Positive photosensitive resin composition and cured product thereof

JP7591893B2Active Publication Date: 2024-11-29KANEKA CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020153228
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-11
Publication Date
2024-11-29
Estimated Expiration
2040-09-11

AI Technical Summary

Benefits of technology

【0018】 本発明は、優れたアルカリ可溶性と耐熱性を有する高分子化合物を提供することである。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591893000001
    Figure 0007591893000001
  • Figure 0007591893000002
    Figure 0007591893000002
  • Figure 0007591893000003
    Figure 0007591893000003
Patent Text Reader

Abstract

To provide a positive photosensitive resin composition which exhibits excellent patterning properties and heat resistance.SOLUTION: The positive photosensitive resin composition contains (A) a polymer including formula (1) in a repeating unit, (B) a photoacid generator, and (C) a solvent. Each R independently represents a hydrogen atom or an acid-decomposable group which is easily decomposed by an acid to change to hydrogen atoms.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive-type photosensitive resin composition, which is a material widely used in the electronics field such as semiconductors and displays, etc. The present invention also relates to a cured product obtained by curing the positive-type photosensitive resin composition. [Background technology]

[0002] Photosensitive resins, which are widely used in the electronics field such as semiconductors and displays, need to be soluble in an alkaline developer when forming a pattern by photolithography. Therefore, polymer compounds having an alkali-soluble acidic group are used. Among them, the development of a photosensitive resin having particularly high heat resistance is required, and for example, a photosensitive resin composition using a polyimide resin having potentially high heat resistance has been proposed. As a specific technical example, for example, Patent Documents 1 and 2 describe a photosensitive composition using a polyimide resin containing a phenol group as an alkali-soluble acidic group in the polymer molecule. Patent Documents 3 and 4 describe a photosensitive composition using a polyimide resin containing a carboxyl group as an acidic group in the polymer molecule.

[0003] However, in the case of resins containing phenolic groups, in order to express solubility in an alkaline developer during pattern formation by photolithography, it is necessary to add a large amount of low-molecular-weight components such as phenolic oligomers and crosslinkers that have low acidity, and while resins with carboxyl groups have high acidity, the carboxyl groups themselves are prone to oxidation and thermal decomposition at high temperatures.Therefore, there is a demand for polymeric compounds that contain acidic groups with high acidity and excellent heat resistance. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-040273 A [Patent Document 2] JP 2008-197418 A [Patent Document 3] Patent No. 3972481 [Patent Document 4] Patent No. 5735341 Summary of the Invention [Problem to be solved by the invention]

[0005] Therefore, an object of the present invention is to provide a polyimide-based photosensitive resin composition having excellent patterning properties, as well as excellent heat resistance and electrical insulation properties. [Means for solving the problem]

[0006] As a result of extensive investigations aimed at achieving the above object, it has been discovered that a positive-type photosensitive resin composition having excellent patterning properties, as well as excellent heat resistance and electrical insulation properties, can be obtained by using a polymer containing an acidic group of a specific structure protected by a specific acid-dissociable protecting group in the main chain.

[0007] [1] A positive photosensitive resin composition comprising, as essential components, (A) a polymer having a repeating unit represented by the following general formula (1) and / or (2), (B) a photoacid generator, and (C) a solvent: (In the general formulas (1) and (2), R each independently represents a hydrogen atom or an acid-decomposable group that is easily decomposed by an acid to a hydrogen atom, and X represents a tetravalent organic group.)

[0008] [ka]

[0009] [ka]

[0010] [2] The positive photosensitive resin composition according to [1], wherein R in the above general formula (1) and / or (2) is any one selected from a hydrogen atom, an alkoxymethyl group, an alkoxycarbonyl group, a trialkylsilyl group, and an acetal.

[0011] [3] The positive photosensitive resin composition according to [2], wherein R in the above general formula (1) and / or (2) is any acid-decomposable group selected from a tert-butoxycarbonyl group, a methoxymethyl group, a trimethylsilyl group, and a tetrahydropyranyl group.

[0012] [4] The positive photosensitive resin composition according to any one of [1] to [3], wherein X in the general formula (1) and / or (2) contains at least one aromatic ring structure.

[0013] [5] The positive photosensitive resin composition according to any one of [1] to [4], wherein the (B) photoacid generator is a nonionic photoacid generator.

[0014] [6] The positive photosensitive resin composition according to any one of [1] to [5], wherein the (B) photoacid generator is a compound selected from the group consisting of oxime sulfonate compounds and imide sulfonate compounds.

[0015] [7] The positive photosensitive resin composition according to any one of [1] to [6], further comprising a photosensitizer.

[0016] [8] The positive photosensitive resin composition according to any one of [1] to [7], further comprising a silane coupling agent.

[0017] [9] A cured product obtained by curing the positive photosensitive resin composition according to any one of the above [1] to [8]. Effect of the Invention

[0018] The present invention provides a polymer compound having excellent alkali solubility and heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] (Positive-type photosensitive resin composition) It has been found that a positive-type photosensitive resin composition can be provided that contains, as essential components, (A) a polymer containing, as a repeating unit, a structure represented by the following general formula (1) and / or (2), (B) a photoacid generator, and (C) a solvent, and that the general formula (1) or (2) is characterized by having an isocyanuric acid skeleton, and thus has excellent patterning properties, heat resistance, and electrical insulation properties. (In general formulas (1) and (2), R each independently represents a hydrogen atom or an acid-decomposable group that is easily decomposed by an acid to a hydrogen atom, and X represents a tetravalent organic group.)

[0020] [ka]

[0021] [ka]

[0022] (Component (A): Polymer) The positive photosensitive resin composition contains, as component (A), a polymer having a specific structure in the repeating unit as an essential component.

[0023] The component (A) of the present invention is a polymer having a polyamic acid structure represented by the following general formula (1) and / or a polymer having a polyimide structure represented by the following general formula (2): (In the general formulas (1) and (2), R each independently represents a hydrogen atom or an acid-decomposable group that is easily decomposed by an acid to a hydrogen atom, and X represents a tetravalent organic group.)

[0024] [ka]

[0025] [ka]

[0026] As an example of a method for synthesizing the polyamic acid of the general formula (1), although the production method is not particularly limited, for example, an isocyanate compound having a nitro group as represented by chemical formulas (3) to (5) is reacted with KCON to obtain an isocyanuric acid compound, and the nitro group is reduced to obtain a diamine compound represented by general formula (6), which is reacted with a tetracarboxylic dianhydride in a suitable solvent at room temperature while stirring to obtain the polyamic acid.

