A layer of material that encases the surface

By adjusting chamber pressure and precursor flow rates, the method addresses film shrinkage and stress issues in semiconductor deposition, resulting in reduced substrate warpage and improved film integrity.

JP7594587B2Active Publication Date: 2024-12-04APPLIED MATERIALS INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022525713
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-01
Filing Date
2020-10-27
Publication Date
2024-12-04
Estimated Expiration
2040-10-27

AI Technical Summary

Technical Problem

Conventional semiconductor deposition methods face challenges in balancing film shrinkage and stress properties, leading to issues like wafer warpage and increased compressive stress due to outgassing and oxygen incorporation, which affect the quality of integrated circuits.

Method used

A deposition method involving controlled adjustments of chamber pressure and precursor flow rates to create a denser, protective silicon-containing layer, limiting outgassing and oxygen uptake, thereby reducing film shrinkage and maintaining controlled compressive stress.

Benefits of technology

The method produces films with reduced shrinkage and controlled stress, providing a protective coating that limits substrate warpage and maintains film integrity during exposure to atmospheric conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594587000001
    Figure 0007594587000001
  • Figure 0007594587000002
    Figure 0007594587000002
  • Figure 0007594587000003
    Figure 0007594587000003
Patent Text Reader

Abstract

An exemplary deposition method may include delivering a silicon-containing precursor and a carrier precursor to a processing region of a semiconductor processing chamber. The method may include forming a plasma of the silicon-containing precursor and the carrier precursor within the processing region of the semiconductor processing chamber. The method may include depositing a first amount of silicon-containing material on a substrate disposed within the processing region of the semiconductor processing chamber. The deposition may occur at a first chamber pressure. The method may include adjusting the first chamber pressure to a second chamber pressure lower than the first chamber pressure. The method may include depositing a second amount of silicon-containing material on the first amount of silicon-containing material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefit of priority to U.S. patent application Ser. No. 62 / 929,291, filed Nov. 1, 2019, the contents of which are incorporated by reference in their entirety for all purposes.

[0002] Technical Field

[0002] The present technology relates to semiconductor deposition processes. More specifically, the present technology relates to methods of depositing materials with reduced stress effects. [Background technology]

[0003] background

[0003] Integrated circuits are made possible by processes that produce intricately patterned layers of material on substrate surfaces. Fabricating patterned materials on substrates requires controlled methods of formation and removal of exposed material. The material properties of the produced films can contribute to substrate effects, which can cause wafer warping and other problems during processing.

[0004]

[0004] Therefore, there is a need for improved systems and methods that can be used to manufacture high quality devices and structures. These and other needs are addressed by the present technique. Summary of the Invention

[0005] An exemplary deposition method may include delivering a silicon-containing precursor and a carrier precursor to a processing region of a semiconductor processing chamber. The method may include forming a plasma of the silicon-containing precursor and the carrier precursor in the processing region of the semiconductor processing chamber. The method may include depositing a first quantity of silicon-containing material on a substrate disposed in the processing region of the semiconductor processing chamber. The deposition may occur at a first chamber pressure. The method may include adjusting the first chamber pressure to a second chamber pressure that is lower than the first chamber pressure. The method may include depositing a second quantity of silicon-containing material on the first quantity of silicon-containing material.

[0006] In some embodiments, the silicon-containing precursor is a silicon-oxygen-containing precursor and the silicon-containing material can be or include silicon oxide. The first chamber pressure can be less than about 20 Torr and the second chamber pressure can be less than about 10 Torr. The substrate temperature can be maintained at about 300° C. or greater during deposition of the first amount of the silicon-containing material and the second amount of the silicon-containing material. The carrier precursor can be or include argon. The method can include increasing a volumetric flow rate of the carrier precursor while adjusting the first chamber pressure to the second chamber pressure. The second amount of the silicon-containing material can be characterized by a higher density than the first amount of the silicon-containing material. The silicon-containing precursor can be or include tetraethylorthosilicate. The second amount of the silicon-containing material can be characterized by a thickness of about 100 nm or less.

[0007]

[0007] Some embodiments of the present technique may include a deposition method. The method may include delivering a silicon-containing precursor and a carrier precursor to a processing region of a semiconductor processing chamber. The method may include forming a plasma of the silicon-containing precursor and the carrier precursor in the processing region of the semiconductor processing chamber. The method may include depositing a first amount of silicon-containing material on a substrate disposed in the processing region of the semiconductor processing chamber. The deposition may occur at a first chamber pressure. The method may include adjusting the carrier precursor from a first volumetric flow rate to a second volumetric flow rate greater than the first volumetric flow rate. The method may include depositing the second amount of silicon-containing material on the first amount of silicon-containing material.

