Photosensitive composition, cured product and organic electroluminescence display device
A photosensitive composition with benzodifuranone or perylene black pigments and a specific relaxation time ratio forms a pixel dividing layer in organic EL display devices, achieving low driving voltage and high brightness, resolving the visibility and lifespan trade-off.
Patent Information
- Application Number
- JP2020110109
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-06-26
AI Technical Summary
Organic EL display devices face high driving voltage issues when using a black pixel dividing layer without a polarizing plate, leading to reduced brightness and a trade-off between visibility and lifespan.
A photosensitive composition comprising benzodifuranone or perylene black pigments with a benzimidazole skeleton, a resin, a photosensitizer, and a solvent, formulated to achieve a specific spin-spin relaxation time ratio (X) of 55 to 125, which forms a pixel dividing layer with low driving voltage and high brightness.
The composition enables high brightness with low driving voltage, addressing the visibility and lifespan trade-off in organic EL display devices by optimizing the pixel dividing layer.
Smart Images

Figure 0007592989000047 
Figure 0007592989000048 
Figure 0007592989000049
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive composition, a cured product, and an organic electroluminescence display device. [Background technology]
[0002] Many products equipped with organic electroluminescence (EL) display devices have been developed, such as smartphones, televisions, and in-vehicle monitors. Organic EL display devices are self-emitting display devices that emit light using energy generated by the recombination of electrons injected from the cathode and holes injected from the anode, and each light-emitting pixel, such as red / blue / green or white, is formed in the openings of a patterned pixel division layer that also functions as an insulating layer.
[0003] Usually, a polarizing plate is provided on the front panel of an organic EL display device, i.e., the side where light is output from the pixel section, to suppress reflection of external light such as sunlight and improve visibility. However, it is well known that the polarizing plate blocks part of the light output from the light-emitting pixel section, resulting in unavoidable loss of brightness. In order to obtain high brightness, a high driving voltage must be applied, which places a heavy burden on the light-emitting element, and this is a technical hurdle in developing an organic EL display device with a long product life.
[0004] In recent years, therefore, attempts have been made to create a panel structure without a polarizing plate, and a technology that imparts an external light reflection suppressing function by blackening the pixel division layer to eliminate the trade-off relationship between visibility and lifespan has been attracting particular attention. As a material for forming a black pixel division layer, for example, Patent Document 1 discloses a negative photosensitive composition that contains an organic black pigment or a mixed-color organic black pigment dispersed to have a cumulant average particle size within a specific range. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-160473 A Summary of the Invention [Problem to be solved by the invention]
[0006] When a black pixel dividing layer is formed using the negative photosensitive composition disclosed in Patent Document 1, there is a problem that the driving voltage is high immediately after starting to drive the organic EL display device even though it does not have a polarizing plate. [Means for solving the problem]
[0007] The present invention relates to a photosensitive composition comprising (a-1) a benzodifuranone-based black pigment and / or (a-2) a perylene-based black pigment having a benzimidazole skeleton, (b) a resin, (c) a photosensitizer, and (d) a solvent, wherein the value of X in formula (1) is 55 to 125. X = T2 / A (1) In formula (1), T2 is the measurement nucleus for the T2 measurement sample. 1 The spin-spin relaxation time (ms) measured by the Carr-Purcell-Meiboom-Gill method using a H pulsed nuclear magnetic resonance spectrometer is shown as the average value of three measurements. A represents the content (wt %) of all components excluding particle components and solvent components in the total amount (100 wt %) of the T2 measurement sample, and is 6.50 to 8.80. Effect of the Invention
[0008] According to the photosensitive composition of the present invention, a pixel dividing layer that can provide high brightness at a low driving voltage in an organic EL display device can be formed. [Brief description of the drawings]
[0009] [Figure 1] 1 shows a process for producing an organic EL display device including a process for forming a pixel dividing layer in all of the examples and comparative examples. [Diagram 2]1 is a graph showing the relationship between the value of X in formula (1) and the driving voltage (V) of an organic EL display device. The horizontal axis is the value of X, and the vertical axis is the driving voltage (V). All examples are represented by plots of circles (●), and all comparative examples are represented by plots of triangles (▲). [Diagram 3] 1 is a graph showing the relationship between the maximum cumulative particle diameter Dmax and the driving voltage (V) of an organic EL display device. The horizontal axis is Dmax (nm) and the vertical axis is driving voltage (V). All examples are represented by circle (●) plots, and Comparative Examples 3 to 6 are represented by triangle (▲) plots. [Figure 4] 1 is a graph showing the relationship between the maximum cumulative particle size Dmax and the relaxation time T2. The horizontal axis is Dmax (nm) and the vertical axis is relaxation time T2 (ms). All examples are represented by circle (●) plots, and Comparative Examples 3 to 6 are represented by triangle (▲) plots. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. A numerical range expressed using "~" means a range including the numerical values before and after "~" as the lower and upper limits. The pixel division layer means a pixel division layer provided in an organic EL display device. Visible light means light in the wavelength range of 380 nm or more and less than 780 nm, and near ultraviolet light means light in the wavelength range of 200 nm or more and less than 380 nm. Light shielding means a function of reducing the intensity of transmitted light compared to the intensity of light incident perpendicularly to the cured film, and light shielding property means the degree of shielding visible light.
[0011] The photosensitive composition means a photosensitive composition that is sensitive to near ultraviolet light and is an alkali-developable type, and does not include compositions that are not sensitive to near ultraviolet light or organic solvent-developable compositions. The resin means a compound having a polymer chain and a weight-average molecular weight of 1000 or more, and does not include low-molecular compounds having a weight-average molecular weight of less than 1000. The weight-average molecular weight (Mw) is a value obtained by analyzing by gel permeation chromatography using tetrahydrofuran as a carrier and converting the value using a calibration curve based on standard polystyrene.
[0012] The "CI" used to name colorants is an abbreviation for Color Index Generic Name, and is based on the Color Index published by The Society of Dyers and Colourists. For colorants that are registered in the Color Index, the Color Index Generic Name represents the chemical structure or crystal form of the pigment or dye. For color classification, for example, yellow pigments include pigments that belong to "CI Pigment Yellow", blue pigments include pigments that belong to "CI Pigment Blue", red pigments include pigments that belong to "CI Pigment Red", and purple pigments include pigments that belong to "CI Pigment Violet", and the same is true for orange pigments, brown pigments, green pigments, black pigments, etc. For colorants that are not registered in the Color Index, specific structures are shown.
[0013] Carbon blacks classified as CI Pigment Black 7 and the like are classified as inorganic black pigments regardless of their crystallinity, conductivity, or manufacturing method. Azine compounds such as aniline black are classified as dyes or pigments depending on their molecular weight, and are classified as black dyes in this specification. Therefore, for example, CI Pigment Black 1 and 21 are not included in the organic black pigments in this specification. Azo black pigments do not include inorganic black pigments whose surface is modified with an organic group having an azo group.
[0014] As a result of extensive investigations, the present inventors have found that by forming a pixel dividing layer using a photosensitive composition in which the value of x in formula (1) is 55 to 125, the driving voltage of an organic EL display device can be reduced.
[0015] That is, the photosensitive composition of the present invention contains (a-1) a benzodifuranone-based black pigment and / or (a-2) a perylene-based black pigment having a benzimidazole skeleton, (b) a resin, (c) a photosensitizer, and (d) a solvent, and is a photosensitive composition in which the value of X in formula (1) is 55 to 125. X = T2 / A ··· (1) In formula (1), T2 represents the average value when the spin-spin relaxation time (ms) measured by the Carr-Purcell-Meiboom-Gill method using a pulsed nuclear magnetic resonance apparatus for measurement nucleus 1 H is measured three times. A represents the content (wt%) of all components except the particle component and the solvent component in 100 wt% of the total amount of the T2 measurement sample, and is 6.50 to 8.80.
[0016] In this specification, T2 means the value measured by the following measurement method. <T2 Measurement Conditions> Measuring device: Pulsed nuclear magnetic resonance apparatus “BRUKER” (registered trademark) minispec mp20 manufactured by Bruker BioSpin Measurement nucleus: 1 H Frequency of the measurement nucleus: 19.95 MHz Pulse width: 2.18 μs (90° pulse) Pulse repetition time: 10 seconds Solid content of the T2 measurement sample: 10.00 wt% Container for filling the T2 measurement sample: 10 mmφ NMR sample tube Liquid temperature of the T2 measurement sample: Kept constant at 25.0 °C by a temperature control function (under atmospheric pressure) Operation before measurement: Leave it in the probe for 20 minutes to stabilize the liquid temperature of the measurement sample. Calculation method of T2: For the T2 measurement sample, the average value when the spin-spin relaxation time (ms) measured by the Carr-Purcell-Meiboom-Gill method using a pulsed nuclear magnetic resonance apparatus for measurement nucleus 1 H is measured three times, and the average value is calculated and rounded to the first decimal place.
[0017] The T2 measurement sample here means an object for measuring T2, and corresponds to a photosensitive composition prepared so that the solid content is 10.00% by weight. The solid content (wt%) of the photosensitive composition refers to 100 times the weight (g) of the residue after heating 1.00 g of the photosensitive composition for 30 minutes on a hot plate set at an actual temperature of 200° C. under atmospheric pressure / air. In order to obtain good coating properties and improve the film thickness uniformity of the pixel division layer finally obtained, the photosensitive composition for forming the black pixel division layer is usually designed to have a solid content in the range of 10.00 to 30.00% by weight.
[0018] As a method for preparing a measurement sample, when the solid content of the photosensitive composition exceeds 10.00% by weight, a single or multiple solvents are added so as to have the same solvent composition as the (d) solvent component contained in the photosensitive composition, and the mixture is stirred and diluted so as to have a solid content of 10.00% by weight. When multiple solvents are added, a mixed solvent previously prepared so as to have the same mixing ratio as the (d) solvent is added to the photosensitive composition.
[0019] Conversely, if the solid content of the photosensitive composition is less than 10.00% by weight, the photosensitive composition is maintained and stirred under atmospheric pressure / liquid temperature 25±1°C conditions, and the (d) solvent is evaporated without heating to concentrate it to a solid content of 11.00% by weight, and then a single or multiple solvents are added and stirred so that the solvent component in the T2 measurement sample has the same solvent composition as the (d) solvent in the photosensitive composition before dilution, and the mixture is diluted to a solid content of 10.00% by weight. If the (d) solvent is not volatile under atmospheric pressure, it may be concentrated by a reduced pressure operation.
[0020] If the components of the (d) solvent contained in the photosensitive composition are unknown, they can be analyzed by gas chromatography-mass spectrometry. If the solid content of the photosensitive composition is originally 10.00% by weight, the above-mentioned operation of adjusting the solid content is not necessary, and the composition can be used as it is as a T2 measurement sample.
[0021] The method for measuring the relaxation time by pulse nuclear magnetic resonance analysis will be described below.
[0022] There are two types of methods: the Solid-Echo method, which applies a 90° pulse, then changes the phase by 90° and applies a second 90° pulse to induce an echo phenomenon, and the Carr-Purcell-Meiboom-Gill method, which applies a 180° pulse, which changes the phase by 90°, to the rotating magnetic field generated by applying a 90° pulse, and measures the attenuation behavior of each of the resulting echo intensities. The former method is applied when a solid sample with a short relaxation time is the measurement target, and the latter method, which can offset the imperfection of the phase, is applied when a liquid sample with a long relaxation time is the measurement target. Since the measurement sample in the present invention is a liquid dispersion containing solid particles, T2 is defined as the value measured by applying the latter method.
[0023] When a magnetic field is applied to a sample as a pulse, the nuclear spins of the protons in the sample are excited into a state where they are aligned. The process by which this returns to the original random ground state over time is called the relaxation phenomenon, and the time required for this process is the relaxation time, and it is known that the decay curve of the magnetization intensity is expressed as a function of the relaxation time. In other words, the relaxation time is a parameter that indicates the speed of the relaxation phenomenon. The process by which the magnetization in a plane perpendicular to the static magnetic field approaches zero over time and returns to equilibrium is called spin-spin relaxation, and its speed is expressed by the transverse relaxation time.
[0024] This transverse relaxation time is defined as the relaxation time T2 (ms). The relaxation time T2 (ms) is determined by the interaction between protons in the measurement sample placed in a magnetic field. The unit (ms) means milliseconds, and the relaxation time T2 (ms) is a positive value (T2>0). In other words, the higher the molecular mobility, the smaller the interaction between adjacent protons, and the larger the relaxation time T2 (ms). Conversely, the lower the molecular mobility, the greater the interaction between adjacent protons, and the smaller the relaxation time T2 (ms).
[0025] The relaxation time T2 (ms) of the T2 measurement sample can be controlled mainly by the molecular mobility of the dispersion medium. The dispersion medium is a medium for dispersing the particle components to be dispersed, and refers to all components other than the particle components contained in the T2 measurement sample.
