Contact lenses and their manufacturing method
A balanced monomer composition for contact lenses addresses hydrophilicity and oxygen permeability issues, achieving comfortable and durable silicone hydrogel lenses by using specific proportions of phosphorylcholine ester, hydrophilic, and siloxanyl monomers, resulting in lenses with improved hydrophilicity and mechanical strength.
Patent Information
- Application Number
- JP2020211555
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-12-21
AI Technical Summary
Conventional silicone hydrogel contact lenses face issues with insufficient hydrophilicity leading to lens clouding and reduced oxygen permeability, while maintaining appropriate moisture content and mechanical strength is challenging, especially when high MPC and hydrophilic monomer content is used.
A monomer composition comprising specific proportions of phosphorylcholine group-containing methacrylic ester, hydrophilic monomers, acrylamide-containing monomers, siloxanyl group-containing itaconic acid diester, and siloxanyl group-containing (meth)acrylate monomers, along with optional components, is used to create a contact lens polymer with balanced water content, mechanical strength, and improved hydrophilicity.
The composition results in contact lenses with enhanced hydrophilicity, mechanical strength, and oxygen permeability, ensuring comfort and ease of handling without dryness or clouding, even after prolonged wear.
Smart Images

Figure 0007593096000001 
Figure 0007593096000002 
Figure 0007593096000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a monomer composition for contact lenses, a polymer thereof, and a contact lens comprising the polymer, which has excellent mechanical strength and an appropriate water content and is therefore easy to handle and comfortable to wear, and a method for producing the same. [Background technology]
[0002] Conventional hydrogel contact lenses have an insufficient supply of oxygen to the cornea of the eye, and therefore have safety problems when worn for long periods of time. Silicone hydrogel contact lenses have been developed as contact lenses that solve this problem and improve safety. However, there is a problem in terms of the manufacturing method of contact lenses, that is, it is difficult to make the surface of silicone hydrogel contact lenses hydrophilic. That is, when silicone hydrogel contact lenses are manufactured by the cast molding method using a polypropylene mold, which is a general manufacturing method for soft contact lenses, the silicone monomers of the raw material are polymerized in a state oriented at the interface with the mold, because polypropylene is hydrophobic. As a result, silicone polymer parts are present on the lens surface, and therefore the hydrophilicity of the lens surface is reduced.
[0003] If the hydrophilicity of the soft contact lens surface is insufficient, there is a concern that the lens will become cloudy due to lipids and proteins adhering to the lens, or that eye diseases will occur due to the adhering substances.Therefore, for silicone hydrogel contact lenses with insufficient hydrophilicity, the surface is coated with plasma gas or hydrophilic polymer after the lens is formed, or a surface graft polymer is formed with hydrophilic monomer.However, these surface treatments require many devices and steps to manufacture soft contact lenses compared to when surface treatment is not required, and are therefore undesirable for mass production.
[0004] Patent Document 1 discloses a method for producing a lens from a composition for silicone hydrogel that contains a silicone monomer having a (meth)acryloyl group, a hydrophilic monomer having a vinyl group, a crosslinkable monomer, and a polymerization initiator having a 10-hour half-life temperature of 70° C. to 100° C. Patent Document 1 aims to improve the hydrophilicity of the lens surface by utilizing the difference in polymerizability of the raw material monomers, but still fails to achieve satisfactory hydrophilicity.
[0005] Patent Document 2 discloses a silicone hydrogel contact lens obtained from a composition containing 2-methacryloyloxyethyl phosphorylcholine (MPC), dimethacryloyl silicone macromer, and (3-methacryloxy-2-hydroxypropyloxy)propylbis(trimethylsiloxy)methylsilane (SiGMA). However, although the contact lens disclosed in Patent Document 2 shows an improvement in the hydrophilicity of the lens surface, it has a problem of reduced oxygen permeability.
[0006] Patent Documents 3 and 4 disclose compositions containing a siloxanyl group-containing itaconic acid diester monomer having a primary hydroxyl group and MPC, and state that the polymer can be used for contact lenses. The contact lens disclosed in Patent Document 3 exhibits good results in terms of hydrophilicity of the lens surface and oxygen permeability, while the contact lens disclosed in Patent Document 4 exhibits good results in addition to these in terms of breaking elongation and peelability. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2015 / 001811 [Patent Document 2] JP 2014-089477 A [Patent Document 3] International Publication No. 2018 / 135421 [Patent Document 4] International Publication No. 2020 / 054711 Summary of the Invention [Problem to be solved by the invention]
[0008] However, although the contact lenses according to Patent Documents 3 and 4 are favorable in terms of hydrophilicity of the lens surface and oxygen permeability, they contain a large amount of MPC and other hydrophilic monomers, and therefore have a high water content, which may cause dryness when worn for a long time. In addition, if the content of silicone monomer is increased in order to adjust the water content to an appropriate level, the mechanical strength may deteriorate, which may cause a foreign body sensation when worn for a long time, and the contact lenses may become difficult to handle.