[0008] In some embodiments, the silicon-containing precursor is a silicon-oxygen-containing precursor and the silicon-containing material may be or include silicon oxide. The second volumetric flow rate may be more than 50% greater than the first volumetric flow rate. The method may include adjusting the first chamber pressure to a second chamber pressure lower than the first chamber pressure while adjusting the carrier precursor from the first volumetric flow rate to the second volumetric flow rate. The first chamber pressure may be less than about 15 Torr and the second chamber pressure may be less than about 7 Torr. The second amount of silicon-containing material may be characterized by a thickness of about 100 nm or less. The second amount of silicon-containing material may be characterized by a compressive stress greater than or about the compressive stress associated with the first amount of silicon-containing material.

[0009]

[0009] The technique may also include a deposition method. The method may include delivering a silicon-oxygen containing precursor and a carrier precursor to a processing region of a semiconductor processing chamber. The method may include forming a plasma of the silicon-oxygen containing precursor and the carrier precursor in the processing region of the semiconductor processing chamber. The method may include depositing a first amount of silicon-oxygen containing material on a substrate disposed in the processing region of the semiconductor processing chamber. The deposition may occur at a first chamber pressure. The method may include adjusting the first chamber pressure to a second chamber pressure lower than the first chamber pressure. The method may include increasing a volumetric flow rate of the carrier precursor while adjusting the chamber pressure. The method may include depositing a second amount of silicon-oxygen containing material on the first amount of silicon-oxygen containing material.

[0010] In some embodiments, the first chamber pressure can be less than about 20 Torr and the second chamber pressure can be less than about 10 Torr. The silicon-oxygen containing precursor can be or include tetraethylorthosilicate, and the carrier precursor can be or include argon. A first amount of the silicon-oxygen containing material can be deposited for a first period of time, and a second amount of the silicon-oxygen containing material can be deposited for a second period of time that is shorter than the first period of time.

[0011]

[0011] Such techniques may offer many advantages over conventional systems and techniques. For example, the present process may produce films that are characterized by reduced film shrinkage. Additionally, operation of embodiments of the present technology may produce films that maintain a controlled compressive stress when exposed to the atmosphere. These and other embodiments, along with many of their advantages and features, will be described in more detail in conjunction with the following description and accompanying figures.

[0012] A further understanding of the nature and advantages of the disclosed technology may be realized by reference to the remaining portions of the specification and drawings. [Brief description of the drawings]

[0013] [Figure 1] 1 shows a schematic cross-sectional view of an exemplary processing chamber in accordance with some embodiments of the present technique. [Diagram 2]

[0014] 1 illustrates exemplary operations in a deposition method according to some embodiments of the present technique. [Figure 3A-3C]

[0015] 3A-3C show schematic views of a substrate during a deposition operation according to some embodiments of the present technique. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014]

[0016] Some of the figures are included as schematic diagrams. It is understood that these figures are for illustrative purposes and should not be considered to be to scale unless specifically stated to be to scale. Furthermore, as schematic diagrams, the figures are provided to aid in understanding and may not include all aspects or information compared to realistic representations and may include exaggerated material for illustrative purposes.

[0015]

[0017] In the accompanying figures, similar components or features may have the same reference label. Additionally, various components of the same type may be distinguished by tracing the reference numbers with a letter that distinguishes the similar components. When only a first reference number is used in this specification, the description is applicable to any one of the similar components having the same first reference number, regardless of the letter.

[0016]

[0018] During semiconductor manufacturing, various deposition and etching operations can be utilized to fabricate structures on a substrate. Silicon oxide and other silicon-containing materials are routinely formed in many operations to develop semiconductor substrates. As an example, silicon oxide can be deposited by many processes including chemical vapor deposition and plasma deposition. Silicon oxide deposited or formed in some processes can be characterized by the amount of hydrogen and / or carbon incorporated into the film, which may be contained in precursors such as silane and tetraethylorthosilicate. During subsequent processing, such as during subsequent annealing, the silicon oxide film may be exposed to high temperatures. This high temperature exposure can cause outgassing of residual materials incorporated during the deposition process and shrinkage of the film.

[0017]

[0019] To limit shrinkage effects, some conventional techniques may produce denser oxide films, but denser films may exhibit elevated internal stresses. Silicon oxide may be characterized by compressive stresses, which may increase as it shrinks or densifies. This may cause high aspect ratio features to buckle, and in some circumstances, substrate or wafer warpage. Additionally, silicon oxide may be a relatively porous film. After processing, the substrate may be exposed to the atmosphere, and oxygen from moisture may become incorporated into the film. Oxygen absorbed into the film may also make the film denser, which may also increase the compressive stress of the film. Conventional techniques have been challenged to balance the shrinkage and stress characteristics of the produced film.