[0026] On the other hand, the value of A represents the content (wt%) of all components excluding particle components and solvent components in the total amount (100 wt%) of the T2 measurement sample, and is 6.50 to 8.80. This numerical range means that the content (%) of particle components in the T2 measurement sample is 1.20 to 3.50 wt%, and at the same time, the content of particle components in the solid content of the photosensitive composition is 12 to 35 wt%. The value of A is preferably 7.50 to 8.60 in order to reduce the driving voltage.
[0027] The value of X in formula (1) is calculated by dividing the value of T2 by the value of A and rounding off to the first decimal place. It means the relaxation time (ms / wt%) converted to 1.00 wt% of all components excluding particle components and solvent components. The particle components referred to here include the component (a) contained in the photosensitive composition, which will be described later. All components excluding particle components and solvent components include the components (b) and (c) contained in the photosensitive composition, which will be described later. The solvent components include the solvent used in the preparation of the T2 measurement sample and the component (d) contained in the photosensitive composition.
[0028] The photosensitive composition satisfies the condition that the value of X in formula (1) is 55 to 125. When the value of X in formula (1) is 55 to 125, a pixel dividing layer having excellent light-shielding properties can be formed, and the driving voltage for obtaining high brightness in an organic EL display device having the same can be reduced. Hereinafter, the characteristic of being able to drive at a low voltage when obtaining high brightness is referred to as low voltage driving. From the viewpoint of low voltage driving, the value of X is preferably 60 to 100, and more preferably 65 to 85.
[0029] The photosensitive composition of the present invention contains (a-1) a benzodifuranone-based black pigment (hereinafter, sometimes referred to as component (a-1)) and / or (a-2) a perylene-based black pigment having a benzimidazole skeleton (hereinafter, sometimes referred to as component (a-2)). Hereinafter, component (a-1) and component (a-2) may be collectively referred to as component (a).
[0030] Component (a) is a pigment that has both high visible light absorption and high near-infrared transmittance, and allows easy mask alignment using a near-infrared camera, making it possible to form a pixel division layer that has both high positional accuracy and high light blocking properties. In addition, since component (a) is a pigment with excellent insulating properties, the pixel division layer filled with component (a) preferably has high insulating properties.
[0031] When the photosensitive composition has negative photosensitivity, that is, when it is a negative photosensitive composition, it preferably contains at least the (a-1) component from the viewpoint of good optical compatibility with the photopolymerization initiator contained in the (c) photosensitizer and low-voltage operation. On the other hand, when the photosensitive composition has positive photosensitivity, that is, when it is a positive photosensitive composition, it preferably contains the (a-2) component from the viewpoint of good optical compatibility with the photoacid generator contained in the (c) photosensitizer and low-voltage operation.
[0032] The component (a-1) refers to an organic black pigment having, in the molecule, a benzodifuranone skeleton in which two furanone rings are condensed to one benzene ring.
[0033] An example of the (a-1) component is bis-oxodihydroindolylene-benzodifuranone described in International Publication No. 2009 / 010521. In particular, from the viewpoint of low-voltage operation, it is preferable that the (a-1) component contains at least one compound selected from the group consisting of the compound represented by formula (2), the compound represented by formula (3), and their isomers. The isomers referred to here include geometric isomers and tautomers. The isomers may be contained as a mixture, or a plurality of compounds having an isomeric relationship may form a mixed crystal to constitute one crystallite or primary particle.
[0034] [ka]
[0035] [ka]
[0036] In formula (2) and formula (3), R 1 and R 6 R each independently represents a hydrogen atom, CH3, CF3 or a fluorine atom. 2 , R 3 , R 4 , R 5 , R 7 , R 8 , R 9 and R 10 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, a cycloalkenyl group having 1 to 12 carbon atoms, an alkynyl group having 1 to 12 carbon atoms, COOH, COOR 11 , COO - , CONH2, CONHR 11 ,CONR 11 R 12 , C.N., O.H., O.R. 11 , O.C.O.R. 11 , OCONH2, OCONHR 11 ,OCONR 11 R 12 Represents R 2 and R 3 , R 3 and R 4 , R 4 and R 5 , R 7 and R 8 , R 8 and R 9 , and R 9 and R 10 is a direct bond or O, S, NH, or NR 11 They may be joined by R 11 and R 12each independently represents an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, a cycloalkenyl group having 1 to 12 carbon atoms, or an alkynyl group having 1 to 12 carbon atoms.
[0037] Among these, from the viewpoint of low-voltage driving, the component (a-1) is R in formula (2). 1 ~R 10 is a hydrogen atom or an isomer thereof. That is, it is more preferable that the (a-1) component contains a compound represented by formula (4) or an isomer thereof. The compound represented by formula (4) may be a commercially available product, such as "Irgaphor" (registered trademark) Black S0100CF and Experimental Black 582 (both manufactured by BASF).
[0038] [ka]
[0039] The component (a-2) refers to an organic black pigment having a benzimidazole skeleton and a perylene skeleton. Among them, the component (a-2) preferably contains a compound represented by formula (5) and / or a compound represented by formula (6). These cis-trans isomers may be included as a mixture, or a plurality of compounds may form a mixed crystal to constitute one crystallite or primary particle.
[0040] [ka]
[0041] [ka]
[0042] In formula (5) and formula (6), R 13 ~R 20each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or a hydroxyl group.
[0043] Among them, from the viewpoint of low-voltage operation, R 13 ~R 20 is a hydrogen atom. That is, it is more preferable that the component (a-2) contains a perylene-based black pigment consisting of a mixture of a compound represented by formula (7) which is a cis isomer and a compound represented by formula (8) which is a trans isomer. From the viewpoints of high UV transmittance, excellent exposure sensitivity, and low driving voltage, it is even more preferable that the component (a-2) contains 30% by weight or more of the trans isomer, with the total of the cis and trans isomers being 100% by weight.
[0044] The mixture of the compound represented by formula (7) and the compound represented by formula (8) may be a commercially available product, such as "Lumogen Black" (registered trademark) FK4281 (manufactured by BASF). The component (a-2) may be treated with a rosin-based treatment agent in order to reduce the dry aggregation of the pigment and to increase the deaggregation in the wet dispersion treatment described below. The rosin-based treatment agent is preferably 5 to 25% by weight of the pigment surface, which is insolubilized by acid precipitation. The fine pigment containing a rosin-based treatment agent may be a commercially available product, such as "Lumogen Black" (registered trademark) K0087 and "Paliogen Black" (registered trademark) EH0788 (both manufactured by BASF).
[0045] [ka]
[0046] [ka]
[0047] The photosensitive composition of the present invention may further contain other particle components for the purpose of adjusting the optical properties of the pixel division layer. Examples of such components include organic black pigments other than component (a), as well as organic yellow pigments, organic orange pigments, organic red pigments, organic blue pigments, organic purple pigments, and inorganic black pigments.
[0048] Examples of organic black pigments other than the component (a) include azomethine-based black pigments described in JP 2010-116549 A and JP 2017-193689 A, and anthraquinone-based black pigments described in JP 2018-145353 A. Examples of organic yellow pigments include CI Pigment Yellow 120, 138, 139, 151, 175, 180, 185, 181, 192, 193, and 194. Examples of organic orange pigments include CI Pigment Orange 13, 36, 43, 61, 64, 71, and 72.
[0049] Examples of organic red pigments include CI Pigment Red 122, 123, 149, 178, 179, 180, 189, 190, 202, 209, 254, 255, and 264. Examples of organic blue pigments include CI Pigment Blue 15, 15:1, 15:2, 15:3, 15:6, 16, 56, 57, 60, 61, 64, 65, 66, 75, 79, and 80. Examples of organic purple pigments include CI Pigment Violet 19, 23, 29, 32, and 37. Examples of inorganic black pigments include carbon black and titanium nitride coated with a polymer. Among these, azomethine black pigments and carbon black coated with a polymer are preferred.
[0050] In general, when comparing multiple particle dispersions made of the same type of particle components that differ only in the specific surface area of the particle components, it is known that there is a certain range in which the larger the specific surface area of the particle components, the smaller the relaxation time T2, and the smaller the specific surface area, the longer the relaxation time T2. However, when comparing photosensitive compositions with different components and / or manufacturing methods, for example, the surface smoothness, functional groups, charge, and activity of the particle components, as well as interactions with components (b) to (d), affect the molecular mobility of the entire dispersion medium in a complex manner, so that the relaxation time T2 depends on all the components and the manufacturing method of the dispersion. Therefore, in order to obtain the effects of the present invention, it is necessary to control the value of X in formula (1) to be 55 to 125, taking into consideration these various parameters comprehensively.
[0051] The means for controlling the value of X in formula (1) by the particle component is not particularly limited. However, the specific surface area of the particle component contained in the photosensitive composition is preferably 10 to 100 m 2 / g is preferable, and 20 to 60m 2 / g is more preferable. When a mixture of multiple types of particles is used, the specific surface area can be calculated by the weighted average of the specific surface area of each particle. If the specific surface area is within the above-mentioned range, it is easy to control the value of X to a range of 55 to 125. The specific surface area here means the specific surface area measured by the BET method using nitrogen as the adsorption gas.
[0052] The average primary particle diameter of the particle component is preferably 10 to 150 nm, more preferably 40 to 100 nm. If the average primary particle diameter is within the above-mentioned range, uneven distribution of pigment aggregates is suppressed, and the value of X can be easily controlled to a range of 55 to 125. The average primary particle diameter here refers to the number average value of the primary particle diameter calculated by a particle size measurement method using an image analysis type particle size distribution measurement device. A transmission electron microscope (TEM) can be used to take the image, and the average primary particle diameter can be calculated from an image of 100 or more primary particles taken under a condition of 50,000 times magnification. If the particles are not spherical, the average value of the major axis and minor axis is taken as the primary particle diameter. For image analysis, the image analysis type particle size distribution software Mac-View manufactured by Mountech Co., Ltd. can be used.
[0053] The average primary particle size can be controlled by wet-pulverization, which can be, for example, in the case of component (a), a known method such as solvent salt milling.
[0054] In the photosensitive composition, the component (a-1) preferably has a coating material on its surface, and the coating material preferably contains silica.
[0055] When the photosensitive composition of the present invention has negative photosensitivity, it is more preferable that the (a-1) component contains at least one compound selected from the group consisting of the compound represented by formula (2), the compound represented by formula (3) and / or their isomers, the (c) photosensitizer contains a compound having two or more radical polymerizable groups in the molecule and a photopolymerization initiator, and the (a-1) component further has a coating material on its surface, and the coating material contains silica.Moreover, it is most preferable that the (b) resin contains the (b-1) basic group-containing resin, the (b-1) basic group-containing resin contains a (meth)acrylic block copolymer having a quaternary ammonium base, and the quaternary ammonium base contains a structure consisting of a salt of a quaternary ammonium cation and a carbon atom-containing counter anion. Silica here refers to silicon dioxide (SiO2) or hydrous silicon dioxide (SiO2·H2O). Silica has a smaller interaction with the electrode surface that forms the openings of the pixel dividing layer than organic pigments, and when the value of X in formula (1) is controlled to be the same, it is possible to obtain the effect of lowering the driving voltage. As for silica to be used as a coating material, silica obtained by reacting an organic acid and / or inorganic acid with an alkali metal silicate is preferable, since it has excellent adhesion to the pigment surface and can produce a dense silica layer.
[0056] As a method for coating with component (a-1), for example, after component (a-1) is deaggregated in an aqueous medium, a dilute aqueous solution of sulfuric acid and a dilute aqueous solution of an alkaline alkali metal silicate are added continuously and in parallel, respectively, to neutralize the pigment surface and precipitate hydrated silica, which is deposited in layers. The pigment is then dehydrated, sintered, and pulverized by a dry heat treatment to obtain the pigment. The heat treatment temperature is preferably 230°C or higher in order to enhance adhesion to the pigment surface. In order to maintain the particle shape before heating and suppress the generation of foreign matter, a temperature of 280°C or lower is more preferable. From the same viewpoint, the heating time is preferably 1 to 6 hours.
[0057] In order to enhance the effect of low-voltage driving by the coating material containing silica, the number of reactive silanol groups per SiO2 equivalent mass must be 5.00 × 10 10 / g or more, 7.50×10 18 It is preferable to dehydrate and sinter the silica so that the silanol group content is 1 / g or less. The number of reactive silanol groups can be calculated by reacting the residual silanol groups of the silica with the silane treating agent (3,3,3-trifluoropropyl)chlorodimethylsilane in an organic solvent in the presence of a base catalyst, and then quantifying the total amount of fluorine using combustion ion chromatography. When components other than silica contain fluorine atoms, the amount of fluorine derived from these components can be subtracted from the calculation.
[0058] The effect of the coating material containing silica is particularly effective when the photosensitive composition is a negative photosensitive composition, when the photocuring of the film cannot be sufficiently promoted in the exposure step described below, for example, when a pixel division layer having a step is formed by halftone processing and a spacer function is imparted, and when driving at a low voltage. The halftone processing here means a method of forming a pattern having a shape with a difference in film thickness between a thick film part and a thin film part on the substrate surface by developing after pattern exposure using a halftone exposure mask having openings with different light transmittances in the surface.