[0027] [ka]

[0028] [ka]

[0029] [ka]

[0030] [ka]

[0031] The isocyanuric acid derivative can be synthesized according to a conventional method in organic chemistry. For example, when the organic group R in the above general formula (1) is a hydrogen atom, the isocyanuric acid derivative can be obtained by heating and stirring an isocyanate compound and KOCN in a suitable solvent, as shown in the following reaction formula (7).

[0032] [ka]

[0033] The diamine can be obtained by reducing the dinitro compound obtained by the above reaction formula (7). The reduction method is not particularly limited, and a known method can be used. For example, catalytic reduction with hydrogen gas using Pd / C as a catalyst can be used as shown in the following reaction formula (8).

[0034] [ka]

[0035] Examples of the tetracarboxylic acid dianhydride used in obtaining the polyamic acid (1) of the present invention are not particularly limited, and include, for example, 2,2'-hexafluoropropylidenediphthalic dianhydride, 2,2-bis(4-hydroxyphenyl)propane dibenzoate-3,3',4,4'-tetracarboxylic dianhydride, butane tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutane tetracarboxylic acid, 1,2,3 aliphatic or alicyclic tetracarboxylic dianhydrides such as 2,4-cyclopentanetetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 3,5,6-tricarboxynorbonane-2-acetic dianhydride, 2,3,4,5-tetrahydrofurantetracarboxylic dianhydride, 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic dianhydride, and bicyclo[2,2,2]-oct-7-ene-2,3,5,6-tetracarboxylic dianhydride;Pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenylsulfone tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dimethyldiphenylsilane tetracarboxylic dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic dianhydride, 1,2,3,4-furan tetracarboxylic dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride aromatic tetracarboxylic dianhydrides such as 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(phthalic acid)phenylphosphine oxide dianhydride, p-phenylene-bis(triphenylphthalic acid) dianhydride, m-phenylene-bis(triphenylphthalic acid) dianhydride, bis(triphenylphthalic acid)-4,4'-diphenylether dianhydride, and bis(triphenylphthalic acid)-4,4'-diphenylmethane dianhydride, and derivatives thereof, which may be used alone or in combination of two or more kinds;

[0036] As the diamine used in the synthesis of the polyamic acid of the present invention, in addition to the isocyanuric acid skeleton-containing diamine compound (6), other diamine compounds can be used in combination. These diamine compounds are not particularly limited, but examples thereof include [bis(4-amino-3-carboxy)phenyl]methane, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminophenylethane, 4,4'-diaminophenylether, 4,4'-diaminophenylsulfide, 4,4'-diaminophenylsulfone, 1,5-diaminonaphthalene, 3,3-dimethyl-4,4'-diaminobiphenyl, 5-amino-1-(4'-aminophenyl)-2-(2-methylphenyl)-2-(2-phenyl ... nyl)-1,3,3-trimethylindane, 6-amino-1-(4'-aminophenyl)-1,3,3-trimethylindane, 4,4'-diaminobenzanilide, 3,5-diamino-3'-trifluoromethylbenzanilide, 3,5-diamino-4'-trifluoromethylbenzanilide, 3,4'-diaminodiphenyl ether, 2,7-diaminofluorene, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-methylene-bis(2-chloroaniline), 2,2',5,5' -Tetrachloro-4,4'-diaminobiphenyl, 2,2'-dichloro-4,4'-diamino-5,5'-dimethoxybiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(3-amino phenoxy)phenyl]sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(4-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)-biphenyl, 1,3'-bis(4-aminophenoxy)benzene, 1,3'-bis(3-aminophenoxy)benzene, 9,9-bis(4-aminophenyl)fluorene, 4,4'-(p-phenyleneisopropylidene)bisaniline, 4,Aromatic diamines such as 4'-(m-phenyleneisopropylidene)bisaniline, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, and 4,4'-bis[4-(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl; aromatic diamines having two amino groups bonded to an aromatic ring and a heteroatom other than the nitrogen atom of the amino group, such as diaminotetraphenylthiophene; 1,1-meta-xylylenediamine, 1,3-propanediamine, tetramethylenediamine, pentamethylenediamine, octamethylenediamine, nonamethylenediamine, Examples of the diamine include aliphatic diamines and alicyclic diamines such as diamine, 4,4-diaminoheptamethylenediamine, 1,4-diaminocyclohexane, isophoronediamine, tetrahydrodicyclopentadienylenediamine, hexahydro-4,7-methanoindanylenediamine, tricyclo[6,2,1,02.7]-undecylenedimethyldiamine, and 4,4'-methylenebis(cyclohexylamine), and their derivatives. These can be used alone or in any ratio to add to the isocyanuric acid skeleton-containing diamine compound represented by general formula (6).

[0037] The polyamic acid synthesis solvent is not particularly limited, but may be any solvent that dissolves the diamine component, the tetracarboxylic dianhydride component, and the generated polyamic acid. For example, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-methylcaprolactam, dimethylsulfoxide, tetramethylurea, pyridine, dimethylsulfone, hexamethylsulfoxide, γ-butyrolactone, isopropyl alcohol, methoxymethylpentanol, dipentene, ethylene glycol, ethylene glycol ether ... Chill amyl ketone, methyl nonyl ketone, methyl ethyl ketone, methyl isoamyl ketone, methyl isopropyl ketone, methyl cellosolve, ethyl cellosolve, methyl cellosolve acetate, ethyl cellosolve acetate, butyl carbitol, ethyl carbitol, ethylene glycol, ethylene glycol monoacetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol, propylene glycol monoacetate, propylene glycol monomethyl ether, propylene glycol tert-butyl ether, dipropylene glycol monomethyl ether, diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, dipropylene glycol monoacetate monomethyl ether, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxy Butyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutylene, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methylcyclohexene, propyl ether, dihexyl ether, dioxane, n-hexane, n-pentane, n-octane, diethyl ether, cyclohexanone, ethylene carbonate, propylene carbonate, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate,Examples of the propylene glycol monoethyl ether acetate include propylene glycol monoethyl ether acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, diglyme, 4-hydroxy-4-methyl-2-pentanone, 3-methoxy-N,N-dimethylpropanamide, 3-ethoxy-N,N-dimethylpropanamide, and 3-butoxy-N,N-dimethylpropanamide. These may be used alone or in combination of two or more.

[0038] The reaction conditions for synthesizing the polyamic acid are not particularly limited, and known conditions can be used. For example, the diamine monomer is sufficiently dissolved in a solvent, and the acid dianhydride monomer is added little by little at room temperature, followed by stirring at room temperature for 24 hours.

[0039] As described above, the example of general formula (1) has been described. R is preferably any one selected from a hydrogen atom, an alkoxymethyl group, an alkoxycarbonyl group, a trialkylsilyl group, and an acetal, more preferably any one selected from a tert-butoxycarbonyl group, a methoxymethyl group, a trimethylsilyl group, and a tetrahydropyranyl group, and particularly preferably a hydrogen atom. X preferably contains at least one aromatic ring structure.

