Liquid crystal display device and polarizing plate

By using a polyester film with specific retardation and an antireflection layer in the polarizing plate, the issue of rainbow-like color spots in liquid crystal displays is resolved, enhancing visibility and polarization stability.

JP7593423B2Active Publication Date: 2024-12-03TOYOBO CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023001436
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-03-04
Filing Date
2023-01-10
Publication Date
2024-12-03
Estimated Expiration
2035-11-20

AI Technical Summary

Technical Problem

Liquid crystal display devices using polyester films as polarizer protective films experience rainbow-like color spots due to changes in polarization state when using light sources with narrow emission spectra, particularly those incorporating quantum dots, which are not effectively addressed by existing solutions.

Method used

Incorporating a polyester film with specific retardation (1500 to 30000 nm) and an antireflection or low reflection layer into the polarizing plate to maintain polarization state stability, reducing surface reflection, and aligning the transmission axis of the polarizer with the fast axis of the polyester film to minimize deviations.

Benefits of technology

The solution effectively suppresses rainbow-like color spots across various viewing angles, ensuring improved visibility and maintaining polarization integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593423000002
    Figure 0007593423000002
  • Figure 0007593423000003
    Figure 0007593423000003
  • Figure 0007593423000004
    Figure 0007593423000004
Patent Text Reader

Abstract

Liquid crystal display device having a light source that emits excitation light and a backlight source that includes quantum dots In this case, when a polyester film is used as a polarizer protective film, rainbow spots are also observed. To provide a liquid crystal display device in which the noise is suppressed. The present invention relates to a backlight source, two polarizing plates, and a polarizing plate disposed between the two polarizing plates. A liquid crystal display device having a liquid crystal cell, wherein the backlight source is a light source that emits excitation light. and quantum dots, and at least one of the polarizers is a polarizer. A polyester film is laminated on at least one surface of the The polyester film has a retardation of 1500 to 30000 nm. A liquid crystal display having an anti-reflection layer and / or a low-reflection layer laminated on at least one surface of the film. display device.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid crystal display device and a polarizing plate. The present invention relates to a liquid crystal display device and a polarizing plate. [Background technology]

[0002] The polarizing plates used in liquid crystal displays (LCDs) are usually made of polyvinyl alcohol (PVA). The polarizer, which is dyed with iodine, is sandwiched between two polarizer protection films. In most cases, triacetyl cellulose (TAC) film is used as a protective film. In recent years, as LCDs have become thinner, there has been a demand for thinner polarizing plates. However, to achieve this, the thickness of the TAC film used as a protective film must be reduced. If the thickness is too small, the mechanical strength is not sufficient and the moisture permeability is deteriorated. In addition, TAC film is very expensive, and polyester film is a cheaper alternative. However, there is a problem that rainbow-like color spots are observed. .

[0003] When a birefringent oriented polyester film is placed on one side of the polarizer, When the linearly polarized light emitted from the polarizer passes through the polyester film, The polarization state of the transmitted light changes as the birefringence of the oriented polyester film multiplied by its thickness. The retardation of the light produced by the reflective layer causes interference colors that are specific to the retardation of the reflective layer. When a discontinuous emission spectrum is used, the transmitted light intensity varies depending on the wavelength, resulting in rainbow-like color spots. (See Proceedings of the 15th Micro-Optical Conference, pages 30-31.) .

[0004] As a means to solve the above problems, a white light emitting diode (LED) or the like is used as a backlight source. A white light source with a continuous and wide emission spectrum is used, and a polarizer protection film is also used. It has been proposed to use an oriented polyester film having a certain retardation. (Patent Document 4) White light-emitting diodes have a continuous and wide light emission spectrum in the visible light region. Therefore, the envelope of the interference color spectrum of the transmitted light that has passed through the birefringent medium Focusing on the linear shape, the retardation of the oriented polyester film can be controlled to It is proposed that a spectrum similar to the emission spectrum of the source can be obtained, and rainbow spots can be suppressed. It is being done.

[0005] The orientation direction of the oriented polyester film and the polarization direction of the polarizing plate are perpendicular to each other, or By making the polarizer parallel, the linearly polarized light emitted from the polarizer passes through the oriented polyester film. The light passes through the oriented polyester film while maintaining its polarized state. By controlling the birefringence of the film and increasing the uniaxial orientation, the light incident from an oblique direction can be polarized. When the oriented polyester film is viewed obliquely, However, when the uniaxial orientation is high, the film is not aligned in the same direction as when viewed obliquely. Therefore, the deviation of the main axis direction when the linearly polarized light is It is believed that the deviation becomes smaller, and the change in the polarization state becomes less likely to occur. By controlling the emission spectrum of the light source, the orientation state of the birefringent material, and the orientation axis direction, It was believed that the change in state would be suppressed, rainbow-like color spots would not occur, and visibility would be significantly improved. . [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2002-116320 A [Patent Document 2] JP 2004-219620 A [Patent Document 3] JP 2004-205773 A [Patent Document 4] WO2011 / 162198 Summary of the Invention [Problem to be solved by the invention]

[0007] A liquid crystal display device using a polarizing plate using a polyester film as a polarizer protective film When manufacturing industrially, the direction of the transmission axis of the polarizer and the fast axis of the polyester film are usually aligned. The polarizers are arranged so that they are always perpendicular to each other. The vinyl alcohol film is produced by longitudinal uniaxial stretching. The polyvinyl alcohol film used is usually a long film in the stretching direction. The polyester film used as the protective film is produced by stretching longitudinally and then transversely. Therefore, the main axis direction of the polyester film is the horizontal direction. The orientation axis of the polyester film used is approximately perpendicular to the longitudinal direction of the film. These films are usually laminated together so that their longitudinal directions are parallel to each other to create polarizing light. In this way, the fast axis of the polyester film and the transmission axis of the polarizer are usually perpendicular. In this case, the polyester film is arranged to have a specific retardation. It uses a unidirectional polyester film and is designed to be a continuous, wide-angle light source such as a white LED. By using a light source with a broad emission spectrum, the rainbow color spot is significantly improved. However, the backlight source consists of a light source that emits excitation light and a light-emitting layer that contains quantum dots. However, it was found that a new problem still exists in the case of iridescence.

[0008] In recent years, the demand for expanding the color gamut has increased, and in addition to white light sources using quantum dot technology, The emission spectrum of the light source is divided into R (red), G (green), and B (blue) wavelength regions, respectively. Liquid crystal display devices that have a clear peak in relative luminescence intensity have been developed. Using a phosphor with clear emission peaks in the R (red) and G (green) regions and a blue LED The white LED light source uses a phosphorescent material, a three-wavelength white LED light source, and a red laser. A wide color gamut compatible LCD display using various types of light sources, including a combination of white LED light sources. These white light sources are all based on the YAG yellow light that has been widely used up until now. The half-width of the peak is narrower than that of a light source made of a white light-emitting diode using a color phosphor. These white light sources use polyester films with retardation as the polarizing plate components. When the film is used as a polarizer protection film, the light source emitting the above-mentioned excitation light and the quantum dot The problem is similar to that of a liquid crystal display device having a backlight source made of a light-emitting layer containing I discovered that it exists.

[0009] That is, one of the objects of the present invention is to provide a light source that emits excitation light and a backlight that includes quantum dots. As typified by light sources, backlight sources have relatively narrow half-widths of the emission spectrum. In a liquid crystal display device having a light source, a polyester film is used as a polarizer protective film. The present invention aims to provide a liquid crystal display device and a polarizing plate in which rainbow spots are suppressed even when a liquid crystal display using a liquid crystal display device having a polarizing plate is used. [Means for solving the problem]

[0010] Representative aspects of the present invention are as follows. Section 1. A backlight source, two polarizing plates, and a liquid crystal cell disposed between the two polarizing plates. A liquid crystal display device having: The backlight light source includes a light source that emits excitation light and quantum dots, At least one of the polarizing plates has a polarizer on at least one surface thereof made of polyester. A thermoplastic resin film is laminated on the surface of the substrate. The polyester film has a retardation of 1500 to 30000 nm. , An anti-reflection layer and / or a low reflection layer is laminated on at least one surface of the polyester film. It has been said that LCD display device. Section 2. A backlight source, two polarizing plates, and a liquid crystal cell disposed between the two polarizing plates. A liquid crystal display device having: The backlight light source has a wavelength of 400 nm or more and less than 495 nm, and a wavelength of 495 nm or more and 600 nm or more. The emission spectrum has peaks in the wavelength ranges of 600 nm to 780 nm, and 600 nm to 780 nm. The light emitted has a peak having a half-width of 5 nm or more, At least one of the polarizing plates has a polarizer on at least one surface thereof made of polyester. A thermoplastic resin film is laminated on the surface of the substrate. The polyester film has a retardation of 1500 to 30000 nm. , An anti-reflection layer and / or a low reflection layer is laminated on at least one surface of the polyester film. It has been said that LCD display device. Section 3. The backlight light source has a wavelength of 400 nm or more and less than 495 nm, or 495 nm or more and 600 nm or less. Emission spectrum peaks in the wavelength ranges of 600 nm to 750 nm and 600 nm to 750 nm, respectively. Item 3. The liquid crystal display device according to item 2, wherein each peak has a half-value width of 5 nm or more. Section 4. Item 1. The surface reflectance of the antireflection layer at a wavelength of 550 nm is 2.0% or less. 4. A liquid crystal display device according to any one of claims 1 to 3. Section 5. A polarizing plate having a polyester film laminated on at least one surface of a polarizer, The polyester film has a retardation of 1500 to 30000 nm, An anti-reflection layer and / or a low reflection layer is laminated on at least one surface of the polyester film. There are Polarizing light for liquid crystal display device having a light source emitting excitation light and a backlight light source containing quantum dots light board Section 6. A polarizing plate having a polyester film laminated on at least one surface of a polarizer, The polyester film has a retardation of 1500 to 30000 nm, An anti-reflection layer and / or a low reflection layer is laminated on at least one surface of the polyester film. There are 400nm or more but less than 495nm, 495nm or more but less than 600nm, and 600nm or more It has a peak top in each wavelength region below 780 nm, and the half-width of each peak is 5 nm. The polarizing plate for a liquid crystal display device has a backlight source having the above-mentioned emission spectrum. Section 7. Item 5. The surface reflectance of the antireflection layer surface at a wavelength of 550 nm is 2.0% or less. 7. Or the polarizing plate according to claim 6. Effect of the Invention