[0059] A specific example of a method for forming a pixel division layer by halftone processing is the method described in International Publication WO2019 / 182041. Note that, for the purpose of controlling the value of X in formula (1), the above-mentioned silica may be partially surface-modified with a silane coupling agent such as blocked isocyanate silane.
[0060] The photosensitive composition of the present invention contains a (b) resin (hereinafter, sometimes referred to as component (b)). Component (b) has the effect of stabilizing the dispersion state of the particle components and also serves as a binder that constitutes the pixel dividing layer.
[0061] The means for controlling the value of X in formula (1) by the (b) component is not particularly limited, but examples include a method of manipulating the molecular weight distribution of the component belonging to the (b) component, the number of functional groups that have adsorptivity for particle components, the number of adsorption points per molecule adsorbed to one particle, the number of molecules that take a bridging-type adsorption form spanning multiple particles, and the affinity with the molecules of the (d) solvent described below.
[0062] The (b) resin preferably contains (b-1) a basic group-containing resin and / or (b-2) an alkali-soluble resin, which may be referred to as the (b-1) component and the (b-2) component, respectively.
[0063] When the photosensitive composition is a negative photosensitive composition, it is preferable to contain the (b-1) component and the (b-2) component from the viewpoint of low voltage driving. On the other hand, when the photosensitive composition is a positive photosensitive composition, it is preferable to contain only the (b-2) component from the viewpoint of low voltage driving. Note that a resin that contains a basic group and corresponds to an alkali-soluble resin is defined as belonging to the (b-1) component.
[0064] The component (b-1) refers to a resin having one or more basic groups in the molecule, and corresponds to a so-called resin-type dispersant.
[0065] Examples of the basic group include a primary amino group, a secondary amino group, a tertiary amino group, and salts thereof, as well as a quaternary ammonium base. The bonding site of the basic group in the resin structure is not particularly limited, and may be a terminal group, a linking group, a side chain and / or a part of the main chain, and may form a cyclic structure or a polyamine structure. Among them, in order to control the value of X in the formula (1) within the range of 55 to 125, a tertiary amino group and a quaternary ammonium base are preferred, and it is more preferred that the (b-1) component contains both functional groups. Note that the amide structure and the imide structure, which are nitrogen-containing structures, do not belong to the basic group referred to here.
[0066] Examples of basic groups having a cyclic structure include organic groups having an unsubstituted or substituted nitrogen-containing heterocyclic structure, such as a pyridyl group, a piperazinyl group, an N-methylpiperazinyl group, an N-ethylpiperazinyl group, an N-hydroxyethylpiperazinyl group, and a piperidyl group.
[0067] Examples of the basic group having a polyamine structure include a linear polyalkyleneamine structure containing only a tertiary amino group, a linear polyalkyleneamine structure containing at least a quaternary ammonium base, and a linear or branched polyalkyleneimine structure containing at least a primary amino group or a secondary amino group. Among these, a linear polyalkyleneamine structure containing only a tertiary amino group is preferred.
[0068] The (b-1) component preferably has a polymer chain having at least solvent affinity at a site other than the basic group. Examples of the solvent-philic polymer chain include polyether polymer chains, (meth)acrylic polymer chains, polyurethane polymer chains, polyester polymer chains, and polyamide polymer chains. Among them, from the viewpoint of low-voltage driving, polyether polymer chains and (meth)acrylic polymer chains are preferred, and it is more preferred that the (b-1) component contains both polymer chains. The term (meth)acrylic here means methacrylic or acrylic.
[0069] The weight average molecular weight (Mw) of the resin belonging to the component (b-1) is preferably from 1,000 to 25,000, and more preferably from 3,000 to 15,000, from the viewpoint of low voltage driving.
[0070] The base number of the resin belonging to the (b-1) component is preferably 3 to 100 (mgKOH / g), more preferably 10 to 50 (mgKOH / g), from the viewpoint of low-voltage driving. The base number (mgKOH / g) here refers to the weight (mg) of potassium hydroxide equivalent to hydrochloric acid required to neutralize 1 g of the (b-1) component. It can be measured by neutralizing 1 g of the (b-1) component with a hydrochloric acid solution and then titrating with a potassium hydroxide solution. In addition, the base number can also be calculated as the base equivalent (g / mol), which is the weight of the resin per 1 mol of basic group. The base number can be measured by potentiometric titration using an automatic potentiometric titrator (AT-510; manufactured by Kyoto Electronics Manufacturing Co., Ltd.) and using a 0.1 mol / L hydrochloric acid solution as a titration reagent and tetrahydrofuran as a titration solvent, based on "JIS K2501 (2003)". If the resin is poorly soluble in tetrahydrofuran, ethanol or 2-propanol may be used.
[0071] In order to control the value of X within the range of 55 to 125, the content of the component (b-1) is preferably 5 to 50% by weight, and more preferably 10 to 40% by weight, relative to 100% by weight of the component (a).
[0072] Examples of the resin having a linear polyalkyleneamine structure containing only a tertiary amino group and a polyether polymer chain include a resin obtained by grafting a polyether polymer chain to an aliphatic polyamine compound having a primary amino group and a secondary amino group. A resin having a structure represented by formula (9) can be preferably used to control the value of X to within the range of 55 to 125.
[0073] [ka]
[0074] In formula (9), the number of repeating units is n 1 is an integer from 1 to 9. 21 , R 22 each independently represents an alkylene group having 1 to 5 carbon atoms. * represents a bonding site with an alkylene oxide structure.
[0075] From the viewpoint of low-voltage driving, n 1 is preferably 1 to 5, and R 21 and R 22 are preferably methylene, ethylene or propylene groups. * is preferably a bonding site with an ethylene oxide structure or a propylene oxide structure. The polyether polymer chain preferably has a polyalkylene structure containing an ethylene oxide structure and a propylene oxide structure, and the terminal group is preferably a hydroxyl group. In formula (9), the polyalkylene oxide structure refers to a structure in which three or more alkylene oxide structures are linked together as repeating units.
[0076] A resin having a tertiary amino group and / or a quaternary ammonium salt group and having a (meth)acrylic polymer chain can also be preferably used to control the value of X within the range of 55-125.
[0077] As the structure of the resin, a (meth)acrylic block copolymer is desirable because it can enhance the adsorption efficiency of the particle component containing the (a) component by the continuous arrangement of the structural units having a basic group in the molecular structure and the narrowly controlled molecular weight distribution. The (meth)acrylic block copolymer referred to here is a (meth)acrylic copolymer in which a structure (A block) in which 10 or more structural units having a basic group are connected and a structure (B block) in which 10 or more structural units not having a basic group are connected are bonded. Examples of the (meth)acrylic block copolymer include (meth)acrylic copolymers such as AB diblock type, ABA triblock type, or BAB triblock type, which include an A block having a structural unit represented by formula (10) and a B block not having a structural unit represented by formula (10). Examples of the constituent units of the B block include structural units derived from copolymerization components such as (meth)acrylic esters and (meth)acrylamides not having a basic group. Methods for synthesizing (meth)acrylic block copolymers include, for example, ATRP (Atom transfer polymerization) and RAFT (Reversible addition fragmentation chain transfer polymerization) methods, the CFRP (Controlled free radical polymerization) method disclosed in WO 2006 / 074969, and living radical polymerization methods using organotellurium compounds.
[0078] [ka]
[0079] R 23 R represents a hydrogen atom or a methyl group. 24 R represents a divalent linking group having 1 to 5 carbon atoms. 25 and R 26 each independently represents an alkyl group having 1 to 5 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a benzyl group. * represents a bonding site with a carbon atom.
[0080] From the viewpoint of low voltage drive, R 24 is preferably a methylene group, an ethylene group or a propylene group, R 25 and R 26 are each independently preferably a methyl group, an ethyl group, or a propyl group. Most preferably, they are structures derived from N,N-dimethylaminoethyl (meth)acrylate or N,N-diethylaminoethyl (meth)acrylate.
[0081] When the component (a-1) contains at least one compound selected from the group consisting of compounds represented by formula (2), compounds represented by formula (3), and / or isomers thereof, and the photosensitizer (c) further contains a compound having two or more radically polymerizable groups in the molecule and a photopolymerization initiator, it is preferred that the resin (b) contains the component (b-1), the component (b-1) contains a (meth)acrylic block copolymer having a quaternary ammonium base, and the quaternary ammonium base has a structure consisting of a salt of a quaternary ammonium cation and a carbon atom-containing counter anion. It is more preferable that the copolymer contains a structure consisting of a salt of a quaternary ammonium cation and a counter anion containing a carbon atom, and does not contain a structure consisting of a salt of a quaternary ammonium cation and a counter anion containing a chlorine atom. As a specific example, it is more preferable that the copolymer contains a (meth)acrylic block copolymer having a structural unit represented by formula (11).
[0082] As a method for synthesizing a (meth)acrylic block copolymer having a structural unit represented by formula (11), for example, a method of quaternizing the tertiary amino groups of a (meth)acrylic block copolymer having a structural unit represented by the above formula (10) can be mentioned, and all of the tertiary amino groups may be quaternized, or a part of them may be quaternized. The quaternization reaction may be directly carried out by heating in the coexistence of an organic acid, a glycidyl ether, and an organic solvent, which are the desired counter anion sources, or may be first converted into a quaternary ammonium base containing a halogen anion and then subjected to anion exchange.
[0083] [ka]
[0084] R 27 R represents a hydrogen atom or a methyl group. 28 R represents a divalent linking group having 1 to 5 carbon atoms. 29 ~R 31 each independently represents an alkyl group having 1 to 5 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a benzyl group. - represents a carbon atom-containing counter anion. * represents a bond site with a carbon atom.
[0085] From the viewpoint of low voltage drive, R 28 is preferably a methylene group, an ethylene group or a propylene group, R 29 ~R 31 are each independently preferably a methyl group, an ethyl group, a propyl group or a benzyl group. - Examples of the carboxylate anion include a carboxylate anion and an aromatic sulfonate anion, with a carboxylate anion being preferred. Examples of the carboxylate anion include an acetate anion, a lactate anion, a benzenecarboxylate anion, a naphthalenecarboxylate anion, and a p-styrenecarboxylate anion.
[0086] As the (meth)acrylic block copolymer having a quaternary ammonium base consisting of a salt of a quaternary ammonium cation and a carbon atom-containing counter anion, a commercially available product may be used, and examples thereof include "DISPERBYK" (registered trademark)-2013 and 2025.
[0087] The component (b-2) refers to a resin that has an alkali-soluble group, an acid value of 5 (mgKOH / g) or more, does not have the above-mentioned basic group, and has a weight average molecular weight (Mw) of 1000 to 150000. The alkali-soluble group refers to a hydroxyl group, a carboxyl group, a phosphate group, and a sulfo group. The presence of an alkali-soluble group increases the solubility in a developer, making it easier to selectively remove the unexposed areas in negative photolithography and the exposed areas in positive photolithography, resulting in good patterning properties of the pixel division layer.
[0088] The acid value is the weight (mg) of potassium hydroxide required to neutralize 1g of resin, and can be measured by titrating 1g of resin with a potassium hydroxide solution. The acid value can also be used to calculate the acid equivalent (g / mol), which is the weight of resin per 1mol of acidic groups.
[0089] The acid value can be measured by potentiometric titration using an automatic potentiometric titrator (AT-510; manufactured by Kyoto Electronics Manufacturing Co., Ltd.) with a 0.1 mol / L potassium hydroxide solution as a titration reagent and tetrahydrofuran as a titration solvent in accordance with JIS K2501 (2003). If the resin has poor solubility in tetrahydrofuran, ethanol, 2-propanol or dimethylformamide may be used.
[0090] Examples of the (b-2) component include an alkali-soluble maleimide resin, an alkali-soluble (meth)acrylic resin, an alkali-soluble polyimide resin, an alkali-soluble polyimide precursor, an alkali-soluble polybenzoxazole resin, an alkali-soluble polybenzoxazole precursor, an alkali-soluble cardo resin, an alkali-soluble epoxy (meth)acrylate resin, an alkali-soluble polysiloxane resin, an alkali-soluble novolac resin, an alkali-soluble polyurethane resin, an alkali-soluble polyester resin, and an alkali-soluble polyether resin. Among these, from the viewpoint of low-voltage driving, an alkali-soluble maleimide resin, an alkali-soluble (meth)acrylic resin, an alkali-soluble polyimide resin, an alkali-soluble polyimide precursor, and an alkali-soluble cardo resin are preferred, and it is more preferred to use an alkali-soluble maleimide resin and an alkali-soluble (meth)acrylic resin in combination. In addition, when a resin has a structural unit derived from maleimide, it is defined as belonging to the alkali-soluble maleimide resin even if it has a structural unit derived from a copolymerization component other than maleimide.
[0091] The alkali-soluble polyimide precursor refers to an alkali-soluble resin from which a polyimide resin can be obtained by heat treatment in the curing step described below, and specifically refers to an alkali-soluble polyamic acid or an alkali-soluble polyamic acid ester.
