SUBSTRATE PROCESSING METHOD, SEMICONDUCTOR DEVICE MANUFACTURING METHOD, SUBSTRATE PROCESSING APPARATUS, AND PROGRAM

JP7594610B2Active Publication Date: 2024-12-04KOKUSAI DENKI KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022571474
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-24
Filing Date
2021-12-21
Publication Date
2024-12-04
Estimated Expiration
2041-12-21

AI Technical Summary

Benefits of technology

【0007】 本開示によれば、プラズマを用いて低温で高品質な膜を形成する技術を提供することが可能となる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594610000001
    Figure 0007594610000001
  • Figure 0007594610000002
    Figure 0007594610000002
  • Figure 0007594610000003
    Figure 0007594610000003
Patent Text Reader

Abstract

The present invention has a step for forming a film on a substrate by performing, a prescribed number of times, a cycle including: a step for supplying a raw material gas to a substrate in a treatment container; (b) a step for exciting a nitrogen and hydrogen containing gas to a plasma state and supplying the excited gas to the substrate in the treatment container; and (c) a step for exciting an inert gas to a plasma state and supplying the excited inert gas to the substrate in the treatment container, wherein the pressure in the treatment container in step (c) is lower than that in step (b).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a substrate processing method, a semiconductor device manufacturing method, a substrate processing apparatus, and a program. [Background technology]

[0002] Semiconductor devices, such as memory devices such as flash memories and DRAMs, and logic devices such as CPUs, are required to become more highly integrated every year. To achieve high integration, a technology is required to form an extremely thin film on a fine circuit pattern with high precision. For example, a method of alternately supplying a source gas and a reactive gas to a substrate is one of the film formation methods. In recent years, the wiring dimensions have tended to become finer, so it is important to improve the uniformity of the film thickness and film quality of the film formed on the substrate and the reproducibility of these. In addition, with the changes in structure and materials in next-generation devices, a film formation technology that can obtain high-quality films at low temperatures is required.

[0003] An example of a film formed on a substrate is a silicon nitride film (SiN film), and the SiN film may be used as an etching stopper layer when etching a silicon oxide film (SiO film) or the like using, for example, a hydrogen fluoride (HF) aqueous solution. One of the deposition techniques for forming a SiN film is a technique for forming a film at a low temperature using plasma (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-93551 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when a film is formed at a low temperature using plasma, the wet etching resistance of the film may decrease, and the film quality may deteriorate. An object of the present disclosure is to provide a technology for forming a high-quality film at a low temperature using plasma. [Means for solving the problem]

[0006] According to one aspect of the present disclosure, (a) supplying a source gas to a substrate in a processing chamber; (b) exciting a nitrogen and hydrogen containing gas into a plasma state and supplying the gas to the substrate in the processing chamber; (c) exciting an inert gas into a plasma state and supplying the gas to the substrate in the processing chamber; forming a film on the substrate by performing a cycle including the steps of: A technique is provided for lowering the pressure in the processing vessel in (c) below the pressure in the processing vessel in (b). Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a technique for forming a high-quality film at a low temperature using plasma. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus suitably used in one embodiment of the present disclosure, showing a processing furnace 202 portion in vertical cross section. [Diagram 2] FIG. 2 is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus preferably used in one embodiment of the present disclosure, and shows a processing furnace 202 portion in a cross-sectional view taken along line AA in FIG. [Diagram 3] FIG. 3 is a schematic configuration diagram of a controller 121 of a substrate processing apparatus suitably used in one embodiment of the present disclosure, and is a block diagram showing a control system of the controller 121. [Figure 4]FIG. 4 is a schematic configuration diagram of an electrode unit in a substrate processing apparatus suitably used in one embodiment of the present disclosure, and is a perspective view of the electrode unit. [Diagram 5] FIG. 5 is a diagram illustrating an example of a processing sequence according to an embodiment of the present disclosure. [Figure 6] FIG. 6 is a diagram showing an example of a processing sequence in the first modification of the present disclosure. [Figure 7] Fig. 7(a) is a diagram showing an example in which the intervals between the multiple wafers 200 are set to the intervals between the wafers 200 when the boat 217 supports the maximum number of wafers 200 that can be supported by the boat 217. Fig. 7(b) is a diagram showing an example in which the intervals between the multiple wafers 200 are set to more than twice the intervals between the wafers 200 when the boat 217 supports the maximum number of wafers 200 that can be supported by the boat 217. Fig. 7(c) is a diagram showing an example in which the intervals between the multiple wafers 200 are set to more than four times the intervals between the wafers 200 when the boat 217 supports the maximum number of wafers 200 that can be supported by the boat 217. [Figure 8] FIG. 8 is a diagram showing the measurement results of the wet etching rate (WER) and film thickness of the SiN film of evaluation sample 1 within the wafer surface. [Figure 9] FIG. 9 is a diagram showing the measurement results of the WER and film thickness in the wafer surface of the SiN film of evaluation sample 2. In FIG. [Figure 10] FIG. 10 is a diagram showing the measurement results of the WER and film thickness in the wafer surface of the SiN film of evaluation sample 3. In FIG. [Figure 11] FIG. 11 is a diagram showing the measurement results of the WER and film thickness in the wafer surface of the SiN film of evaluation sample 4. In FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <One aspect of the present disclosure> Hereinafter, one embodiment of the present disclosure will be described mainly with reference to Figures 1 to 5 and 7(a) to 7(c). Note that the drawings used in the following description are all schematic, and the dimensional relationships of the elements, the ratios of the elements, etc. shown in the drawings do not necessarily match the actual ones. Furthermore, the dimensional relationships of the elements, the ratios of the elements, etc. between multiple drawings do not necessarily match.

[0010] (1) Configuration of the substrate processing device 1, the process furnace 202 has a heater 207 as a temperature regulator (heating unit). The heater 207 is cylindrical and is installed vertically by being supported by a holding plate. The heater 207 also functions as an activation mechanism (thermal excitation unit) that activates (excites) gas by heat.

[0011] A reaction tube 203 is disposed concentrically with the heater 207 inside the heater 207. The reaction tube 203 is made of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC) and is formed in a cylindrical shape with a closed upper end and an open lower end. A manifold 209 is disposed concentrically with the reaction tube 203 below the reaction tube 203. The manifold 209 is made of a metal material such as stainless steel (SUS) and is formed in a cylindrical shape with an open upper end and a closed lower end. The upper end of the manifold 209 engages with the lower end of the reaction tube 203 and is configured to support the reaction tube 203. An O-ring 220a is provided between the manifold 209 and the reaction tube 203 as a seal member. The reaction tube 203 is installed vertically like the heater 207. The reaction tube 203 and the manifold 209 mainly constitute a processing vessel (reaction vessel). A processing chamber 201 is formed in a cylindrical hollow portion of the processing vessel. The processing chamber 201 is configured to be capable of accommodating a wafer 200 as a substrate. In the processing chamber 201, i.e., in the processing vessel, processing is performed on the wafer 200.

[0012] Nozzles 249a to 249c serving as first to third supply units are provided in the processing chamber 201 so as to penetrate the sidewall of the manifold 209, respectively. The nozzles 249a to 249c are also referred to as first to third nozzles, respectively. The nozzles 249a to 249c are made of a heat-resistant material such as quartz or SiC. Gas supply pipes 232a to 232c are connected to the nozzles 249a to 249c, respectively. The nozzles 249a to 249c are different nozzles, and each of the nozzles 249a and 249c is provided adjacent to the nozzle 249b.

[0013] Gas supply pipes 232a-232c are provided with mass flow controllers (MFCs) 241a-241c, which are flow rate controllers (flow rate control parts), and valves 243a-243c, which are on-off valves, in order from the upstream side of the gas flow. Gas supply pipes 232d-232f are connected to the gas supply pipes 232a-232c downstream of the valves 243a-243c. Gas supply pipes 232d-232f are provided with MFCs 241d-241f and valves 243d-243f, which are provided from the upstream side of the gas flow. Gas supply pipes 232a-232f are made of a metal material, such as SUS.

[0014] As shown in FIG. 1 and FIG. 2, the nozzles 249a to 249c are provided in a circular space between the inner wall of the reaction tube 203 and the wafers 200 in a plan view, from the lower part to the upper part of the inner wall of the reaction tube 203, so as to rise upward in the arrangement direction of the wafers 200. That is, the nozzles 249a to 249c are provided in a region horizontally surrounding the wafer arrangement region on the side of the wafer arrangement region in which the wafers 200 are arranged, so as to extend along the wafer arrangement region. In a plan view, the nozzle 249b is disposed so as to face an exhaust port 231a (described later) on a straight line across the center of the wafer 200 loaded into the processing chamber 201. The nozzles 249a and 249c are disposed so as to sandwich a straight line L passing through the nozzle 249b and the center of the exhaust port 231a from both sides along the inner wall of the reaction tube 203 (the outer periphery of the wafers 200). The straight line L is also a straight line passing through the nozzle 249b and the center of the wafer 200. In other words, the nozzle 249c can be said to be provided on the opposite side of the nozzle 249a with the straight line L in between. The nozzles 249a and 249c are arranged symmetrically, that is, symmetrically, with the straight line L as the axis of symmetry. Gas supply holes 250a to 250c for supplying gas are provided on the side surfaces of the nozzles 249a to 249c, respectively. The gas supply holes 250a to 250c are each opened to face (face) the exhaust port 231a in a plan view, and can supply gas toward the wafer 200. A plurality of gas supply holes 250a to 250c are provided from the lower part to the upper part of the reaction tube 203.

[0015] From the gas supply pipe 232a, a raw material (raw material gas) is supplied into the processing chamber 201 via the MFC 241a, the valve 243a, and the nozzle 249a.

[0016] From the gas supply pipe 232b, a reactant (reaction gas), for example, a gas containing nitrogen (N) and hydrogen (H), is supplied into the processing chamber 201 via the MFC 241b, the valve 243b, and the nozzle 249b. The N and H containing gas acts as an N source (nitrogen source, nitriding gas, nitriding agent).

[0017] From the gas supply pipe 232c, a reactant (reaction gas), for example, an oxygen (O)-containing gas, is supplied into the processing chamber 201 via the MFC 241c, the valve 243c, and the nozzle 249c. The O-containing gas acts as an O source (oxygen source, oxidizing gas, oxidizing agent).

[0018] From the gas supply pipes 232d-232f, an inert gas is supplied into the processing chamber 201 via the MFCs 241d-241f, the valves 243d-243f, the gas supply pipes 232a-232c, and the nozzles 249a-249c, respectively. The inert gas acts as a purge gas, a carrier gas, a dilution gas, etc. As will be described later, the inert gas can be excited into a plasma state in the processing chamber 201 and then supplied. In that case, the inert gas can also act as a modifying gas.

[0019] A raw material gas supply system is mainly composed of the gas supply pipe 232a, the MFC 241a, and the valve 243a. An N- and H-containing gas supply system (reactive gas supply system) is mainly composed of the gas supply pipe 232b, the MFC 241b, and the valve 243b. An O-containing gas supply system (reactive gas supply system) is mainly composed of the gas supply pipe 232c, the MFC 241c, and the valve 243c. An inert gas supply system is mainly composed of the gas supply pipes 232d to 232f, the MFCs 241d to 241f, and the valves 243d to 243f. As described above, when an inert gas acts as a modifying gas, the inert gas supply system can also be called a modifying gas supply system.

[0020] Any or all of the various gas supply systems described above may be configured as an integrated gas supply system 248 in which the valves 243a-243f, MFCs 241a-241f, etc. are integrated. The integrated gas supply system 248 is connected to the gas supply pipes 232a-232f, respectively, and is configured so that the supply operation of various gases into the gas supply pipes 232a-232f, i.e., the opening and closing operation of the valves 243a-243f and the flow rate adjustment operation by the MFCs 241a-241f, etc., are controlled by a controller 121, which will be described later. The integrated gas supply system 248 is configured as an integrated or separate type integrated unit, and can be attached and detached to and from the gas supply pipes 232a-232f, etc., in units of integrated units, and is configured so that maintenance, replacement, expansion, etc. of the integrated gas supply system 248 can be performed in units of integrated units.

[0021] An exhaust port 231a for exhausting the atmosphere in the processing chamber 201 is provided at the lower side of the side wall of the reaction tube 203. As shown in FIG. 2, the exhaust port 231a is provided at a position facing the nozzles 249a to 249c (gas supply holes 250a to 250c) across the wafer 200 in a plan view. The exhaust port 231a may be provided along the side wall of the reaction tube 203 from the lower part to the upper part, that is, along the wafer arrangement area. An exhaust pipe 231 is connected to the exhaust port 231a. The exhaust pipe 231 is made of a metal material such as SUS. A vacuum pump 246 as a vacuum exhaust device is connected to the exhaust pipe 231 via a pressure sensor 245 as a pressure detector (pressure detection unit) for detecting the pressure in the processing chamber 201 and an APC (Auto Pressure Controller) valve 244 as a pressure regulator (pressure adjustment unit). The APC valve 244 can evacuate and stop the evacuation of the processing chamber 201 by opening and closing the valve while the vacuum pump 246 is operating, and further, can adjust the pressure in the processing chamber 201 by adjusting the valve opening based on pressure information detected by the pressure sensor 245 while the vacuum pump 246 is operating. The APC valve 244 can also be called an exhaust valve. An exhaust system is mainly configured by the exhaust pipe 231, the APC valve 244, and the pressure sensor 245. The vacuum pump 246 may be included in the exhaust system.

