a hydrogenated petroleum resin obtained by hydrogenating two copolymers selected from a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer. For example, the base resin may include a hydrogenated C9-cyclic diolefin resin in which the ethylene functional group of a copolymer of a C9 mixed fraction and a cyclic diolefin is hydrogenated.

[0041] According to an embodiment, the base resin may include a hydrogenated C9 dicyclopentadiene (DCPD) copolymer. For example, the base resin may be a hydrogenated C9 dicyclopentadiene (DCPD) copolymer resin.

[0042] According to an embodiment, the molecular weight regulator is a chain transfer agent, and may include thiols or halocarbons such as carbon tetrachloride.

[0043] According to an embodiment, the molecular weight regulator may include a thiol, i.e., an organic mercaptan-based molecular weight regulator including one or more thiol groups. For example, the organic mercaptan-based molecular weight regulator may include an aliphatic mercaptan compound, a cyclic aliphatic mercaptan compound, an aromatic mercaptan compound, or a combination thereof.

[0044] According to an embodiment, the number of thiol groups contained in the organic mercaptan molecular weight regulator is not particularly limited, but may include 1 to 4 thiol groups per molecule, and each thiol group may include a hydrocarbon group having 1 to 20 carbons, preferably 1 to 15 carbons.

[0045] In addition to the hydrocarbon group and the thiol group, other substituents may be added, and examples of such substituents include hydroxy groups, carboxylic acid groups, ether groups, ester groups, sulfide groups, amine groups, amide groups, and the like.

[0046] According to an embodiment, the molecular weight regulator is an organic compound having a thiol group, and is not particularly limited thereto, and may include, for example, alkyl mercaptans such as ethyl mercaptan, butyl mercaptan, hexyl mercaptan, or dodecyl mercaptan; thiol phenols such as phenyl mercaptan or benzyl mercaptan; hydroxyl group-containing or carboxylic acid group-containing mercaptans such as 2-mercaptoethanol, thiol glycolic acid, or 3-mercaptopropionic acid; or mercaptans having two or more functional groups such as pentaerythritol tetrakis(3-mercapto)propionate; or mixtures thereof.

[0047] For example, the molecular weight regulator may be methyl mercaptan, ethyl mercaptan, butyl mercaptan, octyl mercaptan, lauryl mercaptan, mercaptoethanol, mercaptopropanol, mercaptobutanol, mercaptoacetic acid, mercaptopropionic acid, benzyl mercaptan, phenyl mercaptan, cyclohexyl mercaptan, 1-thioglycerol, 2,2'-dimercaptodiethyl ether, or 2,2'-dimercaptodipropyl ether. , 2,2'-dimercaptodiisopropyl ether, 3,3'-dimercaptodipropyl ether, 2,2'-dimercaptodiethyl sulfide, 3,3'-dimercaptodipropyl sulfide, bis(β-mercaptoethoxy)methane, bis(β-mercaptoethylthio)methane, trimethylolpropane trithioglycolate, pentaerythritol tetrathioglycolate, or mixtures thereof.

[0048] For example, the molecular weight regulator can include ethyl mercaptan, butyl mercaptan, hexyl mercaptan, dodecyl mercaptan, phenyl mercaptan, benzyl mercaptan; mercaptoethanol, thiol glycolic acid, mercaptopropionic acid, pentaerythritol tetrakis(3-mercapto)propionate, or mixtures thereof.

[0049] According to an embodiment, the molecular weight regulator may be n-dodecyl mercaptan represented by the following formula 1, 2-mercaptoethanol represented by the following formula 2, or a mixture thereof, to maximize the effect of molecular weight regulation.

[0050] [ka]

[0051] [ka]

[0052] According to an embodiment, the additive may further include a viscosity modifier.

[0053] According to an embodiment, the viscosity modifier may include a low viscosity resin having a viscosity of 20 to 500 cps at 25° C. The viscosity modifier may be any resin that satisfies the above viscosity requirements without any particular limitations.

[0054] For example, the low viscosity resin can include hydrogenated DCPD-C9 copolymer resin, hydrogenated dicyclopentadiene (DCPD) resin, and mixtures thereof.

[0055] Here, the hydrogenated dicyclopentadiene (DCPD) C9 copolymer resin means a white thermoplastic resin obtained through polymerization and hydrogenation of dicyclopentadiene (DCPD). As such a hydrogenated dicyclopentadiene (DCPD) C9 copolymer resin, a commercially available resin such as SUKOREZ (registered trademark) resin can also be used.

[0056] According to an embodiment, the viscosity modifier includes a hydrogenated dicyclopentadiene (DCPD)·C9 copolymer resin having the following structure, thereby maximizing the effects of viscosity control and improvement of air permeability resistance:

[0057] [ka]

[0058] The modified petroleum resin according to an embodiment is a modified petroleum resin in which at least one of C5 monomer, C5 mixed fraction, C9 monomer, C9 mixed fraction, cyclic diolefin monomer and linear olefin monomer is polymerized, and at least a part of the hydrogenated or non-hydrogenated petroleum resin is modified with the molecular weight regulator. By modifying the end of the petroleum resin with the molecular weight regulator, it is not only excellent in compatibility and blendability with rubber, but also can be made compatible with the amorphous region of the polymer to form a membrane, and the processability and air permeability resistance can be further improved. On the other hand, if the end is not modified with the molecular weight regulator, the compatibility with rubber is low due to high non-polarity, and the blending is not performed well. As a result, the processability and performance of the final product are deteriorated.

[0059] According to another embodiment, the modified petroleum resin includes at least one repeating unit derived from a C9 mixed fraction, and the modified petroleum resin is end-modified with the molecular weight regulator, which can further improve compatibility and compoundability with rubber, and can further improve processability and air permeability resistance.