[0092] An alkali-soluble cardo resin is an alkali-soluble resin having a cardo skeleton. A cardo skeleton is a skeleton in which two aromatic groups are connected by single bonds to a quaternary carbon atom, which is a ring carbon atom that constitutes a ring structure such as a fluorene skeleton.
[0093] The weight average molecular weight (Mw) of the resin belonging to the component (b-2) is preferably from 2,000 to 50,000, and more preferably from 3,000 to 30,000, from the viewpoint of low voltage driving.
[0094] The acid value of the resin belonging to the component (b-2) is preferably from 30 to 300 (mgKOH / g), and more preferably from 50 to 200 (mgKOH / g), from the viewpoint of low-voltage driving.
[0095] When the photosensitive composition is a negative photosensitive composition, from the viewpoint of low voltage driving, it is preferable that the component (b-2) contains at least one resin selected from the group consisting of a resin having a structure represented by formula (12), a resin having a structure represented by formula (13), a resin having a structure represented by formula (14), and a resin having a structure represented by formula (15). When the component (b-2) contains a resin having a structure represented by formula (13) or a resin having a structure represented by formula (14), R 40 and R 41 It is particularly desirable for the ring structure to be derived from tetrahydrophthalic anhydride.
[0096] [ka]
[0097] In formula (12), R 32 and R 33 , R 35 and R 36 R each independently represents a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms. 34 and R 37 each independently represents a monovalent organic group having 1 to 16 carbon atoms. * represents a bonding site with a carbon atom.
[0098] [ka]
[0099] In formula (13), R 38 and R 39 R each independently represents a hydrogen atom or a methyl group. 40 represents a divalent organic group having 2 to 6 carbon atoms. * represents a bonding site with a carbon atom.
[0100] [ka]
[0101] In formula (14), R 42and R 43 R each independently represents a hydrogen atom or a methyl group. 41 represents a divalent organic group having 2 to 6 carbon atoms. * represents a bonding site.
[0102] [ka]
[0103] In formula (15), R 44 represents a hydrogen atom or a methyl group. * represents the bonding site with a carbon atom.
[0104] Among them, it is more preferable that the component (b-2) contains a resin having a structure represented by formula (12). From the viewpoint of low-voltage driving, R 32 , R 33 , R 35 and R 36 is preferably a hydrogen atom, and R 34 and R 37 is preferably a monovalent organic group having 6 to 16 carbon atoms and a cyclic structure which may have a substituent. That is, it is more preferable to contain a resin having a structure represented by formula (16).
[0105] [ka]
[0106] In formula (16), R 45 and R 46 R each independently represents a direct bond or a divalent linking group having 1 to 4 carbon atoms. 47 and R 48 Each of n independently represents a monovalent organic group having one ethylenically unsaturated double bond or a carboxyl group. 1 and n 2 represents an integer, each independently being 0 to 3. 45 and (R 47 )n 2 The total number of carbon atoms contained in 46 and (R 48 )n 3The total number of carbon atoms contained in each of these independently is 0 to 10.
[0107] The resin having the structure represented by formula (16) can be derived from a maleimide compound such as N-phenylmaleimide, N-benzylmaleimide, N-cyclohexylmaleimide, N-carboxyphenylmaleimide, N-dicarboxymaleimide, N-carboxycyclohexylmethylmaleimide, etc. In addition, preferred examples of the monovalent organic group having one ethylenically unsaturated double bond include an organic group obtained by addition reaction of a glycidyl group of glycidyl (meth)acrylate with a carboxyl group derived from N-carboxyphenylmaleimide.
[0108] The resin having the structure represented by formula (12) and the resin having the structure represented by formula (16) are preferably copolymers of an N-substituted maleimide compound and a compound having one ethylenically unsaturated double bond in the molecule. Examples of the synthesis method include a method of heating in a solvent in the presence of a thermal polymerization initiator and a molecular weight regulator. From the viewpoint of low-voltage operation and developability, it is more preferable that the structural unit derived from the N-substituted maleimide compound is 15 to 50 mol %.
[0109] Examples of compounds having one ethylenically unsaturated double bond in the molecule include benzyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, methyl (meth)acrylate, n-butyl (meth)acrylate, ethyl (meth)acrylate, polyethylene glycol (meth)acrylate, isobornyl acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, (meth)acrylic acid, and styrene. Examples of molecular weight regulators include 1,1-diphenylethylene, n-octyl mercaptan, and n-dodecyl mercaptan.
[0110] When the dye-type dispersion aid (e) contains a compound having an alkali-soluble group and an aromatic tetracarboxylic acid bisimide skeleton or a salt thereof, it is preferable that the resin (b) contains an alkali-soluble resin (b-2) and the component (b-2) contains an alkali-soluble polyimide precursor from the viewpoint of low-voltage driving. An example of the alkali-soluble polyimide precursor is a resin having a structure represented by formula (17). A specific example is an alkali-soluble polyimide precursor in which an alkali-soluble group is partially esterified, as described in JP-A-2002-278061.
[0111] [ka]
[0112] In formula (17), R 49 and R 50 R represents a divalent to octavalent organic group. 51 and R 52 represents a hydroxyl group or -COOM, and each may be a single group or different groups may be mixed. M represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms. r represents an integer of 2 to 6. s represents an integer of 0 to 6. However, R 51 is a hydroxyl group, R 49 has an aromatic ring, and R 52 is a hydroxyl group, R 50 has an aromatic ring. R 49 -(R 51 )r represents a residue of an acid dianhydride. 49 is preferably an organic group having 5 to 50 carbon atoms and having an aromatic ring or a cyclic aliphatic group. R 50 -(R 52 )s represents a diamine residue. 50 is preferably an organic group having 5 to 40 carbon atoms and having an aromatic ring or a cyclic aliphatic group.
[0113] The photosensitive composition of the present invention contains a photosensitizer (c). Hereinafter, this may be referred to as component (c). Component (c) is also an effective component for controlling the value of X in formula (1), and it is particularly desirable that the component (c) does not inhibit the interaction between the particle component and component (b).
[0114] When the photosensitive composition is a negative photosensitive composition, the (c) photosensitizer contains (c-1) a compound having two or more radical polymerizable groups in the molecule and a photopolymerization initiator. Hereinafter, this may be referred to as component (c-1). From the viewpoint of low-voltage driving, the photosensitive composition of the present invention contains at least one compound selected from the group consisting of the compound represented by formula (2), the compound represented by formula (3) and their isomers, and further, it is preferable that the (c) photosensitizer contains a compound having two or more radical polymerizable groups in the molecule and a photopolymerization initiator.
[0115] On the other hand, when the photosensitive composition is a positive photosensitive composition, the (c) photosensitizer contains a (c-2) quinone diazide compound. Hereinafter, this may be referred to as component (c-2). From the viewpoint of low-voltage driving, the photosensitive composition of the present invention preferably contains a compound represented by formula (5) and / or a compound represented by formula (6), and further, the (c) photosensitizer preferably contains a quinone diazide compound.
[0116] The inclusion of component (c-1) gives the compound the ability to undergo photocuring through a radical polymerization reaction upon exposure to active actinic rays such as ultraviolet light, thereby forming a negative pattern in which the exposed areas become insoluble in a developer.
[0117] Examples of the radically polymerizable group include a vinyl group and a (meth)acrylic group, with a (meth)acrylic group being preferred in terms of excellent photocurability. The (meth)acrylic group refers to a methacryl group or an acrylic group.
[0118] As the compound belonging to component (c-1) having two or more radically polymerizable groups in the molecule, it is preferable to contain a combination of a pentafunctional or hexafunctional (meth)acrylate compound and a bifunctional (meth)acrylate compound in order to obtain high photocurability and improve the processing margin in the development step described below, and to prevent electrode breakage by making the pattern edge of the pixel division layer have a low taper shape.
[0119] Examples of the pentafunctional or hexafunctional (meth)acrylate compound include ε-caprolactone-modified hexafunctional acrylates “KAYARAD” (registered trademark) DPCA-20, DPCA-30, DPCA-60, and DPCA-120 (all manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0120] Examples of bifunctional (meth)acrylate compounds include "KAYARAD" (registered trademark) HX-220 (hereinafter referred to as "HX-220"), HX-620 (both manufactured by Nippon Kayaku Co., Ltd.), and fluorene-based (meth)acrylates. Among them, the compound represented by formula (18) is preferred.
[0121] [ka]
[0122] In formula (18), R 53 and R 54 R each independently represents an organic group represented by formula (19) or a hydroxyl group. 55 and R 56 Each independently represents a hydrogen atom or a methyl group. 1 and t 2 each independently represents an integer of 0 to 2.
[0123] [ka]
[0124] An example of a commercially available product of the compound represented by formula (18) is “OGSOL” (registered trademark) EA-0250P (manufactured by Osaka Gas Chemicals Co., Ltd.; hereinafter, “EA-0250P”), which is a PGMEA solution containing 50% by weight of the compound represented by formula (20).
[0125] [ka]
[0126] In formula (19), * represents a binding site.
[0127] The content of the compound having two or more radical polymerizable groups in its molecule is preferably 15 to 50% by weight, with the total amount of the compound having two or more radical polymerizable groups in its molecule and the aforementioned (b-2) component being 100% by weight.
[0128] Examples of the photopolymerization initiator include oxime ester-based photopolymerization initiators, alkylphenone-based photopolymerization initiators, and acylphosphine oxide-based photopolymerization initiators. Among these, from the viewpoint of low-voltage driving, oxime ester-based photopolymerization initiators are preferred because they have excellent photocuring properties in the deep parts of the film.
[0129] Examples of the oxime ester photopolymerization initiator include a compound represented by formula (21), a compound represented by formula (22), "ADEKA CRUISE" (registered trademark) NCI-831E (manufactured by ADEKA CORPORATION, hereinafter referred to as "NCI-831E"), a compound described in JP2008 / 100955A, a compound described in WO2006 / 018405A, and "Irgacure" (registered trademark) OXE03 (all manufactured by BASF, hereinafter referred to as "OXE03").
[0130] [ka]
[0131] [ka]
[0132] The content of the photopolymerization initiator is preferably 1 to 10% by weight based on 100% by weight of the total solid content in the photosensitive composition, from the viewpoint of achieving both a tapered shape of the pattern edge and low-voltage driving.
[0133] The component (c-2) is exposed to active actinic rays such as ultraviolet light in the exposure step and is converted into a compound having an alkali-soluble group. This component relatively increases the dissolution rate of the film in the exposed areas compared to the unexposed areas, thereby enabling patterning of the pixel division layer by positive photolithography.
[0134] As the component (c-2), a naphthoquinone diazide compound is preferred, and a reaction product of esterifying a compound having a phenolic hydroxyl group with naphthoquinone diazide sulfonyl chloride is more preferred.
[0135] The photosensitive composition of the present invention contains a solvent (d). The solvent (d) here includes water. The component (d) is an essential component for controlling the value of X in formula (1) within the range of 55 to 125, and it is desirable to contain an organic solvent because of its excellent dissolving power for the component (b). In addition, when the photosensitive composition contains the component (b), particularly the component (b-1), while at least a part of the component (a) is directly adsorbed to the particle component, it is preferable to select an organic solvent that does not prevent the component (b-1) from being adsorbed to the particle component.
[0136] As the (d) solvent, from the viewpoint of the dissolving power of the above-mentioned (b) component, ether-based solvents, acetate-based solvents, cyclic ester-based solvents, and alcohol-based solvents can be preferably used, and the value of X in formula (1) can be controlled by using one or more of them in combination.
[0137] Examples of ether-based solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether (hereinafter, "PGME"), propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, and dipropylene glycol monoethyl ether.
[0138] Examples of acetate-based solvents include propylene glycol monomethyl ether acetate (hereinafter, "PGMEA"), 3-methoxybutyl acetate (hereinafter, "MBA"), butyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, and diethylene glycol monoethyl ether acetate.
[0139] Examples of cyclic ester solvents include β-propiolactone, γ-butyrolactone (hereinafter, “γ-BL”), γ-valerolactone, δ-valerolactone, γ-caprolactone, and ε-caprolactone.
[0140] An example of the alcohol-based solvent is 3-methoxy-1-butanol (hereinafter, "MB").
[0141] The photosensitive composition of the present invention preferably further contains a dye-type dispersion aid (e). Hereinafter, this may be referred to as component (e). Component (e) adsorbs to the pigment surface of component (a) to provide a suitable charge, and has the effect of mainly enhancing the interaction with component (b). Note that component (e) does not belong to the particle component.
[0142] The component (e) is preferably a dye having an alkali-soluble group or a salt thereof, such as a perylene dye, a perinone dye, a cyanine dye, a phthalocyanine dye, an azo dye, an azomethine dye, an anthraquinone dye, a quinacridone dye, a dioxazine dye, a xanthene dye, a triarylmethane dye, or a quinophthalone dye. The alkali-soluble group here refers to a hydroxyl group, a carboxyl group, or a sulfo group, as described above.
