Porous electrode-supported electrolyte membrane and method for producing the same
The porous electrode-supported electrolyte membrane addresses carbon dioxide reduction limitations by enhancing diffusion and preventing membrane swelling, thereby improving efficiency and longevity.
Patent Information
- Application Number
- JP2023522159
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-21
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-05-21
AI Technical Summary
Existing carbon dioxide reduction technologies face limitations in the concentration and diffusion of carbon dioxide due to the use of gas phase versus aqueous phase methods, leading to reduced efficiency and swelling of electrolyte membranes, which compromises the carbon dioxide reduction reaction.
A porous electrode-supported electrolyte membrane is developed with a porous reduction electrode bonded to an electrolyte membrane, having an average pore diameter of 1 μm or more, and thermocompression bonded to prevent swelling and enhance carbon dioxide diffusion.
The porous electrode-supported electrolyte membrane improves carbon dioxide reduction efficiency by reducing diffusion resistance and preventing membrane swelling, maintaining high efficiency over time.
Smart Images

Figure 0007594215000002 
Figure 0007594215000003 
Figure 0007594215000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a porous electrode-supported electrolyte membrane and a method for producing a porous electrode-supported electrolyte membrane. [Background technology]
[0002] From the viewpoint of preventing global warming and ensuring a stable supply of energy, carbon dioxide reduction technology has been attracting attention. There are reduction devices using artificial photosynthesis technology and reduction devices using electrolytic reduction technology as devices for carbon dioxide reduction technology. Artificial photosynthesis technology is a technology that advances the oxidation reaction of water and the reduction reaction of carbon dioxide by irradiating an oxidation electrode made of a photocatalyst with light. Electrolytic reduction technology is a technology that advances the oxidation reaction of water and the reduction reaction of carbon dioxide by applying a voltage between an oxidation electrode and a reduction electrode made of metal. Artificial photosynthesis technology using sunlight and electrolytic reduction technology using electricity derived from renewable energy have attracted attention as technologies that can recycle carbon dioxide into carbon monoxide, formic acid, hydrocarbons such as ethylene, and alcohols such as methanol and ethanol, and have been actively researched in recent years.
[0003] In artificial photosynthesis technology and carbon dioxide electrolytic reduction technology, a reaction system has been used in which a reduction electrode is immersed in an aqueous solution, and carbon dioxide dissolved in the aqueous solution is supplied to the reduction electrode for reduction (see Non-Patent Documents 1 and 2). However, in this carbon dioxide reduction method, there is a limit to the concentration of carbon dioxide dissolved in the aqueous solution and the diffusion coefficient of carbon dioxide in the aqueous solution, which limits the amount of carbon dioxide that can be supplied to the reduction electrode.
[0004] To address this issue, research is being conducted into supplying gaseous carbon dioxide to the reduction electrode in order to increase the amount of carbon dioxide supplied to the reduction electrode. According to Non-Patent Document 3, by using a reaction device having a structure capable of supplying gaseous carbon dioxide to the reduction electrode, the amount of carbon dioxide supplied to the reduction electrode is increased, and the reduction reaction of carbon dioxide is promoted. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] Satoshi Yotsuhashi and 6 others, “CO2 Conversion with Light and Water by GaN Photoelectrode”, Japanese Journal of Applied Physics, 51, 2012, p.02BP07-1-p.02BP07-3 [Non-Patent Document 2] Yoshio Hori and others, “Formation of Hydrocarbons in the Electrochemical Reduction of Carbone Dioxide at a Copper Electrode in Aqueous Solution”, Journal of the Chemical Society, 85(8), 1989, p.2309-p.2326 [Non-Patent Document 3] Qingxin Jia and 2 others, “Direct Gas-phase CO2 Reduction for Solar Methane Generation Using a Gas Diffusion Electrode with a BiVO4:Mo and a Cu-In-Se Photoanode”, Chemistry Letter, 47, 2018, p.436-439 Summary of the Invention [Problem to be solved by the invention]
[0006] The carbon dioxide reduction reaction shown in formulas (1) to (4) proceeds in combination with the water oxidation reaction shown in formula (5).