[0011] The liquid crystal display device and the polarizing plate of the present invention are free from rainbow-like color spots at any observation angle. It is possible to ensure good visibility that is significantly suppressed. [Brief description of the drawings]

[0012] [Figure 1] An example where multiple peaks exist within a single wavelength region is shown. [Diagram 2] An example where multiple peaks exist within a single wavelength region is shown. [Diagram 3] An example where multiple peaks exist within a single wavelength region is shown. [Figure 4] An example where multiple peaks exist within a single wavelength region is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In general, a liquid crystal display device has a backlight source (also called a "backlight unit") In order from the side where they are placed to the side where the image is displayed (the viewing side), the rear module, the liquid crystal cell and a front module. The rear module and the front module are generally transparent. A substrate, a transparent conductive film formed on the surface facing the liquid crystal cell, and a polarizing plate disposed on the opposite side In other words, the polarizing plate is In the front module, the LED is placed on the side that displays the image (the viewing side). do.

[0014] The liquid crystal display device of the present invention includes at least a backlight source and a polarizer disposed between two polarizers. The backlight light source has a wavelength of 400 nm or more and less than 495 nm. 495nm to less than 600nm, and 600nm to 780nm in each wavelength range Each has a peak top, and the half-width of each peak is 5 nm or more. It is preferable that the peak wavelengths of blue, green, and red are defined as follows in the CIE chromaticity diagram: 435.8nm (blue), 546.1nm (green), and 700nm (red) respectively. It is known that the wavelengths of 400 nm to less than 495 nm and 495 nm to 600 nm are The wavelength ranges of less than 600 nm and 780 nm are blue and green, respectively. The light source having the emission spectrum described above is an excitation light and a backlight source including at least a quantum dot. The phosphors have emission peaks in the red and green regions when excited by light, and blue White LED light source using phosphor method combined with LED, white LED light source using three wavelength method, red Examples of the phosphors include a white LED light source combined with a laser. As the color phosphor, for example, a nitride phosphor having a basic composition of CaAlSiN3:Eu, etc. , Sulfide phosphors with a basic composition of CaS:Eu, etc., and Examples of the green phosphor among the above phosphors include silicate phosphors. For example, sialon-based phosphors based on β-SiAlON:Eu, etc. Examples of such phosphors include silicate-based phosphors having a basic composition such as SiO 2 :Eu.

[0015] In addition to the backlight source, polarizing plate, and liquid crystal cell, the liquid crystal display device may also include other components, such as a color Filters, lens films, diffusion sheets, anti-reflection films, etc. may be used as appropriate. A brightness enhancement film may be provided between the light source side polarizing plate and the backlight source. The upper film, for example, transmits one linearly polarized light and reflects the linearly polarized light perpendicular to the first linearly polarized light. Examples of the reflective polarizing plate include the reflective polarizing plate manufactured by Sumitomo 3M Limited. DBEF (registered trademark) (Dual Brightness Enhancement The brightness enhancement film of the FT Film series is preferably used. In general, the absorption axis of the reflective polarizing plate is parallel to the absorption axis of the light source side polarizing plate. .

[0016] Of the two polarizing plates arranged in the liquid crystal display device, at least one of them is made of polyvinyl chloride. At least one side of the polarizer is coated with polyvinyl alcohol (PVA) or the like, which is dyed with iodine. It is preferable that the sheet is laminated with an ester film. From the viewpoint of suppressing rainbow-like color spots, The polyester film has a specific retardation and has at least one surface thereof It is preferable that an anti-reflection layer and / or a low reflection layer is laminated. The low reflection layer may be provided on the surface of the polyester film opposite to the surface on which the polarizer is laminated. Alternatively, the polarizer may be provided on the surface on which the polyester film is laminated, or on both surfaces. Preferably, the polarizing film is laminated on the surface of the polyester film opposite to the surface on which the polarizing film is laminated. It is preferable to provide an antireflection layer and / or a low reflection layer. When an anti-reflection layer and / or a low reflection layer is provided on the lamination surface, the layer is preferably made of polyester fiber. It is preferable that the anti-reflection layer and / or the low-reflection layer are provided between the film and the polarizer. Between the polyester film and the adhesive layer, other layers (e.g., an adhesive layer, a hard coat layer, an anti-glare layer, etc.) In order to further suppress rainbow-like color spots, a bias layer, an antistatic layer, an antifouling layer, etc. may be present. The refractive index of the polyester film in the direction parallel to the photon transmission axis is 1.53 or more and 1. The other surface of the polarizer is preferably covered with a TAC film or an acrylic film. The laminate is made of films with no birefringence, such as norbornene films. However, it is not always necessary to laminate a film on the other side of the polarizer (three-layer polarizing plate). It is not necessary to use a polarizing plate with two layers (a polarizing plate with two layers). When polyester films are used, the slow axes of both polyester films are approximately parallel to each other. Preferably, it is a row.

[0017] The polyester film may be laminated to the polarizer via any adhesive. The adhesive may be directly laminated without using any adhesive. As an example, a water-based adhesive (i.e., an adhesive component is dissolved in water or For example, polyvinyl alcohol as the main component can be used. Adhesives containing urethane resin and / or urethane resin can be used. In order to improve the properties, an isocyanate compound and / or an epoxy compound may be used as necessary. Another example of an adhesive that can be used is a photocurable adhesive. In one embodiment, a solvent-free UV-curable adhesive is preferred. The photocurable resin may be, for example, a mixture of a photocurable epoxy resin and a photocationic polymerization initiator. A mixture thereof can also be mentioned.

[0018] The backlight is configured as an edge light type that uses a light guide plate and a reflector as components. The backlight source may be a light source that emits excitation light. Examples of backlight sources that include quantum dots and quantum light sources include "400 nm to 495 nm" 495nm to less than 600nm, and 600nm to 780nm in each wavelength range Each has a peak top, and the half-width of each peak is 5 nm or more. In addition, the quantum dots are preferably, for example, This can be used as a light-emitting layer in a backlight.

[0019] The application of quantum dot technology to LCDs has been attracting attention in recent years due to the growing demand for a wider color gamut. This is a technology that uses ordinary white LEDs as a backlight source. In contrast, the excitation light can only reproduce about 20% of the visible spectrum. When using a backlight source consisting of a light source that emits excited light and a light-emitting layer containing quantum dots, It is said that it will be possible to reproduce more than 60% of the colors in the spectrum that the human eye can see. The quantum dot technology that has been put to practical use is Nanosys' QDEF TM or QD Vis ion Color IQ TM etc.

[0020] The light-emitting layer containing quantum dots is made of a resin material such as polystyrene. The device is made up of a number of pixels that emit light of different colors based on the excitation light emitted from the light source. The light-emitting layer is, for example, a red light-emitting layer disposed in the red pixel, a green light-emitting layer disposed in the green pixel, and The light emitting layer is a green light emitting layer disposed in a blue pixel, and a blue light emitting layer disposed in a blue pixel. The quantum dots in the layer generate emission light of different wavelengths (colors) based on the excitation light. do.

[0021] Examples of such quantum dot materials include CdSe, CdS, ZnS:Mn, and In. N, InP, CuCl, CuBr, and Si, and their quantum dot particle sizes The size of one side of the quantum dot material is, for example, about 2 to 20 nm. Among them, InP is an example of a red light emitting material, and CdSc is an example of a green light emitting material. Examples of blue emitting materials include CdS. In such a light emitting layer, By changing the size (particle size) and material composition of the quantum dots, the emission wavelength can be changed. It has been confirmed that the size (particle size) of quantum dots and the material can be controlled and the material can be incorporated into the resin material. They are mixed together and applied separately to each pixel. In addition, heavy metals such as cadmium are used in many applications. The use of this genus is being restricted, so we have developed a new type of fluororesin that maintains the same brightness and stability as conventional fluororesin. Cadmium-free quantum dots are also being developed.

[0022] A blue LED is used as a light source to emit excitation light, but lasers such as semiconductor lasers are also used. When excitation light from a light source passes through the light-emitting layer, 400nm or more but less than 495nm, 495nm or more but less than 600nm, and 600nm or more but less than 7 An emission spectrum with peaks at each wavelength region below 80 nm is produced. The narrower the half-width of the peak in each wavelength region, the wider the color gamut becomes. Therefore, the light emission efficiency is reduced when the color gamut is increased. The shape of the spectrum is designed.

[0023] There are two main implementation methods for light sources using quantum dots, although they are not limited to the following: The first method is the on-edge method, which mounts quantum dots along the edge (side) of the backlight light guide plate. The quantum dot, which is a particle with a diameter of several nanometers to several tens of nanometers, is placed in a glass tube with a diameter of several millimeters. The light from the blue LED enters the glass tube, which is then sealed and placed between the blue LED and the light guide plate. The blue light that hits the quantum dots is converted into green or red light. The advantage of the LD method is that it can reduce the amount of quantum dots used even on a large screen. This is a surface mounting method in which quantum dots are placed on a light plate. This quantum dot film is then sandwiched between two barrier films and sealed in place. The barrier film serves to prevent the quantum dots from deteriorating due to water and oxygen. The blue LED is placed on the edge (side) of the light guide plate, just like the on-edge method. The light enters the light guide plate and becomes a planar blue light, which illuminates the quantum dot film. There are two major advantages to this method. First, the light from the blue LED passes through the light guide plate and hits the quantum dots. Therefore, the impact of heat from the LED is small, making it easier to ensure reliability. Because it is in film form, it can be easily adapted to a wide range of screen sizes, from small to large.