[0040] The same applies to the general formula (2).

[0041] Next, a method for synthesizing the polyimide represented by the general formula (2) will be described.

[0042] The polyimide (2) of the present invention can be obtained by imidizing the polyamic acid (1) described above. The imidization method can be any known method, and is not particularly limited, including, for example, a thermal imidization method in which a polyamic acid solution is stirred at high temperature and a chemical imidization method in which an imidization catalyst is added to a polyamic acid solution and then stirred. In the thermal imidization method, the temperature range is 120 o C~400 o C, preferably 150 o C~250 o It's C.

[0043] In the chemical imidization method, a basic catalyst and an acid anhydride are added to the imidization reaction solution at -30 o C~200 o C, preferably 0 o C~150 o The reaction is carried out in C. The amount of the basic catalyst is 0.5 to 30 times by mole, preferably 2 to 20 times by mole, the amount of the amic acid group, and the amount of the acid anhydride is 1 to 50 times by mole, preferably 3 to 30 times by mole, the amount of the amic acid group.

[0044] Applicable basic catalysts include pyridine, triethylamine, trimethylamine, 3-picoline, isoquinoline, and the like.

[0045] Examples of the acid anhydride used in the catalytic imidization include acetic anhydride, trimellitic anhydride, pyromellitic anhydride, and trifluoroacetic anhydride.

[0046] The isocyanuric acid group (NH group) of the isocyanuric acid group-containing polymer obtained as described above is protected with a functional group that is decomposed by acid, and the isocyanuric acid group becomes an acid decomposable group, and the polymer of the present invention can be obtained. The functional group that protects the isocyanuric acid is not particularly limited, and examples thereof include tert-butoxycarbonyl group, tetrahydropyranyl group, trimethylsilyl group, dimethylvinylsilyl group, dimethylbutylsilyl group, acetal group, and tert-butyl group. On the other hand, normal alkyl group, phenyl group, etc. that are not decomposed by acid are not suitable. From the viewpoint of reactivity, it is preferable to protect the polymer with a tert-butoxycarbonyl group, tetrahydropyranyl group, etc.

[0047] The amount of the specific acidic group introduced is not necessarily limited by the type and conditions of the alkaline developer used in photolithography, but the amount of the structure (1) or (2) described above is from 0.01 mmol / g to 10 mmol / g per gram of the component (A) polymer, and from the viewpoints of making it easy to control the solubility in the developer and to form a pattern, it is preferably from 0.1 mmol / g to 5 mmol / g.

[0048] (Component (B): Photoacid generator) In the photosensitive resin composition of the present invention, a photoacid generator is an essential component, and the type is not particularly limited, and a plurality of types can be used in combination.

[0049] The photoacid generator that can be used is not particularly limited, and examples thereof include metal fluoroboron complex salts and boron trifluoride complex compounds as described in U.S. Pat. No. 3,379,653; bis(perfluoroalkylsulfonyl)methane metal salts as described in U.S. Pat. No. 3,586,616; aryldiazonium compounds as described in U.S. Pat. No. 3,708,296; aromatic onium salts of Group VIa elements as described in U.S. Pat. No. 4,058,400; aromatic onium salts of Group Va elements as described in U.S. Pat. No. 4,069,055; dicarbonyl chelates of Group IIIa to Va elements as described in U.S. Pat. No. 4,068,091; thiopyrylium salts as described in U.S. Pat. No. 4,139,655; and MF compounds as described in U.S. Pat. No. 4,161,478. 6 - Group VIa elements in the form of anions (where M is selected from phosphorus, antimony and arsenic); arylsulfonium complex salts as described in U.S. Pat. No. 4,231,951; aromatic iodonium and aromatic sulfonium complex salts as described in U.S. Pat. No. 4,256,828; bis[4-(diphenylsulfonio)phenyl]sulfide-bishexafluorometal salts (e.g., phosphates, arsenates, antimonates, etc.) as described by W.R. Watt et al. in Journal of Polymer Science, Polymer Chemistry Edition, Vol. 22, p. 1789 (1984); 6 F 5 ) 4 - and aromatic iodonium complex salts and aromatic sulfonium complex salts represented by the formula:

[0050] Preferred photoacid generators include arylsulfonium complex salts, aromatic sulfonium and iodonium salts of halogen-containing complex ions, and aromatic onium salts of Group II, V, and VI elements, sulfonate esters, and carboxylate esters. Some of these salts are commercially available as FX-512 (3M), UVR-6990 and UVR-6974 (Union Carbide), UVE-1014 and UVE-1016 (General Electric), KI-85 (Degussa), and SP-152 and SP-172 (Asahi Denka).

[0051] The onium salt is tetrafluoroborate (BF 4 - ), hexafluorophosphate (PF 6 - ), hexafluoroantimonate (SbF 6 - ), hexafluoroarsenate (AsF 6 - ), hexachloroantimonate (SbCl 6 - ), tetraphenylborate, tetrakis(trifluoromethylphenyl)borate, tetrakis(pentafluoromethylphenyl)borate, perchlorate ion (ClO 4 - ), trifluoromethanesulfonate ion (CF 3 SO 3 - ), fluorosulfonate ion (FSO 3 - ), sulfonium salts and iodonium salts having anions such as toluenesulfonate ion, trinitrobenzenesulfonate anion, and trinitrotoluenesulfonate anion.