[0060] The modified petroleum resin according to an embodiment will be described later, and has a structure in which one or more of the C5 monomer, C5 mixed fraction, C9 monomer, C9 mixed fraction, cyclic diolefin monomer, and linear olefin monomer are polymerized through an addition polymerization reaction or a chain polymerization reaction, and the molecular weight regulator is bound to at least one of both ends of an at least partially hydrogenated or non-hydrogenated petroleum resin.

[0061] The modified petroleum resin may include at least one repeat unit derived from a C9 mixed fraction.

[0062] According to one embodiment, the modified petroleum resin has a structure in which repeating units such as those shown in the following formula 4a are bonded: For example, the modified petroleum resin may include the following structure formed by the polymerization of styrene, α-methylstyrene, vinyltoluene, indene, methylindene, dicyclopentadiene, and α-methylstyrene and methylindene, as well as alkylated derivative monomers of these components, which are contained in the C9 mixed fraction.

[0063] [ka]

[0064] The above formula 4a is merely an example, and in addition to the above structure, other C5 monomers, C9 monomers, cyclic diolefin monomers, and linear olefin monomers not shown may be included as repeating units.

[0065] For example, the modified petroleum resin is a polymer represented by the above structure, and the polymer means a random polymer, but is not limited thereto, and includes block copolymers, alternating copolymers, and the like.

[0066] Although not shown separately, the modified petroleum resin may have a structure in which at least one of the repeating units represented by Formula 4a is hydrogenated.

[0067] In another embodiment, the modified petroleum resin may include a structure in which the following repeating units are bonded: For example, at least one of the ends of the modified petroleum resin has a structure having a double bond, and a structure having a double bond at both ends is exemplarily represented by the following formula 4b.

[0068] [ka]

[0069] In this way, the double bond located at at least one end is bound to the molecular weight regulator to form a petroleum resin (e.g., a polymer of a C9 mixed fraction) modified with the molecular weight regulator. The molecular weight regulator may be bound to either end or only one end, as shown in the following chemical formula 4c, which is illustratively represented.

[0070] Although not shown separately, the modified petroleum resin may include a structure in which at least one of the repeating units represented by formula 4b or 4c is hydrogenated.

[0071] [ka]

[0072] According to one embodiment, the additive containing the modified petroleum resin has a number average molecular weight (Mn) of 200 to 500, and within this range, the modified polymer may have excellent compatibility with raw rubber and processability. If the number average molecular weight is less than 200, there may be a problem of low compounding efficiency, and if it is more than 500, compounding processability may be reduced.

[0073] According to one embodiment, the additive containing the modified petroleum resin has excellent processability due to its non-polarity, and has low crystallinity and can be dissolved in the amorphous region of the polymer to form a film, thereby further improving processability and air permeability resistance. In addition, the additive has a viscosity of 2,500 to 4,000 cps at 60°C and a glass transition temperature of -25°C to -15°C.

[0074] The viscosity of the additive may be from 2,700 to 3,800, or from 3,000 to 3,500.

[0075] If the glass transition temperature of the additive is lower than -25°C, there may be a problem in air permeability resistance, and if it is higher than -15°C, there may be a problem in low temperature durability.

[0076] According to an embodiment, the additive may have an aromaticity of 20% to 60%. For example, the additive may have an aromaticity of 30% to 50%, or 35% to 45%. If the aromaticity is less than 20%, the compatibility with the raw rubber is low, and the effect of improving the air permeability resistance of the gas barrier film produced thereby is negligible, and if it exceeds 60%, the processability may be reduced due to an increase in the glass transition temperature (Tg).

[0077] According to one embodiment, the additive may include a modified petroleum resin and a viscosity modifier, and the modified petroleum resin and the viscosity modifier may be included in an amount of 80 to 98 wt % and 2 to 20 wt %, respectively.

[0078] The viscosity modifier does not participate in the formation of the structure of the product polymer, but serves to adjust the viscosity of the reactants and the product. Therefore, the additive can be obtained by carrying out a polymerization reaction by adding a polymerization catalyst and / or heat to a solution containing one or more of a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer, a molecular weight modifier, and a viscosity modifier, and the polymerization reaction product can be a mixture of a modified petroleum resin and a viscosity modifier.

[0079] According to an embodiment, the resin composition may have excellent compatibility with raw rubber and improved air permeation resistance by blending the base resin and additives in an appropriate ratio.

[0080] The resin composition has a number average molecular weight (Mn) of 100 to 550, a glass transition temperature of 0° C. to 60° C., a softening point of 50° C. to 90° C., and an aromaticity of 5 to 35%.

[0081] For example, the number average molecular weight (Mn) of the resin composition may be 150 to 500, 200 to 450, 250 to 400, or 300 to 350.

[0082] For example, the glass transition temperature can be from 5°C to 65°C, from 10°C to 60°C, from 15°C to 55°C, from 20°C to 50°C, from 25°C to 45°C, or from 30°C to 40°C.

[0083] For example, the softening point may be between 55°C and 85°C.

[0084] For example, the aromaticity may be between 10% and 30%.

[0085] When the resin composition satisfies the above-mentioned physical properties, the compatibility with rubber is improved and the resin composition has excellent air permeation resistance.

[0086] The C5 monomer, the C5 mixed fraction, the C9 monomer, the C9 mixed fraction, the cyclic diolefin monomer, and the linear olefin monomer are as described above, and various specific examples of the molecular weight regulator, the viscosity regulator, etc. are as described above.

[0087] [Method of producing resin composition] According to one embodiment, the method for producing the resin composition includes blending a base resin, at least a portion of which is hydrogenated or non-hydrogenated petroleum resin, with an additive, at least a portion of which is a modified petroleum resin having a structure in which a molecular weight regulator is bonded to at least one of both ends of the hydrogenated or non-hydrogenated petroleum resin, at a temperature of 100° C. to 180° C. to obtain a semi-solid resin, where the semi-solid state refers to a material in an intermediate state between a solid and a liquid.