[0024] In the present invention, the backlight light source has a wavelength of 400 nm or more and less than 495 nm, or 495 nm or more and less than 600 nm. The emission spectrum is in the wavelength range of 600 nm or less and 780 nm or less. It is preferable that the four peaks have a half-width of 5 nm or more. The wavelength range of 430 nm or more and less than 495 nm is preferably 430 nm or more and less than 470 nm. The wavelength region of 495 nm or more and less than 600 nm is more preferably 510 nm or less. The wavelength range of 600 nm to 780 nm is more preferable. Alternatively, it is 600 nm or more and 750 nm or less, and more preferably, it is 630 nm or more and 700 nm or less. More preferably, the half-width of each peak is 630 nm or more and 680 nm or less. The lower limit of the value range is preferably 10 nm or more, more preferably 15 nm or more, and Preferably, it is 20 nm or more. From the viewpoint of securing an appropriate color gamut, the upper half width of each peak is The limit is preferably 140 nm or less, more preferably 120 nm or less, and even more preferably 100 nm or less. More preferably, the thickness is 80 nm or less, even more preferably, the thickness is 60 nm or less, and even more preferably, the thickness is 80 nm or less. The half-width here is the peak intensity at the wavelength of the peak top. The wavelength range described here is the peak width (nm) at half the intensity. Any combination of the individual upper and lower limits is contemplated. Any combination of the individual upper and lower limits of the range is contemplated. The emission spectrum of the backlight source is, for example, a multi-channel Measurements can be made using a spectrometer such as PMA-12.

[0025] Wavelength range of 400nm or more and less than 495nm, wavelength range of 495nm or more and less than 600nm or in any wavelength region of 600 nm or more and 780 nm or less, If peaks exist, consider the following: Multiple peaks are independent peaks. In some cases, it is preferable that the half-width of the peak with the highest peak intensity is within the above range. Similarly, for other peaks that have an intensity of 70% or more of the highest peak intensity, It is more preferable that the width is within the above range. For an independent peak, the peak with the highest intensity among the multiple peaks is selected. If the half-width can be measured directly, use the half-width. has regions on both the short-wavelength side and the long-wavelength side of the peak where the intensity is half the peak intensity In other words, multiple peaks overlap, and each peak has half the intensity of the other peaks. If no region of intensity exists between the peaks, the peaks are regarded as one peak as a whole. In this case, a peak having a shape in which multiple peaks overlap is the highest peak. The width (nm) of the peak at half the intensity of the peak is defined as the half-width. The point with the highest peak intensity is the peak top. The half-widths, if any, are indicated by double-headed arrows in FIGS.

[0026] In FIG. 1, peaks A and B are peaks on the short wavelength side and the long wavelength side, respectively, starting from the peak. There is a point where the intensity is 1 / 2. Therefore, peaks A and B are independent peaks. In the case of Figure 1, the half-width was evaluated using the width of the double-headed arrow of peak A, which has the highest peak intensity. It is enough to value it.

[0027] In FIG. 2, peak A has two points on the short wavelength side and long wavelength side where the intensity is half of the peak intensity. However, peak B does not have a point on the long wavelength side where the peak intensity is 1 / 2. In this way, peak A and peak B are regarded as one independent peak. For a single independent peak with overlapping peaks, the most When the half-width of a peak with high intensity can be measured directly, the half-width is used as an independent The half-width of the peak is therefore the width of the double-headed arrow in Figure 2. That is the thing.

[0028] In Figure 3, there is no point on the short wavelength side where the peak intensity is half that of the peak A. For QB, there is no point on the long wavelength side where the peak intensity is 1 / 2. Therefore, in Figure 3, As in the case of Figure 2, peaks A and B are regarded as one independent peak. The half-width is indicated by the double-headed arrow.

[0029] In FIG. 4, peak A has two points on the short wavelength side and the long wavelength side where the intensity is half of the peak intensity. However, peak B does not have a point on the long wavelength side where the peak intensity is 1 / 2. Peak A and Peak B are regarded as one independent peak. For an independent peak with a similar shape, the peak with the highest intensity among the multiple peaks is used. If the half-width of the highest peak can be measured directly, the half-width is used. In the case of 4, the half-width is the width indicated by the double-headed arrow.

[0030] 1 to 4 show an example of a wavelength region of 400 nm or more and less than 495 nm, but other wavelength regions are also possible. The same idea applies to the

[0031] Among the multiple peaks, the peak with the highest peak intensity is determined as the peak top. In addition, the wavelength range of 400 nm or more and less than 495 nm, and the wavelength range of 495 nm or more and less than 600 nm The peak with the highest peak intensity in the wavelength region of 600 nm to 780 nm It is preferable that the peaks in the 495n wavelength region and the 495n wavelength region are independent of each other. The peak with the highest peak intensity in the wavelength region of 600 nm or more and less than 600 nm, and the peak with the highest peak intensity in the wavelength region of 600 nm or more The wavelength region between the peak with the highest peak intensity in the wavelength region below 780 nm has a strong peak intensity. The peak with the highest peak intensity in the wavelength range from 600 nm to 780 nm It is preferable in terms of color clarity that there exists an area where the intensity is 1 / 3 or less.

[0032] The emission spectrum of the backlight light source was measured using a multi-channel spectrometer manufactured by Hamamatsu Photonics. Measurements can be made using a spectrometer such as PMA-12.

[0033] As a result of intensive research, the present inventors have discovered that a light source that emits excitation light and a backlight that includes quantum dots The backlight source has a relatively narrow half-width of each peak in the emission spectrum, such as a 3D light source. In the liquid crystal display device, an antireflection layer and / or a low reflection layer are provided as a polarizer protective film. If a polyester film having a specific retardation is used, rainbow spots are suppressed. The present invention has been found to provide a liquid crystal display device and a polarizing plate useful for providing the same. The mechanism by which the occurrence of rainbow-like color spots is suppressed is believed to be as follows.

[0034] When an oriented polyester film is placed on one side of the polarizer, The linearly polarized light emitted from the polarizer changes its polarization state when it passes through the polyester film. One of the factors that change the polarization state is the change in the interface between the air layer and the oriented polyester film. The refractive index difference or the refractive index difference at the interface between the polarizer and the oriented polyester film has an effect. It is possible that linearly polarized light incident on an oriented polyester film passes through each interface. When the light is reflected, a part of it is reflected due to the difference in refractive index between the interfaces. The light conditions change, and this is thought to be one of the causes of the rainbow-like color spots. Therefore, an anti-reflection layer or a low reflection layer is applied to the surface of the oriented polyester film to reduce the surface reflection. By reducing the reflection at the interface between the air layer and the oriented polyester film, the reflection is suppressed and the rainbow is reduced. It is believed that this suppresses color spots.

[0035] As described above, the light source that emits excitation light and the backlight light source that contains quantum dots are representative. The backlight source has a relatively narrow half-width of each peak in the emission spectrum, and the polarizer protection film is By combining a polarizing plate using polyester film as the film, a rainbow-like It is possible to suppress color spots and achieve good visibility.

[0036] The polarizing plate is provided with a polarizer protection film made of a polyester film on at least one side of the polarizer. It is preferable that the polyester film used in the polarizer protective film is laminated. The film preferably has a retardation of 1500 to 30000 nm. If the retardation is within the above range, rainbow spots tend to be more easily reduced, which is preferable. The preferred lower limit of retardation is 3000 nm, the next most preferred lower limit is 3500 nm. A more preferable lower limit is 4000 nm, a further preferable lower limit is 6000 nm, and a further preferable lower limit is 8000 nm. The preferred lower limit is 8000 nm. The preferred upper limit is 30000 nm. Polyester films with retardation become considerably thicker and are not suitable for use as industrial materials. In this document, retardation is not a separate indication. Unless otherwise noted, this refers to in-plane retardation.

[0037] The retardation can also be calculated by measuring the refractive index and thickness in two axial directions. A commercially available automatic birefringence measuring device such as KOBRA-21ADH (Oji Scientific Instruments Co., Ltd.) was used. The refractive index can also be measured using an Abbe refractometer (measurement wavelength 589 nm). It can be calculated by:

[0038] Retardation of polyester film (Re: in-plane retardation) and retardation in the thickness direction The ratio (Re / Rth) of the thermal retardation (Rth) is preferably 0.2 or more, and more preferably 0.3 or more, preferably 0.4 or more, preferably 0.5 or more, more preferably 0.5 or more The retardation in the thickness direction is preferably 0.6 or more. The larger the ratio (Re / Rth), the more isotropic the birefringence becomes, and the more the rainbow-like appearance changes depending on the observation angle. The occurrence of color spots tends to be less likely. The ratio of retardation to thickness retardation (Re / Rth) is 2.0. The upper limit of the ratio of the retardation to the thickness direction retardation (Re / Rth) is preferably 2.0. The thickness direction retardation is the difference between the two birefringences △ when the film is viewed from the thickness direction cross section. It means the average retardation obtained by multiplying Nxz and ΔNyz by the film thickness d.

[0039] In order to suppress rainbow-like color spots, the NZ coefficient of the polyester film is set to 2.5 or less. It is preferable that the ratio is 2.0 or less, more preferably 1.8 or less, and even more preferably 2.0 or less. More preferably, it is 1.6 or less. In a completely uniaxial (uniaxially symmetric) film, NZ The coefficient is 1.0, so the lower limit of the NZ coefficient is 1.0. However, completely uniaxial (uniaxial As the film approaches the orientation direction, the mechanical strength in the direction perpendicular to the orientation direction decreases significantly. It is necessary to pay attention to the trend.

