Dye-sensitized solar cells
The dye-sensitized solar cell design with a reflective layer and larger titanium oxide particles improves power generation efficiency by increasing light reflection and electrolyte penetration, addressing the inefficiencies of existing designs.
Patent Information
- Application Number
- JP2020113491
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-30
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-06-30
AI Technical Summary
Existing dye-sensitized solar cells do not sufficiently improve power generation efficiency, particularly under low-intensity light conditions, despite the implementation of reflective layers.
A dye-sensitized solar cell design featuring a reflective layer on the power generation layer's upper and side surfaces, with larger titanium oxide particles in the reflective layer to enhance light reflection and electrolyte penetration, and a structure that allows partial exposure of the power generation layer to improve light exposure and electrolyte infiltration.
The design increases power generation efficiency by enhancing light reflection and electrolyte impregnation, leading to improved power output, especially under low-intensity lighting conditions.
Smart Images

Figure 0007590823000001 
Figure 0007590823000002 
Figure 0007590823000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a dye-sensitized solar cell. [Background technology]
[0002] Dye-sensitized solar cells have been attracting attention as a new alternative to silicon-based solar cells. Dye-sensitized solar cells have the advantage of being able to generate more power under low-intensity light, such as indoor lighting, than silicon-based solar cells, and are expected to be applied in a variety of fields.
[0003] In dye-sensitized solar cells, various structures have been proposed to increase the amount of power generated by improving the efficiency of incident light utilization. For example, a structure has been proposed in which a reflective layer is formed on the upper surface of the power generation layer, so that the light that has passed through the power generation layer is reflected by the reflective layer and returned to the power generation layer, thereby increasing the amount of power generated by the power generation layer (Patent Document 1).
[0004] Furthermore, a structure has been proposed in which a reflective layer is formed only on a portion of the upper surface of the power generation layer, thereby exposing the power generation layer from the reflective layer and making it easier to fill the exposed portion of the power generation layer with electrolyte (Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-119189 A [Patent Document 2] JP 2014-199788 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, simply forming such a reflective layer does not sufficiently improve the amount of electricity generated by the dye-sensitized solar cell.
[0007] The present invention has been made in consideration of the above problems, and has an object to improve the amount of power generated by a dye-sensitized solar cell. [Means for solving the problem]
[0008] The dye-sensitized solar cell according to the present invention is characterized by having a substrate, a first electrode layer provided on a surface of the substrate, a power generation layer provided on the first electrode layer and containing a dye and an electrolyte, a reflective layer provided on at least a portion of an upper surface and a side surface of the power generation layer, and a second electrode layer provided on the reflective layer.
[0009] In the dye-sensitized solar cell, the power generation layer may have a thickness of 0.5 μm to 6.5 μm.
[0010] In the dye-sensitized solar cell, the reflective layer and the first electrode layer may be in contact with each other in a cross-sectional view, and the length of the portion where the reflective layer and the first electrode layer are in contact with each other in a cross-sectional view may be 0.1 μm to 50 μm.
[0011] In the above dye-sensitized solar cell, the power generation layer may include a plurality of first particles, and the reflective layer may include a plurality of second particles, the average particle size of the plurality of second particles being larger than the average particle size of the plurality of first particles.
[0012] In the dye-sensitized solar cell, the second average particle size may be 50 nm to 600 nm.
[0013] In the dye-sensitized solar cell, a part of the upper surface of the power generation layer may extend beyond the reflective layer in a plan view.
[0014] In the dye-sensitized solar cell, at least a portion of the side surfaces may be exposed and not covered with the reflective layer.
[0015] In the dye-sensitized solar cell, the reflective layer may entirely cover the upper surface and the side surfaces of the power generating layer.
[0016] In the dye-sensitized solar cell, at least a part of the side surface may be inclined with respect to a perpendicular line to the upper surface.
[0017] In the dye-sensitized solar cell, the reflective layer may have a first portion having a first thickness and a second portion having a second thickness smaller than the first thickness.
[0018] In the dye-sensitized solar cell, at least one of the upper surface and at least a portion of the side surface may be provided with projections and recesses.