[0088] According to an embodiment, the weight ratio of the base resin to the additive may be 12:1 to 1:12. For example, in the resin composition, the weight ratio of the base resin to the additive may be 11:1 to 1:1, 10:1 to 1:1, or 9:1 to 1:1.

[0089] According to an embodiment, the content of the base resin is greater than the content of the additives, for example, the weight ratio of the content of the base resin to the content of the additives may be 9:1 to 5:5.

[0090] When the content ratio of the base resin to the additive is within the above-mentioned range, compatibility with raw rubber for tire innerliners and processability are improved, making it possible to produce a tire innerliner with improved air permeability resistance.

[0091] According to an embodiment, the additive may further include a viscosity modifier, and details regarding the viscosity modifier are described above.

[0092] According to an embodiment, the additive may be obtained by carrying out a polymerization reaction by adding a polymerization catalyst and / or heat to a solution containing one or more of a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer, a molecular weight modifier, and a viscosity modifier.

[0093] According to an embodiment, the polymerization catalyst may be selected from the group consisting of Lewis acid catalysts, halohydric acids, AlCl3, BF3, and mixtures thereof.

[0094] For example, the polymerization catalyst may be selected from AlCl3, BF3, SnCl4, TiCl4, AgClO4, I2, and mixtures thereof.

[0095] According to one embodiment, the application of heat may be performed at about 230 to about 280°C.

[0096] According to one embodiment, the polymerization reaction of the additive may be carried out under a pressure of 5 to 10 bar for about 1 to about 3 hours.

[0097] [Rubber composition] According to one embodiment, there is provided a rubber composition comprising raw rubber and the above-mentioned resin composition, the resin composition being contained in an amount of 1 to 50 parts by weight based on 100 parts by weight of the raw rubber.

[0098] If the content of the resin composition is less than 1 part by weight, it is difficult to expect improvement in air permeability resistance, and if it exceeds 50 parts by weight, the dispersibility during compounding of raw rubber decreases, causing a decrease in the physical properties of the rubber compound.

[0099] According to an embodiment, the rubber composition may further include a homogenizer, a reinforcing agent, a vulcanization aid, sulfur, and a vulcanization accelerator in addition to the raw rubber and the resin composition.

[0100] According to an embodiment, the rubber composition may include 1 to 8 parts by weight of a homogenizing agent, 20 to 80 parts by weight of a reinforcing agent, and 0.1 to 10 parts by weight of a vulcanization aid, based on 100 parts by weight of raw rubber.

[0101] According to an embodiment, the rubber composition may further include 0.1 to 2 parts by weight of sulfur and 0.5 to 5 parts by weight of a vulcanization accelerator based on 100 parts by weight of raw rubber.

[0102] The components constituting the rubber composition together with the resin will be described in detail below.

[0103] According to an embodiment, the raw rubber is not particularly limited as long as it has an olefinic double bond (carbon-carbon double bond), and may be natural rubber, synthetic rubber, or a mixture thereof.

[0104] According to an embodiment, the raw rubber may include at least one selected from the group consisting of natural rubber (NR), butadiene rubber, nitrile rubber, silicone rubber, isoprene rubber, styrene-butadiene rubber (SBR), isoprene-butadiene rubber, styrene-isoprene-butadiene rubber, acrylonitrile-butadiene rubber (NBR), ethylene-propylene-diene rubber, halogenated butyl rubber, halogenated isoprene rubber, halogenated isobutylene copolymer, chloroprene rubber, butyl rubber, and halogenated isobutylene-p-methylstyrene rubber.

[0105] For example, the raw rubber may include a mixture of natural and synthetic rubbers. For example, the raw rubber may be a mixture of halogenated butyl rubber (e.g., chlorinated butyl rubber) and natural rubber.

[0106] According to an embodiment, the rubber composition may include a homogenizing agent, such as 40MS (manufactured by Stricktol), which can improve the kneadability of butyl rubber and natural rubber, which do not mix well.

[0107] According to an embodiment, the rubber composition may include a reinforcing agent. For example, the reinforcing agent may include carbon black. The carbon black improves the processability of the rubber composition due to its high specific surface area, and the film made from the final rubber composition has advantageous effects such as improved abrasion resistance, improved rolling resistance, and prevention of cracking or deterioration due to ultraviolet rays.

[0108] The type of carbon black is not particularly limited, and any carbon black generally used in the field of tires can be used. For example, the carbon black may be furnace black, acetylene black, thermal black, channel black, graphite, or the like.

[0109] Furthermore, the physical properties of the carbon black, such as the particle diameter, pore volume, and specific surface area, are not particularly limited, and various types of carbon black conventionally used in the rubber industry, such as SAF, ISAF, HAF, FEF, GPF, and SRF (all of which are abbreviations for carbon black classified according to the US ASTM standard D-1765-82a), can be appropriately used.

[0110] The carbon black is preferably contained in an amount of 20 to 80 parts by weight per 100 parts by weight of raw rubber. The carbon black is an essential element in rubber compounding as a reinforcing filler, and if the carbon black content is below the above range, the reinforcing effect is reduced, whereas if the carbon black content exceeds the above range, dispersion becomes difficult.

[0111] According to an embodiment, the reinforcing agent may be, in addition to the carbon black, mineral powders such as silica, clay, and talc; carbonates such as magnesium carbonate and calcium carbonate; and alumina hydrates such as aluminum hydroxide.

[0112] According to an embodiment, the rubber composition may contain sulfur. The sulfur may be any sulfur that can proceed with the vulcanization process without any particular limitation. The sulfur content is 0.1 to 2 parts by weight per 100 parts by weight of raw rubber, and the air permeability resistance of the film made from the final rubber composition may be improved.