[0009] Therefore, an object of the present invention is to provide a monomer composition for contact lenses that has an appropriate water content and excellent mechanical strength, and is comfortable to wear and easy to handle, even when it contains a large amount of MPC and a hydrophilic monomer, without increasing the content of silicone monomer. Weight Combined Polymerization for Contact Lenses Body The present invention provides a contact lens and a method for producing the same. [Means for solving the problem]
[0010] As a result of intensive research, the present inventors have found that the above-mentioned object can be achieved by using, as a contact lens raw material, a monomer composition comprising MPC, a specific hydrophilic monomer, an acrylamide-containing monomer, a siloxanyl group-containing itaconic acid diester monomer, and a siloxanyl group-containing (meth)acrylate, each of which is blended in a specific range of amount, and have thus completed the present invention.
[0011] That is, according to the present invention, there is provided a composition containing (A) a phosphorylcholine group-containing methacrylic ester monomer represented by formula (1), (B) one or more hydrophilic monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, ethylene glycol monovinyl ether, diethylene glycol monovinyl ether, and N-vinylpyrrolidone, (C) one or more acrylamide-containing monomers selected from N,N-dimethylacrylamide and N,N-diethylacrylamide, (D) a siloxanyl group-containing itaconic acid diester monomer represented by formula (2), and (E) a siloxanyl group-containing (meth)acrylate represented by formula (3), wherein the composition contains 5 to 25 mass% of (A), 5 to 30 mass% of (B), 10 to 35 mass% of (C), 7 to 27 mass% of (D), and 15 to 40 mass% of (E) based on the total amount of components (A) to (E) in the composition. death , The total content of (A) and (B) relative to the content of (C) is in a mass ratio [(A) + (B)] / (C) of 0.8 to 1.5. Monomer composition for contact lenses A contact lens having a hydrate of a polymer for contact lenses, the polymer being a polymer of the above, and a water content of 45% or less, a modulus of 0.3 MPa to 0.7 MPa, and a breaking elongation of 200% or more. is provided.
[0012] [ka]
[0013] [ka]
[0014] [ka] [In formula (3), R1 is a hydrogen atom or a methyl group, m is 0 or 1, and n is 5 to 20.]
[0016] According to another aspect of the present invention, Noko Intactren Z A method of manufacture is provided.
[0017] That is, the present invention relates to the following [1] to [ 3 ] regarding. [1] A composition containing (A) a phosphorylcholine group-containing methacrylic ester monomer represented by formula (1), (B) one or more hydrophilic monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, ethylene glycol monovinyl ether, diethylene glycol monovinyl ether, and N-vinylpyrrolidone, (C) one or more acrylamide-containing monomers selected from N,N-dimethylacrylamide and N,N-diethylacrylamide, (D) a siloxanyl group-containing itaconic acid diester monomer represented by formula (2), and (E) a siloxanyl group-containing (meth)acrylate represented by formula (3), wherein the composition contains 5 to 25 mass% of (A), 5 to 30 mass% of (B), 10 to 35 mass% of (C), 7 to 27 mass% of (D), and 15 to 40 mass% of (E) based on the total amount of components (A) to (E) in the composition. The total content of (A) and (B) relative to the content of (C) is in a mass ratio [(A)+(B)] / (C) of 0.8 to 1.5. Monomer composition for contact lenses A contact lens having a hydrate of a polymer for contact lenses, the polymer being a polymer of the above, and a water content of 45% or less, a modulus of 0.3 MPa to 0.7 MPa, and a breaking elongation of 200% or more. . [ka] [ka] [ka] [In formula (3), R 1 is a hydrogen atom or a methyl group. m is 0 or 1, and n is 5 to 20. [2] The contact lens according to the above [1], wherein the composition further contains (F) a monomer other than the components (A) to (E) in an amount of 30 parts by mass or less per 100 parts by mass of the total amount of the components (A) to (E). Z. [ 3 ] (A) a phosphorylcholine group-containing methacrylic ester monomer represented by formula (1), (B) one or more hydrophilic monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, ethylene glycol monovinyl ether, diethylene glycol monovinyl ether, and N-vinylpyrrolidone, (C) one or more acrylamide-containing monomers selected from N,N-dimethylacrylamide, and N,N-diethylacrylamide, and (D) a monomer represented by formula (2): and (E) a siloxanyl group-containing (meth)acrylate represented by formula (3), the composition contains 5 to 25 mass% of (A), 5 to 30 mass% of (B), 10 to 35 mass% of (C), 7 to 27 mass% of (D), and 15 to 40 mass% of (E) based on the total amount of components (A) to (E) in the composition, and the total amount of (A) and (B) relative to the amount of (C) is a mass ratio [(A)+(B)] / (C) of 0.8 to 1.5. The method comprises the steps of: (1) mixing a polymer for contact lenses with one or more solvents selected from water, methanol, ethanol, 1-propanol, and 2-propanol to remove unreacted matter; and (2) immersing the polymer for contact lenses from which the unreacted matter has been removed in physiological saline to hydrate it. As described in [1] aboveA method for manufacturing contact lenses. [ka] [ka] [ka] [In formula (3), R 1 is a hydrogen atom or a methyl group. m is 0 or 1, and n is 5 to 20. Effect of the Invention
[0018] The monomer composition for contact lenses of the present invention essentially contains the components (A) to (E) in specific proportions, and the polymer can provide a silicone hydrogel contact lens that has an appropriate water content and excellent mechanical strength, and is comfortable to wear and easy to handle. Furthermore, the method for producing contact lenses of the present invention can produce silicone hydrogel contact lenses with the above-mentioned excellent performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will now be described in further detail. The monomer composition for contact lenses of the present invention is characterized by being a composition containing a phosphorylcholine group-containing methacrylic ester monomer represented by formula (1) [component (A)], one or more hydrophilic monomers selected from (B) hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, ethylene glycol monovinyl ether, diethylene glycol monovinyl ether and N-vinylpyrrolidone [component (B)], one or more acrylamide-containing monomers selected from (C) N,N-dimethylacrylamide and N,N-diethylacrylamide [component (C)], a siloxanyl group-containing itaconic acid diester monomer represented by formula (2) [component (D)], and a siloxanyl group-containing (meth)acrylate represented by formula (3) [component (E)] in a specific ratio. Hereinafter, the monomer composition for contact lenses of the present invention may be simply referred to as the composition of the present invention. The composition of the present invention may further contain a specific amount of one or more components selected from (F) a monomer other than the above (A) to (E) [component (F)] and (G) a solvent having a hydroxyl group [component (G)]. The composition of the present invention may also contain (H) a polymerization initiator [component (H)]. The composition of the present invention is a homogeneous transparent liquid containing the above-mentioned components (A) to (E) as essential components, and components (F) to (H) as optional components.