[0019] In the dye-sensitized solar cell, the reflective layer may contain a plurality of particles, and the particles may penetrate to a depth of 0.3 μm or more on the power generation layer side at the interface between the power generation layer and the reflective layer. Effect of the Invention
[0020] According to the present invention, the amount of power generated by a dye-sensitized solar cell can be improved. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2A is a plan view (part 1) of the dye-sensitized solar cell according to the first embodiment during its manufacture, and FIG. 2B is a cross-sectional view taken along line II in FIG. [Diagram 2] FIG. 2(a) is a plan view (part 2) of the dye-sensitized solar cell according to the first embodiment during production, and FIG. 2(b) is a cross-sectional view taken along line II in FIG. [Diagram 3] FIG. 2A is a plan view (part 3) of the dye-sensitized solar cell according to the first embodiment during production, and FIG. 2B is a cross-sectional view taken along line II in FIG. [Figure 4] FIG. 2A is a plan view (part 4) of the dye-sensitized solar cell according to the first embodiment during production, and FIG. 2B is a cross-sectional view taken along line II in FIG. [Diagram 5] FIG. 5(a) is a plan view (part 5) of the dye-sensitized solar cell according to the first embodiment during production, and FIG. 5(b) is a cross-sectional view taken along line II in FIG. [Figure 6]FIG. 1A is a plan view (part 6) of the dye-sensitized solar cell according to the first embodiment during production, and FIG. 1B is a cross-sectional view taken along line II in FIG. [Figure 7] FIG. 1(a) is a plan view (part 7) of the dye-sensitized solar cell according to the first embodiment during production, and (b) is a cross-sectional view taken along line II in (a). [Figure 8] FIG. 1A is a plan view (part 8) of the dye-sensitized solar cell according to the first embodiment during production, and FIG. 1B is a cross-sectional view taken along line II in FIG. [Figure 9] FIG. 2 is a cross-sectional view of the dye-sensitized solar cell according to the first embodiment during use. [Figure 10] FIG. 10 is a cross-sectional view illustrating the effect obtained by inclining the side surface of the power generation layer with respect to the upper surface in the first embodiment. [Figure 11] 1(a) to 1(c) are plan views (part 1) illustrating examples of the planar layout of the power generation layer and the reflective layer according to the first embodiment. [Figure 12] 1(a) to 1(c) are plan views (part 2) illustrating examples of the planar layout of the power generation layer and the reflective layer according to the first embodiment. [Figure 13] FIG. 12(b) is a perspective view of the dye-sensitized solar cell 20 according to the example of FIG. [Figure 14] FIG. 12(c) is a perspective view of the dye-sensitized solar cell 20 according to the example of FIG. [Figure 15] 5(a) to 5(d) are cross-sectional views showing examples of the thicknesses of the power generation layer and the reflective layer in the first embodiment. [Figure 16] FIG. 15 is a diagram showing a schematic diagram illustrating how the amount of power generated by a dye-sensitized solar cell changes depending on the length W and thickness a, based on the results of FIGS. 15(a) to (d). [Figure 17] FIG. 2 is a schematic diagram showing the relationship between the particle size of titanium particles and the intensity of light reflected by titanium oxide particles. [Figure 18] FIG. 4 is a cross-sectional view of a dye-sensitized solar cell according to a second embodiment. [Figure 19] 1(a) to 1(d) are cross-sectional views of a dye-sensitized solar cell according to a third embodiment. [Figure 20] FIG. 11 is a cross-sectional view of a dye-sensitized solar cell according to a fourth embodiment. [Figure 21] 1 is a diagram (part 1) showing the results of investigating the amount of power generated by a dye-sensitized solar cell when the length W and thickness a are changed in an example. [Figure 22] 1 is a graph (part 2) showing the power generation amount of a dye-sensitized solar cell when the length W and thickness a are changed in an example. [Diagram 23] 13 is a graph (part 3) showing the results of investigating the amount of power generated by a dye-sensitized solar cell when the length W and thickness a are changed in the examples. [Figure 24] 13 is a fourth diagram showing the results of investigating the amount of power generated by a dye-sensitized solar cell when the length W and thickness a are changed in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] (First embodiment) The dye-sensitized solar cell according to the present embodiment will be described in detail with reference to its manufacturing method. Figures 1(a), 2(a), 3(a), 4(a), 5(a), 6(a), 7(a), and 8(a) are plan views of the dye-sensitized solar cell according to the present embodiment during its manufacturing process. Figures 1(b), 2(b), 3(b), 4(b), 5(b), 6(b), 7(b), and 8(b) are cross-sectional views taken along line II in Figures 1(a), 2(a), 3(a), 4(a), 5(a), 6(a), 7(a), and 8(a).
[0023] 1(a) and (b), a glass substrate having a square shape in a plan view is prepared as the transparent substrate 10. The length of one side of the transparent substrate 10 is 5 mm to 40 mm, for example, 10 mm. The thickness of the transparent substrate 10 is 0.1 mm to 3 mm, for example, 1.1 mm. Note that a transparent plastic plate may be used as the transparent substrate 10 instead of the glass substrate.
[0024] Next, an ITO (Indium Tin Oxide) layer is formed to a thickness of 0.1 μm to 0.5 μm as a transparent electrode layer (first electrode layer) 11 on the transparent substrate 10. Note that instead of the ITO layer, any of an FTO (Fluorine doped Tin Oxide) layer, a zinc oxide layer, a laminated film of an indium-tin composite oxide layer and a silver layer, and an antimony-doped tin oxide layer may be formed as the transparent electrode layer 11.
[0025] Furthermore, an alcohol solution prepared from titanium alkoxide is applied onto the transparent electrode layer 11, and the alcohol solution is heated and dried to form a reverse electron transfer prevention layer 12 with a thickness of about 5 nm to 0.1 μm. The drying temperature in this step is not particularly limited, and the reverse electron transfer prevention layer 12 is formed by heating to 450° C. to 650° C., for example, 550° C.