[0113] According to an embodiment, the rubber composition may include a vulcanization accelerator, where "vulcanization" refers to crosslinking via at least one sulfur atom. Examples of the vulcanization accelerator include thiuram-based accelerators such as tetramethylthiuram monosulfide, tetramethylthiuram disulfide, and tetraethylthiuram disulfide; thiazole-based accelerators such as Nt-butylbenzothiazole-2-sulfenamide (TBBS), 2-mercaptobenzothiazole, and dibenzothiazole disulfide; sulfenamide-based accelerators such as N-cyclohexyl-2-benzothiazylsulfenamide and N-oxydiethylene-2-benzothiazolylsulfenamide; guanidine-based accelerators such as diphenylguanidine (DPG) and di-orthotolylguanidine; aldehyde-amine-based accelerators such as n-butylaldehyde-aniline condensate and butylaldehyde-monobutylamine condensate; aldehyde-ammonia-based accelerators such as hexamethylenetetramine; and thiourea-based accelerators such as thiocarbanilide. When the vulcanization accelerator is blended, one kind may be used alone, or two or more kinds may be used in combination. The vulcanization accelerator may be dibenzothiazole disulfide.

[0114] The content of such a vulcanization accelerator is 0.5 to 5 parts by weight per 100 parts by weight of raw rubber, so that the air permeability resistance of the film produced from the final rubber composition can be improved.

[0115] According to an embodiment, the rubber composition may include a vulcanization aid. As mentioned above, "vulcanization" refers to crosslinking through at least one sulfur atom.

[0116] Examples of the vulcanization aid include metal oxides such as zinc oxide (zinc oxide) and magnesium oxide; metal hydroxides such as potassium hydroxide; metal carbonates such as zinc carbonate and basic zinc carbonate; fatty acids such as stearic acid and oleic acid; aliphatic metal salts such as zinc stearate and magnesium stearate; amines such as di(n-butyl)amine and dicyclohexylamine; ethylene dimethacrylate, diallyl phthalate, N,Nm-phenylenedimaleimide, triallyl isocyanurate, and trimethylolpropane trimethacrylate.

[0117] When such a vulcanization aid is used, one kind may be used alone or two or more kinds may be used in combination. The content of such a vulcanization aid is 0.1 to 10 parts by weight per 100 parts by weight of raw rubber, and the air permeability resistance of the film produced from the final rubber composition can be improved.

[0118] According to an embodiment, the rubber composition may further contain, if necessary, one or more of various additives used in the rubber industry, such as antioxidants, vulcanization retarders, peptizers, plasticizers, etc. The amount of these additives is preferably 0.1 to 10 parts by weight per 100 parts by weight of raw rubber.

[0119] The composition containing the above-mentioned components can be manufactured into a gas barrier film by using a known method. For example, the gas barrier film can be applied to a tire as, for example, an inner liner.

[0120] According to an embodiment, the rubber composition may be prepared by kneading the above-mentioned components using a kneading machine such as a plastomill, a Banbury mixer, a roll, or an internal mixer.

[0121] According to one embodiment, the above-mentioned components other than sulfur and vulcanization accelerator are first mixed, and then sulfur and vulcanization accelerator are added to the obtained mixture, and further mixed to prepare the composition.

[0122] The rubber composition produced by the above method can be used as a material for forming a gas barrier film. The gas barrier film produced in this way has excellent mechanical properties (hardness, tensile strength, modulus, etc.). In particular, it has excellent air permeability resistance and can be applied to a film for a tire inner liner.

[0123] The rubber composition obtained according to one embodiment was prepared into a rubber test piece, and the gas permeability was measured according to the method of KS M ISO 2556. The gas permeability was 150 cm 3 For example, the gas permeability may be 145 cm 3 / (m 2 1·day·atm) or less. In addition, the rubber specimen may have a glass transition temperature (Tg) of -16°C or less. The rubber specimen has advantages in that the processability is improved, the manufacturing cost is reduced, and the physical properties of the final product are improved, since the glass transition temperature of the rubber specimen is -16°C or less.

[0124] The rubber specimen may be prepared by a method commonly used in the art using the rubber composition. For example, the rubber composition may be compressed and molded using a hot press to prepare a specimen having a size of 12 cm x 12 cm (horizontal x vertical) and a thickness of 0.5 mm ± 0.2 mm, and then the gas permeability may be measured under an atmosphere of 25°C and 60 RH%.

[0125] The resin composition can be used as an additive to the rubber composition forming an existing tire, for example, as a resin to replace process oil added to improve the compatibility of raw materials in the manufacturing process of tire inner liners.

[0126] The tire inner liner rubber composition according to one aspect of the present invention includes a resin composition according to an embodiment of the present invention instead of a process oil, and thus has improved air permeability resistance and processability compared to a case where the rubber composition includes an existing process oil.

[0127] For example, existing known process oils include petroleum-based oils such as paraffinic oils, naphthenic oils, aromatic oils, and combinations thereof.

[0128] [tire] FIG. 1 is a diagram illustrating a schematic configuration of a tire.

[0129] Referring to FIG. 1, the tire includes a tread portion 1, a shoulder portion 2, a sidewall portion 3, a bead portion 4, a belt portion 5, an inner liner portion 6, a carcass portion 7, and a cap ply portion 8.

[0130] The tread portion is a portion that comes into direct contact with the road surface and is located outside the cap ply, and is made of highly wear-resistant rubber. It also plays a role in improving the wet and dry grip of the tire on the road surface in the transportation device.

[0131] The shoulder portion is located on the side of the tread between the tread and the sidewall portion and serves to connect the sidewall portion and the tread.

[0132] The sidewall portion is located between the tread and the bead portion and covers the side surface of the tire. The sidewall portion covers the carcass portion to protect the carcass portion from external stimuli and suppresses deformation of the tire due to centrifugal force generated in the tire when a transportation device is in operation, thereby ensuring stable operation of the transportation device.