[0020] Component (A): Phosphorylcholine group-containing methacrylic ester monomer Component (A) is a phosphorylcholine group-containing methacrylic ester monomer represented by formula (1), specifically 2-methacryloyloxyethyl phosphorylcholine (MPC). By including component (A), the hydrophilicity and lubricity of the surface of a contact lens produced from the polymer of the composition of the present invention can be improved. [ka]
[0021] The content of component (A) is 5 to 25% by mass, preferably 8 to 20% by mass, and more preferably 8 to 18% by mass, based on the total amount of monomer components (A) to (E) in the composition of the present invention. If it is less than 5% by mass, sufficient hydrophilicity of the contact lens surface cannot be obtained, and if it exceeds 25% by mass, it becomes difficult to dissolve component (A) in the composition of the present invention, and there is a concern that the mechanical strength of the contact lens may decrease.
[0022] Component (B): hydrophilic monomer The component (B) is one or more hydrophilic monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, ethylene glycol monovinyl ether, diethylene glycol monovinyl ether, and N-vinylpyrrolidone. By including a predetermined amount of the component (B), the mechanical strength of the resulting contact lens is improved. Specific examples of component (B) include N-vinylpyrrolidone, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, ethylene glycol monovinyl ether, and diethylene glycol monovinyl ether, and from the viewpoint of ease of incorporation into the final contact lens, N-vinylpyrrolidone, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate are preferred. Component (B) may be any one of these monomers or a mixture of two or more of them. In this specification, "(meth)acrylate" and "(meth)acrylic ester" mean acrylate and / or methacrylate, acrylic ester and / or methacrylic ester, respectively.
[0023] The content of component (B) is 5 to 30 mass% based on the total amount of monomer components (A) to (E) in the composition of the present invention, preferably 5 to 25 mass%, and more preferably 10 to 25 mass%. If it is less than 5 mass%, there is a concern that the resulting contact lens will become brittle, and if it exceeds 30 mass%, there is a concern that the water content will be high.
[0024] Component (C): Acrylamide-containing monomer Component (C) is one or more acrylamide-containing monomers selected from N,N-dimethylacrylamide and N,N-diethylacrylamide. By containing a predetermined amount of component (C), the water content of the resulting contact lens can be adjusted to an appropriate level.
[0025] The content of component (C) is 10 to 35% by mass, preferably 10 to 30% by mass, and more preferably 15 to 30% by mass, based on the total amount of monomer components (A) to (E) in the composition of the present invention. If it is less than 10% by mass, there is a concern that the water content of the resulting contact lens will be high, and if it exceeds 35% by mass, there is a concern that the oxygen permeability will decrease.
[0026] The total content of components (A) and (B) relative to the content of component (C) is preferably in a mass ratio [component (A) + (B)] / component (C) of 0.8 to 3.5, more preferably 0.8 to 2.5, and even more preferably 0.8 to 1.5. By setting the mass ratio to 0.8 to 3.5, contact lenses having an appropriate water content and good mechanical strength can be easily obtained.
[0027] Component (D): Siloxanyl group-containing itaconic acid diester monomer Component (D) is a siloxanyl group-containing itaconic acid diester monomer represented by formula (2): Component (D) is a component that contributes to improving the oxygen permeability and transparency of the contact lens produced. [ka]
[0028] The content of component (D) is 7 to 27% by mass, preferably 7 to 25% by mass, and more preferably 10 to 22% by mass, based on the total amount of monomer components (A) to (E) in the composition of the present invention. If it is less than 7% by mass, it may be difficult to dissolve component (A) in the composition of the present invention, and the obtained polymer for contact lenses may become cloudy, while if it exceeds 27% by mass, there is a concern that the breaking elongation of the contact lens will decrease.