[0040] The NZ coefficient is expressed as |Ny-Nz| / |Ny-Nx|, where Ny is the bending moment along the slow axis. Nx is the refractive index in the direction perpendicular to the slow axis (the refractive index in the fast axis direction), and Nz is the refractive index in the thickness direction. The refractive index is shown in Fig. 1. A molecular orientation meter (MOA-6004, manufactured by Oji Instruments Co., Ltd.) was used. The orientation axis of the film was determined using the above method, and the biaxial refractive index (Ny , Nx, where Ny>Nx, and the refractive index in the thickness direction (Nz) were measured using an Abbe refractometer (Atago The value thus obtained is |N The NZ coefficient can be found by substituting |y-Nz| / |Ny-Nx|.

[0041] In order to further suppress rainbow-like color spots, the Ny-Nx value of the polyester film is It is preferably 0.05 or more, more preferably 0.07 or more, and further preferably 0.08 or more. The upper limit is preferably 0.09 or more, more preferably 0.1 or more. However, in the case of polyethylene terephthalate films, the upper limit is preferably about 1.5. It is nice.

[0042] In a more preferred embodiment of the present invention, the direction parallel to the transmission axis direction of the polarizer constituting the polarizing plate is The refractive index of the polyester film is preferably in the range of 1.53 to 1.62. This suppresses reflection at the interface between the polarizer and the polyester film, and reduces rainbow reflection. If the refractive index exceeds 1.62, the color spots observed from an oblique angle can be suppressed. When the polarizer is rotated, rainbow-like color spots may occur. The refractive index of the film is preferably 1.61 or less, more preferably 1.60 or less. It is preferably 1.59 or less, and more preferably 1.58 or less.

[0043] On the other hand, the lower limit of the refractive index of the polyester film in the direction parallel to the transmission axis of the polarizer is 1 If the refractive index is less than 1.53, the polyester film will not crystallize properly. The properties obtained by stretching, such as dimensional stability, mechanical strength, and chemical resistance, are insufficient. This is not preferable because the refractive index is preferably 1.56 or more, and more preferably 1. 57 or more. Any range combining the upper and lower limits of the refractive indexes described above is assumed. can be.

[0044] The refractive index of the polyester film in the direction parallel to the transmission axis of the polarizer is 1.53 or more. To achieve a range below .62, the polarizer must be aligned with the transmission axis of the polarizer and the polyester film. It is preferable that the fast axis (perpendicular to the slow axis) is parallel. The refractive index in the fast axis direction, which is perpendicular to the slow axis, is increased by the stretching treatment in the film-forming process described below. The fast axis of polyester film can be adjusted to a low value of 1.53 to 1.62. By aligning the direction of the polarizer with the transmission axis of the polarizer, the The refractive index of the ester film can be set to 1.53 to 1.62. The angle between the transmission axis of the polarizer and the fast axis of the polarizer protective film is -15° to 15°. °, preferably -10° to 10°, more preferably -5° to 5°, and even more preferably -3° to 3°, even more preferably from -2° to 2°, and even more preferably from -1° to 1°. In a preferred embodiment, the parallel means substantially parallel. The term "allows for the inevitable misalignment that occurs when laminating the polarizer and the protective film" means that the polarizer and the protective film are laminated together. This means that the transmission axis and the fast axis are parallel to each other to the extent that the slow axis can be measured. For example, it can be measured using a molecular orientation meter (MOA-6004, manufactured by Oji Instruments Co., Ltd.) can be done.

[0045] In other words, the refractive index of the polyester film in the fast axis direction is 1.53 to 1.62. Preferably, the polarizer and the polyester film are laminated so that the transmission axis of the polarizer and the fast axis of the polyester film are approximately parallel to each other. This reduces the refractive index of the polyester film to 1.53 in the direction parallel to the transmission axis of the polarizer. It can be set to 1.62 or more.

[0046] The polarizer protective film made of the above polyester film has an incident light side (light source side) and an outgoing light side. It can be used for both the light side (the viewing side) and the polarizing plate arranged on the incident light side. The polarizer protective film made of the polyester film has a polarizer as a starting point. They may be arranged on the incident light side, on the liquid crystal cell side, or on both sides. It is preferable that the polarizing plate is disposed at least on the incident light side. Regarding the above, the polarizer protective film made of the polyester film is Whether they are placed as points on the liquid crystal side, on the light output side, or on both sides However, it is preferable that the light emitting element is disposed at least on the exit light side.

[0047] The polyester used in polyester film is polyethylene terephthalate or Although polyethylene naphthalate can be used, other copolymer components may be contained. These resins have excellent transparency, thermal and mechanical properties, and are suitable for stretching. Therefore, the retardation can be easily controlled. The intrinsic birefringence of the film is large, and the direction of the fast axis (perpendicular to the slow axis) is changed by stretching the film. The refractive index can be kept low, and the film thickness can be increased relatively easily even if it is thin. Since a large retardation can be obtained, it is the most suitable material.

[0048] In addition, in order to suppress the deterioration of optically functional dyes such as iodine dyes, It is desirable for the thermoplastic film to have a light transmittance of 20% or less at a wavelength of 380 nm. The light transmittance at 0 nm is preferably 15% or less, more preferably 10% or less, and even more preferably 5% or less. When the light transmittance is 20% or less, the optically functional dye is not irradiated with ultraviolet light. The transmittance is measured in a direction perpendicular to the plane of the film. It is determined by spectrophotometer (e.g. Hitachi U-3500 type). can.

[0049] In order to reduce the transmittance of the polyester film to 20% or less at a wavelength of 380 nm, It is desirable to appropriately adjust the type and concentration of the absorbent and the thickness of the film. The ultraviolet absorbing agents used are known substances. The ultraviolet absorbing agents include organic ultraviolet absorbing agents and Although inorganic ultraviolet absorbents are exemplified, organic ultraviolet absorbents are preferred from the viewpoint of transparency. Organic ultraviolet absorbers include benzotriazoles, benzophenones, and cyclic iminoesters. Stereo and combinations thereof are also possible, provided that the absorbance falls within the range specified by the present invention. There is no particular limitation. However, from the viewpoint of durability, benzothazoles, cyclic iminoesters, etc. In the case where two or more kinds of ultraviolet absorbing agents are used in combination, ultraviolet rays having different wavelengths are absorbed. Since the ultraviolet ray absorbing effect can be improved by simultaneously absorbing the ultraviolet ray.

[0050] Benzophenone-based UV absorbers, Benzotriazole-based UV absorbers, Acrylonitrile Examples of the aryl ultraviolet absorbers include 2-[2'-hydroxy-5'-(methacryloyloxy) 2-[2'-hydroxy-5'-phenyl]-2H-benzotriazole -(methacryloyloxyethyl)phenyl]-2H-benzotriazole, 2-[2' -Hydroxy-5'-(methacryloyloxypropyl)phenyl]-2H-benzo Triazole, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2 ',4,4'-Tetrahydroxybenzophenone, 2,4-di-tert-butyl-6- (5-Chlorobenzotriazol-2-yl)phenol, 2-(2'-hydroxy-3 '-tert-Butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2- (5-chloro(2H)-benzotriazol-2-yl)-4-methyl-6-(tert -butyl)phenol, 2,2'-methylenebis(4-(1,1,3,3-tetramethyl butyl)-6-(2H-benzotriazol-2-yl)phenol and the like. Examples of cyclic iminoester-based ultraviolet absorbents include 2,2'-(1,4-phenylene)bis(phenylene)- 4H-3,1-benzoxazinon-4-one, 2-methyl-3,1-benzox 2-Butyl-3,1-benzoxazin-4-one, 2-phenyl- 3,1-benzoxazin-4-one, but is not limited to these. It's not something like that.

[0051] In addition to the ultraviolet absorber, various additives other than the catalyst may be used within a range that does not impair the effects of the present invention. It is also a preferred embodiment to contain the additives. Subparticles, alkali metal compounds, alkaline earth metal compounds, phosphorus compounds, antistatic agents, light resistance agents, flame retardants, heat stabilizers, antioxidants, anti-gelling agents, surfactants, etc. In order to achieve high transparency, it is also preferable that the polyester film does not substantially contain particles. "Substantially no particles" means, for example, in the case of inorganic particles, When inorganic elements are quantified, the amount is 50 ppm or less, preferably 10 ppm or less, and particularly preferably means a content below the detection limit.

[0052] At least one surface of the polyester film, which is a polarizer protective film, is coated with an anti-reflection It is preferable to provide a stop layer and / or a low reflection layer. The surface reflectance of the anti-reflection layer is 2.0%. If the content exceeds 2.0%, rainbow-like color spots are easily visible. The surface reflectance is more preferably 1.6% or less, further preferably 1.2% or less, particularly preferably 1.6% or less. The lower limit of the surface reflectance of the antireflection layer is preferably 1.0% or less. The reflectance can be measured by any method, for example, a spectrophotometer (Island The light reflectance at a wavelength of 550 nm was measured using the UV-3150 manufactured by Tsu Seisakusho. It can be measured from the surface of the side.

[0053] The anti-reflection layer may be a single layer or a multilayer. In the case of a single layer, the anti-reflection layer is made of a polyester film. The thickness of the low refractive index layer made of a material with a lower refractive index than the gyro is set to 1 / 4 wavelength of the light wavelength or an odd number thereof. If the anti-reflection layer is multi-layered, the anti-reflection effect can be obtained. The low refractive index layer and the high refractive index layer are alternately stacked in two or more layers, and the thickness of each layer is appropriately controlled. If necessary, a hard coat layer may be provided between the anti-reflection layers to provide an anti-reflection effect. It is also possible to laminate the layers and to form an antifouling layer on the hard coat layer.