[0018]

[0020] The present technique can overcome these limitations by adjusting deposition parameters and materials to create a sealing layer around the generated film. For example, the present technique can include depositing a surface layer of material that can create a protective coating. This coating can limit outgassing of the bulk film, which can limit shrinkage, and can also provide a barrier to oxygen uptake, which can densify the film and increase stress. After describing the general aspects of the chamber according to an embodiment of the present technique in which the plasma processing operations discussed below can be performed, specific methodologies and component configurations can be discussed. It should be understood that the described technique can be used to improve many film formation processes, and therefore the present technique is not intended to be limited to the specific films and processes discussed, but can be applied to a variety of processing chambers and operations.

[0019]

[0021] FIG. 1 illustrates a cross-sectional view of an exemplary processing chamber 100 according to some embodiments of the present technology. The diagram may provide an overview of a system that may incorporate one or more aspects of the present technology and / or be specifically configured to perform one or more operations according to embodiments of the present technology. Additional details of the chamber 100 or the method performed may be further described below. Although the chamber 100 may be utilized to form a film layer according to some embodiments of the present technology, it should be understood that the method may be similarly performed in any chamber in which film formation may occur. The processing chamber 100 may include a chamber body 102, a substrate support 104 disposed within the chamber body 102, and a lid assembly 106 coupled with the chamber body 102 and enclosing the substrate support 104 within a processing volume 120. The substrate 103 may be provided in the processing volume 120 through an opening 126, which may be sealed in a conventional manner for processing using a slit valve or door. The substrate 103 may be seated on a surface 105 of the substrate support during processing. The substrate support 104 can be rotatable along an axis 147, as indicated by arrow 145, where the shaft 144 of the substrate support 104 can be positioned. Alternatively, the substrate support 104 can be elevated to rotate as needed during the deposition process.

[0020]

[0022] The plasma profile modulator 111 may be disposed within the processing chamber 100 to control the plasma distribution across the substrate 103 disposed on the substrate support 104. The plasma profile modulator 111 may include a first electrode 108 that may be disposed adjacent to the chamber body 102 and may separate the chamber body 102 from other components of the lid assembly 106. The first electrode 108 may be part of the lid assembly 106 or may be a separate sidewall electrode. The first electrode 108 may be an annular or ring-shaped member and may be a ring electrode. The first electrode 108 may be a continuous loop around the circumference of the processing chamber 100 surrounding the processing volume 120 or may be discontinuous at selected locations as required. The first electrode 108 may also be a perforated electrode, such as a perforated ring or mesh electrode, or may be a plate electrode, such as a secondary gas distributor, for example.

[0021]

[0023] One or more isolators 110a, 110b, which may be a dielectric material such as ceramic or metal oxide, e.g., aluminum oxide and / or aluminum nitride, may contact the first electrode 108 and electrically and thermally isolate the first electrode 108 from the gas distributor 112 and the chamber body 102. The gas distributor 112 may define an aperture 118 for distributing the process precursors to the processing volume 120. The gas distributor 112 may be coupled to a first power source 142, such as an RF generator, an RF power source, a DC power source, a pulsed DC power source, a pulsed RF power source, or any other power source capable of being coupled to a process chamber. In some embodiments, the first power source 142 may be an RF power source.

[0022]

[0024] The gas distributor 112 can be a conductive gas distributor or a non-conductive gas distributor. The gas distributor 112 can also be formed from conductive and non-conductive components. For example, the body of the gas distributor 112 can be conductive, while the faceplate of the gas distributor 112 can be non-conductive. The gas distributor 112 can be powered, for example, by a first power source 142 as shown in FIG. 1, or the gas distributor 112 can be coupled to ground in some embodiments.

[0023]

[0025] The first electrode 108 can be coupled to a first conditioning circuit 128 that can control the ground path of the processing chamber 100. The first conditioning circuit 128 can include a first electronic sensor 130 and a first electronic controller 134. The first electronic controller 134 can be or include a variable capacitor or other circuit element. The first conditioning circuit 128 can be or include one or more inductors 132. The first conditioning circuit 128 can be any circuit that allows for a variable or controllable impedance under the plasma conditions present in the processing volume 120 during processing. In some illustrated embodiments, the first conditioning circuit 128 can include a first circuit leg and a second circuit leg coupled in parallel between ground and the first electronic sensor 130. The first circuit leg can include a first inductor 132A. The second circuit leg can include a second inductor 132B coupled in series with the first electronic controller 134. The second inductor 132B can be disposed between the first electronic controller 134 and a node connecting both the first and second circuit legs to the first electronic sensor 130. The first electronic sensor 130 can be a voltage or current sensor and can be coupled to the first electronic controller 134, which can allow for some closed-loop control of the plasma conditions within the process volume 120.