[0029] Component (E): Siloxanyl group-containing (meth)acrylate Component (E) is a siloxanyl group-containing (meth)acrylate represented by formula (3). Component (E) is a component that contributes to improving the oxygen permeability and adjusting the mechanical strength of the contact lens produced. [ka] [In formula (3), R 1 is a hydrogen atom or a methyl group; m is 0 or 1, and n is 5 to 20.
[0030] The content of component (E) is 15 to 40 mass% based on the total amount of monomer components (A) to (E) in the composition of the present invention, preferably 15 to 35 mass%, and more preferably 20 to 35 mass%. If it is less than 15 mass%, there is a concern that the oxygen permeability of the contact lens will decrease, and if it exceeds 40 mass%, there is a concern that the mechanical strength of the contact lens will decrease.
[0031] The total content of components (D) and (E) is preferably 35 to 60 mass%, and more preferably 40 to 55 mass%, based on the total amount of monomer components (A) to (E) in the composition of the present invention. By making the total content of components (D) and (E) 35 mass% or more, the oxygen permeability of the resulting contact lens becomes good. In addition, by making it 60 mass% or less, the mechanical strength of the resulting contact lens becomes good, and the contact lens becomes easy to handle.
[0032] Component (F): Monomer other than (A) to (E) The component (F) is a monomer other than the components (A) to (E). The component (F) is an optional component that can be blended for the purposes of adjusting the physical properties of the resulting contact lens and improving the solvent resistance. Examples of the component (F) include N-vinylpiperidin-2-one, N-vinyl-ε-caprolactam, N-vinyl-3-methyl-2-caprolactam, acryloylmorpholine, N-vinyl-N-methylacetamide, N-vinylacetamide, N-vinylformamide, (meth)acrylic acid, 2-methacryloyloxyethylsuccinic acid, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, methoxypolyethylene glycol methacrylate, 3- Examples of the crosslinking agent include monomers such as (methacryloyloxy)propyl tris(trimethylsilyloxy)silane and methyl bis(trimethylsiloxy)silylpropyl glycerol methacrylate, and crosslinking agents such as silicone dimethacrylate represented by formula (4), ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, methylene bisacrylamide, allyl methacrylate, (2-allyloxy)ethyl methacrylate, 2-(2-vinyloxyethoxy)ethyl acrylate, 2-(2-vinyloxyethoxy)ethyl methacrylate, and divinylbenzene. The component (F) may be any one of these monomers, or a mixture of two or more of them. [ka] [In formula (4), p and r are each 0 or 1, and q is 5 to 20.]
[0033] When the component (F) is contained, its content is not particularly limited, but is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less, relative to 100 parts by mass of the total amount of the monomer components (A) to (E) in the composition of the present invention. When it is 30 parts by mass or less, the physical properties can be adjusted without impairing the surface hydrophilicity and mechanical strength of the obtained contact lens. Furthermore, when the component (F) has a crosslinking agent, the content of the crosslinking agent is preferably 0.1 to 3 parts by mass, more preferably 0.1 to 2 parts by mass, relative to 100 parts by mass of the total amount of the monomer components (A) to (E) in the composition of the present invention. When it is 0.1 to 2 parts by mass, the solvent resistance can be improved without impairing the mechanical strength.
[0034] (G) Ingredient; Solvent The component (G) is a solvent having a hydroxyl group. The component (G) is an optional component and may be added for the purpose of improving the solubility of the component (A) in the composition of the present invention. Examples of the component (G) include alcohols and carboxylic acids. The use of a solvent having a hydroxyl group has the advantage of increasing the dissolution rate of the component (A) in the composition of the present invention, making it easier to dissolve. Examples of alcohols include ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol, 1-pentanol, 2-pentanol, tert-amyl alcohol, 1-hexanol, 1-octanol, 1-decanol, and 1-dodecanol. Examples of carboxylic acids include glycolic acid, lactic acid, and acetic acid. The (G) component may be any one of these solvents or a mixture of two or more of them. In terms of the solubility of the (A) component and the pH stability of the composition of the present invention, one or more selected from ethanol, 1-propanol, 2-propanol, and 1-hexanol are particularly preferred.
[0035] When component (G) is contained, its content is not particularly limited, but is preferably 15 parts by mass or less, and more preferably 10 parts by mass or less, relative to 100 parts by mass of the total amount of monomer components (A) to (E) in the composition of the present invention. If it is 15 parts by mass or less, it facilitates dissolution of component (A) without impairing the water content or mechanical strength of the resulting contact lens.