[0054] The anti-reflection layer may have a moth-eye structure. The surface is formed with a concave-convex structure with a pitch smaller than the wavelength. This structure is The aim is to change the sudden and discontinuous change in refractive index in Therefore, by forming a moth-eye structure on the surface, the light on the surface of the film can be The formation of an anti-reflection layer using a moth-eye structure is described in, for example, JP-A-2001- This can be done with reference to 517319.

[0055] The anti-reflection layer can be formed, for example, by applying a vapor deposition method to the surface of the substrate (polyester film). Dry coating method to form an anti-reflective layer by deposition or sputtering method, A wet coating method in which an antireflection coating liquid is applied and dried to form an antireflection layer. The composition of the anti-reflection layer and the method of forming the same are described below. There are no particular limitations on the material as long as it satisfies the above characteristics.

[0056] The low reflection layer may be a known one. For example, a thin film of a metal or oxide may be used. At least one layer is laminated by deposition or sputtering, or one layer of an organic thin film is laminated. The low reflection layer is formed by a method of coating a plurality of layers. A layer having a lower refractive index than the hard coat layer laminated on the polymer film or polyester film. The low reflection layer is preferably coated with a layer of an organic thin film having a surface reflection of 0.1 to 1.0 nm. The ratio is preferably less than 5%, more preferably 4% or less, and even more preferably 3% or less. The lower limit is preferably about 0.8% to 1.0%.

[0057] The anti-reflection layer and / or the low-reflection layer may further be provided with an anti-glare function. In other words, the combination of the anti-reflection layer and the anti-glare layer can further suppress rainbow spots. The combination of a reflective layer and an antiglare layer, or the combination of an antireflection layer, a low reflection layer and an antiglare layer may be used. A combination of a low reflection layer and an antiglare layer is preferred. As the antiglare layer, a known antiglare layer is used. For example, from the viewpoint of suppressing the surface reflection of the film, a polyester film It is preferable that an antiglare layer is laminated on the antiglare layer, and then an antireflection layer or a low reflection layer is laminated on the antiglare layer. .

[0058] When providing an anti-reflection layer or a low-reflection layer, the polyester film is easily adhered to the surface. In this case, in order to suppress interference caused by reflected light, it is preferable to have a bending strength of the easy-adhesion layer. The refractive index is set to be close to the geometric mean of the refractive index of the anti-reflection layer and the refractive index of the polyester film. The refractive index of the adhesive layer can be adjusted by a known method. For example, titanium, germanium, or other metal species can be added to the binder resin. This can be easily adjusted.

[0059] The polyester film is corona-treated and coated to improve adhesion to the polarizer. It is also possible to subject the material to treatment such as firing and / or flame treatment.

[0060] In the present invention, in order to improve adhesion to a polarizer, at least At least one of polyester resin, polyurethane resin or polyacrylic resin on one side It is preferable that the adhesive layer has a main component of the adhesive. The term refers to a component that is 50% by mass or more of the solid components constituting the composition. The coating liquid used is a water-soluble or water-dispersible copolymer polyester resin, an acrylic resin, and a polyurethane. Aqueous coating solutions containing at least one of the above-listed resins are preferred. For example, Patent No. 3567927, Patent No. 3589232, Patent No. 3589 Disclosed in Patent Publication No. 233, Patent Publication No. 3900191, and Patent Publication No. 4150982, etc. The water-soluble or water-dispersible copolymer polyester resin solution, acrylic resin solution, or polyurethane Examples include ethyl acetate resin solutions.

[0061] The adhesive layer is formed by applying the coating liquid to one or both sides of a uniaxially stretched film in the longitudinal direction, The film is dried at 100 to 150°C and then stretched in the transverse direction to obtain the final product. The coating weight of the layer is 0.05 to 0.20 g / m 2 It is preferable to control the coating amount to 0.0. 5g / m 2 If it is less than this, the adhesion to the obtained polarizer may be insufficient. Coating amount: 0.20g / m 2 If it exceeds this value, blocking resistance may decrease. When providing an easy-adhesion layer on both sides of the sterilized film, the coating amount of the easy-adhesion layer on both sides should be the same. These values ​​may be different from each other and can be set independently within the above ranges.

[0062] It is preferable to add particles to the adhesive layer in order to impart slipperiness. It is preferable to use particles with a diameter of 2 μm or less. If the average particle size of the particles exceeds 2 μm, the particles The particles contained in the adhesive layer are, for example, tin oxide. Talc, barium sulfate, calcium carbonate, calcium sulfate, silica, alumina, talc, calcium Olin, clay, calcium phosphate, mica, hectorite, zirconia, tungsten oxide Inorganic particles such as fluorine, lithium fluoride, and calcium fluoride, as well as styrene-based, acrylic-based, Examples of the organic polymer particles include melamine-based, benzoguanamine-based, and silicone-based particles. These may be added to the adhesive layer alone or in combination of two or more. It is also possible.

[0063] The coating liquid can be applied by a known method. Birth roll coat method, gravure coat method, kiss coat method, roll brush method, Spray coating method, air knife coating method, wire bar coating method, and pipe doctor method These methods can be carried out alone or in combination.

[0064] The average particle size of the above particles is measured by the following method. SEM) and magnification was set so that the smallest particle was 2-5 mm in size. The maximum diameter (the distance between the two most distant points) of 300 to 500 particles is measured and the average value is calculated. The average particle size is taken as the average particle size.

[0065] The polyester film used as the polarizer protection film is a typical polyester film. For example, a polyester resin may be melted and The non-oriented polyester extruded into a sheet is heated to a temperature above the glass transition temperature. After stretching in the machine direction using the speed difference of the rolls, it is stretched in the cross direction by a tenter and then heat-treated. The following method is exemplified.

[0066] The polyester film used in the present invention may be either a uniaxially oriented film or a biaxially oriented film. It may be a room.

[0067] The film-forming conditions for the polyester film are specifically described as follows: longitudinal stretching temperature, transverse stretching temperature The temperature is preferably 80 to 130° C., and particularly preferably 90 to 120° C. The slow axis is in the TD direction. In order to orient the film so as to obtain the above-mentioned orientation, the longitudinal stretching ratio is preferably 1.0 to 3.5 times, and particularly The transverse stretching ratio is preferably 1.0 to 3.0 times. The transverse stretching ratio is preferably 2.5 to 6.0 times. The thickness is preferably 3.0 to 5.5 times, and more preferably 3.0 to 5.5 times. For orientation, the longitudinal stretching ratio is preferably 2.5 to 6.0 times, and particularly preferably 3.0 to 6.0 times. The transverse stretching ratio is preferably 1.0 to 3.5 times, and more preferably 1. .0 to 3.0 times.

[0068] Setting the stretching temperature low also reduces the refractive index in the fast axis direction of the polyester film. This is a favorable measure for increasing the retardation. The temperature is preferably from 100 to 250°C, and particularly preferably from 180 to 245°C.

[0069] In order to suppress the variation in retardation, it is preferable that the film has small unevenness in thickness. The stretching temperature and stretching ratio have a large effect on the thickness unevenness of the film. It is preferable to optimize the film formation conditions in order to reduce the retardation. In order to prevent this, if the longitudinal stretching ratio is reduced, the longitudinal thickness unevenness may become large. Since there is a region where the stretch ratio becomes extremely poor within a certain range, if this range is excluded, It is preferable to set the film forming conditions by using a roller.

[0070] The thickness unevenness of the polyester film is preferably 5.0% or less, and more preferably 4.5% or less. More preferably, the ratio is 4.0% or less, and even more preferably, the ratio is 3.0% or less. The thickness unevenness of the film can be measured as follows. A tape-shaped film sample (3 m) was taken and was then inserted into an electronic printer manufactured by Seiko EM Co., Ltd. Using a micrometer, Millitron 1240, measure the thickness at 100 points at 1 cm intervals. The maximum thickness (dmax), minimum thickness (dmin), and average thickness (d) were calculated from the measured values, and the following formula was used: The thickness unevenness (%) is calculated by the following formula: It is preferable to carry out the measurement three times and calculate the average value. Thickness unevenness (%) = ((dmax-dmin) / d) x 100 As mentioned above, in order to control the retardation of polyester film within a specific range, This can be achieved by appropriately setting the stretching ratio, stretching temperature, and film thickness. For example, the higher the stretching ratio, the lower the stretching temperature, and the thicker the film, the higher the retardation. Conversely, the lower the stretching ratio and the higher the stretching temperature, the easier it is to obtain a film The thinner the film, the easier it is to obtain low retardation. However, if the film is made thicker, Therefore, the film thickness is appropriately set within the range described below. In addition to controlling the retardation, it is also desirable to take into account the physical properties required for processing. It is preferable to set the final film formation conditions based on the above.

[0071] The thickness of the polyester film is not limited, but is preferably in the range of 15 to 300 μm. More preferably, the thickness is in the range of 15 to 200 μm. Theoretically, it is possible to obtain a retardation of 1500 nm or more. In the latter case, the anisotropy of the mechanical properties of the film becomes significant, making it prone to tearing and ripping, and is therefore an industrial material. The practical use of the material is significantly reduced. A particularly preferable lower limit of the thickness is 25 μm. The upper limit of the thickness of the polarizer protection film is 300 μm. If it exceeds this limit, the thickness of the polarizing plate will become too thick. From the viewpoint of practical use as a polarizer protective film, the upper limit of the thickness is 2 The upper limit of the thickness is preferably 100 μm, which is approximately the same as that of a general TAC film. In order to control the retardation within the range of the present invention even in the above thickness range, In particular, the polyester used as the film substrate is preferably polyethylene terephthalate. .