[0052] Specific examples of sulfonium salts include triphenylsulfonium hexafluoroacylanate, triphenylsulfonium hexafluoroborate, triphenylsulfonium tetrafluoroborate, triphenylsulfonium tetrakis(pentafluorobenzyl)borate, methyldiphenylsulfonium tetrafluoroborate, methyldiphenylsulfonium tetrakis(pentafluorobenzyl)borate, dimethylphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluoroantimonate, diphenylnaphthylsulfonium hexafluoroarsenate, tritoylsulfonium hexafluorophosphate, anisyldiphenylsulfonium hexafluoroantimonate, 4-butoxyphenyldiphenylsulfonium tetrafluoroborate, 4-butoxyphenyldiphenylsulfonium tetrakis(pentafluorobenzyl)borate, 4-chlorophenyldiphenyl Sulfonium hexafluoroantimonate, tris(4-phenoxyphenyl)sulfonium hexafluorophosphate, di(4-ethoxyphenyl)methylsulfonium hexafluoroarsenate, 4-acetylphenyldiphenylsulfonium tetrafluoroborate, 4-acetylphenyldiphenylsulfonium tetrakis(pentafluorobenzyl)borate, tris(4-thiomethoxyphenyl)sulfonium hexafluorophosphate, di(methoxysulfonylphenyl)methylsulfonium hexafluoroantimonate, di(methoxynaphthyl)methylsulfonium tetrafluoroborate, di(methoxynaphthyl)methylsulfonium tetrakis(pentafluorobenzyl)borate, di(carbomethoxyphenyl)methylsulfonium hexafluorophosphate, (4-octyloxyphenyl)diphenylsulfonium tetrakis(3,5-bis-trifluoromethylphenyl)borate, tris(dodecylphenyl)sulfonium tetrakis(3,5-bis-trifluoromethylphenyl)borate, 4-acetamidophenyldiphenylsulfonium tetrafluoroborate, 4-acetamidophenyldiphenylsulfonium tetrakis(pentafluorobenzyl)borate, dimethylnaphthylsulfonium hexafluorophosphate, trifluoromethyldiphenylsulfonium tetrafluoroborate, trifluoromethyldiphenylsulfonium tetrakis(pentafluorobenzyl)borate, phenylmethylbenzylsulfonium hexafluorophosphate, 10-methylphenoxathiinium hexafluorophosphate , 5-methylthianthrenium hexafluorophosphate, 10-phenyl-9,9-dimethylthioxanthenium hexafluorophosphate, 10-phenyl-9-oxothioxanthenium tetrafluoroborate, 10-phenyl-9-oxothioxanthenium tetrakis(pentafluorobenzyl)borate, 5-methyl-10-oxothianthreneium tetrafluoroborate, 5-methyl-10-oxothianthreneium tetrakis(pentafluorobenzyl)borate, and 5-methyl-10,10-dioxothianthreneium hexafluorophosphate. These can be used alone or in combination of two or more.

[0053] Specific examples of iodonium salts include (4-n-decyloxyphenyl)phenyliodonium hexafluoroantimonate, [4-(2-hydroxy-n-tetradecyloxy)phenyl]phenyliodonium hexafluoroantimonate, [4-(2-hydroxy-n-tetradecyloxy)phenyl]phenyliodonium trifluorosulfonate, [4-(2-hydroxy-n-tetradecyloxy)phenyl]phenyliodonium hexafluorophosphate, and [4-(2-hydroxy-n-tetradecyloxy)phenyl]phenyliodonium hexafluorophosphate. Bis(4-t-butylphenyl)iodonium tetrakis(pentafluorophenyl)borate, bis(4-t-butylphenyl)iodonium hexafluoroantimonate, bis(4-t-butylphenyl)iodonium hexafluorophosphate, bis(4-t-butylphenyl)iodonium trifluorosulfonate, bis(4-t-butylphenyl)iodonium tetrafluoroborate, bis(dodecylphenyl)iodonium hexafluoroantimonate, bis(dodecylphenyl)iodonium tetrafluoroborate, bis(dodecylphenyl)iodonium dodecylphenyliodonium hexafluorophosphate, bis(dodecylphenyl)iodonium trifluoromethylsulfonate, di(dodecylphenyl)iodonium hexafluoroantimonate, di(dodecylphenyl)iodonium triflate, diphenyliodonium bisulfate, 4,4'-dichlorodiphenyliodonium bisulfate, 4,4'-dibromodiphenyliodonium bisulfate, 3,3'-dinitrodiphenyliodonium bisulfate, 4,4'-dimethyldiphenyliodonium bisulfate, 4,4'-bissuccinimide Examples of suitable diazonium salts include diphenyliodonium bisulfate, 3-nitrodiphenyliodonium bisulfate, 4,4'-dimethoxydiphenyliodonium bisulfate, bis(dodecylphenyl)iodonium tetrakis(pentafluorophenyl)borate, (4-octyloxyphenyl)phenyliodonium tetrakis(3,5-bis-trifluoromethylphenyl)borate, and other aromatic diazonium salts, such as p-methoxybenzenediazonium hexafluoroantimonate.

[0054] As the sulfonate esters, various sulfonic acid derivatives can be used, for example, disulfones, disulfonyldiazomethanes, disulfonylmethanes, sulfonylbenzoylmethanes, imide sulfonates such as trifluoromethylsulfonate derivatives, benzoin sulfonates, sulfonates of 1-oxy-2-hydroxy-3-propyl alcohol, pyrogallol trisulfonates, and benzylsulfonates. Specifically, diphenyl disulfone, ditosyl disulfone, bis(phenylsulfonyl)diazomethane, bis(chlorophenylsulfonyl)diazomethane, bis(xylylsulfonyl)diazomethane, phenylsulfonylbenzoyldiazomethane, bis(cyclohexylsulfonyl)methane, 1,8-naphthalenedicarboxylic acid imide methyl sulfonate, 1,8-naphthalenedicarboxylic acid imide tosyl sulfonate, 1,8-naphthalenedicarboxylic acid imide trifluoromethyl sulfonate, 1,8-naphthalenedicarboxylic acid imide camphorsulfonate, succinic acid imide phenyl sulfonate, succinic acid imide tosyl sulfonate Examples of the photoacid generator include succinimide trifluoromethylsulfonate, succinimide camphorsulfonate, phthalimide trifluorosulfonate, cis-5-norbornene-endo-2,3-dicarboxylic acid imide trifluoromethylsulfonate, benzoin tosylate, 1,2-diphenyl-2-hydroxypropyl tosylate, 1,2-di(4-methylmercaptophenyl)-2-hydroxypropyl tosylate, pyrogallol methylsulfonate, pyrogallol ethylsulfonate, 2,6-dinitrophenyl methyl tosylate, ortho-nitrophenyl methyl tosylate and para-nitrophenyl tosylate. These can be used alone or in combination of two or more. In the present invention, carboxylic acid esters can also be used as photoacid generators.

[0055] The content of the photoacid generator in the positive photosensitive resin composition is not particularly limited, but from the viewpoint of curability, it is preferably 0.01 to 10 parts by weight per 100 parts by weight of component (A), and more preferably 0.1 to 5.0 parts by weight from the viewpoint of the balance of physical properties of the cured product. If the amount of the photoacid generator is small, the deprotection reaction may not proceed sufficiently, and the patterning property may be reduced. Moreover, if the amount of the photoacid generator is large, it may be undesirable because it may cause coloring or impair heat resistance or light resistance.

[0056] (Photosensitizer) The positive photosensitive resin composition may contain a photosensitizer. By adding a photosensitizer, the positive photosensitive resin composition can be made more sensitive to visible light and can be made more sensitive to high wavelength light such as g-line (436 nm), h-line (405 nm) and i-line (365 nm). By using these sensitizers in combination with the above-mentioned photoacid generator, the patterning property of the positive photosensitive resin composition can be adjusted. Examples of the sensitizer include anthracene-based compounds and thioxanthone-based compounds.