[0036] The composition of the present invention may be a composition containing (H) a polymerization initiator [component (H)]. When component (H) is contained, care must be taken in storing the composition of the present invention, but the composition of the present invention has the advantage that the polymer for contact lenses of the present invention can be easily obtained with stable quality by simply heating the composition of the present invention. The component (H) is not particularly limited, but any known thermal polymerization initiator can be used. Examples of the (H) component include 2,2'-azobisisobutyronitrile and dimethyl 2,2-Azobis(2-methylpropionate) 2,2'-Azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-Azobis(2,4-dimethylvaleronitrile), 2,2'-Azobis[2-(2-imidazolin-2-yl)propane]disulfate dihydrate, 2,2'-Azobis(2-methylpropionamidine)dihydrochloride, 2,2'-Azobis[N-(2-carboxyethyl)-2-methylpropionamidine]dihydrate, 2,2'-Azobis[2-(2-imidazolin-2-yl)propane], 2,2'-Azobis(1-imino-1-pyrrolidino-2-methylpropane)dihydrochloride, 2,2' azo-based polymerization initiators such as 2,2'-azobis[2-methyl-N-{1,1-bis(hydroxymethyl)-2-hydroxyethyl}propionamide], 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis(2-methylpropionamidine) dihydrochloride, and 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide]; and peroxide-based polymerization initiators such as benzoyl peroxide, t-butyl hydroperoxide, cumene hydroperoxide, lauroyl peroxide, t-butyl peroxyhexanoate, and 3,5,5-trimethylhexanoyl peroxide. As the component (H), any one of these polymerization initiators may be blended, or two or more of them may be blended. As the component (H), an azo-based polymerization initiator is preferable from the viewpoint of safety and availability, and 2,2'-azobisisobutyronitrile, dimethyl 2,2-azobis(2-methylpropionate), and 2,2'-azobis(2,4-dimethylvaleronitrile) are particularly preferable from the viewpoint of reactivity.
[0037] When component (H) is contained, its content is preferably 0.1 to 3 parts by mass, more preferably 0.2 to 1 part by mass, per 100 parts by mass of the total amount of monomer components (A) to (E) in the composition of the present invention. If it is less than 0.1 part by mass, the polymerizability of the composition of the present invention may be insufficient, and the advantage of incorporating component (H) may not be obtained. If it exceeds 3 parts by mass, when the polymer for contact lenses obtained by polymerization is washed to produce contact lenses, the reactive decomposition products of component (H) may not be sufficiently extracted and removed.
[0038] The method for producing the composition of the present invention is not particularly limited, and the composition can be produced by adding each component in any order or all at once to a stirring (mixing) device and stirring and mixing the components at 40°C or less until they are uniform. However, when component (H) is included, in order to avoid the initiation of a polymerization reaction during mixing, if component (H) is a thermal polymerization initiator, it is preferable to mix at a temperature of 40°C or less and at least 10°C lower than the 10-hour half-life temperature of the initiator. In terms of improving the solubility of component (A) in the composition of the present invention, it is preferable to mix and dissolve the three components (A), (B), and (D) and then add and mix the other components.
[0039] The composition of the present invention may contain other components (other components) than the above-mentioned components within a range that does not impair the object of the present invention. Examples of other components include polymerizable ultraviolet absorbers and polymerizable dyes as colorants. By incorporating an ultraviolet absorber, the burden on the eyes caused by ultraviolet rays such as sunlight can be reduced. In addition, by incorporating a dye, a colored contact lens can be obtained. The content of each of the other components in the composition of the present invention is preferably 5 parts by mass or less, and more preferably 3 parts by mass or less, per 100 parts by mass of the total amount of the monomer components (A) to (E) in the composition of the present invention.
[0040] The polymer for contact lenses of the present invention is a polymer of the composition of the present invention explained above, and when the composition does not contain component (H), it is preferable to add a polymerization initiator to carry out the polymerization reaction. As the polymerization initiator to be added, the initiators exemplified as component (H) can be used. When the composition of the present invention contains the component (H), the polymer for contact lenses of the present invention also contains the component (H).
[0041] Next, an embodiment of the method for producing the polymer for contact lenses of the present invention will be described. Note that the production method shown below is one embodiment for obtaining the polymer for contact lenses of the present invention, and the polymer for contact lenses of the present invention is not limited to the polymer obtained by this production method. Hereinafter, unless otherwise specified, the term "composition" refers to the composition of the present invention, and the term "polymer" refers to the polymer for contact lenses of the present invention.
[0042] The polymer is produced by using a mold (metal mold) having a hydrophobic surface made of polypropylene or the like, filling the mold with the composition, and polymerizing the composition. In the case of a composition that does not contain component (H), a polymerization initiator similar to that of component (H) is added to the composition in an amount approximately equal to that of component (H) and then filling the mold. The polymerization is carried out for 1 hour or more at 45 to 140°C according to the decomposition temperature of the polymerization initiator used. After the polymerization is completed, the mixture is cooled to 60°C or less, and the produced polymer is removed from the mold.
[0043] The polymerization atmosphere is not particularly limited, but an inert gas atmosphere such as nitrogen or argon is preferable in terms of improving the polymerization rate. Examples of a method for providing such an inert gas atmosphere include aeration of the composition with an inert gas and a method for providing such an atmosphere at the place where the composition is filled into a mold.