[0026] The reverse electron transfer prevention layer 12 is not formed on a partial region 10a at the corner of the transparent substrate 10, so that the transparent electrode layer 11 is exposed. The partial region 10a has an area of 0.2% to 5.6% of the area of the power generation layer, for example, 2%. The shape of the partial region 10a is not particularly limited.
[0027] 2(a) and (b), a first titanium oxide paste 13a is formed on the reverse electron transfer prevention layer 12 by screen printing to a thickness of 1 μm to 20 μm, for example, 5 μm. Here, PST-30NRD manufactured by JGC Catalysts and Chemicals is used as the first titanium oxide paste 13a. The average particle size of the titanium oxide particles contained in the first titanium oxide paste 13a is 5 nm to 50 nm, for example, 20 nm. The printing area of the first titanium oxide paste 13a on the transparent substrate 10 is 0.01 cm2. 2 ~4cm 2 , e.g. 0.98cm 2 The first titanium oxide paste 13a is not limited to the above, and a paste obtained by kneading titanium oxide particles with a solvent such as ethyl cellulose may be used as the first titanium oxide paste 13a.
[0028] 3(a) and (b), a second titanium oxide paste 14a, PST-400C manufactured by JGC Catalysts and Chemicals, is formed on the first titanium oxide paste 13a by screen printing. The thickness of the second titanium oxide paste 14a is not particularly limited, but is set to 0.3 μm to 100 μm, for example, 42 μm, here. Furthermore, the printing area of the second titanium oxide paste 14a on the transparent substrate 10 is set to 0.011 cm 2 ~4.1cm 2 , e.g. 1 cm 2 As with the first titanium oxide paste 13a, a paste obtained by kneading titanium oxide particles into a solvent such as ethyl cellulose may be used as the second titanium oxide paste 14a.
[0029] The titanium oxide particles contained in the second titanium oxide paste 14a have an average particle size of 50 nm to 600 nm, for example 400 nm, which is larger than the average particle size in the first titanium oxide paste 13a. The particle size of titanium oxide can be measured by adjusting the magnification of a scanning electron microscope or a transmission electron microscope so that about 80 to 150 crystal grains are included in one image, taking multiple photographs so that there are a total of 400 crystal grains or more, measuring the total number of crystal grains in the photograph, and using the Feret diameter. The average value can be used as the average particle size.
[0030] In addition, the first titanium oxide paste 13a and the second titanium oxide paste 14a are not formed on a partial region 10a of the transparent substrate 10, so that the transparent electrode layer 11 is left exposed.
[0031] Next, as shown in Figures 4(a) and (b), the first and second titanium oxide pastes 13a and 14a are heated to evaporate organic matter, and the first and second titanium oxide pastes 13a and 14a are converted into the power generation layer 13 and the reflective layer 14, respectively. The heating conditions for the titanium oxide pastes 13a and 14a are not particularly limited. In this embodiment, the titanium oxide pastes 13a and 14a are heated to a temperature of 450°C to 650°C, for example, 600°C. The heating time is 10 minutes to 120 minutes, for example, 30 minutes.
[0032] This results in a structure in which the upper surface 13p and the side surface 13q of the power generation layer 13 are each covered with the reflective layer 14. In addition, in the power generation layer 13 formed by the coating method, the side surface 13q is inclined with respect to the perpendicular line G of the upper surface 13p, and as a result, the power generation layer 13 becomes thinner from the center to the end portion 13r of the power generation layer 13. Note that in this example, the reflective layer 14 is formed on all of the multiple side surfaces 13q of the power generation layer 13, but this embodiment is not limited to this. For example, the reflective layer 14 may be formed only on some of the multiple side surfaces 13q. Furthermore, the power generation layer 13 may be cylindrical with only one side surface 13q, and the reflective layer 14 may be formed only on a part of the side surface 13q.
[0033] In this embodiment, the power generating layer 13 and the reflective layer 14 are formed from the titanium oxide pastes 13a and 14a, but the materials of the power generating layer 13 and the reflective layer 14 are not limited to these. For example, the power generating layer 13 and the reflective layer 14 may each be formed from semiconductor particles of an oxide of any of Cd, Zn, In, Pb, Mo, W, Sb, Bi, Cu, Hg, Ti, Ag, Mn, Fe, V, Sn, Zr, Sr, Ga, Si, Cr, and Nb. Furthermore, the power generating layer 13 and the reflective layer 14 may each be formed from particles of a perovskite oxide such as SrTiO3 or CaTiO3.
[0034] 5(a) and 5(b), the power generation layer 13 and the reflective layer 14 are immersed in a solvent 15 containing a dye, and the dye is adsorbed to each of the power generation layer 13 and the reflective layer 14. Here, the solvent 15 is a toluene-based solvent in which MK-2 is dissolved as a dye. The temperature of the solvent 15 is 0°C to 80°C, for example, 50°C, and the immersion time is 10 minutes to 12 hours, for example, 1 hour. Note that the titanium oxide particles contained in the power generation layer 13 have a smaller average particle size than the titanium oxide particles contained in the reflective layer 14, so that many fine gaps are formed in the power generation layer 13. As a result, the amount of dye adsorbed to the power generation layer 13 is greater than the amount of dye adsorbed to the reflective layer 14.