[0057] Specific examples of the anthracene-based compound include anthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-dimethylanthracene, 9,10-dibutoxyanthracene, 9,10-dipropoxyanthracene, 9,10-diethoxyanthracene, 1,4-dimethoxyanthracene, 9-methylanthracene, 2-ethylanthracene, 2-tert-butylanthracene, 2,6-di-tert-butylanthracene, 9,10-diphenyl-2,6-di-tert-butylanthracene, etc. In particular, from the viewpoint of easy availability, anthracene, 9,10-dimethylanthracene, 9,10-dibutoxyanthracene, 9,10-dipropoxyanthracene, 9,10-diethoxyanthracene, etc. are preferred as the anthracene-based compound.

[0058] As the anthracene-based compound, anthracene is preferred from the viewpoint of excellent transparency of the cured product, and 9,10-dibutoxyanthracene, 9,10-dipropoxyanthracene, 9,10-diethoxyanthracene, and the like are preferred from the viewpoint of excellent compatibility with the curable composition.

[0059] Specific examples of the thioxanthone compounds include thioxanthone, 2-chlorothioxanthone, and 2,5-diethyldioxanthone.

[0060] These sensitizers may be used alone or in combination of two or more.

[0061] The content of the sensitizer in the curable composition of the present invention is not particularly limited as long as it is an amount that can exert a sensitizing effect, but is preferably 0.01 to 300 mol, more preferably 0.1 mol to 100 mol, relative to 1 mol of the photoacid generator. If the amount of the sensitizer is small, the sensitizing effect cannot be obtained, and development may take a long time, which may have an unfavorable effect on the developability. On the other hand, if the amount of the sensitizer is large, there is a risk that color may remain in the cured product or that heat resistance or light resistance may be impaired.

[0062] (Silane coupling agent) The positive photosensitive resin composition may contain a silane coupling agent for the purpose of improving adhesion. The silane coupling agent is not particularly limited as long as it is a compound having at least one functional group reactive with an organic group and at least one hydrolyzable silicon group in the molecule. As the group reactive with an organic group, from the viewpoint of handling, at least one functional group selected from an epoxy group, a methacryl group, an acrylic group, an isocyanate group, an isocyanurate group, a vinyl group, and a carbamate group is preferable, and from the viewpoint of curing and adhesion, an epoxy group, a methacryl group, or an acrylic group is particularly preferable. As the hydrolyzable silicon group, from the viewpoint of handling, an alkoxysilyl group is preferable, and from the viewpoint of reactivity, a methoxysilyl group or an ethoxysilyl group is particularly preferable.

[0063] Examples of preferred silane coupling agents include alkoxysilanes having an epoxy functional group, such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane; and alkoxysilanes having a methacryl group or an acryl group, such as 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, methacryloxymethyltrimethoxysilane, methacryloxymethyltriethoxysilane, acryloxymethyltrimethoxysilane, and acryloxymethyltriethoxysilane.

[0064] The amount of the silane coupling agent added can be appropriately set, but is preferably 0.1 to 20 parts by weight, more preferably 0.3 to 10 parts by weight, and even more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the compound having a photopolymerizable functional group. If the amount added is small, the adhesiveness improving effect is not achieved, and if the amount added is large, it may have an adverse effect on the physical properties of the cured product.

[0065] Furthermore, these coupling agents, silane coupling agents, epoxy compounds, etc. may be used alone or in combination of two or more.

[0066] (filling material) The positive photosensitive resin composition may contain a filler if necessary.Various types of filler are used, including inorganic fillers such as silica-based fillers (quartz, fume silica, precipitated silica, silicic anhydride, fused silica, crystalline silica, ultrafine powder amorphous silica, etc.), silicon nitride, silver powder, alumina, aluminum hydroxide, titanium oxide, glass fiber, carbon fiber, mica, carbon black, graphite, diatomaceous earth, clay, clay, talc, calcium carbonate, magnesium carbonate, barium sulfate, and inorganic balloon, as well as fillers that are generally used or proposed as fillers for conventional sealing materials, such as epoxy-based fillers.

[0067] (Anti-aging agent) The positive photosensitive resin composition may contain an antioxidant, which may include commonly used antioxidants such as hindered phenol-based antioxidants, as well as citric acid, phosphoric acid, and sulfur-based antioxidants.

[0068] As the hindered phenol-based antioxidant, various types can be used, including Irganox 1010 available from Ciba Specialty Chemicals.

[0069] Examples of the sulfur-based antiaging agents include mercaptans, mercaptan salts, sulfides (sulfide carboxylates, hindered phenol-based sulfides, etc.), polysulfides, dithiocarboxylates, thioureas, thiophosphates, sulfonium compounds, thioaldehydes, thioketones, mercaptals, mercaptols, monothioacids, polythioacids, thioamides, and sulfoxides. These antiaging agents may be used alone or in combination of two or more.

[0070] (UV absorber) The positive photosensitive resin composition may contain an ultraviolet absorbing agent. Examples of the ultraviolet absorbing agent include 2(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole and bis(2,2,6,6-tetramethyl-4-piperidine)sebacate. These ultraviolet absorbing agents may be used alone or in combination of two or more.

[0071] (solvent) The solvent used is not particularly limited, and specific examples thereof include ether-based solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and diethyl ether; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; glycol-based solvents such as propylene glycol-1-monomethyl ether-2-acetate (PGMEA) and ethylene glycol diethyl ether; and halogen-based solvents such as chloroform, methylene chloride, and 1,2-dichloroethane.

[0072] From the viewpoint of polyamic acid and polyimide, DMF, DMAc, γ-butyrolactone, NMP, tetrahydrofuran, 1,3-dioxolane, and propylene glycol-1-monomethyl ether-2-acetate are preferred as the solvent. The amount of the solvent used can be appropriately set, but the preferred lower limit of the amount used per 1 g of the positive photosensitive resin composition used is 0.1 mL, and the preferred upper limit of the amount used is 10 mL. If the amount of the solvent used is small, it may be difficult to obtain the effect of using the solvent, such as low viscosity. In addition, if the amount of the solvent used is large, the solvent may remain in the material, which may cause problems such as thermal cracking, and may be disadvantageous in terms of cost, resulting in a decrease in industrial utility value. As these solvents, one type may be used, or two or more types may be used as a mixed solvent.

[0073] (others) To the positive photosensitive resin composition, colorants, release agents, flame retardants, flame retardant assistants, surfactants, defoamers, emulsifiers, leveling agents, anti-repellents, ion trapping agents (antimony-bismuth, etc.), thixotropy imparting agents, tackifiers, storage stability improvers, ozone degradation inhibitors, light stabilizers, thickeners, plasticizers, reactive diluents, antioxidants, heat stabilizers, electrical conductivity imparting agents, antistatic agents, radiation shielding agents, nucleating agents, phosphorus-based peroxide decomposers, lubricants, pigments, rust inhibitors, metal deactivators, thermal conductivity imparting agents, physical property adjusters, and the like can be added within the scope of not impairing the objects and effects of the present invention.