[0044] The pressure inside the mold can be atmospheric pressure to slight pressure. When polymerizing in an inert gas atmosphere, the gauge pressure is 1 kgf / cm. 2 The following pressures are preferred:
[0045] The contact lens of the present invention is a silicone hydrogel contact lens, which is a hydrate of the above-mentioned polymer. Here, hydrate means that the polymer contains water, and the contact lens of the present invention is one in which the polymer is hydrated and exhibits a hydrogel form, that is, the silicone hydrogel contact lens of the present invention. However, since the polymer contains unreacted substances, by-products, etc., and optionally (G) solvent, the polymer is purified by washing or the like before hydration. Hereinafter, unless otherwise specified, the term "contact lens" refers to the contact lens of the present invention. In this specification, the term "silicone hydrogel" refers to a hydrogel having a silicone moiety in the polymer. Since the composition of the present invention contains the silicone-containing monomers (D) and (E), the polymer has a silicone moiety in the polymer and can form a silicone hydrogel by hydrating (containing water).
[0046] The water content of the contact lens is preferably 45% or less, more preferably 42% or less, and even more preferably 40% or less, in the water content measurement described in the examples. By making the water content 45% or less, the contact lens is less likely to feel dry even when worn for a long time. In addition, the mechanical strength of the contact lens is preferably a modulus of 0.3 MPa to 0.7 MPa and a breaking elongation of 200% or more, in the mechanical strength measurement described in the examples. By making the modulus 0.3 MPa to 0.7 MPa and the breaking elongation of 200% or more, the contact lens is less likely to feel a foreign body sensation even when worn for a long time, and the contact lens is easy to handle. Note that "moderate water content" refers to a water content of 45% or less, in the water content measurement described in the examples. In addition, "excellent mechanical strength" refers to a modulus of 0.3 MPa to 0.7 MPa and a breaking elongation of 200% or more, in the mechanical strength measurement described in the examples.
[0047] Next, an embodiment of a method for producing a contact lens of the present invention will be described. Note that the production method described below is one embodiment for obtaining a contact lens of the present invention, and the contact lens of the present invention is not limited to the contact lens obtained by this production method.
[0048] The method for producing a contact lens of the present invention preferably comprises the steps of: (1) mixing a polymer for contact lenses with one or more solvents selected from water, methanol, ethanol, 1-propanol, and 2-propanol and removing any unreacted substances; and (2) immersing the polymer for contact lenses from which the unreacted substances have been removed in physiological saline to hydrate it.
[0049] The above step (1) is a step of purifying the polymer removed from the mold by washing it with a solvent to remove unreacted substances such as unreacted monomers and impurities. As the solvent, for example, water, methanol, ethanol, 1-propanol, 2-propanol, or a mixture thereof can be used. The washing can be performed, for example, by immersing the polymer in the above alcohol at 10 to 40°C for 10 minutes to 5 hours, and then immersing it in water for 10 minutes to 5 hours. In addition, between the alcohol washing and the water washing, washing may be performed by immersing the polymer in a water-containing alcohol having an alcohol concentration of 20 to 50 wt% for 10 minutes to 5 hours. As the water, pure water, ion-exchanged water, etc. are preferable.
[0050] The above step (2) is a step of obtaining a contact lens by immersing the polymer, which has been purified by removing unreacted substances by washing, in physiological saline and hydrating it to a predetermined water content. As the physiological saline, borate buffered saline or phosphate buffered saline may be used. Since these physiological saline solutions are used in storage solutions for soft contact lenses, the polymer may be immersed in the storage solution for soft contact lenses to hydrate it. From the viewpoint of hydration, it is preferable that the osmotic pressure of these physiological saline solutions is 250 to 400 mOms / kg.
[0051] The contact lenses of the present invention have a good hydrophilicity on the lens surface, are resistant to adhesion of dirt such as lipids, and even if dirt does adhere, they can be easily washed off, and have excellent mechanical strength, so that they can be used for about one month under normal usage conditions if desired. Of course, they may be replaced in a shorter period of time. EXAMPLES
[0052] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.
[0053] The components constituting the compositions of the examples and comparative examples are shown below. Component (A): Phosphorylcholine group-containing methacrylic ester monomer MPC: (2-methacryloyloxyethyl) phosphorylcholine
[0054] Component (B): hydrophilic monomer NVP: N-vinylpyrrolidone HEMA: 2-hydroxyethyl methacrylate HPMA: 2-Hydroxypropyl methacrylate HBMA: 2-Hydroxybutyl methacrylate ·EGMV: Ethylene glycol monovinyl ether ·DEGMV: Diethylene glycol monovinyl ether
[0055] Component (C): Acrylamide-containing monomer ·DMAA: N,N-Dimethylacrylamide ·DEAA: N,N-diethylacrylamide
[0056] Component (D): Siloxanyl group-containing itaconic acid diester monomer ETS: a compound of formula (2)
[0057] Component (E): Siloxanyl group-containing methacrylate X-22-174ASX: In formula (3), R 1Compound in which is a methyl group and m is 0 [number average molecular weight (Mn); approximately 900]
[0058] Component (F): Monomer other than (A) to (E) MMA: Methyl methacrylate ·SiGMA: Methylbis(trimethylsiloxy)silylpropyl glycerol methacrylate EGDMA: Ethylene glycol dimethacrylate TEGDV: Triethylene glycol divinyl ether X-22-164AS: A compound in which p=r=0 in formula (4) [number average molecular weight (Mn); about 900]
[0059] (G) Ingredient; Solvent · NPA: 1-propanol (normal propyl alcohol) HeOH: 1-Hexanol (normal hexanol)
[0060] Component (H): Polymerization initiator AIBN: 2,2'-azobis(isobutyronitrile) (10-hour half-life temperature: 65°C)
[0061] The compositions, polymers, and contact lenses (model contact lenses) of the respective Examples and Comparative Examples were evaluated according to the following evaluation items. Hereinafter, "contact lenses (model contact lenses)" in each evaluation item and each table includes not only those of the respective Examples but also those of the respective Comparative Examples.