[0007] CO2+ 2H + + 2e - → CO + H2O (1) CO2+ 2H + + 2e - → HCOOH (2) CO2+ 6H + +6e - → CH3OH + H2O (3) CO2+ 8H + +8e - → CH4+ 2H2O (4) 2H2O + 4h + → O2+ 4H + (5)
[0008] In the gas-phase carbon dioxide reduction device, the aqueous solution in the reduction tank is removed and gas-phase carbon dioxide is filled in, but simply filling the tank with gas-phase carbon dioxide does not allow protons (H + ) cannot move in the gas phase, so it is necessary to join the electrolyte membrane and the reduction electrode. Furthermore, simply joining a plate-shaped reduction electrode to the electrolyte membrane does not allow the gas phase carbon dioxide to reach the interface between the reduction electrode and the electrolyte membrane, so it is necessary to make the reduction electrode porous so that the gas phase carbon dioxide can reach the interface between the reduction electrode and the electrolyte membrane. With this porous reduction electrode, if the pore size is small, there is a problem that the diffusion resistance of carbon dioxide within the electrode is large, reducing the efficiency of the carbon dioxide reduction reaction.
[0009] When using an electrolyte membrane as a proton exchange membrane, it is common to immerse the membrane in boiling nitric acid or boiling pure water to improve the proton mobility of the membrane. These treatments convert the proton exchange groups in the membrane into H + However, this process causes the electrolyte membrane to absorb excess water and become swollen. This is because the electrolyte membrane has a polymer reverse micelle structure, which causes it to swell and increase its water content.
[0010] When this swollen electrolyte membrane is bonded to a porous reduction electrode and used as a porous electrode-supported electrolyte membrane in a gas-phase reduction device, the aqueous solution in the oxidation tank gradually permeates into the reduction electrode during the carbon dioxide reduction reaction, causing the aqueous solution to cover the surface of the porous electrode to which gas-phase carbon dioxide should be supplied, resulting in a problem of the efficiency of the carbon dioxide reduction reaction deteriorating over time.
[0011] The present invention has been made in view of the above, and has an object to improve the efficiency of gas-phase reduction of carbon dioxide. [Means for solving the problem]
[0012] A porous electrode-supported electrolyte membrane according to one embodiment of the present invention is a porous electrode-supported electrolyte membrane used in a gas-phase reduction device for reducing carbon dioxide, the porous electrode having an electrolyte membrane and a porous reduction electrode directly bonded onto the electrolyte membrane, the porous reduction electrode having an average pore diameter of 1 μm or more. 97μm or less Yes The electrolyte membrane and the porous reduction electrode were then laminated and heat-pressed. .
[0013] A method for producing a porous electrode-supported electrolyte membrane according to one embodiment of the present invention is a method for producing a porous electrode-supported electrolyte membrane used in a gas-phase reduction device for reducing carbon dioxide, the method comprising the steps of immersing an electrolyte membrane in boiling nitric acid and boiling pure water, and laminating and thermocompressing a porous reduction electrode on a surface of the electrolyte membrane, the porous reduction electrode having an average pore diameter of 1 μm or more after thermocompression bonding. 97μm or less It is. Effect of the Invention
[0014] According to the present invention, the efficiency of gas-phase reduction of carbon dioxide can be improved. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the configuration of a porous electrode-supported electrolyte membrane of the present embodiment. [Diagram 2] FIG. 2 is a flow chart showing an example of a method for producing a porous electrode-supported electrolyte membrane. [Diagram 3] FIG. 3 is a diagram showing an example of a state in which thermocompression bonding is performed in the production of a porous electrode-supported electrolyte membrane. [Figure 4] FIG. 4 is a diagram showing an example of the configuration of a gas-phase reduction device for carbon dioxide including a porous electrode-supported electrolyte membrane. [Diagram 5] FIG. 5 is a diagram showing an example of the configuration of another gas-phase reduction device for carbon dioxide, which is provided with a porous electrode-supported electrolyte membrane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The present invention is not limited to the embodiment described below, and may be modified without departing from the spirit of the present invention.
[0017] [Configuration of porous electrode-supported electrolyte membrane] A porous electrode-supported electrolyte membrane 20 of this embodiment will be described with reference to the cross-sectional view of FIG.
[0018] The porous electrode-supported electrolyte membrane 20 in FIG. 1 comprises an electrolyte membrane 6 and a porous reduction electrode 5 directly bonded onto the surface of the electrolyte membrane 6 .