[0143] When the component (a-2) contains a compound represented by formula (5) and / or a compound represented by formula (6), and the photosensitizer (c) further contains a quinone diazide compound, the dye-type dispersing aid (e) preferably contains a compound having an alkali-soluble group and an aromatic tetracarboxylic acid bisimide skeleton, or a salt thereof, in order to control the value of X in formula (1) within the range of 55 to 125. It is more preferable that the dye-type dispersing aid contains a compound having two or more sulfo groups or carboxyl groups in the molecule and having an aromatic tetracarboxylic acid bisimide skeleton, or a salt thereof.
[0144] When the photosensitive composition contains the (e) component, it is preferable to contain a cyclic ester solvent as the (d) component from the viewpoint of low voltage driving. As the aromatic tetracarboxylic acid bisimide skeleton, for example, a perylene tetracarboxylic acid bisimide skeleton and a naphthalene tetracarboxylic acid bisimide skeleton are preferably mentioned. Among them, it is more preferable to contain a compound having a perylene tetracarboxylic acid bisimide skeleton. Specific examples of the (e) component include sulfonic acid derivatives obtained by sulfonating organic pigments having a perylene tetracarboxylic acid bisimide skeleton such as CI Pigment Red 149, 178, 179, CI Pigment Violet 29, and CI Pigment Black 31 and 32, and they can be preferably used in combination with the above-mentioned alkali-soluble polyimide precursor.
[0145] The photosensitive composition may further contain a thermal crosslinking agent regardless of whether it is negative type or positive type. By containing a thermal crosslinking agent, it is possible to improve the film strength and heat resistance of the pixel division layer finally obtained by thermal crosslinking in the curing process. Examples of the thermal crosslinking agent include compounds having two or more epoxy groups.
[0146] Examples of compounds having two or more epoxy groups include TR-FR-201 (manufactured by Tronly), "TECHMORE" (registered trademark) VG-3101L (manufactured by Printec Co., Ltd., hereinafter referred to as "VG-3101L"), and "TEPIC" (registered trademark) S, G, P, and L (all manufactured by Nissan Chemical Industries, Ltd.).
[0147] The photosensitive composition may further contain other components such as a surfactant, a leveling agent, an antioxidant, and an ultraviolet absorbing agent.
[0148] The photosensitive composition of the present invention may be prepared, for example, by mixing the components (a), (b) and (d) to prepare a pigment dispersion by wet dispersion treatment, and then adding the component (c) and other components to the pigment dispersion and stirring the mixture, and filtering the mixture through a filter as necessary.
[0149] The dispersing machine for performing the wet dispersion process may be a wet media dispersing machine or a wet media-less dispersing machine, but it is preferable to use a wet media dispersing machine because of its excellent dispersion process efficiency. Examples of the wet media dispersing machine include bead mills such as "Levomill" (registered trademark) (manufactured by Asada Iron Works), "Nano-Getter" (registered trademark) (manufactured by Ashizawa Finetech), "DYNO-MILL" (registered trademark) (manufactured by Willy A. Bachofen), "Spike Mill" (registered trademark) (manufactured by Inoue Seisakusho Co., Ltd.), "Sand Grinder" (registered trademark) (manufactured by DuPont), "Ultra Apex Mill Advance" (registered trademark) (manufactured by Hiroshima Metal & Machinery Co., Ltd.), and "NEO-Alpha Mill" (registered trademark) (manufactured by AIMEX Co., Ltd.).
[0150] Examples of media for the disperser include zirconia beads and zircon beads. The bead diameter is preferably 0.03 to 5 mmφ, and the higher the sphericity, the more preferable. Specific examples of commercially available products include "TORECERAM" (registered trademark) (manufactured by Toray Industries, Inc.) and "YTZ" (registered trademark) (manufactured by Nikkato Corporation). It is particularly preferable to use beads in the range of 0.03 to 0.5 mmφ, and the bead filling rate in the disperser vessel is preferably 70 to 90% by volume.
[0151] There are no particular limitations on the dispersion conditions, but when using a wet media disperser, it is desirable to input the necessary and sufficient mechanical energy according to the vessel diameter and agitator shape. Agitator shapes include disk type and pin type. The amount of mechanical energy input is determined by the shear force and dispersion processing time. The shear force is determined by a complex combination of various parameters, including the specific gravity and diameter of the beads, the filling rate in the vessel, the viscosity of the pigment dispersion, and the peripheral speed (m / s) of the agitator in the disperser.
[0152] The value of X in formula (1) is preferably controlled by setting a plurality of dispersion conditions at two or more stages. In controlling the value of X to be within the range of 55 to 125, it is desirable to increase the peripheral speed stepwise from the initial dispersion stage to the end of dispersion stage in order to achieve both the progress of micronization and the suppression of re-agglomeration. If necessary, the (b) component and / or the (d) component may be added in multiple stages during the process of wet media dispersion treatment.
[0153] When the value of X in formula (1) is controlled to be the same, the photosensitive composition of the present invention preferably has a maximum cumulative particle diameter Dmax in the particle size distribution of the particle components based on the light scattering intensity measured by dynamic light scattering method of 150 to 350 nm, more preferably 170 to 250 nm. The maximum cumulative particle diameter Dmax here refers to a value measured on a sample for measuring the maximum cumulative particle diameter Dmax. The sample for measuring the maximum cumulative particle diameter Dmax refers to a measurement object obtained by mixing the photosensitive composition with an equal amount of dilution solvent in three separate times so that the photosensitive composition / dilution solvent = 1 / 99 (weight ratio) and stirring on a shaker for 10 minutes. The dilution solvent is the same solvent as the (d) solvent contained in the photosensitive composition.
[0154] The particle size distribution referred to here can be measured using a dynamic light scattering particle size distribution measuring device "SZ-100 (manufactured by Horiba, Ltd.)" and refers to the particle size distribution based on the light scattering intensity relative to a light source.
[0155] The maximum cumulative particle diameter Dmax means a particle diameter corresponding to 99% of the cumulative particle size distribution curve, accumulating from the small particle diameter side to the large particle diameter side, and is essentially a value calculated as the 99% cumulative diameter (D99). The maximum cumulative particle diameter Dmax here is based on light scattering intensity, and is an index that is completely different from the relationship with the cumulant average diameter in the dynamic light scattering method described in JP 2019-160473 A. In addition, in the dynamic light scattering method, when a photosensitive composition containing a pigment dispersion liquid produced by a so-called breakdown method in which a pigment such as component (a) is finely divided from a large particle diameter to a small particle diameter using a wet disperser is measured, the 99% cumulative diameter (D99) calculated based on the light scattering intensity is larger than the 99% cumulative diameter (D99) calculated based on the volume, and is even larger than the 99% cumulative diameter (D99) calculated based on the number.
[0156] The cured product of the present invention is a cured product obtained by curing a photosensitive composition. The cured product can be used, for example, as a pixel dividing layer of an organic EL display device, a TFT flattening layer, a black matrix of a liquid crystal display device, a black column spacer, a near-infrared highly transparent black film of a solid-state imaging device, a near-infrared highly transparent black film for a bezel of a touch panel, and the like, and the application is not particularly limited. The cured product means a product obtained through a process of heating a photosensitive composition at a temperature of 200°C or more and 400°C or less under atmospheric pressure for 10 minutes or more.
[0157] As a specific example of a method for obtaining a cured product of the photosensitive composition of the present invention, a method for forming a pixel division layer will be described below. The pixel division layer can be obtained, for example, by a known photolithography method including a coating step, a pre-bake step, an exposure step, a development step, and a curing step in this order.
[0158] The optical density of the pixel division layer per 1.0 μm of film thickness is preferably 0.5 or more, more preferably 0.7 or more, in order to suppress reflection of external light and enhance the value of the display device, and is preferably 1.5 or less, more preferably 1.3 or less, in order to achieve low voltage driving.
[0159] The optical density means a value obtained by measuring the incident light intensity and transmitted light intensity of a pixel division layer formed on a transparent substrate to a thickness of 1.5 μm using an optical densitometer (X-Rite 361T, manufactured by X-Rite Corporation) and calculating the value from the following formula, and dividing the result by the film thickness value of 1.5. The higher the optical density, the higher the light blocking property. As the transparent substrate, a transparent glass substrate "Tempax (manufactured by AGC Technoglass Co., Ltd.)" can be preferably used.
[0160] Optical density = log 10 (I0 / I) I0: Incident light intensity I: transmitted light intensity The organic EL display device of the present invention is an organic EL display device comprising the above-mentioned cured product. In the organic EL display device, the cured product is preferably contained in a pixel dividing layer and a TFT planarizing layer. EXAMPLES
[0161] The present invention will be described in detail below with reference to examples and comparative examples, but the aspects of the present invention are not limited to these. First, the evaluation methods used in the examples and comparative examples will be described. <Calculating the minimum required exposure> ITO was formed on the entire surface of a 150 mm x 150 mm alkali-free glass substrate by sputtering, and low-temperature annealing was performed at 150 ° C for 30 minutes in a dry nitrogen atmosphere to obtain a substrate with an ITO film having a thickness of 10 nm. The photosensitive composition of the example or comparative example was applied to the surface of the ITO film by a spin coater, adjusting the rotation speed so that the thickness of the final cured film was 1.5 μm, to obtain a coating film. In the case of a negative photosensitive composition, the coating film was prebaked at 100 ° C for 2 minutes under atmospheric pressure using a hot plate (SCW-636; manufactured by Dai Nippon Screen Mfg. Co., Ltd.), to obtain a prebaked film-formed substrate, which was then cut into two pieces. The minimum required development time was determined as the time elapsed from the time when one of the prebaked film-formed substrates was immersed in a tray containing a 2.38 wt % TMAH aqueous solution to dissolve the prebaked film until the substrate surface was visually observed.
[0162] Furthermore, the other prebaked film-formed substrate was used to perform patterning exposure with g, h, and i mixed rays of an ultra-high pressure mercury lamp through a sensitivity measurement grayscale mask (MDRM MODEL 4000-5-FS; Opto-Line International) in a double-sided alignment single-sided exposure device (Mask Aligner PEM-6M; Union Optical Co., Ltd.), to obtain an exposed film. Next, using a small photolithography developing device (AD-2000; Takizawa Sangyo Co., Ltd.), the substrate was developed by paddle method using a 2.38 wt% TMAH aqueous solution for 1.5 times the development time required for the above-mentioned minimum development time. Furthermore, the substrate was rinsed by shower method for 30 seconds with deionized water, and then the substrate was rotated at 200 rpm for 30 seconds to dry, to obtain a developed film-formed substrate having a patterned developed film.
[0163] Next, the resolution pattern of the developed film was observed using an FPD inspection microscope (MX-61L; Olympus Corporation), and the exposure dose (mJ / cm) required to open the developed film was determined so that the mask bias was −2 μm for the opening dimension of the line and space pattern, which was 40 μm wide (opening dimension of the developed film: 38 μm, pattern line width: 42 μm). 2 (i-line equivalent value) was defined as the minimum required exposure amount (exposure sensitivity) of the negative photosensitive composition.
[0164] On the other hand, the minimum required exposure dose of the positive photosensitive composition was determined in the same manner as in the case of the negative photosensitive composition described above, except that the pre-bake temperature of the coating film was set to 120°C, the paddle development time was set to 90 seconds, and the mask bias was set to 0 μm (opening dimension of the developed film: 40 μm, pattern line width: 40 μm).
[0165] (1) Evaluation of the optical density (OD / μm) of the cured film For the optical density evaluation substrates obtained in Examples 1 to 9 and Comparative Examples 1 to 6, in which a 1.5 μm-thick cured film was formed on the surface of a transparent glass substrate "Tempax" (manufactured by AGC Technoglass Co., Ltd.), the total optical density (Total OD value) was measured at three points on the film surface side using an optical densitometer (manufactured by X-Rite Corporation; X-Rite 361T) to calculate the average value, and the value was divided by 1.5, rounded off to one decimal place to obtain the OD value per 1.0 μm of cured film thickness (OD / μm).
[0166] The evaluation was based on the criterion that the higher the OD / μm, the better the light-shielding properties of the cured film. The OD value of Tempax without a cured film was measured separately and found to be 0.00, so the OD value of the substrate for optical density evaluation was considered to be the OD value of the cured film. The thickness of the cured film was measured at three locations on the surface using a stylus film thickness measuring device (Tokyo Seimitsu Co., Ltd.; Surfcom), and the average value was rounded off to one decimal place to obtain a value up to one decimal place.
[0167] (2) Evaluation of maximum cumulative particle size Dmax in particle size distribution The particle size distribution of the photosensitive compositions of Examples 1 to 9 and Comparative Examples 1 to 6 was measured by the following method, and the maximum cumulative particle diameter Dmax was calculated. Since the dynamic light scattering method uses the Brownian motion of particle components as a data source, it is difficult in principle to obtain a sufficiently high measurement accuracy as an absolute value for samples with Dmax exceeding 500 nm, that is, samples containing coarse particles. Therefore, samples with Dmax exceeding 500 nm were marked as ">500 nm" in the table and were rejected regardless of the results.