[0022] Below the manifold 209, a seal cap 219 is provided as a furnace port cover body capable of airtightly closing the lower end opening of the manifold 209. The seal cap 219 is made of a metal material such as SUS, and is formed in a disk shape. An O-ring 220b is provided on the upper surface of the seal cap 219 as a seal member that abuts against the lower end of the manifold 209. Below the seal cap 219, a rotation mechanism 267 is provided for rotating the boat 217, which will be described later. A rotation shaft 255 of the rotation mechanism 267 is made of a metal material such as SUS, and is connected to the boat 217 through the seal cap 219. The rotation mechanism 267 is configured to rotate the wafers 200 by rotating the boat 217. The seal cap 219 is configured to be vertically raised and lowered by a boat elevator 115 as a lifting mechanism installed outside the reaction tube 203. The boat elevator 115 is configured as a transfer device (transfer mechanism) that transfers the wafers 200 into and out of the processing chamber 201 by raising and lowering the seal cap 219.

[0023] A shutter 219s is provided below the manifold 209 as a furnace port cover that can airtightly close the lower end opening of the manifold 209 when the seal cap 219 is lowered and the boat 217 is carried out of the processing chamber 201. The shutter 219s is made of a metal material such as SUS and is formed in a disk shape. An O-ring 220c is provided on the upper surface of the shutter 219s as a seal member that comes into contact with the lower end of the manifold 209. The opening and closing operation (lifting and lowering operation, rotating operation, etc.) of the shutter 219s is controlled by a shutter opening and closing mechanism 115s.

[0024] The boat 217 as a support for supporting the substrate is configured to support a plurality of wafers 200, for example, 25 to 200, in a horizontal position and aligned vertically with their centers aligned with each other in multiple stages. That is, the boat 217 is configured to arrange the plurality of wafers 200 in a horizontal position and spaced apart vertically. The boat 217 is made of a heat-resistant material such as quartz or SiC. At the bottom of the boat 217, heat insulating plates 218 made of a heat-resistant material such as quartz or SiC are supported in multiple stages. As shown in FIG. 7(a) to FIG. 7(c), the boat 217 has a plurality of columns 217a, for example, three to four columns 217a, and a plurality of support parts 217b provided on each of the columns 217a, and is configured to support a plurality of wafers 200 by each of the plurality of support parts 217b.

[0025] A temperature sensor 263 serving as a temperature detector is installed in the reaction tube 203. By adjusting the power supply to the heater 207 based on temperature information detected by the temperature sensor 263, the temperature distribution in the process chamber 201 becomes a desired one. The temperature sensor 263 is installed along the inner wall of the reaction tube 203.

[0026] An electrode 300 for generating plasma is provided outside the reaction tube 203, i.e., outside the processing vessel (processing chamber 201). By applying power to the electrode 300, it is possible to convert gas into plasma and excite it inside the reaction tube 203, i.e., inside the processing vessel (processing chamber 201), i.e., to excite the gas into a plasma state. Hereinafter, exciting the gas into a plasma state is also simply referred to as plasma excitation. The electrode 300 is configured to generate a capacitively coupled plasma (abbreviated as CCP) inside the reaction tube 203, i.e., inside the processing vessel (processing chamber 201), by applying power, i.e., high-frequency power (RF power).

[0027] 2, an electrode 300 and an electrode fixture 301 for fixing the electrode 300 are disposed between the heater 207 and the reaction tube 203. The electrode fixture 301 is disposed inside the heater 207, the electrode 300 is disposed inside the electrode fixture 301, and the reaction tube 203 is disposed inside the electrode 300.

[0028] As shown in FIG. 1 and FIG. 2, the electrode 300 and the electrode fixture 301 are provided in a space between the inner wall of the heater 207 and the outer wall of the reaction tube 203, which is annular in plan view, so as to extend from the lower part to the upper part of the outer wall of the reaction tube 203 in the arrangement direction of the wafers 200. The electrode 300 is provided parallel to the nozzles 249a to 249c. The electrode 300 and the electrode fixture 301 are arranged and disposed in a concentric arc shape with the reaction tube 203 and the heater 207 in plan view, and so as to be out of contact with the reaction tube 203 and the heater 207. The electrode fixture 301 is made of an insulating material (insulator) and is provided so as to cover at least a part of the electrode 300 and the reaction tube 203, so that the electrode fixture 301 can also be called a cover (insulating cover, insulating wall, insulating plate) or a cross-sectional arc cover (cross-sectional arc body, cross-sectional arc wall).

[0029] As shown in FIG. 2, a plurality of electrodes 300 are provided, and these electrodes 300 are fixed and installed on the inner wall of an electrode fixing tool 301. More specifically, as shown in FIG. 4, a protrusion (hook) 301a capable of hooking the electrode 300 is provided on the inner wall surface of the electrode fixing tool 301, and an opening 300c that is a through hole through which the protrusion 301a can be inserted is provided in the electrode 300. By hooking the electrode 300 on the protrusion 301a provided on the inner wall surface of the electrode fixing tool 301 through the opening 300c, the electrode 300 can be fixed to the electrode fixing tool 301. Note that FIG. 4 shows an example in which two openings 300c are provided in one electrode 300, and one electrode 300 is fixed by hooking it on two protrusions 301a, that is, an example in which one electrode 300 is fixed at two points. 2 shows an example in which nine electrodes 300 are fixed to one electrode fixture 301, while FIG. 4 shows an example in which twelve electrodes 300 are fixed to one electrode fixture 301.

[0030] The electrode 300 is made of an oxidation-resistant material such as nickel (Ni). The electrode 300 can be made of a metal material such as SUS, aluminum (Al), or copper (Cu), but by making the electrode 300 of an oxidation-resistant material such as Ni, deterioration of electrical conductivity can be suppressed, and a decrease in plasma generation efficiency can be suppressed. Furthermore, the electrode 300 can be made of a Ni alloy material to which Al is added. In this case, an aluminum oxide film (AlO film), which is an oxide film with high heat resistance and corrosion resistance, can be formed on the outermost surface of the electrode 300. The AlO film formed on the outermost surface of the electrode 300 acts as a protective film (block film, barrier film) and can suppress the progress of deterioration inside the electrode 300. This makes it possible to further suppress the decrease in plasma generation efficiency due to the decrease in electrical conductivity of the electrode 300. The electrode fixture 301 is made of an insulating material (insulator), for example, a heat-resistant material such as quartz or SiC. The material of the electrode fixture 301 is preferably the same as the material of the reaction tube 203.

[0031] As shown in FIG. 2, the electrode 300 includes a first electrode 300a and a second electrode 300b. The first electrode 300a is connected to a high frequency power source (RF power source) 320 via a matching unit 305. The second electrode 300b is grounded to earth and serves as a reference potential (0V). The first electrode 300a is also referred to as a hot electrode or a HOT electrode, and the second electrode 300b is also referred to as a ground electrode or a GND electrode. The first electrode 300a and the second electrode 300b are each configured as a plate-like member having a rectangular shape when viewed from the front. At least one first electrode 300a is provided, and at least one second electrode 300b is provided. FIGS. 1, 2, and 4 show an example in which a plurality of first electrodes 300a and a plurality of second electrodes 300b are provided. 2 shows an example in which six first electrodes 300a and three second electrodes 300b are provided on one electrode fixture 301, while FIG. 4 shows an example in which eight first electrodes 300a and four second electrodes 300b are provided on one electrode fixture 301. By applying RF power between the first electrode 300a and the second electrode 300b from the RF power source 320 via the matching device 305, plasma is generated in the region between the first electrode 300a and the second electrode 300b. This region is also referred to as a plasma generation region.

[0032] The surface area of ​​the first electrode 300a is preferably two or more times and three or less times the surface area of ​​the second electrode 300b. If the surface area of ​​the first electrode 300a is less than two times the surface area of ​​the second electrode 300b, the potential distribution may be narrowed, and the plasma generation efficiency may be reduced. If the surface area of ​​the first electrode 300a is more than three times the surface area of ​​the second electrode 300b, the potential distribution may spread to the edge portion of the wafer 200, and the wafer 200 may become an obstacle and the plasma generation efficiency may be saturated. In this case, discharge may also occur at the edge portion of the wafer 200, causing plasma damage to the wafer 200. By making the surface area of ​​the first electrode 300a two or more times and three or less times the surface area of ​​the second electrode 300b, it is possible to increase the plasma generation efficiency and suppress plasma damage to the wafer 200. 2, the electrodes 300 (first electrode 300a, second electrode 300b) are arranged in an arc shape in a plan view and are arranged at equal intervals, that is, so that the distances (gaps) between adjacent electrodes 300 (first electrode 300a, second electrode 300b) are equal. As described above, the electrodes 300 (first electrode 300a, second electrode 300b) are provided parallel to the nozzles 249a to 249c.

[0033] Here, the electrode fixture 301 and the electrode 300 (the first electrode 300a and the second electrode 300b) can also be referred to as an electrode unit. As shown in FIG. 2, the electrode unit is preferably arranged at a position avoiding the nozzles 249a to 249c, the temperature sensor 263, the exhaust port 231a, and the exhaust pipe 231. FIG. 2 shows an example in which two electrode units are arranged to face each other across the center of the wafer 200 (reaction tube 203), avoiding the nozzles 249a to 249c, the temperature sensor 263, the exhaust port 231a, and the exhaust pipe 231. FIG. 2 shows an example in which the two electrode units are arranged line-symmetrically, i.e., symmetrically, with respect to the straight line L as the axis of symmetry in a plan view. By arranging the electrode units in this manner, it is possible to arrange the nozzles 249a-249c, the temperature sensor 263, the exhaust port 231a, and the exhaust pipe 231 outside the plasma generation region in the processing chamber 201, thereby making it possible to suppress plasma damage to these components, wear and tear of these components, and breakage of these components, as well as generation of particles from these components.

[0034] A plasma excitation unit (activation mechanism) that excites (activates) a gas into a plasma state is mainly constituted by the electrodes 300, i.e., the first electrode 300a and the second electrode 300b. The plasma excitation unit may also include an electrode fixture 301, a matching box 305, and an RF power supply 320.

[0035] As shown in Fig. 3, the controller 121, which is a control unit (control means), is configured as a computer including a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, the storage device 121c, and the I / O port 121d are configured to be able to exchange data with the CPU 121a via an internal bus 121e. An input / output device 122 configured as, for example, a touch panel, is connected to the controller 121. An external storage device 123 can also be connected to the controller 121.

[0036] The storage device 121c is composed of, for example, a flash memory, a hard disk drive (HDD), a solid state drive (SSD), etc. A control program for controlling the operation of the substrate processing apparatus, a process recipe in which the procedure and conditions of the process described later are described, etc. are readably stored in the storage device 121c. The process recipe is a combination of procedures in the process described later that are executed by the controller 121 in the substrate processing apparatus to obtain a predetermined result, and functions as a program. Hereinafter, the process recipe, the control program, etc. are collectively referred to simply as a program. In addition, the process recipe is also simply referred to as a recipe. In this specification, when the word program is used, it may include only a recipe, only a control program, or both. The RAM 121b is configured as a memory area (work area) in which the program, data, etc. read by the CPU 121a are temporarily stored.

[0037] The I / O port 121d is connected to the above-mentioned MFCs 241a to 241f, valves 243a to 243f, pressure sensor 245, APC valve 244, vacuum pump 246, temperature sensor 263, heater 207, rotation mechanism 267, boat elevator 115, shutter opening / closing mechanism 115s, RF power supply 320, matching box 305, etc.

[0038] The CPU 121a is configured to read and execute a control program from the storage device 121c, and to read a recipe from the storage device 121c in response to an input of an operation command from the input / output device 122, etc. The CPU 121a is configured to control the flow rate adjustment operation of various gases by the MFCs 241a to 241f, the opening and closing operations of the valves 243a to 243f, the opening and closing operation of the APC valve 244 and the pressure adjustment operation by the APC valve 244 based on the pressure sensor 245, the start and stop of the vacuum pump 246, the temperature adjustment operation of the heater 207 based on the temperature sensor 263, the rotation and rotation speed adjustment operation of the boat 217 by the rotation mechanism 267, the lifting and lowering operation of the boat 217 by the boat elevator 115, the opening and closing operation of the shutter 219s by the shutter opening and closing mechanism 115s, the impedance adjustment operation by the matching device 305, the power supply to the RF power source 320, etc., in accordance with the contents of the read recipe.

[0039] The controller 121 can be configured by installing the above-mentioned program stored in the external storage device 123 in a computer. The external storage device 123 includes, for example, a magnetic disk such as an HDD, an optical disk such as a CD, a magneto-optical disk such as an MO, and a semiconductor memory such as a USB memory or an SSD. The storage device 121c and the external storage device 123 are configured as computer-readable recording media. Hereinafter, these are collectively referred to simply as recording media. When the term recording media is used in this specification, it may include only the storage device 121c alone, only the external storage device 123 alone, or both of them. The program may be provided to the computer using a communication means such as the Internet or a dedicated line without using the external storage device 123.

[0040] (2) Substrate processing An example of a process sequence for forming a nitride film, which is an insulating film, as a thin film on a wafer 200 as a substrate, as one step of a manufacturing process of a semiconductor device using the above-mentioned substrate processing apparatus, that is, a film formation sequence, will be described. In the following description, the operation of each part constituting the substrate processing apparatus is controlled by a controller 121.

[0041] In the processing sequence of this embodiment shown in FIG. (a) supplying a source gas to the wafer 200 in a processing chamber; (b) a step of exciting a N and H containing gas into a plasma state and supplying the gas to the wafer 200 in the processing chamber; (c) exciting an inert gas into a plasma state and supplying the gas to the wafer 200 in the processing chamber; Specifically, the method includes a step of forming a film on the wafer 200 by performing a cycle including the steps of: The pressure in the processing vessel in (c) is made lower than the pressure in the processing vessel in (b).