[0019] The porous reduction electrode 5 is directly laminated on the electrolyte membrane 6 and bonded by thermocompression. The porous reduction electrode 5 preferably has an average pore size of 1 μm or more after thermocompression. The porous reduction electrode 5 is, for example, a porous body of copper, platinum, gold, silver, indium, palladium, gallium, nickel, tin, cadmium, or an alloy thereof, or a porous body of silver oxide, copper oxide, copper(II) oxide, nickel oxide, indium oxide, tin oxide, tungsten oxide, tungsten(VI) oxide, copper oxide, or the like, or a porous metal complex having a metal ion and an anionic ligand.
[0020] The electrolyte membrane 6 is, for example, Nafion (registered trademark), Forblue, or Aquivion, which is a perfluorocarbon material having a carbon-fluorine skeleton.
[0021] [Method of manufacturing a porous electrode-supported electrolyte membrane] An example of a method for manufacturing the porous electrode-supported electrolyte membrane 20 of this embodiment will be described with reference to the flow chart of FIG.
[0022] In step S1, in order to reduce the resistance of the electrolyte membrane 6 to proton conduction, the electrolyte membrane 6 is immersed in boiling nitric acid and boiling pure water.
[0023] In step S2, the porous reduction electrode 5 is placed on the electrolyte membrane 6 and thermocompression-bonded by a thermocompression bonding device (e.g., a hot press machine). Specifically, as shown in Fig. 3, the porous reduction electrode 5 is placed on the electrolyte membrane 6 and disposed between two copper plates 40a, 40b, and the electrolyte membrane 6 and the porous reduction electrode 5 are thermocompression-bonded together with the copper plates 40a, 40b by the thermocompression bonding device. During thermocompression bonding, the heating temperature is preferably set to 100°C or higher and lower than 180°C.
[0024] After the thermocompression bonding, the assembly is quickly cooled to obtain a porous electrode-supported electrolyte membrane 20 in which the electrolyte membrane 6 and the porous reduction electrode 5 are joined together.
[0025] [Gas-phase reduction device (artificial photosynthesis)] Next, a gas-phase reduction device 100 for carbon dioxide having the porous electrode-supported electrolyte membrane 20 of this embodiment will be described with reference to Fig. 4. The gas-phase reduction device 100 shown in Fig. 4 is a reduction device that utilizes artificial photosynthesis technology to reduce carbon dioxide by light irradiation.
[0026] The gas-phase reduction device 100 includes an oxidation chamber 1 and a reduction chamber 4 formed by dividing the internal space in a housing in two by a porous electrode-supported electrolyte membrane 20. The porous electrode-supported electrolyte membrane 20 is disposed with the electrolyte membrane 6 facing the oxidation chamber 1 and the reduction electrode 5 facing the reduction chamber 4.
[0027] An oxidation vessel 1 is filled with an aqueous solution 3. An oxidation electrode 2 made of a semiconductor or a metal complex is inserted into the aqueous solution 3.
[0028] The oxidation electrode 2 is a compound exhibiting photoactivity and redox activity, such as a nitride semiconductor, titanium oxide, amorphous silicon, a ruthenium complex, or a rhenium complex. The oxidation electrode 2 is electrically connected to the porous reduction electrode 5 by a conductor 7.
[0029] The aqueous solution 3 is, for example, an aqueous potassium hydrogen carbonate solution, an aqueous sodium hydrogen carbonate solution, an aqueous potassium chloride solution, an aqueous sodium chloride solution, an aqueous sodium hydroxide solution, an aqueous potassium hydroxide solution, an aqueous rubidium hydroxide solution, or an aqueous cesium hydroxide solution. During the reduction reaction, helium gas is supplied to the aqueous solution 3 from a tube 8.
[0030] Carbon dioxide is supplied from a gas inlet 10 to the reduction tank 4, and the reduction tank 4 is filled with carbon dioxide or a gas containing carbon dioxide.
[0031] The light source 9 is disposed so as to irradiate light onto the oxidation electrode 2. The light source 9 is, for example, a xenon lamp, a pseudo-sun light source, a halogen lamp, a mercury lamp, or sunlight. The light source 9 may be a combination of these.