[0062] [Transparency of polymer] The transparency of the polymer was visually evaluated according to the following criteria. ○:Transparent △: Slightly cloudy ×: Cloudy
[0063] [Transparency of contact lenses] After purifying the polymer, it was immersed in physiological saline as described in ISO-18369-3 and allowed to swell to obtain a hydrogel, which was used as a model contact lens and visually evaluated according to the following criteria. ○:Transparent △: Slightly cloudy ×: Cloudy
[0064] [Mechanical strength measurement of contact lenses] To evaluate the mechanical strength of the model contact lenses, a Yamaden BAS-3305(W) breaking strength analyzer was used to measure the modulus (MPa) according to JIS-K7127. A load cell of 2N was used. Model contact lenses cut to a width of 2 mm were used as measurement samples, which were pulled at a speed of 1 mm / sec with a clamp distance of 6 mm, and the modulus was measured from the initial stress. The distance until the sample broke was also measured, and the elongation rate relative to the sample length of 6 mm was taken as the breaking elongation [%]. The modulus and breaking elongation were expressed together with symbols within the following ranges. Modulus [MPa] ◎: 0.4 or more and 0.6 or less ○: 0.3 or more and less than 0.4, or more than 0.6 and less than 0.7 ×: Less than 0.3 or more than 0.7 Elongation at break [%] ◎: 250 or more ○: 200 or more and less than 250 ×: Less than 200
[0065] [Water content of contact lenses] The water content of the model contact lenses was measured according to the method described in ISO 18369-4. The water content [%] is indicated with a symbol within the following range. ◎:30 or more and 40 or less 〇: More than 40 but less than 45 △: More than 45 but less than 55 ×: Over 55
[0066] [Oxygen permeability coefficient of contact lenses] The oxygen permeability coefficient of the model contact lenses was measured according to the method described in ISO 18369-4. The oxygen permeability coefficient is also indicated by a symbol in the following range. ◎: 85 or higher ○: 70 or more and less than 85 ×: Less than 70
[0067] [Example 1] 0.50g (10% by mass) of MPC, 0.45g (9% by mass) of HPMA, 1.05g (21% by mass) of ETS, 0.05g (1 part by mass) of EGDMA, and 0.40g (8 parts by mass) of NPA were mixed in a container and stirred at room temperature until MPC was dissolved. Furthermore, 0.25g (5% by mass) of NVP, 1.25g (25% by mass) of DEAA, 1.50g (30% by mass) of X-22-174ASX, and 0.03g (0.6 parts by mass) of AIBN were added to the container and stirred at room temperature until homogenous to obtain a composition. The composition was poured into a 25mm x 70mm x 0.2mm cell sandwiched between two polypropylene plates using a 0.1mm thick polyethylene terephthalate sheet as a spacer, and into a lens mold, and the atmosphere in the oven was replaced with nitrogen. The temperature was then raised to 95° C. and maintained at 95° C. for 4 hours to polymerize the composition, thereby obtaining a polymer. The polymer was removed from the cell and the lens mold. The polymer was immersed in 100 g of a 50 wt% 2-propanol aqueous solution for 4 hours, and then immersed in 100 g of ion-exchanged water for 4 hours to remove unreacted substances and other substances, and purified. The purified polymer was immersed in physiological saline according to ISO-18369-3, and allowed to swell (hydrate) to prepare a model contact lens. The obtained model contact lenses were divided into sizes and shapes suitable for each of the above evaluations, and each evaluation was carried out. The blending ratio of each component in the composition, the polymerization conditions, and the evaluation results are shown in Table 1. The numerical value of each component in the "Other Components" column in the table indicates the number of parts by mass per 100 parts by mass of the total amount of components (A) to (E).