[0168] <How to prepare samples for measuring maximum cumulative particle size Dmax> The dilution solvent was mixed in equal amounts in three batches so that the photosensitive composition / dilution solvent ratio was 1 / 99 (weight ratio), and the mixture was stirred on a shaker for 10 minutes. The dilution solvent used was the same as the (d) solvent contained in the photosensitive composition.
[0169] <Measuring method for maximum cumulative particle size Dmax> Measurement equipment: Dynamic light scattering particle size distribution measurement equipment "SZ-100 (manufactured by Horiba, Ltd.)" Light source: Wavelength 532nm / 10mW (semiconductor pumped solid-state laser) Temperature of sample liquid: 25±1℃ (atmospheric pressure) Calculation method: The cumulative 99% diameter was determined based on the light scattering intensity, and the average value of three measurements was calculated. The value was rounded off to the first decimal place to obtain the maximum cumulative particle diameter Dmax.
[0170] (3) Calculate the value of X in formula (1) For the photosensitive compositions of Examples 1 to 9 and Comparative Examples 1 to 6, the relaxation time T2 was measured under the following conditions, and the value of T2 was divided by the value of A and rounded off to the first decimal place to calculate the value of X. X = T2 / A (1) In formula (1), T2 is the measurement nucleus for the T2 measurement sample. 1 The spin-spin relaxation time (ms) measured by the Carr-Purcell-Meiboom-Gill method using a H pulsed nuclear magnetic resonance spectrometer is shown as the average value of three measurements. A represents the content (wt%) of all components in the T2 measurement sample excluding the particle component and the solvent component, and is 6.50 to 8.80.
[0171] <Preparation method of T2 measurement sample> Add the same solvent as the (d) solvent contained in the photosensitive composition so that the solid content becomes 10.00 wt%, seal it, and stir on a shaker for 10 minutes.
[0172] <T2 measurement conditions> Measuring device: Pulse nuclear magnetic resonance device “BRUKER” (registered trademark) minispec mp20 manufactured by Bruker BioSpin Measuring nucleus: 1 H Frequency of the measuring nucleus: 19.95 MHz Pulse width: 2.18 μs (90° pulse) Pulse repetition time: 10 seconds Container for filling the T2 measurement sample: 10 mmφ NMR sample tube Liquid temperature of the T2 measurement sample: Constant at 25.0 °C by temperature control function (under atmospheric pressure) Operation before measurement: Leave it in the probe for 20 minutes to stabilize the liquid temperature of the measurement sample. Calculation method of T2: For the T2 measurement sample, the measuring nucleus 1 The average value was calculated when the spin-spin relaxation time (ms) measured by the Carr-Purcell-Meiboom-Gill method using a pulse nuclear magnetic resonance device for H was measured 3 times, and the first decimal place was rounded off.
[0173] (4) Evaluation of the driving voltage of the organic EL display device The organic EL display devices obtained in Examples 1 to 9 and Comparative Examples 1 to 6 were caused to emit light while changing the driving voltage from a lower limit of 2.0 V to an upper limit of 8.0 V. All the organic EL display devices used for the evaluation were of the bottom emission type, and the alkali-free glass substrate 11 in FIG. 2 was on the light extraction side. The luminance of the green light emitted from 220 light-emitting pixels was measured using a spectro-radiance meter (CS-1000A manufactured by Konica Minolta) and converted to a value per unit area, 6000 (cd / m2 The driving voltage at which a luminance of 1000 nm was obtained was measured.
[0174] Note that "per unit area" here means per unit area of the light-emitting pixel portion, and the area of the pixel dividing layer formation portion is not included in the above conversion. The driving voltage was calculated by rounding off the first decimal place. Evaluation was based on the following criteria, with AA and A to C being pass, and D to E being fail. AA: The driving voltage is less than 4.0V. A: The driving voltage is 4.0V or more and less than 4.5V. B: The driving voltage is 4.5V or more and less than 5.0V. C: The driving voltage is 5.0V or more and less than 5.5V. D: The driving voltage is 5.5V or more and less than 6.0V. E: The driving voltage is 6.0 V or more.
[0175] The following provides information on the chemical structures, solid contents, etc. of the various raw materials used in the examples and comparative examples. "Benzodifuranon-based black pigment 1": "Irgaphor" (registered trademark) Black S0100CF. Corresponding to the compound represented by formula (4). "Perylene-based black pigment 1": an isomer mixture (weight ratio 1:1) of the compound represented by formula (7) and the compound represented by formula (8). It corresponds to a perylene-based black pigment having a benzimidazole skeleton. The specific surface area measured by the BET method is 50 m 2 / g. "Basic group-containing resin 1": a compound represented by formula (23) (n 1 is 1 and R 21 and R 22 is an ethylene group, and * is the linking site to the ethylene oxide structure. Solid content 100% by weight.
[0176] [ka]
[0177] "DISPERBYK-2013": A (meth)acrylic block copolymer having a quaternary ammonium base consisting of a salt of a quaternary ammonium cation and a counter anion containing a carbon atom, and having no quaternary ammonium base consisting of a salt of a quaternary ammonium cation and a counter anion containing a chlorine atom. The solid content is 97% by weight, with an acid value of 7 mgKOH / g and a base value of 18 mgKOH / g. "BYK-LPN21116": A PGMEA solution of a resin having a structural unit represented by formula (24), a structural unit represented by formula (25), and a structural unit represented by formula (26). Solid content: 40% by weight. The acid value of the solid content excluding the solvent is 1 mg KOH / g or less, and the base value is 70 mg KOH / g. It does not have a quaternary ammonium base consisting of a salt of a quaternary ammonium cation and a carbon atom-containing counter anion.
[0178] [ka]
[0179] [ka]
[0180] [ka]
[0181] "ZCR-1569H": PGMEA solution of alkali-soluble epoxy (meth)acrylate resin (manufactured by Nippon Kayaku Co., Ltd.: acid value of solids excluding solvent: 98 mg KOH / g, weight average molecular weight: 3900, solids: 70% by weight). "SPC-3410": In formula (13), R 38 is a methyl group, and R 39 is a hydrogen atom, and R 40A PGMEA solution of an alkali-soluble (meth)acrylic resin having a structural unit derived from tetrahydrophthalic anhydride. A solution of a resin having a structure in which hydroxyl groups of structural units of a copolymer consisting of structural unit 1 derived from styrene and structural unit 3 derived from tricyclodecanyl methacrylate (=60 / 10 / 30 mol%) obtained by reacting acrylic acid with the glycidyl group of the structural unit derived from glycidyl methacrylate, further undergoes ring-opening addition reaction with 36 mol% of carboxyl groups derived from tetrahydrophthalic anhydride (Showa Denko K.K.: solid content 42% by weight, weight average molecular weight (Mw) 7300, solid acid value 75 mgKOH / g).
[0182] "Solsperse 41000": an alkali-soluble polyether resin that does not have a basic group but has a phosphate group (manufactured by Lubrizol Corporation, solid content 100% by weight). "Surfactant solution 1": PGMEA solution of Megafac F-559 (DIC Corporation). Solid content: 1% by weight. "Additive solution 1": PGMEA solution of "KAYAMER" (registered trademark) PM-21 (manufactured by Nippon Kayaku Co., Ltd.). Solid content: 10% by weight. "Dye-type dispersing aid 1": CI Basic Blue 140. It is a copper phthalocyanine sulfonamide dye having three N,N-dimethylaminopropyl groups in the molecule. "Dye-type dispersing agent 2": a compound represented by formula (27) (integer n 2 (= a mixture of 2 to 4). It corresponds to a compound having two or more alkali-soluble groups in the molecule and having an aromatic tetracarboxylic acid bisimide skeleton.
[0183] [ka]
[0184] "Solsperse 22000": an azo dye having a sulfo group and no aromatic tetracarboxylic acid bisimide skeleton. "Solsperse 12000S": A copper phthalocyanine dye that has a sulfo group and does not have an aromatic tetracarboxylic acid bisimide skeleton.
[0185] (Synthesis Example 1: Synthesis of "Alkali-soluble Methacrylic Resin Solution A") 145.00g of PGMEA was placed in a reaction vessel as a solvent, and the liquid temperature was raised to 120°C while stirring and replacing with nitrogen. 10.00g of styrene (0.10mol), 85.20g of glycidyl methacrylate (0.60mol), 66.00g of monomethacrylate having a tricyclodecane skeleton (Hitachi Chemical Co., Ltd. "FA-513M"; 0.30mol), and 8.47g of 2,2'-azobis-2-methylbutyronitrile were added dropwise over 3 hours, and the mixture was further stirred at 90°C for 2 hours. Next, the atmosphere in the reaction vessel was replaced with air, and 43.20g of acrylic acid (0.60mol), 0.70g of trisdimethylaminomethylphenol, and 0.12g of hydroquinone were added, and the reaction was continued at 100°C for 12 hours.
[0186] Thereafter, 56.20 g of tetrahydrophthalic anhydride (0.37 mol) and 0.70 g of triethylamine were added, and the mixture was reacted at a liquid temperature of 100° C. for 3.5 hours to synthesize a PGMEA solution of alkali-soluble methacrylic resin a. The alkali-soluble methacrylic resin a had a weight average molecular weight of 8,400, an acid value of 80 mgKOH / g, and a double bond equivalent of 480 g / mol. 38 is a methyl group, and R 39 is a hydrogen atom, and R 40 The alkali-soluble methacrylic resin solution A was obtained by adding PGMEA and stirring the mixture so that the solid content of the alkali-soluble methacrylic resin solution A was 40% by weight.
[0187] (Synthesis Example 2: Synthesis of "Alkali-soluble Polyimide Resin B") Under a dry nitrogen stream, 150.15 g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (0.41 mol), 6.20 g of 1,3-bis(3-aminopropyl)tetramethyldisiloxane (0.02 mol), and 13.65 g of 3-aminophenol (0.13 mol) serving as an end-capping agent were dissolved in 500.00 g of N-methyl-2-pyrrolidone (hereinafter, "NMP") serving as an organic solvent, to which 155.10 g of bis(3,4-dicarboxyphenyl)ether dianhydride (0.50 mol) and 150 g of NMP were added, and the mixture was stirred at 20°C for 1 hour, and further stirred at 180°C for 4 hours while removing water. After the reaction was completed, the reaction solution was poured into 10 L of water, and the resulting precipitate was collected by filtration, washed five times with water, and dried in a vacuum dryer at 80°C for 20 hours to synthesize alkali-soluble polyimide resin B in the form of white powder and with a weight average molecular weight (Mw) of 25,000.
[0188] (Synthesis Example 3: Synthesis of "alkali-soluble maleimide resin solution C") 150.00g of PGMEA was placed in a reaction vessel as a solvent, and the mixture was stirred while replacing with nitrogen and heated to a liquid temperature of 120°C. A mixture of 25.00g of N-benzylmaleimide (0.13mol), 15.00g of methyl methacrylate (0.15mol), 25.00g of 2-hydroxyethyl methacrylate (0.19mol), 10.00g of acrylic acid (0.14mol), 0.50g of n-octyl mercaptan, 5.00g of 2,2'-azobis-2-methylbutyronitrile and 50.00g of PGMEA was added dropwise thereto over a period of 3 hours, and the mixture was stirred for 2 hours while maintaining the liquid temperature at 90°C to react, and then cooled to obtain a PGMEA solution of an alkali-soluble maleimide resin c having a structure represented by formula (12). The weight average molecular weight (Mw) of the alkali-soluble maleimide resin c was 16000. Furthermore, PGMEA was added and stirred so that the solid content of the alkali-soluble maleimide resin c in the PGMEA solution was 20% by weight, thereby obtaining an alkali-soluble maleimide resin solution C.
[0189] (Synthesis Example 4: Synthesis of "alkali-soluble polyimide precursor D") 18.30g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (0.05mol) was dissolved in 100mL of acetone and 17.4g of propylene oxide (0.30mol) and cooled to -15℃. A solution of 20.40g of 3-nitrobenzoyl chloride (0.11mol) dissolved in 100mL of acetone was added dropwise to this. After the dropwise addition, the reaction was carried out at -15℃ for 4 hours, and then the temperature was returned to room temperature. The precipitated white solid was filtered and dried in vacuum at 50℃. 30g of the obtained white solid was placed in a 300mL stainless steel autoclave, dispersed in 250mL of methyl cellosolve, and 2g of 5% palladium-carbon was added. Hydrogen was introduced into this with a balloon, and the reduction reaction was carried out at room temperature. After 2 hours, it was confirmed that the balloon did not shrink any more, and the reaction was terminated.