[0032] [Example of porous electrode-supported electrolyte membrane] As the porous electrode-supported electrolyte membrane 20 to be placed in the above-mentioned gas-phase reduction device 100, Examples 1-6 were prepared by changing the average pore size or the heating temperature during the thermocompression bonding process, and a gas-phase reduction test described below was performed. The porous electrode-supported electrolyte membrane of Examples 1-6 will be described below.
[0033] <Example 1> In Example 1, a copper porous body having a thickness of 0.2 mm and a porosity of 65% was used as the material for the porous reduction electrode 5, and Nafion, which is a proton exchange membrane, was used as the material for the electrolyte membrane 6.
[0034] In step S1, in order to reduce the resistance of proton conduction, the electrolyte membrane 6 was immersed in boiling nitric acid and boiling pure water, respectively. It was confirmed that this treatment reduced the resistance of proton conduction of the electrolyte membrane 6 to 3.0 to 3.5 Ω.
[0035] In step S2, the sample in which the porous reduction electrode 5 was laminated on the electrolyte membrane 6 was sandwiched between two copper plates and a hot press machine, and pressure was applied vertically to the surface of the porous reduction electrode 5 at a heating temperature of 150° C., and the sample was left for 3 minutes. Thereafter, the sample was quickly cooled and taken out, and a porous electrode-supported electrolyte membrane 20 in which the electrolyte membrane 6 and the porous reduction electrode 5 were bonded was obtained.
[0036] After the thermocompression bonding, the porous reduction electrode 5 had a thickness of 0.14 mm, a porosity of 50%, and an average pore diameter of 1.3 μm.
[0037] <Example 2> In Example 2, a porous electrode-supported electrolyte membrane 20 was produced using a copper porous body having a thickness of 0.2 mm and a porosity of 79% as the material for the porous reduction electrode 5. The thickness of the porous reduction electrode 5 after thermocompression bonding was 0.14 mm, the porosity was 70%, and the average pore diameter was 15 μm. All other conditions were the same as those in Example 1.
[0038] <Example 3> In Example 3, a porous electrode-supported electrolyte membrane 20 was produced using a copper porous body having a thickness of 0.2 mm and a porosity of 93% as the material for the porous reduction electrode 5. The thickness of the porous reduction electrode 5 after thermocompression bonding was 0.14 mm, the porosity was 90%, and the average pore diameter was 97 μm. All other conditions were the same as those in Example 1.
[0039] <Example 4> In Example 4, similarly to Example 3, a porous electrode-supported electrolyte membrane 20 was produced using a copper porous body having a thickness of 0.2 mm and a porosity of 93% as the material for the porous reduction electrode 5. The heating temperature when applying pressure with the hot press was set to 100° C. All conditions other than the heating temperature were the same as those in Example 3.
[0040] <Example 5> In Example 5, similarly to Example 3, a porous electrode-supported electrolyte membrane 20 was produced using a copper porous body having a thickness of 0.2 mm and a porosity of 93% as the material for the porous reduction electrode 5. The heating temperature when applying pressure with the hot press was set to 120° C. All conditions other than the heating temperature were the same as those in Example 3.
[0041] <Example 6> In Example 6, similarly to Example 3, a porous electrode-supported electrolyte membrane 20 was produced using a copper porous body having a thickness of 0.2 mm and a porosity of 93% as the material for the porous reduction electrode 5. The heating temperature when applying pressure with the hot press was set to 180° C. All conditions other than the heating temperature were the same as those in Example 3.
[0042] [Electrochemical measurements and gas / liquid production measurements] Each of the porous electrode-supported electrolyte membranes 20 of Examples 1 to 6 was attached to the gas-phase reduction device 100 of FIG. 4, and the following reduction reaction test was carried out.
[0043] The oxidation tank 1 was filled with the aqueous solution 3. The aqueous solution 3 was a 1.0 mol / L aqueous solution of potassium hydroxide.
[0044] The oxidation electrode 2 was placed in the oxidation tank 1 so as to be submerged in the aqueous solution 3. A semiconductor photoelectrode prepared as follows was used for the oxidation electrode 2. A thin film of GaN, which is an n-type semiconductor, and AlGaN were epitaxially grown in that order on a sapphire substrate, and Ni was then vacuum-deposited on the AlGaN and heat-treated to form a NiO promoter thin film to prepare a semiconductor photoelectrode.