[0035] The dye is not limited to the above, and metal complex dyes or organic dyes may be used as the dye. Among these, examples of metal complex dyes include transition metal complexes such as ruthenium-cis-diaqua-bipyridyl complex, ruthenium-tris complex, ruthenium-bis complex, osmium-tris complex, and osmium-bis complex. In addition, zinc-tetra(4-carboxyphenyl)porphyrin and iron-hexacyanide complex are also examples of metal complex dyes.
[0036] Examples of organic dyes include 9-phenylxanthene dyes, coumarin dyes, acridine dyes, triphenylmethane dyes, tetraphenylmethane dyes, quinone dyes, azo dyes, indigo dyes, cyanine dyes, merocyanine dyes, xanthene dyes, and carbazole compound dyes.
[0037] 6(a) and (b), 1 μL to 50 μL, for example, about 20 μL, of the solid electrolyte precursor 16 is dropped onto the reflective layer 14, thereby allowing the solid electrolyte precursor 16 to permeate into the power generation layer 13 via the reflective layer 14. In this embodiment, the solid electrolyte precursor 16 is a solution in which iodine, 1,3-dimethylimidazolium iodide (DMII), acetonitrile, and polyethylene oxide with a molecular weight of 1,000,000 are mixed uniformly.
[0038] Thereafter, the power generation layer 13 is heated to volatilize excess acetonitrile contained in the solid electrolyte precursor 16, thereby obtaining a power generation layer 13 impregnated with a solid electrolyte. The heating conditions are not particularly limited, but the power generation layer 13 is heated to a temperature of 50°C to 150°C, for example, 100°C. The heating time is 1 minute to 60 minutes, for example, 30 minutes. Thereafter, the power generation layer 13 is returned to room temperature. The solid electrolyte is also contained in the reflective layer 14. However, as described above, the titanium oxide particles contained in the power generation layer 13 have a smaller average particle size than the titanium oxide particles contained in the reflective layer 14, so many fine gaps are generated in the power generation layer 13. Therefore, the amount of solid electrolyte contained in the power generation layer 13 is greater than the amount of solid electrolyte contained in the reflective layer 14.
[0039] The electrolyte contained in the solid electrolyte precursor 16 is not limited to DMII. For example, iodine salts such as pyridinium salts, imidazolium salts, and triazolium salts, which are in a solid state near room temperature, or room-temperature molten salts in a molten state, can be used as the ionic liquid. Examples of such room-temperature molten salts include quaternary ammonium iodide compounds such as 1-methyl-3-propylimidazolium iodide, 1-butyl-3-methylimidazolium iodide (BMII), and 1-ethyl-pyridinium iodide.
[0040] Next, as shown in FIG. 7(a) and (b), a titanium foil having a platinum layer formed on its surface by a sputtering method is prepared as a positive electrode plate (second electrode layer) 17. Here, a titanium foil is used as the positive electrode plate, but the layer structure of the positive electrode plate 17 is not particularly limited. The platinum layer side of the positive electrode plate 17 is then brought into close contact with the reflective layer 14. At this time, by bringing the positive electrode plate 17 into close contact with the reflective layer 14 in a reduced pressure atmosphere or in a vacuum, it is possible to prevent air bubbles from entering between the reflective layer 14 and the positive electrode plate 17. In addition to the above-mentioned platinum, the material of the positive electrode plate 17 may also be metals having catalytic functions such as palladium, rhodium, and indium. The positive electrode plate 17 may also be made of graphite. Furthermore, the positive electrode plate 17 may also be made of carbon carrying platinum, indium-tin composite oxide, tin oxide doped with antimony, and tin oxide doped with fluorine. Other materials include organic semiconductors such as poly(3,4-ethylenedioxythiophene) (PEDOT) and polythiophenes.
[0041] Although the shape and size of the positive electrode plate 17 are not particularly limited, here, a square positive electrode plate 17 is used, which is obtained by excluding a partial region 10a of the transparent substrate 10. The length of one side of the positive electrode plate 17 is 0.11 mm to 2.1 mm, for example 10 mm, and the thickness of the positive electrode plate 17 is 5 μm to 10 μm, for example 100 μm.
[0042] 8(a) and (b), ultraviolet curing resin is applied to each side surface of the transparent substrate 10 and the positive electrode plate 17, and the ultraviolet curing resin is cured by irradiating ultraviolet rays to form a sealing resin layer 19. If the time between applying the ultraviolet curing resin and irradiating ultraviolet rays is too long, the ultraviolet curing resin will penetrate into the power generation layer 13 and cover its surface. To prevent this, it is preferable to irradiate ultraviolet rays within 10 minutes after applying the ultraviolet curing resin.
[0043] In this manner, the basic structure of the dye-sensitized solar cell 20 according to the present embodiment is completed. In this dye-sensitized solar cell 20, the transparent electrode layer 11 functions as a negative electrode, and the iodide ions (I - ) and triiodide ion (I3 - ) serves to conduct electrons between the transparent electrode layer 11 and the positive electrode plate 17. When the end of a cross section of the power generation layer 13 including the reflective layer 14 is observed with various microscopes such as a scanning electron microscope and a transmission electron microscope, it can be confirmed that the transparent electrode layer 11 and the reflective layer 14 are in contact with each other.