[0072] In addition, the method of blending the ultraviolet absorbing agent into the polyester film may be a known method. For example, a combination of a UV absorber and a polymer that have been dried in advance using a kneading extruder may be used. The raw materials for the film are blended to prepare a master batch, and the desired mass is added at the time of film production. The blending can be carried out by, for example, mixing the turbatch with the polymer raw material.

[0073] At this time, the concentration of the UV absorber in the master batch is set to be uniformly dispersed and economical. In order to effectively mix the components, the concentration is preferably 5 to 30% by mass. The conditions for the extrusion were as follows: a kneading extruder was used; the extrusion temperature was set to 290 It is preferable to extrude the mixture at a temperature of 290°C or less for 1 to 15 minutes. The weight loss is large, and the viscosity of the master batch also decreases significantly. In this case, it becomes difficult to mix the UV absorber uniformly. And / or an antistatic agent may be added.

[0074] The polyester film is made of at least three layers, and the middle layer of the film is made of ultraviolet light. It is preferable to add a UV absorber to the intermediate layer. Specifically, it can be prepared as follows: For the outer layer, polyester pellets are used. Germany, master batch containing UV absorbent and polyester pellets for the middle layer The mixture is mixed in a predetermined ratio, dried, and then fed to a known melt lamination extruder and slit-shaped die. The mixture is extruded from the mold into a sheet, and cooled and solidified on a casting roll to obtain an unstretched film. i.e., two or more extruders, three-layer manifolds or junction blocks (e.g., corner The film layers that make up the two outer layers and the intermediate layer are constructed using a junction block with a mold junction. The three layers are then extruded from the die and cooled by a casting roll. In this invention, the raw polyester film is treated to remove the optical defects. In order to remove foreign matter contained in the ter, high-precision filtration is performed during melt extrusion. Preferred. Filter particle size of filter media used for high-precision filtration of molten resin (initial filtration efficiency 95%) If the filtering particle size of the filter medium exceeds 15 μm, it is preferable that the filtering particle size is 20 μm or less. It is easy for the removal of foreign matter from above to be insufficient. EXAMPLES

[0075] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the above, and may be modified as necessary within the scope of the present invention. It is also possible to use the above-mentioned method, and all of these methods are included in the technical scope of the present invention. The methods for evaluating physical properties in the examples are as follows.

[0076] (1) Refractive index of polyester film Using a molecular orientation meter (Oji Instruments, MOA-6004 molecular orientation meter), Determine the slow axis direction of the film and cut it into a 4 cm x 2 cm rectangle so that the slow axis direction is parallel to the long side. The sample was cut into a shape and used as a measurement sample. The refractive index of the two perpendicular axes ( Refractive index in the slow axis direction: Ny, fast axis (refractive index in the direction perpendicular to the slow axis direction): Nx), and The refractive index in the thickness direction (Nz) was measured using an Abbe refractometer (Atago Co., Ltd., NAR-4T, measuring wavelength 5 89 nm).

[0077] (2) Retardation (Re) Retardation is the anisotropy of the refractive index of two perpendicular axes on the film (△Nxy = |Nx A parameter defined by the product of the film thickness d (nm) and the film thickness (△Nxy×d) It is a measure of optical isotropy and anisotropy. The biaxial refractive index anisotropy (△Nxy) is The absolute value of the difference in refractive index between the two axes (|Nx-Ny|) is calculated by the method (1) above. The anisotropy (△Nxy) of the film was calculated. The film thickness d (nm) was measured using an electric micrometer. (Fine Leaf, Millitron 1245D) was used for measurement, and the units were converted to nm. From the product (△Nxy × d) of the refractive index anisotropy (△Nxy) and the film thickness d (nm), , and retardation (Re) were calculated.

[0078] (3) Thickness retardation (Rth) The thickness retardation is the two birefringences △N when viewed from the cross section of the film thickness direction. xz (=|Nx-Nz|) and △Nyz (=|Ny-Nz|) are the film thicknesses, respectively. This is a parameter that indicates the average retardation obtained by multiplying by d. Calculate Nx, Ny, Nz and film thickness d (nm) in the same manner as in the measurement, and (△Nxz × d The average value of (△Nyz×d) was calculated to obtain the thickness retardation (Rth). .

[0079] (4) NZ coefficient The values ​​of Ny, Nx, and Nz obtained in (1) above are calculated using the formula (NZ = |Ny-Nz| / |N y-Nx|) to obtain the value of the NZ coefficient.

[0080] (5) Measurement of the emission spectrum of the backlight light source The liquid crystal display device used in each example is a BRAVIA KDL-40W manufactured by Sony. 920A (Liquid crystal display having a light source emitting excitation light and a backlight light source including quantum dots The emission spectrum of the backlight source of this liquid crystal display device was measured by a Hamamatsu Photonics When measured using a multichannel spectrometer PMA-12 manufactured by Cosmos, The emission spectrum was observed to have peaks at 528 nm and 630 nm. The half-width of the peak was 17 nm to 34 nm. was set to 20 msec.

[0081] (6)Reflectance Using a spectrophotometer (Shimadzu Corporation, UV-3150), 5-degree reflection at a wavelength of 550 nm was performed. The reflectance was measured from the surface of the anti-reflection layer side (or the low reflection layer side). Apply black marker to the side opposite the anti-reflection layer (or low-reflection layer) of the , and measure with black vinyl tape (Kyowa Vinyl Tape HF-737, width 50 mm) It was determined.

[0082] (7) Iridescence observation The liquid crystal display device obtained in each Example was visually observed in a dark place from the front and from an oblique direction. The occurrence of the above phenomenon was judged as follows. Here, the oblique direction is the direction of the image of the liquid crystal display device. This means a range of 30 to 60 degrees from the normal direction of the surface.

[0083] ○: No rainbow spots observed △: Slight rainbow spots observed ×: Iridescence observed ××: Iridescence is significantly observed

[0084] (Production Example 1-Polyester A) When the temperature of the esterification reactor reached 200°C, 86.4 parts by mass of terephthalic acid was added. and 64.6 parts by mass of ethylene glycol were added, and ammonium trioxide was added as a catalyst while stirring. 0.017 parts by mass of thimon, 0.064 parts by mass of magnesium acetate tetrahydrate, and triethyl 0.16 parts by mass of amine was charged. Then, the pressure was increased and the temperature was raised to 0.34 MPa and 2 After carrying out the pressurized esterification reaction at 40°C, the esterification reactor was returned to normal pressure and phosphoric acid was added. 0.014 parts by mass of trimethyl phosphate was added. After 15 minutes, the mixture was dispersed using a high-pressure disperser. After 10 minutes, the obtained esterification reaction product was transferred to a polycondensation reactor and polycondensed under reduced pressure at 280°C. The reaction was carried out.

[0085] After the polycondensation reaction is complete, the mixture is filtered using a Naslon filter with a 95% cutoff diameter of 5 μm. Cooling water extruded in strand form from a nozzle and pre-filtered (pore size: 1 μm or less) The resulting polyethylene terephthalate was cooled and solidified using a tungsten carbide (Teflon) sintering machine and cut into pellets. The intrinsic viscosity of the resin (A) is 0.62 dl / g, and the inert particles and the internal precipitate particles are substantially (Hereinafter referred to as PET(A)).

[0086] (Production Example 2 - Polyester B) The dried UV absorber (2,2'-(1,4-phenylene)bis(4H-3,1-phenylene) 10 parts by weight of oxazinone-4-one, 10 parts by weight of particle-free PET (A) (intrinsic viscosity 0.62 dl / g) 90 parts by mass were mixed and extruded in a kneading extruder to obtain a polypropylene containing an ultraviolet absorbing agent. Ethylene terephthalate resin (B) was obtained (hereinafter referred to as PET (B)).

[0087] (Production Example 3 - Preparation of Adhesion Modifier Coating Solution) By carrying out an ester exchange reaction and a polycondensation reaction in a conventional manner, a dicarboxylic acid component (di (based on the total carboxylic acid components) 46 mol% terephthalic acid, 46 mol% isophthalic acid, and 8 mol% sodium 5-sulfonatoisophthalate, as glycol component (glycol component (based on the total amount) 50 mol % ethylene glycol and 50 mol % neopentyl glycol % composition, a water-dispersible sulfonate metal salt group-containing copolymer polyester resin was prepared. , 51.4 parts by weight of water, 38 parts by weight of isopropyl alcohol, 5 parts by weight of n-butyl cellosolve After mixing 0.06 parts by mass of the mixture and 0.06 parts by mass of a nonionic surfactant, heat and stir until the temperature reaches 77°C. 5 parts by mass of the water-dispersible sulfonate metal salt group-containing copolymer polyester resin was added, and the resin After stirring until no lumps remain, the resin water dispersion is cooled to room temperature and the solids concentration is 5 A homogeneous water-dispersible copolymer polyester resin solution having a concentration of 0.0 mass% was obtained. 3 parts by mass of a copolymer (manufactured by Fuji Silysia Co., Ltd., Silisia 310) was dispersed in 50 parts by mass of water. Then, 99.46 parts by mass of the water-dispersible copolymer polyester resin solution was mixed with Silicea 310 to obtain a water-dispersible copolymer polyester resin solution. Add 0.54 parts by mass of the dispersion liquid, add 20 parts by mass of water while stirring, and prepare an adhesive modification coating liquid. Got it.

[0088] (Production Example 4 - Preparation of high refractive index coating agent) Methyl methacrylate 80 parts, methacrylic acid 20 parts, azoisobutyronitrile 1 part 200 parts of isopropyl alcohol was charged into a reaction vessel, and the mixture was reacted at 80°C for 7 hours under a nitrogen atmosphere. The reaction gave an isopropyl alcohol solution of a polymer having a weight average molecular weight of 30,000. The resulting polymer solution was further diluted with isopropyl alcohol to a solid content of 5%, and the acrylic The acrylic resin solution B was then mixed with the following components to obtain a mixture of acrylic resin solution B and acrylic resin solution B. A coating liquid for forming a high refractive index layer was obtained.