[0042] In this specification, such a processing sequence (gas supply sequence) may be expressed as follows for convenience: Similar notations will be used in the following descriptions of other aspects, modifications, and the like.

[0043] (raw material gas → plasma-excited N- and H-containing gas → plasma-excited inert gas) × n

[0044] 5 shows an example in which the pressure in the processing vessel in (c) is set lower than the pressure in the processing vessel in (a). Furthermore, FIG. 5 shows an example in which the pressure in the processing vessel in (c) is set lower than the pressure in the processing vessel in (b), and the pressure in the processing vessel in (b) is set lower than the pressure in the processing vessel in (a).

[0045] 5 shows an example in which the time for which the inert gas is excited into a plasma state and supplied in (c) is longer than the time for which the N- and H-containing gas is excited into a plasma state and supplied in (b), and also shows an example in which the time for which the inert gas is excited into a plasma state and supplied in (c) is longer than the time for which the raw material gas is supplied in (a). More specifically, FIG. 5 shows an example in which the time for which the inert gas is excited into a plasma state and supplied in (c) is longer than the time for which the N- and H-containing gas is excited into a plasma state and supplied in (b), and the time for which the N- and H-containing gas is excited into a plasma state and supplied in (b) is longer than the time for which the raw material gas is supplied in (a).

[0046] In addition, the processing sequence shown in FIG. 5 shows an example in which a cycle of (a), (b), and (c) is performed in this order is repeated multiple times (n times). In this case, n is an integer of 2 or more. FIG. 5 further shows an example in which after (a) is performed and before (b), the processing vessel is purged with an inert gas in a non-plasma atmosphere. Note that after (b) is performed and before (c), the processing vessel may be purged with an inert gas in a non-plasma atmosphere. In addition, when the cycle is performed multiple times, after (c) is performed and before (a), the processing vessel may be purged with an inert gas in a non-plasma atmosphere. This makes it possible to suppress the mixing of the gases in a plasma state in the processing vessel, the resulting unintended reaction, the generation of particles, and the like. These processing sequences can be expressed as follows. Note that purging performed in a non-plasma atmosphere is represented by P below.

[0047] (Source gas → P → plasma-excited N- and H-containing gas → plasma-excited inert gas) × n (Source gas → P → Plasma excited N and H containing gas → P → Plasma excited inert gas) × n (Source gas → P → Plasma excited N and H containing gas → Plasma excited inert gas → P) × n (Source gas → P → Plasma excited N and H containing gas → P → Plasma excited inert gas → P) × n

[0048] In (b), it is preferable to excite the N- and H-containing gas into a plasma state inside the processing vessel by applying power to the electrode 300 provided outside the processing vessel. In (c), it is preferable to excite the inert gas into a plasma state inside the processing vessel by applying power to the electrode 300 provided outside the processing vessel.

[0049] In (a), it is preferable to supply the raw material gas to the wafer 200 from the side of the wafer 200. In (b), it is preferable to supply the N- and H-containing gas to the wafer 200 after exciting it into a plasma state from the side of the wafer 200. In (c), it is preferable to supply the inert gas to the wafer 200 after exciting it into a plasma state from the side of the wafer 200.

[0050] In the following, an example of forming a nitride film as the film will be described. Here, the nitride film includes a silicon nitride film (SiN film) as well as a nitride film containing carbon (C), oxygen (O), boron (B), and the like. That is, the nitride film includes a silicon nitride film (SiN film), a silicon carbonitride film (SiCN film), a silicon oxynitride film (SiON film), a silicon oxycarbonitride film (SiOCN film), a silicon boron carbonitride film (SiBCN film), a silicon boron nitride film (SiBN film), a silicon boron oxycarbonitride film (SiBOCN film), a silicon boron oxynitride film (SiBON film), and the like. In the following, an example of forming a SiN film as the nitride film will be described.

[0051] The term "wafer" used in this specification may mean the wafer itself or a laminate of the wafer and a predetermined layer or film formed on its surface. The term "surface of the wafer" used in this specification may mean the surface of the wafer itself or the surface of a predetermined layer or the like formed on the wafer. When described in this specification, "forming a predetermined layer on a wafer" may mean forming a predetermined layer directly on the surface of the wafer itself or forming a predetermined layer on a layer or the like formed on the wafer. When used in this specification, the term "substrate" is synonymous with the term "wafer".

[0052] (Wafer charge) A plurality of wafers 200 are loaded (wafer charge) into the boat 217. After that, the shutter 219s is moved by the shutter opening / closing mechanism 115s to open the lower end opening of the manifold 209 (shutter open). The wafers 200 include product wafers and dummy wafers.

[0053] (Boatload) 1, the boat 217 supporting the multiple wafers 200 is lifted by the boat elevator 115 and loaded (boat loaded) into the processing chamber 201. In this state, the seal cap 219 seals the lower end of the manifold 209 via the O-ring 220b.

[0054] (Pressure and temperature regulation) After the boat loading is completed, the inside of the processing chamber 201, i.e., the space in which the wafers 200 are present, is evacuated (reduced pressure exhaust) by the vacuum pump 246 so that the inside of the processing chamber 201 is at a desired pressure (vacuum level). At this time, the pressure inside the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 244 is feedback-controlled based on the measured pressure information (pressure adjustment). Also, the wafers 200 in the processing chamber 201 are heated by the heater 207 so that the temperature is a desired processing temperature. At this time, the power supply to the heater 207 is feedback-controlled based on temperature information detected by the temperature sensor 263 so that the inside of the processing chamber 201 has a desired temperature distribution (temperature adjustment). Also, the rotation mechanism 267 starts rotating the wafers 200. The evacuation inside the processing chamber 201 and the heating and rotation of the wafers 200 are all continued at least until the processing of the wafers 200 is completed.

[0055] (Film formation process) Then, the following steps 1, 2, and 3 are executed in sequence.

[0056] [Step 1] In step 1, a source gas is supplied to the wafer 200 in the processing chamber 201.

[0057] Specifically, the valve 243a is opened to allow the source gas to flow into the gas supply pipe 232a. The source gas has a flow rate adjusted by the MFC 241a, is supplied into the processing chamber 201 through the nozzle 249a, and is exhausted from the exhaust port 231a. At this time, the source gas is supplied to the wafer 200 from the side of the wafer 200 (source gas supply). At this time, the valves 243d to 243f may be opened to supply an inert gas into the processing chamber 201 through each of the nozzles 249a to 249c.

[0058] The processing conditions in this step are as follows: Treatment temperature: 250 to 550°C, preferably 400 to 500°C Treatment pressure: 100 to 4000 Pa, preferably 100 to 1000 Pa Raw gas supply flow rate: 0.1 to 3 slm Raw material gas supply time: 1 to 100 seconds, preferably 1 to 30 seconds Inert gas supply flow rate (per gas supply pipe): 0 to 10 slm Examples include:

[0059] In this specification, the expression of a numerical range such as "250 to 550°C" means that the lower limit and the upper limit are included in the range. Therefore, for example, "250 to 550°C" means "250°C or more and 550°C or less". The same applies to other numerical ranges. In this specification, the process temperature means the temperature of the wafer 200 or the temperature inside the process chamber 201, and the process pressure means the pressure inside the process chamber 201. A gas supply flow rate of 0 slm means that the gas is not supplied. These are also applicable to the following explanations.

[0060] By supplying, for example, a chlorosilane-based gas as a raw material gas to the wafer 200 under the above-mentioned processing conditions, a Si-containing layer containing Cl is formed on the top surface of the wafer 200 as a base. The Si-containing layer containing Cl is formed on the top surface of the wafer 200 by physical adsorption or chemical adsorption of molecules of the chlorosilane-based gas, physical adsorption or chemical adsorption of molecules of a substance obtained by decomposing a part of the chlorosilane-based gas, deposition of Si by thermal decomposition of the chlorosilane-based gas, or the like. The Si-containing layer containing Cl may be an adsorption layer (physical adsorption layer or chemical adsorption layer) of molecules of the chlorosilane-based gas or molecules of a substance obtained by decomposing a part of the chlorosilane-based gas, or may be a deposition layer of Si containing Cl. In this specification, the Si-containing layer containing Cl is also simply referred to as a Si-containing layer. Under the above-mentioned processing conditions, physical adsorption or chemical adsorption of the molecules of the chlorosilane-based gas or the molecules of a substance formed by decomposition of a part of the chlorosilane-based gas onto the outermost surface of the wafer 200 occurs predominantly (preferentially), and deposition of Si due to thermal decomposition of the chlorosilane-based gas occurs slightly or almost not at all. That is, under the above-mentioned processing conditions, the Si-containing layer contains an overwhelming amount of adsorption layers (physical adsorption layers or chemical adsorption layers) of the molecules of the chlorosilane-based gas or the molecules of a substance formed by decomposition of a part of the chlorosilane-based gas, and contains a slight amount or almost no deposition layer of Si containing Cl.

[0061] After the Si-containing layer is formed, the valve 243a is closed to stop the supply of the source gas into the processing chamber 201. Then, the processing chamber 201 is evacuated to remove gas remaining in the processing chamber 201 from the processing chamber 201 (purging). At this time, the valves 243d to 243f are opened to supply an inert gas into the processing chamber 201. The inert gas acts as a purge gas. The processing chamber 201 is purged under a non-plasma atmosphere. This makes it possible to suppress the mixing of the source gas remaining in the processing chamber 201 with the N- and H-containing gas supplied into the processing chamber 201 in step 2, and the resulting unintended reaction (for example, gas-phase reaction or plasma gas-phase reaction), generation of particles, etc.

[0062] The processing conditions for purging are as follows: Treatment temperature: 250 to 550°C, preferably 400 to 500°C Processing pressure: 1~20Pa Inert gas supply flow rate (per gas supply pipe): 0.05 to 20 slm Inert gas supply time: 1 to 600 seconds, preferably 1 to 40 seconds Examples include:

[0063] As the source gas, for example, a silane-based gas containing silicon (Si) as the main element constituting the film formed on the wafer 200 can be used. As the silane-based gas, for example, a gas containing Si and a halogen, that is, a halosilane-based gas can be used. The halogen includes chlorine (Cl), fluorine (F), bromine (Br), iodine (I), etc. As the halosilane-based gas, for example, the above-mentioned chlorosilane-based gas containing Si and Cl can be used.

[0064] As the source gas, for example, a chlorosilane-based gas such as monochlorosilane (SiH3Cl, abbreviated as MCS) gas, dichlorosilane (SiH2Cl2, abbreviated as DCS) gas, trichlorosilane (SiHCl3, abbreviated as TCS) gas, tetrachlorosilane (SiCl4, abbreviated as 4CS) gas, hexachlorodisilane gas (Si2Cl6, abbreviated as HCDS) gas, octachlorotrisilane (Si3Cl8, abbreviated as OCTS) gas, etc. As the source gas, one or more of these can be used.

[0065] As the raw material gas, in addition to the chlorosilane-based gas, for example, a fluorosilane-based gas such as tetrafluorosilane (SiF4) gas or difluorosilane (SiH2F2) gas, a bromosilane-based gas such as tetrabromosilane (SiBr4) gas or dibromosilane (SiH2Br2) gas, or an iodosilane-based gas such as tetraiodosilane (SiI4) gas or diiodosilane (SiH2I2) gas can be used. One or more of these can be used as the raw material gas.

[0066] In addition to these, the source gas may be, for example, a gas containing Si and an amino group, i.e., an aminosilane-based gas. An amino group is a monovalent functional group obtained by removing hydrogen (H) from ammonia, a primary amine, or a secondary amine, and can be represented as -NH2, -NHR, or -NR2. R represents an alkyl group, and the two Rs in -NR2 may be the same or different.

[0067] As the source gas, for example, aminosilane gases such as tetrakis(dimethylamino)silane (Si[N(CH3)2]4, abbreviated as 4DMAS) gas, tris(dimethylamino)silane (Si[N(CH3)2]3H, abbreviated as 3DMAS) gas, bis(diethylamino)silane (Si[N(C2H5)2]2H2, abbreviated as BDEAS) gas, bis(tertiarybutylamino)silane (SiH2[NH(C4H9)]2, abbreviated as BTBAS) gas, and (diisopropylamino)silane (SiH3[N(C3H7)2], abbreviated as DIPAS) gas can be used. As the source gas, one or more of these can be used.

[0068] As the inert gas, for example, nitrogen (N2) gas, argon (Ar) gas, helium (He) gas, neon (Ne) gas, xenon (Xe) gas, krypton (Kr) gas, radon (Rn) gas, or other rare gases can be used. As the inert gas, one or more of these can be used. This also applies to each step described later.

[0069] [Step 2] After step 1 is completed, a N- and H-containing gas is excited into a plasma state and supplied to the wafer 200 in the processing chamber 201, that is, to the Si-containing layer formed on the wafer 200.

[0070] Specifically, the valve 243b is opened to allow N and H containing gas to flow into the gas supply pipe 232b. The N and H containing gas is adjusted in flow rate by the MFC 241b, supplied into the processing chamber 201 via the nozzle 249b, and exhausted from the exhaust port 231a. At this time, the N and H containing gas is supplied to the wafer 200 from the side of the wafer 200 (N and H containing gas supply). At this time, the valves 243d to 243f may be opened to supply an inert gas into the processing chamber 201 via each of the nozzles 249a to 249c.