[0045] The light source 9 is a 300W high-pressure xenon lamp (cuts out wavelengths of 450 nm or more, illuminance 6.6 mW / cm 2 The light source 9 was fixed so that the surface of the oxidation electrode 2 on which the oxidation promoter was formed was the irradiated surface. The light irradiation area of the oxidation electrode 2 was set to 2.5 cm 2 It was decided.
[0046] Helium (He) was fed from a tube 8 to the oxidation tank 1, and carbon dioxide (CO2) was fed from a gas inlet 10 to the reduction tank 4, each at a flow rate of 5 ml / min and a pressure of 0.18 MPa. In this system, the reduction reaction of carbon dioxide can proceed at the three-phase interface consisting of [electrolyte membrane-copper-gas phase carbon dioxide] in the porous electrode-supported electrolyte membrane 20. The apparent area of the porous reduction electrode 5 to which carbon dioxide is directly supplied is approximately 6.25 cm2.2 It is.
[0047] After the oxidation tank 1 and reduction tank 4 were thoroughly replaced with helium and carbon dioxide, the oxidation electrode 2 was uniformly irradiated with light using a light source 9. Electrons flow between the oxidation electrode 2 and the porous reduction electrode 5 due to the light irradiation.
[0048] The current value between the oxidation electrode 2 and the porous reduction electrode 5 during light irradiation was measured using an electrochemical measurement device (Solartron, 1287-type potentiogalvanostat). In addition, gas and liquid in the oxidation tank 1 and reduction tank 4 were sampled at any time during light irradiation, and the reaction products were analyzed using a gas chromatograph, liquid chromatograph, and gas chromatograph mass spectrometer. As a result, it was confirmed that oxygen was produced in the oxidation tank 1, and hydrogen, carbon monoxide, formic acid, methane, methanol, ethanol, and ethylene were produced in the reduction tank 4.
[0049] The test results of Examples 1-6 will be described later together with the test results of Examples 7-14 and Comparative Examples 1-4.
[0050] [Gas phase reduction device (electrolytic reduction)] Next, a gas-phase reduction device 200 for carbon dioxide including the porous electrode-supported electrolyte membrane 20 of this embodiment will be described with reference to Fig. 5. The gas-phase reduction device 200 shown in Fig. 5 is a reduction device that utilizes an electrolytic reduction technique in which a current is passed between an oxidation electrode and a reduction electrode to reduce carbon dioxide.
[0051] The gas-phase reduction device 200 includes an oxidation chamber 1 and a reduction chamber 4 formed by dividing the internal space in a housing in two by a porous electrode-supported electrolyte membrane 20. The porous electrode-supported electrolyte membrane 20 is disposed such that the electrolyte membrane 6 side faces the oxidation chamber 1 and the reduction electrode 5 side faces the reduction chamber 4.
[0052] An oxidation vessel 1 is filled with an aqueous solution 3. An oxidation electrode 2 made of a semiconductor or a metal complex is inserted into the aqueous solution 3.
[0053] The oxidation electrode 2 is made of, for example, platinum, gold, silver, copper, indium, or nickel.
[0054] The aqueous solution 3 is the same as that of the gas-phase reduction apparatus 100 in FIG.
[0055] Carbon dioxide is supplied from a gas inlet 10 to the reduction tank 4, and the reduction tank 4 is filled with carbon dioxide or a gas containing carbon dioxide.
[0056] A power source 11 is electrically connected to the oxidation electrode 2 and the porous reduction electrode 5 by electrical leads 7 .
[0057] [Example of porous electrode-supported electrolyte membrane] As the porous electrode-supported electrolyte membrane 20 to be placed in the gas-phase reduction device 200, Examples 7-12 were prepared by changing the average pore size or the temperature during the thermocompression treatment, and a gas-phase reduction test was carried out as described below. The porous electrode-supported electrolyte membrane of Examples 7-12 will be described below. The porous electrode-supported electrolyte membrane 20 of Examples 7-12 was prepared in the same manner as the porous electrode-supported electrolyte membrane 20 of Examples 1-6.
[0058] <Example 7> The porous electrode-supported electrolyte membrane 20 of Example 7 was produced by the same procedure as in Example 1. The heating temperature during thermocompression bonding was 150° C., and the porous reduction electrode 5 after thermocompression bonding had a thickness of 0.14 mm, a porosity of 50%, and an average pore diameter of 1.3 μm.