[0024]

[0026] The second electrode 122 may be coupled to the substrate support 104. The second electrode 122 may be embedded in the substrate support 104 or coupled to a surface of the substrate support 104. The second electrode 122 may be a plate, a perforated plate, a mesh, a wire screen, or any other distributed arrangement of conductive elements. The second electrode 122 may be a conditioning electrode and may be coupled to a second conditioning circuit 136 by a conduit 146, such as a cable with a selected resistance, such as, for example, 50 ohms, disposed on a shaft 144 of the substrate support 104. The second conditioning circuit 136 may have a second electronic sensor 138 and a second electronic controller 140, which may be a second variable capacitor. The second electronic sensor 138 may be a voltage or current sensor and may be coupled to the second electronic controller 140 to further control the plasma conditions in the process volume 120.

[0025]

[0027] A third electrode 124, which may be a bias electrode and / or an electrostatic chucking electrode, may be coupled to the substrate support 104. The third electrode may be coupled to a second power source 150 through a filter 148, which may be an impedance matching circuit. The second power source 150 may be DC power, pulsed DC power, RF bias power, pulsed RF source or bias power, or a combination of these or other power sources. In some embodiments, the second power source 150 may be RF bias power.

[0026]

[0028] The lid assembly 106 and substrate support 104 of FIG. 1 can be used with any processing chamber for plasma or thermal processing. During operation, the processing chamber 100 can provide real-time control of plasma conditions within the processing volume 120. The substrate 103 can be placed on the substrate support 104, and process gases can flow through the lid assembly 106 using the inlet 114 according to any desired flow plan. The gases can exit the processing chamber 100 through the outlet 152. Power can be coupled with the gas distributor 112 to establish a plasma within the processing volume 120. In some embodiments, the substrate can be subjected to an electrical bias using the third electrode 124.

[0027]

[0029] Upon energizing the plasma in the process volume 120, a potential difference may be established between the plasma and the first electrode 108. A potential difference may also be established between the plasma and the second electrode 122. The electronic controllers 134, 140 may then be used to adjust the flow characteristics of the ground paths represented by the two adjustment circuits 128 and 136. Set points may be provided to the first adjustment circuit 128 and the second adjustment circuit 136 to provide independent control of the deposition rate and center-to-edge plasma density uniformity. In an embodiment where the electronic controllers can both be variable capacitors, the electronic sensor may adjust the variable capacitors to maximize the deposition rate and independently minimize the thickness non-uniformity.

[0028]

[0030] Each of the conditioning circuits 128, 136 may have a variable impedance that can be adjusted using the respective electronic controller 134, 140. If the electronic controller 134, 140 is a variable capacitor, the capacitance range of each variable capacitor and the inductance of the first inductor 132A and the second inductor 132B may be selected to provide an impedance range. This range may depend on the frequency and voltage characteristics of the plasma, and the capacitance range of each variable capacitor may be minimum. Thus, when the capacitance of the first electronic controller 134 is minimum or maximum, the impedance of the first conditioning circuit 128 may be high, resulting in a plasma shape with minimum aerial or lateral reach on the substrate support. When the capacitance of the first electronic controller 134 approaches a value that minimizes the impedance of the first conditioning circuit 128, the aerial reach of the plasma is maximized, effectively covering the entire working area of ​​the substrate support 104. As the capacitance of the first electronic controller 134 deviates from the minimum impedance setting, the plasma shape may shrink from the chamber walls and the aerial coverage of the substrate support may decrease. The second electronic controller 140 may have a similar effect, increasing and decreasing the aerial coverage of the plasma above the substrate support as the capacitance of the second electronic controller 140 may change.

[0029]

[0031] The electronic sensors 130, 138 may be used to regulate the respective circuits 128, 136 in a closed loop. Depending on the sensor type used, a current or voltage set point may be attached to each sensor, which may be equipped with control software that determines adjustments to the respective electronic controllers 134, 140 to minimize deviations from the set point. As a result, the plasma shape may be selected and dynamically controlled during processing. Although the above discussion is based on the electronic controllers 134, 140 being variable capacitors, it should be understood that any electronic component with adjustable characteristics may be used to provide adjustable impedance to the regulation circuits 128 and 136.

[0030]

[0032] FIG. 2 illustrates exemplary operations in a deposition method 200 according to some embodiments of the present technique. The method can be performed in a variety of processing chambers, including the processing chamber 100 described above. The method 200 can include several optional operations that may or may not be specifically associated with some embodiments of the method according to the present technique. For example, many of the operations are described to provide a broader scope of structure formation, but are not critical to the technique or may be performed by alternative methodologies as will be readily understood. The method 200 can illustrate operations as shown diagrammatically in FIGS. 3A-3C, which are described in conjunction with the operations of the method 200. It should be understood that the figures show only partial schematic views, and that the substrate support can include any number of additional materials and features having various properties and aspects, as shown in the figures.