[0074] (Pattern formation method) The positive photosensitive resin composition is applied in a layer form on a substrate, followed by drying to obtain a laminate (substrate / photosensitive resin composition). The laminate is then exposed to light and developed with an alkaline developer to form a pattern.

[0075] As a light source for photocuring (exposing) the positive photosensitive resin composition, a light source that emits light having an absorption wavelength of the polymerization initiator and sensitizer used may be used, and a light source having a wavelength in the range of 200 to 450 nm (e.g., a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a high-power metal halide lamp, a xenon lamp, a carbon arc lamp, or a light-emitting diode) can usually be used.

[0076] The exposure dose for photocuring the negative photosensitive resin composition is not particularly limited, but is preferably 1 to 10,000 mJ / cm2, more preferably 1 to 3,000 mJ / cm2. If the exposure dose is too low, the positive photosensitive resin composition may not dissolve in the developer. Even the unexposed area, which is exposed to a large amount of light, may dissolve in the developer.

[0077] In order to remove the solvent and improve the physical properties of the cured product, heat may be applied before or after photocuring to perform pre-baking and after-baking. The curing temperature can be appropriately set, but is preferably 40 to 400°C, and more preferably 60 to 350°C.

[0078] There is no particular limitation on the method for forming a pattern using an alkaline developer, and the desired pattern can be formed by dissolving and removing the unexposed areas using a commonly used developing method such as an immersion method or a spray method.

[0079] In addition, the developer used in the alkaline development can be any commonly used developer without any particular limitation. Specific examples of the developer include organic alkaline aqueous solutions such as tetramethylammonium hydroxide (TMAH) aqueous solution and choline aqueous solution, and inorganic alkaline aqueous solutions such as potassium hydroxide aqueous solution, sodium hydroxide aqueous solution, potassium carbonate aqueous solution, sodium carbonate aqueous solution and lithium carbonate aqueous solution. The aqueous solution may contain alcohol and surfactants to adjust the dissolution rate. The concentration of the aqueous solution is preferably 25% by weight or less, more preferably 10% by weight or less, and even more preferably 5% by weight or less, from the viewpoint of easily achieving a contrast between the exposed and unexposed areas.

[0080] (Application) The positive photosensitive resin composition of the present invention can be used in various applications. For example, it can be used as a transparent material, an optical material, an optical lens, an optical film, an optical sheet, an adhesive for optical components, an optical adhesive for optical waveguide coupling, an adhesive for fixing peripheral components of an optical waveguide, an adhesive for bonding DVDs, a pressure sensitive adhesive, a dicing tape, an electronic material, an insulating material (including a printed circuit board, an electric wire coating, etc.), a high voltage insulating material, an interlayer insulating film, a passivation film for TFT, a gate insulating film for TFT, an interlayer insulating film for TFT, a transparent flattening film for TFT, an insulating packing, an insulating coating material, an adhesive, a high heat resistance adhesive, a high heat dissipation adhesive, an optical adhesive, an adhesive for LED elements, an adhesive for various substrates, an adhesive for a heat sink, a paint, a UV powder paint, an ink, a colored ink, an ink for UV inkjet, a coating material (including a hard coat, a sheet, a film, a coat for release paper, a coat for optical disks, and a coat for optical fibers, etc.), a molding material (including a sheet, a film, and FRP, etc.), a sealing material, a potting material. , sealing materials, sealing materials for light-emitting diodes, sealing materials for optical semiconductors, hollow structures for CMOS / CCD sensors, hollow structures for MEMS devices, liquid crystal sealants, sealants for display devices, sealing materials for electrical materials, sealing materials for various solar cells, high heat-resistant sealants, resist materials, liquid resist materials, color resists, dry film resist materials, solder resist materials, binder resins for color filters, transparent flattening materials for color filters, binder resins for black matrices, photospacer materials for liquid crystal cells, transparent sealing materials for OLED elements, photolithography, materials for solar cells, materials for fuel cells, display materials, recording materials, vibration-proof materials, waterproof materials, moisture-proof materials, heat-shrinkable rubber tubes, O-rings, photosensitive drums for copiers, solid electrolytes for batteries, gas separation membranes, concrete protective materials, linings, soil injection agents, cold and heat storage materials, sealing materials for sterilization treatment equipment, contact lenses, and oxygen-permeable membranes. The isocyanuric acid skeleton-containing polymer may also be used as an additive to other resins, etc. EXAMPLES

[0081] The present invention will be described in more detail below based on examples, but the present invention is not limited to the following examples.

[0082] (Patterning evaluation) A patterning evaluation sample was prepared using the resin composition obtained in the examples and comparative examples. First, the resin composition obtained in the examples and comparative examples was spin-coated on a glass substrate, and heated on a hot plate heated to 100°C for 2 minutes. Next, using an exposure device (high pressure mercury lamp, manual exposure machine, manufactured by Dai Nippon Kaken Co., Ltd.), exposure was performed with an optimal integrated light amount for each resin composition through a mask engraved with a 50 μm line and space pattern (soft contact exposure), and the substrate was left for 1 minute after exposure. After that, the substrate was immersed in an alkaline developer (2.38% aqueous TMAH solution) for 180 seconds, and then washed with water for 30 seconds to form a pattern. Then, the substrate was heated on a hot plate at 200°C for 60 minutes to obtain a patterning evaluation sample.

[0083] The pattern shape of the obtained patterning evaluation sample was observed using a 3D measuring laser microscope (LEXT OLS4000, manufactured by Olympus) and a stylus-type surface shape measuring instrument (Dektak150, manufactured by Veeco), and the state of the 50 μm line and space was evaluated according to the following criteria.

[0084] <Evaluation criteria> ○: Practical level (no residual film on 50μm line and space) ×: Not suitable for practical use (film remains in 50 μm line and space) (Heat resistance evaluation) Using a thermogravimetric analyzer (TGA, manufactured by Shimadzu Corporation), the temperature was raised from room temperature to 500°C at a rate of 10°C / min, and evaluation was performed using the 5% weight loss temperature as an index.

[0085] (Electrical insulation evaluation) The resin compositions obtained in the Examples and Comparative Examples were spin-coated on a glass substrate with a molybdenum thin film, and heated on a hot plate heated to 100°C for 2 minutes. Next, after exposure to 300 mJ / cm2 using an exposure device (high pressure mercury lamp, manual exposure device, manufactured by Dainihon Kaken Co., Ltd.), the substrate was heated on a hot plate at 230°C for 30 minutes to form a film of the photosensitive resin composition, and an aluminum electrode (3 mmΦ) was formed on the film using a vacuum deposition machine to create a capacitor. The leakage current between the upper and lower electrodes was measured using a semiconductor parameter analyzer (Agilent 4156) when a voltage of 30 V was applied.