[0190] After the reaction was completed, the catalyst palladium compound was removed by filtration, and the mixture was concentrated with a rotary evaporator to obtain a hydroxyl group-containing diamine compound 1. Under a dry nitrogen stream, 21.2 g of hydroxyl group-containing diamine compound 1 (0.035 mol), 7.00 g of 4,4'-diaminodiphenyl ether (0.035 mol), and 1.20 g of bis(3-aminopropyl)tetramethyldisiloxane (0.005 mol) were dissolved in 400 g of NMP. 31.00 g of 4,4'-oxydiphthalic dianhydride (0.10 mol) was added together with 50 g of NMP and stirred at 40 ° C for 1 hour. Then, 5.50 g of 3-aminophenol (0.050 mol) was added as a terminal blocking agent and reacted by stirring at 40 ° C for 1 hour. After stirring, the solution was cooled to room temperature, and then the solution was poured into 3 L of water to obtain a white precipitate. The precipitate was collected by filtration, washed three times with water, and then dried in a vacuum dryer at 50° C. for 72 hours to obtain a powder, thereby obtaining an alkali-soluble polyimide precursor D having an acid equivalent of 220 g / mol.
[0191] (Synthesis Example 5: Synthesis of "quinone diazide compound a") Under a dry nitrogen stream, 21.23 g (0.05 mol) of TrisP-PA (manufactured by Honshu Chemical Industry Co., Ltd.), which is a compound having a phenolic hydroxyl group, and 33.58 g (0.125 mol) of 5-naphthoquinone diazide sulfonyl chloride were dissolved in 450.00 g of 1,4-dioxane and brought to room temperature. 12.65 g (0.125 mol) of triethylamine mixed with 50.00 g of 1,4-dioxane was added dropwise while maintaining the temperature in the system at 25 to 35°C. After the dropwise addition, the mixture was stirred at 30°C for 2 hours. Next, the triethylamine salt was filtered, the filtrate was poured into water, and the precipitate was filtered and collected. The precipitate was dried in a vacuum dryer to obtain a quinone diazide compound a represented by formula (28).
[0192] [ka]
[0193] (Synthesis Example 6: Synthesis of "Benzodifuranone-based black pigment 2") 500.00g of the benzodifuranone black pigment represented by formula (4) was put into a glass container containing 4500.00g of deionized water and stirred with a dissolver to obtain a preliminary stirred solution of an aqueous pigment suspension. This was sucked up with a tube pump and sent to a bead mill equipped with a vessel filled with 0.4mmφ zirconia beads (manufactured by Toray: Treceram (registered trademark)) at a filling rate of 75% by volume, and two-pass dispersion was performed at a discharge rate of 300mL / min. Next, the solution was sent to a bead mill equipped with a vessel filled with 0.05mmφ zirconia beads (manufactured by Toray: Treceram (registered trademark)) at a filling rate of 75% by volume, and circulation dispersion was performed for 6 hours at a discharge rate of 300mL / min, and pressure filtration was performed with a filter with a diameter of 10μm, after which the entire amount was discharged into a glass container and stirred again.
[0194] A solution of sodium silicate (Na2O·nSiO2·mH2O: 10% by weight as sodium oxide, 30% by weight as silicon dioxide: alkaline) diluted 100 times with deionized water and a 0.001 mol / L aqueous sulfuric acid solution were added simultaneously in parallel, with the addition rates of each being adjusted so that the pH of the aqueous pigment suspension was maintained in the range of 2 or more and less than 7, so that the amount of silica coating was 10 parts by weight per 100 parts by weight of the benzodifuranone black pigment represented by formula (4), and silica hydrate was precipitated and coated on the surface of the benzodifuranone black pigment represented by formula (4).
[0195] Next, water washing and filtration were repeated three times using a Nutsche filter to remove water-soluble impurities. Furthermore, a granular solid acid adsorbent (synthetic aluminum silicate) was added and stirred for 5 hours to capture metal ions, and then filtered to obtain a black filtrate. This was heated in an oven at an actual temperature of 90°C under dry air for 6 hours to remove moisture and powderize, and further heated in an oven at an actual temperature of 260°C under dry air for 1 hour to dehydrate and sinter, forming a coating layer made of silica. A dry grinding process was performed using a jet mill for 30 minutes to size the product, and benzodifuranone-based black pigment 2 was obtained.
[0196] The elements on the surface and cut surface of Benzodifuranone-based black pigment 2 were analyzed by SEM-EDX, and it was confirmed that the pigment surface was covered with silicon and oxygen atoms. In addition, the organic components were thermally decomposed and removed by firing for 6 hours in an electric furnace at an actual temperature of 800°C, and based on the weight of the residue, it was believed that the components of Benzodifuranone-based black pigment 2 were 100 parts by weight of the benzodifuranone-based black pigment represented by formula (4) and 10 parts by weight of silica. The specific surface area of Benzodifuranone-based black pigment 2 measured by the BET method was 40 m 2 In addition, the number of reactive silanol groups per SiO2-equivalent mass of the silica coating layer in the benzodifuranone-based black pigment 2 was 7.10 × 10 18 / g.
[0197] Example 1 34.00g of basic group-containing resin 1 and 109.52g of SPC-3410 were mixed with 736.48g of PGMEA, which is an organic solvent, and stirred for 10 minutes, after which 120.00g of benzodifuranone-based black pigment 2 was added and stirred for 30 minutes to obtain a preliminary stirring liquid. The preliminary stirring liquid was sent to a bead mill in which zirconia beads of 0.4mmφ were filled in the vessel at a vessel filling rate of 75% by volume, and wet dispersion treatment was performed by circulation at a peripheral speed of 8m / s for 1 hour. Furthermore, the liquid was sent to a bead mill in which zirconia beads of 0.05mmφ were filled in the vessel at a vessel filling rate of 75% by volume, and wet dispersion treatment was performed by circulation at a peripheral speed of 8m / s for 2 hours, and further wet dispersion treatment was performed at a peripheral speed of 9m / s for 2 hours to prepare a pigment dispersion liquid 1 with a solid content of 20.00% by weight.
[0198] Next, under yellow light, 0.60g of NCI-831E, which is a photopolymerization initiator, and 0.30g of TR-FR-201, which is a thermal crosslinking agent, were added to a mixed solvent of 17.00g of MBA and 35.83g of PGMEA, and the mixture was stirred for 10 minutes to dissolve. 11.67g of SPC-3410, 1.20g of dipentaerythritol hexaacrylate (hereinafter, "DPHA"), 0.75g of HX-220, and 2.40g of EA-0250P were added to the mixture and stirred to obtain a preparation. 30.25g of pigment dispersion 1 was mixed into the preparation and stirred for 30 minutes to prepare negative photosensitive composition 1 with a solid content of 15.00% by weight. The blending weights of each raw material are shown in Tables 1-2. The Dmax of negative photosensitive composition 1 was measured by the above-mentioned method, and was found to be 214 nm. In addition, based on the above-mentioned method, the negative photosensitive composition 1 was diluted with a mixed solvent of PGMEA and MBA to a solid content of 10.00% by weight, and the relaxation time T2 was measured. The value of X in formula (1) was calculated to be 73.
[0199] [Table 1]
[0200] [Table 2]
[0201] Negative photosensitive composition 1 was applied to the surface of a transparent glass substrate "Tempax" (manufactured by AGC Technoglass Co., Ltd.) using a spin coater, adjusting the rotation speed so that the final thickness of the cured film obtained would be 1.5 μm, to obtain a coating film. The coating film was then prebaked at atmospheric pressure at 100° C. for 120 seconds using a hot plate (SCW-636; manufactured by Dainippon Screen Mfg. Co., Ltd.) to obtain a prebaked film. Using a double-sided alignment single-sided exposure device, the entire surface of the prebaked film was irradiated with the g, h, and i mixed rays of an ultra-high pressure mercury lamp at the minimum required exposure amount determined by the above-mentioned method, to obtain an exposed film. Next, using a small photolithography developing device (AD-2000; manufactured by Takizawa Sangyo Co., Ltd.), the substrate was developed with a 2.38 wt % TMAH aqueous solution by paddle type for 1.5 times the minimum required developing time, and then rinsed with deionized water by shower type for 30 seconds to obtain a developed film, and using a high-temperature inert gas oven (INH-9CD-S; manufactured by Koyo Thermo Systems Co., Ltd.), the developed film was heated at 250°C for 60 minutes under a nitrogen atmosphere to obtain a substrate for optical density evaluation having a cured film with a thickness of 1.5 μm, and the optical density (OD / μm) was evaluated by the above-mentioned method, and was found to be 1.0.
[0202] Next, a bottom-emission type organic EL display device having a cured film made of the cured product of the negative-type photosensitive composition 1 as a pixel dividing layer was produced by the following method, and the driving voltage was evaluated. FIG. 2 shows a process for producing an organic EL display device, including a process for forming a pixel dividing layer.
[0203] A silver alloy (an alloy consisting of 99.00% by weight of silver and 1.00% by weight of copper) was formed on the entire surface of an alkali-free glass substrate 11 having a length of 70 mm and a width of 70 mm by a sputtering method. An alkali-soluble novolac-based positive resist was used, and the substrate was immersed in a silver alloy etching solution SEA-1 at a liquid temperature of 30° C. for etching to obtain a patterned silver alloy film 12 having a thickness of 100 nm. Furthermore, an ITO film was formed on the entire surface by a sputtering method. An alkali-soluble novolac-based positive resist was used, and the substrate was immersed in a 5% by weight aqueous solution of oxalic acid at a liquid temperature of 50° C. for 5 minutes, washed with deionized water for 2 minutes by showering, dried by air blowing, and heated at 150° C. for 30 minutes in a dry nitrogen atmosphere to obtain an ITO film 13 having a thickness of 10 nm and the same pattern. By the above steps, a first electrode-forming substrate having a first electrode consisting of a laminated pattern of a silver alloy film / ITO film was obtained on the surface of the alkali-free glass substrate.
[0204] The negative photosensitive composition 1 was applied to the surface of the first electrode-formed substrate using a spin coater, adjusting the number of revolutions so that the film thickness of the pixel division layer finally obtained was 1.5 μm, to obtain a coating film. Furthermore, the coating film was prebaked at 100° C. under atmospheric pressure for 120 seconds using a hot plate to obtain a prebaked film. Using a double-sided alignment single-sided exposure device, the prebaked film was pattern-exposed with the minimum required exposure amount through a negative exposure mask (220 openings of 260 μm in length and 70 μm in width) to obtain an exposed film. Next, using a small photolithography development device, the development time was 1.5 times the minimum required development time, and the development was performed using a 2.38 wt % TMAH aqueous solution in a paddle type, and the film was rinsed with deionized water in a shower type for 30 seconds to obtain a patterned developed film. Using a high-temperature inert gas oven, the developed film was heated at 250°C for 60 minutes under a nitrogen atmosphere to obtain a pixel division layer forming substrate having a pixel division layer 14 with a thickness of 1.5 μm and 220 openings (258 μm in length / 68 μm in width) within an area of 30 mm in length / 30 mm in width at the center of the first electrode forming substrate.
[0205] Next, the organic EL layer 15 including the light-emitting layer is formed in the opening of the pixel division layer 14 by vacuum deposition. -3Under deposition conditions of 0.1 Pa or less, the pixel division layer forming substrate 1 was rotated with respect to the deposition source, and first, a compound (HT-1) represented by formula (29) was deposited to a thickness of 10 nm as a hole injection layer, and a compound (HT-2) represented by formula (30) was deposited to a thickness of 50 nm as a hole transport layer. Next, a compound (GH-1) represented by formula (31) was deposited to a thickness of 40 nm as a host material, and a compound (GD-1) represented by formula (32) was deposited to a thickness of 40 nm on the light emitting layer. Next, a compound (ET-1) represented by formula (33) and a compound (LiQ) represented by formula (34) were deposited to a thickness of 40 nm as an electron transport material in a volume ratio of 1:1. The structures of the compounds used to form the organic EL layer 15 are shown below.
[0206] [ka]
[0207] [ka]
[0208] [ka]
[0209] [ka]
[0210] [ka]
[0211] [ka]
[0212] Next, after depositing a compound (LiQ) to a thickness of 2 nm, a silver / magnesium alloy (volume ratio 10:1) was deposited to a thickness of 150 nm to form a second electrode 16. Next, a cap-shaped glass plate was attached and sealed using an epoxy resin adhesive under a low humidity / nitrogen atmosphere to obtain an organic EL display device. The layers constituting the organic EL layer 15 are very thin compared to the pixel division layer described above, and a high measurement accuracy cannot be obtained using a stylus-type film thickness measurement device. Therefore, each layer was measured using a quartz crystal oscillation-type film thickness monitor suitable for thin films of less than 100 nm, and the average value of three points on the surface was rounded off to the nearest decimal place to obtain the film thickness. The driving voltage of the organic EL display device obtained above was measured using the above-mentioned method, and was 4.6 V. The evaluation results are shown in Table 3.