[0133] The bead portion is an area in which one or more strands of steel wires are present around the end of the carcass, the steel wires being completely covered by a rubber membrane, and serves to mount and fix the tire to the wheel rim, in particular to prevent separation of the tire from the wheel rim when air leaks out.

[0134] The belt portion is a coating layer located between the tread portion and the carcass portion, and serves to prevent damage to internal structures such as the carcass portion due to external impacts or external conditions, and to increase the contact area between the tread portion and the road surface.

[0135] The inner liner is located at the innermost part of the tire and serves to prevent air from leaking out of the tire and to maintain a constant air pressure within the tire.

[0136] The carcass is made of high-strength synthetic fibers and serves to form and maintain the framework of the tire, withstanding loads and impacts transmitted during operation of the transportation equipment and maintaining air pressure.

[0137] The cap ply is a protective layer located below the tread and serves to protect internal components from heat transferred from the tread and from external impacts.

[0138] [Tread section] The tread portion functions to improve the grip of the tire on the road surface. The grip means the adhesion between the tire and the road surface, and if the grip is improved, the braking performance of the vehicle when cornering or stopping is improved.

[0139] The tread portion may be formed using a rubber composition including raw rubber and resin, and may include a single layer of the rubber composition or a laminate of multiple rubber compositions.

[0140] The raw rubber may include natural rubber, synthetic rubber, or a combination thereof.

[0141] For example, the natural rubber may be common natural rubber or modified natural rubber, and the synthetic rubber may be butadiene rubber, nitrile rubber, silicone rubber, isoprene rubber, styrene-butadiene rubber (SBR), isoprene-butadiene rubber, styrene-isoprene-butadiene rubber, acrylonitrile-butadiene rubber (NBR), ethylene-propylene-diene rubber, halogenated butyl rubber, halogenated isoprene rubber, halogenated isobutylene copolymer, chloroprene rubber, butyl rubber, halogenated isobutylene-p-methylstyrene rubber, or mixtures thereof.

[0142] For example, the resin may be selected from the resin compositions described above, hydrocarbon resins, alkylphenolic resins, phenolic / acetylene resins, terpene phenolic resins, rosin-derived resins, and mixtures thereof.

[0143] The tread portion may further include a tire cord in addition to the rubber composition.

[0144] The tire cord can be appropriately selected by those skilled in the art, taking into consideration adhesion to rubber, rigidity and fatigue resistance of the tire, heat resistance and dimensional stability.

[0145] Examples of the tire cord include rayon, nylon, polyester, aramid, steel, etc. If necessary, a conductive material may be mixed into the tire cord.

[0146] The rubber composition for treads may further include a homogenizing agent, a reinforcing agent, a vulcanization aid, sulfur, and a vulcanization accelerator in addition to the raw rubber and resin. The homogenizing agent, reinforcing agent, vulcanization aid, sulfur, and vulcanization accelerator are described in the present specification.

[0147] If necessary, various additives such as vegetable oils and antioxidants may be further added.

[0148] The content of the components contained in the rubber composition for treads can be appropriately selected by those skilled in the art depending on the desired physical properties.

[0149] [Shoulder] The shoulder portion is disposed between the tread portion and the sidewall portion, connecting the tread portion to the sidewall portion located on the side of the tire. The shoulder portion is the thickest of all the components of the tire, and is therefore designed to allow heat generated inside the shoulder portion to be easily discharged to the outside during running.

[0150] For example, the shoulder portion may have a round shoulder structure or a square shoulder structure.

[0151] The shoulder portion can be formed by utilizing a rubber composition for a tread, and a person skilled in the art can appropriately select the composition ratio of the components according to the desired physical properties.

[0152] [Sidewall] The sidewall portion refers to the side portion of the tire that extends from the shoulder to the bead side and serves to protect the carcass portion inside the tire. In particular, the sidewall portion not only absorbs shocks transmitted during the up and down movements of the tire, but also accommodates repeated tire inflation and deflation while the vehicle is traveling.

[0153] The sidewall portion can be formed from a rubber composition containing raw rubber and a tire cord.

[0154] For example, the raw rubber may include natural rubber, synthetic rubber, modified natural rubber, or combinations thereof.

[0155] The natural rubber and the synthetic rubber are referred to as described in the tread portion.

[0156] The modified natural rubber is obtained by modifying or purifying natural rubber in order to improve the compatibility and physical properties of general natural rubber, and examples of such modified natural rubber include epoxidized natural rubber, deproteinized natural rubber, and hydrogenated natural rubber.

[0157] As for the tire cord, as described above with respect to the tread portion, aramid fiber can be used from the viewpoint of improving impact resistance.

[0158] In addition to the raw rubber and tire cord described above, the rubber composition used to produce the sidewall portion may further contain various additives, such as a homogenizing agent, a reinforcing agent, a vulcanization aid, sulfur, a vulcanization accelerator, vegetable oil, and an antioxidant, as necessary.

[0159] The content of the rubber composition components used in the manufacture of the sidewall portion can be appropriately selected by those skilled in the art depending on the desired physical properties.

[0160] [Bead part] The bead portion is a portion of the tire that comes into contact with the wheel, and serves to fix the tire to the wheel and maintain air tightness when the tire is filled with air.

[0161] The bead portion may include one or more steel wires coated with rubber, the one or more steel wires being twisted between each other.

[0162] [Belt section] The belt portion is located below the tread portion and serves to maintain the contact area of ​​the tread portion, and to absorb external shocks transmitted from the tread portion, as well as to support the load applied to the tire.

[0163] The belt portion may be formed of a rubber composition including raw rubber and tire cords. Here, the tire cords may be arranged in the circumferential direction of the tire to withstand external forces acting in the circumferential direction of the tire.