[0086] (Synthesis example A) A 2L flask was charged with 1L of N,N-dimethylformamide and 38g of potassium cyanate, and heated to 75℃. Next, 224g of 4-nitrophenyl isocyanate was added dropwise using a dropping funnel, and the mixture was stirred for 30 minutes after the dropwise addition to complete the reaction. After that, N,N-dimethylformamide was removed under reduced pressure, and 1L of ethyl acetate and 3L of water were added. Concentrated hydrochloric acid was then added to the aqueous layer to collect the precipitate, which was then recrystallized with ethanol to obtain white crystals.

[0087] Next, 30 g of the compound white crystals obtained above, 1 g of palladium catalyst Pd / C, and 200 mL of dimethylacetamide were added to a 500 mL flask, and the flask was heated with H 2 The mixture was reacted under a 50° C. atmosphere for 6 hours with stirring at 90° C. After the reaction was completed, the solvent was distilled off, and the solid was washed with water. The solid was recrystallized from ethanol to obtain diamine compound 1 represented by the following chemical formula (9).

[0088] [ka]

[0089] (Synthesis Example 1) In a 200mL flask, 30g of N,N-dimethylformamide as a solvent, 3.1g of the diamine compound 1 obtained in the above synthesis example, and 4.4g of 2,2'-hexafluoropropylidenediphthalic dianhydride were added and stirred at room temperature under a nitrogen atmosphere for 24 hours. Furthermore, 10g of N,N-dimethylformamide, 1.9g of pyridine, and 5.0g of acetic anhydride were added in sequence to the flask, and the mixture was stirred for 3 hours while heating to 90°C. After the mixture returned to room temperature, 300mL of isopropyl alcohol was added to the flask, and the precipitate was collected. The mixture was washed three times with 300mL of isopropyl alcohol, and the obtained precipitate was dried under reduced pressure at 80°C for 6 hours to obtain polyimide resin A.

[0090] Next, 3 g of polyimide resin A was added to 25 mL of 1-methylpyrrolidone, and 0.1 g of pyridine and 3 g of di-tert-butyl dicarbonate were further added, followed by stirring at 70° C. for 1 hour. 1 Completion of the protection reaction was confirmed by disappearance of the NH peak of isocyanuric acid by -NMR, yielding polyimide resin A-1 in which the isocyanuric acid group was protected.

[0091] (Synthesis Example 2) Polyimide A was obtained in the same manner as in Synthesis Example 1, and then 3 g of polyimide resin A was added to 27 mL of 1-methylpyrrolidone, and 0.5 g of toluenesulfonic acid and 3 g of dihydropyran were further added, followed by stirring at 70° C. for 3 hours. 1 Completion of the protection reaction was confirmed by disappearance of the NH peak of isocyanuric acid by -NMR, yielding polyimide resin A-2 in which the isocyanuric acid group was protected.

[0092] (Synthesis Example 3) Polyimide resin A was obtained in the same manner as in Synthesis Example 1, and then 3 g of polyimide resin A was added to 25 mL of 1-methylpyrrolidone, and 3 g of hexamethyldisilazane was further added thereto, followed by stirring at 70° C. for 3 hours. 1 Completion of the protection reaction was confirmed by disappearance of the NH peak of isocyanuric acid by -NMR, yielding polyimide resin A-3 in which the isocyanuric acid group was protected.

[0093] (Synthesis Example 4) Polyimide resin A-4 having protected isocyanuric acid groups was obtained in the same manner as in Synthesis Example 1, except that 1 g of 1,2,3,4-cyclobutanetetracarboxylic dianhydride was used instead of the tetracarboxylic dianhydride in Synthesis Example 1.

[0094] (Synthesis example B) A 2L flask was charged with 1L of N,N-dimethylformamide and 38g of potassium cyanate, and heated to 75℃. Next, 224g of 3-nitrophenyl isocyanate was added dropwise using a dropping funnel, and the mixture was stirred for 30 minutes after the dropwise addition to complete the reaction. After that, N,N-dimethylformamide was removed under reduced pressure, and 1L of ethyl acetate and 3L of water were added. Concentrated hydrochloric acid was then added to the aqueous layer to collect the precipitate, which was then recrystallized with ethanol to obtain white crystals.

[0095] Next, 30.0 g of the white crystals of the compound obtained above, 1 g of palladium catalyst Pd / C, and 200 mL of dimethylacetamide were added to a 500 mL flask, and the flask was heated with H 2 The mixture was reacted under a 50° C. atmosphere for 6 hours with stirring at 90° C. After the reaction was completed, the solvent was distilled off, and the solid was washed with water. The mixture was recrystallized from ethanol to obtain diamine compound 2 represented by the following chemical formula (10).

[0096] [ka]

[0097] (Synthesis Example 5) In a 200mL flask, 30g of N,N-dimethylformamide as a solvent, 3.1g of the diamine compound 2 obtained in the above synthesis example, and 4.4g of 2,2'-hexafluoropropylidenediphthalic dianhydride were added and stirred at room temperature under a nitrogen atmosphere for 24 hours. Furthermore, 10g of N,N-dimethylformamide, 1.9g of pyridine, and 5.0g of acetic anhydride were added in sequence to the flask, and the mixture was stirred for 3 hours while heating to 90°C. After the mixture returned to room temperature, 300mL of isopropyl alcohol was added to the flask, and the precipitate was collected. The mixture was washed three times with 300mL of isopropyl alcohol, and the obtained precipitate was dried under reduced pressure at 80°C for 6 hours to obtain polyimide resin B.

[0098] Next, 3 g of polyimide resin B was added to 27 mL of 1-methylpyrrolidone, and 0.1 g of pyridine and 3 g of di-tert-butyl dicarbonate were further added, followed by stirring at 70° C. for 1 hour. 1 Completion of the protection reaction was confirmed by disappearance of the NH peak of isocyanuric acid by -NMR, yielding polyimide resin B-1 in which the isocyanuric acid group was protected.

[0099] (Synthesis Example 6) Polyimide resin B was obtained in the same manner as in Synthesis Example 5, and then 3 g of polyimide resin B was added to 50 mL of 1-methylpyrrolidone, and 0.5 g of toluenesulfonic acid and 3 g of dihydropyran were further added, followed by stirring at 70° C. for 3 hours. 1 Completion of the protection reaction was confirmed by disappearance of the NH peak of isocyanuric acid by -NMR, yielding polyimide resin B-2 in which the isocyanuric acid group was protected.