[0071] At this time, by applying RF power between the first electrode 300a and the second electrode 300b, plasma is generated in the region between the first electrode 300a and the second electrode 300b. As a result, the N and H-containing gas is excited into a plasma state, and NH x * (x is an integer from 1 to 3) and other activated species are generated and supplied to the wafer 200 (plasma excited N and H containing gas supply). * , NH2 * , NH3 * In this case, a N- and H-containing gas containing active species such as the above is supplied. Note that * means a radical. The same applies to the following explanation.

[0072] In addition, before the N- and H-containing gas is excited into a plasma state and supplied to the wafer 200, a period during which the N- and H-containing gas is supplied without being excited into a plasma state may be provided. That is, before the plasma-excited N- and H-containing gas is supplied to the wafer 200, a non-plasma-excited N- and H-containing gas may be supplied, that is, a non-plasma-excited N- and H-containing gas may be pre-flowed (non-plasma-excited N- and H-containing gas pre-flow). In this case, the N- and H-containing gas is first supplied without being excited into a plasma state, and after a predetermined period has elapsed, RF power may be applied between the first electrode 300a and the second electrode 300b while the supply of the N- and H-containing gas is continued. This makes it possible to generate more stable plasma and active species.

[0073] The processing conditions in this step are as follows: Treatment temperature: 250 to 550°C, preferably 400 to 500°C Treatment pressure: 2 to 100 Pa, preferably 20 to 70 Pa N and H-containing gas supply flow rate: 0.1 to 10 slm N and H-containing gas supply time: 10 to 600 seconds, preferably 1 to 50 seconds Inert gas supply flow rate (per gas supply pipe): 0 to 10 slm RF power: 100~1000W RF frequency: 13.56MHz or 27MHz Examples include:

[0074] By supplying the N and H containing gas excited to a plasma state to the wafer 200 under the above-mentioned processing conditions, at least a part of the Si-containing layer formed on the wafer 200 is nitrided (modified). As a result, a silicon nitride layer (SiN layer) is formed as a layer containing Si and N on the top surface of the wafer 200 as a base. When the SiN layer is formed, impurities such as Cl contained in the Si-containing layer are converted to NH x * In the process of the modification reaction of the Si-containing layer by the active species such as Cl, a gaseous substance containing at least Cl is formed and is exhausted from the processing chamber 201. As a result, the SiN layer has less impurities such as Cl compared to the Si-containing layer formed in step 1.

[0075] After the SiN layer is formed, the valve 243b is closed to stop the supply of the N- and H-containing gas into the processing chamber 201. Thereafter, step 3 is performed. Prior to this, the processing chamber 201 may be purged under a non-plasma atmosphere. In this case, gas remaining in the processing chamber 201 can be removed from the processing chamber 201 (purging) by a processing procedure similar to that of purging in step 1. This makes it possible to suppress the mixing of the plasma-excited N- and H-containing gas remaining in the processing chamber 201 with the plasma-excited inert gas supplied into the processing chamber 201 in step 3, and the resulting unintended reaction (e.g., plasma gas-phase reaction), generation of particles, and the like.

[0076] The N- and H-containing gas acts as a nitriding agent (nitrogen source, nitriding gas). The N- and H-containing gas is both an N-containing gas and an H-containing gas. The N- and H-containing gas preferably has an NH bond.

[0077] As the N- and H-containing gas, for example, ammonia (NH3) gas, diazane (N2H2) gas, hydrazine (N2H4) gas, N3H8 gas, or other hydrogen nitride gas can be used. As the N- and H-containing gas, one or more of these can be used.

[0078] As the N- and H-containing gas, for example, a nitrogen (N), carbon (C) and hydrogen (H)-containing gas can be used. As the N-, C- and H-containing gas, for example, an amine-based gas or an organic hydrazine-based gas can be used. The N-, C- and H-containing gas can be an N-containing gas, a C-containing gas, an H-containing gas, and an N- and C-containing gas.

[0079] Examples of N- and H-containing gases that can be used include ethylamine-based gases such as monoethylamine (C2H5NH2, abbreviated as MEA) gas, diethylamine ((C2H5)2NH, abbreviated as DEA) gas, and triethylamine ((C2H5)3N, abbreviated as TEA) gas; methylamine-based gases such as monomethylamine (CH3NH2, abbreviated as MMA) gas, dimethylamine ((CH3)2NH, abbreviated as DMA) gas, and trimethylamine ((CH3)3N, abbreviated as TMA) gas; and organic hydrazine-based gases such as monomethylhydrazine ((CH3)HN2H2, abbreviated as MMH) gas, dimethylhydrazine ((CH3)2N2H2, abbreviated as DMH) gas, and trimethylhydrazine ((CH3)2N2(CH3)H, abbreviated as TMH) gas. One or more of these can be used as the N- and H-containing gas.

[0080] [Step 3] After step 2 is completed, an inert gas is excited into a plasma state and supplied to the wafer 200 in the processing chamber 201, that is, to the SiN layer formed on the wafer 200.

[0081] Specifically, the valves 243d-243f are opened to allow the inert gas to flow into the gas supply pipes 232d-232f, respectively. The inert gas is adjusted in flow rate by the MFCs 241d-241f, supplied into the process chamber 201 via the nozzles 249a-249c, respectively, and exhausted from the exhaust port 231a. At this time, the inert gas is supplied to the wafer 200 from the side of the wafer 200 (inert gas supply).

[0082] At this time, by applying RF power between the first electrode 300a and the second electrode 300b, plasma is generated in the region between the first electrode 300a and the second electrode 300b. As a result, the inert gas is excited into a plasma state, and active species are generated and supplied to the wafer 200 (plasma-excited inert gas supply). At this time, the inert gas containing the active species is supplied to the wafer 200.

[0083] When N2 gas is used as the inert gas, for example, the N2 gas is excited into a plasma state, and N x * (x is an integer between 1 and 2) and other activated species are generated and supplied to the wafer 200 (plasma-excited N2 gas supply). * , N2 * Thus, N2 gas containing activated species such as these is supplied.

[0084] When Ar gas is used as the inert gas, the Ar gas is excited into a plasma state, and the Ar * and other activated species are generated and supplied to the wafer 200 (plasma excited Ar gas supply). * Thus, Ar gas containing activated species such as these is supplied.

[0085] When He gas is used as the inert gas, for example, the He gas is excited into a plasma state, and * and other activated species are generated and supplied to the wafer 200 (plasma excited He gas supply). *Thus, He gas containing activated species such as the above is supplied.

[0086] As the inert gas, these gases may be mixed and used as a mixed gas in the processing chamber 201. For example, as the inert gas, a mixed gas of N2 gas and Ar gas may be used, a mixed gas of N2 gas and He gas may be used, or a mixed gas of N2 gas, Ar gas, and He gas may be used.

[0087] In addition, before supplying the inert gas to the wafer 200 after exciting it to a plasma state, a period during which the inert gas is supplied without being excited to a plasma state may be provided. That is, before supplying the plasma-excited inert gas to the wafer 200, a non-plasma-excited inert gas may be supplied, that is, a non-plasma-excited inert gas may be pre-flowed (non-plasma-excited inert gas pre-flow). In this case, first, the inert gas is supplied without being excited to a plasma state, and after a predetermined period has elapsed, RF power may be applied between the first electrode 300a and the second electrode 300b while the supply of the inert gas is continued. This makes it possible to generate more stable plasma and active species.

[0088] The processing conditions in this step are as follows: Treatment temperature: 250 to 550°C, preferably 400 to 500°C Treatment pressure: 2 to 6 Pa, preferably 2.66 to 5.32 Pa, more preferably 3 to 4 Pa a Inert gas supply flow rate (per gas supply pipe): 0.01 to 2 slm Inert gas supply time: 1 to 600 seconds, preferably 10 to 60 seconds RF power: 100~1000W RF frequency: 13.56MHz or 27MHz Examples include:

[0089] Under the above-mentioned processing conditions, an inert gas is excited into a plasma state and supplied to the wafer 200, whereby the SiN layer formed on the wafer 200 is modified. At this time, impurities such as Cl remaining in the SiN layer form a gaseous substance containing at least Cl during the process of the modification reaction of the SiN layer by the active species, and are discharged from the processing chamber 201. As a result, the SiN layer modified in this step has less impurities such as Cl compared to the SiN layer formed in step 2. Furthermore, this modification densifies the SiN layer, and the SiN layer modified in this step has a higher density compared to the SiN layer formed in step 2.

[0090] In addition, NH x * Due to a modification reaction caused by active species such as NH, the content of impurities such as Cl in the SiN layer formed in step 2 is reduced compared to the content of impurities such as Cl in the Si-containing layer formed in step 1. However, the SiN layer formed in step 2 contains impurities such as NH x * In this step, impurities such as Cl may remain at a level of several atomic percent due to the presence of active species such as NH x * Impurities such as Cl that remain in the SiN layer and cannot be completely removed by active species such as NH x * The active species different from the active species such as N * , N2 * , Ar * , He * It can be removed by active species such as

[0091] At this time, it is preferable to set the pressure in the process chamber 201 in this step, i.e., step 3, lower than the pressure in the process chamber 201 in step 2. Furthermore, it is preferable to set the pressure in the process chamber 201 in step 3 lower than the pressure in the process chamber 201 in step 2, and the pressure in the process chamber 201 in step 2 lower than the pressure in the process chamber 201 in step 1. In this way, by adjusting the pressure balance between each step, it is possible to prevent NH x * The lifetime of the active species such as N x * , Ar * , He * In particular, the lifetime of the N x * , Ar * , He * It is possible to lengthen the lifetime of active species such as H, H, and H. In order to adjust the pressure balance between the steps as described above, it is preferable to make the supply flow rate of the inert gas supplied in step 3 smaller than the supply flow rate of the N- and H-containing gas supplied in step 2. That is, by controlling the balance of the supply flow rates of the gases supplied in each step, it is possible to adjust the pressure balance between the steps and optimize the lifetime of each active species generated in each step.

[0092] In addition, in this step, it is desirable to lower the pressure in the process chamber 201 to 2 Pa or more and 6 Pa or less, preferably 2.66 Pa or more and 5.32 Pa or less, more preferably 3 Pa or more and 4 Pa ​​or less. In this case, it is preferable to lower the process pressure in this step than the process pressure in steps 1 and 2. Note that, by lowering the flow rate of the inert gas supplied in this step to a value lower than the flow rate of the inert gas supplied in the purge, and further to a value lower than the flow rate of the N- and H-containing gas supplied in step 2, such a reduction in the process pressure can be promoted. FIG. 5 shows an example in which the flow rate of the inert gas supplied in this step is lowered to a value lower than the flow rate of the inert gas supplied in the purge, and further to a value lower than the flow rate of the N- and H-containing gas supplied in step 2, thereby promoting the reduction in the process pressure.

[0093] In this step, if the pressure in the processing chamber 201 is set to less than 2 Pa, N2 generated together with the activated species when the inert gas is excited into a plasma state will be + , Ar + , He + The amount of ions generated increases rapidly, and ion attack on the wafer 200 may occur excessively. This may increase the wet etching rate (hereinafter, WER) of the SiN film finally formed, and may reduce the wet etching resistance of the SiN film finally formed. This is believed to be due to the fact that the surface layer of the SiN layer is attacked by ions, thereby reducing the density of the surface layer of the SiN layer, and therefore the film density of the SiN film finally formed.

[0094] In addition, this ion attack may occur excessively especially at the outer periphery of the wafer 200, and the WER of the SiN film finally formed may be high at the outer periphery of the wafer 200, and the wet etching resistance of the SiN film finally formed may tend to be lowered at the outer periphery of the wafer 200. That is, this ion attack may deteriorate the WER uniformity of the SiN film finally formed in the wafer plane, that is, the wet etching resistance uniformity of the wafer plane. In addition, this ion attack may destroy the film structure of the SiN film at the outer periphery of the wafer 200, and the portion may change to a sparse film, and as a result, the film thickness of the SiN film finally formed tends to be thick at the outer periphery of the wafer 200. That is, this ion attack may deteriorate the film thickness uniformity of the SiN film finally formed in the wafer plane.

[0095] In contrast, in this step, the pressure in the processing chamber 201 is set to 2 Pa or more, so that the N2 generated together with the activated species when the inert gas is excited into a plasma state can be prevented. + , Ar + , He + It is possible to reduce the amount of ions generated, and suppress the occurrence of ion attack on the wafer 200. This makes it possible to avoid an increase in the WER of the SiN film that is finally formed, and to prevent a decrease in the wet etching resistance of the SiN film that is finally formed. This is believed to be because, although ions are generated, the ion attack on the surface layer of the SiN layer is suppressed, thereby suppressing a decrease in the density of the surface layer of the SiN layer, and thus suppressing a decrease in the film density of the SiN film that is finally formed.

[0096] By suppressing this ion attack, the WER of the SiN film finally formed becomes higher at the outer periphery of the wafer 200, and it is also possible to eliminate the tendency that the wet etching resistance of the SiN film finally formed decreases at the outer periphery of the wafer 200. That is, by suppressing this ion attack, it is possible to suppress the deterioration of the WER uniformity of the SiN film finally formed in the wafer plane, that is, the wet etching resistance uniformity in the wafer plane. In addition, by suppressing this ion attack, it is also possible to eliminate the tendency that the thickness of the SiN film finally formed becomes thicker at the outer periphery of the wafer 200. That is, by suppressing this ion attack, it is also possible to suppress the deterioration of the thickness uniformity of the SiN film finally formed in the wafer plane.

[0097] In this step, the ion attack suppression effect can be further improved by setting the pressure in the processing chamber 201 to 2.66 Pa or more, and the above-mentioned effects can be more fully obtained. In this step, the ion attack suppression effect can be further improved by setting the pressure in the processing chamber 201 to 3 Pa or more, and the above-mentioned effects can be more fully obtained.