[0031]

[0033] Method 200 may include additional operations prior to the initiation of the listed operations. For example, the additional processing operations may include forming structures on the semiconductor substrate, which may include both the formation and removal of materials. Pre-processing operations may be performed in the chamber in which method 200 may be performed, or processing may be performed in one or more other processing chambers prior to delivering the substrate to the semiconductor processing chamber in which method 200 may be performed. In either case, method 200 may optionally include delivering the semiconductor substrate to a processing region of a semiconductor processing chamber, such as processing chamber 100 described above, or other chamber, which may include the components described above. The substrate may be deposited on a substrate support, which may be a pedestal, such as substrate support 104, which may be present in a processing region of a chamber, such as processing volume 120 described above. An exemplary substrate 305 prior to the initiation of deposition is shown in FIG. 3A.

[0032]

[0034] The substrate 305 may be any number of materials on which materials may be deposited. The substrate may be or include silicon, germanium, a dielectric material including silicon oxide or silicon nitride, a metallic material, or any number of combinations of these materials, which may be the substrate 305 or a material formed on the substrate 305. In some embodiments, optional processing operations such as pretreatment may be performed to prepare the surface of the substrate 305 for deposition. For example, pretreatment may be performed to provide certain ligand terminations on the surface of the substrate, which may facilitate nucleation of the film to be deposited. Additionally, removal of material, such as reduction of native oxides or etching of material, or any other operation that may prepare one or more exposed surfaces of the substrate 305 for deposition may be performed.

[0033]

[0035] In operation 205, one or more precursors may be delivered to the processing region of the chamber. For example, in an exemplary embodiment where a silicon-containing film including a silicon oxide film may be formed, a silicon-containing precursor may be delivered to the processing region of the processing chamber. The silicon-containing precursor may be a silicon-oxygen-containing precursor in some embodiments. Along with the silicon-containing precursor, a carrier precursor may be delivered, which in some embodiments may be or include an inert or noble metal precursor. In some embodiments of the present technique, plasma-enhanced deposition may be performed, which may facilitate the reaction and deposition of the material. As described above, some embodiments of the present technique may involve the formation or deposition of silicon-oxygen materials, which may be conventionally characterized by certain porosity and stress, as well as additional effects that may occur upon subsequent exposure to air or high temperatures.

[0034]

[0036] The delivered precursors may be used to form a plasma in a processing region of the semiconductor processing chamber in operation 210. In operation 215, a silicon-containing material 307 may be deposited on a substrate 305, as may be shown in FIG. 3B. As described further below, the deposition may be a first amount of silicon-containing material, which may be formed or deposited in contact with and / or over the substrate. The deposition of the first amount of material may occur at a first set of processing conditions, and may produce a bulk layer of material of any thickness that may be beneficial in a particular process. For example, embodiments of the present technology may be used to produce films characterized by any thickness, such as from a few nanometers or less to a few micrometers or more.

[0035]

[0037] The first set of chamber conditions may include any number of process conditions or parameters under which deposition may be performed. For example, deposition may occur under a set of conditions that may include, by way of example, chamber temperature, precursors, pressure, plasma power, precursor flow rates, deposition time, and any number of other chamber conditions, which may constitute a first set of conditions under which a first amount of material may be deposited. In operation 220, one or more chamber conditions may be adjusted to a second condition, thereby generating a second set of chamber conditions. The adjustment may occur, for example, while deposition continues, or the process may be stopped and resumed at a separate interruption while conditions are adjusted. Next, as shown in FIG. 3C, a second amount of silicon-containing material 310 may be deposited in operation 225, which may occur under a second set of chamber conditions. The first amount of material and the second amount of material may together generate a combined layer of material.

[0036]

[0038] During the transition between the first set of chamber conditions and the second set of chamber conditions, any number of conditions can be maintained or adjusted. For example, the adjustment may include changing one or more conditions of the first set of conditions while maintaining one or more other conditions of the first set of conditions. The conditions can be adjusted to change one or more film properties of the material to be deposited. For example, in some embodiments, one or more film properties can be adjusted, but the material of the first amount of material can be the same material as the second amount of material. For example, the second amount of material can be characterized by an increased density compared to the first amount of material in embodiments of the present technology and can provide a protective or sealing layer around the first amount of material, such as a bulk layer of material. The second amount of material can protect against both outgassing from the first amount of material and ingress of oxygen when the substrate is exposed to the atmosphere, such as when the substrate may be removed from the vacuum environment, as in optional operation 230.