[0089] Acrylic resin solution B 5 parts by weight Bisphenol A diglycidyl ether 0.25 parts by weight Titanium oxide particles with an average particle size of 20 nm: 0.5 parts by weight Triphenylphosphine 0.05 parts by mass 14.25 parts by weight of isopropyl alcohol

[0090] (Production Example 5 - Preparation of low refractive index coating agent) 2,2,2-trifluoroethyl acrylate (45 parts by mass), perfluorooctyl Ethyl acrylate (45 parts by mass), acrylic acid (10 parts by mass), azoisobutyronitrile A reaction vessel was charged with ethanol (1.5 parts by mass) and methyl ethyl ketone (200 parts by mass), and the mixture was placed in a nitrogen atmosphere. The reaction was carried out at 80°C for 7 hours under atmospheric pressure to obtain a polymer with a weight average molecular weight of 20,000. The resulting polymer solution was diluted with methyl ethyl ketone to a solids concentration of 5 mass %. % to obtain fluoropolymer solution C. The obtained fluoropolymer solution C was diluted with the following The components were mixed in this manner to obtain a coating liquid for forming a low refractive index layer.

[0091] Fluoropolymer solution C 4 4 parts by mass 1,10-bis(2,3-epoxypropoxy) - 2,2,3,3,4,4,5,5,6,6,7,7 , 8,8,9,9 - Hexadecafluorodecane (Kyoeisha Chemical, Fluorite FE-16) 1 part by mass Triphenylphosphine 0.1 parts by mass Methyl ethyl ketone 19 parts by weight

[0092] (Production Example 6 - Preparation of Antiglare Layer Coating Agent-1) Unsaturated double bond-containing acrylic copolymer Cyclomer P ACA-Z250 (Daicel Chemical Industry Co., Ltd.) (49 parts by mass), cellulose acetate propionate CAP482- 20 (number average molecular weight 75,000) (manufactured by Eastman Chemical Company) (3 parts by mass), acrylic Monomer AYARAD DPHA (manufactured by Nippon Kayaku Co., Ltd.) (49 parts by weight), acrylic-styrene copolymer (average particle size 4.0 μm) (manufactured by Sekisui Chemical Co., Ltd.) (2 parts by mass), and Irga Cure 184 (BASF) (10 parts by mass) was added to the methacrylate so that the solid content was 35% by mass. Add the coating solution for forming the antiglare layer to a mixed solvent of ethyl ethyl ketone:1-butanol = 3:1. Got it.

[0093] (Production Example 7 - Preparation of Antiglare Layer Coating Agent-2) Unsaturated double bond-containing acrylic copolymer Cyclomer P ACA-Z250 (Daicel Chemical Industry Co., Ltd.) (49 parts by mass), cellulose acetate propionate CAP482- 0.5 (number average molecular weight 25,000) (manufactured by Eastman Chemical Co.) (3 parts by weight), acrylic Monomer AYARAD DPHA (manufactured by Nippon Kayaku Co., Ltd.) (49 parts by mass), acrylic-styrene Polyethylene copolymer (average particle size 4.0 μm) (manufactured by Sekisui Chemical Co., Ltd.) (4 parts by mass), and The solid content of Gacure 184 (BASF) (10 parts by mass) was adjusted to 35% by mass. In addition to a mixed solvent of methyl ethyl ketone:1-butanol=3:1, a coating solution for forming an anti-glare layer obtained.

[0094] (Production Example 8 - Preparation of Antiglare Layer Coating Agent-3) Unsaturated double bond-containing acrylic copolymer Cyclomer P ACA-Z250 (Daicel Chemical Industry Co., Ltd.) (49 parts by mass), cellulose acetate propionate CAP482- 0.2 (number average molecular weight 15,000) (manufactured by Eastman Chemical Co.) (3 parts by mass), acrylic Monomer AYARAD DPHA (manufactured by Nippon Kayaku Co., Ltd.) (49 parts by mass), acrylic-styrene Ren copolymer (average particle size 4.0 μm) (manufactured by Sekisui Plastics Co., Ltd.) (2 parts by mass), Irugaki Methylure 184 (BASF) (10 parts by mass) was added to make the solid content 35% by mass. Add to a mixed solvent of ethyl ethyl ketone:1-butanol = 3:1 to obtain a coating solution for forming an antiglare layer. Ta.

[0095] (Polarizer protection film 1) 90 mass of particle-free PET(A) resin pellets as raw material for the intermediate layer of the base film 10 parts by mass of PET(B) resin pellets containing 10 parts by mass of PET and 10 parts by mass of UV absorber were cooled to 135°C for 6 hours. After drying under pressure (1 Torr), the mixture was fed to extruder 2 (for intermediate layer II) and PET(A ) was dried by a conventional method and fed to extruder 1 (for outer layer I and outer layer III), The two polymers were dissolved at 85°C. Each of them was filtered through a stainless steel sintered filter medium (nominal filtration The filter is then stacked in a two-type, three-layer merging block, and the filter is then cooled by a nozzle. After extruding it into a sheet, it was cast at a surface temperature of 30°C using an electrostatic casting method. The film was then wound around a rolling drum and cooled to solidify, forming an unstretched film. The extrusion rates of the extruders were adjusted so that the thickness ratio of the III layers was 10:80:10. .

[0096] Next, the unstretched PET film was coated on both sides with the reverse roll method, with the amount of coating after drying being 0.08g / m 2 After applying the adhesiveness modifying coating solution, the adhesiveness modifying coating solution was heated at 80° C. for 20 seconds. Dry.

[0097] The unstretched film on which this coating layer was formed was introduced into a tenter stretching machine, and the ends of the film were While being held by a grip, the film was introduced into a hot air zone at 125°C and stretched 4.0 times in the width direction. Next, while maintaining the width stretched in the width direction, it is treated at a temperature of 225°C for 10 seconds, and then The film is stretched uniaxially in the axial direction by 3.0% relaxation, resulting in a film thickness of approximately 100 μm. obtained.

[0098] The coating solution for forming a high refractive index layer is applied to one of the coating surfaces of the uniaxially stretched PET film. The coating was dried at 150° C. for 2 minutes to form a high refractive index layer having a thickness of 0.1 μm. The coating solution for forming the low refractive index layer obtained by the above method is applied onto the substrate, and dried at 150° C. for 2 minutes. A low refractive index layer having a thickness of 0.1 μm is formed, and a polarizer protective film 1 having an antireflection layer laminated thereon is formed. Got it.

[0099] (Polarizer protection film 2) Polarizer protection film 1 except that the line speed was changed to change the thickness of the unstretched film. The film was formed in the same manner as in Example 1, and an anti-reflection layer was laminated on the film to obtain a polarizer protection film having a thickness of about 80 μm. Film 2 was obtained.

[0100] (Polarizer protection film 3) Polarizer protection film 1 except that the line speed was changed to change the thickness of the unstretched film. The film was formed in the same manner as in Example 1, and an anti-reflection layer was laminated on the film to obtain a polarizer protection film having a thickness of about 60 μm. Film 3 was obtained.

[0101] (Polarizer protection film 4) Polarizer protection film 1 except that the line speed was changed to change the thickness of the unstretched film. The film was formed in the same manner as in Example 1, and an anti-reflection layer was laminated on the film to obtain a polarizer protection film having a thickness of about 40 μm. Film 4 was obtained.

[0102] (Polarizer protection film 5) An unstretched film prepared in the same manner as the polarizer protective film 1 was heated and The material is heated to 105°C using a group of rolls and an infrared heater, and then run through a group of rolls with different peripheral speeds. After stretching 3.3 times in the machine direction, it is introduced into a hot air zone at a temperature of 130°C and stretched 4.0 times in the width direction. An anti-reflection layer was laminated on the polarizer protection film 1 in the same manner as in the polarizer protection film 1. The film had a thickness of about 30 mm. A polarizer protective film 5 having a thickness of 1.0 μm was obtained.

[0103] (Polarizer protection film 6) The film was prepared in the same manner as the polarizer protective film 1, except that no anti-reflection layer was provided. A polarizer protective film 6 having a film thickness of about 100 μm was obtained.

[0104] (Polarizer protection film 7) A polarizer protective film was prepared in the same manner as polarizer protective film 2, except that no anti-reflection layer was provided. On one side of the photon protection film, apply an antiglare layer coat so that the thickness after curing is 8 μm. The coating agent-1 was applied and dried in an oven at 80℃ for 60 seconds. Then, the coating agent-1 was applied to the surface of the substrate. Fusion UV Systems Japan, light source H bulb) was used, and the exposure dose was 300mJ / cm 2 The antiglare layer was laminated by irradiating ultraviolet light at 1000 nm. Then, a polarizer protection film was applied on the antiglare layer. An antireflection layer was laminated in the same manner as in Example 1 to obtain a polarizer protective film 7.

[0105] (Polarizer protection film 8) A polarizer protective film was prepared in the same manner as the polarizer protective film 3, except that no anti-reflection layer was provided. An antiglare layer and a reflective layer are formed on one of the coating surfaces of the polarizer protection film in the same manner as the polarizer protection film 7. A polarizer protective film 8 was obtained by laminating an anti-reflection layer thereon.