[0098] In this step, if the pressure in the processing chamber 201 is set to a pressure exceeding 6 Pa, N x * , Ar * , He * The lifetime of the activated species such as N2O3 and N3O4 may become shorter, and the activated species may have difficulty reaching the center of the wafer 200. x * , Ar * , He *Such activated species may be deactivated at a high rate before reaching the center of the wafer 200. This may result in a high WER of the SiN film finally formed at the center of the wafer 200, and as a result, the wet etching resistance of the SiN film finally formed may decrease at the center of the wafer 200. In other words, the uniformity of the WER of the SiN film finally formed within the wafer surface, i.e., the uniformity of the wet etching resistance within the wafer surface, may deteriorate. In addition, N x * , Ar * , He * Such active species are deactivated at a high rate before reaching the center of the wafer, which may result in insufficient densification of the film at the center of the wafer, and the thickness of the SiN film finally formed may be thick at the center of the wafer 200. That is, the thickness uniformity of the SiN film finally formed within the wafer may be deteriorated. This is considered to be because the SiN layer modification effect is sufficient at the outer periphery of the wafer 200 where the active species can easily reach, whereas the SiN layer modification effect is insufficient at the center of the wafer 200 where the active species cannot easily reach, resulting in a difference in the modification effect of the SiN layer between the outer periphery and the center of the wafer 200.

[0099] In contrast, in this step, the pressure inside the processing chamber 201 is set to 6 Pa or less, so that N x * , Ar * , He * It is possible to extend the lifetime of active species such as N x * , Ar * , He *It is possible to allow active species such as N to sufficiently reach the center of the wafer 200. This makes it possible to prevent the WER of the SiN film that is finally formed from being high at the center of the wafer 200, and to prevent the wet etching resistance of the SiN film that is finally formed from being reduced at the center of the wafer 200. In other words, it is possible to suppress deterioration of the WER uniformity within the wafer surface of the SiN film that is finally formed, that is, the wet etching resistance uniformity within the wafer surface. In addition, N x * , Ar * , He * By allowing the active species such as SiO 2 to reach the center of the wafer 200 sufficiently, it is possible to prevent the thickness of the SiN film finally formed from being thick at the center of the wafer 200. That is, it is possible to suppress the deterioration of the thickness uniformity within the wafer of the SiN film finally formed. This is considered to be because not only the effect of modifying the SiN layer at the outer periphery of the wafer 200 is sufficiently obtained, but also the effect of modifying the SiN layer at the center of the wafer 200 is sufficiently obtained. Also, it is considered to be because not only the effect of densifying the SiN layer at the outer periphery of the wafer 200 is sufficiently obtained, but also the effect of densifying the SiN layer at the center of the wafer 200 is sufficiently obtained.

[0100] In this step, the pressure in the processing chamber 201 is set to 5.32 Pa or less. x * , Ar * , He * In this step, the pressure in the process chamber 201 is set to 4 Pa ​​or less, so that the N x * , Ar * , He * The effect of improving the lifetime of active species such as those mentioned above can be further enhanced, and the above-mentioned effects can be obtained more sufficiently.

[0101] For the above reasons, in this step, it is desirable to set the pressure inside the processing chamber 201 to 2 Pa or more and 6 Pa or less, preferably 2.66 Pa or more and 5.32 Pa or less, and more preferably 3 Pa or more and 4 Pa ​​or less.

[0102] In addition, it is preferable to set the time during which the inert gas is excited into a plasma state and supplied in this step (step 3) longer than the time during which the N- and H-containing gas is excited into a plasma state and supplied in step 2. In addition, it is preferable to set the time during which the inert gas is excited into a plasma state and supplied in this step (step 3) longer than the time during which the raw material gas is supplied in step 1. Furthermore, it is preferable to set the time during which the inert gas is excited into a plasma state and supplied in this step (step 3) longer than the time during which the N- and H-containing gas is excited into a plasma state and supplied in step 2, and to set the time during which the N- and H-containing gas is excited into a plasma state and supplied in step 2 longer than the time during which the raw material gas is supplied in step 1. By adjusting the balance of the exposure time of the gas or active species to the wafer 200 between each step (hereinafter also referred to as the exposure time of the active species or the exposure time of the gas, etc.), it is possible to prevent the wafer 200 from being exposed to NH x * In step 3, the reforming reaction caused by active species such as N x * , Ar * , He * In particular, the reforming reaction caused by the active species N in step 3 can be optimized. x * , Ar * , He * It is possible to optimize the reforming reaction by active species such as those mentioned above.

[0103] After the modification process of the SiN layer is completed, the application of RF power to the electrode 300 is stopped, and the supply of the plasma excited inert gas to the wafer 200 is stopped. When the above cycle is repeated multiple times, after the step 3 is completed, the step 1 is performed again, but before that, the inside of the processing chamber 201 may be purged under a non-plasma atmosphere. In this case, gas remaining in the processing chamber 201 can be removed from the inside of the processing chamber 201 by a processing procedure similar to the purging in the step 1 (purging). This makes it possible to suppress the mixing of the plasma excited inert gas remaining in the processing chamber 201 with the raw material gas supplied into the processing chamber 201 in the step 1, and the resulting unintended reaction (for example, gas-phase reaction or plasma gas-phase reaction), generation of particles, etc.

[0104] Examples of the inert gas that can be used include nitrogen (N2) gas, argon (Ar) gas, helium (He) gas, neon (Ne) gas, xenon (Xe) gas, krypton (Kr) gas, radon (Rn) gas, etc. One or more of these gases can be used as the inert gas.

[0105] [Perform the cycle a set number of times] By performing the above-mentioned steps 1, 2, and 3 asynchronously, i.e., by performing a cycle a predetermined number of times (n times, n is an integer equal to or greater than 1), a film of a predetermined thickness, for example, a silicon nitride film (SiN film) of a predetermined thickness, can be formed on the surface of the wafer 200 as a base. It is preferable to repeat the above-mentioned cycle multiple times. That is, it is preferable to make the thickness of the SiN layer formed per cycle thinner than the desired film thickness, and to repeat the above-mentioned cycle multiple times until the thickness of the SiN film formed by stacking the SiN layers reaches the desired thickness. Note that, when a gas containing N, C, and H is used as the reactive gas, it is also possible to form, for example, a silicon carbonitride layer (SiCN layer) in step 2, and by performing the above-mentioned cycle a predetermined number of times, it is also possible to form, for example, a silicon carbonitride film (SiCN film) as a film on the surface of the wafer 200.

[0106] (After purging and atmospheric pressure recovery) After the process of forming a SiN film of a desired thickness on the wafer 200 is completed, an inert gas is supplied as a purge gas from each of the nozzles 249a to 249c into the processing chamber 201 and exhausted from the exhaust port 231a. This purges the processing chamber 201, and gas and reaction by-products remaining in the processing chamber 201 are removed from the processing chamber 201 (after-purge). Thereafter, the atmosphere in the processing chamber 201 is replaced with the inert gas (inert gas replacement), and the pressure in the processing chamber 201 is returned to normal pressure (return to atmospheric pressure).

[0107] (Boat unloading) Thereafter, the seal cap 219 is lowered by the boat elevator 115, and the lower end of the manifold 209 is opened. Then, the processed wafers 200 supported by the boat 217 are carried out from the lower end of the manifold 209 to the outside of the reaction tube 203 (boat unloading). After the boat unloading, the shutter 219s is moved, and the lower end opening of the manifold 209 is sealed by the shutter 219s via the O-ring 220c (shutter closing).

[0108] (Wafer cooling) After the boat is unloaded, that is, after the shutter is closed, the processed wafers 200 are cooled down to a predetermined temperature at which they can be removed while still supported by the boat 217 (wafer cooling).

[0109] (wafer discharge) After the wafers are cooled, the processed wafers 200 are cooled to a predetermined temperature at which they can be removed, and are then removed from the boat 217 (wafer discharging).

[0110] This completes the series of processes for forming a film on the wafer 200. This series of processes is performed a predetermined number of times.

[0111] In this embodiment, the film formation process is performed in the processing chamber 201 with a plurality of wafers 200 supported by the boat 217. In this case, as shown in FIG. 7(a), the interval (arrangement pitch) between the plurality of wafers 200 during the film formation process may be the interval (arrangement pitch) between the wafers 200 when the maximum number of wafers 200 that can be supported by the boat 217 is supported. The interval (arrangement pitch) between the wafers 200 means the interval (distance) between adjacent wafers 200. For example, when the maximum number of wafers 200 that can be supported by the boat 217 is 100, the film formation process may be performed with the 100 wafers 200 supported by the support parts 217b of the boat 217. The interval (arrangement pitch) between the wafers 200 in FIG. 7(a), that is, the interval (arrangement pitch) between the support parts 217b supporting the wafers 200, may be, for example, 6 to 12 mm.

[0112] Also, for example, as shown in FIG. 7(b) and FIG. 7(c), when performing the film forming process, the interval (arrangement pitch) between the multiple wafers 200 may be set larger than the interval (arrangement pitch) between the wafers 200 when the maximum number of wafers 200 that can be supported by the boat 217 is supported. This makes it possible to suppress the active species from colliding with the wafers 200 when flowing between adjacent wafers 200 and being deactivated, and to increase the probability that the active species reaches the center of the wafer 200. This makes it possible to suppress the WER of the SiN film that is finally formed from being high at the center of the wafer 200, and to suppress the wet etching resistance of the SiN film that is finally formed from being reduced at the center of the wafer 200. That is, it is possible to suppress the deterioration of the WER uniformity within the wafer of the SiN film that is finally formed, that is, the wet etching resistance uniformity within the wafer. It is also possible to suppress the thickness of the SiN film that is finally formed from being thick at the center of the wafer 200. That is, it is possible to suppress the deterioration of the thickness uniformity within the wafer of the SiN film that is finally formed. In particular, N x * , Ar *, He * Among other active species, N x * Since active species such as these have a relatively short lifetime and are easily deactivated, this effect is particularly pronounced in step 3.

[0113] In this case, for example, as shown in FIG. 7(b), when performing the film formation process, the interval (arrangement pitch) between the multiple wafers 200 may be set to be twice or more the interval (arrangement pitch) between the wafers 200 when the maximum number of wafers 200 that can be supported by the boat 217 is supported. For example, when the maximum number of wafers 200 that can be supported by the boat 217 is 120, the film formation process may be performed in a state where every other wafer 200 is supported by the support portion 217b of the boat 217. In this case, the interval (arrangement pitch) between the wafers 200 may be set to, for example, 12 to 24 mm or more. This can further suppress the active species from being deactivated due to collision with the wafers 200, and can further increase the probability that the active species reaches the center of the wafers 200. This makes it possible to sufficiently prevent the WER of the SiN film finally formed from being high at the center of the wafer 200, and to sufficiently prevent the wet etching resistance of the SiN film finally formed from being reduced at the center of the wafer 200. That is, it is possible to sufficiently prevent the deterioration of the WER uniformity of the SiN film finally formed within the wafer surface, i.e., the wet etching resistance uniformity within the wafer surface. It is also possible to sufficiently prevent the thickness of the SiN film finally formed from being thick at the center of the wafer 200. That is, it is possible to sufficiently prevent the deterioration of the film thickness uniformity within the wafer surface of the SiN film finally formed. In particular, N x * , Ar * , He * Among other active species, N x * Since active species such as these have a relatively short lifetime and are easily deactivated, this effect is particularly pronounced in step 3.

[0114] In this case, when performing the film forming process, the interval (arrangement pitch) between the multiple wafers 200 may be set to be three times or more the interval (arrangement pitch) between the wafers 200 when the maximum number of wafers 200 that can be supported by the boat 217 is supported. For example, when the maximum number of wafers 200 that can be supported by the boat 217 is 120, the film forming process may be performed in a state where every third wafer 200 is supported by the support portion 217b of the boat 217. In this case, the interval (arrangement pitch) between the wafers 200 may be set to, for example, 18 to 36 mm or more. This can further suppress the active species from being deactivated due to collision with the wafers 200, and can further increase the probability that the active species reaches the center of the wafer 200. This makes it possible to more sufficiently suppress the WER of the SiN film finally formed from being high at the center of the wafer 200, and more sufficiently suppress the wet etching resistance of the SiN film finally formed from being reduced at the center of the wafer 200. That is, it becomes possible to more sufficiently suppress the deterioration of the WER uniformity of the SiN film finally formed within the wafer surface, that is, the wet etching resistance uniformity within the wafer surface. It also becomes possible to more sufficiently suppress the thickness of the SiN film finally formed from being thick at the center of the wafer 200. That is, it becomes possible to more sufficiently suppress the deterioration of the film thickness uniformity within the wafer surface of the SiN film finally formed. In particular, N x * , Ar * , He * Among other active species, N x * Since active species such as these have a relatively short lifetime and are easily deactivated, this effect is particularly pronounced in step 3.