[0037]

[0039] Regarding the silicon-containing precursor and the carrier precursor, any number of precursors can be used in the present technology. For example, the silicon-containing precursor can include any silicon-containing material, such as an organosilane, which can include silane, disilane, and other materials. The additional silicon-containing material can include silicon, carbon, oxygen, or nitrogen, such as, for example, tetraethylorthosilicate or trisilylamine. In some embodiments, the additional precursor can be delivered with the silicon-containing precursor, such as an oxygen-containing precursor, a nitrogen-containing precursor, or any other precursor. The carrier precursor can be or include an inert or noble gas, such as argon, helium, krypton, xenon, or other precursor that may promote plasma generation or process effects, such as, for example, ion bombardment.

[0038]

[0040] The pressure in the processing region can affect the amount of ionization and bombardment carried out during deposition, which can affect the density of the film produced. Thus, in some embodiments, adjusting the process conditions can include changing the pressure in the processing region from a first chamber pressure to a second chamber pressure. Reducing the processing pressure can increase ion bombardment by increasing the mean free path between atoms and increasing the energy and bombardment at the film surface. Increasing the bombardment can produce a film characterized by increased density. Thus, in some embodiments, the processing pressure can be reduced between the deposition of the first amount and the deposition of the second amount, which can produce a denser surface layer to protect against outgassing and oxygen ingress, as explained above.

[0039]

[0041] The first set of conditions can include a pressure in the process chamber of 50 Torr or less, and can be about 40 Torr or less, about 30 Torr or less, about 20 Torr or less, about 15 Torr or less, about 12 Torr or less, about 10 Torr or less, or less. After a sufficient amount of bulk deposition has been performed, the pressure can be stepped down or reduced to a second chamber pressure to produce a second amount of material. For example, the second chamber pressure can be about 15 Torr or less, and can be about 12 Torr or less, about 10 Torr or less, about 9 Torr or less, about 8 Torr or less, about 7 Torr or less, about 6 Torr or less, about 5 Torr or less, about 4 Torr or less, about 3 Torr or less, about 2 Torr or less, about 1 Torr, or less. Regardless of the first chamber pressure, a delta chamber pressure can be generated between the first chamber pressure and the second chamber pressure, which can be about 1 Torr or greater, about 2 Torr or greater, about 4 Torr or greater, about 6 Torr or greater, about 8 Torr or greater, about 10 Torr or greater, or more.

[0040]

[0042] The method 200 can perform deposition at one or more process temperatures, which may be about 200° C. or higher, about 250° C. or higher, about 300° C. or higher, about 350° C. or higher, about 400° C. or higher, about 450° C. or higher, about 500° C. or higher, or more. Furthermore, the silicon-containing precursor, which may be a silicon-oxygen containing precursor, can be characterized by a flow rate that can be maintained during deposition of the first amount of silicon-containing material and the second amount of silicon-containing material. For example, the flow of the silicon-containing precursor can be maintained during adjustment between the first set of conditions and the second set of conditions. In some embodiments, the flow rate of the silicon-containing precursor can be increased or decreased between the first set of conditions and the second set of conditions.

[0041]

[0043] Similarly, the flow rate of the carrier precursor can also be adjusted between the deposition of the first amount and the deposition of the second amount, for example, from a first volumetric flow rate to a second volumetric flow rate that is greater than the first volumetric flow rate. For example, the partial pressure of the silicon-containing precursor can be reduced by increasing the amount of carrier precursor, such as argon. In the case of a silicon-oxygen-containing precursor, this can increase the incorporation of oxygen at the film surface and reduce the amount of carbon and / or hydrogen incorporated in the film. The increased argon can increase the bombardment at the surface, which can densify the film and further remove incorporated carbon or hydrogen.

[0042]

[0044] Thus, in some embodiments, the second volumetric flow rate may be at least about 10% greater than the first volumetric flow rate, at least about 20%, at least about 30%, at least about 40%, at least about 50%, at least about 60%, at least about 70%, at least about 80% greater. It may be greater, at least about 90% greater, at least about 100% greater, at least about 120% greater, at least about 140% greater, at least about 160% greater, at least about 180% greater, at least about 200% greater, or greater. In some embodiments, one or more conditions may be adjusted together or simultaneously during the transition, such as, for example, by simultaneously decreasing the pressure and increasing the volumetric flow rate of the carrier precursor. Any number of process parameters may be adjusted, including those described or other relevant parameters.

[0043]

[0045] As previously mentioned, the second amount of silicon-containing material can be characterized by an increased density compared to the first amount of silicon-containing material. This can also create increased stress characteristics in the second amount of silicon-containing material, which can otherwise increase the compressive stress of the combination film. Thus, in some embodiments, the second amount of silicon-containing material can be limited in thickness. For example, the first amount of silicon-containing material can be characterized by a compressive stress of -100 MPa or less, -90 MPa or less, about -80 MPa or less, about -70 MPa or less, about -60 MPa or less, about -50 MPa or less, about -40 MPa or less, or less. The second amount of silicon-containing material can be characterized by a compressive stress of -100 MPa or greater, and can be characterized by a film compressive stress of about -120 MPa or greater, about -140 MPa or greater, about -160 MPa or greater, about -180 MPa or greater, about -200 MPa or greater, about -220 MPa or greater, about -240 MPa, about -260 MPa or greater, about -280 MPa or greater, about -300 MPa or greater, or higher.