[0044] Furthermore, in this embodiment, as described above, the average particle size of the titanium oxide particles contained in the second titanium oxide paste 14a is larger than the average particle size of the titanium oxide particles contained in the first titanium oxide paste 13a. Reflecting this, the average particle size of the titanium oxide particles contained in the reflective layer 14 is larger than the average particle size of the titanium oxide particles contained in the power generation layer 13. As a result, the light reflectance of the reflective layer 14 is larger than the light reflectance of the power generation layer 13.
[0045] Fig. 9 is a cross-sectional view of the dye-sensitized solar cell 20 during use. As shown in Fig. 9, in actual use, light L is incident on the power generation layer 13 through the transparent substrate 10. This causes the dye adsorbed on the power generation layer 13 to enter an excited state, and electrons are transferred from the dye to the titanium oxide particles. Then, iodide ions (I - ) and triiodide ion (I3 - ) to the positive electrode plate 17, thereby generating electricity.
[0046] In this embodiment, the titanium oxide particles of the reflective layer 14 function as scatterers that scatter the light L, so that the light L is reflected by the reflective layer 14 and returns to the power generation layer 13. As a result, the power generation layer 13 is exposed to the light L more frequently than in the absence of the reflective layer 14, and the power generation efficiency of the power generation layer 13 is improved.
[0047] In particular, by forming the reflective layer 14 from titanium oxide particles in this manner, the solid electrolyte precursor 16 flows through the gaps between the multiple titanium oxide particles in the process of Figure 6(b), making it easier to permeate the solid electrolyte precursor 16 into the power generation layer 13.
[0048] Moreover, in this example, the average particle size of the titanium oxide particles in the reflective layer 14 is made larger than that in the power generation layer 13. This widens the gaps between the titanium oxide particles in the reflective layer 14, facilitating the flow of the solid electrolyte precursor 16, and also increases the intensity of light scattering by the titanium oxide particles in the reflective layer 14, thereby improving the light reflectance of the reflective layer 14.
[0049] Furthermore, in this embodiment, the reflective layer 14 is formed on the entire surface of each of the upper surface 13p and the side surface 13q of the power generating layer 13. Therefore, the power generating layer 13 is exposed to more light L than in the case where the reflective layer 14 is formed only on a portion of either the upper surface 13p or the side surface 13q, and the power generating efficiency of the power generating layer 13 can be further improved.
[0050] In this example, the side surface 13q is inclined with respect to the top surface 13p, which provides the following effect.
[0051] 10 is a cross-sectional view for explaining the effect obtained by inclining the side surface 13q of the power generation layer 13 with respect to the top surface 13p. As shown in FIG. 10, consider the case where light L is incident on the side surface 13q. In this case, the light L travels along the in-plane direction after being reflected by the side surface 13q. Therefore, even if there is a shadow on the dye-sensitized solar cell 20 where the light L does not hit, the light L can also penetrate into the power generation layer 13 in the shadow, and substantially the entire power generation layer 13 can be exposed to the light L.
[0052] Next, we will explain examples of the planar layout of each of the power generation layer 13 and the reflective layer 14. Figures 11(a) to (c) and Figures 12(a) to (c) are plan views showing examples of the planar layout of each of the power generation layer 13 and the reflective layer 14 according to this embodiment.
[0053] 11(a) is a plan view of the power generation layer 13 when the entire surface thereof is covered with the reflective layer 14. As a result, light L is reflected by all of the side surfaces 13q and the entire top surface 13p of the power generation layer 13, thereby increasing the amount of power generation by the power generation layer 13 as described above.
[0054] 11(b) and (c) are plan views of a case where a part of the upper surface 13p of the power generation layer 13 protrudes from the reflective layer 14. A part of the upper surface 13p of the power generation layer 13 protrudes from the reflective layer 14 means that the reflective layer 14 is not formed on the entire upper surface 13p of the power generation layer 13 when viewed in a plan view, and the reflective layer 14 covers a part of the upper surface 13p of the power generation layer 13, and the reflective layer 14 does not cover the other part of the upper surface 13p of the power generation layer 13. When the upper surface 13p protrudes from the reflective layer 14 in this way, the solid electrolyte precursor 16 can be directly infiltrated into the power generation layer 13 in the step of FIG. 6(b), and the amount of the solid electrolyte precursor 16 impregnated in the power generation layer 13 can be increased. This can increase the number of electronic conductors in the power generation layer 13, making electronic conduction smoother.
[0055] 12(a) to (c) are plan views showing cases where the centers of the power generating layer 13 and the reflective layer 14 are offset from each other. In this case as well, the amount of power generated by the power generating layer 13 can be increased, as in the example of FIG. 11(a).