[0164] For example, the raw rubber may include natural rubber, synthetic rubber, modified natural rubber, or combinations thereof.

[0165] The natural rubber and the synthetic rubber are as described above in relation to the tread portion, and the modified natural rubber is as described above in relation to the sidewall portion.

[0166] Regarding the tire cord, refer to the description of the tread portion.

[0167] The rubber composition for the belt portion may further include an adhesive for strong adhesion to the tire cord, such as latex, rosin-based resin, terpene-phenolic resin, aliphatic petroleum resin, aromatic petroleum resin, and dicyclopentadiene-based petroleum resin.

[0168] The component composition ratio of the rubber composition for the belt portion can be appropriately selected by those skilled in the art depending on the desired physical properties.

[0169] [Inner liner part] The inner liner part may include the gas barrier film described above, or the inner liner part may include both the gas barrier film described above and a polyamide-based gas barrier film made of a rubber composition including a mixture of raw rubber and a polyamide-based resin.

[0170] For example, the inner liner portion may be formed of a single layer structure of a gas barrier film according to an embodiment of the present invention, or may have a multi-layer structure including a gas barrier film layer according to an embodiment of the present invention and a polyamide-based gas barrier film layer.

[0171] For example, such a polyamide-based gas barrier film may comprise a copolymer containing polyamide units and polyether units, or a mixture of a polymer containing polyamide units and a polymer containing polyether units.

[0172] The ratio of the polyamide units contained in the polyamide-based gas barrier film may be higher than the ratio of the polyether units, for example, the weight ratio of the polyamide units to the polyether units contained in the gas barrier film may be 9.5:0.5 to 5.5:4.5.

[0173] The polyamide unit may be a main repeating unit contained in one polyamide resin selected from the group consisting of nylon 6, nylon 66, nylon 46, nylon 11, nylon 12, nylon 610, nylon 612, nylon 6 / 66 copolymer, nylon 6 / 66 / 610 copolymer, nylon MXD6, nylon 6T, nylon 6 / 6T copolymer, nylon 66 / PP copolymer, nylon 66 / PPS copolymer, methoxymethylated 6-nylon, methoxymethylated 6-610-nylon, and methoxymethylated 612-nylon.

[0174] The polyether-based unit may be, for example, a main repeating unit contained in one polyether-based resin selected from the group consisting of polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyoxyethylene diamine, polyoxypropylene diamine, polyoxytetramethylene diamine, and copolymers thereof.

[0175] The inner liner part may further include an adhesive film on its surface to maintain a firm bond with the adjacent components. The adhesive film may be a single layer or multiple layers. When the adhesive film is a multiple layer, any one of the multiple layers may be a release film including an oxygen barrier film. The oxygen barrier film may include a gas barrier film according to an embodiment of the present invention.

[0176] The thickness of the inner liner portion is not particularly limited, and can be appropriately selected by a person skilled in the art in consideration of the fuel consumption and air permeability resistance of the transportation equipment.

[0177] [Carcass] The carcass portion is located above the inner liner portion and forms the skeleton of the tire. It has the functions of maintaining the tire's outer shape, maintaining the internal air pressure, and cushioning against external shocks.

[0178] The carcass portion is made of a rubber composition containing raw rubber and a tire cord material, and the tire cord material can be arranged in the radial direction so as to withstand a force acting in the radial direction of the tire.

[0179] For example, the raw rubber may include natural rubber, synthetic rubber, modified natural rubber, or combinations thereof.

[0180] The natural rubber and the synthetic rubber are as described above in relation to the tread portion, and the modified natural rubber is as described above in relation to the sidewall portion.

[0181] Regarding the tire cord, refer to the description of the tread portion.

[0182] The rubber composition for the carcass may further include the adhesive described above for strong adhesion to the tire cord.

[0183] The component composition ratio of the rubber composition for the carcass can be appropriately selected by those skilled in the art depending on the desired physical properties.

[0184] [Cap ply part] The cap ply portion is disposed between the belt portion and the tread portion, and serves to fix the belt portion.

[0185] The cap ply portion may be formed from rayon, nylon, polyester, aramid, or steel. For example, the cap ply portion may be constructed from a nylon film.

[0186] The cap ply portion may further include an adhesive to improve adhesion, if desired.

[0187] Examples of adhesives that can be used include latex, rosin-based resins, terpene-phenol resins, aliphatic petroleum resins, aromatic petroleum resins, and dicyclopentadiene-based petroleum resins.

[0188] In addition, the cap ply portion may further include one or more of a heat resisting agent, an antioxidant, a stabilizer, a reinforcing agent, an antifoaming agent, and a filler, if necessary.

[0189] The composition ratio of the components of the cap ply portion material can be appropriately selected by those skilled in the art depending on the desired physical properties.

[0190] The present invention will be described in more detail below through examples. However, the scope and contents of the present invention should not be construed as being narrowed or limited by the following examples. In addition, based on the disclosure of the present invention including the following examples, it is clear that a person skilled in the art can easily implement the present invention, even though no specific experimental results have been presented, and it goes without saying that such modifications and alterations fall within the scope of the claims.

[0191] In addition, the experimental results presented below are only representative experimental results of the above-mentioned examples and comparative examples, and the respective effects of various embodiments of the present invention that are not explicitly presented below will be specifically described in the relevant sections. EXAMPLES

[0192] (Production of resin composition)

[0193] <Production Example 1> Based on 100 parts by weight of a composition consisting of 93% by weight of refined C9 fraction (manufactured by YCNCC) and 7% by weight of viscosity modifier LP200 (manufactured by Kolon Industries), 2.5 parts by weight of molecular weight modifier n-dodecyl mercaptan was added and polymerization reaction was carried out for 2 hours at 260°C and high pressure (5 to 10 bar). When the polymerization catalyst BF3 was added, the polymerization reaction was carried out for 2 hours at 180°C and high pressure (5 to 10 bar). The polymerized product was degassed to remove unreacted reactants, and a resin composition for additive use was produced.