[0044]

[0046] If the second silicon-containing material were to be sufficiently thick, the overall compressive stress of the combined layer could cause any of the aforementioned problems. Thus, in some embodiments, the second amount of silicon-containing material can be maintained at a thickness of about 150 nm or less, about 130 nm or less, about 110 nm or less, about 100 nm or less, about 90 nm or less, about 80 nm or less, about 70 nm or less, about 60 nm or less, about 50 nm or less, about 40 nm or less, about 30 nm or less, about 20 nm or less, about 10 nm or less, about 5 nm or less, about 1 nm or less, or less.

[0045]

[0047] Additionally, to ensure controlled outgassing due to increased processing temperatures and limit ingress of atmospheric moisture, the second amount of silicon-containing material can be maintained at a thickness of about 0.5 nm or more, about 1 nm or more, about 5 nm or more, about 10 nm or more, about 15 nm or more, about 20 nm or more, about 25 nm or more, about 30 nm or more, or more. The minimum thickness to provide the associated benefits can be related, at least in part, to the density of the second amount of material. For example, the denser the material formed, the thinner the layer. However, compressive stress can also increase as the layer becomes denser, and thus the density or stress and thickness of the second amount of material can be controlled to provide the associated benefits while limiting the effects of increased compressive stress.

[0046]

[0048] Depending on the process conditions, deposition of a first amount of material may be performed for a first time and deposition of a second amount of material may be performed for a second time that is shorter than the first time. For example, in some embodiments, to limit the thickness of the second amount of material, the second time may be about 30 seconds or less, about 25 seconds or less, about 20 seconds or less, about 15 seconds or less, about 10 seconds or less, about 5 seconds or less, or less.

[0047]

[0049] By creating a relatively thin layer of denser material over the bulk material, shrinkage of the film can be limited or substantially prevented while maintaining the desired stress characteristics of the combined film. For example, depending on the thickness of the first and second amounts of material, the combined layer can be characterized by an overall compressive stress of about -70 MPa or less, about -65 MPa or less, about -60 MPa or less, about -55 MPa or less, or less. Furthermore, shrinkage of the film can be reduced by about 10% or more, about 15% or more, about 20% or more, about 25% or more, about 30% or more, about 35% or more, about 40% or more, about 45% or more, about 50% or more, about 55% or more, about 60% or more, or more, compared to a film without a sealing layer during subsequent processing or exposure to air.

[0048]

[0050] In the foregoing description, for purposes of explanation, numerous details are set forth in order to provide an understanding of various embodiments of the present technology. However, it will be apparent to one skilled in the art that particular embodiments may be practiced without some of these details, or with additional details.

[0049]

[0051] Although several embodiments have been disclosed, those skilled in the art will recognize that various modifications, alternative constructions, and equivalents may be used without departing from the spirit of the embodiments. Moreover, some well-known processes and elements have not been described to avoid unnecessarily obscuring the present technology. Thus, the above description should not be interpreted as limiting the scope of the present technology. Furthermore, although a method or process may be described sequentially or stepwise, it should be understood that the operations may be performed simultaneously or in a different order than that described.

[0050]

[0052] Where a range of values ​​is presented, unless the context clearly dictates otherwise, it is understood that each intervening value between the upper and lower limits of that range is also specifically disclosed to the smallest unit of the unit of the lower limit. Any narrower range between any stated or unstated intervening value in a stated range, as well as any other stated or intervening value in that stated range, are also encompassed. The upper and lower limits of these smaller ranges may be individually included or excluded in the range, and each range in which either, neither, or both limits are included in the narrower range is also encompassed within the technology, subject to the specifically excluded limit in the stated range. Where a stated range includes one or both of the limits, ranges excluding either or both of the included limits are also included.

[0051]

[0053] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly indicates otherwise. Thus, for example, reference to "a precursor" includes a reference to a plurality of such precursors, reference to "a layer" includes a reference to one or more layers and equivalents thereof known to those skilled in the art, and so forth.

[0052]

[0054] Additionally, the terms "comprise(s)", "comprising", "contain(s)", "containing", "include(s)", and "including", when used in this specification and claims, are intended to specify the presence of stated features, integers, components, or steps, but do not exclude the presence or addition of one or more other features, integers, components, steps, operations, or groups.