[0115] In this case, for example, as shown in FIG. 7(c), when performing the film formation process, the interval (arrangement pitch) between the multiple wafers 200 may be set to be four times or more the interval (arrangement pitch) between the wafers 200 when the maximum number of wafers 200 that can be supported by the boat 217 is supported. For example, when the maximum number of wafers 200 that can be supported by the boat 217 is 120, the film formation process may be performed in a state where every third wafer 200 is supported by the support portion 217b of the boat 217. In this case, the interval (arrangement pitch) between the wafers 200 may be set to, for example, 24 to 48 mm or more. This can further suppress the active species from being deactivated due to collision with the wafers 200, and further increase the probability that the active species reaches the center of the wafers 200. This makes it possible to further prevent the WER of the SiN film finally formed from being high at the center of the wafer 200, and further prevent the wet etching resistance of the SiN film finally formed from being reduced at the center of the wafer 200. That is, it is possible to further prevent the deterioration of the WER uniformity within the wafer surface of the SiN film finally formed, that is, the wet etching resistance uniformity within the wafer surface. It is also possible to further prevent the thickness of the SiN film finally formed from being thick at the center of the wafer 200. That is, it is possible to further prevent the deterioration of the film thickness uniformity within the wafer surface of the SiN film finally formed. In particular, N x * , Ar * , He * Among other active species, N x * Since active species such as these have a relatively short lifetime and are easily deactivated, this effect is particularly pronounced in step 3.

[0116] However, if the interval (arrangement pitch) of the wafers 200 is too large, the number of wafers 200 that can be subjected to a film forming process at one time decreases, which may result in a decrease in productivity. In consideration of keeping productivity at a practical level, it is preferable to set the interval (arrangement pitch) of the wafers 200 to 5 times or less the interval (arrangement pitch) of the wafers 200 when the maximum number of wafers 200 that can be supported by the boat 217 is supported. In this case, the interval (arrangement pitch) of the wafers 200 can be set to, for example, 30 to 60 mm or less.

[0117] From these facts, in order to increase the probability that the activated species reach the center of the wafer 200 and to bring productivity to a practical level, it is preferable to set the spacing (arrangement pitch) of multiple wafers 200 to, for example, 12 mm or more and 60 mm or less.

[0118] In order to increase the probability that the active species reach the center of the wafer 200 while keeping the productivity at a practical level, it is preferable to set the interval (arrangement pitch) of the multiple wafers 200 to, for example, 15 mm or more and 60 mm or less. In order to further increase the probability that the active species reach the center of the wafer 200 while keeping the productivity at a practical level, it is preferable to set the interval (arrangement pitch) of the multiple wafers 200 to, for example, 18 mm or more and 60 mm or less, more preferably 24 mm or more and 60 mm or less, even more preferably 36 mm or more and 60 mm or less, and even more preferably 48 mm or more and 60 mm or less. These can be said to be the arrangement pitches of the wafers 200 that place more importance on the probability that the active species reach the center of the wafer 200.

[0119] In order to increase the productivity while increasing the probability that the active species reach the center of the wafer 200, the interval (arrangement pitch) between the multiple wafers 200 is, for example, preferably 12 mm to 48 mm, more preferably 12 mm to 40 mm, even more preferably 12 mm to 36 mm, and even more preferably 12 mm to 30 mm. These can be said to be the arrangement pitches of the wafers 200 that place more importance on productivity.

[0120] The upper and lower limit values ​​of the numerical range of the interval (arrangement pitch) of the plurality of wafers 200 described above can be appropriately combined in consideration of the balance between the probability that the active species will reach the center of the wafer 200 and the productivity. In these cases, the wafers 200 are not necessarily supported every few wafers by the boat 217 having an interval (arrangement pitch) of the support parts 217b of, for example, 6 to 12 mm, but the wafers 200 may be supported by the boat 217 having an interval (arrangement pitch) of the support parts 217b itself within the numerical range described above.

[0121] (3) Effects of this mode According to this aspect, one or more of the following effects can be obtained.

[0122] (a) By adjusting the pressure balance between each step so that the pressure in the process chamber 201 in step 3 is lower than the pressure in the process chamber 201 in step 2, N x * , Ar * , He * It is possible to optimize the lifetime of active species such as . This makes it possible to enhance the modification effect of the SiN layer in step 3. As a result, it is possible to lower the WER of the SiN film finally formed, and improve the wet etching resistance of the SiN film finally formed. In addition, it is possible to densify the SiN film finally formed, and it is possible to form a SiN film with high film density. That is, it is possible to improve the film quality of the SiN film finally formed, and it is possible to form a high-quality SiN film. In addition, in order to adjust the pressure balance between each step as described above, it is preferable to make the supply flow rate of the inert gas supplied in step 3 smaller than the supply flow rate of the N- and H-containing gas supplied in step 2.

[0123] Furthermore, it is preferable to adjust the pressure balance between each step so that the pressure in the process chamber 201 in step 3 is lower than the pressure in the process chamber 201 in step 2, and the pressure in the process chamber 201 in step 2 is lower than the pressure in the process chamber 201 in step 1. This reduces the amount of NH x * It is possible to optimize the lifetime of active species such as N x * , Ar * , He * In particular, the lifetime of the N x * , Ar * , He * It is possible to extend the lifetime of active species such as . This makes it possible to enhance the effect of modifying the SiN layer in step 3. As a result, it is possible to lower the WER of the SiN film that is finally formed, and it is possible to improve the wet etching resistance of the SiN film that is finally formed. In other words, it is possible to improve the film quality of the SiN film that is finally formed, and it is possible to form a high-quality SiN film.

[0124] (b) In step 3, the pressure in the processing chamber 201 is set to 2 Pa or more, preferably 2.66 Pa or more, and more preferably 3 Pa or more. This reduces the amount of N2 generated together with the activated species when the inert gas is excited into a plasma state. + , Ar + , He +The amount of ions generated can be reduced, and ion attack on the wafer 200 can be suppressed. This makes it possible to avoid the WER of the SiN film finally formed from becoming high, and to avoid the wet etching resistance of the SiN film finally formed from decreasing. In addition, by suppressing ion attack, it is possible to eliminate the tendency that the WER of the SiN film finally formed becomes high at the outer periphery of the wafer 200, and it is possible to eliminate the tendency that the wet etching resistance of the SiN film finally formed from decreasing at the outer periphery of the wafer 200. That is, it is possible to suppress the deterioration of the WER uniformity in the wafer plane of the SiN film finally formed, that is, the wet etching resistance uniformity in the wafer plane. In addition, by suppressing ion attack, it is possible to eliminate the tendency that the film thickness of the SiN film finally formed becomes thick at the outer periphery of the wafer 200. That is, it is possible to suppress the deterioration of the film thickness uniformity in the wafer plane of the SiN film finally formed.

[0125] (c) In step 3, the pressure in the processing chamber 201 is set to 6 Pa or less, preferably 5.32 Pa or less, and more preferably 4 Pa ​​or less, thereby preventing N generated when the inert gas is excited into a plasma state. x * , Ar * , He * This can lengthen the lifetime of active species such as N, and allows the active species to reach the center of the wafer 200 sufficiently. This makes it possible to prevent the WER of the SiN film finally formed from being high at the center of the wafer 200, and to prevent the wet etching resistance of the SiN film finally formed from being reduced at the center of the wafer 200. In other words, it is possible to suppress deterioration of the WER uniformity within the wafer surface of the SiN film finally formed, that is, the wet etching resistance uniformity within the wafer surface. In addition, N x * , Ar * , He *By allowing the active species such as SiO 2 to reach the center of the wafer 200 sufficiently, it is possible to prevent the thickness of the SiN film finally formed from being thick at the center of the wafer 200. In other words, it is possible to suppress deterioration of the in-wafer thickness uniformity of the SiN film finally formed.

[0126] (d) In step 3, the time during which the inert gas is excited into a plasma state and supplied is longer than the time during which the N- and H-containing gas is excited into a plasma state and supplied in step 2. In this way, the balance of the exposure time of the active species to the wafer 200 between the steps is adjusted so that the time during which the inert gas is excited into a plasma state and supplied in step 3 is longer than the time during which the N- and H-containing gas is excited into a plasma state and supplied in step 2 x * , Ar * , He * In other words, it is possible to more appropriately cause the above-mentioned reforming reaction. If the time during which the inert gas is excited into a plasma state and supplied in step 3 is shorter than the time during which the N- and H-containing gas is excited into a plasma state and supplied in step 2, the N x * , Ar * , He * The modification effect of active species such as those mentioned above may be insufficient.

[0127] In addition, it is preferable to adjust the balance of the exposure time of the gas to the wafer 200 between each step so that the time during which the inert gas is excited into a plasma state and supplied in step 3 is longer than the time during which the source gas is supplied in step 1. x * , Ar * , He * In other words, it is possible to more appropriately cause the above-mentioned reforming reaction. In addition, if the time during which the inert gas is excited into a plasma state and supplied in step 3 is shorter than the time during which the raw material gas is supplied in step 1, N x * , Ar * , He* The modification effect of active species such as those mentioned above may be insufficient.

[0128] Furthermore, it is preferable to adjust the balance of the exposure time of the gases, etc. to the wafer 200 between each step so that the time during which the inert gas is excited into a plasma state and supplied in step 3 is longer than the time during which the N- and H-containing gas is excited into a plasma state and supplied in step 2, and the time during which the N- and H-containing gas is excited into a plasma state and supplied in step 2 is longer than the time during which the source gas is supplied in step 1. x * In step 3, the reforming reaction caused by active species such as N x * , Ar * , He * In particular, the reforming reaction caused by the active species N in step 3 can be optimized. x * , Ar * , He * In other words, it is possible to more appropriately cause the above-mentioned reforming reaction to occur.

[0129] (e) In step 3, by applying power to the electrode 300 provided outside the processing vessel, the inert gas inside the processing vessel is excited into a plasma state, thereby making it possible to prevent the occurrence of abnormal discharge. This makes it possible to suppress damage to members inside the processing vessel and damage to the wafer 200, and further makes it possible to suppress the generation of particles.

[0130] For example, when an electrode for plasma generation is provided in a plasma generation chamber communicating with the inside of a processing vessel, and an inert gas is excited to a plasma state in the plasma generation chamber under the pressure conditions described above and ejected into the processing vessel, an abnormal discharge may occur. That is, in this case, localized discharges that are difficult to control may occur randomly near the ejection port that ejects the active species generated in the plasma generation chamber from the plasma generation chamber into the processing vessel. When such an abnormal discharge occurs in the plasma generation chamber, damage may occur to the inner wall of the partition that constitutes the plasma generation chamber and the nozzle provided in the plasma generation chamber. When such an abnormal discharge occurs outside the plasma generation chamber, i.e., in the processing vessel, damage may occur to the members in the processing vessel and the wafer. In either case, particles may be induced. When the processing pressure is lowered, the mean free path of the active species becomes longer, the amount of charge-up on the inner wall of the ejection port increases, and the electric field extending from the ejection port to the outside of the ejection port may become stronger. As a result, kinetic energy sufficient to generate an abnormal discharge may be given to plasma electrons through the electric field acceleration. That is, the lower the processing pressure, the more likely it is that abnormal discharge will occur.

[0131] In response to this, by applying power to the electrode 300 provided outside the processing vessel, the inert gas inside the processing vessel is excited into a plasma state, thereby preventing the occurrence of the abnormal discharge described above, suppressing damage to members inside the processing vessel and to the wafer 200, and making it possible to suppress the generation of particles. Note that this effect is particularly pronounced as the processing pressure is lowered.

[0132] In step 2, the N and H-containing gas is excited into a plasma state inside the processing vessel by applying power to the electrode 300 provided outside the processing vessel, thereby preventing the occurrence of abnormal discharge. This makes it possible to suppress damage to members inside the processing vessel and damage to the wafer 200, and further suppress the generation of particles.

[0133] (f) When performing the film formation process, the interval (arrangement pitch) between the multiple wafers 200 is set larger than the interval (arrangement pitch) between the wafers 200 when the maximum number of wafers 200 that can be supported by the boat 217 is supported, thereby making it possible to suppress deactivation due to collision of the active species with the wafers 200. As a result, it becomes possible to increase the probability that the active species reaches the center of the wafer 200. This makes it possible to suppress the WER of the SiN film that is finally formed from being high at the center of the wafer 200, and to suppress the wet etching resistance of the SiN film that is finally formed from being reduced at the center of the wafer 200. That is, it becomes possible to suppress deterioration of the WER uniformity within the wafer surface of the SiN film that is finally formed, that is, the wet etching resistance uniformity within the wafer surface. It is also possible to suppress the thickness of the SiN film that is finally formed from being thick at the center of the wafer 200. That is, it becomes possible to suppress deterioration of the thickness uniformity within the wafer surface of the SiN film that is finally formed. In particular, N x * , Ar * , He * Among other active species, N x * Since the active species such as H, Ar, and H2 have a relatively short lifetime and are easily deactivated, this effect is particularly noticeable in step 3. That is, when an inert gas such as N2 gas, Ar gas, or He gas, especially N2 gas, is excited into a plasma state and supplied to the wafer 200, this effect is particularly noticeable.

[0134] For example, when performing the film formation process, the interval (arrangement pitch) between the multiple wafers 200 may be set to be at least twice the interval (arrangement pitch) between the wafers 200 when the maximum number of wafers 200 that can be supported by the boat 217 is supported. In this case, the interval (arrangement pitch) between the wafers 200 can be set to, for example, 12 to 24 mm or more. This can further suppress deactivation of the active species due to collision with the wafers 200, and can further increase the probability that the active species will reach the center of the wafers 200, thereby sufficiently achieving the above-mentioned effects.

[0135] Furthermore, for example, when performing the film formation process, the interval (arrangement pitch) between the multiple wafers 200 may be set to three times or more the interval (arrangement pitch) between the wafers 200 when the maximum number of wafers 200 that can be supported by the boat 217 is supported. In this case, the interval (arrangement pitch) between the wafers 200 can be set to, for example, 18 to 36 mm or more. This can further suppress deactivation of the active species due to collision with the wafers 200, and further increase the probability that the active species will reach the center of the wafer 200, thereby more fully achieving the above-mentioned effects.