[0068] [Examples 2 to 8] Model contact lenses of each Example were prepared in the same manner as in Example 1, except that the blending ratio of each component in the composition and the polymerization conditions were as shown in Table 1. Furthermore, the model contact lenses of each Example were evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0069] [Comparative Example 1] 1.25g (25% by mass) of MPC, 1.00g (20% by mass) of EGMV, 1.10g (22% by mass) of ETS, and 0.75g (15 parts by mass) of NPA were mixed in a container and stirred at room temperature until MPC was dissolved. Furthermore, 0.5g (10% by mass) of NVP, 1.15g (23 parts by mass) of X-22-174ASX, 0.15g (3 parts by mass) of X-22-164AS, and 0.035g (0.7 parts by mass) of AIBN were added to the container and stirred at room temperature until homogenized to obtain a composition of Comparative Example 1. The composition of Comparative Example 1 was poured into a 25 mm x 70 mm x 0.2 mm cell sandwiched between two polypropylene plates using a 0.1 mm thick polyethylene terephthalate sheet as a spacer, and into a lens mold, and the atmosphere in an oven was replaced with nitrogen. The temperature was then raised to 65°C and maintained at 65°C for 2 hours, and then raised to 100°C and maintained at 100°C for 2 hours to polymerize the composition and obtain a polymer. The polymer was removed from the cell and lens mold. The polymer was immersed in 100 g of a 50 wt% 2-propanol aqueous solution for 4 hours, and then immersed in 100 g of ion-exchanged water for 4 hours to remove unreacted substances and other substances, and purified. The purified polymer was immersed in physiological saline according to ISO-18369-3, and allowed to swell (hydrate) to prepare a model contact lens. The obtained model contact lenses were divided into sizes and shapes suitable for each of the above evaluations, and each evaluation was carried out. The blending ratio of each component in the composition of Comparative Example 1, the polymerization conditions, and the evaluation results are shown in Table 2. The contact lens of Comparative Example 1 had a lower water content than the contact lenses of each Example.
[0070] [Comparative Examples 2 to 4] The compositions, polymers, and model contact lenses for each Comparative Example were prepared in the same manner as in Comparative Example 1, except that the blending ratio of each component in the composition for each Comparative Example and the polymerization conditions were as shown in Table 2. The evaluation results are shown in Table 2. The contact lens of Comparative Example 2 had a lower water content than the contact lenses of each Example. The contact lens of Comparative Example 3 had a lower mechanical strength than the contact lenses of each Example. The contact lens of Comparative Example 4 had a lower transparency than the contact lenses of each Example, and the following evaluations could not be carried out.
[0071] [Table 1]
[0072] [Table 2]
Claims
1. (A) a phosphorylcholine group-containing methacrylic ester monomer represented by formula (1), (B) one or more hydrophilic monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, ethylene glycol monovinyl ether, diethylene glycol monovinyl ether, and N-vinylpyrrolidone; (C) one or more acrylamide-containing monomers selected from N,N-dimethylacrylamide and N,N-diethylacrylamide; (D) a siloxanyl group-containing itaconic acid diester monomer represented by formula (2), (E) a siloxanyl group-containing (meth)acrylate represented by formula (3), A composition comprising: a contact lens having a hydrate of a polymer for contact lenses, which is a polymer of a monomer composition for contact lenses, the composition containing 5 to 25% by mass of (A), 5 to 30% by mass of (B), 10 to 35% by mass of (C), 7 to 27% by mass of (D), and 15 to 40% by mass of (E) based on the total amount of components (A) to (E) in the composition, and the total amount of (A) and (B) relative to the amount of (C) is a mass ratio [(A)+(B)] / (C) of 0.8 to 1.5; A contact lens having a water content of 45% or less, a modulus of 0.3 MPa to 0.7 MPa, and a breaking elongation of 200% or more. [Formula 1] [Case 2] [C3] [In formula (3), R 1 is a hydrogen atom or a methyl group; m is 0 or 1, and n is 5 to 20.
2. 2. The contact lens of claim 1, wherein the composition further comprises (F) a monomer other than the components (A) to (E) in an amount of 30 parts by mass or less per 100 parts by mass of the total amount of the components (A) to (E).
3. (A) a phosphorylcholine group-containing methacrylic ester monomer represented by formula (1), (B) one or more hydrophilic monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, ethylene glycol monovinyl ether, diethylene glycol monovinyl ether, and N-vinylpyrrolidone; (C) one or more acrylamide-containing monomers selected from N,N-dimethylacrylamide and N,N-diethylacrylamide; (D) a siloxanyl group-containing itaconic acid diester monomer represented by formula (2), (E) a siloxanyl group-containing (meth)acrylate represented by formula (3), A composition comprising: a step (1) of mixing a polymer for contact lenses, which is a polymer of a monomer composition for contact lenses, containing 5 to 25 mass% of (A), 5 to 30 mass% of (B), 10 to 35 mass% of (C), 7 to 27 mass% of (D), and 15 to 40 mass% of (E) based on the total amount of components (A) to (E) in the composition, and the total amount of (A) and (B) to the amount of (C) is in a mass ratio of 0.8 to 1.5, [(A)+(B)] / (C), with one or more solvents selected from water, methanol, ethanol, 1-propanol, and 2-propanol, and removing unreacted substances; The method for producing a contact lens according to claim 1, further comprising a step (2) of immersing the contact lens polymer from which the unreacted substances have been removed in physiological saline to hydrate it. [C4] [C5] [C6] [In formula (3), R 1 is a hydrogen atom or a methyl group, m is 0 or 1, and n is 5 to 20.]
Citation Information
Patent Citations
Hydrogel contact lens and preparation method thereof
CN103467652A
Wettable silicone hydrogel contact lenses and related compositions and methods
JP2014089477A
Method for making silicone hydrogel contact lenses
US20190300654A1
Method for producing silicone-containing copolymer molded article having hydrophilic surface, and silicone hydrogel contact lens having hydrophilic surface
WO2015001811A1
Contact lens monomer composition, contact lens polymer and method for manufacturing same, and contact lens and method for manufacturing same
WO2018135421A1