[0194] <Production Example 2> The additive obtained in Preparation Example 1 was blended with a C9 / dicyclopentadiene (DCPD) copolymer resin (SU-400 or SU-490) in a weight ratio of 3:7 at a high temperature (100°C to 180°C) to produce a resin composition.

[0195] <Production Example 3> manufacturing The additive obtained in Example 1 was blended with C9 / dicyclopentadiene (DCPD) copolymer resin (SU-400 or SU-490) in a weight ratio of 1:9 at a high temperature (100°C to 180°C) to prepare a resin composition.

[0196] <Test Example 1: Evaluation of resin composition> The glass transition temperature, softening point, viscosity, number average molecular weight, and aromaticity of the resin compositions produced in Production Examples 1 to 3 were measured and are shown in Table 1 below.

[0197] The glass transition temperature was confirmed through differential scanning calorimetry (DSC) analysis.

[0198] The softening point was measured using the ring and ball softening method (ASTM E28). A resin was melted and poured into a ring frame, which was then placed in a beaker containing glycerin. A ball was then placed on the ring containing the resin, and the temperature was raised at a rate of 2.5°C per minute to measure the temperature (softening point) at which the resin melted and the ball fell.

[0199] The viscosity was measured using a Brookfield viscometer (ASTM D3236) using spindle #27.

[0200] The number average molecular weight was determined as a polystyrene-equivalent number average molecular weight (Mn) by gel permeation chromatography (Model HP-1100 (manufactured by Hewlett-Packard Company)).

[0201] The aromaticity was confirmed via nuclear magnetic resonance (NMR) analysis.

[0202] [Table 1]

[0203] (Manufacture of rubber specimens) <Example 1> 100 parts by weight of raw rubber consisting of 80 parts by weight of chlorinated butyl rubber (HT-1066 (manufactured by Exxon Chemical)) and 20 parts by weight of natural rubber (NR (manufactured by Sritrang)), 10 parts by weight of the resin composition produced in Production Example 2, 4 parts by weight of homogenizing agent (40MS (manufactured by Strucktol)), 60 parts by weight of carbon black (N-660 (manufactured by Pentacarbon)), 3 parts by weight of zinc oxide (ZnO (manufactured by Kemai Chem)), and 2 parts by weight of stearic acid (manufactured by Kemai Chem) were placed in a Banbury mixer and mixed at 150°C, and then the primary compounded rubber was discharged. Next, 0.5 parts by weight of sulfur (manufactured by Miwon Chem) and 1.2 parts by weight of a vulcanization accelerator (DM (dibenzothiazole disulfide) (manufactured by Sunsine)) were added to the primary compounded rubber in a Banbury mixer, and the rubber was vulcanized at 100°C and then released to prepare a rubber specimen.

[0204] <Example 2> A rubber specimen was prepared in the same manner as in Example 1, except that 10 parts by weight of the resin composition prepared in Preparation Example 3 was used instead of the resin composition prepared in Preparation Example 2.

[0205] <Comparative Example 1> A rubber specimen was prepared in the same manner as in Example 1, except that 10 parts by weight of the additive prepared in Preparation Example 1 was used instead of the resin composition prepared in Preparation Example 2.

[0206] <Comparative Example 2> A rubber specimen was prepared in the same manner as in Example 1, except that 10 parts by weight of process oil (TDAE (manufactured by H&R)) was used instead of the resin composition prepared in Preparation Example 2.

[0207] <Comparative Example 3> A rubber specimen was prepared in the same manner as in Example 1, except that 10 parts by weight of paraffin oil (manufactured by MICHANG Petroleum Co., Ltd.) was used instead of the resin composition prepared in Preparation Example 2.

[0208] <Comparative Example 4> A rubber specimen was prepared in the same manner as in Example 1, except that 10 parts by weight of naphthenic oil (manufactured by MICHANG Petroleum Co., Ltd.) was used instead of the resin composition prepared in Preparation Example 2.

[0209] <Comparative Example 5> A rubber specimen was prepared in the same manner as in Example 1, except that 10 parts by weight of 40MS (Strucktol) was used instead of the resin composition prepared in Preparation Example 2.

[0210] <Comparative Example 6> A rubber specimen was prepared in the same manner as in Example 1, except that 10 parts by weight of C9 / dicyclopentadiene (DCPD) copolymer resin (SU-400 (manufactured by Kolon Co., Ltd.)) was used instead of the resin composition prepared in Preparation Example 2.

[0211] <Test Example 2: Evaluation of physical properties of rubber specimens> The properties of the rubber specimens prepared in Examples 1 and 2 and Comparative Examples 1 to 6 were measured, and the results are shown in Table 2 below.

[0212] [Table 2]

[0213] The rheometer results measured by a rubber rheometer are parameters related to the behavior of the rubber composition and the cure rate when applied to a process, and are related to the processability during tire manufacturing. Here, if the values ​​(Toq(Min), Toq(Max)) are very high or very low, it means that it is not easy to apply to an existing process and a new process design is necessary. When comparing the results of Toq(Min), Toq(Max), Tc50 (time to reach 50% cure), Tc90 (time to reach 90% cure) of Example 1 presented in Table 2 with the results of Comparative Examples 1 to 4, it can be seen that the specifications are easily applicable to existing processes.

[0214] In addition, the results of Mooney viscosity and mechanical properties (modulus, tensile strength, elongation, hardness, etc.) shown in Table 2 above indicate that the results of Examples 1 and 2 are comparable to or better than the results of Comparative Examples 2 to 5.

[0215] The gas permeability and Tg value are values ​​related to air permeability resistance and processability, respectively. The lower the gas permeability, the higher the usability as a tire inner liner, and the lower the Tg value, the more advantageous it is in the process.