Claims

1. delivering a silicon-containing precursor and a carrier precursor to a processing region of a semiconductor processing chamber; forming a plasma of the silicon-containing precursor and the support precursor in the processing region of the semiconductor processing chamber; depositing a first amount of a silicon-containing material onto a substrate disposed in the processing region of the semiconductor processing chamber, the depositing occurring at a first chamber pressure; adjusting the first chamber pressure to a second chamber pressure lower than the first chamber pressure; and depositing a second amount of the silicon-containing material onto the first amount of the silicon-containing material. Including, a substrate temperature is maintained at or above 300° C. during deposition of the first amount of the silicon-containing material and the second amount of the silicon-containing material; The deposition method of claim 1, wherein the second amount of the silicon-containing material is characterized by a higher density than the first amount of the silicon-containing material.

2. The deposition method of claim 1, wherein the silicon-containing precursor is a silicon-oxygen-containing precursor and the silicon-containing material comprises silicon oxide.

3. 2. The deposition method of claim 1, wherein the first chamber pressure is less than or equal to 20 Torr and the second chamber pressure is less than or equal to 10 Torr.

4. 10. The method of claim 1, further comprising increasing a volumetric flow rate of the support precursor while adjusting the first chamber pressure to the second chamber pressure, the support precursor comprising argon.

5. 2. The deposition method of claim 1, wherein the silicon-containing precursor comprises tetraethylorthosilicate and the second amount of the silicon-containing material is characterized by a thickness of 100 nm or less.

6. delivering a silicon-containing precursor and a carrier precursor to a processing region of a semiconductor processing chamber; forming a plasma of the silicon-containing precursor and the support precursor in the processing region of the semiconductor processing chamber; depositing a first amount of silicon-containing material onto a substrate disposed in the processing region of the semiconductor processing chamber, the depositing occurring at a first chamber pressure; adjusting the support precursor from a first volumetric flow rate to a second volumetric flow rate greater than the first volumetric flow rate; and depositing a second amount of the silicon-containing material onto the first amount of the silicon-containing material. Including, The method of deposition, wherein a substrate temperature is maintained at or above 300° C. during deposition of the first amount of the silicon-containing material and the second amount of the silicon-containing material.

7. 7. The deposition method of claim 6, wherein the silicon-containing precursor is a silicon-oxygen-containing precursor, the silicon-containing material comprises silicon oxide, and the second volumetric flow rate is more than 50% greater than the first volumetric flow rate.

8. 7. The method of claim 6, further comprising adjusting the first chamber pressure to a second chamber pressure lower than the first chamber pressure while adjusting the support precursor from the first volumetric flow rate to the second volumetric flow rate.

9. 9. The deposition method of claim 8, wherein the first chamber pressure is less than or equal to 15 Torr and the second chamber pressure is less than or equal to 7 Torr.

10. 7. The deposition method of claim 6, wherein the second amount of the silicon-containing material is characterized by a thickness of 100 nm or less, and the second amount of the silicon-containing material is characterized by a compressive stress equal to or greater than a compressive stress associated with the first amount of the silicon-containing material.

11. delivering a silicon-oxygen containing precursor and a carrier precursor to a processing region of a semiconductor processing chamber; forming a plasma of the silicon-oxygen containing precursor and the support precursor in the processing region of the semiconductor processing chamber; depositing a first amount of a silicon-oxygen containing material onto a substrate disposed in the processing region of the semiconductor processing chamber, the depositing occurring at a first chamber pressure; adjusting the first chamber pressure to a second chamber pressure lower than the first chamber pressure; increasing the volumetric flow rate of the support precursor while adjusting the chamber pressure; and depositing a second amount of the silicon-oxygen containing material on the first amount of the silicon-oxygen containing material. Including, The deposition method, wherein a substrate temperature is maintained at or above 300° C. during deposition of the first amount of the silicon-oxygen containing material and the second amount of the silicon-oxygen containing material.

12. 12. The deposition method of claim 11, wherein the first chamber pressure is less than or equal to 20 Torr and the second chamber pressure is less than or equal to 10 Torr, the silicon-oxygen containing precursor comprises tetraethylorthosilicate, and the support precursor comprises argon.

13. 12. The method of claim 11, wherein the first amount of the silicon-oxygen containing material is deposited for a first period of time and the second amount of the silicon-oxygen containing material is deposited for a second period of time that is shorter than the first period of time.

Citation Information

Patent Citations

  • Non-volatile memory having silicon nitride charge trap layer

    CN103280446A

  • Method to enable high temperature processing without chamber drifting

    CN110140193A

  • Non-volatile memory with silicon nitride charge trap layer

    JP2012506640A

  • Method and precursors for manufacturing 3D devices

    JP2016149537A

  • Methods of depositing high performance coatings and encapsulated electronic devices

    JP2016523442A