[0136] Furthermore, for example, when performing the film formation process, the interval (arrangement pitch) between the multiple wafers 200 may be set to four or more times the interval (arrangement pitch) between the wafers 200 when the maximum number of wafers 200 that can be supported by the boat 217 is supported. In this case, the interval (arrangement pitch) between the wafers 200 can be set to, for example, 24 to 48 mm or more. This can further suppress deactivation of the active species due to collision with the wafers 200, and further increase the probability that the active species will reach the center of the wafers 200, thereby more fully achieving the above-mentioned effects.

[0137] (g) The above-mentioned various effects are particularly noticeable when an inert gas is excited into a plasma state and supplied to the wafer 200 from the side of the wafer 200 in step 3. The above-mentioned various effects are particularly noticeable when an N- and H-containing gas is excited into a plasma state and supplied to the wafer 200 from the side of the wafer 200 in step 2. The above-mentioned various effects are particularly noticeable when a raw material gas is supplied to the wafer 200 from the side of the wafer 200 in step 1. However, the present disclosure is not limited to the case where various gases are supplied to the wafer 200 from the side of the wafer 200.

[0138] (h) When a film is formed at a low temperature using plasma, the wet etching resistance of the film may decrease, and the film quality may deteriorate. However, according to the present embodiment, even when a film is formed at a low temperature using plasma, the above-mentioned various effects can be obtained, and a high-quality film can be formed.

[0139] (4) Variations The processing sequence in this embodiment can be modified as shown in the following modified examples. These modified examples can be combined as desired. Unless otherwise specified, the processing procedure and processing conditions in each step of each modified example can be the same as the processing procedure and processing conditions in each step of the above-mentioned processing sequence.

[0140] (Variation 1) By using a source gas containing Si-N bonds as the source gas, the source gas can act not only as a Si source but also as an N source, and the supply of N- and H-containing gas can be omitted. That is, in the film forming process, a SiN film may be formed on the wafer 200 by the process sequence shown in FIG. 6 and below.

[0141] (Source gas → P → Plasma excited inert gas → P) × n

[0142] in this case, (a) supplying a source gas to the wafer 200 in a processing chamber; (c) exciting an inert gas into a plasma state and supplying the gas to the wafer 200 in the processing chamber; Specifically, a cycle including these steps is performed a predetermined number of times to form a film on the wafer 200. The above-described processing sequence shows an example in which a cycle of performing (a) and (c) asynchronously is performed a predetermined number of times with a process of purging the processing vessel between them.

[0143] In this case as well, it is desirable to set the pressure inside the processing vessel in (c) to 2 Pa or more and 6 Pa or less, preferably 2.66 Pa or more and 5.32 Pa or less, and more preferably 3 Pa or more and 4 Pa ​​or less.

[0144] The source gas in this modification, that is, the source gas containing Si-N bonds, may be a silylamine gas such as monosilylamine ((SiH3)NH2, abbreviated as MSA) gas, disilylamine ((SiH3)2NH, abbreviated as DSA) gas, or trisilylamine ((SiH3)3N, abbreviated as TSA) gas. One or more of these may be used as the source gas. Of these, it is preferable to use TSA containing three Si-N bonds as the source gas. These source gases may be supplied to the wafer 200 from the above-mentioned source gas supply system. The process conditions may be the same as those in step 1 of the process sequence of the above-mentioned embodiment.

[0145] In this modification, the inert gas may be N2 gas or a rare gas such as Ar gas, He gas, Ne gas, or Xe gas, as in the inert gas in step 3 of the processing sequence of the above embodiment. One or more of these may be used as the inert gas. Among these, it is preferable to use N2 gas as the inert gas in this modification. These inert gases may be supplied to the wafer 200 from the inert gas supply system described above. The processing conditions may be the same as those in step 3 of the processing sequence of the above embodiment.

[0146] In this modification, the same effects as those of the above embodiment can be obtained. In addition, according to this modification, the supply of N and H-containing gas can be omitted, and the processing time can be shortened. As a result, the throughput, i.e., the productivity, can be improved.

[0147] (Variation 2) The above cycle may further include a step of supplying an O-containing gas to the wafer 200. In this case, a silicon oxynitride film (SiON film) can be formed on the wafer 200. In this case, the O-containing gas may be supplied to the wafer 200 without being excited into a plasma state, or the O-containing gas may be excited into a plasma state and then supplied. That is, in the film forming process, a SiON film may be formed on the wafer 200 by the process sequence shown below. Note that, as in the above embodiment, purging before and after the supply of the plasma-excited inert gas may be omitted.

[0148] (Source gas → P → O-containing gas → P → Plasma-excited N- and H-containing gas → P → Plasma-excited inert gas → P) × n (Source gas → P → Plasma excited N and H containing gas → P → O containing gas → P → Plasma excited inert gas → P) × n (Source gas → P → Plasma excited N and H containing gas → P → Plasma excited inert gas → P → O containing gas → P) × n (Source gas → P → Plasma excited O-containing gas → P → Plasma excited N- and H-containing gas → P → Plasma excited inert gas → P) × n (Source gas → P → Plasma excited N and H containing gas → P → Plasma excited O containing gas → P → Plasma excited inert gas → P) × n (Source gas → P → Plasma excited N and H containing gas → P → Plasma excited inert gas → P → Plasma excited O containing gas → P) × n

[0149] In these cases, an O-containing gas can be supplied to the wafer 200 from the above-mentioned O-containing gas supply system. The process conditions can be the same as those in step 2 of the process sequence of the above-mentioned embodiment. A hydrogen (H)-containing gas may be supplied together with the O-containing gas. The H-containing gas can be supplied from, for example, a raw material gas supply system or a N and H-containing gas supply system.

[0150] Examples of the O-containing gas that can be used include oxygen (O2) gas, ozone (O3) gas, water vapor (HO gas), hydrogen peroxide (HO2) gas, nitrous oxide (NO) gas, nitrogen monoxide (NO2) gas, carbon monoxide (CO) gas, carbon dioxide (CO2) gas, etc. One or more of these can be used as the O-containing gas.

[0151] When supplying a H-containing gas together with an O-containing gas, the H-containing gas may be, for example, hydrogen (H2) gas or deuterium ( 2 H2) gas, etc. can be used. 2 H2 gas is also called D2 gas. One or more of these gases can be used as the H-containing gas.

[0152] In this modified example, the same effects as those of the above-mentioned embodiment can be obtained. That is, even if the cycle further includes a step of supplying an O-containing gas to the wafer 200 and forming a SiON film on the wafer 200, the same effects as those of the above-mentioned embodiment can be obtained.

[0153] The cycle described above in the first modification may further include a step of supplying an O-containing gas to the wafer 200. In this case, it is also possible to form a SiON film on the wafer 200. In this case, the O-containing gas may be supplied to the wafer 200 without being excited into a plasma state, or the O-containing gas may be excited into a plasma state and then supplied. That is, in the film forming process, a SiON film may be formed on the wafer 200 by the process sequence shown below. In this case, as in the above embodiment, purging before and after the supply of the plasma-excited inert gas may be omitted.

[0154] (Source gas → P → O-containing gas → P → Plasma-excited inert gas → P) × n (Source gas → P → Plasma excited inert gas → P → O-containing gas → P) × n (Source gas → P → Plasma excited O-containing gas → P → Plasma excited inert gas → P) × n (Source gas → P → Plasma excited inert gas → P → Plasma excited O-containing gas → P) × n

[0155] In this case, too, the same effects as those of the above-mentioned embodiment and modification 1 can be obtained. That is, even if the cycle further includes a step of supplying an O-containing gas to the wafer 200 and forming a SiON film on the wafer 200, the same effects as those of the above-mentioned embodiment and modification 1 can be obtained.

[0156] <Other Aspects of the Disclosure> Although the embodiments of the present disclosure have been specifically described above, the present disclosure is not limited to the above embodiments and can be modified in various ways without departing from the spirit and scope of the present disclosure.

[0157] For example, in addition to performing steps 1, 2, and 3 as one cycle in this order a predetermined number of times (n times, n is an integer equal to or greater than 1) as in the processing sequence in the above embodiment, the order in which each step is performed may be changed as in the processing sequence shown below. In these cases, the same effects as those of the above embodiment can be obtained.

[0158] (Step 1 → Step 2 → Step 3) × n (Step 2 → Step 3 → Step 1) × n (Step 3 → Step 1 → Step 2) × n

[0159] However, if the final step in the cycle is step 1 or step 2, the composition and modification effect of the outermost surface of the finally formed film may differ from those of the remaining portions. Therefore, as in the processing sequence shown below, it is preferable to perform step 2 or step 3 after the final cycle is completed, and fine-tune the film quality of the outermost surface of the finally formed film so that the degree of nitridation by step 2 and the degree of modification by step 3 are equivalent to those of the layers formed up to that point.

[0160] (Step 2 → Step 3 → Step 1) × n → Step 2 → Step 3 (Step 3 → Step 1 → Step 2) × n → Step 3

[0161] Also, for example, like the processing sequence in the above-mentioned embodiment, steps 1, 2, and 3 are one cycle and this cycle is performed a predetermined number of times (n times, n is an integer of 1 or more), or steps 1 and 2 may be performed multiple times (m times, m is an integer of 2 or more) and then step 3 may be performed, and this cycle may be performed a predetermined number of times (n times, n is an integer of 1 or more). Also, after performing step 1, steps 2 and 3 may be performed multiple times (m times, m is an integer of 2 or more) and then this cycle may be performed a predetermined number of times (n times, n is an integer of 1 or more). These processing sequences can be expressed as follows. In these cases, the same effects as those of the above-mentioned embodiment can be obtained.

[0162] (Step 1 → Step 2 → Step 3) × n [(Step 1 → Step 2) × m → Step 3] × n [Step 1 → (Step 2 → Step 3) × m] × n

[0163] Also, for example, steps 1 and 2 may be performed in a state where a plurality of wafers 200 are supported by a boat 217 as shown in FIG. 7(a), and step 3 may be performed in a state where a plurality of wafers 200 are supported by a boat 217 as shown in FIG. 7(b) or FIG. 7(c). That is, the interval (arrangement pitch) P1 between the plurality of wafers 200 in step 3 may be set larger than the interval (arrangement pitch) P2 between the plurality of wafers 200 in steps 1 and 2 (P1>P2). In this case, for example, it is preferable to set P1≧2P2, more preferably to set P1≧3P2, and even more preferably to set P1≧4P2. For example, when P2 is set to 6 to 12 mm, it is preferable to set P1 to 12 to 24 mm or more, more preferably to set P1 to 18 to 36 mm or more, and even more preferably to set P1 to 24 to 48 mm or more. In these cases, in step 3, the boat 217 having the interval (arrangement pitch) of the support parts 217b of, for example, 6 to 12 mm supports the wafers 200 every few wafers. The boat 217 having the interval (arrangement pitch) of the support parts 217b itself within the above-mentioned numerical range may support the wafers 200. In these cases, a first processing chamber and a second processing chamber having the same configuration as the processing chamber 201 may be prepared, and steps 1 and 2 may be performed in the first processing chamber, and step 3 may be performed in the second processing chamber. In this case, the same effect as the above-mentioned embodiment can be obtained. Furthermore, in this case, the number of wafers 200 subjected to steps 1 and 2 can be made larger than the number of wafers 200 subjected to step 3.

[0164] Also, for example, step 1 may be performed in a state where a plurality of wafers 200 are supported by a boat 217 as shown in FIG. 7(a), and steps 2 and 3 may be performed in a state where a plurality of wafers 200 are supported by a boat 217 as shown in FIG. 7(b) or FIG. 7(c). That is, the interval (arrangement pitch) P1 between the plurality of wafers 200 in steps 2 and 3 may be set larger than the interval (arrangement pitch) P2 between the plurality of wafers 200 in step 1 (P1>P2). In this case, for example, it is preferable to set P1≧2P2, more preferably to set P1≧3P2, and even more preferably to set P1≧4P2. For example, when P2 is set to 6 to 12 mm, it is preferable to set P1 to 12 to 24 mm or more, more preferably to set P1 to 18 to 36 mm or more, and even more preferably to set P1 to 24 to 48 mm or more. In these cases, in steps 2 and 3, the boat 217 having the interval (arrangement pitch) of the support parts 217b of, for example, 6 to 12 mm supports the wafers 200 every few wafers. The boat 217 having the interval (arrangement pitch) of the support parts 217b itself within the above-mentioned numerical range may support the wafers 200. In these cases, a first processing chamber and a second processing chamber having the same configuration as the processing chamber 201 may be prepared, and step 1 may be performed in the first processing chamber, and steps 2 and 3 may be performed in the second processing chamber. In this case, the same effect as the above-mentioned embodiment can be obtained. Furthermore, in this case, the number of wafers 200 subjected to step 1 can be made larger than the number of wafers 200 subjected to steps 2 and 3.

[0165] Furthermore, for example, the plasma generation method may be Capacitively Coupled Plasma (CCP) or Inductively Coupled Plasma (ICP). In this case, the same effects as those of the above-mentioned embodiment can be obtained.

[0166] It is preferable that the recipes used for each process are prepared individually according to the process contents and stored in the storage device 121c via an electric communication line or an external storage device 123. Then, when starting each process, it is preferable that the CPU 121a appropriately selects an appropriate recipe according to the process contents from among the multiple recipes stored in the storage device 121c. This makes it possible to form films of various film types, composition ratios, film qualities, and film thicknesses with good reproducibility using a single substrate processing device. It is also possible to reduce the burden on the operator and quickly start each process while avoiding operational errors.