[0056] FIG. 13 is a perspective view of the dye-sensitized solar cell 20 according to the example of FIG. 12(b). FIG. 14 is a perspective view of the dye-sensitized solar cell 20 according to the example of FIG. 12(c). As shown in FIG. 13 and FIG. 14, in these examples, the upper surface of the power generation layer 13 is covered with the reflective layer 14, and one of the multiple side surfaces of the power generation layer 13 is exposed without being covered with the reflective layer 14. When the side surface of the power generation layer 13 is exposed in this manner, the solid electrolyte precursor 16 enters from the side surface in the process of FIG. 6(b), making it easier to infiltrate the electrolyte precursor 16 into the power generation layer 13, and the amount of the solid electrolyte precursor 16 impregnated into the power generation layer 13 can be increased. This can increase the number of electronic conductors in the power generation layer 13, making electronic conduction smoother.
[0057] Incidentally, it is believed that the amount of electricity generated in the power generating layer 13 varies depending on the respective thicknesses of the power generating layer 13 and the reflective layer 14.
[0058] 15(a) to (d) are cross-sectional views showing examples of the thicknesses of the power generation layer 13 and the reflective layer 14. Fig. 15(a) is a cross-sectional view showing a case where the thickness a of the power generation layer 13 is increased and the thickness of the reflective layer 14 is decreased. When the thickness of the reflective layer 14 is decreased in this manner, the amount of light L that transmits through the reflective layer 14 increases, and the amount of light L that returns from the reflective layer 14 to the power generation layer 13 decreases.
[0059] On the other hand, when the thickness of the reflective layer 14 is reduced in this way, the length W of the portion where the reflective layer 14 and the back electron transfer prevention layer 12 contact each other in a cross-sectional view is reduced. This makes it easier for the solid electrolyte precursor 16 to permeate the reflective layer 14, and increases the amount of the solid electrolyte precursor 16 that reaches the power generation layer 13 from the side surface 13q.
[0060] 15(b) is a cross-sectional view of the case where the thickness a of the power generation layer 13 is increased and the thickness of the reflective layer 14 is also increased. When the reflective layer 14 is made thicker in this way, the amount of light L reflected by the reflective layer 14 increases, and the amount of light L returning to the power generation layer 13 from the reflective layer 14 increases.
[0061] However, by increasing the size of the reflective layer 14 in this way, the length W becomes larger, and it becomes more difficult for the solid electrolyte precursor 16 to permeate the reflective layer 14 .
[0062] Fig. 15(c) is a cross-sectional view in the case where the thickness a of the power generation layer 13 is reduced and the reflective layer 14 is also made thinner. Reducing the thickness of the reflective layer 14 in this way reduces the amount of light L returning from the reflective layer 14 to the power generation layer 13, as in the case of Fig. 15(a). Furthermore, by reducing the size of the power generation layer 13, the amount of solid electrolyte precursor 16 impregnated in the power generation layer 13 is also reduced.
[0063] 15(d) is a cross-sectional view in the case where the thickness a of the power generation layer 13 is reduced and the reflective layer 14 is thickened. By thickening the reflective layer 14 in this manner, the amount of light L reflected by the reflective layer 14 can be increased.
[0064] However, by making the reflective layer 14 thicker, the length W increases, making it difficult for the solid electrolyte precursor 16 to penetrate the reflective layer 14. Moreover, because the thickness a of the power generation layer 13 is small, the amount of the solid electrolyte precursor 16 impregnated in the power generation layer 13 also decreases.
[0065] As described above, the amount of light L returning to the power generation layer 13 and the amount of solid electrolyte precursor 16 impregnated in the power generation layer 13 change depending on the width W and the thickness a of the power generation layer 13. These factors also change the amount of power generated by the dye-sensitized solar cell 20.
[0066] FIG. 16 is a diagram showing a schematic diagram of how the amount of power generated by the dye-sensitized solar cell 20 changes depending on the length W and thickness a, based on the results of FIGS. 15(a) to (d).
[0067] 16, the amount of impregnation of the solid electrolyte precursor 16 in the power generation layer 13 decreases when the thickness a is decreased or the length W is increased. Moreover, the amount of light returning from the reflective layer 14 to the power generation layer 13 increases when the length W is increased. Thus, in order to increase the amount of power generation when the reflective layer 14 is formed as in this embodiment, it is preferable to keep the thickness a and the length W within an appropriate range R.
[0068] In particular, the amount of electricity generated by the dye-sensitized solar cell 20 can be effectively increased by setting the thickness a to 0.5 μm to 6.5 μm and the length W to 0.1 μm to 50 μm. It is more preferable to set the thickness a in the range of 0.5 μm to 3 μm. Within this range, the thinner the thickness a, the higher the light transmittance, and the more light is reflected by the reflective layer 14. Therefore, the thinner the thickness a, the higher the amount of electricity generated compared to when there is no reflective layer. However, in order to maintain the power generation capacity, the thickness of the power generation layer 13 is preferably in the range of 0.5 μm or more. Also, it is preferable to set the length W in the range of 15 μm to 50 μm. The thicker the width W of the reflective layer 14, the less light passes through the reflective layer 14, and the more light is reflected. Therefore, the thicker the width W of the reflective layer 14, the higher the amount of electricity generated compared to when there is no reflective layer 14. However, the thicker the reflective layer 14, the more the electrolyte is hindered from penetrating into the reflective layer 14, so that the electrolyte is less likely to penetrate into the power generation layer 13. In order to maintain the power generation capacity, the upper limit of the width W is preferably set to 50 μm.