[0106] (Polarizer protection film 9) A polarizer protective film was prepared in the same manner as polarizer protective film 4, except that no anti-reflection layer was provided. On one side of the photon protection film, apply an antiglare layer coat so that the thickness after curing is 8 μm. The coating agent-2 was applied and dried in an oven at 80℃ for 60 seconds. Then, the coating agent-2 was applied to the surface of the substrate. Fusion UV Systems Japan, light source H bulb) was used, and the exposure dose was 300mJ / cm 2The antiglare layer was laminated by irradiating ultraviolet light at 1000 nm. Then, a polarizer protection film was applied on the antiglare layer. An antireflection layer was laminated in the same manner as in Example 1 to obtain a polarizer protective film 9.

[0107] (Polarizer protection film 10) A polarizer protective film was prepared in the same manner as Polarizer Protective Film 5, except that no anti-reflection layer was provided. An antiglare layer is laminated on one of the coated surfaces of the polarizer protection film in the same manner as the polarizer protection film 7. Thus, a polarizer protective film 10 was obtained (without laminating an antireflection layer).

[0108] (Polarizer protection film 11) A polarizer protective film was prepared in the same manner as polarizer protective film 1, except that no anti-reflection layer was provided. On one side of the photon protection film, apply an antiglare layer coat so that the thickness after curing is 8 μm. The coating agent-3 was applied and dried in an oven at 80℃ for 60 seconds. Then, the coating agent-3 was applied and dried in an oven at 80℃ for 60 seconds. Fusion UV Systems Japan, light source H bulb) was used, and the exposure dose was 300mJ / cm 2 The film was irradiated with ultraviolet light at 400 nm to obtain a polarizer protective film 11 having an antiglare layer laminated thereon.

[0109] (Polarizer protection film 12) A polarizer protective film was prepared in the same manner as polarizer protective film 2, except that no anti-reflection layer was provided. On one side of the photon protection film, apply an antiglare layer coat so that the thickness after curing is 8 μm. The coating agent-1 was applied and dried in an oven at 80℃ for 60 seconds. Then, the coating agent-1 was applied to the surface of the substrate. Fusion UV Systems Japan, light source H bulb) was used, and the exposure dose was 300mJ / cm 2 The antiglare layer was laminated by irradiating ultraviolet light at 1000 nm. Then, a polarizer protection film was applied on the antiglare layer. A low refractive index layer was laminated in the same manner as in Example 1. In this way, a low reflection layer was laminated on the antiglare layer. A polarizer protective film 12 was obtained.

[0110] Using the polarizer protective films 1 to 12, liquid crystal displays were produced as described below.

[0111] Example 1 A polarizer protection film 1 is attached to one side of a polarizer made of PVA and iodine, so that the transmission axis of the polarizer is aligned with the filter. The film is attached so that its fast axis is perpendicular to the substrate, and a TAC film (Fujifilm) is attached to the opposite side. A polarizing plate 1 was prepared by attaching a polarizer protection film (manufactured by Epson Corporation, thickness 80 μm). A polarizer was laminated on the surface of the film that did not have an anti-reflection layer to create a polarizing plate. BRAVIA KDL-40W920A (a light source that emits excitation light and quantum dots) manufactured by Y company The polarizing plate on the viewing side of the liquid crystal display device having a backlight source including a polyester film The polarizing plate 1 is replaced with the polarizing plate 1 so that the film is on the opposite side (distal) to the liquid crystal, and a liquid crystal display device is manufactured. The direction of the transmission axis of the polarizing plate 1 was the same as that of the polarizing plate before the replacement. It was replaced as follows.

[0112] Example 2 The same procedure as in Example 1 was repeated except that the polarizer protective film 1 was replaced with the polarizer protective film 2. A liquid crystal display device was fabricated.

[0113] Example 3 The same procedure as in Example 1 was repeated except that the polarizer protective film 1 was replaced with the polarizer protective film 3. A liquid crystal display device was fabricated.

[0114] Example 4 The same procedure as in Example 1 was repeated, except that the polarizer protective film 1 was replaced with the polarizer protective film 4. A liquid crystal display device was fabricated.

[0115] Example 5 A polarizer protective film 4 is used instead of the polarizer protective film 1, and its fast axis is the transmission axis of the polarizer. A liquid crystal display device was produced in the same manner as in Example 1, except that the film was attached so as to be parallel to the axis. .

[0116] Example 6 The same procedure as in Example 1 was repeated, except that the polarizer protective film 1 was replaced with the polarizer protective film 7. A liquid crystal display device was fabricated.

[0117] Example 7 The same procedure as in Example 1 was repeated except that the polarizer protective film 1 was replaced with the polarizer protective film 8. A liquid crystal display device was fabricated.

[0118] Example 8 The same procedure as in Example 1 was repeated, except that the polarizer protective film 1 was replaced with the polarizer protective film 9. A liquid crystal display device was fabricated.

[0119] Example 9 The same procedure as in Example 1 was repeated except that the polarizer protective film 1 was replaced with the polarizer protective film 12. A liquid crystal display device was fabricated.

[0120] Comparative Example 1 The same procedure as in Example 1 was repeated except that the polarizer protective film 1 was replaced with the polarizer protective film 5. A liquid crystal display device was fabricated.

[0121] Comparative Example 2 The same procedure as in Example 1 was repeated except that the polarizer protective film 1 was replaced with the polarizer protective film 6. A liquid crystal display device was fabricated.

[0122] Comparative Example 3 The same procedure as in Example 1 was repeated except that the polarizer protective film 1 was replaced with the polarizer protective film 10. A liquid crystal display device was fabricated.

[0123] Comparative Example 4 The same procedure as in Example 1 was repeated except that the polarizer protective film 1 was replaced with the polarizer protective film 11. A liquid crystal display device was fabricated.

[0124] The liquid crystal display devices obtained in the respective Examples were subjected to measurement of rainbow spots, and the results are shown in Table 1 below.

[0125] [Table 1] [Industrial Applicability]

[0126] The liquid crystal display device and the polarizing plate of the present invention have a significant reduction in the occurrence of rainbow-like color spots at any angle. This will ensure good visibility with minimal disturbance, making a significant contribution to the industrial sector.

Claims

1. A liquid crystal display device having a backlight source, two polarizing plates, and a liquid crystal cell disposed between the two polarizing plates, The backlight light source includes a light source that emits excitation light and quantum dots, At least one of the polarizing plates has a polyester film laminated on at least one surface of a polarizer such that an angle between a transmission axis of the polarizer and a fast axis of the polyester film is −15 degrees to 15 degrees; The polyester film has an in-plane retardation of 6000 nm or more and 30000 nm or less, A liquid crystal display device in which an anti-reflection layer and / or a low-reflection layer is laminated on at least one surface of the polyester film (however, excluding liquid crystal display devices having a polarizing plate in which a polyester film having a hard coat layer laminated thereon, the polyester film having an in-plane retardation of 8000 nm or more, a difference (nx-ny) between a refractive index (nx) in a slow axis direction in which the refractive index is large and a refractive index (ny) in a fast axis direction perpendicular to the slow axis direction is 0.07 to 0.20, and the refractive index (nh) of the hard coat layer, and the refractive index (nx) in the slow axis direction and the refractive index (ny) in the fast axis direction of the polyester film satisfy the relationship ny<nh<nx).

2. A liquid crystal display device having a backlight source, two polarizing plates, and a liquid crystal cell disposed between the two polarizing plates, the backlight light source has an emission spectrum having peak tops in the wavelength regions of 400 nm or more and less than 495 nm, 495 nm or more and less than 600 nm, and 600 nm or more and 780 nm or less, and a half-value width of each peak is 5 nm or more and 80 nm or less, At least one of the polarizing plates has a polyester film laminated on at least one surface of a polarizer such that an angle between a transmission axis of the polarizer and a fast axis of the polyester film is −15 degrees to 15 degrees; The polyester film has an in-plane retardation of 6000 nm or more and 30000 nm or less, A liquid crystal display device in which an anti-reflection layer and / or a low-reflection layer is laminated on at least one surface of the polyester film (however, excluding liquid crystal display devices having a polarizing plate in which a polyester film having a hard coat layer laminated thereon, the polyester film having an in-plane retardation of 8000 nm or more, a difference (nx-ny) between a refractive index (nx) in a slow axis direction in which the refractive index is large and a refractive index (ny) in a fast axis direction perpendicular to the slow axis direction is 0.07 to 0.20, and the refractive index (nh) of the hard coat layer, and the refractive index (nx) in the slow axis direction and the refractive index (ny) in the fast axis direction of the polyester film satisfy the relationship ny<nh<nx).

3. 3. The liquid crystal display device according to claim 2, wherein the backlight light source has emission spectrum peak tops in the wavelength regions of 400 nm or more and less than 495 nm, 495 nm or more and less than 600 nm, and 600 nm or more and 750 nm or less, and the half width of each peak is 5 nm or more and 80 nm or less.

4. 4. The liquid crystal display device according to claim 1, wherein the antireflection layer has a surface reflectance of 2.0% or less at a wavelength of 550 nm.

5. 5. The liquid crystal display device according to claim 1, wherein the polyester film has a ratio (Re / Rth) of retardation (Re) to retardation in a thickness direction (Rth) of 0.2 or more and 2.0 or less.

6. 6. The liquid crystal display device according to claim 1, further comprising another layer between the antireflection layer and / or the low reflection layer and the polyester film.

7. 6. The liquid crystal display device according to claim 1, further comprising an antiglare layer between the antireflection layer and / or low reflection layer and the polyester film.

Citation Information

Patent Citations

  • JP1975051328A

  • Optical film, polarizing plate using the same, method for producing the same and liquid crystal display

    JP2002116320A

  • Polarizing plate and its manufacturing method, and liquid crystal display device using the same

    JP2004205773A

  • Polarizing plate protective film, and polarizing plate and liquid crystal display device using the same,

    JP2004219620A

  • Polarizing plate protection film, polarizing plate and liquid crystal display apparatus using same

    JP2009014886A