[0059] <Example 8> In Example 8, a porous electrode-supported electrolyte membrane 20 was produced using a copper porous body having a thickness of 0.2 mm and a porosity of 79% as the material for the porous reduction electrode 5. The thickness of the porous reduction electrode 5 after thermocompression bonding was 0.14 mm, the porosity was 70%, and the average pore diameter was 15 μm. All other conditions were the same as those in Example 7.
[0060] <Example 9> In Example 9, a porous electrode-supported electrolyte membrane 20 was produced using a copper porous body having a thickness of 0.2 mm and a porosity of 93% as the material for the porous reduction electrode 5. The thickness of the porous reduction electrode 5 after thermocompression bonding was 0.14 mm, the porosity was 90%, and the average pore diameter was 97 μm. All other conditions were the same as those in Example 7.
[0061] <Example 10> In Example 10, similarly to Example 9, a porous electrode-supported electrolyte membrane 20 was produced using a copper porous body having a thickness of 0.2 mm and a porosity of 93% as the material for the porous reduction electrode 5. The heating temperature when applying pressure with the hot press was set to 100° C. All conditions other than the heating temperature were the same as those in Example 9.
[0062] <Example 11> In Example 11, similarly to Example 9, a porous electrode-supported electrolyte membrane 20 was produced using a copper porous body having a thickness of 0.2 mm and a porosity of 93% as the material for the porous reduction electrode 5. The heating temperature when applying pressure with the hot press was set to 120° C. All conditions other than the heating temperature were the same as those in Example 9.
[0063] <Example 12> In Example 12, similarly to Example 9, a porous electrode-supported electrolyte membrane 20 was produced using a copper porous body having a thickness of 0.2 mm and a porosity of 93% as the material for the porous reduction electrode 5. The heating temperature when applying pressure with the hot press was set to 180° C. All conditions other than the heating temperature were the same as those in Example 9.
[0064] [Electrochemical measurements and gas / liquid production measurements] Each of the porous electrode-supported electrolyte membranes 20 of Examples 7 to 12 was attached to the gas-phase reduction device 200 of FIG. 5, and the following reduction reaction test was carried out.
[0065] The oxidation tank 1 was filled with the aqueous solution 3. The aqueous solution 3 was a 1.0 mol / L aqueous solution of potassium hydroxide.
[0066] The oxidation electrode 2 is placed on a plate with a surface area of approximately 0.55 cm 2The electrode was placed in the oxidation tank 1 so that it was submerged in the aqueous solution 3. The oxidation electrode 2 was made of platinum (manufactured by Nilaco Corporation).
[0067] Helium (He) was fed from a tube 8 to the oxidation tank 1, and carbon dioxide (CO2) was fed from a gas inlet 10 to the reduction tank 4, each at a flow rate of 5 ml / min and a pressure of 0.18 MPa. In this system, the reduction reaction of carbon dioxide can proceed at the three-phase interface consisting of [electrolyte membrane-copper-gas phase carbon dioxide] in the porous electrode-supported electrolyte membrane 20. The apparent area of the porous reduction electrode 5 to which carbon dioxide is directly supplied is approximately 6.25 cm2. 2 It is.
[0068] After the oxidation tank 1 and reduction tank 4 were thoroughly replaced with helium and carbon dioxide, a voltage of 2.0 V was applied from the power source 11 to cause electrons to flow between the oxidation electrode 2 and the porous reduction electrode 5 .
[0069] The current value between the oxidation electrode 2 and the porous reduction electrode 5 when a voltage was applied was measured using an electrochemical measurement device.
[0070] In addition, the gas and liquid in the oxidation tank 1 and reduction tank 4 were sampled at any time during voltage application, and the reaction products were analyzed using a gas chromatograph, liquid chromatograph, and gas chromatograph mass spectrometer. As a result, it was confirmed that oxygen was produced in the oxidation tank 1, and hydrogen, carbon monoxide, formic acid, methane, methanol, ethanol, and ethylene were produced in the reduction tank 4.
[0071] [Comparison example] Comparative Examples 1-4 were prepared which were different from the Examples in average pore size or temperature during thermocompression treatment. Comparative Examples 1 and 2 were arranged as the porous electrode-supported electrolyte membrane 20 in the gas-phase reduction apparatus 100 of FIG. 4, and Comparative Examples 3 and 4 were arranged as the porous electrode-supported electrolyte membrane 20 in the gas-phase reduction apparatus 200 of FIG. 5, and tests similar to those of Examples 1-6 and Examples 7-12 were performed.