[0213] [Table 3]
[0214] (Examples 2 to 4) Pigment dispersions 2 to 4 with a solid content of 20.00% by weight were obtained in the same manner as in Example 1, except that the blending weights of each raw material shown in Tables 1 and 2 were used, and negative photosensitive compositions 2 to 4 with a solid content of 15.00% by weight were prepared using these in the blending weights shown in Table 2, respectively, and Dmax, the value of X in formula (1), and OD / μm of the cured film were evaluated. Furthermore, organic EL display devices were produced using each of the negative photosensitive compositions 2 to 4 in the same manner as in Example 1, and the driving voltage was evaluated. The evaluation results are shown in Table 3.
[0215] (Examples 5 to 6) A preliminary dispersion was prepared with the blending weight of each raw material shown in Table 1, and the preliminary stirring liquid was sent to a bead mill in which zirconia beads of 1.0 mmφ were filled in a vessel with a vessel filling rate of 75% by volume, and a wet dispersion treatment was performed by a circulation method at a peripheral speed of 7 m / s for 1 hour. Furthermore, the liquid was sent to a bead mill in which zirconia beads of 0.05 mmφ were filled in a vessel with a vessel filling rate of 75% by volume, and a wet dispersion treatment was performed by a circulation method at a peripheral speed of 8 m / s for 3 hours, to obtain pigment dispersions 5 to 6 with a solid content of 20.00 wt %, respectively. Negative photosensitive compositions 5 to 6 with a solid content of 15.00 wt % were prepared using the pigment dispersions 5 to 6 with the blending weight of each raw material shown in Table 2, and Dmax, the value of X in formula (1), and OD / μm of the cured film were evaluated. Furthermore, organic EL display devices were produced using the negative photosensitive compositions 5 to 6 in the same procedure as in Example 1, and the driving voltage was evaluated. The evaluation results are shown in Table 3.
[0216] Comparative Example 1 3.35g of PGMEA, 1.00g of MB, 0.75g of alkali-soluble methacrylic resin solution A, and 0.30g of BYK-LPN21116 were added to a 30mL container SV-30 (manufactured by Nichiden Rika Glass Co., Ltd.). Furthermore, 0.60g of benzodifuranone-based black pigment 1 was added and sealed. Ten identical containers were made, filled with 80% by volume of zirconia beads (0.3 mm) relative to the container volume, sealed, and wet dispersion treatment was performed in a batch manner for 5 hours using a paint shaker (manufactured by Asada Iron Works Co., Ltd.) at a vibration frequency of 643 rpm, and the zirconia beads and pigment dispersion were filtered. The 10 containers were mixed together in a 100mL container to give pigment dispersion 7. The blend weights of each raw material are shown in Table 4. Using the pigment dispersion 7, a negative photosensitive composition 7 having a solid content of 17.00 wt% was prepared with the blending weight of each raw material shown in Table 5. Since it was difficult to stably measure the Dmax of the negative photosensitive composition 7 with high accuracy by the above-mentioned method, the cumulant average particle diameter was measured by the method described in JP-A-2019-160473 using a concentrated particle size analyzer FPAR-1000 (manufactured by Otsuka Electronics Co., Ltd.), and the result was 178 nm. In addition, the value of X in formula (1) and the OD / μm of the cured film were evaluated. Furthermore, an organic EL display device was produced using the negative photosensitive composition 7 in the same procedure as in Example 1, and the driving voltage was evaluated. The evaluation results are shown in Table 6.
[0217] [Table 4]
[0218] [Table 5]
[0219] [Table 6]
[0220] Comparative Example 2 Pigment dispersion 8 having a solid content of 17.00 wt% was prepared in the same manner as in Comparative Example 1, except that 0.27 g of CI Pigment Blue 15:6, 0.09 g of CI Pigment Violet 29, and 0.24 g of CI Pigment Orange 64 were used instead of 0.60 g of benzodifuranone-based black pigment 1, with the blending weight of each raw material shown in Table 4. Negative-type photosensitive composition 8 having a solid content of 17.00 wt% was prepared using pigment dispersion 8 with the blending weight of each raw material shown in Table 5. The cumulant average particle diameter measured in the same manner as in Comparative Example 1 was 99 nm. The value of X in formula (1) and the OD / μm of the cured film were evaluated. Furthermore, an organic EL display device was produced in the same manner as in Example 1 using negative-type photosensitive composition 8, and the driving voltage was evaluated. The evaluation results are shown in Table 6.
[0221] Comparative Example 3 A preliminary dispersion was prepared with the blend weight of each raw material shown in Table 4, and the preliminary stirring liquid was sent to a bead mill in which zirconia beads of 0.4 mmφ were filled in a vessel with a vessel filling rate of 75% by volume, and a wet dispersion treatment was performed by circulation at a peripheral speed of 7 m / s for 5 hours to obtain a pigment dispersion 9 with a solid content of 20.00 wt %. A negative photosensitive composition 9 with a solid content of 15.00 wt % was prepared using the pigment dispersion 9 with the blend weight of each raw material shown in Table 5, and Dmax, the value of X in formula (1), and the OD / μm of the cured film were evaluated. Furthermore, an organic EL display device was produced using the negative photosensitive composition 9 in the same procedure as in Example 1, and the driving voltage was evaluated. The evaluation results are shown in Table 6.
[0222] Comparative Example 4 A preliminary dispersion was prepared with the blend weight of each raw material shown in Table 4, and the preliminary stirring liquid was sent to a bead mill in which zirconia beads of 0.1 mmφ were filled in a vessel with a vessel filling rate of 75% by volume, and a wet dispersion treatment was performed by circulation at a peripheral speed of 12 m / s for 5 hours to obtain a pigment dispersion 10 with a solid content of 20.00 wt %. A negative photosensitive composition 10 with a solid content of 15.00 wt % was prepared with the blend weight of each raw material shown in Table 5 using the pigment dispersion 10, and Dmax, the value of X in formula (1), and the OD / μm of the cured film were evaluated. Furthermore, an organic EL display device was produced using the negative photosensitive composition 10 in the same procedure as in Example 1, and the driving voltage was evaluated. The evaluation results are shown in Table 6.
[0223] Example 7 72.48g of alkali-soluble polyimide precursor D was added to 880.00g of mixed solvent (PGME / γ-BL=70 / 30 (weight ratio)) and stirred for 30 minutes, and 7.25g of dye-type dispersing aid 2 was added and stirred for 10 minutes. 40.27g of perylene-based black pigment 1 was added to this and stirred for 30 minutes to obtain a preliminary stirring liquid. The liquid was sent to a bead mill in which zirconia beads of 0.05mmφ were filled in the vessel with a vessel filling rate of 75% by volume, and wet dispersion treatment was performed for 1 hour at a peripheral speed of 8m / s by circulation, and further wet dispersion treatment was performed for 2 hours at a peripheral speed of 9m / s to obtain pigment dispersion liquid 11 with a solid content of 12.00% by weight. The blending weights of each raw material are shown in Table 7. Using the pigment dispersion 11, a positive photosensitive composition 1 having a solid content of 12.00% by weight was prepared with the blend weight of each raw material shown in Table 8, and Dmax and the value of X in formula (1) were evaluated. In addition, the OD / μm of the cured film was evaluated in the same manner as in Example 1, except that the pre-bake temperature was set to 120°C, and the exposure process was omitted. Furthermore, an organic EL display device was produced using the positive photosensitive composition 1 in the same manner as in Example 1, except that the pre-bake temperature was set to 120°C, a positive exposure mask in which the light-shielding portion and the opening portion were inverted with the same pattern size instead of the negative exposure mask, and the development time was set to 90 seconds, and the driving voltage was evaluated. The evaluation results are shown in Table 9.
[0224] [Table 7]
[0225] [Table 8]
[0226] [Table 9]
[0227] (Examples 8 to 9 and Comparative Examples 5 to 6) Pigment dispersions 12 to 15 were prepared in the same manner as in Example 7, with the blend weights shown in Table 7. Positive photosensitive compositions 2 to 5 with a solid content of 12.00 wt % were prepared using pigment dispersions 12 to 15, with the blend weights of each raw material shown in Table 8, and Dmax, the value of X in formula (1), and the OD / μm of the cured film were evaluated in the same manner as in Example 7. The evaluation results are shown in Table 9. It can be seen that, in Examples 1 to 9, the driving voltage required to obtain a certain luminance is lower than that in Comparative Examples 1 to 6. According to FIG. 3, there is a certain correlation between the value of X and the driving voltage, and when the value of X in formula (1) is within the range of 55 to 125, a preferably low driving voltage is obtained. Also, according to FIG. 4, it can be seen that, in the examples in which the value of X in formula (1) is within the range of 55 to 125, an even more preferably low driving voltage is obtained when the maximum cumulative particle diameter Dmax is within the range of 150 to 350 nm. On the other hand, according to FIG. 4, the plot is random, and no correlation is observed between Dmax and relaxation time T2. From the above results, it is understood that the value of X in formula (1) is dominant in determining the driving voltage, and the photosensitive composition of the present invention is useful. [Explanation of symbols]
[0228] 1: Alkaline-free glass substrate 2: Silver alloy film 3: ITO film 4: Pixel division layer 5: Organic EL layer 6:Second electrode
Claims
1. (a-1) contains a benzodifuranone-based black pigment, (b) a resin, (c) a photosensitizer, and (d) a solvent, and the value of X in formula (1) is 55 to 125; The (b) resin contains (b-1) a basic group-containing resin and (b-2) an alkali-soluble resin, The basic group-containing resin (b-1) contains a resin having a structure represented by formula (9), The (c) photosensitive agent is a photosensitive composition containing a compound having two or more radically polymerizable groups in the molecule and a photopolymerization initiator. X=T 2 / A... (1) (In formula (1), T 2 , T 2 Measurement sample Measurement nucleus 1 The spin-spin relaxation time (ms) measured by the Carr-Purcell-Meiboom-Gill method using a 1 H pulsed nuclear magnetic resonance spectrometer is shown as an average value when measured three times. A is the T 2 It represents the content (wt%) of all components excluding particle components and solvent components in the total weight of the measurement sample (100 wt%), and is 6.50 to 8.
80. [Formula 1] (In formula (9), the number of repeating units n 1 is an integer from 1 to 9. R 21 and R 22 each independently represent an alkylene group having 1 to 5 carbon atoms. * represents a bonding site with an alkylene oxide structure.)
2. 2. The photosensitive composition according to claim 1, wherein the maximum cumulative particle diameter Dmax in the particle size distribution of the particle components based on the light scattering intensity measured by a dynamic light scattering method is 150 to 350 nm.
3. The photosensitive composition according to claim 1 or 2, wherein the (a-1) benzodifuranone black pigment contains at least one compound selected from the group consisting of a compound represented by formula (2), a compound represented by formula (3), and an isomer thereof. [chemical 2] [C3] (In formula (2) and formula (3), R 1 and R 6 are each independently a hydrogen atom, CH 3 , C.F. 3 or a fluorine atom. 2 , R 3 , R 4 , R 5 , R 7 , R 8 , R 9 and R 10 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, a cycloalkenyl group having 1 to 12 carbon atoms, an alkynyl group having 1 to 12 carbon atoms, COOH, COOR 11 , COO - , C.O.N.H. 2 , C.O.N.R. 11 , C.O.R. 11 R 12 , C.N., O.H., O.R. 11 , O.C.O.R. 11 , OCONH 2 , OCONH.R. 11 , OCONR. 11 R 12 Represents R 2 and R 3 , R 3 and R 4 , R 4 and R 5 , R 7 and R 8 , R 8 and R 9 And R 9 and R 10 is a direct bond or O, S, NH or NR 11 They may be linked by R 11 and R 12 each independently represents an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, a cycloalkenyl group having 1 to 12 carbon atoms, or an alkynyl group having 1 to 12 carbon atoms.
4. The photosensitive composition according to claim 3, wherein the (b-1) basic group-containing resin contains a (meth)acrylic block copolymer having a quaternary ammonium salt group, and the quaternary ammonium salt group has a structure consisting of a salt of a quaternary ammonium cation and a carbon atom-containing counter anion.
5. 5. The photosensitive composition according to claim 1, wherein the benzodifuranone black pigment (a-1) has a coating material on its surface, and the coating material contains silica.
6. 6. The photosensitive composition according to claim 1, wherein the alkali-soluble resin (b-2) contains a resin having a structure represented by formula (12): [C4] (In formula (12), R 32 and R 33 And R 35 and R 36 R each independently represents a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms. 34 and R 37 Each independently represents a monovalent organic group having 1 to 16 carbon atoms. * represents a bonding site with a carbon atom.
7. A cured product of the photosensitive composition according to any one of claims 1 to 6.
8. An organic electroluminescence display device comprising the cured product according to claim 7 .
Citation Information
Patent Citations
Coloring material liquid for color filter, colored composition for color filter, color filter and display device
JP2018025797A
Display device including resin composition and black bank manufactured using the same
JP2018528447A
Coloring photosensitive composition for forming organic electroluminescent element partition, partition, organic electroluminescent element, image display device, and lighting
JP2019160473A
Pigment dispersion, negative photosensitive composition, and cured product
JP2020070352A
Olefin resin and method for producing same
WO2015147186A1