[0100] (Synthesis Example 7) Polyimide resin B was obtained in the same manner as in Synthesis Example 5, and then 3 g of polyimide resin B was added to 27 mL of 1-methylpyrrolidone, and 3 g of hexamethyldisilazane was further added thereto, followed by stirring at 70° C. for 3 hours. 1 Completion of the protection reaction was confirmed by disappearance of the NH peak of isocyanuric acid by -NMR, yielding polyimide resin B-3 in which the isocyanuric acid group was protected.

[0101] (Synthesis Example 8) Polyimide resin B-4 having protected isocyanuric acid groups was obtained in the same manner as in Synthesis Example 5, except that 1 g of 1,2,3,4-cyclobutanetetracarboxylic dianhydride was used instead of the tetracarboxylic dianhydride in Synthesis Example 5.

[0102] Example 1 Photosensitive composition 1 was prepared by mixing 10.0 g of a 10% NMP solution of polyimide resin (A-1) described in Synthesis Example 1 as component (A) and 0.05 g of Irgacure PAG169 (manufactured by BASF) as component (B).

[0103] Example 2 Photosensitive composition 2 was prepared by mixing 10.0 g of a 10% NMP solution of polyimide resin (A-2) described in Synthesis Example 2 as component (A) and 0.05 g of Irgacure PAG169 (manufactured by BASF) as component (B).

[0104] Example 3 Photosensitive composition 3 was prepared by mixing 10.0 g of a 10% NMP solution of polyimide resin (A-3) described in Synthesis Example 3 as component (A) and 0.05 g of Irgacure PAG169 (manufactured by BASF) as component (B).

[0105] Example 4 Photosensitive composition 4 was prepared by mixing 10.0 g of a 10% NMP solution of polyimide resin (A-4) described in Synthesis Example 4 as component (A) and 0.05 g of Irgacure PAG169 (manufactured by BASF) as component (B).

[0106] Example 5 Photosensitive composition 5 was prepared by mixing 10.0 g of a 10% NMP solution of polyimide resin (B-1) described in Synthesis Example 5 as component (A) and 0.05 g of Irgacure PAG169 (manufactured by BASF) as component (B).

[0107] Example 6 Photosensitive composition 6 was prepared by mixing 10.0 g of a 10% NMP solution of polyimide resin (B-2) described in Synthesis Example 6 as component (A) and 0.05 g of Irgacure PAG169 (manufactured by BASF) as component (B).

[0108] Example 7 Photosensitive composition 7 was prepared by mixing 10.0 g of a 10% NMP solution of the polyimide resin (B-3) described in Synthesis Example 7 as component (A) and 0.05 g of Irgacure PAG169 (manufactured by BASF) as component (B).

[0109] Example 8 Photosensitive composition 8 was prepared by mixing 10.0 g of a 10% NMP solution of polyimide resin (B-4) described in Synthesis Example 8 as component (A) and 0.05 g of Irgacure PAG169 (manufactured by BASF) as component (B).

[0110] Comparative Example 1 Photosensitive composition 9 was prepared by dissolving 0.5 g of a phenol-containing resin, Marukalinker M (polyvinylphenol resin, manufactured by Maruzen Petrochemical Co., Ltd.), protected with a tert-butoxycarbonyl group as a comparison for component (A), and 0.10 g of Irgacure PAG169 (manufactured by BASF Co., Ltd.) as component (B) in 3.5 g of PGMEA (propylene glycol monomethyl ether acetate) as solvent (C).

[0111] (result) The above-mentioned evaluations were carried out on the photosensitive resin compositions obtained in Examples 1 to 8 and Comparative Example 1. The results are shown in Table 1.

[0112] [Table 1] [Industrial Applicability]

[0113] The present invention can be utilized in various fields, such as insulating interlayer films for electronic devices such as semiconductors and displays, adhesives, coating agents, and sealants.

Claims

1. A positive-type photosensitive resin composition comprising, as essential components, (A) a polymer containing a structure represented by the following general formula (1) and / or (2) as a repeating unit, (B) a photoacid generator, and (C) a solvent. (In the general formulas (1) and (2), R each independently represents a hydrogen atom or an acid-decomposable group that is easily decomposed by an acid to a hydrogen atom, and X represents a tetravalent organic group, except for the case where all of the R linked to the isocyanuric ring in the general formula (1) and / or (2) are hydrogen atoms.) 【Chemistry 1】 【Chemistry 2】

2. 2. The positive photosensitive resin composition according to claim 1, wherein R in the general formula (1) and / or (2) is any one selected from the group consisting of a hydrogen atom, an alkoxymethyl group, an alkoxycarbonyl group, a trialkylsilyl group, and an acetal.

3. 3. The positive photosensitive resin composition according to claim 2, wherein R in the general formula (1) and / or (2) is any acid-decomposable group selected from a tert-butoxycarbonyl group, a methoxymethyl group, a trimethylsilyl group, and a tetrahydropyranyl group.

4. 4. The positive photosensitive resin composition according to claim 1, wherein X in the general formula (1) and / or (2) contains at least one aromatic ring structure.

5. 5. The positive photosensitive resin composition according to claim 1, wherein the photoacid generator of the component (B) is a nonionic photoacid generator.

6. 6. The positive photosensitive resin composition according to claim 1, wherein the photoacid generator of the component (B) is a compound selected from the group consisting of an oxime sulfonate compound and an imide sulfonate compound.

7. 7. The positive photosensitive resin composition according to claim 1, further comprising a photosensitizer.

8. 8. The positive photosensitive resin composition according to claim 1, further comprising a silane coupling agent.

9. A cured product obtained by curing the positive photosensitive resin composition according to any one of claims 1 to 8.

10. A polyimide represented by the following general formula (2): (R represents an acid-decomposable group selected from an alkoxymethyl group, an alkoxycarbonyl group, a trialkylsilyl group, and an acetal, and X represents a tetravalent organic group.) 【Chemistry 3】

11. 11. The polyimide according to claim 10, wherein R is any acid-decomposable group selected from the group consisting of a tert-butoxycarbonyl group, a methoxymethyl group, a trimethylsilyl group, and a tetrahydropyranyl group.

Citation Information

Patent Citations

  • Method of seperating elements of semiconductor device

    JP1982035341A

  • Photosensitive polymer composition, method for producing relief pattern and electronic parts

    JP2003337415A

  • Photosensitive polyimide-silicone composition, protective film and flexible printed wiring board

    JP2008040273A

  • Polyimide copolymer, positive type photosensitive resin composition and method for forming pattern

    JP2008184499A

  • Photosensitive polyimide composition and method for preparing the same

    JP2008197418A