[0069] The reflectance of the reflective layer 14 also depends on the particle size of the titanium oxide particles contained in the reflective layer 14 .
[0070] FIG. 17 is a schematic diagram showing the relationship between the particle size of titanium oxide particles and the intensity I of light reflected by the titanium oxide particles. As shown in FIG. 17, the intensity I of light backscattering by titanium oxide particles varies depending on the particle size of the titanium oxide particles. In particular, when the absorption wavelength of the dye is 400 nm to 700 nm, the larger the particle size, the greater the backscattering intensity I for light with a wavelength of 400 nm to 700 nm when the particle size is 70 nm or less, and when the particle size exceeds 70 nm, the smaller the particle size, the smaller the backscattering intensity I. However, the larger the particle size, the greater the light blocking rate. Therefore, it is preferable to set the particle size of the titanium oxide particles in the range of 50 nm to 600 nm to increase the backscattering intensity I and the light blocking rate, thereby increasing the amount of power generation in the power generation layer 13. More preferably, the particle size of the titanium oxide particles is preferably set to 300 nm to 600 nm. In the range of 300 nm to 600 nm, the effect of light reflection to the power generation layer 13 due to light blocking becomes greater, and the amount of power generation improves in the range of large particle sizes. However, if the particle size is 600 nm or more, the backscattering intensity I will be low and the reflection of light that contributes to power generation will be reduced, so a particle size of 600 nm or less is preferable.
[0071] Second embodiment Fig. 18 is a cross-sectional view of a dye-sensitized solar cell 30 according to the second embodiment. In Fig. 18, the same elements as those described in the first embodiment are denoted by the same reference numerals as in the first embodiment, and their description will be omitted below.
[0072] 18, in this embodiment, a sealing resin layer 19 is provided at a distance from the side surface 13q of the power generation layer 13. Then, a solid electrolyte precursor 16 is filled between the sealing resin layer 19 and the side surface 13q, and the solid electrolyte precursor 16 is heated to volatilize the acetonitrile, thereby forming a solid electrolyte 31.
[0073] Third embodiment Figures 19(a) to (d) are cross-sectional views of a dye-sensitized solar cell 40 according to the third embodiment. In Figures 19(a) to (d), the same elements as those in the first and second embodiments are denoted by the same reference numerals as those in these embodiments, and their description will be omitted below. In Figures 19(a) to (d), the positive electrode plate 17 and the sealing resin layer 19 are omitted to avoid complicating the drawings.
[0074] As shown in Figures 19(a) to (d), in this embodiment, the reflective layer 14 has a first portion 14f having a first thickness T1 and a second portion 14g having a second thickness T2 smaller than the first thickness T1.
[0075] Since the second portion 14g has a smaller thickness than the first portion 14f, the solid electrolyte precursor 16 can easily permeate into the power generation layer 13 through the second portion 14g. This makes it possible to increase the amount of solid electrolyte impregnated into the power generation layer 13, thereby improving the power generation efficiency in the power generation layer 13.
[0076] (Fourth embodiment) Fig. 20 is a cross-sectional view of a dye-sensitized solar cell 50 according to the fourth embodiment. In Fig. 20, the same elements as those in the first to third embodiments are denoted by the same reference numerals as those in these embodiments, and description thereof will be omitted below.
[0077] As shown in FIG. 20, in this embodiment, the upper surface 13p and the side surface 13q of the power generation layer 13 are provided with unevenness. In this embodiment, the unevenness is defined as a difference between a convex portion of the power generation layer 13 toward the reflective layer 14 and a concave portion of the reflective layer 14 toward the power generation layer 13 in the range of 0.3 to 0.5 μm. The method of forming the unevenness is not particularly limited. For example, the upper surface 13p and the side surface 13q each naturally become roughened surfaces reflecting the titanium oxide particles contained in the reflective layer 14, and the roughened surfaces may be used as the unevenness as they are. In this case, when the magnification is adjusted so that 50 or more titanium oxide particles of the reflective layer 14 present at the interface between the power generation layer 13 and the reflective layer 14 are included in one image using a scanning electron microscope, a structure is obtained in which one or more titanium oxide particles are embedded in the power generation layer 14 with a difference between the unevenness of 0.3 μm or more. Alternatively, the unevenness may be formed by roughening the upper surface 13p and the side surface 13q after the power generation layer 13 is formed.
[0078] As a result, light L is diffusely reflected by each of upper surface 13p and side surface 13q, and each portion of power generation layer 13 generates power from the diffusely reflected light L, thereby improving the power generation efficiency of power generation layer 13. EXAMPLES
[0079] As an example, the dye-sensitized solar cell 20 according to the first embodiment was fabricated and its characteristics were examined. PST-30NRD manufactured by JGC Catalysts and Chemicals was used as the first titanium oxide paste 13a, which is the material of the power generation layer 13. PST-400C manufactured by JGC Catalysts and Chemicals was used as the second titanium oxide paste 14a, which is the material of the reflective layer 14.