[0072] <Comparative Example 1> In Comparative Example 1, a porous electrode-supported electrolyte membrane was produced in the same manner as in Example 1, using a copper porous body having a thickness of 0.2 mm and a porosity of 51%. The thickness of the porous reduction electrode after thermocompression bonding was 0.14 mm, the porosity was 30%, and the average pore diameter was 0.11 μm. All other conditions were the same as in Example 1.
[0073] <Comparative Example 2> In Comparative Example 2, the heating temperature during thermocompression bonding was set to 80° C. All other conditions were the same as those in Example 3.
[0074] <Comparative Example 3> In Comparative Example 3, a porous electrode-supported electrolyte membrane was produced in the same manner as in Example 7, using a copper porous body having a thickness of 0.2 mm and a porosity of 51%. The thickness of the porous reduction electrode after thermocompression bonding was 0.14 mm, the porosity was 30%, and the average pore diameter was 0.11 μm. All other conditions were the same as in Example 7.
[0075] <Comparative Example 4> In Comparative Example 4, the heating temperature during thermocompression bonding was set to 80° C. All other conditions were the same as those in Example 9.
[0076] [Evaluation of Examples and Comparative Examples] Next, the test results of Examples 1-12 and Comparative Examples 1-4 will be described. Table 1 shows the Faraday efficiency of the carbon dioxide reduction reaction after 1 hour and the Faraday efficiency maintenance rate of the carbon dioxide reduction reaction after 20 hours for Examples 1-12 and Comparative Examples 1-4.
[0077] [Table 1]
[0078] As shown in formula (6), the Faraday efficiency indicates the ratio of the current value used in each reduction reaction to the current value flowing between the electrodes when irradiated with light or when a voltage is applied.
[0079] Faraday efficiency of each reduction reaction [%] = (charge consumed in each reduction reaction) / (charge flowing between the oxidation electrode and reduction electrode) × 100 (6)
[0080] Here, the "charge consumed in each reduction reaction" in formula (6) can be calculated by converting the measured amount of reaction product of each reduction reaction into the charge required for that reduction reaction. When the amount of reaction product of each reduction reaction is A [mol], the number of electrons required for the reduction reaction is Z, and the Faraday constant is F [C / mol], it was calculated using formula (7).
[0081] Charge consumed in each reduction reaction [C] = A × Z × F (7)
[0082] Further, the Faraday efficiency maintenance rate of each reduction reaction after 20 hours was defined and calculated according to the following formula (8).
[0083] Faraday efficiency maintenance rate of each reduction reaction after 20 hours [%] = (Faraday efficiency of each reduction reaction after 20 hours) / (Faraday efficiency of each reduction reaction after 1 hour) × 100 (8)
[0084] When comparing the Faraday efficiency of the carbon dioxide reduction reaction after one hour between Examples 1-5, Comparative Example 1, Examples 7-11 and Comparative Example 3, it was found that Examples 1-5 and 7-11 had higher Faraday efficiency of the carbon dioxide reduction reaction after one hour than Comparative Examples 1 and 3.
[0085] Table 1 shows the evaluation results of the diffusion coefficient of carbon dioxide in the porous electrode, which depends on the pore size. According to this, in Examples 1-5 and 7-11, where the pore size exceeds 1 μm, the saturation value is 6.0×10 -6 m 2 s -1 (self-diffusion coefficient), which was found to be approximately 1.5 times that of Comparative Examples 1 and 3.
[0086] From these findings, it was found that by using a porous electrode-supported electrolyte membrane 20 composed of porous electrodes with an average pore diameter of 1 μm or more, at which the diffusion coefficient of carbon dioxide reaches a saturated value, the amount of carbon dioxide supplied to the porous reduction electrode 5 was increased, thereby improving the efficiency of the carbon dioxide reduction reaction.
[0087] When comparing Examples 1-5, Comparative Example 2, Examples 7-11, and Comparative Example 4 with respect to the Faraday efficiency maintenance rate of the carbon dioxide reduction reaction after 20 hours, Examples 1-5 and 7-11 had a higher Faraday efficiency maintenance rate of the carbon dioxide reduction reaction after 20 hours than Comparative Examples 2 and 4.