[0216] In this regard, the gas permeation rate of Examples 1 and 2 is 132 cm 3 / (m 2 ·day·atm) and 125cm 3 / (m 2 ·day·atm), which shows a significantly improved gas permeability compared to the rubber specimens of Comparative Examples 1 to 5.

[0217] In addition, it can be seen that Examples 1 and 2 have lower Tg values ​​than Comparative Example 6, and thus have improved processability.

[0218] From these results, it can be seen that the rubber composition for tire innerliners according to the present invention not only satisfies the basic physical properties required for tire construction, i.e., tensile strength, abrasion resistance, durability, hardness, etc., but also improves processability and significantly improves air permeability resistance.

Claims

1. A method for producing a olefin copolymer comprising: a base resin comprising a copolymer of a C9 mixed fraction and a cyclic diolefin monomer; and an additive comprising a modified petroleum resin having a structure in which an organic mercaptan-based molecular weight regulator containing one or more thiol groups (—SH) is bonded to at least one end of an at least partially hydrogenated or non-hydrogenated petroleum resin, A resin composition, wherein the weight ratio of said base resin to said additive is from 9:1 to 1:

1.

2. The base resin is The weight average molecular weight (Mw) is 200 to 2,000; The softening point is 80° C. to 150° C. The viscosity measured at 160°C is 250 to 2,000 cps; 2. The resin composition according to claim 1, which has a glass transition temperature of 30°C to 100°C.

3. 2. The resin composition of claim 1, wherein the molecular weight regulator comprises ethyl mercaptan, butyl mercaptan, hexyl mercaptan, dodecyl mercaptan, phenyl mercaptan, benzyl mercaptan, mercaptoethanol, thiol glycolic acid, mercaptopropionic acid, pentaerythritol tetrakis(3-mercapto)propionate, or a combination thereof.

4. The additive is The number average molecular weight (Mn) is 200 to 500; 2. The resin composition according to claim 1, which has a glass transition temperature of -25 to -15°C.

5. The additive further comprises a viscosity modifier, The resin composition according to claim 1 , wherein the viscosity modifier comprises a low viscosity resin having a viscosity measured at 25° C. of 20 to 500 cps.

6. The low viscosity resin is hydrogenated dicyclopentadiene (DCPD). 96. The resin composition of claim 5, comprising a copolymer resin, hydrogenated dicyclopentadiene (DCPD), or a combination thereof.

7. The resin composition according to claim 1, wherein the additive has a viscosity measured at 60°C of 2,000 to 4,000 cps.

8. The resin composition comprises The number average molecular weight (Mn) is 100 to 550; The glass transition temperature is 0° C. to 60° C.

2. The resin composition according to claim 1, which has a softening point of 50°C to 90°C.

9. 2. The resin composition of claim 1, wherein the resin composition has an aromaticity of 5% to 35%.

10. Raw rubber; The resin composition according to any one of claims 1 to 9, The resin composition is contained in an amount of 1 to 50 parts by weight based on 100 parts by weight of raw rubber.

11. The rubber composition of claim 10 , wherein the rubber composition is free of process oil.

12. The rubber composition according to claim 10, further comprising 1 to 8 parts by weight of a homogeneous compounding agent, 20 to 80 parts by weight of a reinforcing agent, and 0.1 to 10 parts by weight of a vulcanization aid, based on 100 parts by weight of raw rubber.

13. The rubber composition according to claim 12, further comprising 0.1 to 2 parts by weight of sulfur and 0.5 to 5 parts by weight of a vulcanization accelerator, based on 100 parts by weight of raw rubber.

14. The rubber composition is prepared into a rubber specimen and has a gas permeability of 150 cm3 as measured by the method of KSM ISO2556. 3 / (m 2 · day · atm) or less, The rubber composition according to claim 12, having a glass transition temperature (Tg) of -16°C or lower.

15. A gas barrier film comprising the rubber composition according to claim 10.

16. A tire comprising the gas barrier film of claim 15.

17. A method for producing a semi-solid resin, comprising blending a base resin comprising a copolymer of a C9 mixed fraction and a cyclic diolefin monomer with an additive comprising a modified petroleum resin having a structure in which an organic mercaptan molecular weight regulator containing one or more thiol groups (-SH) is bonded to at least one of both ends of an at least partially hydrogenated or non-hydrogenated petroleum resin at a temperature of 100°C to 180°C, A method for producing a resin composition, wherein the weight ratio of the base resin to the additive is 9:1 to 1:

1.

18. The additive further comprises a viscosity modifier; The method for producing a resin composition according to claim 17, wherein the viscosity modifier comprises a low-viscosity resin having a viscosity measured at 25°C of 20 to 500 cps.

19. The additive is obtained by carrying out a polymerization reaction by adding a polymerization catalyst and / or heat to a solution containing at least a part of a hydrogenated or non-hydrogenated petroleum resin, an organic mercaptan molecular weight regulator containing one or more thiol groups (-SH), and a viscosity regulator. The method for producing a resin composition according to claim 18.

20. The polymerization catalyst is AlCl 3 , B.F. 3 , SnCl 4 , TiCl 4 , AgClO 4 , I 2 20. The method of claim 19, further comprising:

21. The method for producing a resin composition according to claim 19, wherein the application of heat is carried out at 230°C to 280°C.

Citation Information

Patent Citations

  • Tread rubber composition

    JP1993214170A

  • Thermal polymerization of dicyclopentadiene

    JP1996048723A

  • Resin composition for forming injection-molded product and injection-molded product

    JP2009256504A

  • Copolymer, and rubber composition and tire using the same

    JP2013231196A

  • Elastomer blend for tires containing a hydrocarbon resin with a high glass transition temperature

    JP2017533296A