[0080] 21 to 24 are diagrams obtained by investigating the amount of power generated by the dye-sensitized solar cell 20 when the length W and thickness a (see FIGS. 15(a) to (d)) are changed. In the investigation, the amounts of power generated in the first comparative example and the second comparative example were also investigated. In the first comparative example, the reflective layer 14 was not formed. In the second comparative example, the reflective layer 14 was formed only on the upper surface 13p of the power generation layer 13, and the reflective layer 14 was not formed on the side surface 13q.
[0081] In the examples, the amount of power generated was investigated for each of a case where the reflective layer 14 was formed on only one of the side surfaces 13q opposing each other in a cross-sectional view, and a case where the reflective layer 14 was formed on both of the side surfaces 13q opposing each other.
[0082] 21 to 24, the amount of power generated by the dye-sensitized solar cell 20 could be effectively increased by providing the reflective layer 14 on the upper and side surfaces of the power generation layer 13. Furthermore, by setting the thickness a to 0.5 μm to 6.5 μm and the length W to 0.1 μm to 50 μm, the amount of power generated was 103% or more of that in the first comparative example. [Explanation of symbols]
[0083] 10 Transparent substrate 10a Partial area 11 Transparent electrode layer 12 Reverse electron transfer prevention layer 13 Power generation layer 13a First titanium oxide paste 13f lower layer 13g upper layer 13p top 13q side 13r end 14 Reflective layer 14a Second titanium oxide paste 14f First Part 14g Second part 14p Titanium oxide particles 14q Pigment 15 Solvents 16 Solid electrolyte precursor 17 Positive plate 19 Sealing resin layer 31 Solid electrolyte 20, 30, 40, 50 Dye-sensitized solar cells
Claims
1. A substrate; A first electrode layer provided on a surface of the substrate; a power generation layer provided on the first electrode layer and including a dye and an electrolyte; a reflective layer provided on at least a portion of an upper surface of the power generation layer and at least a portion of a side surface of the power generation layer; a second electrode layer provided on the reflective layer; having A dye-sensitized solar cell, wherein, in a plan view, a part of the upper surface of the power generation layer protrudes from the reflective layer.
2. 2. The dye-sensitized solar cell according to claim 1, wherein the power generation layer has a thickness of 0.5 μm to 6.5 μm.
3. 3. The dye-sensitized solar cell according to claim 1, wherein the reflective layer and the first electrode layer are in contact with each other in a cross-sectional view, and a length of a portion where the reflective layer and the first electrode layer are in contact with each other in a cross-sectional view is 0.1 μm to 50 μm.
4. the power generation layer includes a plurality of first particles; the reflective layer includes a plurality of second particles; 4. The dye-sensitized solar cell according to claim 1, wherein the average particle size of the second particles is larger than the average particle size of the first particles.
5. 5. The dye-sensitized solar cell according to claim 4, wherein the second particles have an average particle size of 50 nm to 600 nm.
6. 6. The dye-sensitized solar cell according to claim 1, wherein at least a portion of the side surfaces is exposed and not covered with the reflective layer.
7. 6. The dye-sensitized solar cell according to claim 1, wherein the reflective layer covers the entire upper surface and the entire side surface of the power generation layer.
8. 8. The dye-sensitized solar cell according to claim 1, wherein at least a part of the side surface is inclined with respect to a line perpendicular to the upper surface.
9. 9. The dye-sensitized solar cell according to claim 1, wherein the reflective layer has a first portion having a first thickness and a second portion having a second thickness smaller than the first thickness.
10. 10. The dye-sensitized solar cell according to claim 1, wherein at least one of the upper surface and the side surface is provided with projections and recesses.
11. the reflective layer comprises a plurality of particles; 11. The dye-sensitized solar cell according to claim 10, wherein the particles penetrate into the power generation layer side by a depth of 0.3 μm or more at the interface between the power generation layer and the reflective layer.
12. A substrate, A first electrode layer provided on a surface of the substrate; a power generation layer provided on the first electrode layer and including a dye and an electrolyte; a reflective layer provided on at least a part of an upper surface and a side surface of the power generation layer; a second electrode layer provided on the reflective layer; a side surface of the substrate, a side surface of the first electrode layer, and a side surface of the second electrode layer are located at substantially the same position in a plan view of the substrate; A dye-sensitized solar cell, characterized in that an area from a side surface of the first electrode layer to a side surface of the second electrode layer is sealed with a sealing resin layer.
13. A dye-sensitized solar cell as described in Claim 12, characterized in that, in a planar view of the substrate, the power generation layer is provided up to the position of a side surface of the first electrode layer.
Citation Information
Patent Citations
Photoelectrode and dye-sensitized solar cell
JP2012119189A
Photoelectric conversion element, and photoelectric conversion element module
JP2012256470A
Dye-sensitized solar cell element
JP2014199788A
Photoelectric conversion element and dye-sensitized solar cell
JP2014229434A