[0088] In Examples 1-5 and 7-11, there was no visible liquid on the electrode surface after 20 hours. On the other hand, in Comparative Examples 2 and 4, several hundred μL of liquid was attached to the electrode surface after 20 hours, and it was found that the Faraday efficiency maintenance rate was reduced because gaseous carbon dioxide could not be directly supplied to the electrode surface. It was confirmed that the liquid attached to the electrode surface was mainly an aqueous solution that permeated from the oxidation tank 1 through the electrolyte membrane 6 regardless of whether the carbon dioxide reduction reaction proceeded or not. This is thought to be due to the electrolyte membrane 6 becoming swollen with excess moisture, and the aqueous solution 3 in the oxidation tank 1 permeating into it. On the other hand, in Examples 1-5 and 7-11, the moisture contained in the electrolyte membrane could be vaporized by performing the thermocompression bonding at a temperature condition of 100°C or higher. It is thought that this suppresses the permeation of the aqueous solution through the electrolyte membrane, thereby improving the maintenance rate of the carbon dioxide reduction reaction.
[0089] Furthermore, Table 1 shows the measured resistance of the proton conduction of the electrolyte membrane 6. In Examples 1-5 and 7-11, the resistance was as low as 3.0 to 3.5 Ω, and it was confirmed that the effect of reducing the resistance of the proton conduction was not lost even after thermocompression bonding. On the other hand, in Examples 6 and 12, the resistance of the ion conduction of the electrolyte membrane 6 increased to 360 Ω. As a result, the current value between the electrodes was extremely low and the amount of the reaction product was below the detection limit (3%) of the evaluation system, so no record was made. This is thought to be because the proton exchange group of the electrolyte membrane was decomposed by performing the thermocompression treatment at a high temperature condition of 180°C.
[0090] As described above, according to this embodiment, the porous electrode supported electrolyte membrane 20 of this embodiment has the electrolyte membrane 6 and the porous reduction electrode 5 directly bonded onto the electrolyte membrane 6, and the average pore diameter of the porous reduction electrode 5 is set to be 1 μm or more. This reduces the diffusion resistance of carbon dioxide within the electrode, and improves the efficiency of the gas phase reduction of carbon dioxide. Furthermore, in the process of bonding the electrolyte membrane 6 and the porous reduction electrode 5, pressure is applied while heating to suppress swelling of the electrolyte membrane 6, thereby improving the life of the porous electrode supported electrolyte membrane 20. [Explanation of symbols]
[0091] Porous electrode supported electrolyte membrane 20 Porous reduction electrode 5 Electrolyte membrane 6
Claims
1. A porous electrode-supported electrolyte membrane for use in a gas-phase reduction device for reducing carbon dioxide, comprising: An electrolyte membrane; A porous reduction electrode is directly bonded onto the electrolyte membrane, The average pore diameter of the porous reduction electrode is 1 μm or more and 97 μm or less, The electrolyte membrane and the porous reduction electrode were laminated and heat-pressed. Porous electrode-supported electrolyte membrane.
2. A method for producing a porous electrode-supported electrolyte membrane for use in a gas-phase reduction device for reducing carbon dioxide, comprising the steps of: Immersing the electrolyte membrane in boiling nitric acid and boiling pure water; A step of superposing a porous reduction electrode on a surface of the electrolyte membrane and thermocompressing the electrode, The average pore size of the porous reduction electrode after thermocompression bonding is 1 μm or more and 97 μm or less. A method for producing a porous electrode-supported electrolyte membrane.
3. A method for producing the porous electrode-supported electrolyte membrane according to claim 2, comprising the steps of: The method for producing a porous electrode-supported electrolyte membrane, wherein the heating temperature for the thermocompression bonding is 100° C. or higher and lower than 180° C.
Citation Information
Patent Citations
Carbon dioxide reducing electrode and carbon dioxide reducing device
JP2020023726A
Co2 reductive reaction apparatus
JP2021059760A
Method and device for preparing reduction product of carbon dioxide
KR1020210034348A
Method for electrochemically converting carbon dioxide
US20130146470A1
System for reducing and fixing carbon dioxide, method for reducing and fixing carbon dioxide, and method for producing useful carbon resource
WO2012128148A1