[0167] The above-mentioned recipes may not only be newly created, but may also be prepared by modifying an existing recipe that has already been installed in the substrate processing apparatus. When modifying a recipe, the modified recipe may be installed in the substrate processing apparatus via an electric communication line or a recording medium on which the recipe has been recorded. In addition, an existing recipe that has already been installed in the substrate processing apparatus may be directly modified by operating the input / output device 122 provided in the existing substrate processing apparatus.

[0168] In the above-mentioned various aspects and various modifications, an example of forming a film using a batch-type substrate processing apparatus that processes multiple substrates at a time has been described. The present disclosure is not limited to the above-mentioned various aspects and various modifications, and can be suitably applied, for example, to a case where a film is formed using a single-wafer type substrate processing apparatus that processes one or several substrates at a time. In addition, in the above-mentioned various aspects and various modifications, an example of forming a film using a substrate processing apparatus having a hot-wall type processing furnace has been described. The present disclosure is not limited to the above-mentioned various aspects and various modifications, and can be suitably applied to a case where a film is formed using a substrate processing apparatus having a cold-wall type processing furnace.

[0169] When using these substrate processing apparatuses, each process can be performed using the same processing procedures and processing conditions as those in the various aspects and modified examples described above, and the same effects as those in the various aspects and modified examples described above can be obtained.

[0170] The above-mentioned various aspects and modifications may be used in appropriate combination. The processing procedures and processing conditions in such a combination may be the same as those in the above-mentioned various aspects and modifications. EXAMPLES

[0171] Using the substrate processing apparatus in the above embodiment, a SiN film was formed on a wafer by the processing sequence in the above embodiment. DCS gas was used as the source gas, NH3 gas was used as the N and H-containing gas, and N2 gas was used as the inert gas. The processing pressure in step 3 was set to the following four pressure conditions (pressure conditions 1 to 4), and a SiN film was formed on a wafer under each condition, to produce four types of SiN film evaluation samples 1 to 4. When producing evaluation samples 1 to 4, the processing conditions other than the processing pressure in step 3 were the same processing conditions within the processing condition range in the above embodiment, and the wafer interval (arrangement pitch) was 15 to 40 mm in all cases.

[0172] Pressure condition 1: 0.01 Torr (1.33 Pa) Pressure condition 2: 0.02 Torr (2.66 Pa) Pressure condition 3: 0.04 Torr (5.32 Pa) Pressure condition 4: 0.06 Torr (7.98 Pa)

[0173] After preparing the evaluation samples 1 to 4, the WER and film thickness of the SiN film of each of the evaluation samples 1 to 4 in the wafer plane were measured. The results are shown in Figs. 8 to 11. The horizontal axis in Figs. 8 to 11 indicates the distance (radius) from the center of the wafer 200, with 0 mm indicating the center of the wafer and 150 mm and -150 mm indicating the outer periphery (edge) of the wafer 200. The vertical axis on the left side of Figs. 8 to 11 indicates the WER in arbitrary units (au), and the vertical axis on the right side indicates the film thickness in arbitrary units (au). In the figures, ◇ indicates the film thickness, and ● indicates the WER. Figs. 8 to 11 respectively show the measurement results of the WER and film thickness in the wafer plane of the SiN film of the evaluation samples 1 to 4.

[0174] From FIG. 8, it can be seen that in the SiN film of evaluation sample 1, where the processing pressure in step 3 was set to pressure condition 1, the WER at the outer periphery of the wafer is higher than the WER at the center of the wafer. It can also be seen that the film thickness of the SiN film of evaluation sample 1 is thicker at the outer periphery of the wafer than at the center of the wafer. In other words, it can be seen that the WER uniformity within the wafer and the film thickness uniformity within the wafer of the SiN film of evaluation sample 1 are both not good. The reason why the WER of the SiN film of evaluation sample 1 is higher at the outer periphery of the wafer is due to the N2 gas generated when the N2 gas is excited into plasma under pressure condition 1. + The reason why the thickness of the SiN film of the evaluation sample 1 was thicker at the periphery of the wafer is thought to be due to the N2 gas generated when the N2 gas was excited into plasma under pressure condition 1. + It is believed that the cause of this is that the ion attack by the SiN film destroyed the film structure of the SiN film at the outer periphery of the wafer, changing that portion into a sparse film.

[0175] 9 shows that the WER is equivalent at the wafer periphery and wafer center for the SiN film of evaluation sample 2, where the processing pressure in step 3 is set to pressure condition 2. It is also shown that the film thickness is equivalent at the wafer periphery and wafer center for the SiN film of evaluation sample 2. In other words, it is shown that the wafer WER uniformity and wafer film thickness uniformity for the SiN film of evaluation sample 2 are both extremely good.

[0176] 10, it can be seen that the WER is equivalent at the outer periphery and the center of the wafer for the SiN film of evaluation sample 3, in which the processing pressure in step 3 was set to pressure condition 3. It can also be seen that the film thickness is equivalent at the outer periphery and the center of the wafer for the SiN film of evaluation sample 3. In other words, it can be seen that the WER uniformity within the wafer and the film thickness uniformity within the wafer for the SiN film of evaluation sample 3 are both extremely good.

[0177] From FIG. 11, it can be seen that in the SiN film of evaluation sample 4, in which the processing pressure in step 3 was set to pressure condition 4, the WER at the wafer center is higher than the WER at the wafer periphery. It can also be seen that the film thickness at the wafer center is thicker than the film thickness at the wafer periphery for the SiN film of evaluation sample 4. In other words, it can be seen that the wafer-wide WER uniformity and wafer-wide film thickness uniformity for the SiN film of evaluation sample 4 are both not good. The reason why the WER of the SiN film of evaluation sample 4 is higher at the wafer center is due to the N generated when the N2 gas is plasma-excited under pressure condition 4. * , N2 * Reactive species such as N * The reason for this is thought to be that the proportion of active species such as niobium and niobium that are deactivated before reaching the center of the wafer is high, and the film modification effect at the center of the wafer is insufficient. Also, the thickness of the SiN film of evaluation sample 4 is thicker at the center of the wafer because of N generated when N2 gas is plasma-excited under pressure condition 4. * , N2 * Reactive species such as N * This is believed to be because a high proportion of active species such as these are deactivated before reaching the center of the wafer, resulting in insufficient densification of the film at the center of the wafer.

[0178] From the above, it was found that the WER uniformity within the wafer and the film thickness uniformity within the wafer are extremely high, and a high-quality SiN film can be formed by setting the processing pressure in step 3 to 0.02 Torr (2.66 Pa) to 0.04 Torr (5.32 Pa). It was also confirmed that the WER uniformity within the wafer and the film thickness uniformity within the wafer are extremely high, and a high-quality SiN film can be formed by setting the processing pressure in step 3 to 2 to 6 Pa. [Explanation of symbols]

[0179] 200 wafers 201 Processing Room

Claims

1. (a) supplying a source gas to a substrate; (b) after (a), supplying a nitrogen- and hydrogen-containing gas to the substrate while exciting the gas into a plasma state; (c) supplying an inert gas, which is at least one of N 2 gas and a rare gas, to the substrate while exciting the inert gas into a plasma state; (d) between (a) and (b), supplying a purge gas, which is at least one of N 2 gas and a rare gas, to the space in which the substrate is present, to purge the space in which the substrate is present under a non-plasma atmosphere; forming a film on the substrate by performing a cycle including the steps of: (c) making the pressure of the space in which the substrate is present lower than the pressure of the space in which the substrate is present in (b); A substrate processing method, comprising: (c) setting a supply flow rate of gas supplied to a space in which the substrate exists lower than a supply flow rate of gas supplied to a space in which the substrate exists in (d).

2. 2. The substrate processing method according to claim 1, wherein the pressure in the space in which the substrate exists in (c) is set to 2 Pa or more and 6 Pa or less.

3. 2. The substrate processing method according to claim 1, wherein the pressure in the space in which the substrate exists in (c) is set to 2.66 Pa or more and 5.32 Pa or less.

4. 2. The substrate processing method according to claim 1, wherein the pressure in the space in which the substrate exists in (c) is set to 3 Pa or more and 4 Pa ​​or less.

5. 5. The substrate processing method according to claim 1, wherein the time during which the inert gas is excited into a plasma state and supplied in (c) is longer than the time during which the nitrogen- and hydrogen-containing gas is excited into a plasma state and supplied in (b).

6. 2. The substrate processing method according to claim 1, wherein the time during which the inert gas is excited into a plasma state and supplied in (c) is longer than the time during which the source gas is supplied in (a).

7. A substrate processing method described in any one of claims 1 to 6, wherein the pressure in the space in which the substrate is present in (c) is made lower than the pressure in the space in which the substrate is present in (d).

8. The inert gas is N 2 The method for processing a substrate according to any one of claims 1 to 7, further comprising the step of:

9. 8. The substrate processing method according to claim 1, wherein the inert gas contains Ar gas.

10. The nitrogen and hydrogen containing gas is NH 3 Gas, N 2 H 2 Gas, N 2 H 4 Gas, N 3 H 8 10. The substrate processing method according to claim 1, further comprising at least one of the following gases:

11. 11. The substrate processing method according to claim 1, wherein the source gas contains a halosilane gas.

12. The substrate processing method according to any one of claims 1 to 11, wherein in (c), the inert gas is excited into a plasma state inside the processing vessel by applying electric power to an electrode provided outside the processing vessel in which the substrate is processed.

13. 13. The substrate processing method according to claim 1, wherein the step of forming a film on the substrate is performed in a processing vessel with the plurality of substrates supported by a support, and the spacing between the plurality of substrates is set to be greater than the spacing between the substrates when the maximum number of substrates that can be supported by the support is supported.

14. The substrate processing method according to claim 13 , wherein in the step of forming a film on the substrate, the spacing between the substrates is set to be at least twice the spacing between the substrates when the maximum number of substrates that can be supported by the support is supported.

15. The substrate processing method according to any one of claims 1 to 14, wherein the step of forming a film on the substrate is performed with a plurality of the substrates arranged in a processing vessel, and the distance between the plurality of substrates is set to 12 mm or more and 60 mm or less.

16. The substrate processing method according to any one of claims 1 to 14, wherein the step of forming a film on the substrate is performed with a plurality of the substrates arranged in a processing vessel, and the distance between the plurality of substrates is set to 15 mm or more and 60 mm or less.

17. 17. The substrate processing method according to claim 1, wherein in (c), the inert gas is excited into a plasma state and supplied to the substrate from a side of the substrate.

18. (a) supplying a source gas to a substrate; (b) after (a), supplying a nitrogen- and hydrogen-containing gas to the substrate while exciting the gas into a plasma state; (c) supplying an inert gas, which is at least one of N 2 gas and a rare gas, to the substrate while exciting the inert gas into a plasma state; (d) between (a) and (b), supplying a purge gas, which is at least one of N 2 gas and a rare gas, to the space in which the substrate is present, to purge the space in which the substrate is present under a non-plasma atmosphere; forming a film on the substrate by performing a cycle including the steps of: (c) making the pressure of the space in which the substrate is present lower than the pressure of the space in which the substrate is present in (b); A method for manufacturing a semiconductor device, comprising the steps of: (c) causing a flow rate of the gas supplied to the space in which the substrate is present to be smaller than a flow rate of the gas supplied to the space in which the substrate is present to be in (d).

19. a processing vessel in which the substrate is processed; a source gas supply system for supplying a source gas into the processing vessel; a nitrogen and hydrogen-containing gas supply system for supplying a nitrogen and hydrogen-containing gas into the processing vessel; an inert gas supply system that supplies an inert gas, which is at least one of N 2 gas and a rare gas, into the processing vessel; a plasma excitation unit for exciting the gas into a plasma state; a pressure adjusting unit for adjusting a pressure inside the processing vessel; a control unit configured to be capable of controlling the source gas supply system, the nitrogen- and hydrogen-containing gas supply system, the inert gas supply system, the plasma excitation unit, and the pressure adjustment unit so that a pressure in the processing vessel in (c) is lower than a pressure in the processing vessel in (b) and a supply flow rate of gas supplied into the processing vessel in (c) is lower than a supply flow rate of gas supplied into the processing vessel in (d), the control unit being configured to be capable of controlling the source gas supply system, the nitrogen- and hydrogen-containing gas supply system, the inert gas supply system, the plasma excitation unit, and the pressure adjustment unit so that a pressure in the processing vessel in (c) is lower than a pressure in the processing vessel in (b), and a supply flow rate of gas supplied into the processing vessel in (c) is lower than a supply flow rate of gas supplied into the processing vessel in (d), A substrate processing apparatus comprising:

20. (a) supplying a source gas to a substrate; (b) after (a), supplying a nitrogen- and hydrogen-containing gas to the substrate while exciting the gas into a plasma state; (c) supplying an inert gas, which is at least one of N 2 gas and a rare gas, to the substrate while exciting the gas into a plasma state; (d) between (a) and (b), supplying a purge gas, which is at least one of N 2 gas and a rare gas, to the space in which the substrate is present, to purge the space in which the substrate is present under a non-plasma atmosphere; forming a film on the substrate by performing a predetermined number of cycles including the steps of: a step of lowering the pressure of the space in which the substrate is present in (c) to be lower than the pressure of the space in which the substrate is present in (b), and lowering the supply flow rate of gas supplied to the space in which the substrate is present in (c) to be lower than the supply flow rate of gas supplied to the space in which the substrate is present in (d); A program for causing a computer to execute the above in a substrate processing apparatus.

Citation Information

Patent Citations

  • Semiconductor device manufacturing method, substrate processing method, substrate processing apparatus and program

    JP2013093551A

  • Film forming method and film forming apparatus of silicon nitride film